Method for producing oxidized cellulose nanofiber dispersion

The method of stirring and standing cellulose nanofibers at specific conditions enhances viscosity retention, addressing the issue of viscosity loss during mixing, thereby maintaining effective thickening performance.

JP2024138861APending Publication Date: 2024-10-09NIPPON PAPER IND CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023049573
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Cellulose nanofibers experience significant viscosity reduction when stirred during mixing with partners that impart a thickening function, leading to ineffective thickening performance.

Method used

A method involving a stirring step at 2000 to 6000 rpm for 1 to 90 minutes, followed by a standing step at 4 to 35°C for 12 hours or more, and optionally a dilution step to produce an oxidized cellulose nanofiber dispersion with improved viscosity retention.

Benefits of technology

The method effectively suppresses viscosity reduction before and after stirring, maintaining effective thickening properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138861000001
    Figure 2024138861000001
  • Figure 2024138861000002
    Figure 2024138861000002
Patent Text Reader

Abstract

To provide a method for producing an oxidized cellulose nanofiber dispersion that is capable of suppressing viscosity loss before and after agitation when mixed with a counterpart to which thickening function is imparted.SOLUTION: There is provided a method for producing oxidized cellulose nanofiber dispersion including: a stirring step for stirring an oxidized cellulose nanofiber dispersion having a solid concentration of 0.1 to 5.0 mass% for 1 to 90 minutes under a condition of a rotational speed of 2000 to 6000 rpm; and, after the stirring step, a leaving step of allowing the oxidized cellulose nanofiber dispersion to leave at a temperature of 4 to 35°C for 12 hours or longer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention. [Background technology]

[0002] Nanotechnology, a technique for freely controlling substances in the nanometer range, that is, at the atomic and molecular scale, is expected to produce a variety of convenient new materials and devices. One such example is cellulose nanofiber, which is obtained by finely breaking down plant fibers. This cellulose nanofiber is highly crystalline and features a low thermal expansion coefficient and high elastic modulus. In addition, it has a high aspect ratio, so it is expected that it will have the effect of adding strength and stabilizing shape when compounded with rubber or resin. In addition, this cellulose nanofiber has viscosity characteristics such as pseudoplasticity and thixotropy in the dispersed state, and it is expected to be effective as an additive such as a thickener.

[0003] Various developments and researches on cellulose nanofibers have been conducted, and for example, Patent Document 1 discloses fine cellulose fibers (cellulose nanofibers) in which some of the hydroxyl groups of cellulose are converted to carboxyl groups and have a number average fiber diameter of 2 to 150 nm. These cellulose nanofibers have the property of having high viscosity at low shear rates and low viscosity at high shear rates. Because of these viscosity characteristics, cellulose nanofibers are used as a thickening agent in various fields such as cosmetics, food, civil engineering, building materials, inks, and paints. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2008-1728 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, when the cellulose nanofibers described in Patent Document 1 are used as a thickener, there is a problem in that the viscosity is significantly reduced when a stirring process is carried out during mixing with the other substance to which the thickening function is to be imparted.

[0006] Therefore, the present invention aims to provide a method for producing an oxidized cellulose nanofiber dispersion that is capable of suppressing the decrease in viscosity before and after stirring when a stirring process is carried out when mixing with an agent that imparts a thickening function. [Means for solving the problem]

[0007] The present invention provides the following (1) to (5). (1) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention, comprising a stirring step of stirring an oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0% by mass at a rotation speed of 2000 to 6000 rpm for 1 to 90 minutes, and a standing step of standing the oxidized cellulose nanofiber dispersion at a temperature of 4 to 35°C for 12 hours or more after the stirring step. (2) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention as described in (1), further comprising a dilution step of diluting the oxidized cellulose nanofiber dispersion to a solids concentration of 0.1 to 0.8 mass % after the standing step. (3) The method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to (1) or (2), wherein the oxidized cellulose nanofiber has a carboxyl amount of 0.2 to 2.0 mmol / g relative to the bone dry mass of the oxidized cellulose nanofiber. (4) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention described in (2), characterized in that in the dilution step, 5 to 100 parts by mass of a dispersant is further added per 100 parts by mass of the solid content of the oxidized cellulose nanofiber. (5) A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention as described in (2), further comprising, after the dilution step, a step of adding 5 to 100 parts by mass of a dispersant per 100 parts by mass of the solid content of oxidized cellulose nanofibers in the oxidized cellulose nanofiber dispersion, and mixing. Effect of the Invention

[0008] According to the present invention, it is possible to provide a method for producing an oxidized cellulose nanofiber dispersion that is capable of suppressing the decrease in viscosity before and after stirring when a stirring process is carried out when mixing with a counterpart that imparts a thickening function. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The method for producing an oxidized cellulose nanofiber (oxidized CNF) dispersion with improved viscosity retention of the present invention includes a stirring step in which an oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0 mass% is stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which the oxidized cellulose nanofiber dispersion is allowed to stand at a temperature of 4 to 35°C for 12 hours or more after the stirring step.

