Active energy ray-curable adhesive composition and adhesive sheet

The active energy ray-curable adhesive composition with specific antioxidants ensures strong adhesion before curing and easy removal after high-temperature exposure, addressing the inadequacies of existing technologies.

JP2024138892APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023049609
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing adhesive compositions fail to provide sufficient releasability under high temperature conditions, such as heat treatment at 175°C, with residual adhesive strength issues.

Method used

An active energy ray-curable adhesive composition containing an acrylic resin and a combination of primary and secondary antioxidants, specifically dimers, trimers, or tetramers without ortho-hydroxyl group binding sites, and phosphorus-based antioxidants, to reduce adhesive strength after irradiation even at high temperatures.

Benefits of technology

The composition achieves excellent releasability with no adhesive residue, maintaining strong adhesive strength before irradiation and reducing it effectively after exposure to high temperatures.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138892000001
    Figure 2024138892000001
  • Figure 2024138892000002
    Figure 2024138892000002
  • Figure 2024138892000003
    Figure 2024138892000003
Patent Text Reader

Abstract

To provide an adhesive which has good adhesive force before irradiation with active energy rays, reduces the adhesive force after irradiation with active energy rays even when being exposed to high temperature, has no adhesive deposit and has excellent peelability.SOLUTION: An active energy ray-curable adhesive composition contains an acrylic resin (A) and an antioxidant (B), where the antioxidant (B) contains a primary antioxidant (B1) and a secondary antioxidant (B2) (excluding antioxidant (B1)), and the primary antioxidant (B1) is a dimer, a trimer or a tetramer, and the secondary antioxidant (B2) is a phosphors-based antioxidant.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an active energy ray-curable pressure-sensitive adhesive composition and a pressure-sensitive adhesive sheet, and more specifically to a pressure-sensitive adhesive composition used as a pressure-sensitive adhesive in a peel-off pressure-sensitive adhesive sheet for temporary surface protection when processing workpieces such as semiconductor wafers, printed circuit boards, processed glass products, metal plates, plastic plates, etc., and in particular to an active energy ray-curable peel-off pressure-sensitive adhesive composition and pressure-sensitive adhesive sheet. [Background technology]

[0002] Conventionally, in the manufacturing process of integrated circuits using semiconductor wafers, such as drilling holes, adhesive sheets for surface protection are used to temporarily protect the surface of the workpiece in order to prevent the workpiece from being soiled or damaged.In recent years, due to the fine processing technology and the thinning of the workpiece, an appropriate adhesive force is required for the workpiece, while after the surface protection function is completed, the adhesive sheet for surface protection must be peeled off, and it is required that the adhesive sheet can be peeled off with a light force without leaving any adhesive residue.In addition, in recent years, adhesive sheets for surface protection are used not only for semiconductor wafers but also for the processing of various other materials.

[0003] For such a pressure-sensitive adhesive sheet, an active energy ray-curable pressure-sensitive adhesive composition that can be cured by irradiation with active energy rays and reduce the adhesive strength is effective, and active energy ray curability is exhibited, for example, by (1) blending at least one of a monomer and an oligomer having an ethylenically unsaturated group with an acrylic resin, or (2) using an ethylenically unsaturated group-containing acrylic resin in which the acrylic resin itself contains an ethylenically unsaturated group. Among them, an ethylenically unsaturated group-containing acrylic resin in which the acrylic resin itself contains an ethylenically unsaturated group has a small amount of low molecular weight components even after curing by irradiation with active energy rays, and is therefore advantageous in reducing adhesive residue after peeling.

[0004] In recent years, in the manufacturing process of electronic components, components with adhesive tape attached are often exposed to high temperatures. For this reason, the adhesive tapes used in the manufacturing process of electronic components are required to have heat resistance so that they can withstand high temperature conditions. Patent document 1 discloses an adhesive sheet coated with an active energy ray-curable adhesive having a glass transition temperature of -50°C or higher and 10°C or lower, and describes that even after heat treatment, the adhesive strength between the wafer chip and the adhesive sheet decreases after irradiation with active energy rays, allowing the wafer chip to be easily picked up.

[0005] Furthermore, Patent Document 2 describes an adhesive that has excellent removable properties even after being exposed to high temperature and humid heat conditions by incorporating a phosphorus-based antioxidant into an acrylic resin.

