Long-fiber nonwoven fabric and production method thereof

A long-fiber nonwoven fabric with controlled fused and non-fused portions addresses moisture retention and penetration issues, enabling effective plant growth in desert environments.

JP2024138804APending Publication Date: 2024-10-09TORAY INDUSTRIES INC

Patent Information

Application Number
JP2023049500
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing nonwoven fabrics used for bed-cover cultivation in desert environments fail to maintain sufficient moisture in the soil and inhibit plant growth due to high penetration resistance and removal requirements.

Method used

A long-fiber nonwoven fabric with specific area ratios and thickness ratios of fused and non-fused portions, composed of thermoplastic resin fibers, is developed to retain moisture and reduce penetration resistance, allowing plants to grow without hindrance.

Benefits of technology

The fabric effectively retains soil moisture and supports plant growth by minimizing penetration resistance, making it suitable for seedling-growing sheets and other applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138804000001_ABST
    Figure 2024138804000001_ABST
Patent Text Reader

Abstract

To provide a long-fiber nonwoven fabric which allows soil to retain sufficient water content when laid, and allows a plant to grow without obstruction even when kept laid down.SOLUTION: A long-fiber nonwoven fabric composed of fiber including a thermoplastic resin as a main component, having an area ratio of fused part of 5% or more and 25% or less, a ratio of thickness at fused part of the long-fiber nonwoven fabric TE(μm) to thickness at non-fused part of the long-fiber nonwoven fabric TNE(μm), i.e. TE / TNE, of 0.05 or more and 0.15 or less, and an apparent density of 0.10 g / cm3 or more and 0.25 g / cm3 or less.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a long-fiber nonwoven fabric and a method for producing the same. [Background technology]

[0002] In recent years, there has been a strong call for solutions to environmental issues, and desertification in particular is an issue that needs to be resolved because it is caused by a variety of interconnected social problems.

[0003] To combat this desertification, greening activities are being carried out, but when it comes to germinating and raising crop seedlings, issues include evaporation of water from the sand, and growth hindrances caused by weather and animals.

[0004] Traditionally, field cover cultivation has been practiced, in which a sheet is directly placed over the soil, crops, and seedlings to promote germination and seedling growth and to protect the crops from frost, rain, hail, etc. The "field cover sheet" used for this purpose is not only used for greening activities, but also to adjust the growth rate and shipping time of crops, and the field cover sheet is peeled off and then re-covered to check the condition of the crops, and the field cover sheet is attached and removed as appropriate.

[0005] As such a covering sheet, a nonwoven fabric made of continuous fibers is often used because it has air and water permeability, and is also excellent in light transmission and heat retention. For example, Patent Document 1 proposes an agricultural covering material made of a nonwoven fabric with a specific basis weight, which is composed of core-sheath type composite continuous fibers with a specific monofilament fineness, with a polyester-based polymer in the core and a polypropylene-based polymer in the sheath, and has a thermocompression bonded portion formed by a specific embossing process. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2015-223152 A Summary of the Invention [Problem to be solved by the invention]

[0007] The sheet described in Patent Document 1 is made of a nonwoven fabric composed of relatively thick fibers, with sheath-core structure yarns in the surface layer, in which the melting point of the resin in the sheath is lower than that of the resin in the core, and is therefore considered to have a certain degree of abrasion resistance. However, the sheet must be removed after a certain amount of time has passed so as not to inhibit the growth of plants when they germinate. It is possible to make cuts in the sheet in anticipation of the plants germinating, but in that case, there is a problem that it is not possible to sufficiently prevent the soil from drying out.

[0008] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a long-fiber nonwoven fabric which retains sufficient moisture in the soil when laid down, and does not inhibit plant growth even when left laid down. [Means for solving the problem]

[0009] As a result of extensive research into achieving the above-mentioned object, the inventors have found that by setting the area ratio and apparent density of the fused portions of the long-fiber nonwoven fabric within specific ranges, and further setting the ratio of the thickness of the fused portions to the thickness of the non-fused portions within specific ranges, not only will the long-fiber nonwoven fabric have the performance to retain sufficient moisture in the soil when laid down, but it will also be possible to lower the penetration resistance of the long-fiber nonwoven fabric to an extent that plants can break through the long-fiber nonwoven fabric and sprout.

[0010] The present invention has been completed based on these findings, and provides the following inventions.

[0011] [1] A long-fiber nonwoven fabric composed of fibers mainly composed of thermoplastic resin and having fused and non-fused parts, the area ratio of the fused parts being 5% or more and 25% or less, and the thickness T NE (μm) vs. thickness TE Ratio of T (μm) E / T NE is 0.05 or more and 0.15 or less, and the apparent density of the long fiber nonwoven fabric is 0.10 g / cm 3 More than 0.25g / cm 3 The following is a long fiber nonwoven fabric.

[0012] [2] The maximum tensile stress σ of the long fiber nonwoven fabric max Tensile stress σ of the long fiber nonwoven fabric at 3% elongation (N / 5cm) 3% Ratio σ of (N / 5cm) 3% / σ max The long-fiber nonwoven fabric according to the above item [1], wherein the linear modulus is 0.80 or more and 0.97 or less.

[0013] [3] Thickness T of the non-fused portion NE The long-fiber nonwoven fabric according to the above [1] or [2], wherein (μm) is 800 μm or more and 1500 μm or less.

[0014] [4] The length T of the long side of the fused portion L (μm) vs. the length T of the short side of the fused portion S Ratio of T (μm) S / T L The long-fiber nonwoven fabric according to any one of the above [1] to [3], wherein the value is 0.10 or more and 0.80 or less.

[0015] [5] The fused portion has a plurality of fused portions, and the average shortest distance T between the fused portions B (μm) vs. the length T of the short side of the fused portion S Ratio of T (μm) S / T B The long-fiber nonwoven fabric according to any one of the above [1] to [4], wherein the value is 0.01 or more and 0.30 or less.

[0016] [6] The basis weight of the long fiber nonwoven fabric is 100 g / m 2 More than 200g / m 2 The long-fiber nonwoven fabric according to any one of the above [1] to [5], which is as follows:

[0017] [7] A step of spinning a thermoplastic resin through an outlet hole of a spinneret and drawing the resin by suction to form a fiber; collecting the fibers on a moving net conveyor to form a fibrous web; a step of contacting both sides of the fiber web with a heating surface to perform primary fusion to form a temporarily fused sheet; a step of mechanically entangling the pre-fused sheet to form an entangled sheet; a step of heat fusing the entangled sheet with a pair of rolls; The method for producing a long-fiber nonwoven fabric according to any one of the above [1] to [6], The spinning speed in the suction drawing is 3000 m / min or more and 6000 m / min or less, The temperature of the heating surface during the primary fusion is 60° C. or more and 120° C. or less lower than the melting point of the thermoplastic resin, and the linear pressure of the heating surface is 100 N / cm or more and 900 N / cm or less, The surface temperature of the pair of rolls during the heat fusion is 5°C to 70°C lower than the melting point, and the linear pressure of the pair of rolls is 100 N / cm to 900 N / cm. A method for producing long fiber nonwoven fabric. Effect of the Invention

