Aromatic polyether ketone molding, and producing method thereof
The aromatic polyetherketone molded article with a larger surface crystallite size and dispersed phase addresses the challenge of achieving high mechanical strength and elongation, ensuring durability through stress absorption and impact distribution.
Patent Information
- Application Number
- JP2023049520
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing resin molded articles struggle to achieve both high mechanical strength and high elongation, particularly in sliding members like gear members, where stress concentration is a concern.
An aromatic polyetherketone molded article with a matrix phase and dispersed phase, where the surface layer has a larger crystallite size than the inner portion, enhanced by electron beam irradiation, incorporating carbon black or carbon nanotubes to promote grain growth in the surface layer.
The article achieves high mechanical strength and large elongation in the surface layer, with improved durability by absorbing impact in the inner part, preventing local stress concentration and enhancing durability.
Smart Images

Figure 2024138821000005 
Figure 2024138821000006 
Figure 2024138821000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an aromatic polyether ketone molded article that can be used for various parts. [Background technology]
[0002] In the field of industrial machinery, there is a demand for replacing metal parts with resin molded bodies from the viewpoint of weight reduction, etc. Patent Document 1 discloses a technology for improving the mechanical strength of resin molded bodies. This technology can improve the mechanical strength of resin molded bodies by improving the crystallinity of the resin component and restricting the degree of freedom of molecular motion. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-150984 A Summary of the Invention [Problem to be solved by the invention]
[0004] Parts for which resin molded bodies are expected to replace metal parts include sliding members such as gear members. For sliding members, in order to improve durability, it is advantageous for them to have high mechanical strength as well as high elongation. However, there are few known techniques that can achieve both high mechanical strength and high elongation in resin molded bodies.
[0005] In view of the above circumstances, an object of the present invention is to provide an aromatic polyether ketone molded article having both high mechanical strength and large elongation in a surface layer portion. [Means for solving the problem]
[0006] In order to achieve the above object, an aromatic polyether ketone molded article according to one embodiment of the present invention includes a matrix phase and a dispersed phase dispersed in the matrix phase. The matrix phase is composed of an aromatic polyether ketone. The dispersed phase is composed of at least one of carbon black and carbon nanotubes. The aromatic polyether ketone molded article is composed of a surface layer portion and an inner portion. The crystallite size of the matrix phase in the surface layer portion is greater than 63 Å. The inner portion constitutes the inside of the surface layer portion, and the crystallite size of the matrix phase is smaller than that of the surface layer portion.
[0007] In this aromatic polyether ketone molded article, the crystallite size is larger in the surface layer portion constituting the surface than in the inner portion inside the surface layer portion, and therefore, in this aromatic polyether ketone molded article, in addition to the high mechanical strength inherent to aromatic polyether ketone, the surface layer portion to which external forces are more easily applied can achieve large elongation. On the other hand, in this aromatic polyether ketone molded article, since the inner part having a small crystallite size has high impact absorption, impacts applied to the surface layer part are absorbed by the inner part, and thus the surface layer part is less likely to be locally subjected to large stress, resulting in even higher durability.
[0008] The aromatic polyether ketone constituting the matrix phase may have a molecular weight distribution with a maximum peak molecular weight in the range of 50,000 or more. The dispersed phase may be made of carbon black, and the area ratio of the region in the surface layer portion occupied by the dispersed phase having a particle size of 0.1 μm or more may be 0.6% or more. The dispersed phase may be composed of carbon nanotubes, and the area ratio of the region in the surface layer that is occupied by the dispersed phase having a particle size of 0.1 μm or more may be 1.9% or more. The matrix phase may be composed of polyether ether ketone. The aromatic polyether ketone molded article may be configured as a sliding member. The aromatic polyether ketone molded article may be configured as a gear member.
[0009] In a method for producing an aromatic polyether ketone molded article according to one embodiment of the present invention, a molded article is produced by injection molding, in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of aromatic polyether ketone. The surface of the molded body is irradiated with an electron beam.
