Photosensitive resin composition, photosensitive film, cured product, and electronic component using them

The photosensitive resin composition allows for efficient coating and selective removal of unexposed areas using photolithography, addressing the complexity of existing methods and enhancing the reliability of electronic components.

JP2024138806AInactive Publication Date: 2024-10-09TORAY INDUSTRIES INC

Patent Information

Application Number
JP2023049502
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing methods for covering multiple elements on a substrate with a film-like material require complicated laser removal processes, complicating the coating process.

Method used

A photosensitive resin composition comprising an acrylic resin, a cationically polymerizable compound, a thermal cationic polymerization initiator, and a photocationic polymerization initiator, allowing for selective removal of unexposed areas through photolithography.

Benefits of technology

Facilitates simultaneous coating of multiple elements on a substrate and improves processing yield by enabling precise removal of unexposed resin areas, resulting in electronic components with enhanced reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138806000001
    Figure 2024138806000001
  • Figure 2024138806000002
    Figure 2024138806000002
  • Figure 2024138806000003
    Figure 2024138806000003
Patent Text Reader

Abstract

To provide a photosensitive resin composition which is excellent in coating property of an element, and can remove a part of a coating part by photolithography, a photosensitive film and a cured product using the same, and an electronic component using them.SOLUTION: A photosensitive resin composition contains (a) an acrylic resin, (b) a cationic polymerizable compound, (c) a thermal cationic polymerization initiator, and (d) a photo-cationic polymerization initiator, where (a) the acrylic resin contains (a1) an acrylic resin having a glass transition temperature of -40°C or higher and 30°C or lower, and (a2) an acrylic resin having a glass transition temperature of 60°C or higher and 110°C or lower.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a photosensitive resin composition, a photosensitive film, a cured product, and an electronic part using these. [Background technology]

[0002] Conventionally, package formats such as dual in-line package (DIP), small outline package (SOP), and quad flat package (QFP) have been used as semiconductor integrated circuit (IC) packages. On the other hand, in recent years, packages have become smaller and more highly integrated, and CSP (chip size package) in which the IC chip package size is equivalent to the chip size has been adopted. In addition, due to the demand for smaller and thinner ICs, the method of connecting the IC and package terminals has changed from the gold wire used in the past to flip chip connection, which connects the active surface of the IC to the connection terminals with solder balls or gold bumps.

[0003] On the other hand, quartz crystal devices, such as quartz crystal resonators and SAW filters, are used for the synchronization reference signal of various ICs, clocks, and noise filters in communication circuits by applying the piezoelectric phenomenon to electric circuits. Since quartz crystal devices convert electric signals into physical vibrations and vice versa, the active surface of the element must exist in space, and these elements must be packaged in a hollow structure. In the past, to protect the element from the external environment, the element was placed in an embossed laminated ceramic, the element and the electrodes were connected by wire bonding, and the metal sealing was performed by sealing with metal welding. However, with the miniaturization and thinning of communication devices, such as mobile phones, a method has been proposed in which the active surface of the element and the package substrate are flip-chip connected, the space formed by the element, bumps, and package substrate is maintained, and resin sealing is performed in a hollow structure. As a resin sealing method for this purpose, there have been proposed a method in which uneven parts formed by mounting an element on a substrate are filled with a film-like sealing material while maintaining the space formed by the element-bump-package substrate, and a method in which a film-like material is made to conform to the uneven shape formed by mounting the electronic components to cover and protect the electronic components (Patent Documents 1 to 3).

[0004] Furthermore, in recent years, electronic component modules have been proposed that integrate electronic components that were previously manufactured separately and are given functionality. A method has been proposed for electronic component modules in which multiple elements are arranged on a substrate and these elements are collectively covered with a film-like material (Patent Document 4). [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4053483 [Patent Document 2] Patent No. 4730652 [Patent Document 3] JP 2003-17979 A [Patent Document 4] Patent No. 6089567 Summary of the Invention [Problem to be solved by the invention]

[0006] Although it is possible to cover multiple elements arranged on a substrate, such as an electronic component module, with a film-like material all at once, when connecting part of the element to an electrode after covering, the covering film material must be removed with a laser, making the process complicated.

[0007] The present invention has been made in consideration of the above circumstances, and aims to provide a photosensitive resin composition that has excellent element coverage and allows part of the coverage to be removed by photolithography, a photosensitive film and cured product using the same, and electronic components using these. [Means for solving the problem]

[0008] In order to solve the above problems, the present invention has the following configuration. (1) A composition comprising (a) an acrylic resin, (b) a cationic polymerizable compound, (c) a thermal cationic polymerization initiator, and (d) a photo-cationic polymerization initiator, The (a) acrylic resin is a photosensitive resin composition including (a1) an acrylic resin having a glass transition temperature of -40°C or more and 30°C or less, and (a2) an acrylic resin having a glass transition temperature of 60°C or more and 110°C or less. (2) The photosensitive resin composition according to (1) above, wherein the (a1) acrylic resin has a weight average molecular weight of 600,000 or more and 1,800,000 or less. (3) The photosensitive resin composition according to (1) or (2), wherein the (a2) acrylic resin has a weight average molecular weight of 10,000 or more and 100,000 or less. (4) The photosensitive resin composition according to any one of (1) to (3), comprising the (a1) acrylic resin in an amount of 10 mass % or more and 30 mass % or less based on 100 mass % of the total of all components excluding the solvent. (5) The photosensitive resin composition according to any one of (1) to (4) above, wherein the (a2) acrylic resin is contained in an amount of 15% by mass or more and 45% by mass or less based on 100% by mass of the total of all components excluding the solvent. (6) The photosensitive resin composition according to any one of (1) to (5), wherein the ratio of the content (by mass) of the (c) thermal cationic polymerization initiator to the content (by mass) of the (d) photo cationic polymerization initiator is 0.1 or more and 1 or less. (7) The photosensitive resin composition according to any one of (1) to (6) above, further comprising (e) a radically polymerizable compound. (8) The photosensitive resin composition according to (7) above, further comprising (f) a radical polymerization initiator. (9) A photosensitive film comprising the photosensitive resin composition according to any one of (1) to (8). (10) A cured product obtained by curing the photosensitive resin composition according to any one of (1) to (8) above or the photosensitive film according to (9) above. (11) An electronic part comprising the cured product according to (10) above. Effect of the Invention

[0009] By using the photosensitive resin composition of the present invention, it is possible to collectively cover a plurality of elements arranged on a substrate, and after covering, to remove the unexposed portions of the photosensitive resin composition by photolithography, thereby improving the yield in the processing step and obtaining electronic components with excellent reliability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The photosensitive resin composition, photosensitive film, cured product, and electronic parts using these of the present invention will be described in detail below. However, the present invention is not limited to the following embodiments, and can be modified in various ways depending on the purpose and application.