[0018] According to the present invention, a long-fiber nonwoven fabric can be obtained that retains sufficient moisture in the soil when laid down and does not inhibit plant growth even when left laid down. In particular, since the long-fiber nonwoven fabric of the present invention has the above-mentioned effects, it can be suitably used for seedling-raising sheets such as bed covering sheets. [Brief description of the drawings]

[0019] [Figure 1] FIG. 1 is a diagram illustrating the thickness TE of a fused portion and the thickness TNE of a non-fused portion in one embodiment of the long-fiber nonwoven fabric of the present invention. [Diagram 2] FIG. 2 is a schematic top view illustrating the length TL of the long side of the fused portion in one embodiment of the present invention in which the fused portion of the long-fiber nonwoven fabric is a parallelogram. [Diagram 3] FIG. 3 is a schematic top view illustrating the length TL of the long side of the fused portion in one embodiment of the present invention in which the fused portion is rectangular. [Figure 4] FIG. 4 is a schematic top view illustrating the length TL of the long side of the fused portion in one embodiment of the present invention in which the fused portion of the long-fiber nonwoven fabric is rhombic. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0020] The long-fiber nonwoven fabric of the present invention is composed of fibers mainly composed of a thermoplastic resin, and has fused portions and non-fused portions, the area ratio of the fused portions being 5% or more and 25% or less, and the thickness T NE (μm) vs. thickness T E Ratio of T (μm) E / T NE is 0.05 or more and 0.15 or less, and the apparent density of the long fiber nonwoven fabric is 0.10 g / cm 3 More than 0.25g / cm 3 The components are described in detail below, but the present invention is not limited to the scope of the following description as long as it does not deviate from the gist of the present invention, and various modifications are possible without departing from the gist of the present invention.

[0021] [Thermoplastic resin] First, the nonwoven fabric of the present invention is composed of fibers mainly composed of a thermoplastic resin. Examples of the thermoplastic resin include polyester, polyamide, polyolefin, and mixtures or copolymers thereof. Among them, polyester is preferably used because of its excellent durability such as mechanical strength, heat resistance, water resistance, and chemical resistance.

[0022] Polyester is a polymer having an acid component and a diol component as monomers. In the present invention, as the acid component, aromatic carboxylic acids such as terephthalic acid (ortho form), isophthalic acid, and terephthalic acid, aliphatic dicarboxylic acids such as adipic acid and sebacic acid, and alicyclic dicarboxylic acids such as cyclohexane carboxylic acid can be used. As the diol component, ethylene glycol, diethylene glycol, etc. can be used.

[0023] Specific examples of the polyester include polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate, polylactic acid, polybutylene succinate, etc. As the polyester used as the high melting point polymer described later, polyethylene terephthalate (PET) is most preferably used because it has a higher melting point, excellent heat resistance, and excellent rigidity.

[0024] Additives such as crystal nucleating agents, matting agents, lubricants, pigments, mildewproofing agents, antibacterial agents, flame retardants, metal oxides, aliphatic bisamides and / or alkyl-substituted aliphatic monoamides, and hydrophilic agents can be added to these polyesters within the scope of the present invention. Among them, metal oxides such as titanium oxide reduce the surface friction of the fibers and prevent the fibers from fusing together, thereby improving spinnability, and also improve the fusing property of the nonwoven fabric by increasing the thermal conductivity during the fusing molding of the nonwoven fabric with a heated roll. In addition, aliphatic bisamides such as ethylene bisstearic acid amide and / or alkyl-substituted aliphatic monoamides have the effect of increasing the releasability between the heated roll and the nonwoven fabric web, thereby improving the transportability.

[0025] [fiber] The fibers according to the present invention are mainly composed of the thermoplastic resin. In the present invention, "mainly composed of a thermoplastic resin" means that the mass of the thermoplastic resin is more than 50% by mass with respect to the mass of the entire fiber. The fibers according to the present invention may be single-component fibers or composite fibers in which a low-melting point polymer having a melting point lower than that of a high-melting point polymer is arranged around the high-melting point polymer. In the case of such composite fibers, the fibers are easily fused firmly within the nonwoven fabric, resulting in a nonwoven fabric with low penetration resistance. On the other hand, in the case of single-component fibers, the fibers are less damaged by mechanical entanglement and are easily entangled, resulting in a bulky nonwoven fabric with high strength.

[0026] When the above fibers are composite fibers, the difference between the melting points of the high melting point polymer and the low melting point polymer (hereinafter sometimes simply referred to as the melting point difference) is preferably 10°C or more and 140°C or less. In other words, it is preferable that the low melting point polymer has a melting point that is 10°C or more and 140°C or less lower than the melting point of the high melting point polymer. When the difference in melting points is 10°C or more, more preferably 20°C or more, and even more preferably 30°C or more, a long-fiber nonwoven fabric with high fusion between the fibers is obtained. In addition, when the difference is 140°C or less, more preferably 120°C or less, and even more preferably 100°C or less, a long-fiber nonwoven fabric in which film formation of the fibers is suppressed is obtained.

[0027] The melting point of the high melting point polymer is preferably in the range of 120° C. or higher and 320° C. or lower. A melting point of 120° C. or higher, more preferably 150° C. or higher, and even more preferably 180° C. or higher results in a long-fiber nonwoven fabric with excellent shape stability that can maintain its shape even when used in a high-temperature location such as a sandy surface. A melting point of 320° C. or lower, more preferably 300° C. or lower, and even more preferably 280° C. or lower prevents the fibers from becoming a film, resulting in a long-fiber nonwoven fabric with appropriate strength.

[0028] On the other hand, the melting point of the low melting point polymer is preferably in the range of 100° C. or more and 310° C. or less while ensuring the above-mentioned difference in melting points. By having a melting point of 100° C. or more, more preferably 130° C. or more, and even more preferably 160° C. or more, the long-fiber nonwoven fabric has excellent shape stability and can maintain its shape even when subjected to processing that involves the application of heat. In addition, by having a melting point of 310° C. or less, more preferably 290° C. or less, and even more preferably 270° C. or less, the long-fiber nonwoven fabric is prevented from forming a film and has appropriate breathability.

[0029] In the present invention, the melting point of a thermoplastic resin is measured using a differential scanning calorimeter (e.g., PerkinElmer's "DSC-2" model) at a heating rate of 20° C. / min and a measurement temperature range of 30° C. to 350° C., and the temperature at which the obtained melting endothermic curve gives an extreme value is defined as the melting point of the thermoplastic resin. For resins whose melting endothermic curve does not show an extreme value in the differential scanning calorimeter, the resin is heated on a hot plate, and the temperature at which the resin melts under a microscope is defined as the melting point.