[0010] (Oxidized Cellulose Nanofiber (Oxidized CNF)) The oxidized CNF used in the present invention can be obtained by defibrating oxidized cellulose obtained by introducing carboxyl groups into a cellulose raw material.

[0011] (raw materials) Examples of cellulose raw materials include plant materials (e.g., wood, bamboo, hemp, jute, kenaf, agricultural waste, cloth, pulp (softwood unbleached kraft pulp (NUKP), softwood bleached kraft pulp (NBKP), hardwood unbleached kraft pulp (LUKP), hardwood bleached kraft pulp (LBKP), softwood unbleached sulfite pulp (NUSP), softwood bleached sulfite pulp (NBSP), thermomechanical pulp (TMP), recycled pulp, waste paper, etc.), animal materials (e.g., ascidians), algae, microorganisms (e.g., acetic acid bacteria (Acetobacter)), and those derived from microbial products, and any of these can be used. Cellulose raw materials derived from plants or microorganisms are preferred, and cellulosic raw materials derived from plants are more preferred.

[0012] (Introduction of carboxyl group) Carboxyl groups can be introduced into the above-mentioned cellulose raw material by oxidizing (carboxylating) it by a known method.

[0013] One example of oxidation is a method in which a cellulose raw material is oxidized in water using an oxidizing agent in the presence of an N-oxyl compound, a bromide, an iodide, or a mixture thereof. This oxidation reaction selectively oxidizes the primary hydroxyl group at the C6 position of the pyranose ring on the cellulose surface. As a result, oxidized cellulose having aldehyde groups and carboxyl groups (-COOH) or carboxylate groups (-COO-) on the surface can be obtained. The concentration of cellulose during the reaction is not particularly limited, but is preferably 5% by mass or less.

[0014] The term "N-oxyl compound" refers to a compound capable of generating a nitroxy radical. Any compound that can promote the desired oxidation reaction can be used as the N-oxyl compound. For example, 2,2,6,6-tetramethylpiperidine-1-oxy radical (TEMPO) and its derivatives (e.g., 4-hydroxyTEMPO) can be mentioned.

[0015] The amount of the N-oxyl compound used is not particularly limited as long as it is a catalytic amount capable of oxidizing the raw cellulose. The amount is preferably 0.01 mmol to 10 mmol, more preferably 0.01 mmol to 1 mmol, and even more preferably 0.05 mmol to 0.5 mmol, per 1 g of bone dry cellulose. The concentration of the N-oxyl compound is preferably about 0.1 mmol / L to 4 mmol / L in the reaction system.

[0016] Bromides are compounds that contain bromine, including alkali metal bromides that can dissociate and ionize in water, while iodides are compounds that contain iodine, including alkali metal iodides.

[0017] The amount of bromide or iodide used can be selected within a range that can promote the oxidation reaction. The total amount of bromide and iodide is preferably 0.1 mmol to 100 mmol, more preferably 0.1 mmol to 10 mmol, and even more preferably 0.5 mmol to 5 mmol, per 1 g of bone-dry cellulose.

[0018] The oxidizing agent may be any known oxidizing agent, such as halogen, hypohalous acid, halous acid, perhalogen acid or their salts, halogen oxides, peroxides, etc. Among these, sodium hypochlorite is preferred, which is inexpensive and has a low environmental impact.

[0019] The amount of the oxidizing agent used is preferably 0.5 mmol to 500 mmol, more preferably 0.5 mmol to 50 mmol, and even more preferably 1 mmol to 25 mmol, per 1 g of bone-dry cellulose, and is preferably 1 mol to 40 mol per 1 mol of the N-oxyl compound, for example.

