Polybutylene terephthalate resin film, and method for producing polybutylene terephthalate resin film
A polybutylene terephthalate resin film with a mixture of resins of varying intrinsic viscosities stabilizes crystallinity, reducing sagging and wrinkles while maintaining mechanical strength and heat resistance.
Patent Information
- Application Number
- JP2023049454
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Polybutylene terephthalate resin films experience significant sagging and wrinkles due to high crystallinity, which compromises their dimensional stability and appearance, while blending with low-melting-point additives or resins compromises heat resistance and other inherent properties.
A polybutylene terephthalate resin film composed of a mixture of two or more resins with different intrinsic viscosities, maintaining a high content of polybutylene terephthalate resin and controlled molecular weight distribution to stabilize crystallinity and reduce dimensional changes.
The film exhibits reduced sagging and wrinkles while preserving mechanical strength, heat resistance, and electrical insulation, achieving a balanced performance.
Smart Images

Figure 2024138780000001 
Figure 2024138780000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polybutylene terephthalate resin film and a method for producing a polybutylene terephthalate resin film. [Background technology]
[0002] Polybutylene terephthalate resin films, which are primarily composed of polybutylene terephthalate resin, are excellent in mechanical strength, chemical resistance, electrical insulation, and the like, and also have excellent heat resistance, formability, and recyclability. Therefore, they are sometimes used in fields where high performance is required, such as when the usage environment is high temperature or when they are used in parts where voltage is applied. Polybutylene terephthalate resin has a high melting point of about 224° C. and also has high crystallinity, so that a polybutylene terephthalate resin film can have high heat resistance, high mechanical strength, and high electrical insulation. On the other hand, since polybutylene terephthalate resin has high crystallinity, when it is extruded from a molten state into a film shape and then cooled and solidified in the process of forming a polybutylene terephthalate resin film, the difference between the density in the molten state and the density of the crystal is large, and the dimensions change significantly upon solidification, and this dimensional change is likely to cause sagging and wrinkles in the resulting polybutylene terephthalate resin film.
[0003] In order to overcome these problems, attempts have been made to obtain a smooth polybutylene terephthalate resin film with less sagging and wrinkles by blending a non-crystalline resin component or a crystalline resin component with a low degree of crystallinity with the polybutylene terephthalate resin.
[0004] For example, Patent Document 1 proposes "a method of using a thermoplastic polymer having a melting point of less than 220°C as an additive to a polybutylene terephthalate molding composition in order to reduce necking during stretching of a sheet of the polybutylene terephthalate molding composition or a polybutylene terephthalate resin film." This technique is effective for obtaining a smooth polybutylene terephthalate resin film with little sagging or wrinkles; however, because a thermoplastic polymer with a low melting point is deliberately added to polybutylene terephthalate resin, which has a high melting point and high heat resistance, the heat resistance is slightly reduced. Furthermore, even if other amorphous resins or crystalline resins with reduced crystallinity are blended, the heat resistance as well as the transparency and texture may change, resulting in a polybutylene terephthalate resin film that is slightly different from the intended result, despite the film being produced with the aim of obtaining a polybutylene terephthalate resin film made of polybutylene terephthalate resin. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2020 / 208053 Summary of the Invention [Problem to be solved by the invention]
[0006] In view of the above circumstances, an object of the present invention is to provide a polybutylene terephthalate resin film that maintains the inherent performance of polybutylene terephthalate resin while suppressing appearance defects such as sagging and wrinkles, and a method for producing a polybutylene terephthalate resin film. [Means for solving the problem]
[0007] In view of the above problems, the present inventors have conducted research and found that the above problems can be solved by using two types of polybutylene terephthalate resins having different intrinsic viscosities. Specifically, the above problems were solved by the following means. <1> A polybutylene terephthalate resin film having a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, The polybutylene terephthalate resin film is a mixture of two or more kinds of polybutylene terephthalate resins having substantially the same composition but different intrinsic viscosities. <2> Among the polybutylene terephthalate resins contained in the mixture, the difference in intrinsic viscosity of at least two types is 0.10 dL / g or more. <1> 2. The polybutylene terephthalate resin film according to claim 1 . <3> At least two of the polybutylene terephthalate resins contained in the mixture each contain 10 parts by mass or more per 100 parts by mass of the total amount of the polybutylene