[0030] In addition, when the fibers are monocomponent fibers, the melting point of the thermoplastic resin is preferably in the range of 120° C. or more and 320° C. or less. A melting point of preferably 120° C. or more, more preferably 150° C. or more, and even more preferably 180° C. or more results in a long-fiber nonwoven fabric with excellent shape stability that can maintain its shape even when used in a high-temperature location such as a sandy surface. A melting point of 320° C. or less, more preferably 300° C. or less, and even more preferably 280° C. or less suppresses the fibers from becoming a film, resulting in a long-fiber nonwoven fabric with appropriate strength.

[0031] In the case where the above-mentioned fiber is a composite fiber and the thermoplastic resin is a polyester, examples of the combination of a high melting point polymer and a low melting point polymer (hereinafter, the order of high melting point polymer / low melting point polymer) include, for example, combinations of PET / PBT, PET / PTT, PET / polylactic acid, and PET / copolymerized PET. Among these, the combination of PET / copolymerized PET is preferably used because of its excellent spinnability. As the copolymerization component of the copolymerized PET, isophthalic acid copolymerized PET is preferably used because of its excellent spinnability.

[0032] When the above-mentioned fibers are composite fibers, the composite form may be, for example, a concentric sheath-core type, an eccentric sheath-core type, or an island-in-the-sea type, among which the concentric sheath-core type is preferred because it allows the fibers to be fused uniformly and firmly. Furthermore, the cross-sectional shape of the composite fiber may be a circular cross-section, a flat cross-section, a polygonal cross-section, a multi-lobal cross-section, a hollow cross-section, or the like. Among these, it is preferable to use a circular cross-sectional shape as the cross-sectional shape of the composite fiber.

[0033] When the fibers are composite fibers, the content ratio of the high melting point polymer to the low melting point polymer is preferably in the range of 90:10 to 60:40 by mass, more preferably 85:15 to 70:30. By controlling the content of the high melting point polymer to be 60% by mass or more and 90% by mass or less, the durability of the long-fiber nonwoven fabric can be made excellent. On the other hand, by controlling the content of the low melting point polymer to be 10% by mass or more and 40% by mass or less, the fibers constituting the long-fiber nonwoven fabric are firmly fused to each other, and the long-fiber nonwoven fabric can have excellent mechanical strength.

[0034] The average single fiber diameter of the fibers constituting the long-fiber nonwoven fabric of the present invention is preferably in the range of 10.0 μm to 30.0 μm. When the average single fiber diameter is 10.0 μm or more, more preferably 12.0 μm or more, and even more preferably 14.0 μm or more, the long-fiber nonwoven fabric has excellent mechanical strength. On the other hand, when the average single fiber diameter is 30.0 μm or less, more preferably 28.0 μm or less, and even more preferably 26.0 μm or less, the long-fiber nonwoven fabric has higher uniformity and less unevenness.

[0035] In the present invention, the average single fiber diameter (μm) of the fibers is a value measured and calculated according to the following procedure. (1) Ten small sample pieces (100 mm x 100 mm) are randomly taken from the long fiber nonwoven fabric. (2) Take surface photographs at a magnification of 500 to 3,000 times using a scanning electron microscope (SEM, for example, Keyence Corporation's "VHX-D500"), and measure the diameters of 10 single fibers randomly selected from each sample, for a total of 100 single fibers. (3) The arithmetic mean of the measured values ​​of 100 fibers is rounded off to one decimal place to calculate the average single fiber diameter (μm).

[0036] [Long fiber nonwoven fabric] The long-fiber nonwoven fabric of the present invention is a long-fiber nonwoven fabric that is composed of the above-mentioned fibers and has fused parts and non-fused parts. The area ratio of the fused parts is 5% or more and 25% or less. If the area ratio of the fused parts is 5% or more, more preferably 6% or more, and even more preferably 8% or more, the long-fiber nonwoven fabric has sufficient strength and is not prone to fluffing on the surface. On the other hand, if the area ratio of the fused parts is 25% or less, more preferably 20% or less, and even more preferably 18% or less, the gaps between the fibers are reduced, improving breathability.

[0037] In the present invention, the fused portion of the long-fiber nonwoven fabric is a portion that forms a depression on the surface of the long-fiber nonwoven fabric and is formed by the fusion of the thermoplastic fibers that make up the long-fiber nonwoven fabric, i.e., a portion where the thermoplastic fibers are fused and aggregated compared to other portions, and other portions are referred to as non-fused portions. In the present invention, the long-fiber nonwoven fabric may have multiple fused portions, or may have only one fused portion as long as the above-mentioned area ratio is satisfied.

[0038] The area ratio of the fused portions of the long-fiber nonwoven fabric in the present invention is a value obtained as follows. (1) Randomly take five test pieces measuring 1 cm x 1 cm from the long fiber nonwoven fabric. (2) Using a digital microscope (such as Keyence Corporation's "VHX-5000"), photographs are taken at 10 locations on either side of the surface of the long-fiber nonwoven fabric at 20x to 100x magnification so that the fused and non-fused areas are visible. (3) For each of the 10 photographed regions, measure the area of ​​the fused portion within that region and the actual area of ​​that region, and calculate the arithmetic average value for a total of 50 areas. (4) The area of ​​the fused portion is divided by the actual area of ​​the region described above, converted into a percentage, and rounded off to the first decimal place to obtain the area ratio (%) of the fused portion.

[0039] Percentage of fused area (%) = Area of ​​fused area (mm 2 ) / area of ​​rectangular frame (mm 2 ) x 100.

[0040] The area of ​​each fused part is 0.3 mm 2 More than 10.0mm 2 Less than 0.3mm is preferred. 2 More than 0.4mm, preferably 0.4mm 2 By satisfying the above requirements, a long-fiber nonwoven fabric is obtained that has sufficient mechanical strength and further suppresses fluffing on the surface. 2 Less than or equal to 8.0mm, more preferably 2 Less than 6.0mm, more preferably 2When the above condition is satisfied, the long-fiber nonwoven fabric has excellent breathability.

[0041] Next, in the present invention, the thickness T of the non-fused portion of the long fiber nonwoven fabric NE (μm) vs. thickness T of the fused portion of the long fiber nonwoven fabric E Ratio of T (μm) E / T NE The ratio T is 0.05 or more and 0.15 or less. E / T NE When the ratio T is 0.05 or more, more preferably 0.06 or more, the long-fiber nonwoven fabric has higher strength. E / T NE When the ratio is 0.15 or less, more preferably 0.13 or less, and even more preferably 0.11 or less, the resulting long-fiber nonwoven fabric has lower penetration resistance and is highly flexible.