[0020] The cellulose oxidation process can proceed efficiently even under relatively mild conditions. Therefore, the reaction temperature is preferably 4°C to 40°C, and may be room temperature of about 15°C to 30°C. As the reaction proceeds, carboxyl groups are generated in the cellulose, and the pH of the reaction solution decreases. In order to efficiently proceed with the oxidation reaction, it is preferable to add an alkaline solution such as an aqueous sodium hydroxide solution during the reaction to maintain the pH of the reaction solution at about 8 to 12, preferably 10 to 11. The reaction medium is preferably water, for reasons such as ease of handling and the fact that side reactions are unlikely to occur.

[0021] The reaction time in the oxidation reaction can be appropriately set according to the degree of progress of the oxidation, and is usually 0.5 to 6 hours, preferably 0.5 to 4 hours.

[0022] The oxidation reaction may also be carried out in two stages. For example, the oxidized cellulose obtained by filtering after completion of the first-stage reaction can be oxidized again under the same or different reaction conditions, allowing efficient oxidation without reaction inhibition by table salt produced as a by-product in the first-stage reaction.

[0023] Another example is a method of oxidizing cellulose raw materials by contacting them with a gas containing ozone, which oxidizes at least the hydroxyl groups at positions 2 and 6 of the pyranose ring and decomposes the cellulose chain.

[0024] The ozone concentration in the ozone-containing gas is preferably 50 g / m3 to 250 g / m3, and more preferably 50 g / m3 to 220 g / m3. The amount of ozone added to the cellulose raw material is preferably 0.1 parts by mass to 30 parts by mass, and more preferably 5 parts by mass to 30 parts by mass, based on 100 parts by mass of the solid content of the cellulose raw material.

[0025] The ozone treatment temperature is preferably 0° C. to 50° C., and more preferably 20° C. to 50° C. The ozone treatment time is not particularly limited, but is about 1 minute to 360 minutes, and preferably about 30 minutes to 360 minutes. When the ozone treatment conditions are within these ranges, excessive oxidation and decomposition of cellulose can be prevented, and the yield of oxidized cellulose is good.

[0026] After the ozone treatment, an additional oxidation treatment may be performed using an oxidizing agent. The oxidizing agent used in the additional oxidation treatment is not particularly limited, and examples thereof include chlorine compounds such as chlorine dioxide and sodium chlorite, oxygen, hydrogen peroxide, persulfuric acid, and peracetic acid. For example, the additional oxidation treatment can be performed by dissolving these oxidizing agents in a polar organic solvent such as water or alcohol to prepare an oxidizing agent solution, and immersing the cellulose raw material in the solution.

[0027] The amount of carboxyl groups, which indicates the degree of modification of oxidized cellulose, can be adjusted by controlling the reaction conditions such as the amount of oxidizing agent added and the reaction time. The amount of carboxyl groups is preferably about 0.2 to 2.0 mmol / g, more preferably 0.5 to 1.6 mmol / g, based on the bone dry mass of oxidized cellulose. If it is less than 0.2 mmol / g, a large amount of energy is required to defibrate it into oxidized CNF. If more than 2.0 mmol of oxidized cellulose is used as a raw material, the obtained oxidized CNF does not have a fibrous form. The amount of carboxyl groups in oxidized cellulose is usually the same as the amount of carboxyl groups when it is made into cellulose nanofibers.

[0028] (Defibrilization) The device used for defibration is not particularly limited, but examples include devices of high-speed rotation type, colloid mill type, high pressure type, roll mill type, ultrasonic type, etc., and a high-pressure or ultra-high pressure homogenizer is preferable, and a wet high-pressure or ultra-high pressure homogenizer is more preferable. The device is preferably capable of applying a strong shear force to the cellulose raw material or oxidized cellulose (usually a dispersion liquid). The pressure that the device can apply is preferably 50 MPa or more, more preferably 100 MPa or more, and even more preferably 140 MPa or more. The device is preferably a wet high-pressure or ultra-high pressure homogenizer that can apply the above pressure to the cellulose raw material or oxidized cellulose (usually a dispersion liquid) and can apply a strong shear force. This allows efficient defibration. The number of treatments (passes) in the defibration device may be one or two or more, and two or more are preferred.

[0029] In the dispersion process, oxidized cellulose is usually dispersed in a solvent. The solvent is not particularly limited as long as it can disperse oxidized cellulose, but examples include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixtures thereof. Since the cellulose raw material is hydrophilic, it is preferable that the solvent is water.