[0011] The present invention relates to a composition for producing a polymerizable composition comprising: (a) an acrylic resin; (b) a cationic polymerizable compound; (c) a thermal cationic polymerization initiator; and (d) a photocationic polymerization initiator, The (a) acrylic resin is a photosensitive resin composition containing (a1) acrylic resin having a glass transition temperature of -40°C or more and 30°C or less, and (a2) acrylic resin having a glass transition temperature of 60°C or more and 110°C or less.

[0012] <Photosensitive resin composition> The photosensitive resin composition of the present invention contains (a) an acrylic resin, (b) a cationically polymerizable compound, (c) a thermal cationic polymerization initiator, and (d) a photocationic polymerization initiator.

[0013] The (a) acrylic resin includes (a1) acrylic resin having a glass transition temperature of -40°C or more and 30°C or less, and (a2) acrylic resin having a glass transition temperature of 60°C or more and 110°C or less.

[0014] (b) The cationically polymerizable compound is a compound having cationically polymerizable properties.

[0015] (c) The thermal cationic polymerization initiator is a compound that generates an acid directly or indirectly by heat and causes cationic polymerization.

[0016] (d) The photocationic polymerization initiator is a compound that generates an acid directly or indirectly when exposed to light, thereby causing cationic polymerization.

[0017] The photosensitive resin composition of the present invention contains the (a1) acrylic resin, which makes the photosensitive resin composition easy to handle before processing, and enables the photosensitive resin composition to conform to and cover the uneven shape formed by a plurality of elements arranged on a substrate.

[0018] The photosensitive resin composition of the present invention contains the acrylic resin (a2), which increases the storage modulus of the photosensitive resin composition and makes it possible to suppress breakage during processing to conform to uneven shapes.

[0019] The photosensitive resin composition of the present invention contains (a) an acrylic resin, (b) a cationic polymerizable compound, and (d) a photocationic polymerization initiator, and is soluble in a developer before exposure. However, upon exposure, an acid is generated from the photocationic polymerization initiator, and the cationic polymerization reaction of the cationic polymerizable compound proceeds, and the cationic polymerizable compound in the exposed area becomes a crosslinked structure. This makes the exposed area insoluble in the developer, and it becomes possible to remove only the unexposed area with the developer. Furthermore, by containing (c) a thermal cationic polymerization initiator, the storage modulus of the cured product obtained by heat curing the photosensitive resin composition of the present invention is increased, and a cured product with excellent heat resistance can be obtained.

[0020] The thickness of the photosensitive resin composition of the present invention is preferably 10 μm or more because the strength of the photosensitive resin composition is insufficient if it is too thin, and is preferably 200 μm or less because the ability to follow uneven shapes is reduced if it is too thick. Furthermore, from the viewpoint of developability during processing by photolithography, the thickness is more preferably 10 μm or more and 50 μm or less.

[0021] <Acrylic resin> The photosensitive resin composition of the present invention contains (a) an acrylic resin, and the (a) acrylic resin contains (a1) an acrylic resin having a glass transition temperature of -40°C or more and 30°C or less.

[0022] The photosensitive resin composition of the present invention is easy to handle at room temperature when the glass transition temperature of the (a1) acrylic resin is in the range of -40°C to 30°C. The glass transition temperature of the (a1) acrylic resin is more preferably in the range of -20°C to 20°C.

[0023] If the glass transition temperature of the (a1) acrylic resin is less than -40°C, the tack of the photosensitive resin composition of the present invention will be large, which is undesirable since there is a risk of peeling failure occurring when peeling a support or a protective film from the photosensitive film. Also, if the glass transition temperature of the (a1) acrylic resin is more than 30°C, the toughness of the photosensitive resin composition of the present invention will be reduced, which is undesirable since there is a risk of cracking during handling at room temperature.

[0024] The (a1) acrylic resin preferably has a weight-average molecular weight of 600,000 or more and 1,800,000 or less. This allows the resin to have high strength and flexibility when formed into a film, and good handleability. It also allows the resin to exhibit good elongation when processed to conform to uneven shapes. The (a1) acrylic resin more preferably has a weight-average molecular weight of 600,000 or more and 1,400,000 or less.

[0025] The photosensitive resin composition of the present invention preferably contains 10% by mass or more and 30% by mass or less of (a1) acrylic resin in the total of 100% by mass of all components excluding the solvent. By containing 10% by mass or more and 30% by mass or less of (a1) acrylic resin in 100% by mass of the photosensitive resin composition, even if the acrylic resin has a large weight average molecular weight and is difficult to dissolve in a developer, the removability of the unexposed portion of the photosensitive resin composition by photolithography is good. The content of (a1) acrylic resin in 100% by mass of the photosensitive resin composition is more preferably 15% by mass or more and 30% by mass or less.

[0026] The (a1) acrylic resin suitable for the acrylic resin is preferably a polymer having at least two functional groups selected from the group consisting of an epoxy group, a cyano group, a hydroxyl group, an amino group, a hydroxyalkyl group, and a carboxyl group, and further including an acrylic acid ester having a side chain with 1 to 5 carbon atoms and / or a methacrylic acid ester having a side chain with 1 to 5 carbon atoms as a constituent monomer.

[0027] Examples of acrylic acid esters having a side chain with 1 to 5 carbon atoms and methacrylic acid esters having a side chain with 1 to 5 carbon atoms include alkyl acrylic acid esters and alkyl methacrylic acid esters such as methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, butyl acrylate, butyl methacrylate, pentyl acrylate, pentyl methacrylate, as well as alicyclic alcohol esters of acrylic acid and methacrylic acid such as cyclopentyl acrylate and cyclopentyl methacrylate, vinyl acetate, vinylidene chloride, ethyl α-acetoxyacrylate, etc. These acrylic acid esters and methacrylic acid esters can be used alone or in combination.

[0028] In the photosensitive resin composition of the present invention, the (a1) acrylic resin may be used alone or in combination of two or more kinds.

[0029] The photosensitive resin composition of the present invention contains (a2) an acrylic resin having a glass transition temperature of 60°C or higher and 110°C or lower.

[0030] (a2) When the glass transition temperature of the acrylic resin is 60°C or higher and 110°C or lower, the storage modulus of the photosensitive resin composition of the present invention is increased, and breakage of the photosensitive resin composition during processing to conform to an uneven surface can be suppressed.

[0031] If the glass transition temperature of the (a2) acrylic resin is less than 60° C., the contribution to increasing the storage modulus of the photosensitive resin composition of the present invention is small, and the photosensitive resin composition may be torn when processed to conform to the uneven shape, which is undesirable. Also, if the glass transition temperature of the (a2) acrylic resin is more than 110° C., the compatibility with the (a1) acrylic resin decreases, and separation of the (a2) acrylic resin occurs in the photosensitive resin composition, which is undesirable, and therefore the photosensitive film may not be uniform.