[0042] In the present invention, the thickness T of the non-fused portion of the long fiber nonwoven fabric NE (μm), thickness T of the fused portion of the long fiber nonwoven fabric E (μm), thickness ratio T E / T NE Refers to values ​​measured and calculated by the following methods. (i) Ten small sample pieces (5 mm x 20 mm) whose cross sections can be observed are randomly taken from the long-fiber nonwoven fabric using a sharp tool such as scissors or a razor blade. (ii) The cross section of the collected small sample is photographed at 50x to 500x magnification using a scanning electron microscope (SEM, such as Keyence Corporation's "VHX-D500") so that the fused and non-fused areas are visible. (iii) Measure the thickness of the unfused portion at one point on a photograph of each small sample as shown in Figure 1, and call that value T NE (μm), measure the thickness of the fused part at one point in the same way, and use that value as T E (μm). (iv) Measured T NE and T E Using the value of T E / T NE Calculate. (v) Repeat (ii) to (iv) for all the small piece samples, and calculate the T E / T NE The arithmetic mean of is rounded off to two decimal places.

[0043] Thickness T of the non-fused portion of the long fiber nonwoven fabric NE A long-fiber nonwoven fabric having a softness of 800 μm or more, more preferably 850 μm or more, and even more preferably 900 μm or more (μm) can be obtained. On the other hand, a long-fiber nonwoven fabric having a fineness of 1500 μm or less, more preferably 1450 μm or less can be obtained.

[0044] In the present invention, the length T of the long side of the fused portion L (μm) vs. short side length of fusion part T S Ratio of T (μm) S / T L is preferably 0.10 or more and 0.80 or less. S / T L is preferably 0.10 or more, more preferably 0.15 or more, the long-fiber nonwoven fabric has a suppressed anisotropy of mechanical strength. S / T L When the linearity is preferably 0.80 or less, more preferably 0.70 or less, and further preferably 0.60 or less, the long-fiber nonwoven fabric is easy to fold and has excellent handleability.

[0045] The length of the long side of the fused part is T L (μm), length of short side of fusion part T S (μm), and the ratio T S / T L refers to values ​​measured and calculated by the following methods. (i) Ten small sample pieces are randomly taken from the long fiber nonwoven fabric, each of which contains at least one fused portion. (ii) The surface of the collected small sample is photographed at 50x to 500x magnification using a scanning electron microscope (SEM, such as Keyence Corporation's "VHX-D500") so that the fused and non-fused areas are visible. (iii) On the photographs of each small sample, draw tangents parallel to the MD and CD directions at both the top and bottom ends of the fusion part as shown in Figures 2 to 4, and measure the longer distance of the tangents as T. L '(μm), the shorter one is T S The dimensions are expressed in μm. Note that the terms "MD direction" and "CD direction" used here refer to the directions determined by the method described below. (iv) Repeat (ii) and (iii) for all samples, and L Calculate the arithmetic mean value of ' and round it off to the nearest 1 decimal place to obtain T L Let us assume that T S Also L It is calculated in the same way. (v) Calculated T S and T L Using the value of T S / T L Calculate the figure and round off to the third decimal place.

[0046] In the present invention, the sheet has a plurality of fused portions, and the average shortest distance T between the fused portions is B (μm) vs. short side length of fusion part T S Ratio of T (μm) S / T B It is preferable that T is 0.01 or more and 0.30 or less. S / T B is preferably 0.01 or more, more preferably 0.05 or more, and even more preferably 0.10 or more, the long-fiber nonwoven fabric has higher strength. S / T B is preferably 0.30 or less, more preferably 0.25 or less, and even more preferably 0.20 or less, to provide a long-fiber nonwoven fabric with excellent breathability.

[0047] The average shortest distance between the fused parts T B (μm), and the ratio T S / T B refers to values ​​measured and calculated by the following methods. (i) Ten small sample pieces are randomly taken from the long fiber nonwoven fabric, each sample including at least five fused portions. (ii) The surface of the collected small sample is photographed at 50x to 500x magnification using a scanning electron microscope (SEM, such as Keyence Corporation's "VHX-D500") so that the fused and non-fused areas are visible. (iii) On the photographs taken from each small sample, the shortest distance between adjacent fused portions was measured as shown in Figs. 2 to 4, and this distance was designated as T B ' (μm). (iv) Repeat (ii) and (iii) for all samples, and B Calculate the arithmetic mean value of ' and round it off to the nearest 1 decimal place to obtain T B Let us assume that. (v) Calculated T S and T B Using the value of T S / T B Calculate the figure and round off to the third decimal place.

[0048] In the long fiber nonwoven fabric of the present invention, the apparent density is 0.10 g / cm 3 More than 0.25g / cm 3 This apparent density is 0.10 g / cm or less. 3 More preferably, 0.11 g / cm 3 More preferably, 0.12 g / cm 3 By setting the density to 0.25g / cm or more, the nonwoven fabric sheet will have high mechanical strength. 3 Less than or equal to 0.23 g / cm 3 More preferably, 0.21 g / cm 3 By ensuring that the hardness is equal to or less than 1, it is possible to prevent the sheet from becoming a hard nonwoven fabric with poor handleability.

[0049] In the present invention, the apparent density of the long-fiber nonwoven fabric refers to a value calculated by the following formula and rounded off to two decimal places: Apparent density (g / cm 3 )=Weight (g / m 2 ) / Thickness T NE (μm) Here, the thickness is the thickness T of the non-fused portion mentioned above.NE (μm), and the basis weight (g / m 2 ) shall be the value measured by the method described below.

[0050] The weight of the long fiber nonwoven fabric of the present invention is 100 g / m 2 More than 200g / m 2 The following range is preferable: 2 More preferably, 110 g / m 2 More preferably, 120 g / m 2 By setting the weight to 200g / m or more, the long fiber nonwoven fabric will have higher strength. 2 Less than 190 g / m 2 Less than 180g / m 2 When the ratio is equal to or less than 1, the long-fiber nonwoven fabric has good handleability.

[0051] In the present invention, the basis weight of the long-fiber nonwoven fabric refers to a value measured and calculated by the following method. (i) Three samples measuring 25 cm in length and 25 cm in width are randomly selected and their masses are measured. (ii) The arithmetic mean value (g) of the obtained values ​​(g) is calculated per unit area (1 m 2 ) converted to (g / m 2 ) and round the result to the nearest tenth.

[0052] In the present invention, the maximum tensile stress σ max Tensile stress σ of long fiber nonwoven fabric at 3% elongation (N / 5cm) 3% Ratio σ of (N / 5cm) 3% / σ max It is preferable that the ratio σ is 0.80 or more and 0.97 or less. 3% / σ max When the ratio σ is 0.80 or more, more preferably 0.82 or more, and even more preferably 0.84 or more, the long-fiber nonwoven fabric is easily deformed and does not inhibit plant growth. 3% / σ maxWhen the elastic modulus is 0.97 or less, more preferably 0.96 or less, and even more preferably 0.95 or less, the long-fiber nonwoven fabric does not break easily.

