Aromatic polyether ketone molded body and production method therefor
Aromatic polyetherketone molded articles with a matrix phase and dispersed phase of carbon black or nanotubes achieve both high mechanical strength and elongation, addressing the durability needs of sliding members like gear members.
Patent Information
- Application Number
- JP2023049519
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing resin molded articles struggle to achieve both high mechanical strength and high elongation, which are essential for durable sliding members like gear members.
Aromatic polyetherketone molded articles are designed with a matrix phase composed of aromatic polyetherketone and a dispersed phase of carbon black or carbon nanotubes, featuring a large crystallite size and specific molecular weight distribution, enhanced by annealing at a temperature near the matrix phase's melting point.
The solution results in a resin molded article with high mechanical strength and large elongation, suitable for durable sliding members by preventing chipping and enhancing thermal conductivity.
Smart Images

Figure 2024138820000005 
Figure 2024138820000006 
Figure 2024138820000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aromatic polyether ketone molded article that can be used for various parts. [Background technology]
[0002] In the field of industrial machinery, there is a demand for replacing metal parts with resin molded bodies from the viewpoint of weight reduction, etc. Patent Document 1 discloses a technology for improving the mechanical strength of resin molded bodies. This technology can improve the mechanical strength of resin molded bodies by improving the crystallinity of the resin component and restricting the degree of freedom of molecular motion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-150984 A Summary of the Invention [Problem to be solved by the invention]
[0004] Parts for which resin molded bodies are expected to replace metal parts include sliding members such as gear members. For sliding members, in order to improve durability, it is advantageous for them to have high mechanical strength as well as high elongation. However, there are few known techniques that can achieve both high mechanical strength and high elongation in resin molded bodies.
[0005] In view of the above circumstances, an object of the present invention is to provide an aromatic polyether ketone molded article having both high mechanical strength and large elongation. [Means for solving the problem]
[0006] In order to achieve the above object, an aromatic polyether ketone molded article according to one embodiment of the present invention includes a matrix phase and a dispersed phase dispersed in the matrix phase. The matrix phase is composed of aromatic polyether ketone and has a crystallite size greater than 63 Å. The dispersed phase is composed of at least one of carbon black and carbon nanotubes.
[0007] In this aromatic polyether ketone molded article, the matrix phase is composed of aromatic polyether ketone, so that high mechanical strength is obtained. In addition, in this aromatic polyether ketone molded article, the crystallite size of the matrix phase is large, so that high elongation is obtained. In other words, this aromatic polyether ketone molded article can achieve both high mechanical strength and high elongation.
[0008] The aromatic polyether ketone constituting the matrix phase may have a molecular weight distribution with a maximum peak molecular weight in the range of 50,000 or more. The dispersed phase may be composed of carbon black, and the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more may be 0.6% or more. The dispersed phase may be composed of carbon nanotubes, and the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more may be 1.9% or more. The matrix phase may be composed of polyether ether ketone. The aromatic polyether ketone molded article may be configured as a sliding member. The aromatic polyether ketone molded article may be configured as a gear member.
[0009] In one embodiment of the method for producing an aromatic polyether ketone molded article according to the present invention, a molded article is produced by injection molding, in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of an aromatic polyether ketone having a molecular weight distribution with a maximum peak molecular weight in the range of 50,000 or more. The molded body is annealed at a temperature higher than the intermediate temperature between the melting point and the glass transition point of the matrix phase and lower than the melting point of the matrix phase.
[0010] It is known that the crystallite size is difficult to increase in aromatic polyether ketones with large molecular weights. In contrast, in the above-mentioned configuration, at least one of carbon black and carbon nanotubes is dispersed in the matrix phase, and annealing is performed at a high temperature close to the melting point of the matrix phase. In the high-temperature environment during the annealing treatment, molecular motion is active even in aromatic polyether ketones with large molecular weights. In the matrix phase with such active molecular motion, at least one of the carbon black and carbon nanotubes constituting the dispersed phase becomes the nucleus of the crystallites, and grain growth proceeds even in crystallites composed of long molecular chains. As a result, in the above-mentioned configuration, a matrix phase with large crystallite size is obtained. Effect of the Invention
[0011] As described above, the present invention can provide an aromatic polyether ketone molded article having both high mechanical strength and large elongation. [Brief description of the drawings]
[0012] [Figure 1] 1 is a flowchart showing a method for producing a resin molded body according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a plan view showing an example in which the resin molded body is configured as a gear member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Explanation of resin molded body] The present invention relates to an aromatic polyether ketone molded article, which is a resin molded article formed mainly from aromatic polyether ketone. More specifically, the resin molded article according to this embodiment includes a matrix phase made of aromatic polyether ketone and a dispersed phase made of carbon powder and dispersed in the matrix phase. The carbon powder constituting the dispersed phase is made of at least one of carbon black and carbon nanotubes.