[0030] The solids concentration of oxidized cellulose in the dispersion is usually 0.1% by mass or more, preferably 0.2% by mass or more, and more preferably 0.3% by mass or more. This ensures that the amount of liquid relative to the amount of cellulose fiber raw material is appropriate and efficient. The upper limit is usually 10% by mass or less, and preferably 6% by mass or less. This allows fluidity to be maintained.

[0031] The order of the defibration treatment and the dispersion treatment is not particularly limited, and either may be performed first, or they may be performed simultaneously, but it is preferable to perform the defibration treatment after the dispersion treatment. Each combination of treatments needs to be performed at least once, and may be repeated two or more times.

[0032] Prior to the defibration or dispersion treatment, a pretreatment may be carried out as necessary. The pretreatment may be carried out using a mixing, stirring, emulsifying or dispersing device such as a high-speed shear mixer.

[0033] The average fiber diameter of the oxidized CNF of the present invention is preferably 3 nm or more or 500 nm or less. The average fiber diameter and average fiber length of the cellulose nanofibers can be measured, for example, by preparing a 0.001 mass% aqueous dispersion of oxidized CNF, spreading this diluted dispersion thinly on a mica sample stage, and drying it by heating at 50°C to prepare a sample for observation, and measuring the cross-sectional height of the shape image observed with an atomic force microscope (AFM) to calculate the number average fiber diameter or fiber length.

[0034] The average aspect ratio of the oxidized CNF is usually 50 or more. There is no upper limit, but it is usually 1000 or less. The average aspect ratio can be calculated by the following formula: Aspect ratio = average fiber length / average fiber diameter

[0035] (Mixing process) In the stirring step of the present invention, the oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0% by mass is stirred for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm. The solid content concentration of the oxidized CNF dispersion to be subjected to the stirring step is 0.1 to 5.0% by mass, preferably 0.1 to 3.0% by mass. If the concentration is too high, stirring becomes difficult, and if the concentration is too low, the amount of CNF added when added to other materials becomes low, making it difficult to use as a thickener. As the oxidized CNF dispersion to be subjected to the stirring step, the oxidized CNF dispersion after the above-mentioned dispersion and defibration treatment can be subjected to the stirring step as it is, so long as the solid content concentration is within the above range. The solid content concentration can be adjusted by dilution, dehydration, etc. as appropriate. The rotation speed in the stirring step is 2000 to 6000 rpm, preferably 2000 to 3000 rpm, from the viewpoint of thoroughly stirring the entire CNF dispersion. The stirring time is from 1 to 90 minutes, preferably from 5 to 60 minutes, and more preferably from 10 to 60 minutes, from the viewpoint of imparting a shear effect by stirring to the entire CNF dispersion.

[0036] The stirrer used in the stirring process is not particularly limited as long as it can stir an oxidized CNF dispersion having a solid content concentration of 0.1 to 5.0 mass% at the above rotation speed, and examples of such a stirrer include a high-speed stirrer and a high-speed emulsifying disperser. As a high-speed stirrer, for example, a Homo Disper manufactured by Primix Corporation can be used.

[0037] (Standing process) In the standing step of the present invention, the oxidized CNF dispersion after the stirring step is allowed to stand at a temperature of 4 to 35°C, preferably 6 to 25°C, for 12 hours or more, preferably 24 hours or more. The upper limit of the standing time is not particularly limited, but is, for example, 10 days or less from the viewpoint of long-term storage. If the standing time is too short, there is a risk that the temporary viscosity reduction immediately after stirring will not recover. In the standing step, it is preferable to place the oxidized CNF dispersion in a container and stand it in order to prevent evaporation of water in the CNF dispersion. The material of the container is not particularly limited, and may be a glass bottle or a plastic bottle. It is preferable that the container can be closed with a lid.

[0038] (Dilution process) The manufacturing method of the present invention may include a dilution step after the standing step. When the dilution step is included, the oxidized CNF is diluted until the solid content concentration is preferably 0.1 to 0.8% by mass, more preferably 0.1 to 0.6% by mass. The solvent used for dilution may be the same as or different from the solvent of the dispersion before dilution, and examples thereof include water, organic solvents (e.g., hydrophilic organic solvents such as methanol), and mixed solvents thereof. Since the cellulose raw material is hydrophilic, the solvent is preferably water. In the dilution step, the stirring and mixing conditions are not particularly limited as long as the dilution can be performed uniformly, but the dilution is performed, for example, by stirring at a rotation speed of 1000 rpm for 10 minutes.