[0032] The (a2) acrylic resin preferably has a weight-average molecular weight of 10,000 or more and 100,000 or less. This makes it possible to suppress swelling caused by a developer when removing the unexposed parts of the photosensitive resin composition of the present invention by photolithography, and to remove the resin in the unexposed parts with higher resolution. The (a2) acrylic resin more preferably has a weight-average molecular weight of 30,000 or more and 80,000 or less.

[0033] The photosensitive resin composition of the present invention preferably contains 15% by mass or more and 45% by mass or less of (a2) acrylic resin in a total of 100% by mass of all components excluding the solvent. By containing 15% by mass or more and 45% by mass or less of (a2) acrylic resin in 100% by mass of the photosensitive resin composition, the storage modulus of the photosensitive resin composition can be increased, and the strength and flexibility of the photosensitive resin composition when made into a film are high, resulting in good handleability.

[0034] The acrylic resin suitable for the (a2) acrylic resin is preferably a polymer containing a methacrylic acid ester having a side chain with 1 to 5 carbon atoms as a constituent monomer. More specifically, the (a2) acrylic resin means a polymer containing a methacrylic acid ester having a side chain with 1 to 5 carbon atoms as a constituent monomer, and not corresponding to the (a1) acrylic resin. In other words, a polymer containing a methacrylic acid ester having a side chain with 1 to 5 carbon atoms as a constituent monomer and satisfying the condition of the (a1) acrylic resin is classified as the (a1) acrylic resin, and a polymer containing a methacrylic acid ester having a side chain with 1 to 5 carbon atoms as a constituent monomer and not corresponding to the (a1) acrylic resin is classified as the (a2) acrylic resin. As the (a2) acrylic resin, a polymer containing both methyl methacrylate having 1 to 2 carbon atoms and ethyl methacrylate having 1 to 2 carbon atoms as constituent monomers is more preferable from the viewpoint of increasing the glass transition temperature.

[0035] In the photosensitive resin composition of the present invention, the (a2) acrylic resin may be used alone or in combination of two or more kinds.

[0036] <Cationic polymerizable compound> The photosensitive resin composition of the present invention contains (b) a cationic polymerizable compound. Examples of such cationic polymerizable compounds include epoxy resins, vinyl ether resins, and oxetane resins. Although the (b) cationic polymerizable compound is not particularly limited, it is preferably an epoxy resin.

[0037] The epoxy resin is not particularly limited as long as it has two or more epoxy groups in one molecule, and examples thereof include diglycidyl ethers such as bisphenol A, bisphenol F, bisphenol S, resorcinol, dihydroxynaphthalene, and dicyclopentadiene diphenol, epoxidized phenol novolac (phenol novolac type epoxy resin), epoxidized cresol novolac (cresol novolac type epoxy resin), epoxidized trisphenylol methane, epoxidized tetraphenylol ethane, epoxidized metaxylene diamine, and cyclohexane diepoxide. Furthermore, in order to impart flame retardancy, a halogenated epoxy resin, particularly a brominated epoxy resin, may be used. These may be used alone or in combination of two or more.

[0038] Specific examples of compounds having an epoxy group include "Epicron" (registered trademark) 850-S, "Epicron" HP-4032, "Epicron" HP-7200, "Epicron" HP-820, "Epicron" HP-4700, "Epicron" EXA-4710, "Epicron" HP-4770, "Epicron" EXA-859CRP, and "Epicron" EXA-1 514, "Epicron" EXA-4880, "Epicron" EXA-4850-150, "Epicron" EXA-4850-1000, "Epicron" EXA-4816, "Epicron" EXA-4822 (all trade names, manufactured by Dainippon Ink and Chemicals, Inc.), "Rikaresin" (registered trademark) BEO-60E, "Rikaresin" BPO-20E, "Rikaresin" HBE-1 00, "RIKARESIN" DME-100 (all trade names, manufactured by Shin Nippon Rika Co., Ltd.), EP-4003S, EP-4000S (all trade names, manufactured by ADEKA Corporation), PG-100, CG-500, EG-200 (all trade names, manufactured by Osaka Gas Chemicals Co., Ltd.), NC-3000, NC-6000 (all trade names, manufactured by Nippon Kayaku Co., Ltd.), "EPOX" (registered trademark)-MKR508, "E Examples of such products include POX"-MKR540, "EPOX"-MKR710, "EPOX"-MKR1710, VG3101L, VG3101M80 (all trade names, manufactured by Printec Co., Ltd.), "Celloxide" (registered trademark) 2021P, "Celloxide" 2081, "Celloxide" 2083, and "Celloxide" 2085 (all trade names, manufactured by Daicel Chemical Industries, Ltd.).

[0039] The photosensitive resin composition of the present invention preferably contains, as the (b) cationic polymerizable compound, an epoxy resin having an epoxy equivalent of 150 or more and 300 or less. This enables the epoxy resin to form a high-density crosslinked structure in the exposed area, and the resin in the unexposed area can be removed with higher precision by photolithography.

[0040] <Thermal cationic polymerization initiator> The photosensitive resin composition of the present invention contains (c) a thermal cationic polymerization initiator. As such a thermal cationic polymerization initiator, any known compound can be used without any particular limitation. Specifically, For example, aromatic iodonium complex salts and aromatic sulfonium complex salts can be mentioned. Specific examples of aromatic iodonium complex salts include diphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, di(4-nonylphenyl)iodonium hexafluorophosphate, etc. These thermal cationic polymerization initiators may be used alone or in combination of two or more kinds.

[0041] The photosensitive resin composition of the present invention contains the thermal cationic polymerization initiator (c), so that the photosensitive resin composition of the present invention can be heat-cured at a low temperature to form a cured product. The low temperature referred to here is a temperature of 100°C or higher but lower than 150°C.

[0042] The photosensitive resin composition of the present invention preferably contains (c) a thermal cationic polymerization initiator such that the ratio of the content (mass basis) of the (c) thermal cationic polymerization initiator to the content (mass basis) of the (d) photocationic polymerization initiator is 0.1 or more and 1 or less. This allows the cationic polymerizable compound to exhibit sufficient curability, and the storage modulus of the cured product obtained by heat-curing the photosensitive resin composition of the present invention is increased, thereby enabling a cured product with excellent heat resistance to be obtained.

[0043] <Photocationic polymerization initiator> The photosensitive resin composition of the present invention contains (d) a photocationic polymerization initiator. As such a photocationic polymerization initiator, a known compound can be used without any particular limitation. Specific examples thereof include aromatic iodonium complex salts and aromatic sulfonium complex salts. Specific examples of aromatic iodonium complex salts include diphenyliodonium tetrakis(pentafluorophenyl)borate, diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, and di(4-nonylphenyl)iodonium hexafluorophosphate. These (d) photocationic polymerization initiators may be used alone or in combination of two or more.