[0006] Furthermore, Patent Document 3 describes an active energy ray-curable adhesive that contains a hindered phenol-based antioxidant, and thereby has excellent removable properties even after exposure to high temperature and humid heat conditions. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] International Publication 2020 / 100491 [Patent Document 2] JP 2020-158691 A [Patent Document 3] JP 2019-145575 A Summary of the Invention [Problem to be solved by the invention]

[0008] However, in the technology disclosed in Patent Document 1, although the adhesive strength is reduced by irradiation with active energy rays after heat treatment at 150°C and peelability is exhibited, there is a problem that sufficient peelability cannot be obtained under higher temperature conditions, for example, heat treatment conditions of 175°C, and the technology is still not satisfactory.

[0009] Furthermore, even the techniques disclosed in Patent Documents 2 and 3 above have the problem that sufficient peelability cannot be obtained under higher temperature conditions, for example, heat treatment conditions at 175° C., and are still unsatisfactory.

[0010] In view of the above background, the present invention aims to provide an active energy ray-curable peel-type pressure-sensitive adhesive composition which has good adhesive strength before irradiation with active energy rays, is excellent in heat resistance, and has reduced adhesive strength after irradiation with active energy rays even when exposed to high temperatures, and which is capable of producing a pressure-sensitive adhesive having excellent peelability without leaving any adhesive residue. [Means for solving the problem]

[0011] However, in view of these circumstances, the present inventors conducted extensive research and discovered that by using a composition containing an acrylic resin and two types of antioxidants as a pressure-sensitive adhesive composition, a pressure-sensitive adhesive can be obtained which has good adhesive strength before irradiation with active energy rays, and which has reduced adhesive strength after irradiation with active energy rays even when exposed to high temperatures, and which has excellent peelability without leaving any adhesive residue, thereby completing the present invention.

[0012] That is, the present invention provides a pressure-sensitive adhesive composition comprising an acrylic resin (A) and an antioxidant (B), A first aspect of the present invention is an active energy ray-curable pressure-sensitive adhesive composition in which the antioxidant (B) contains a primary antioxidant (B1) and a secondary antioxidant (B2) (excluding the antioxidant (B1)).

[0013] A second aspect of the present invention is a pressure-sensitive adhesive sheet having a pressure-sensitive adhesive layer formed by crosslinking the pressure-sensitive adhesive composition according to the first aspect.

[0014] That is, the present invention has the following aspects [1] to [9]. [1] An active energy ray-curable pressure-sensitive adhesive composition comprising an acrylic resin (A) and an antioxidant (B), wherein the antioxidant (B) comprises a primary antioxidant (B1) and a secondary antioxidant (B2) (excluding the antioxidant (B1)), wherein the primary antioxidant (B1) is a dimer, trimer or tetramer, and the secondary antioxidant (B2) is a phosphorus-based antioxidant. [2] The active energy ray-curable pressure-sensitive adhesive composition according to [1], wherein the acrylic resin (A) has a structural unit derived from an alkyl group-containing (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer other than an amide group (a2). [3] The active energy ray-curable pressure-sensitive adhesive composition according to [1] or [2], wherein the acrylic resin (A) has a structural unit derived from an amide group-containing monomer (a3). [4] The active energy ray-curable pressure-sensitive adhesive composition according to any one of [1] to [3], wherein the acrylic resin (A) further has an ethylenically unsaturated group. [5] The active energy ray-curable pressure-sensitive adhesive composition according to any one of [1] to [4], wherein the acrylic resin (A) has an ethylenically unsaturated group content of 5 to 250 mmol / 100 g. [6] The active energy ray-curable pressure-sensitive adhesive composition according to any one of [1] to [5], wherein the primary antioxidant (B1) has no bonding site with other units at the ortho-position of the hydroxyl group. [7] The active energy ray-curable pressure-sensitive adhesive composition according to any one of [1] to [6], further comprising a crosslinking agent (C). [8] [1] A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer in which the pressure-sensitive adhesive composition according to any one of [1] to [7] is crosslinked. [9] The pressure-sensitive adhesive sheet according to [8], characterized in that the pressure-sensitive adhesive layer is cured and becomes peelable by irradiation with active energy rays. Effect of the Invention