[0010] In the above-mentioned configuration, at least one of carbon black and carbon nanotubes is dispersed in the matrix phase, and the molded body obtained by injection molding is irradiated with an electron beam. A large amount of energy is applied to the surface layer of the molded body by the irradiation with the electron beam, and the molecular motion of the aromatic polyether ketone present in the surface layer is activated. In the surface layer of the molded body, at least one of the carbon black and carbon nanotubes constituting the dispersed phase in the matrix phase where the molecular motion is activated becomes the nucleus of the crystallite, and the grain growth of the crystallite is promoted. As a result, an aromatic polyether ketone molded body having a matrix phase with a large crystallite size in the surface layer is obtained. Effect of the Invention
[0011] As described above, the present invention can provide an aromatic polyether ketone molded article having both high mechanical strength and high elongation in the surface layer portion. [Brief description of the drawings]
[0012] [Figure 1] 1 is a flowchart showing a method for producing a resin molded body according to an embodiment of the present invention. [Diagram 2] FIG. 11 is a plan view showing an example in which the resin molded body is configured as a gear member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Explanation of resin molded body] The present invention relates to an aromatic polyether ketone molded article, which is a resin molded article formed mainly from aromatic polyether ketone. More specifically, the resin molded article according to this embodiment includes a matrix phase made of aromatic polyether ketone and a dispersed phase made of carbon powder and dispersed in the matrix phase. The carbon powder constituting the dispersed phase is made of at least one of carbon black and carbon nanotubes.
[0014] The aromatic polyether ketone constituting the matrix phase is a resin composed of a benzene ring, an ether, and a ketone. In the resin molded product according to the present embodiment, it is preferable to use polyether ether ketone (PEEK) having excellent heat resistance and mechanical strength as the aromatic polyether ketone constituting the matrix phase.
[0015] In the resin molded article according to the present embodiment, the aromatic polyether ketone constituting the matrix phase has a large molecular weight, and specifically, it is preferable that the molecular weight distribution has a maximum peak molecular weight in the range of 50,000 or more. As a result, in the resin molded article according to the present embodiment, the long molecular chains bind each other, thereby obtaining high mechanical strength.
[0016] The resin molded article according to the present embodiment is composed of a surface layer portion having a large crystallite size of the matrix phase and an inner portion forming the inside of the surface layer portion and having a smaller crystallite size of the matrix phase than that of the surface layer portion. Specifically, in the resin molded article according to the present embodiment, the crystallite size of the matrix phase in the surface layer portion is larger than 63 Å.
[0017] As a result, in the surface layer portion of the resin molded product according to this embodiment, the molecular chains constituting each crystallite are less likely to break even when a large tensile stress is applied, and thus a large elongation can be obtained. Therefore, in the resin molded product according to this embodiment, a large elongation can be selectively obtained in the surface layer portion constituting the surface vicinity where a large external stress is likely to be applied.
[0018] In other words, in the resin molded article according to the present embodiment, the matrix phase is composed of long molecular chains, and the crystallite size of the matrix phase in the surface layer is large, so that the surface layer can have both high mechanical strength and large elongation. As a result, the resin molded article according to the present embodiment can have high durability when used in applications such as sliding members.
[0019] The molecular weight distribution of the aromatic polyether ketone constituting the matrix phase can be measured by, for example, gel permeation chromatography. The maximum peak molecular weight refers to the molecular weight corresponding to the number of molecules (frequency) that forms a peak value in the molecular weight distribution curve obtained by molecular weight measurement.
[0020] The crystallite size of the matrix phase can be measured using a diffraction pattern obtained by X-ray diffraction (XRD). In other words, the crystallite size of the matrix phase can be calculated based on the Scherrer formula by measuring the half-width of the maximum peak corresponding to the aromatic polyether ketone in the diffraction pattern.
[0021] The crystallite size of the matrix phase in the surface layer needs only to be larger than 63 Å, and no disadvantages due to the crystallite size being too large have been confirmed at this stage, but it is believed that there is a limit to the improvement in mechanical strength that can be achieved by increasing the crystallite size. From this perspective, the upper limit of the crystallite size of the matrix phase in the surface layer is assumed to be, for example, 250 Å.
[0022] In addition, in the resin molded article according to the present embodiment, since the crystallite size in the matrix phase is smaller in the inner part than in the surface layer part, high impact absorption is obtained, and impacts applied to the surface layer part are well absorbed. As a result, in the resin molded article according to the present embodiment, large stress is unlikely to be locally applied to the surface layer part, and further high durability is obtained.