[0044] The photosensitive resin composition of the present invention preferably contains 0.3 parts by mass or more, more preferably 0.5 parts by mass or more, and even more preferably 0.7 parts by mass or more of the photocationic polymerization initiator (d) relative to 100 parts by mass of the cationically polymerizable compound (b). This allows the cationically polymerizable compound to exhibit sufficient curability, improves the crosslink density of the exposed area, and enables the resin in the unexposed area to be removed with higher resolution by photolithography.

[0045] <Radical polymerizable compound> The photosensitive resin composition of the present invention further contains (e) a radical polymerizable compound, and thus the storage modulus of the cured product obtained by curing the photosensitive resin composition of the present invention with light and / or heat is increased, and a cured product having excellent heat resistance can be obtained. Examples of such radical polymerizable compounds include unsaturated double bond functional groups such as vinyl groups, allyl groups, acryloyl groups, and methacryloyl groups, and / or unsaturated triple bond functional groups such as propargyl groups, and among these, conjugated vinyl groups, acryloyl groups, and methacryloyl groups are preferred in terms of polymerizability. In addition, since cracks occur in the pattern when there are many crosslinking points due to the polymerization reaction, the number of functional groups contained is preferably 1 to 6, and each functional group does not have to be the same group.

[0046] The photosensitive resin composition of the present invention preferably contains 5% by mass or more and 40% by mass or more of the radical polymerizable compound (e) in 100% by mass of the photosensitive resin composition. The content of the radical polymerizable compound (e) in 100% by mass of the photosensitive resin composition is more preferably 10% by mass or more and 35% by mass or less. This increases the storage modulus of the cured product obtained by photo- and / or heat-curing the photosensitive resin composition of the present invention, and allows the production of a cured product with excellent heat resistance.

[0047] The (e) radically polymerizable compound is preferably an acrylic monomer, such as an acrylic acid ester, a methacrylic acid ester, an acrylamide, or a methacrylamide.

[0048] Preferred examples of the acrylic monomer include NK Ester series AM-90G, AM-130G, AM-230G, AMP-20GY, A-LEN-10, A-SA, M-20G, M-40G, M-90G, M-130G, M-230G, M-450G, PHE-1G, SA, HD-N, NOD-N, DOD-N, NPG, 701, 2G, 3G, 4G, 9G, 14G, 23G, 9PG, DCP, BPE-80N, BPE-100, BPE-200, BPE-500, BPE-1300N, TMPT, A-200, A-400, A-600, A-H, and the like manufactured by Shin-Nakamura Chemical Co., Ltd. D-N, A-NOD-N, A-DOD-N, APG-200, APG-400, APG-700, A-PTMG65, A-DCP, ABE-300, A-BPE-4, A-BPE-10, A-BPE-20, 701A, A-TMPT, A-TMPT-9EO, AT-20E, A-GLY -3E, A-GLY-9E, A-GLY-20E, A-9300, A-9200YN, A-TMM-3, A-TMM-3L, A-TMM-3, A-TMM-3LM-N, A-TMMT, ATM-35E, ATM-4P, A-DPH, A-9550, A-DPH-12E, etc. In addition, Kyoeisha Chemical Co., Ltd.'s Light Acrylate Series 1AA, LA, SA, EC-A, MTG-A, EHDG-AT, 130A, DPM-A, PO-A, P2H-A, P-200A, THF-A, IB-XA, HOA(N), HOP-A(N), HOB-A, M-600A, HOA-MS(N), HOA-HH(N), HOA-MPL(N) ), HOA-MPE(N), BA-104, P-1A, 3EG-A, 4EG-A, 9EG-A, 14EG-A, PTMGA-250, NP-A, MPD-A, 1.6HX -A, 1.9ND-A, DCP-A, BP-4EAL, BP-4PA, HPP-A, BP-6EM, TMP-A, PE-3A, PE-4A, DPE-6A, etc.Further examples of the light ester series manufactured by Kyoeisha Chemical Co., Ltd. include E, NB, IB, TB, EH, ID, L, L-7, S, BC, 130MA, 041MA, CH, THF(1000), BZ, PO, IB-X, HO-250(N), HOP(N), HOA(N), HOP-A(N), HOB(N), DM, DE, HO-MS-(N), EG, 2EG, 3EG, 4EG, 9EG, 14EG, 1.4BG, NP, 1.6HX, 1.9ND, G-101P, G-201P, BP-2EMK, and TMP. Further examples include M-101A, M-113, M-120, M-140, M-208, M-211B, M-215, M-220, M-225, M-240, M-305, M-309, M-315, M-321, M-321, M-350, M-400, M-402, M-408, M-450, etc., of the "Aronix (registered trademark)" series manufactured by Toagosei Co., Ltd. These compounds may be contained alone or in combination of two or more kinds.

[0049] (d1) The acrylic monomer is more preferably one having two or less acryloyl groups in one molecule.Specific examples thereof include NK Ester series AM-90G, AM-130G, AM-230G, AMP-20GY, A-LEN-10, A-SA, M-20G, M-40G, M-90G, M-130G, M-230G, M-450G, PHE-1G, SA, HD-N, NOD-N, DOD-N, NPG, 701, 2G, 3G, 4G, 9G, 14G, 23G, 9PG, DCP, and BP manufactured by Shin-Nakamura Chemical Co., Ltd. Examples include E-80N, BPE-100, BPE-200, BPE-500, BPE-1300N, A-200, A-400, A-600, A-HD-N, A-NOD-N, A-DOD-N, APG-200, APG-400, APG-700, A-PTMG65, A-DCP, ABE-300, A-BPE-4, A-BPE-10, A-BPE-20, 701A, A-9300, and A-9200YN. Further examples include the Light Acrylate Series manufactured by Kyoeisha Chemical Co., Ltd.: 3EG-A, 4EG-A, 9EG-A, 14EG-A, TMGA-250, NP-A, MPD-A, 1.6HX-A, BEPG-A, 1.9ND-A, MOD-A, DCP-A, BP-4EA, BP-4PA, BA-134, BP-10EA, and HPP-A. Further examples include Kyoeisha Chemical Co., Ltd.'s Light Ester Series E, NB, IB, TB, EH, ID, L, L-7, S, BC, 130MA, 041MA, CH, THF(1000), BZ, PO, IB-X, HO-250(N), HOP(N), HOA(N), HOP-A(N), HOB(N), DM, DE, HO-MS-(N), EG, 2EG, 3EG, 4EG, 9EG, 14EG, 1.4BG, NP, 1.6HX, 1.9ND, G-101P, G-201P, and BP-2EMK. Further examples include M-101A, M-113, M-120, M-140, M-208, M-211B, M-215, M-220, M-225, and M-240 in the "Aronix (registered trademark)" series manufactured by Toagosei Co., Ltd.