[0039] (Dispersant) The oxidized CNF dispersion produced by the production method of the present invention may contain a dispersant. When a dispersant is added, the amount of the dispersant added is preferably 5 to 100 parts by mass, more preferably 10 to 50 parts by mass, per 100 parts by mass of the solid content of the oxidized CNF, from the viewpoint of the solid content of the CNF. The type of dispersant may be used without particular limitation as long as it exhibits the effects of the present invention, and examples thereof include polyacrylic acid, carboxymethyl cellulose, and polyurethane dispersants.

[0040] In the case where a dispersant is included, the step of adding the dispersant is not particularly limited as long as the effect of the present invention is exhibited. However, the dispersant may be added in the stirring step, the dispersant may be added in the dilution step, or a step of adding the dispersant and mixing may be provided after the dilution step. In addition, when the dilution step is not provided, a step of adding the dispersant and mixing may be provided after the standing step. In the case where the dispersant is added and mixed in a step other than the stirring step and the dilution step, the device used for stirring and mixing is not particularly limited, and a commonly used stirring device may be used. The stirring time is also not particularly limited, and stirring may be performed within a range of about 1 minute to 1 hour.

[0041] (viscosity retention rate) The viscosity retention rate of an oxidized cellulose nanofiber dispersion can be calculated from the viscosity before and after stirring determined by the stability test described below, using the following formula. Viscosity retention rate (%) = (viscosity after stirring / viscosity before stirring) x 100

[0042] (Stability test) For the oxidized cellulose nanofiber dispersion immediately after the dilution step, a B-type viscometer is used to measure the B-type viscosity at 6 rpm, 23°C, and for 1 minute (viscosity before stirring). If the dilution step is not required, the viscosity before stirring can be measured under the same conditions for the dispersion to which shear force has been applied by stirring (1000 rpm, 10 minutes) after the standing step, and if the method includes a step of adding and mixing a dispersant after the dilution step, the viscosity before stirring can be measured under the same conditions for the dispersion after that step.

[0043] After the B-type viscosity measurement, the oxidized cellulose nanofiber dispersion is stirred for 30 minutes (1000 rpm, 23°C) using a high-speed stirrer. Immediately after stirring for 30 minutes, the B-type viscosity is measured using a B-type viscometer at 6 rpm, 23°C, and 1 minute (viscosity after stirring). As the high-speed stirrer, for example, a Homo Disper manufactured by Primix Corporation can be used.

[0044] According to the production method of the present invention, it is possible to produce an oxidized cellulose nanofiber dispersion with improved viscosity retention.

[0045] The reason why the production method of the present invention makes it possible to obtain an oxidized cellulose nanofiber dispersion with improved viscosity retention is believed to be as follows. It is possible to obtain cellulose nanofibers by defibrating oxidized cellulose, and in the cellulose nanofibers obtained in this way, each fiber is swollen (defibrated) to the nano level, but the physical entanglements of the cellulose fibers that existed before defibration remain. When such a dispersion of oxidized cellulose nanofibers is stirred under the stability test conditions (1000 rpm, 23°C), the entangled nanofibers become loose, changing the dispersion state, and the loosened nanofibers become oriented in a certain direction, resulting in the development of pseudoplasticity and a decrease in viscosity. In the production method of the present invention, a stirring step is provided before the stability test, and therefore physical entanglements of the cellulose fibers remaining after defibration can be eliminated in the stirring step. Therefore, the decrease in viscosity before and after the stability test is suppressed, and as a result, an oxidized cellulose nanofiber dispersion with improved viscosity retention can be produced. EXAMPLES

[0046] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0047] (Method for measuring the amount of carboxyl groups) 60 mL of a 0.5% by mass slurry (aqueous dispersion) of oxidized cellulose was prepared, and a 0.1 M aqueous hydrochloric acid solution was added to adjust the pH to 2.5. A 0.05 N aqueous sodium hydroxide solution was then added dropwise, and the electrical conductivity was measured until the pH reached 11. The electrical conductivity was calculated using the following formula from the amount of sodium hydroxide (a) consumed in the neutralization stage of the weak acid, where the change in electrical conductivity was gradual: Amount of carboxyl groups [mmol / g oxidized cellulose] = a [mL] × 0.05 / oxidized cellulose Base mass [g]

[0048] (Stability test) For the oxidized cellulose nanofiber aqueous dispersions of the Examples and Comparative Examples, immediately after the dilution step, the B-type viscosity was measured using a B-type viscometer at 6 rpm, 23°C, and for 1 minute (viscosity before stirring).