[0053] In the present invention, the maximum tensile stress σ max Tensile stress σ at 3% elongation (N / 5cm) 3% Ratio σ of (N / 5cm) 3% / σ max The value to be used shall be measured according to the following procedure in accordance with JIS L1913:2010 "General nonwoven fabric test methods", 6.3 "Tensile strength and elongation", 6.3.1 "Standard time". (i) Three test pieces, each 300 mm long and 50 mm wide, are taken from the long-fiber nonwoven fabric in the MD and CD directions. In the present invention, the MD direction refers to the sheet conveying direction during the production of the nonwoven fabric, i.e., the longitudinal direction of the long-fiber nonwoven fabric or the winding direction of the nonwoven fabric roll, and the CD direction, which will be described later, refers to the direction perpendicular to the sheet conveying direction, i.e., the longitudinal direction of the long-fiber nonwoven fabric or the winding direction of the nonwoven fabric roll. If the long-fiber nonwoven fabric is cut and is not in a rolled state, the MD and CD directions are determined by the following procedure. (a) Within the plane of the long-fiber nonwoven fabric, select one arbitrary direction and take a test piece 300 mm long x 50 mm wide along that direction. (b) Similarly, test pieces measuring 300 mm in length and 50 mm in width are taken at angles rotated 30 degrees, 60 degrees, and 90 degrees from the direction in which the test piece was taken. (c) For each test piece in each direction, the maximum tensile stress of each test piece is measured based on the method for measuring the maximum tensile stress of a long-fiber nonwoven fabric described below. (d) The direction in which the measured value is highest is defined as the MD direction of the long-fiber nonwoven fabric, and the direction perpendicular to this is defined as the CD direction. (ii) For each test piece in the MD and CD directions, a tensile test is carried out using a constant-speed extension type tensile tester with a gripping distance of 200 mm and a tensile speed of 100±10 mm / min. (iii) Calculate the strength (N) at the maximum load until breakage to the nearest 0.1 N, and call this the maximum tensile stress σ max (N / 5cm), and the tensile stress at 3% elongation is σ 3% (N / 5cm). (iv4) The measured maximum tensile stress σ max (N / 5cm) and tensile stress at 3% elongation σ 3% (N / 5cm) and σ 3% / σ max Calculate. (v) Maximum tensile stress σ for three specimens in MD and three specimens in CD max The arithmetic mean value of (N / 5cm) rounded off to the third decimal place, tensile stress at 3% elongation σ 3% The arithmetic mean value of (N / 5cm) rounded off to the third decimal place, σ 3% / σ max The arithmetic mean value of is calculated by rounding off to two decimal places, and σ in the MD direction is calculated. 3% / σ max and σ in the CD direction 3% / σ max The larger value of the ratio σ of the long fiber nonwoven fabric is 3% / σ max However, when the same value is shown in the MD and CD directions, the value in the MD direction is used as the ratio σ of the long fiber nonwoven fabric. 3% / σ max Let us assume that.

[0054] In the present invention, the ratio σ 3% / σ max In order to keep the above range, the needle elongation and needle density in the step of forming an entangled sheet in the manufacturing method of the long-fiber nonwoven fabric can be adjusted to the ranges described below.

[0055] The use of the long-fiber nonwoven fabric of the present invention is not particularly limited. However, since it has the characteristic of low penetration resistance, it can be particularly suitably used as a seedling sheet. This seedling sheet, when placed over the area where seeds are planted, suppresses water evaporation and retains sufficient moisture in the soil, and even if the seeds do not grow in a specific area, they can break the sheet themselves, so that the growth of plants is not hindered even when the sheet is laid down. Of course, the use is not limited to this, and it can also be used as a bandage, fruit tree wrapping material, seat cover, shoe cover, etc. in addition to the seedling sheet.

[0056] [Manufacturing method of long fiber nonwoven fabric] A preferred embodiment of the method for producing the long-fiber nonwoven fabric of the present invention will now be described in detail.

[0057] (1) Fiber formation process First, in this step, the thermoplastic resin is spun out from the nozzle of a spinneret. In the case of a single component fiber, it is preferable to melt the thermoplastic resin at (melting point + 70°C) or less and to spin the thermoplastic resin from the nozzle using a spinneret with a nozzle temperature of the melting point or more and (melting point + 70°C) or less. On the other hand, in the case of using a composite fiber in which a low melting point polymer having a melting point lower than the melting point of a high melting point polymer is arranged around the high melting point polymer as a fiber mainly composed of a thermoplastic resin, the high melting point polymer and the low melting point polymer are melted at temperatures of the melting point or more and (melting point + 70°C) or less, respectively, and the composite fiber in which a low melting point polymer having a melting point lower than the melting point of the high melting point polymer is arranged around the high melting point polymer can be spun out from the nozzle of a spinneret with a nozzle temperature of the melting point or more and (melting point + 70°C) or less.

[0058] The shape of the nozzle of the spinneret may be circular, elliptical, polygonal, multi-lobed, or a combination of these shapes according to the cross-sectional shape of the fiber. Of these, a circular cross-sectional shape is more preferable. For example, when a circular cross-sectional shape is used, bonding points between the fibers can be efficiently obtained, and the fibers can be firmly bonded to each other by heat fusion.

[0059] The thermoplastic resin spun as described above is then drawn under suction by an ejector or the like to form fibers. The spinning speed is preferably 3000 m / min to 6000 m / min.

[0060] (2) Forming a fiber web Next, in this process, the fibers are collected on a moving net conveyor to form a fiber web. The term "collecting the fibers on a moving net conveyor" refers to sequentially depositing the long fibers on a rotating net conveyor, and the net conveyor refers to a belt conveyor in which the belt portion is a punching plate, a net-like material, or a porous body. However, it is preferable to appropriately set the size of the holes, etc., in consideration of the resin constituting the long fibers and the fiber diameter of the long fibers, so that the collected long fibers do not fall into the net conveyor from the penetration portion of the net-like material, or the hole portion of the punching plate or the porous body (hereinafter, these are abbreviated as "hole portion, etc.") or become clogged in the hole portion, etc. The belt portion may be made of metal or synthetic resin. It is also preferable to regulate the arrangement of the fibers by a fiber spreader plate.

[0061] (3) Step of forming a temporary fusion sheet In this step, the heated surfaces of both sides of the fiber web are brought into contact with each other to perform primary fusion to form a pre-fused sheet. Specifically, a method of performing fusion using a pair of heated flat rolls is preferably used. Primary fusion using a pair of heated flat rolls is most preferable from the viewpoint of improving the strength of the long-fiber nonwoven fabric.

[0062] The "flat roll" used in these methods refers to a metal roll or an elastic roll that has no irregularities on the surface of the roll, and further, a pair of upper and lower flat rolls refers to a pair of a metal roll and a metal roll, or a pair of a metal roll and an elastic roll. Here, the elastic roll refers to a roll made of a material having elasticity compared to a metal roll. Examples of the elastic roll include so-called paper rolls made of paper, cotton, aramid paper, etc., and resin rolls made of urethane resin, epoxy resin, silicon resin, polyester resin, hard rubber, etc., or mixtures of these.