[0050] In the photosensitive resin composition of the present invention, the (e) radically polymerizable compound may be used alone or in combination of two or more kinds.

[0051] The (e) radically polymerizable compound described herein refers to a compound having a molecular weight of 100 or more and 2000 or less, having an unsaturated double bond functional group and / or an unsaturated triple bond functional group, and not corresponding to the (b) cationic polymerizable compound.

[0052] <Radical polymerization initiator> The photosensitive resin composition of the present invention may further contain (f) a radical polymerization initiator. The radical polymerization initiator generates radicals directly or indirectly by light and / or heat, thereby causing radical polymerization.

[0053] As such a (f) radical polymerization initiator, which generates radicals by light, a combination of compounds selected from benzophenones, glycines, mercaptos, oximes, benzyl dimethyl ketals, α-hydroxyalkylphenones, α-aminoalkylphenones, acylphosphine oxides, and 2,2'-bis(o-chlorophenyl)-4,4',5,5'-tetraphenylbiimidazole is preferred.

[0054] As such a radical polymerization initiator (f), examples of initiators that generate radicals by heat include organic peroxides and azo compounds. Specific examples include ketone peroxides, peroxyketals, hydroperoxides, dialkyl peroxides, diacyl peroxides, peroxyesters, peroxydicarbonates, azo compounds, and the like. Among these, organic peroxides are preferred. Organic peroxides are preferred because they are less likely to inhibit the cationic polymerization reaction.

[0055] In the present invention, it is more preferable that the photosensitive resin composition contains (e) a radical polymerizable compound and (f) a radical polymerization initiator.

[0056] <Other Ingredients> The photosensitive resin composition of the present invention may further contain additives, such as a polymerization inhibitor, a sensitizer, a surfactant, a silane coupling agent, a titanium chelating agent, a filler, an organic solvent, an ion scavenger, a flame retardant, a colorant, a dissolution regulator, a stabilizer, or an antifoaming agent, as necessary.

[0057] The photosensitive resin composition of the present invention further contains a polymerization inhibitor, which adjusts the exciton concentration, thereby suppressing excessive photoresponse and widening the exposure margin. As the polymerization inhibitor, a basic compound, an aromatic polyol compound, a quinone compound, a hindered phenol compound, etc. can be used.

[0058] The basic compound is a compound that can act as a proton acceptor, i.e., a compound having an unshared electron pair. Specific examples of the basic compound include compounds containing atoms such as nitrogen, sulfur, and phosphorus, and among these, nitrogen-containing compounds are preferred.

[0059] Particularly preferred examples of the nitrogen-containing compound include amine compounds, specifically tertiary amines such as triphenylamine, triethanolamine, triisopropanolamine, N,N-diethyl-3-aminophenol, N-ethyldiethanolamine, and 2-diethylaminoethanol, secondary amines such as diethanolamine, diisopropanolamine, and N-methylbenzylamine, pyrimidine compounds such as pyrimidine, 2-aminopyrimidine, 4-aminopyrimidine, and 5-aminopyrimidine, and derivatives thereof, pyridine compounds such as pyridine, methylpyridine, and 2,6-dimethylpyridine, and derivatives thereof, and aminophenols such as 2-aminophenol and 3-aminophenol, and derivatives thereof.

[0060] Furthermore, these basic substances may be used alone or in combination of two or more kinds.

[0061] The photosensitive resin composition of the present invention may use a sensitizer to absorb ultraviolet light and provide the absorbed light energy to the photocationic polymerization initiator. As the sensitizer, for example, an anthracene compound having an alkoxy group at the 9th and 10th positions (9,10-dialkoxy-anthracene derivative) is preferable. Examples of the alkoxy group include C1-C4 alkoxy groups such as methoxy, ethoxy, and propoxy. The 9,10-dialkoxy-anthracene derivative may further have a substituent. Examples of the substituent include halogen atoms such as fluorine, chlorine, bromine, and iodine atoms, C1-C4 alkyl groups such as methyl, ethyl, and propyl groups, sulfonic acid alkyl ester groups, and carboxylic acid alkyl ester groups. Examples of the alkyl in the sulfonic acid alkyl ester group and carboxylic acid alkyl ester group include C1-C4 alkyl groups such as methyl, ethyl, and propyl. The substitution position of these substituents is preferably the 2-position.

[0062] The photosensitive resin composition of the present invention can improve adhesion to a substrate by containing a surfactant, a silane coupling agent, a titanium chelating agent, or the like.

[0063] Specific examples of silane coupling agents include 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, N-phenyl-3-aminopropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropyltriethoxysilane, p-styryltrimethoxysilane, 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldieth ...triethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltriethoxysilane, 3-methacry Examples of the silane coupling agent include, but are not limited to, 3-methacryloxypropyltriethoxysilane, 3-acryloxypropyltrimethoxysilane, N-2(aminoethyl)3-aminopropylmethyldimethoxysilane, N-2(aminoethyl)3-aminopropyltrimethoxysilane, N-2(aminoethyl)3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, 3-ureidopropyltriethoxysilane, 3-mercaptopropylmethyldimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, etc. In the photosensitive resin composition of the present invention, the above silane coupling agents may be used alone or in combination of two or more.

[0064] The photosensitive resin composition of the present invention is not limited to the use of a filler. Examples of the filler include crystalline silica powder, fused silica powder, alumina, aluminum hydroxide, silicon nitride, magnesium hydroxide, calcium aluminate hydrate, zirconium oxide, zinc oxide, antimony trioxide, antimony pentoxide, titanium oxide, iron oxide, cobalt oxide, chromium oxide, talc, aluminum, gold, silver, nickel, iron, clay, and mica. Among them, aluminum hydroxide, alumina, and silica are preferred from the viewpoint of dispersibility. Among them, silica having a 5% weight loss temperature (thermal decomposition temperature) of 350° C. or higher by TGA (thermal weight loss measurement) is preferably used, preferably spherical silica powder, and more preferably fused spherical silica, from the viewpoint of reflow heat resistance.

[0065] In order to improve the wettability between the organic components in the resin composition used in the photosensitive resin composition of the present invention and the filler, the filler may be surface-treated with a silane coupling agent. Specific examples of the silane coupling agent include the above-mentioned silane coupling agents, which may be used alone or in combination of two or more.

[0066] The organic solvent in the present invention is preferably one that dissolves the photosensitive resin composition. Examples of such organic solvents include ethers, acetates, ketones, aromatic hydrocarbons, N-methyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, and γ-butyrolactone, and these may be used alone or in combination of two or more.