[0049] The oxidized cellulose nanofiber aqueous dispersion after measuring the B-type viscosity was stirred for 30 minutes (1000 rpm, 23°C) using a high-speed stirrer (Homodisper, manufactured by Primix Corporation). Immediately after stirring for 30 minutes, the B-type viscosity was measured using a B-type viscometer at 6 rpm, 23°C, and 1 minute (viscosity after stirring).

[0050] (viscosity retention rate) The viscosity retention rate was calculated according to the following formula using the viscosity before stirring and the viscosity after stirring measured in the stability test. Formula: Viscosity retention rate (%) = (viscosity after stirring / viscosity before stirring) x 100

[0051] (Manufacturing example A) (Production of oxidized cellulose nanofiber aqueous dispersion A) 5.00 g (bone-dry) of bleached, unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 5.1 mmol / g, and the oxidation reaction was started. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 90%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as the "degree of modification") was 1.46 mmol / g. This was adjusted to 1.0 mass% with water and defibrated three times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion A. The average fiber diameter was 4 nm, and the aspect ratio was 270.

[0052] (Manufacturing example B) (Production of oxidized cellulose nanofiber aqueous dispersion B) 5.00 g (bone-dry) of bleached, unbeaten kraft pulp (85% whiteness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 3.4 mmol / g, and the oxidation reaction was started. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 92%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as the "degree of modification") was 1.1 mmol / g. This was adjusted to 1.0 mass% with water and defibrated three times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion B. The average fiber diameter was 4 nm, and the aspect ratio was 273.

[0053] (Manufacturing example C) (Production of oxidized cellulose nanofiber aqueous dispersion C) 5.00 g (bone-dry) of bleached, unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 1.0 mmol / g, and the oxidation reaction was started. During the reaction, the pH of the system decreased, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 93%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups (hereinafter sometimes referred to as "degree of modification") was 0.58 mmol / g. This was adjusted to 1.0 mass% with water and defibrated five times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion C. The average fiber diameter was 4 nm, and the aspect ratio was 290.

[0054] (Manufacturing example D) (Production of oxidized cellulose nanofiber aqueous dispersion D) 5.00 g (bone-dry) of bleached, unbeaten kraft pulp (85% brightness) derived from coniferous trees was added to 500 mL of an aqueous solution containing 20 mg (0.025 mmol per 1 g of bone-dry cellulose) of TEMPO (Sigma Aldrich) and 514 mg (1.0 mmol per 1 g of bone-dry cellulose) of sodium bromide, and the mixture was stirred until the pulp was uniformly dispersed. An aqueous solution of sodium hypochlorite was added to the reaction system so that the sodium hypochlorite concentration was 2.2 mmol / g, and the oxidation reaction was started. The pH of the system decreased during the reaction, but 3 M aqueous sodium hydroxide was added successively to adjust the pH to 10. The reaction was terminated when the sodium hypochlorite was consumed and the pH of the system no longer changed. The mixture after the reaction was filtered through a glass filter to separate the pulp, and the pulp was thoroughly washed with water to obtain oxidized pulp (oxidized cellulose). The pulp yield was 93%, the time required for the oxidation reaction was 60 minutes, and the amount of carboxyl groups was 0.76 mmol / g. This was adjusted to 1.0 mass% with water and defibrated five times using a high-pressure homogenizer to obtain oxidized cellulose nanofiber aqueous dispersion D. The average fiber diameter was 4 nm, and the aspect ratio was 280.

[0055] Example 1 (Mixing process) The oxidized cellulose nanofiber aqueous dispersion A having a solid content concentration of 1.0 mass % obtained in Production Example A was subjected to stirring treatment for 5 minutes at a rotation speed of 3000 rpm using a high-speed stirrer (Homodisper, manufactured by Primix Corporation).

[0056] (Standing process) The oxidized cellulose nanofiber aqueous dispersion A that had been subjected to the stirring treatment in the above stirring step was placed in a plastic container and allowed to stand at 23°C for 7 days.