[0014] The aromatic polyether ketone constituting the matrix phase is a resin composed of a benzene ring, an ether, and a ketone. In the resin molded product according to the present embodiment, it is preferable to use polyether ether ketone (PEEK) having excellent heat resistance and mechanical strength as the aromatic polyether ketone constituting the matrix phase.
[0015] In the resin molded article according to the present embodiment, the aromatic polyether ketone constituting the matrix phase has a large molecular weight, and specifically, it is preferable that the molecular weight distribution has a maximum peak molecular weight in the range of 50,000 or more. As a result, in the resin molded article according to the present embodiment, the long molecular chains bind each other, thereby obtaining high mechanical strength.
[0016] Furthermore, in the resin molded product according to this embodiment, the crystallite size of the aromatic polyether ketone in the matrix phase is large, specifically, larger than 63 Å. As a result, in the resin molded product according to this embodiment, even when a large tensile stress is applied, the molecular chains constituting each crystallite are unlikely to break, and thus large elongation can be obtained.
[0017] In other words, in the resin molded article according to the present embodiment, the matrix phase is composed of long molecular chains, and the crystallite size in the matrix phase is large, so that it is possible to achieve both high mechanical strength and large elongation. As a result, the resin molded article according to the present embodiment has high durability when used in applications such as sliding members.
[0018] The molecular weight distribution of the aromatic polyether ketone constituting the matrix phase can be measured by, for example, gel permeation chromatography. The maximum peak molecular weight refers to the molecular weight corresponding to the number of molecules (frequency) that forms a peak value in the molecular weight distribution curve obtained by molecular weight measurement.
[0019] The crystallite size of the matrix phase can be measured using a diffraction pattern obtained by X-ray diffraction (XRD). In other words, the crystallite size of the matrix phase can be calculated based on the Scherrer formula by measuring the half-width of the maximum peak corresponding to the aromatic polyether ketone in the diffraction pattern.
[0020] The crystallite size of the matrix phase should be larger than 63 Å, and no disadvantages due to being too large have been confirmed at present, but it is believed that there is a limit to the improvement in mechanical strength that can be achieved by increasing the crystallite size of the matrix phase. From this perspective, the upper limit of the crystallite size of the matrix phase is assumed to be, for example, 250 Å.
[0021] 1 is a flowchart showing a method for producing a resin molded body according to the present embodiment. First, in step S01, a raw material is prepared. The raw material prepared in step S01 is prepared as a kneaded product in which, for example, aromatic polyether ketone constituting the matrix phase and carbon powder constituting the dispersed phase are kneaded together.
[0022] In step S01, the aromatic polyether ketone used has a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. In step S01, the carbon powder used has a particle size distribution appropriate for obtaining the effect described in step S03 described later.
[0023] The kneaded material as a raw material is obtained, for example, by kneading aromatic polyether ketone and carbon powder with a single screw extruder, a twin screw extruder, etc. In addition, in step S01, the kneaded material as a raw material can also be prepared as a commercially available product in which aromatic polyether ketone and carbon powder are kneaded in advance.
[0024] Next, in step S02, the raw material prepared in step S01 is molded into a shape according to the application. The raw material can be molded by injection molding. In the raw material molded body obtained in step S02, a dispersed phase made of carbon powder is dispersed in a matrix phase made of aromatic polyether ketone.
[0025] In step S02, since the grain growth of crystallites does not progress easily in the matrix phase having a large molecular weight, it is difficult to obtain a large crystallite size in the matrix phase in the raw material compact obtained in step S02. For this reason, in this embodiment, step S03 is performed to increase the crystallite size of the matrix phase.