[0063] In the step of forming the temporary fused sheet, the temperature at which the fiber web is heated, for example, the surface temperature (heating surface temperature) of the flat rolls when a pair of heated flat rolls is used, is preferably 60°C or more and 120°C or less lower than the melting point of the thermoplastic resin (when multiple thermoplastic resins are used, the melting point of the one with the lowest melting point). By lowering the surface temperature by 60°C or more, more preferably by 70°C or more, relative to the melting point of the thermoplastic resin with the lowest melting point present on the surface of the fibers constituting the fiber web, the strength of the temporary fused sheet can be increased, and a long-fiber nonwoven fabric with excellent processability can be obtained. On the other hand, by lowering the surface temperature (heating surface temperature) by 120°C or less, more preferably by 110°C or less, relative to the melting point, the crystallization of the fibers can be kept to a minimum, and a temporary fused sheet with higher fusion property can be obtained in the fusion step described below.

[0064] For example, when fusion is performed using a pair of heated upper and lower flat rolls, the linear pressure of the pair of flat rolls is preferably 290 N / cm or more and 890 N / cm or less. By setting the linear pressure of the pair of flat rolls to preferably 290 N / cm or more, more preferably 390 N / cm or more, a long-fiber nonwoven fabric having sufficient mechanical strength for conveying the sheet can be obtained. On the other hand, by setting the linear pressure of the pair of flat rolls to 890 N / cm or less, more preferably 790 N / cm or less, excessive fusion can be prevented.

[0065] (4) Forming the interlaced sheet Furthermore, in this step, the pre-fused sheet is mechanically entangled to form an entangled sheet. Examples of the mechanical entanglement method include a water jet punch method and a needle punch method, among which the needle punch method is preferred because it does not require a large amount of water resources and provides high entanglement uniformity.

[0066] The needle density of the needle punch varies depending on the shape and type of needle, but the needle depth is set to 5mm to 20mm, and the needle density is set to 45 needles / cm 2 ~200 pieces / cm 2 It is preferable to punch one side or both sides of the temporary fusion sheet, and the needle density is 50 needles / cm 2 ~120 pieces / cm 2 The needle depth referred to here means the distance from the surface of the bed plate to the tip of the needle that has been pierced during needle punching.

[0067] (5) Process of heat fusing the interlaced sheet In addition, in this step, the entangled sheet is heat-sealed by a pair of rolls. Specifically, the fusion is performed by a hot embossing roll, which is particularly preferred from the viewpoint of improving the strength of the long-fiber nonwoven fabric.

[0068] The fusion temperature by the hot embossing roll is preferably 5°C to 70°C lower than the melting point of the polymer with the lowest melting point present on the fiber surface of the entangled sheet, and more preferably 10°C to 60°C lower. By making the temperature difference between the fusion temperature by the hot embossing roll and the melting point of the polymer with the lowest melting point present on the fiber surface of the entangled sheet 5°C or more, more preferably 10°C or more, excessive fusion can be prevented. On the other hand, by making the temperature difference 70°C or less, more preferably 60°C or less, uniform fusion can be performed within the entangled sheet.

[0069] In addition, the linear pressure of the pair of rolls during fusion is preferably 294 N / cm or more and 882 N / cm or less. By setting the linear pressure to 294 N / cm or more, more preferably 392 N / cm or more, a long-fiber nonwoven fabric with low penetration resistance can be obtained. On the other hand, by setting the linear pressure to 882 N / cm or less, more preferably 784 N / cm or less, the sheet can be prevented from becoming film-like.

[0070] When fusion by a hot embossing roll is used as the heat fusing method of the present invention, the part where the thermoplastic fibers are fused and aggregated by the convex parts of the embossing roll becomes the fused part. For example, when a roll having a predetermined pattern of concaves and convexes only on the upper or lower side is used, and the other roll is a flat roll without concaves and convexes, the fused part refers to the part where the thermoplastic fibers of the long-fiber nonwoven fabric are fused and aggregated by the convex parts of the roll having concaves and convexes and the flat roll. In addition, when an embossing roll is used, which is composed of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface, and the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, the fused part refers to the part where the thermoplastic fibers of the long-fiber nonwoven fabric are fused and aggregated by the convex parts of the upper roll and the convex parts of the lower roll. In this case, the part fused by the upper convex parts and the lower concave parts or the upper concave parts and the lower convex parts is not included in the fused part as used here.

[0071] The shape of the fused portion in the long-fiber nonwoven fabric of the present invention is not particularly limited, and even when a roll having a predetermined pattern of unevenness only on the upper or lower side is used and the other roll is a flat roll without unevenness, or when an embossing roll is made up of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface thereof, and the grooves of the upper roll and the grooves of the lower roll are arranged so as to intersect at a certain angle, and the convex portions of the upper roll and the convex portions of the lower roll are fused, the shape of the fused portion may be a circle, a triangle, a rectangle, a parallelogram, an ellipse, a rhombus, or the like. The arrangement of these fused portions is not particularly limited, and they may be arranged regularly at equal intervals, randomly, or a mixture of different shapes. Among these, it is preferable that the fused portions are arranged at equal intervals from the viewpoint of the uniformity of the long-fiber nonwoven fabric. Furthermore, in terms of partially fusing the long-fiber nonwoven fabric without peeling it off, it is preferable to use an embossing roll consisting of a pair of upper and lower rolls having a plurality of parallel linear grooves formed on the surface thereof, the grooves of the upper roll being arranged so as to intersect with the grooves of the lower roll at a certain angle, and to form a parallelogram-shaped fused portion formed by fusing the convex portions of the upper roll with the convex portions of the lower roll. EXAMPLES

[0072] The present invention will now be described in detail with reference to examples, although the present invention is not limited to these examples.

[0073] [Measurement method] The evaluation methods and measurement conditions used in the examples are described below. Unless otherwise specified, the measurements of each physical property were performed according to the above-mentioned methods.

[0074] (1) Melting point of polyester (℃) The measurements were carried out using a differential scanning calorimeter, "DSC-2" manufactured by PerkinElmer Japan Co., Ltd.

[0075] (2) Intrinsic viscosity of polyester (IV) The intrinsic viscosity (IV) of the polyester was measured and calculated by the following method. (i) 8 g of sample was dissolved in 100 mL of orthochlorophenol. (ii) After placing the solution in an atmosphere at 25°C, measure the relative viscosity η using an Ostwald viscometer. r was calculated using the following formula: η r = η / η 0 =(t × d) / (t 0 ×d 0 ) (Here, η is the viscosity of the polymer solution, η 0 is the viscosity of orthochlorophenol, t is the time it takes for the solution to fall (sec), and d is the density of the solution (g / cm 3 ), t 0 is the fall time of orthochlorophenol (seconds), d 0 is the density of orthochlorophenol (g / cm 3 ) and (iii) Next, the relative viscosity η r The intrinsic viscosity (IV) was calculated from the following formula: Intrinsic viscosity (IV)=0.0242η r +0.2634.