terephthalate resins. <1> or <2> 2. The polybutylene terephthalate resin film according to claim 1 . <4> The thickness of the polybutylene terephthalate resin film is 5 to 200 μm. <1> ~ <3> 13. The polybutylene terephthalate resin film according to claim 12. <5> The intrinsic viscosity of the mixture is 0.80 to 1.40 dL / g. <1> ~ <4> 13. The polybutylene terephthalate resin film according to claim 12. <6> The mixture the difference in intrinsic viscosity between at least two of the polybutylene terephthalate resins contained in the mixture is 0.10 dL / g or more, at least two of the polybutylene terephthalate resins contained in the mixture each contain 10 parts by mass or more per 100 parts by mass of the total amount of the polybutylene terephthalate resin, the thickness of the polybutylene terephthalate resin film is 5 to 200 μm, and the intrinsic viscosity of the mixture is 0.80 to 1.40 dL / g; <1> ~ <5> 13. The polybutylene terephthalate resin film according to claim 12. <7> A method for producing a polybutylene terephthalate resin film by extruding a mixture of at least two polybutylene terephthalate resins, comprising the steps of: The polybutylene terephthalate resin film has a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, A method for producing a polybutylene terephthalate resin film, wherein the polybutylene terephthalate resin is a mixture of two or more polybutylene terephthalate resins having substantially the same resin composition but different intrinsic viscosities. <8> The polybutylene terephthalate resin film <1> ~ <6> The polybutylene terephthalate resin film according to any one of the above items. <7> A method for producing the polybutylene terephthalate resin film according to claim 1. Effect of the Invention
[0008] According to the present invention, it is possible to provide a polybutylene terephthalate resin film in which defects in appearance such as sagging and wrinkles are suppressed, and a method for producing a polybutylene terephthalate resin film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, an embodiment of the present invention (hereinafter, simply referred to as "the present embodiment") will be described in detail. Note that the present embodiment is an example for explaining the present invention, and the present invention is not limited to the present embodiment. In this specification, the use of "to" means that the numerical values before and after it are included as the lower limit and upper limit. In this specification, various physical properties and characteristic values are those at 23° C. unless otherwise specified. The film in this specification includes those in the form of a sheet. Also, the "film" refers to a molded body that is thin relative to its length and width and is generally flat. Also, the "polybutylene terephthalate resin film" in this specification may be a single layer or a multilayer, and is preferably a single layer. If the measurement methods, etc. described in the standards shown in this specification vary from year to year, they will be based on the standards as of January 1, 2022, unless otherwise stated.
[0010] The polybutylene terephthalate resin film of this embodiment is a polybutylene terephthalate resin film having a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, and is characterized in that the polybutylene terephthalate resin is a mixture of two or more polybutylene terephthalate resins having substantially the same composition but different intrinsic viscosities. By adopting such a constitution, it is possible to obtain a polybutylene terephthalate resin film in which defects in appearance such as sagging and wrinkles are suppressed while maintaining the inherent properties of the polybutylene terephthalate resin. In this embodiment, when the total mass is 100 parts by mass, the polybutylene terephthalate resin content is 95 parts by mass or more, so that the mechanical strength, heat resistance, and insulating properties inherent to the polybutylene terephthalate resin can be exhibited at a high level in a well-balanced manner. In addition, by using two or more polybutylene terephthalate resins with different intrinsic viscosities, the molecular weight distribution of the polybutylene terephthalate resin can be made wider. That is, in general, only one type of polybutylene terephthalate resin is used in the production of a film, but in this case, the molecular weight distribution of the polybutylene terephthalate resin tends to be sharp. In this case, it is presumed that a small gap or the like is formed in the T-die during film production, and more polybutylene terephthalate resin is extruded from this part than from other parts, causing unevenness. In this embodiment, by broadening the molecular weight distribution of the polybutylene terephthalate resin, low molecular weight polybutylene terephthalate resin and high molecular weight polybutylene terephthalate resin are mixed together, and it is presumed that while maintaining the performance of the high molecular weight polybutylene terephthalate resin as a crystalline resin, the regularity of the crystal arrangement within the polybutylene terephthalate resin film is disrupted, thereby reducing dimensional change when cooled and solidified. In particular, while injection-molded products made of polybutylene terephthalate resin can be adjusted using additives, polybutylene terephthalate resin films are highly valuable in that they can be molded without the use of additives, as the introduction of air bubbles during molding can cause uneven flow.