[0067] Examples of ethers include ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and ethylene glycol dibutyl ether. Examples of acetates include ethylene glycol monoethyl ether acetate, propylene glycol monomethyl ether acetate, propyl acetate, butyl acetate, isobutyl acetate, 3-methoxybutyl acetate, 3-methyl-3-methoxybutyl acetate, methyl lactate, ethyl lactate, and butyl lactate. Examples of ketones include acetone, methyl ethyl ketone, acetylacetone, methyl propyl ketone, methyl butyl ketone, methyl isobutyl ketone, cyclopentanone, and 2-heptanone. Examples of aromatic hydrocarbons include alcohols such as butyl alcohol, isobutyl alcohol, pentanol, 4-methyl-2-pentanol, 3-methyl-2-butanol, 3-methyl-3-methoxybutanol, and diacetone alcohol, toluene, and xylene.

[0068] The photosensitive resin composition of the present invention may further contain various additives, for example, ion scavengers such as antimony trioxide, antimony pentoxide, and hydrotalcite-based compounds, flame retardants such as halogen compounds and phosphorus compounds, colorants such as thermochromic dyes, inorganic pigments, and organic pigments, and various elastomers such as olefin copolymers, modified nitrile rubbers, modified butadiene rubbers, and modified polybutadiene rubbers.

[0069] <Method of producing photosensitive resin composition> The photosensitive resin composition of the present invention can be obtained, for example, by mixing and dissolving (a) an acrylic resin, (b) a cationic polymerizable compound, (c) a thermal cationic polymerization initiator, (d) a photo cationic polymerization initiator, and, if necessary, other additives. In addition, the photosensitive resin composition of the present invention can be obtained, if necessary, by dissolving these in an organic solvent to form a solution having a solid content concentration of about 10 to 70 mass%.

[0070] The photosensitive resin composition of the present invention may be filtered using filter paper or a filter. The method for filtering the photosensitive resin composition is not particularly limited, but a method of filtering the composition by pressure filtration using a filter having a retention particle size of 0.4 μm to 10 μm is preferred.

[0071] <Form of photosensitive resin composition> The form of the photosensitive resin composition of the present invention is not particularly limited, and may be selected according to the application, such as a film, a rod, a sphere, a pellet, or a varnish. The term "film" as used herein includes a membrane, a sheet, and a plate. The photosensitive film of the present invention is made of the photosensitive resin composition of the present invention. Therefore, the photosensitive film of the present invention may be a film in which the photosensitive resin composition is formed on a support, or may be a photosensitive resin composition in a film form without a support. When used in a varnish form, the above (a) to (d) and additives added as necessary can be dissolved in a solvent. In the present invention, the form of the photosensitive resin composition is preferably a film form. That is, a photosensitive film in which the photosensitive resin composition of the present invention is formed into a film form is preferred. The photosensitive film of the present invention can be obtained, for example, by applying the photosensitive resin composition of the present invention onto a support, and then drying it as necessary.

[0072] Examples of the support include polyester films such as polyethylene terephthalate (PET) films, polyphenylene sulfide films, polyimide films, etc. The bonding surface between the support and the photosensitive film may be surface-treated with silicone, a silane coupling agent, an aluminum chelating agent, polyurea, etc., in order to improve the adhesion and peelability between them. The thickness of the support is not particularly limited, but is preferably 10 to 100 μm from the viewpoint of workability.

[0073] The photosensitive film of the present invention may have a protective film for protecting the photosensitive film. In this case, the protective film can protect the surface of the photosensitive film from contaminants such as dust and dirt in the atmosphere.

[0074] Examples of the protective film in the present invention include polyester films such as polyethylene terephthalate (PET) films, polyolefin films such as polyethylene films and polypropylene films, polyvinyl alcohol films, etc. It is preferable that the protective film has a peel strength such that the photosensitive film and the protective film are not easily peeled off from each other.

[0075] Examples of methods for applying the photosensitive resin composition to a support to prepare the photosensitive film of the present invention include spin coating using a spinner, spray coating, roll coating, screen printing, blade coater, die coater, calendar coater, meniscus coater, bar coater, roll coater, comma roll coater, gravure coater, screen coater, slit die coater, etc. The coating thickness of the photosensitive resin composition varies depending on the coating method, the solids concentration, viscosity, etc. of the photosensitive resin composition to be applied, but it is preferable that the coating thickness of the photosensitive resin composition after drying is adjusted to 0.5 μm to 100 μm.

[0076] Examples of drying devices for drying the applied photosensitive resin composition include ovens, hot plates, and infrared rays. The drying temperature and drying time may be within a range that allows the solvent to volatilize, and it is preferable to appropriately set a range in which the photosensitive film is in an uncured or semi-cured state. Specifically, the drying temperature is preferably within a range of 40°C to 150°C, and the drying time is preferably within a range of 1 minute to several tens of minutes. The drying temperature may be increased stepwise by combining temperatures within this range. For example, when drying the photosensitive resin composition, the photosensitive resin composition may be heated at 50°C, 60°C, and 70°C for 1 minute each.

[0077] <Cured product of photosensitive resin composition> The cured product of the present invention is a cured product obtained by curing the photosensitive resin composition of the present invention or the photosensitive film of the present invention. Therefore, the cured product of the present invention can be obtained by exposing and / or heating the photosensitive resin composition of the present invention to light to form a cured product. In the heat curing of the photosensitive resin composition, the heat curing temperature is preferably within the range of 100°C to 400°C. The form of the cured product of the photosensitive resin composition is not particularly limited, and can be selected according to the application, such as a film, a rod, a sphere, or a pellet. In the present invention, the cured product is preferably a film. In addition, the shape of the cured product can be selected according to the application, such as forming a via hole for conduction, adjusting impedance, electrostatic capacitance, or internal stress, and imparting a heat dissipation function, by forming a pattern of the photosensitive resin composition. The film thickness of the cured product (film made of the cured product) is preferably 0.5 μm or more and 150 μm or less.

[0078] <Electronic components> The photosensitive resin composition or the cured product of the photosensitive film of the present invention can be applied to various electronic parts and devices. The applications are not particularly limited, but can be, for example, image sensors such as CCD and CMOS, gyro sensors using MEMS technology that integrates mechanical elements and electronic circuit elements using semiconductor microfabrication technology, acceleration sensors, pressure sensors, digital mirror devices (DMD), microphones, optical switches, automotive radars, LEDs, and crystal devices such as crystal oscillators and SAW filters. EXAMPLES

[0079] The present invention will be specifically described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0080] <Examples 1 to 28 and Comparative Examples 1 to 4> <Preparation of coating solution for photosensitive resin composition> The following acrylic resin, cationic polymerizable compound, thermal cationic polymerization initiator, photo cationic polymerization initiator, and other additives were mixed to obtain the composition shown in Table 1, and the mixture was stirred and dissolved in a DMF / MIBK mixed solvent at 40°C to a solids concentration of 30 mass % to prepare a coating solution for a photosensitive resin composition.