[0057] (Dilution process) The oxidized cellulose nanofiber aqueous dispersion A that had been subjected to the standing process was placed in a plastic container, deionized water was added, and the mixture was stirred (1000 rpm, 10 minutes) to obtain oxidized cellulose nanofiber aqueous dispersion A diluted to a solids concentration of 0.5 mass%.

[0058] A stability test was conducted on this diluted oxidized cellulose nanofiber aqueous dispersion A, and the B-type viscosity values ​​before and after stirring were obtained. The results are shown in Table 1.

[0059] (Examples 2 to 4) Except for changing the stirring time to 15 minutes (Example 2), 30 minutes (Example 3), and 60 minutes (Example 4), the stirring step, the standing step, and the dilution step were carried out in the same order as in Example 1, and a stability test was carried out. The results are shown in Table 1.

[0060] Example 5 A stability test was carried out by carrying out the stirring step, standing step, and dilution step in the same order as in Example 1, except that oxidized cellulose nanofiber aqueous dispersion B obtained in Production Example B was used. The results are shown in Table 1.

[0061] (Examples 6 to 8) A stability test was carried out by carrying out the stirring step, the standing step, and the dilution step in the same order as in Example 5, except that the stirring time in the stirring step was changed to 15 minutes (Example 6), 30 minutes (Example 7), and 60 minutes (Example 8), respectively. The results are shown in Table 1.

[0062] Example 9 Except for using the oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C, a stability test was carried out by carrying out the stirring step, standing step, and dilution step in that order in the same manner as in Example 1. The results are shown in Table 1.

[0063] (Examples 10 to 12) Stability tests were carried out in the same order as in Example 9, with the exception that the stirring time in the stirring step was changed to 15 minutes (Example 10), 30 minutes (Example 11), and 60 minutes (Example 12), respectively. The results are shown in Table 1.

[0064] Comparative Example 1 The standing and dilution steps were carried out in the same manner as in Example 1, except that instead of oxidized cellulose nanofiber aqueous dispersion A which had not been subjected to the stirring step and had been stirred in the standing step, a dispersion which had not been subjected to the stirring step was used, to obtain an oxidized cellulose nanofiber aqueous dispersion with a solid content concentration of 0.5% by mass. A stability test was carried out on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.

[0065] Comparative Example 2 The standing and dilution steps were carried out in the same manner as in Example 5, except that instead of oxidized cellulose nanofiber aqueous dispersion B which had been stirred in the standing step without being subjected to the stirring step, a dispersion which had not been stirred was used, to obtain an oxidized cellulose nanofiber aqueous dispersion with a solid content concentration of 0.5% by mass. A stability test was carried out on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.

[0066] Comparative Example 3 The standing and dilution steps were carried out in the same manner as in Example 9, except that instead of oxidized cellulose nanofiber aqueous dispersion C which had not been subjected to the stirring step and had been stirred in the standing step, a dispersion which had not been subjected to the stirring step was used, to obtain an oxidized cellulose nanofiber aqueous dispersion with a solid content concentration of 0.5% by mass. A stability test was carried out on this oxidized cellulose nanofiber aqueous dispersion. The results are shown in Table 1.

[0067] [Table 1]

[0068] As can be seen from Table 1, when the methods of Examples 1 to 12 were used, which included a stirring step in which a 0.1 to 5.0 mass% oxidized cellulose nanofiber dispersion was subjected to a stirring treatment for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which the oxidized cellulose nanofiber dispersion was allowed to stand at a temperature of 4 to 35°C for 12 hours or more after the stirring step, the obtained oxidized cellulose nanofiber dispersion had an improved viscosity retention rate when compared with Comparative Examples 1 to 3 in which the stirring step was not performed, which had the same degree of modification.

[0069] (Example 13) The oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D was used, and the stirring step and the standing step were carried out in that order in the same manner as in Example 1, except that the stirring treatment time was changed to 15 minutes.

[0070] (Dilution process) The oxidized cellulose nanofiber aqueous dispersion D that had been left to stand was placed in a plastic container, and polyacrylic acid (Aron A-7100, manufactured by Toagosei Co., Ltd., hereafter sometimes abbreviated as "PAA") was added as a dispersant in an amount of 20 parts by mass per 100 parts by mass of the oxidized cellulose nanofiber solids. Deionized water was then added to this plastic container and stirred (1000 rpm, 10 minutes), yielding a dispersion with a solids concentration of oxidized cellulose nanofiber of 0.5% by mass and a dispersant concentration of 0.1% by mass, relative to the total volume of the dispersion.