[0023] That is, in the resin molded product according to the present embodiment, the crystallite size of the matrix phase is made large in the surface layer portion, while the crystallite size of the matrix phase is intentionally kept small in the inner portion. With this configuration, the resin molded product according to the present embodiment can more effectively improve durability by the synergistic effect between the surface layer portion and the inner portion.
[0024] The thickness of the surface layer in the resin molded product according to the present embodiment can be appropriately determined depending on the application, etc. For example, from the viewpoint of more reliably obtaining the above-mentioned effect of the surface layer, the thickness of the surface layer is preferably 50 μm or more. On the other hand, from the viewpoint of more effectively obtaining the impact absorption property of the inner part, the thickness of the surface layer is preferably kept at 700 μm or less.
[0025] 1 is a flowchart showing a method for producing a resin molded body according to the present embodiment. First, in step S01, a raw material is prepared. The raw material prepared in step S01 is prepared as a kneaded product in which, for example, aromatic polyether ketone constituting the matrix phase and carbon powder constituting the dispersed phase are kneaded together.
[0026] In step S01, it is preferable to use an aromatic polyether ketone having a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. In addition, in step S01, it is possible to use a carbon powder having a particle size distribution appropriate for obtaining the effect described in step S03 described later.
[0027] The kneaded material as a raw material is obtained, for example, by kneading aromatic polyether ketone and carbon powder with a single screw extruder, a twin screw extruder, etc. In addition, in step S01, the kneaded material as a raw material can also be prepared as a commercially available product in which aromatic polyether ketone and carbon powder are kneaded in advance.
[0028] Next, in step S02, the raw material prepared in step S01 is molded into a shape according to the application. The raw material can be molded by injection molding. In the raw material molded body obtained in step S02, a dispersed phase made of carbon powder is dispersed in a matrix phase made of aromatic polyether ketone.
[0029] In the raw material compact obtained in step S02, the crystallite size of the matrix phase is substantially uniform, and the surface layer portion and the inner portion in which the crystallite size of the matrix phase differs from each other are not formed. In this embodiment, step S03 is performed to form the surface layer portion in which the crystallite size of the matrix phase is large.
[0030] In step S03, the surface of the raw material compact obtained in step S02 is irradiated with an electron beam. This selectively applies large energy to the surface layer of the raw material compact that constitutes the surface vicinity. In step S03, in order to sufficiently increase the energy applied to the surface layer of the raw material compact, it is preferable to set the irradiation dose of the electron beam to 50 kGy or more.
[0031] In the matrix phase of the raw material compact, molecular motion becomes active in the surface layer where a large amount of energy is applied by the electron beam irradiation, and grain growth of crystallites proceeds with the carbon powder constituting the dispersed phase as nuclei. Furthermore, the carbon nanotubes constituting the dispersed phase also have the effect of improving the thermal conductivity of the raw material compact as a whole including the matrix phase. Therefore, in a raw material compact whose dispersed phase is composed of carbon nanotubes, the molecular motion of the matrix phase in the surface layer becomes even more active by the electron beam irradiation, and the grain growth of the crystallites is further promoted. On the other hand, the crystallite size is maintained in the inner portion which is not affected by the electron beam irradiation, and a difference in the crystallite size of the matrix phase between the surface layer and the inner portion is formed.
[0032] In particular, in the resin molded article according to this embodiment, the synergistic effect of the dispersion of carbon powder and the irradiation of electron beams can promote the growth of crystallites even in the matrix phase with a large molecular weight where the growth of crystallites is difficult to promote, thereby obtaining a resin molded article having both high mechanical strength and large elongation in the surface layer.
[0033] The effect of promoting grain growth by becoming the nucleus of crystallites in the dispersed phase is considered to be obtained regardless of the size of the dispersed phase, but is more effective when the dispersed phase is made large to some extent. In this respect, in the resin molded product according to this embodiment, when the dispersed phase is made of carbon black, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer is 0.6% or more. Also, when the dispersed phase is made of carbon nanotubes, it is preferable that the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer is 1.9% or more.