[0081] <Acrylic resin> Acrylic resins 1 to 9: (a1) acrylic resin and (a2) acrylic resin were each synthesized as follows: Water, a dispersant, a monomer in which a chain transfer agent and a polymerization initiator were dissolved, and the like were added to a reactor equipped with a mixer and a cooler under a nitrogen atmosphere (or under a nitrogen stream), and the temperature was raised to 60°C to carry out polymerization.

[0082] (a1) As the monomer of the acrylic resin, glycidyl methacrylate having an epoxy group and acrylonitrile having a cyano group were selected as monomers having at least two functional groups selected from the group consisting of an epoxy group, a cyano group, a hydroxyl group, an amino group, a hydroxyalkyl group, and a carboxy group, and further, ethyl acrylate or butyl acrylate was selected as an acrylic acid ester having a side chain having 1 to 5 carbon atoms.

[0083] (a2) As the monomer of the acrylic resin, methyl methacrylate and / or ethyl methacrylate were selected as a methacrylic acid ester having a side chain with 1 to 5 carbon atoms.

[0084] The weight average molecular weights of the obtained (a1) acrylic resin and (a2) acrylic resin were measured by GPC (gel permeation chromatography) method (GPC apparatus: GEL PERMEATION CHROMATOGRAPH, manufactured by Tosoh Corporation, column: TSK-GEL GMHXL 7.8*300 mm*3 columns, manufactured by Tosoh Corporation) and calculated in terms of polystyrene.

[0085] The glass transition temperatures of the (a1) acrylic resin and (a2) acrylic resin obtained were determined by differential scanning calorimetry (DSC). Using a Rigaku DSCvesta, the samples were heated from room temperature to 60°C at a heating rate of 10°C / min, cooled to -60°C, and then heated again to 40°C for measurement. The glass transition temperatures were read from the DSC curves at the second heating time.

[0086] Acrylic resin 1: Weight average molecular weight 800,000, glass transition temperature -4°C, butyl acrylate: acrylonitrile: glycidyl methacrylate = 57:33:1 (molar ratio) Acrylic resin 2: weight average molecular weight 1.4 million, glass transition temperature -32°C, butyl acrylate: ethyl acrylate: glycidyl methacrylate = 60:30:1 (molar ratio) Acrylic resin 3: weight average molecular weight 600,000, glass transition temperature 22°C, butyl acrylate: acrylonitrile: glycidyl methacrylate = 45:45:1 (molar ratio) Acrylic resin 4: weight average molecular weight 400,000, glass transition temperature -4°C, butyl acrylate: acrylonitrile: glycidyl methacrylate = 57:33:1 (molar ratio) Acrylic resin 5: weight average molecular weight 2 million, glass transition temperature -32°C, butyl acrylate: ethyl acrylate: glycidyl methacrylate = 60:30:1 (molar ratio) Acrylic resin 6: weight average molecular weight 35,000, glass transition temperature 104°C, methyl methacrylate:ethyl methacrylate = 80:10 (molar ratio) Acrylic resin 7: weight average molecular weight 80,000, glass transition temperature 65°C, methyl methacrylate:ethyl methacrylate = 5:85 (molar ratio) Acrylic resin 8: weight average molecular weight 200,000, glass transition temperature 84°C, methyl methacrylate: ethyl methacrylate = 50: 40 (molar ratio) Acrylic resin 9: weight average molecular weight 200,000, glass transition temperature 45°C, butyl acrylate: acrylonitrile: glycidyl methacrylate = 31: 59: 1 (molar ratio).

[0087] <Cationic polymerizable compound> Epoxy resin 1: EOCN-102S (epoxy equivalent 217, cresol novolac type epoxy, manufactured by Nippon Kayaku Co., Ltd.) Epoxy resin 2: HP-7200 (epoxy equivalent 260, cyclopentadiene type epoxy, manufactured by DIC Corporation) Epoxy resin 3: YL980 (epoxy equivalent 165, bisphenol A type epoxy, manufactured by Mitsubishi Chemical Corporation) Epoxy resin 4: N-865 (epoxy equivalent 200, modified novolac type epoxy, manufactured by DIC Corporation).

[0088] <Thermal cationic polymerization initiator> Thermal cationic polymerization initiator 1: San-Aid SI-B3 (manufactured by Sanshin Chemical Industry Co., Ltd.).

[0089] <Photocationic polymerization initiator> Photocationic polymerization initiator 1: CPI-310FG (manufactured by San-Apro Co., Ltd.).

[0090] <Radical polymerizable compound> Acrylic monomer 1: BP-6EM (molecular weight 726, bifunctional acrylic monomer, manufactured by Kyoeisha Chemical Co., Ltd.).

[0091] <Radical polymerization initiator> Radical polymerization initiator 1: Perbutyl O (organic peroxide, manufactured by NOF Corporation).

[0092] <Silane coupling agent> Silane coupling agent 1: 3-glycidoxypropyltrimethoxysilane (KBM-403, Shin-Etsu Chemical Co., Ltd.).

[0093] <Filler> Filler 1: spherical silica (SO-C5, average particle size 1.6 μm, manufactured by Admatechs Co., Ltd.).

[0094] (1) Coating and drying on the substrate This photosensitive resin composition coating solution was applied onto a support (a 38 μm thick PET film) using a bar coater, and dried at 100° C. for 5 minutes, after which a 38 μm thick PET film was laminated as a protective film. As a result, a photosensitive film of the photosensitive resin composition having a thickness of 20 μm was obtained.

[0095] (2) Tensile elongation at break evaluation The photosensitive film was subjected to a tensile test at 100°C and a speed of 50 mm / min using a tensile tester (UCT100, manufactured by Orientec Co., Ltd.) with a sample length between chucks of 40 mm and a width of 5 mm. The stress-strain curve up to break was recorded and the tensile elongation at break was calculated.

[0096] (3) Coverage evaluation The coverability when covering the surface of a substrate on which a plurality of electronic components are mounted with a photosensitive film was evaluated by the following procedure.

[0097] The substrate on which multiple electronic components were mounted was an alumina substrate on which evaluation Si chips measuring 0.9 mm wide x 1.1 mm long x 0.3 mm high were flip-chip mounted via 0.04 mm high solder bumps. The Si chips were mounted in 5 rows x 6 columns in the center of the 1 cm x 1 cm alumina substrate, with the spacing between each row of mounted Si chips being 0.5 mm, the spacing between the first and second rows, the third and fourth rows, and the fifth and sixth rows being 0.5 mm, and the spacing between the second and third rows, and the fourth and fifth rows being 0.05 mm.

[0098] A 20 μm-thick photosensitive film with a support attached to one side was placed on the substrate on which the above-mentioned multiple Si chips were mounted, with the surface without the protective film facing the substrate.