[0071] The resulting dispersion was subjected to a stability test to obtain the Brookfield viscosity values ​​before and after stirring. The results are shown in Table 2.

[0072] Example 14 A dispersion with a solids concentration of oxidized cellulose nanofiber of 0.5 mass% and a dispersant concentration of 0.1 mass% was obtained in the same manner as in Example 13, except that the dispersant was changed to carboxymethyl cellulose (Sunrose A04SH, manufactured by Nippon Paper Industries Co., Ltd., hereinafter sometimes abbreviated as "CMC"). A stability test was carried out on the obtained dispersion. The results are shown in Table 2.

[0073] Example 15 A dispersion with an oxidized cellulose nanofiber solids concentration of 0.5 mass% and a dispersant concentration of 0.1 mass% was obtained in the same manner as in Example 13, except that the oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C was used instead of the oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D. A stability test was carried out on the obtained dispersion. The results are shown in Table 2.

[0074] (Example 16) A dispersion with an oxidized cellulose nanofiber solids concentration of 0.5 mass% and a dispersant concentration of 0.1 mass% was obtained in the same manner as in Example 14, except that the oxidized cellulose nanofiber aqueous dispersion C obtained in Production Example C was used instead of the oxidized cellulose nanofiber aqueous dispersion D obtained in Production Example D. A stability test was carried out on the obtained dispersion. The results are shown in Table 2.

[0075] (Comparative Examples 4 to 5) The standing and dilution steps were carried out in the same manner as in Examples 13 and 14, except that instead of oxidized cellulose nanofiber aqueous dispersion D which had not been subjected to the stirring process and had been stirred in the standing process, a dispersion which had not been subjected to the stirring process was used, to obtain dispersions of Comparative Examples 4 and 5, respectively, with an oxidized cellulose nanofiber solids concentration of 0.5 mass% and a dispersant concentration of 0.1 mass%. A stability test was carried out on the obtained dispersions. The results are shown in Table 2.

[0076] [Table 2]

[0077] As can be seen from Table 2, when the methods of Examples 13 to 16 were used, which included a stirring step in which a 0.1 to 5.0 mass% oxidized cellulose nanofiber dispersion was subjected to a stirring treatment for 1 to 90 minutes at a rotation speed of 2000 to 6000 rpm, and a standing step in which the oxidized cellulose nanofiber dispersion was allowed to stand at a temperature of 4 to 35°C for 12 hours or more after the stirring step, the obtained oxidized cellulose nanofiber dispersion had improved viscosity retention even when a dispersant was added, compared to Comparative Examples 4 and 5 in which the stirring step was not performed.

Claims

1. a stirring step of stirring an oxidized cellulose nanofiber dispersion having a solid content concentration of 0.1 to 5.0% by mass at a rotation speed of 2000 to 6000 rpm for 1 to 90 minutes; After the stirring step, the oxidized cellulose nanofiber dispersion is allowed to stand at a temperature of 4 to 35° C. for 12 hours or more. A method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention.

2. The method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to claim 1, further comprising a dilution step of diluting the oxidized cellulose nanofiber dispersion to a solids concentration of 0.1 to 0.8 mass % after the standing step.

3. The method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to claim 1 or 2, wherein the oxidized cellulose nanofiber has a carboxyl amount of 0.2 to 2.0 mmol / g relative to the bone dry mass of the oxidized cellulose nanofiber.

4. The method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention described in claim 2, characterized in that in the dilution step, 5 to 100 parts by mass of a dispersant is further added per 100 parts by mass of the solid content of the oxidized cellulose nanofiber.

5. The method for producing an oxidized cellulose nanofiber dispersion with improved viscosity retention according to claim 2, further comprising the step of adding 5 to 100 parts by mass of a dispersant per 100 parts by mass of the solid content of oxidized cellulose nanofibers in the oxidized cellulose nanofiber dispersion after the dilution step, and mixing.

Citation Information

Patent Citations

  • Concentrate of anion-modified cellulose nanofiber, method for the production thereof and dispersion liquid thereof

    JP2016186018A

  • Cellulose nano-fiber dry solid material and production method therefor, and dry solid material re-dispersion

    JP2017002135A

  • Viscous water base composition and method for producing the same

    JP2017110085A

  • Cellulose nanofiber composition and production method therefor

    JP2022102007A

  • Oxidized cellulose, nanocellulose and their dispersions

    JP2022165987A