[0011] The polybutylene terephthalate resin film of the present embodiment has a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is taken as 100 parts by mass. By adopting such a constitution, a polybutylene terephthalate resin film having excellent properties inherent to polybutylene terephthalate resin can be obtained. The content of polybutylene terephthalate resin in the polybutylene terephthalate resin film of this embodiment is preferably 96 parts by mass or more, more preferably 97 parts by mass or more, even more preferably 98 parts by mass or more, and even more preferably 99 parts by mass or more, with the upper limit being 100 parts by mass, when the total mass of the film is 100 parts by mass.
[0012] The polybutylene terephthalate resin used in this embodiment is a mixture of two or more kinds of polybutylene terephthalate resins having substantially the same composition but different intrinsic viscosities. Here, the composition of two or more polybutylene terephthalate resins is substantially the same means that the structural units and / or raw material monomers of two or more polybutylene terephthalate resins are substantially the same. The structural units and / or raw material monomers are substantially the same, for example, means that 95% by mass or more of the structural units and / or raw material monomers are the same, and more preferably 96% by mass or more, more preferably 97% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more. In this embodiment, the upper limit may be 100% by mass of the structural units and / or raw material monomers are the same. More preferably, in each of the two or more polybutylene terephthalate resins used in the present embodiment, the proportion of butylene terephthalate units having the structure shown below among all structural units excluding terminal groups is preferably 95% by mass or more, more preferably 96% by mass or more, even more preferably 97% by mass or more, even more preferably 98% by mass or more, and even more preferably 99% by mass or more, and the upper limit may be 100% by mass. [ka]
[0013] The polybutylene terephthalate resin used in this embodiment is a mixture of two or more polybutylene terephthalate resins having different intrinsic viscosities. By using two or more polybutylene terephthalate resins having different intrinsic viscosities, the molecular weight distribution of the polybutylene terephthalate resin becomes large, and a polybutylene terephthalate resin film having excellent appearance can be obtained. Specifically, the difference in intrinsic viscosity of at least two of the polybutylene terephthalate resins contained in the mixture is preferably 0.10 dL / g or more, more preferably 0.20 dL / g or more, and even more preferably 0.30 dL / g or more. By making it equal to or greater than the lower limit, the appearance of the film tends to be improved. In addition, the upper limit of the difference in intrinsic viscosity of at least two of the polybutylene terephthalate resins contained in the mixture is, for example, preferably 2.00 dL / g or less, more preferably 1.50 dL / g or less, more preferably 1.00 dL / g or less, and even more preferably 0.50 dL / g or less. By making it equal to or less than the upper limit, the mechanical strength of the obtained polybutylene terephthalate resin film tends to be improved. In this embodiment, the mixture may contain three or more polybutylene terephthalate resins. If three or more types are contained, it is sufficient that two of the polybutylene terephthalate resins in the mixture satisfy the above range, and it is preferable that the two polybutylene terephthalate resins having the first and second highest contents in the mixture satisfy the above range.
[0014] The intrinsic viscosity of the polyethylene terephthalate resin used in this embodiment is preferably 0.50 dL / g or more, more preferably 0.60 dL / g or more, even more preferably 0.65 dL / g or more, even more preferably 0.75 dL / g or more, and preferably 2.00 dL / g or less, more preferably 1.80 dL / g or less, even more preferably 1.50 dL / g or less, and even more preferably 1.45 dL / g or less. By making it equal to or more than the lower limit, the mechanical strength of the obtained polybutylene terephthalate resin film tends to be further improved. In addition, by making it equal to or less than the upper limit, the fluidity of the polybutylene terephthalate resin is improved, and a polybutylene terephthalate resin film with a better appearance tends to be obtained.