[0026] In step S03, the raw material compact obtained in step S02 is annealed. The holding temperature in the annealing in step S03 is higher than the temperature generally set in an annealing aimed at relieving residual stress, specifically, higher than the intermediate temperature between the melting point and the glass transition point of the matrix phase and lower than the melting point of the matrix phase.
[0027] In the raw material compact, molecular motion becomes active even in the matrix phase with a large molecular weight in such a high-temperature environment close to the melting point. In the matrix phase with such active molecular motion, the carbon powder constituting the dispersed phase becomes the nucleus of the crystallite, so that even crystallites composed of long molecular chains tend to grow easily. Furthermore, the carbon nanotubes constituting the dispersed phase also have the effect of improving the thermal conductivity of the raw material compact as a whole, including the matrix phase. Therefore, in the raw material compact in which the dispersed phase is composed of carbon nanotubes, the molecular motion of the matrix phase becomes even more active during annealing, and the grain growth of the crystallites is further promoted.
[0028] That is, in step S03, the dispersion of carbon powder and the annealing treatment at a high temperature close to the melting point of the matrix phase work together to promote grain growth of crystallites in the matrix phase having a large molecular weight, thereby obtaining a resin molded product having a large crystallite size in the matrix phase.
[0029] The effect of promoting grain growth by becoming the nucleus of crystallites in the dispersed phase is considered to be obtained regardless of the size of the dispersed phase, but is more effective when the dispersed phase is made large to some extent. In this respect, in the resin molded product according to this embodiment, when the dispersed phase is made of carbon black, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more is 0.6% or more. Also, when the dispersed phase is made of carbon nanotubes, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more is 1.9% or more.
[0030] On the other hand, in the resin molded body according to the present embodiment, from the viewpoint of moldability, the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more is preferably 20% or less, more preferably 10% or less. The area ratio of the dispersed phase of the resin molded body can be obtained from a photograph of the resin molded body taken with a fluorescent microscope.
[0031] The annealing treatment of the raw material compact in step S03 can be performed using a known heating method, such as hot air heating, far-infrared heating, near-infrared heating, etc. The annealing treatment of the raw material compact is typically performed in the atmosphere, but may also be performed in, for example, a low oxygen partial pressure or an inert gas.
[0032] The resin molded article according to the present embodiment is particularly suitable for application to parts where stress is likely to concentrate locally. Examples of such parts include sliding members such as gear members, seal rings, thrust washers, and bearings. The resin molded article according to the present embodiment configured as a sliding member has high durability.
[0033] A gear member is shown in Fig. 2 as an application example of the resin molded article according to this embodiment as a sliding member. In the gear member, stress tends to concentrate at the tooth base of the multiple teeth T arranged continuously along the outer periphery, but by configuring the gear member as the resin molded article according to this embodiment, the occurrence of chipping of the teeth T can be effectively suppressed.
[0034] [Examples and Comparative Examples] Examples and comparative examples of the above embodiment will be described.
[0035] (Examples 1 to 4 and Comparative Examples 1 and 2) In Examples 1 to 4 and Comparative Examples 1 and 2, samples of resin molded bodies were prepared and each sample was evaluated. In all of Examples 1 to 4 and Comparative Example 2, carbon black was used as the carbon powder constituting the dispersed phase. Comparative Example 1 differs from the above embodiment in that no dispersed phase was used and no annealing treatment was performed. Comparative Example 2 differs from the above embodiment in that no annealing treatment was performed.
[0036] A common aromatic polyether ketone was used in all of Examples 1 to 4 and Comparative Examples 1 and 2. Specifically, a polyether ether ketone "Vestakeep (registered trademark) 5000G" manufactured by Polypla-Evonik was used as the aromatic polyether ketone in all of Examples 1 to 4 and Comparative Examples 1 and 2.
[0037] The same carbon black was used in all of Examples 1 to 4 and Comparative Example 2. Specifically, carbon black "#750B" manufactured by Mitsubishi Chemical Corporation was used in all of Examples 1 to 4 and Comparative Example 2. Note that in Comparative Example 1, no carbon black was used, that is, only aromatic polyether ketone was used.