[0076] (3) Weight of long fiber nonwoven fabric (g / m 2 ) The basis weight of the long fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0077] (4) Thickness T of the non-fused portion of the long fiber nonwoven fabric NE (μm), thickness T of the fused portion of the long fiber nonwoven fabric E (μm), thickness ratio T E / T NE Thickness T of the non-fused portion of the long fiber nonwoven fabric NE (μm), thickness T of the fused portion of the long fiber nonwoven fabric E (μm), thickness ratio T E / T NE was measured and calculated by the above-mentioned method using a scanning electron microscope "VHX-D500" manufactured by Keyence Corporation.

[0078] (5) Apparent density of long fiber nonwoven fabric (g / cm 3 ) The apparent density of the long-fiber nonwoven fabric was measured and calculated by the above-mentioned method.

[0079] (6) Area ratio of fused area (%) The area ratio of the fused portion in the nonwoven fabric was measured and calculated by the above-mentioned method using a digital microscope "VHX-5000" manufactured by Keyence Corporation.

[0080] (7) Length of the long side of the fused part T L (μm), length of short side of fusion part T S (μm), the above ratio T S / T L Length of the long side of the fused part T L (μm), length of short side of fusion part T S (μm), and the ratio T S / T L was measured and calculated using the above-mentioned method using a Keyence Corporation "VHX-D500."

[0081] (8) Average shortest distance between fused parts T B (μm), the above ratio T S / T B Average shortest distance between fused parts of long fiber nonwoven fabric T B (μm), and the ratio T S / T B was measured and calculated using the above-mentioned method using a Keyence Corporation "VHX-D500."

[0082] (9) Ratio of tensile stress at 3% elongation to maximum tensile stress σ 3% / σ max maximum tensile stress σ max Tensile stress σ at 3% elongation (N / 5cm) 3% Ratio σ of (N / 5cm) 3% / σ max was measured and calculated using the above-mentioned method using a Tensilon universal testing machine "RTG-1250" manufactured by A&D Co., Ltd. as the measuring device.

[0083] (10) Penetration resistance (N) Three circular test pieces with a diameter of 8.0 cm were randomly taken from the long-fiber nonwoven fabric and placed on the mounting stand of a constant-speed extension-type tensile tester. Two rods with a diameter of 0.5 mm were then inserted vertically at a speed of 100 mm / min and a load was applied until the test pieces broke. The load at which the test pieces broke was measured, and the arithmetic average value was rounded off to one decimal place to determine the penetration resistance value of the long-fiber nonwoven fabric.

[0084] (11) Moisture retention rate (%) Three square test pieces measuring 8.0 cm x 8.0 cm were randomly taken from the long fiber nonwoven fabric and fixed in a 7.3 cm diameter cup containing 100 mL of water. A blank cup containing water without a test piece was also prepared. The test pieces were then left to stand in a Yamato Scientific Vacuum Drying Oven DP41 at 70°C and 30% humidity for 7 hours, and the arithmetic mean value V (mL) of the remaining water (with test pieces: V A , Blank: V B The moisture retention rate (%) of the test piece was calculated using the following formula: Moisture retention rate (%)=(1-(100―V A ) / (100-V B )) x 100.

[0085] (12) Abrasion resistance Measurements were carried out using a Gakushin type friction tester "G-2 (Gakushin type)" manufactured by Orihara Manufacturing Co., Ltd. Three test pieces measuring 220 mm in length and 30 mm in width were randomly taken from the long fiber nonwoven fabric, and the frictional load was set at 1000 g. "Rinrei Cloth Heavy Packaging No. 314" cloth adhesive tape was used on the frictional element side. The frictional element was operated 50 times, and the appearance after the abrasion test was evaluated on the following 5-point scale. 5: No fuzz at all 4: Almost invisible, but some fuzziness 3: Fluffy and partially pilled 2: Overall, pilling is noticeable 1: Overall, pilling is noticeable and the sample is starting to tear.

[0086] [Resin used] Next, the resins used in the examples and comparative examples will be described in detail. Polyester resin A: Polyethylene terephthalate (PET) dried to a moisture content of 50 ppm by mass or less, with an intrinsic viscosity (IV) of 0.65 and a melting point of 260°C. Polyester resin B: Copolymerized polyethylene terephthalate (CO-PET) dried to a moisture content of 50 ppm by mass or less, with an intrinsic viscosity (IV) of 0.64, an isophthalic acid copolymerization rate of 11 mol%, and a melting point of 230°C.

[0087] [Example 1] (The process of forming fibers) The polyester resin A was melted at a temperature of 295° C. Then, it was spun out from a circular discharge hole of a spinneret whose temperature was set to 295° C. Then, the spun polyester resin A was suction-drawn by an ejector at a spinning speed of 4500 m / min to form a fiber.

[0088] (Step of forming a fiber web) The obtained fibers were sprayed from a fiber-spreading plate to control the fiber arrangement, and the fibers were collected on a moving net conveyor whose moving speed was adjusted so that the basis weight of the obtained nonwoven fabric was 5% or less of the target basis weight, to form a fiber web.

[0089] (Step of forming temporary fusion sheet) The surface temperatures of the obtained nonwoven web were set to 170°C for a pair of upper and lower heated flat rolls, and the linear pressure of the flat rolls was set to 539 N / cm. The fiber web was passed through the pair of upper and lower rolls to bring the heated surfaces into contact with both sides of the fiber web, thereby forming a provisionally fused sheet.

[0090] (Step of forming intertwined sheet) The obtained pre-fused sheet was then sewn with a needle depth of 9 mm and 68 needles / cm on both sides. 2 The mixture was needle punched under the above conditions to obtain an entangled sheet.

[0091] (Process for heat fusing the interlaced sheet) The obtained interlaced sheet was heat-fused using a pair of engraved rolls with a fused area ratio of 10%. The surface temperatures of the upper and lower embossing rolls were both set to 200°C, and the linear pressure of the embossing rolls was set to 686 N / cm, resulting in a basis weight of 160 g / m. 2 The physical properties of the obtained nonwoven fabric are shown in Table 1.

[0092] [Example 2] (The process of forming fibers) The polyester resin A and the polyester resin B were melted at temperatures of 295° C. and 280° C., respectively. Thereafter, the polyester resin A was used as a core component and the polyester resin B was used as a sheath component, and the core:sheath mass ratio was 80:20, and the spinneret temperature was set to 295° C., and the polyester resins were spun from a circular extrusion hole. The spun polyester resins A and B were then suction-drawn by an ejector at a spinning speed of 4,500 m / min, to form a fiber that was a concentric core-sheath type composite fiber. (Step of forming a fiber web) The obtained fibers were sprayed from a fiber-spreading plate to control the fiber arrangement, and the fibers were collected on a moving net conveyor whose moving speed was adjusted so that the basis weight of the obtained nonwoven fabric was 5% or less of the target basis weight, to form a fiber web. (Step of forming temporary fusion sheet) The surface temperatures of the obtained nonwoven web were set to 150°C for a pair of upper and lower heated flat rolls, and the linear pressure of the flat rolls was set to 539 N / cm. The nonwoven web was passed through the pair of upper and lower rolls to bring the heated surfaces into contact with both sides of the fibrous web, thereby forming a provisionally fused sheet. (Step of forming intertwined sheet) The obtained pre-fused sheet was placed on the front and back of the machine with a needle depth of 9 mm and 68 needles / cm on each side. 2 The mixture was needle punched under the above conditions to obtain an entangled sheet. (Process for heat fusing the interlaced sheet) The obtained interlaced sheet was heat-fused using a pair of engraved rolls with a fused area ratio of 10%. The surface temperatures of the upper and lower embossing rolls were both set to 200°C, and the linear pressure of the embossing rolls was set to 686 N / cm, resulting in a basis weight of 160 g / m. 2 The physical properties of the obtained nonwoven fabric are shown in Table 1.