[0015] The polybutylene terephthalate resin of the present embodiment is preferably a blend of a polybutylene terephthalate resin (a1) having an intrinsic viscosity of 0.5 to 1.25 dL / g and a polybutylene terephthalate resin (a2) having an intrinsic viscosity of 1.00 to 2.00 dL / g. The blend ratio (mass ratio) of (a1):(a2) is preferably 1 to 60:99 to 40, more preferably 10 to 60:90 to 40, even more preferably 20 to 60:80 to 40, and even more preferably 30 to 60:70 to 40. In particular, it is preferable that the difference in intrinsic viscosity between the two types of polybutylene terephthalate resins satisfies the above range and also satisfies the difference between (a1) and (a2) above.
[0016] The intrinsic viscosity of the polybutylene terephthalate resin mixture of this embodiment is preferably 0.80 dL / g or more, more preferably 0.90 dL / g or more, even more preferably 1.10 dL / g or more, even more preferably 1.15 dL / g or more, even more preferably 1.20 dL / g or more, and even more preferably 1.25 dL / g or more. By making it equal to or greater than the lower limit, the appearance of the obtained polybutylene terephthalate resin tends to be improved. The upper limit of the intrinsic viscosity of the polybutylene terephthalate resin mixture is preferably 1.40 dL / g or less, and may be 1.35 dL / g or less, or 1.30 dL / g or less. By making it equal to or less than the upper limit, the resin pressure during molding does not become higher than necessary, and the film forming machine can be maintained stably. The resin pressure can also be reduced by reducing the discharge amount per hour, but since this tends to reduce productivity, it is preferable to make the intrinsic viscosity equal to or less than the upper limit.
[0017] The intrinsic viscosity of the polybutylene terephthalate resin is measured at 30° C. in a mixed solvent of 1,1,2,2-tetrachloroethane and phenol in a 1:1 (mass ratio).
[0018] The amount of terminal carboxyl groups in the polybutylene terephthalate resin may be appropriately selected and determined, but is usually 60 eq / ton or less, preferably 50 eq / ton or less, and more preferably 30 eq / ton or less. By making it 60 eq / ton or less, it is possible to make it difficult for gas to be generated during melt molding. The lower limit of the amount of terminal carboxyl groups is not particularly determined, but is usually 10 eq / ton in consideration of the productivity of the production of polybutylene terephthalate resin. The amount of terminal carboxyl groups in the polybutylene terephthalate resin refers to a value obtained by dissolving 0.5 g of the polyalkylene terephthalate resin in 25 mL of benzyl alcohol and measuring by titration using a 0.01 mol / L benzyl alcohol solution of sodium hydroxide. The amount of terminal carboxyl groups can be adjusted by any conventionally known method, such as a method of adjusting polymerization conditions such as the raw material charge ratio during polymerization, polymerization temperature, and pressure reduction method, or a method of reacting a terminal blocking agent.
[0019] In the present embodiment, it is preferable that at least two of the polybutylene terephthalate resins contained in the mixture each contain 1 part by mass or more (preferably 10 parts by mass or more) per 100 parts by mass of the total amount of polybutylene terephthalate resin. By adopting such a constitution, the effect of reducing sagging and wrinkles when the polybutylene terephthalate resin film obtained is formed tends to be further improved. More specifically, the content of at least two kinds of polybutylene terephthalate resins is preferably 1 part by mass or more, more preferably 3 parts by mass or more, even more preferably 10 parts by mass or more, even more preferably 15 parts by mass or more, even more preferably 20 parts by mass or more, even more preferably 25 parts by mass or more, and particularly more preferably 30 parts by mass or more, based on 100 parts by mass of the total amount (mixture) of polybutylene terephthalate resins. Also, the content of at least two kinds of polybutylene terephthalate resins is preferably 90 parts by mass or less, more preferably 80 parts by mass or less, and even more preferably 75 parts by mass or less, based on 100 parts by mass of the total amount (mixture) of polybutylene terephthalate resins. However, it goes without saying that the total amount of polybutylene terephthalate resins does not exceed 100 parts by mass. An example of a blend form of a mixture of polybutylene terephthalate resins is a mixture in which the proportion of one type of polybutylene terephthalate resin contained in the mixture is 25 to 50 parts by mass, the proportion of the other type is 70 to 50 parts by mass, and the total of the other type or types of two or more is 0 to 10 parts by mass.