[0099] The photosensitive film was temporarily attached onto the Si chip under the following conditions: stage temperature 70°C, roll temperature 70°C, vacuum degree 150 Pa, attachment speed 5 mm / sec, and attachment pressure 0.1 MPa.

[0100] Next, the support was peeled off, and the above-mentioned substrate was placed on silicone rubber with an Asker hardness of 10, with the side with the photosensitive film facing down. Using a vacuum laminator (Nikko Materials Co., Ltd., CVP-300T), the temperature was appropriately adjusted to 40 to 100°C, the vacuum pressure was 0.1 to 1.0 MPa, the evacuation time was 30 to 100 seconds, and the pressure time was 30 to 300 seconds, and vacuum lamination was performed, so that the unevenness formed by mounting the Si chip on the alumina substrate was covered with a 20 μm layer made of a photosensitive resin composition (hereinafter, the layer made of the photosensitive resin composition is referred to as the photosensitive resin composition layer).

[0101] Next, the substrate covered with the photosensitive resin composition layer was subjected to a heat curing treatment at 150° C. for 2 hours in an air oven.

[0102] The appearance after covering with the photosensitive resin composition layer was judged according to the following criteria.

[0103] (a) Appearance of the photosensitive resin composition layer between the first and second columns, the third and fourth columns, the fifth and sixth columns, and between each row Whether the photosensitive resin composition layer conformed to the irregularities formed by mounting the Si chip on the alumina substrate was judged by microscopic observation. The photosensitive resin composition layer was judged as ⊚ when it was not broken and conformed sufficiently to the recesses, the photosensitive resin composition layer was judged as x when it was broken, and the photosensitive resin composition layer was judged as ◯ when there were some parts where it was not broken and did not conform sufficiently to the recesses.

[0104] (b) Appearance of the photosensitive resin composition layers in the second and third rows, and the fourth and fifth rows The appearance was evaluated by microscopic observation in the same manner as in (a). A photosensitive resin composition layer that was not broken and had a coating thickness of 3 μm or more was evaluated as ⊚, a photosensitive resin composition layer that was broken was evaluated as x, and a photosensitive resin composition layer that was not broken and had a coating thickness of 3 μm or less was evaluated as ◯.

[0105] (4) Evaluation of developability The protective film of the photosensitive film was peeled off, and the peeled surface of the photosensitive film was laminated onto a silicon wafer using a laminating device (Takatori Corporation, VTM-200M) under the following conditions: stage temperature 80°C, roll temperature 80°C, vacuum degree 150 Pa, application speed 5 mm / sec, and application pressure 0.3 MPa. A photomask having a pattern of L (Line) / S (Space)=1000 / 1000, 500 / 500, 200 / 200, 100 / 100, 75 / 75, 50 / 50, 45 / 45, 40 / 40, 35 / 35, 30 / 30, 25 / 25, 20 / 20 μm was set in an exposure device (Seiwa Optical Manufacturing Co., Ltd., SME-150GA-TRJ), and after peeling off the support, 1000 mJ / cm was applied with the photomask and the photosensitive resin composition layer spaced 50 μm apart. 2 Exposure was performed at an exposure dose of 100 nm (converted to i-line). After exposure, the photosensitive resin composition layer was heated on a hot plate at 100° C. for 5 minutes. Next, paddle development was performed using propylene glycol methyl ether acetate (PGMEA), thereby removing the unexposed parts of the photosensitive resin composition layer. The paddle development was performed for 180 seconds. Next, a rinsing treatment was performed with isopropyl alcohol (IPA) for 60 seconds, and then spin drying was performed. Furthermore, a heat curing treatment was performed in an air oven at 150° C. for 2 hours, and a substrate having a pattern formed thereon was obtained.

[0106] Each pattern substrate obtained by the above pattern formation method was observed at 100x magnification using an optical microscope (Nikon Corporation, ECLIPSE L300) to evaluate the minimum size of L / S when the formed L / S was free of abnormalities such as clogging. Those with L / S=75 / 75 μm or less were judged as ◎, those with L / S=500 / 500 μm or more were judged as ×, and those with L / S=200 / 200 μm or less were judged as ◯.

[0107] [Table 1-1]

[0108] [Table 1-2]

[0109] [Table 1-3]

[0110] [Table 1-4] [Industrial Applicability]

[0111] By using the photosensitive resin composition of the present invention, it is possible to collectively cover a plurality of elements arranged on a substrate, and after covering, to remove the unexposed portions of the photosensitive resin composition by photolithography, thereby improving the yield in the processing step and obtaining electronic components with excellent reliability.

Claims

1. (a) an acrylic resin, (b) a cationic polymerizable compound, (c) a thermal cationic polymerization initiator, and (d) a photo cationic polymerization initiator; The (a) acrylic resin is a photosensitive resin composition including (a1) an acrylic resin having a glass transition temperature of −40° C. or more and 30° C. or less, and (a2) an acrylic resin having a glass transition temperature of 60° C. or more and 110° C. or less.

2. The photosensitive resin composition according to claim 1 , wherein the acrylic resin (a1) has a weight average molecular weight of 600,000 or more and 1,800,000 or less.

3. The photosensitive resin composition according to claim 1 , wherein the acrylic resin (a2) has a weight average molecular weight of 10,000 or more and 100,000 or less.

4. 2. The photosensitive resin composition according to claim 1, wherein the (a1) acrylic resin is contained in an amount of 10 mass% or more and 30 mass% or less based on a total of 100 mass% of all components excluding the solvent.

5. The photosensitive resin composition according to claim 1 , wherein the (a2) acrylic resin is contained in an amount of 15% by mass or more and 45% by mass or less based on a total of 100% by mass of all components excluding the solvent.

6. 2. The photosensitive resin composition according to claim 1, wherein a ratio of the content (by mass) of the (c) thermal cationic polymerization initiator to the content (by mass) of the (d) photo cationic polymerization initiator is 0.1 or more and 1 or less.

7. The photosensitive resin composition according to claim 1 , further comprising (e) a radically polymerizable compound.

8. The photosensitive resin composition according to claim 7, further comprising: (f) a radical polymerization initiator.

9. A photosensitive film comprising the photosensitive resin composition according to claim 1.

10. A cured product obtained by curing the photosensitive resin composition according to any one of claims 1 to 8 or the photosensitive film according to claim 9.

11. An electronic part comprising the cured product according to claim 10.

Citation Information

Patent Citations

  • Formation of tantalum-aluminum alloy film

    JP1985089567A

  • Surface acoustic wave device and its manufacturing method

    JP2003017979A

  • Semiconductor device manufacturing method

    JP4053483B2

  • Manufacturing methods for electronic components

    JP4730652B2

Cited By

  • Photosensitive adhesive composition, photosensitive adhesive dry film, pattern formation method, and laminate production method

    WO2026069892A1