[0034] On the other hand, in the resin molded body according to the present embodiment, from the viewpoint of moldability, the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer portion is preferably 20% or less, more preferably 10% or less. The area ratio of the dispersed phase of the resin molded body can be obtained from a photograph of the resin molded body taken with a fluorescent microscope.
[0035] In addition, in the resin molded product according to the present embodiment, the portion where the crystallites are grown by irradiation with electron beams is limited to the surface layer, and the crystallite size of the inner portion, which occupies the majority of the surface layer, is not changed. Therefore, in this resin molded product, the dimensional change due to the change in crystallite size from the raw material molded product can be kept small.
[0036] The thickness of the surface layer of the resin molded body can be controlled in various ways by changing the conditions of the electron beam irradiation. In addition, in step S03, by irradiating the electron beam while heating the raw material molded body, the grain growth of the crystallites of the matrix phase in the surface layer can be promoted more effectively.
[0037] The resin molded article according to the present embodiment is particularly suitable for application to parts where stress is likely to concentrate on the surface. Examples of such parts include sliding members such as gear members, seal rings, thrust washers, and bearings. The resin molded article according to the present embodiment configured as a sliding member has high durability.
[0038] A gear member is shown in Fig. 2 as an application example of the resin molded article according to this embodiment as a sliding member. In the gear member, stress tends to concentrate at the tooth base of the multiple teeth T arranged continuously along the outer periphery, but by configuring the gear member as the resin molded article according to this embodiment, the occurrence of chipping of the teeth T can be effectively suppressed.
[0039] [Examples and Comparative Examples] Examples and comparative examples of the above embodiment will be described.
[0040] (Examples 1 to 3 and Comparative Examples 1 and 2) In Examples 1 to 3 and Comparative Examples 1 and 2, samples of resin molded bodies were prepared and each sample was evaluated. In all of Examples 1 to 3 and Comparative Example 2, carbon black was used as the carbon powder constituting the dispersed phase. Comparative Example 1 differs from the above embodiment in that no dispersed phase was used and no electron beam irradiation was performed. Comparative Example 2 differs from the above embodiment in that no electron beam irradiation was performed.
[0041] A common aromatic polyether ketone was used in all of Examples 1 to 3 and Comparative Examples 1 and 2. Specifically, a polyether ether ketone "Vestakeep (registered trademark) 5000G" manufactured by Polypla-Evonik was used as the aromatic polyether ketone in all of Examples 1 to 3 and Comparative Examples 1 and 2.
[0042] The same carbon black was used in all of Examples 1 to 3 and Comparative Example 2. Specifically, carbon black "#750B" manufactured by Mitsubishi Chemical Corporation was used in all of Examples 1 to 3 and Comparative Example 2. Note that in Comparative Example 1, no carbon black was used, that is, only aromatic polyether ketone was used.
[0043] Table 1 shows the electron beam irradiation temperature and irradiation dose in Examples 1 to 3. In Examples 1 and 3, the electron beam was irradiated to a sample at room temperature, and in Example 2, the electron beam was irradiated to a sample heated to 250° C. Table 1 also shows the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the samples and the crystallite size of the matrix phase of the samples in Examples 1 to 3 and Comparative Examples 1 and 2.
[0044] The area ratio of the dispersed phase of each sample was obtained from a photograph of each sample taken with a fluorescent microscope "BX53M" manufactured by Olympus Corporation. The crystallite size of the matrix phase of each sample was obtained from the diffraction pattern of each sample obtained by measurement with an X-ray diffraction device "Samartlab" manufactured by Rigaku Corporation.
[0045] In addition, the area ratio of the dispersed phase and the crystallite size of the matrix phase were determined in the surface layer portion for all of the samples according to Examples 1 to 3. That is, the area ratio of the dispersed phase and the crystallite size of the matrix phase shown in Table 1 are the results obtained for the surface layer portion of the sample.
[0046] As shown in Table 1, in all of Examples 1 to 3, the crystallite size of the matrix phase was larger than that of Comparative Example 1. In contrast, in Comparative Example 2, the crystallite size of the matrix phase was equivalent to that of Comparative Example 1. This confirmed that irradiation with electron beams is effective in increasing the crystallite size of the matrix phase in the surface layer. In particular, the crystallite size was the largest in Example 2, and it was confirmed that heating the sample during irradiation with electron beams is even more effective in increasing the crystallite size.