[0020] The polybutylene terephthalate resin used in this embodiment may contain a dicarboxylic acid unit other than terephthalic acid without departing from the spirit of this embodiment. As the dicarboxylic acid other than terephthalic acid constituting the polybutylene terephthalate resin, an aromatic dicarboxylic acid or an ester-forming derivative thereof is preferably used. Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, orthophthalic acid, 1,5-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, biphenyl-2,2'-dicarboxylic acid, biphenyl-3,3'-dicarboxylic acid, biphenyl-4,4'-dicarboxylic acid, diphenylether-4,4'-dicarboxylic acid, diphenylmethane-4,4'-dicarboxylic acid, diphenylsulfone-4,4'-dicarboxylic acid, diphenylisopropylidene-4,4'-dicarboxylic acid, 1,2-bis(phenoxy)ethane-4,4'-dicarboxylic acid, anthracene-2,5-dicarboxylic acid, anthracene-2,6-dicarboxylic acid, p-terphenylene-4,4'-dicarboxylic acid, and pyridine-2,5-dicarboxylic acid. Terephthalic acid is preferably used. These aromatic dicarboxylic acids may be used in combination of two or more. As is well known, in addition to the free acids, these may be used in the polycondensation reaction as ester-forming derivatives such as dimethyl esters. In addition, small amounts of these aromatic dicarboxylic acids can be used in combination with one or more aliphatic dicarboxylic acids such as adipic acid, azelaic acid, dodecanedioic acid, and sebacic acid, and alicyclic dicarboxylic acids such as 1,2-cyclohexanedicarboxylic acid, 1,3-cyclohexanedicarboxylic acid, and 1,4-cyclohexanedicarboxylic acid.
[0021] The dihydroxy compound constituting the polybutylene terephthalate resin may include, in addition to 1,4-butanediol, aliphatic diols such as ethylene glycol, propylene glycol, hexylene glycol, neopentyl glycol, 2-methylpropane-1,3-diol, diethylene glycol, and triethylene glycol, alicyclic diols such as cyclohexane-1,4-dimethanol, and mixtures thereof. In addition, if the amount is small, one or more long-chain diols having a molecular weight of 400 to 6,000, such as polyethylene glycol, poly-1,3-propylene glycol, and polytetramethylene glycol, may be copolymerized. Additionally, aromatic diols such as hydroquinone, resorcin, naphthalenediol, dihydroxydiphenyl ether, and 2,2-bis(4-hydroxyphenyl)propane can also be used. In addition to the above-mentioned bifunctional monomers, a small amount of a trifunctional monomer such as trimellitic acid, trimesic acid, pyromellitic acid, pentaerythritol, or trimethylolpropane may be used in combination to introduce a branched structure, or a monofunctional compound such as a fatty acid may be used in combination to adjust the molecular weight.
[0022] The polybutylene terephthalate resin film of the present embodiment may contain other components within a range that does not impair the effects of the present embodiment, such as flame retardants, flame retardant assistants, ultraviolet absorbers, weather stabilizers, lubricants, colorants such as dyes and pigments, catalyst deactivators, antistatic agents, foaming agents, plasticizers, crystal nucleating agents, crystallization accelerators, other thermoplastic resins, and thermosetting resins. Examples of other thermoplastic resins include modified polybutylene terephthalate resins, polyester resins other than polybutylene terephthalate resins, polyamide resins, polycarbonate resins, polyacetal resins, polyphenylene oxide resins, polyphenylene sulfide resins, acrylic resins, etc., and examples of thermosetting resins include phenol resins, melamine resins, silicone resins, epoxy resins, etc. These may be used alone or in combination of two or more kinds. However, the total amount of other components is 5 parts by mass or less, preferably 4 parts by mass or less, more preferably 3 parts by mass or less, even more preferably 2 parts by mass or less, even more preferably 1 part by mass or less, even more preferably 0.5 parts by mass or less, even more preferably 0.1 parts by mass or less, and particularly more preferably 0.01 parts by mass or less, relative to 100 parts by mass of the polybutylene terephthalate resin film of this embodiment.