[0038] Table 1 shows the holding temperatures and holding times of the annealing treatment in Examples 1 to 4. Table 1 also shows the area ratios of the regions occupied by the dispersed phases having a particle size of 0.1 μm or more in the samples and the crystallite sizes of the matrix phases in the samples in Examples 1 to 4 and Comparative Examples 1 and 2.
[0039] The area ratio of the dispersed phase of each sample was determined from a photograph of each sample taken with a fluorescent microscope "BX53M" manufactured by Olympus Corporation. The crystallite size of the matrix phase of each sample was determined from the diffraction pattern of each sample obtained by measurement with an X-ray diffraction device "Samartlab" manufactured by Rigaku Corporation.
[0040] As shown in Table 1, the crystallite size of the matrix phase in all of Examples 1 to 4 was larger than that in Comparative Example 1. In contrast, the crystallite size of the matrix phase in Comparative Example 2 was equivalent to that in Comparative Example 1. This confirmed that annealing at high temperatures is effective in increasing the crystallite size of the matrix phase.
[0041] [Table 1]
[0042] A tensile test was carried out to evaluate the fracture properties of each sample according to Examples 1 to 4 and Comparative Examples 1 and 2. An "AGX" manufactured by Shimadzu Corporation was used for the tensile test. In the tensile test, each sample was made into an A12 dumbbell shape conforming to JIS K7139 (2009), the tensile speed was 10 mm / min, and the other conditions were the same.
[0043] As a result, in Table 2, the yield strength, yield stroke, and tensile product for Examples 1 to 4 and Comparative Examples 1 and 2 are shown as percentage changes (%) relative to Comparative Example 1. The yield strength and yield stroke were obtained from the stress-strain curve obtained in the tensile test, and the tensile product was calculated from the yield strength and yield stroke.
[0044] In all of Examples 1 to 4, the yield stroke was significantly improved, and the tensile product was 15% or more higher than in Comparative Example 1. On the other hand, the yield stroke in Comparative Example 2 was smaller than in Examples 1 to 4. This confirmed that a large elongation could be obtained by increasing the crystallite size of the matrix phase.
[0045] Next, a gear durability test was conducted on each sample according to Examples 1 to 4 and Comparative Examples 1 and 2 in order to evaluate the product characteristics as a gear member. In the gear durability test, each sample had a gear shape. In the gear durability test for each sample, a gear member (made of S45C) was used as a mating member, and the sample was rotated while meshed with the mating member.
[0046] In addition, the gear durability tests for each sample were conducted under the same conditions, with a rotation speed of 1000 rpm and a torque of 10 N·m. Grease was used as a lubricant between each sample and the mating material during rotation. Each sample was judged as "OK" or "NG" based on the presence or absence of chipped teeth after 1.1 million rotations.
[0047] Table 2 shows the results of the gear durability test for Examples 1 to 4 and Comparative Examples 1 and 2. No chipping of teeth occurred in any of the samples according to Examples 1 to 4, whereas chipping of teeth occurred in all of the samples according to Comparative Examples 1 and 2. This shows that Examples 1 to 4 provide high product characteristics as gear members.
[0048] [Table 2]
[0049] (Examples 5 to 7) In Examples 5 to 7, samples of resin molded bodies were prepared and each sample was evaluated. In all of Examples 5 to 7, carbon nanotubes were used as the carbon powder constituting the dispersed phase. In all of Examples 5 to 7, aromatic polyether ketone was used, which was the same as in Examples 1 to 4 and Comparative Examples 1 and 2.
[0050] Moreover, the same carbon nanotubes were used in all of Examples 5 to 7. Specifically, the carbon nanotubes "NC7000" manufactured by Nanocyl Corporation were used in all of Examples 5 to 7.
[0051] Table 3 shows the holding temperature and holding time of the annealing treatment in Examples 5 to 7. Table 3 also shows the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the samples and the crystallite size of the matrix phase of the samples in Examples 5 to 7 and Comparative Example 1. The area ratio of the dispersed phase and the crystallite size of the matrix phase in each sample were determined by the same method as in Examples 1 to 4 and Comparative Examples 1 and 2.