[0047] [Table 1]
[0048] A tensile test was carried out to evaluate the fracture properties of each sample according to Examples 1 to 3 and Comparative Examples 1 and 2. An "AGX" manufactured by Shimadzu Corporation was used for the tensile test. In the tensile test, each sample was made into an A12 dumbbell shape conforming to JIS K7139 (2009), the tensile speed was 10 mm / min, and the other conditions were the same.
[0049] As a result, in Table 2, the yield strength, yield stroke, and tensile product for Examples 1 to 3 and Comparative Examples 1 and 2 are shown as percentage changes (%) relative to Comparative Example 1. The yield strength and yield stroke were obtained from the stress-strain curve obtained in the tensile test, and the tensile product was calculated from the yield strength and yield stroke.
[0050] In all of Examples 1 to 3, the yield stroke was significantly improved, and the tensile product was 15% or more higher than in Comparative Example 1. On the other hand, the yield stroke in Comparative Example 2 was smaller than in Examples 1 to 3. This confirmed that a large elongation could be obtained by increasing the crystallite size of the matrix phase in the surface layer portion.
[0051] Next, a gear durability test was conducted on each sample according to Examples 1 to 3 and Comparative Examples 1 and 2 in order to evaluate the product characteristics as a gear member. In the gear durability test, each sample had a gear shape. In the gear durability test for each sample, a gear member (made of S45C) was used as a mating member, and the sample was rotated while meshed with the mating member.
[0052] In addition, the gear durability tests for each sample were conducted under the same conditions, with a rotation speed of 1000 rpm and a torque of 10 N·m. Grease was used as a lubricant between each sample and the mating material during rotation. Each sample was judged as "OK" or "NG" based on the presence or absence of chipped teeth after 1.1 million rotations.
[0053] Table 2 shows the results of the gear durability test for Examples 1 to 3 and Comparative Examples 1 and 2. No chipping of teeth occurred in any of the samples according to Examples 1 to 3, whereas chipping of teeth occurred in all of the samples according to Comparative Examples 1 and 2. This shows that Examples 1 to 3 provide high product characteristics as gear members.
[0054] [Table 2]
[0055] (Examples 4 and 5) In Examples 4 and 5, samples of resin molded bodies were prepared and each sample was evaluated. In both Examples 4 and 5, carbon nanotubes were used as the carbon powder constituting the dispersed phase. In both Examples 4 and 5, aromatic polyether ketone was used in common with Examples 1 to 3 and Comparative Examples 1 and 2.
[0056] Moreover, the same carbon nanotube was used in both Examples 4 and 5. Specifically, the carbon nanotube "NC7000" manufactured by Nanocyl Corporation was used in both Examples 4 and 5.
[0057] Table 3 shows the irradiation temperature and irradiation dose of the electron beam in Examples 4 and 5. In Example 4, the sample heated to 250°C was irradiated with the electron beam, and in Example 5, the sample at room temperature was irradiated with the electron beam. Table 3 also shows the area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the samples in Examples 4 and 5 and Comparative Example 1, and the crystallite size of the matrix phase of the samples. The area ratio of the dispersed phase and the crystallite size of the matrix phase in each sample were determined by the same method as in Examples 1 to 3 and Comparative Examples 1 and 2.
[0058] In addition, the area ratio of the dispersed phase and the crystallite size of the matrix phase were determined in the surface layer portion for each of the samples according to Examples 4 and 5. That is, the area ratio of the dispersed phase and the crystallite size of the matrix phase shown in Table 3 are the results obtained for the surface layer portion of each of the samples.
[0059] As shown in Table 3, in both Examples 4 and 5, the crystallite size of the matrix phase was larger than that of Comparative Example 1. In particular, in Example 4, in which the area ratio of the dispersed phase was large, a significantly larger crystallite size was obtained. This confirmed that the effect of promoting grain growth of crystallites was obtained by having a large amount of carbon nanotubes with high thermal conductivity.