[0023] The thickness of the polybutylene terephthalate resin film of this embodiment is preferably 5 μm or more, more preferably 10 μm or more, even more preferably 30 μm or more, even more preferably 50 μm or more, and even more preferably 80 μm or more, from the viewpoint of film strength. Also, the thickness of the polybutylene terephthalate resin film of this embodiment is preferably 200 μm or less, more preferably 180 μm or less, even more preferably 150 μm or less, and even more preferably 120 μm or less, from the viewpoint of functional expression as a film.
[0024] The polybutylene terephthalate resin film of the present embodiment may be a single-layer film or a multi-layer film of two or more layers. In the case of a multi-layer film, examples of layers other than the polybutylene terephthalate resin film include a print layer, an adhesive layer, a sealant layer, an iron film, a polypropylene film, and a thermoplastic resin layer that is a crystalline film such as an ethylene-vinyl acetate copolymer film.
[0025] The polybutylene terephthalate resin film of the present embodiment may be a stretched film or an unstretched film. In the case of a stretched film, it may be a uniaxially stretched film or a biaxially stretched film.
[0026] The polybutylene terephthalate resin film of the present embodiment is used, for example, as a food packaging material.
[0027] Next, a method for producing the polybutylene terephthalate resin film will be described. The method for producing the polybutylene terephthalate resin film of the present embodiment is not particularly limited, and can be selected from general production methods. A specific example is a method for producing a polybutylene terephthalate resin film by extruding a mixture of at least two types of polybutylene terephthalate resins, in which the polybutylene terephthalate resin film has a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, and the polybutylene terephthalate resin is a mixture of two or more types of polybutylene terephthalate resins having substantially the same resin composition and different intrinsic viscosities. The film can be produced by a T-die film production method, an inflation film production method, or the like. If necessary, the film can be stretched. This stretching can be carried out during the film production process, or the film can be taken up as a polybutylene terephthalate resin film and then stretched in a post-process. In this embodiment, two or more types of polybutylene terephthalate resins having different intrinsic viscosities are mixed. This may be done by dry blending pellets of each resin until they are uniform during film formation, or by compounding the resins in advance in a single-screw or twin-screw kneader to form pellets of the mixture and then forming the mixture into a film. EXAMPLES
[0028] The present invention will be described in more detail below with reference to examples. The materials, amounts, ratios, processing contents, processing procedures, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the scope of the present invention is not limited to the specific examples shown below. If the measuring instruments used in the examples are difficult to obtain due to discontinuation or the like, measurements can be made using other instruments with equivalent performance.
[0029] Examples 1 to 4 Pellets of polybutylene terephthalate resin (a polymer of terephthalic acid component and 1,4-butanediol component) having an intrinsic viscosity shown in Table 1 were dry blended at the blend ratios shown in Table 1 (the ratios of the polybutylene terephthalate resin in Table 1 are mass ratios). The pellet blend was charged into an extruder and formed into a film using a T-die under the following conditions to obtain a polybutylene terephthalate resin. From the extruder shown below, under the following conditions, the polybutylene terephthalate resin was extruded in a sheet form from the T-die and taken up by a winder to produce a polybutylene terephthalate resin film. The discharge rate of the extruder and the take-up speed of the film were adjusted to obtain a polybutylene terephthalate resin film with a thickness of 100 μm. A paper tube (the diameter of the tube was wound to 4 inches) was used to obtain a wound body of the polybutylene terephthalate resin film.
[0030] <T-die film forming> Extruder: manufactured by Ikegai, FS40 Screw diameter φ40 mm, L / D = 25, single screw, full flight Die: lip width, 200 mm Film forming conditions: cylinder 250 °C, die 250 °C Cooling roll temperature: set at 60 °C Screw rotation speed: 40 rpm The pellets were placed in a vat and dried in a hot air dryer at 120 °C for 8 hours before film formation and then charged into the extruder.
[0031] <Film winding appearance evaluation> After the wound body of the obtained polybutylene terephthalate resin film was left standing in an environment of 25 °C and 50% RH for 24 hours without applying a load, the winding appearance was observed. The observation was carried out by 5 experts and judged by a majority vote. C or above was regarded as the practical level. A: No sagging or wrinkles were confirmed. B: Slight sagging occurred but was less severe than C, and no distinct wrinkles were confirmed. C: Sagging was clearly present, but no distinct wrinkles were confirmed. D: Sagging and wrinkles occurred clearly.