[0093] [Example 3] A long-fiber nonwoven fabric was obtained under the same conditions as in Example 1, except that in the step of heat-fusing the entangled sheet, the area ratio of the fused parts was changed from 10% to 18%, and the surface temperature of the embossing roll was changed from 200° C. to 210° C. The physical properties of the obtained nonwoven fabric are shown in Table 1.

[0094] [Example 4] (The step of forming a fiber web) The basis weight of the obtained nonwoven fabric is 160 g / m 2 The speed of the net conveyor was adjusted to achieve a weight of 180g / m 2 A long-fiber nonwoven fabric was obtained under the same conditions as in Example 1, except that the moving speed of the net conveyor was adjusted so as to satisfy the following: The physical properties of the obtained nonwoven fabric are shown in Table 1.

[0095] [Example 5] (The step of forming a fiber web) The basis weight of the obtained nonwoven fabric is 160 g / m 2 The speed of the net conveyor was adjusted to achieve a weight of 130 g / m 2 A long-fiber nonwoven fabric was obtained under the same conditions as in Example 1, except that the moving speed of the net conveyor was adjusted so as to satisfy the following: The physical properties of the obtained nonwoven fabric are shown in Table 1.

[0096] [Table 1]

[0097] [Comparative Example 1] Except for not carrying out the step of heat-sealing the entangled sheet, a long-fiber nonwoven fabric was obtained under the same conditions as in Example 1. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0098] [Comparative Example 2] After (the step of forming an entangled sheet), a long-fiber nonwoven fabric was obtained under the same conditions as in Comparative Example 1, except that holes were made in an amount corresponding to 10% of the area of ​​the fused parts in Example 1. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0099] [Comparative Example 3] Except for not carrying out the step of forming an entangled sheet, a long-fiber nonwoven fabric was obtained under the same conditions as in Example 1. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0100] [Comparative Example 4] Except for not carrying out the step of forming an entangled sheet, a long-fiber nonwoven fabric was obtained under the same conditions as in Example 2. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0101] [Comparative Example 5] A long-fiber nonwoven fabric was obtained under the same conditions as in Example 1, except that in the step of heat-sealing the entangled sheet, the linear pressure applied to the fiber web was changed from 686 N / cm to 250 N / cm. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0102] [Comparative Example 6] A long-fiber nonwoven fabric was obtained under the same conditions as in Example 1, except that in the step of heat-sealing the entangled sheet, the area ratio of the fused parts was changed from 10% to 30%. The physical properties of the obtained nonwoven fabric are shown in Table 2.

[0103] [Table 2]

[0104] The characteristics of the obtained nonwoven fabrics are as shown in Tables 1 and 2. The nonwoven fabrics of Examples 1 to 5 had low penetration resistance, moisture retention, and abrasion resistance, and exhibited excellent properties as covering sheets such as seedling sheets.

[0105] On the other hand, the nonwoven fabrics of Comparative Examples 1 to 6 had high penetration resistance (Comparative Examples 1 to 6), low moisture retention, and poor abrasion resistance (Comparative Examples 1 and 2). [Explanation of symbols]

[0106] 1: Fusion part 2: Non-fused part 3:Non-woven fabric 4: Fusion section (parallelogram) 5: Tangent line of fusion part in MD direction 6: Tangent line of fused part in CD direction 7: Fusion part (rectangle) 8: Fusion part (diamond)

Claims

1. A long-fiber nonwoven fabric made of fibers mainly composed of thermoplastic resin and having fused portions and non-fused portions, the fused portions having an area ratio of 5% or more and 25% or less, and a thickness T NE (μm) vs. thickness T E Ratio T (μm) E / T NE is 0.05 or more and 0.15 or less, and the apparent density of the long fiber nonwoven fabric is 0.10 g / cm 3 0.25g / cm or more 3 The following is a long fiber nonwoven fabric.

2. The maximum tensile stress σ of the long fiber nonwoven fabric max The tensile stress σ of the long fiber nonwoven fabric at 3% elongation (N / 5 cm) 3% Ratio σ of (N / 5cm) 3% / σ max The long-fiber nonwoven fabric according to claim 1, wherein the linear modulus is 0.80 or more and 0.97 or less.

3. The thickness T of the non-fused portion NE 3. The long-fiber nonwoven fabric according to claim 1, wherein (μm) is 800 μm or more and 1500 μm or less.

4. The length T of the long side of the fused portion L (μm) vs. the length T of the short side of the fused portion S Ratio T (μm) S / T L The long-fiber nonwoven fabric according to claim 1 or 2, wherein the linear modulus is 0.10 or more and 0.80 or less.

5. The fused portion has a plurality of fused portions, and the average shortest distance T between the fused portions B (μm) vs. the length T of the short side of the fused portion S Ratio T (μm) S / T B The long-fiber nonwoven fabric according to claim 1 or 2, wherein the linearity is 0.01 or more and 0.30 or less.

6. The weight of the long fiber nonwoven fabric is 100 g / m 2 More than 200g / m 23. The long-fiber nonwoven fabric according to claim 1 or 2, wherein:

7. A step of spinning a thermoplastic resin through an outlet hole of a spinneret and drawing the resin by suction to form a fiber; collecting the fibers on a moving net conveyor to form a fibrous web; a step of contacting both sides of the fiber web with a heating surface to perform primary fusion to form a temporarily fused sheet; a step of mechanically entangling the pre-fused sheet to form an entangled sheet; a step of heat fusing the entangled sheet with a pair of rolls; The method for producing a long-fiber nonwoven fabric according to claim 1 or 2, further comprising the steps of: The spinning speed in the suction drawing is 3000 m / min or more and 6000 m / min or less, The temperature of the heating surface during the primary fusion is 60° C. or more and 120° C. or less lower than the melting point of the thermoplastic resin, and the linear pressure of the heating surface is 100 N / cm or more and 900 N / cm or less, The surface temperature of the pair of rolls during the heat fusion is 5° C. to 70° C. lower than the melting point, and the linear pressure of the pair of rolls is 100 N / cm to 900 N / cm. A method for producing long fiber nonwoven fabric.

Citation Information

Patent Citations

  • Agricultural covering material

    JP2015223152A

Cited By

  • Long-fiber nonwoven fabric and production method therefor

    WO2025115585A1