[0060] [Table 3]
[0061] For each sample according to Examples 4 and 5, in order to evaluate the fracture properties, a tensile test was carried out in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. As a result, Table 4 shows the yield strength, yield stroke, and tensile product of Examples 4 and 5 and Comparative Example 1 as a percentage change (%) relative to Comparative Example 1.
[0062] In both Examples 4 and 5, the yield strength and the yield stroke were improved compared to Comparative Example 1, and the tensile product was 35% or more higher. In particular, in Example 4, in which the area ratio of the dispersed phase was large, both the yield strength and the yield stroke were significantly large. This confirmed that a large tensile product could be obtained by increasing the crystallite size of the matrix phase.
[0063] Next, in order to evaluate the product characteristics as gear members for each sample according to Examples 4 and 5 and Comparative Example 1, a gear durability test was conducted in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2. Table 4 shows the results of the gear durability test for Examples 4 and 5 and Comparative Example 1. No chipping of teeth occurred in any of the samples according to Examples 4 and 5. This shows that Examples 4 and 5 have high product characteristics as gear members.
[0064] [Table 4]
[0065] [Other embodiments] Although the embodiment of the present invention has been described above, the present invention is not limited to the above-mentioned embodiment, and various modifications can be made thereto.
[0066] For example, in the resin molded article of the present invention, the molecular weight of the aromatic polyether ketone constituting the matrix phase is not particularly limited as long as sufficient mechanical strength is obtained depending on the application, etc. In other words, the aromatic polyether ketone constituting the matrix phase may have a maximum peak molecular weight in any range in the molecular weight distribution.
[0067] Furthermore, the aromatic polyetherketone constituting the matrix phase of the resin molded article of the present invention may be other than polyetheretherketone (PEEK), and may be, for example, polyetherketone (PEK), polyetherketoneketone (PEKK), polyetheretherketoneketone (PEEKK), polyetherketoneetherketoneketone (PEKEKK), etc. Furthermore, the matrix phase of the resin molded article of the present invention may be a blend of multiple types of aromatic polyetherketones.
[0068] Furthermore, in the present invention, the method for increasing the crystallite size of the surface layer of the aromatic polyether ketone molded article is not limited to electron beam irradiation. Other methods for increasing the crystallite size of the surface layer include, for example, laser irradiation, UV irradiation, excimer irradiation, plasma irradiation, corona irradiation, flame treatment, chemical treatment, etc.
Claims
1. A matrix phase composed of an aromatic polyether ketone; a dispersed phase composed of at least one of carbon black and carbon nanotubes and dispersed in the matrix phase; Including, A surface layer portion in which the crystallite size of the matrix phase is greater than 63 Å; an inner portion constituting an inner side of the surface layer portion, the crystallite size of the matrix phase being smaller than that of the surface layer portion; It consists of Aromatic polyether ketone molding.
2. The aromatic polyether ketone molded article according to claim 1, The aromatic polyether ketone constituting the matrix phase has a molecular weight distribution in which the maximum peak molecular weight is in the range of 50,000 or more. Aromatic polyether ketone molding.
3. The aromatic polyether ketone molded article according to claim 1, the dispersed phase is composed of carbon black; The area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer portion is 0.6% or more. Aromatic polyether ketone molding.
4. The aromatic polyether ketone molded article according to claim 1, the dispersed phase is composed of carbon nanotubes, The area ratio of the region occupied by the dispersed phase having a particle size of 0.1 μm or more in the surface layer portion is 1.9% or more. Aromatic polyether ketone molding.
5. The aromatic polyether ketone molded article according to claim 1, The matrix phase is composed of polyether ether ketone. Aromatic polyether ketone molding.
6. The aromatic polyether ketone molded article according to claim 1, Configured as a sliding member Aromatic polyether ketone molding.
7. The aromatic polyether ketone molded article according to claim 6, Configured as a gear member Aromatic polyether ketone molding.
8. A molded body is produced by an injection molding method, in which a dispersed phase composed of at least one of carbon black and carbon nanotubes is dispersed in a matrix phase composed of an aromatic polyether ketone; The surface of the molded body is irradiated with an electron beam. A method for producing an aromatic polyether ketone molded article.