[0032] Comparative Example 1 and Comparative Example 2 Pellets of polybutylene terephthalate resin (polymer of terephthalic acid component and 1,4-butanediol component) having an intrinsic viscosity shown in Table 1 were fed into an extruder, and otherwise the same procedure as in Example 1 was followed to obtain a polybutylene terephthalate resin film having a thickness of 100 μm. The appearance of the resulting film when wound was evaluated in the same manner as in Example 1.
[0033] [Table 1]
[0034] In Table 1 above, the ratio of each component is a mass ratio. In Table 1 above, the intrinsic viscosity of the mixture means the intrinsic viscosity of the mixture of polybutylene terephthalate resins. In Table 1 above, the intrinsic viscosity difference indicates the difference in intrinsic viscosity of polybutylene terephthalate resins. For example, in Example 1, the difference (0.10 dL / g) between the intrinsic viscosity of polybutylene terephthalate resin A4 (1.20 dL / g) and the intrinsic viscosity of polybutylene terephthalate resin A6 (1.30 dL / g) is 0.10 dL / g. As is clear from the above results, the polybutylene terephthalate resin film of the present invention was free from wrinkles and sagging and had excellent film winding appearance (Examples 1 to 4). In particular, the appearance was further improved by blending two types of polybutylene terephthalate resins in a well-balanced manner (comparison of Examples 1, 3, and 4 with Example 2). Furthermore, the appearance was further improved by increasing the difference in intrinsic viscosity between the two types of polybutylene terephthalate resins (comparison of Examples 3 and 4 with Example 1). In contrast, when one type of polybutylene terephthalate resin was used, the appearance of the polybutylene terephthalate resin was poor (Comparative Examples 1 and 2). That is, the conventional problems of polybutylene terephthalate resin films were manifested.
Claims
1. A polybutylene terephthalate resin film having a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, The polybutylene terephthalate resin film is a mixture of two or more kinds of polybutylene terephthalate resins having substantially the same composition but different intrinsic viscosities.
2. The polybutylene terephthalate resin film according to claim 1 , wherein the difference in intrinsic viscosity between at least two of the polybutylene terephthalate resins contained in the mixture is 0.10 dL / g or more.
3. The polybutylene terephthalate resin film according to claim 1 or 2, wherein at least two of the polybutylene terephthalate resins contained in the mixture each contain 10 parts by mass or more per 100 parts by mass of the total amount of the polybutylene terephthalate resin.
4. The polybutylene terephthalate resin film according to claim 1 or 2, wherein the polybutylene terephthalate resin film has a thickness of 5 to 200 μm.
5. The polybutylene terephthalate resin film according to claim 1 or 2, wherein the intrinsic viscosity of the mixture is 0.80 to 1.40 dL / g.
6. Among the polybutylene terephthalate resins contained in the mixture, the difference in intrinsic viscosity of at least two types is 0.10 dL / g or more; At least two of the polybutylene terephthalate resins contained in the mixture each contain 10 parts by mass or more per 100 parts by mass of the total amount of the polybutylene terephthalate resins; The thickness of the polybutylene terephthalate resin film is 5 to 200 μm, The polybutylene terephthalate resin film according to claim 1, wherein the intrinsic viscosity of the mixture is 0.80 to 1.40 dL / g.
7. A method for producing a polybutylene terephthalate resin film by extruding a mixture of at least two polybutylene terephthalate resins, comprising the steps of: The polybutylene terephthalate resin film has a polybutylene terephthalate resin content of 95 parts by mass or more when the total mass is 100 parts by mass, A method for producing a polybutylene terephthalate resin film, wherein the polybutylene terephthalate resin is a mixture of two or more polybutylene terephthalate resins having substantially the same resin composition but different intrinsic viscosities.
8. The method for producing a polybutylene terephthalate resin film according to claim 7, wherein the polybutylene terephthalate resin film is the polybutylene terephthalate resin film according to claim 1, 2 or 6.
Citation Information
Patent Citations
Photographic base and photographic material
JP1999202446A
Polyester resin composition and its production
JP1999236493A
Polyester composition and polyester molded article made thereof
JP2005350663A
Heat-shrinkable polyester film
JP2009523899A
Method for producing polybutylene terephthalate
JP2013007058A