[0052] As shown in Table 3, in all of Examples 5 to 7, the crystallite size of the matrix phase was larger than that of Comparative Example 1. In particular, in Example 6, in which the area ratio of the dispersed phase was large, a significantly larger crystallite size was obtained. This confirmed that the effect of promoting grain growth of crystallites was obtained by having a large amount of carbon nanotubes with high thermal conductivity.
[0053] [Table 3]
[0054] For Examples 5 to 7, in order to evaluate the fracture properties, tensile tests were carried out in the same manner as for Examples 1 to 4 and Comparative Examples 1 and 2. As a result, Table 4 shows the yield strength, yield stroke, and tensile product for Examples 5 to 7 and Comparative Example 1 as percentage changes (%) relative to Comparative Example 1.
[0055] In all of Examples 5 to 7, the yield strength and the yield stroke were improved compared to Comparative Example 1, and the tensile product was 20% or more higher. In particular, in Example 6, in which the area ratio of the dispersed phase was large, both the yield strength and the yield stroke were the largest. This confirmed that a large tensile product could be obtained by increasing the crystallite size of the matrix phase.
[0056] Next, in order to evaluate the product characteristics as gear members for each sample according to Examples 5 to 7 and Comparative Example, a gear durability test was conducted in the same manner as for Examples 1 to 4 and Comparative Examples 1 and 2. Table 4 shows the results of the gear durability test for Examples 5 to 7 and Comparative Example 1. No chipping of teeth occurred in any of the samples according to Examples 5 to 7. This shows that Examples 5 to 7 have high product characteristics as gear members.
[0057] [Table 4]
[0058] [Other embodiments] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made thereto.
[0059] For example, in the resin molded article of the present invention, the molecular weight of the aromatic polyether ketone constituting the matrix phase is not particularly limited as long as sufficient mechanical strength is obtained depending on the application, etc. In other words, the aromatic polyether ketone constituting the matrix phase may have a maximum peak molecular weight in any range in the molecular weight distribution.
[0060] Furthermore, the aromatic polyetherketone constituting the matrix phase of the resin molded article of the present invention may be other than polyetheretherketone (PEEK), and may be, for example, polyetherketone (PEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), polyetherketoneetherketoneketone (PEKEKK), etc. Furthermore, the matrix phase of the resin molded article of the present invention may be a blend of multiple types of aromatic polyetherketones.
Claims
1. a matrix phase composed of an aromatic polyether ketone and having a crystallite size of greater than 63 Å; a dispersed phase composed of at least one of carbon black and carbon nanotubes and dispersed in the matrix phase; An aromatic polyether ketone molding comprising:
2. The aromatic polyether ketone molded article according to claim 1, The aromatic polyether ketone constituting the matrix phase has a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. Aromatic polyether ketone molding.
3. The aromatic polyether ketone molded article according to claim 1, the dispersed phase is composed of carbon black; The area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more is 0.6% or more. Aromatic polyether ketone molding.
4. The aromatic polyether ketone molded article according to claim 1, the dispersed phase is composed of carbon nanotubes, The area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more is 1.9% or more. Aromatic polyether ketone molding.
5. The aromatic polyether ketone molded article according to claim 1, The matrix phase is composed of polyether ether ketone. Aromatic polyether ketone molding.
6. The aromatic polyether ketone molded article according to claim 1, Configured as a sliding member Aromatic polyether ketone molding.
7. The aromatic polyether ketone molded article according to claim 6, Configured as a gear member Aromatic polyether ketone molding.
8. A molded product is produced by an injection molding method, in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of an aromatic polyether ketone having a molecular weight distribution with a maximum peak molecular weight in the range of 50,000 or more; The molded body is annealed at a temperature higher than the intermediate temperature between the melting point and the glass transition point of the matrix phase and lower than the melting point of the matrix phase. A method for producing an aromatic polyether ketone molded article.
Citation Information
Patent Citations
Molded gear
JP1993172212A
Resin composition
JP1997040864A
Aromatic polyether ketone-based resin molded product and method for producing the same
JP2002284980A
Composite resin of aromatic polyetheretherketoneketone
JP2005133047A
Sheath-core composite fiber having heat resistance
JP2014125708A