[0015] The active energy ray curable adhesive composition of the present invention containing an acrylic resin and an antioxidant (B) uses two kinds of antioxidants (B) in combination, and therefore the adhesive has good adhesive strength before active energy ray irradiation, and even if exposed to high temperatures, the adhesive strength is reduced after active energy ray irradiation, and the adhesive has excellent peelability. When exposed to high temperatures, the acrylic polymer generates an alkyl radical, which further reacts with oxygen to generate a peroxy radical. This peroxy radical extracts hydrogen from the acrylic polymer to generate the next alkyl radical, which itself becomes a hydroperoxide. Furthermore, the hydroperoxide decomposes, and new radicals are generated by the decomposition, so that the deterioration of the polymer progresses at an accelerated rate. In addition, since the active energy ray curable adhesive composition is cured by the radicals, there is also a problem that the curing progresses due to heat before the composition is cured by the active energy ray. In the present invention, the primary antioxidant (B1) donates hydrogen to the peroxy radical, and the acrylic polymer becomes a hydroperoxide without extracting hydrogen. Furthermore, the secondary antioxidant (B2) acts to decompose and stabilize hydroperoxides, thereby suppressing the generation of alkyl radicals, thereby achieving the above-mentioned effects. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0016] Hereinafter, the embodiments of the present invention will be described in detail, but the present invention is not limited to these. In the present invention, "(meth)acrylic" means acrylic or methacrylic, "(meth)acryloyl" means acryloyl or methacryloyl, and "(meth)acrylate" means acrylate or methacrylate, respectively. The acrylic resin is a resin obtained by polymerizing a polymerization component containing at least one kind of (meth)acrylate monomer. In the present invention, the term "sheet" is not particularly distinguished from "film" or "tape" and is used to include these terms.

[0017] The pressure-sensitive adhesive composition of the present invention is mainly used in the pressure-sensitive adhesive layer of a pressure-sensitive adhesive sheet that is intended to be peeled off after being attached to a workpiece such as a metal plate, a plastic plate, a semiconductor wafer, etc. The pressure-sensitive adhesive sheet is formed by coating the pressure-sensitive adhesive composition on a substrate sheet to form a pressure-sensitive adhesive layer, and after being attached to a workpiece, the pressure-sensitive adhesive layer is cured by irradiating the substrate with active energy rays, thereby reducing the adhesive strength, and the sheet can be easily peeled off from the workpiece.

[0018] The pressure-sensitive adhesive composition of the present invention contains an acrylic resin (A) and an antioxidant (B). Each of the components of the pressure-sensitive adhesive composition of the present invention will be described below.

[0019] [Acrylic resin (A)] The acrylic resin (A) used in the present invention preferably has a structural unit derived from an alkyl group-containing (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer (a2), and more preferably has a structural unit derived from an amide group-containing monomer (a3), and, if necessary, a structural unit derived from another copolymerizable monomer (a4). The acrylic resin (A) used in the present invention is preferably obtained by copolymerizing a copolymerization component (a) containing an alkyl group-containing (meth)acrylate (a1), a functional group-containing monomer (a2), an amide group-containing monomer (a3), and, if necessary, other copolymerizable monomers (a4).

[0020] [Alkyl group-containing (meth)acrylate (a1)] The (meth)acrylic acid alkyl ester monomer (a1) preferably has an alkyl group having a carbon number of usually 1 to 20, particularly preferably 1 to 12, and further preferably 1 to 8. If the carbon number is too large, adhesive residue tends to easily occur on the processed member.

[0021] Examples of the (meth)acrylic acid alkyl ester monomer (a1) include aliphatic (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, n-butyl (meth)acrylate, isobutyl (meth)acrylate, tert-butyl (meth)acrylate, n-propyl (meth)acrylate, n-hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, n-octyl (meth)acrylate, isooctyl acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, and isostearyl (meth)acrylate; and alicyclic (meth)acrylic acid alkyl esters such as cyclohexyl (meth)acrylate and isobornyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above (meth)acrylic acid alkyl ester monomers (a1), in terms of copolymerizability, adhesive properties, ease of handling, and ease of availability of raw materials, methyl (meth)acrylate, n-butyl (meth)acrylate, and 2-ethylhexyl (meth)acrylate are preferred, and methyl (meth)acrylate and n-butyl (meth)acrylate are particularly preferred.

[0022] The content of the (meth)acrylic acid alkyl ester monomer (a1) in the copolymerization component (a) of the acrylic resin (A) is usually 30 to 99% by weight, preferably 40 to 90% by weight, and particularly preferably 50 to 80% by weight of the entire copolymerization component (a). If the content is too low, the adhesive strength before irradiation with active energy rays tends to be easily reduced, and if the content is too high, the adhesive strength after irradiation with active energy rays tends to be too high.

[0023] [Functional group-containing monomer (a2)] The functional group-containing monomer (a2) is a monomer having a functional group other than an amide group, and examples of such monomers include hydroxyl group-containing monomers, carboxyl group-containing monomers, amino group-containing monomers, glycidyl group-containing monomers, sulfonic acid group-containing monomers, acetoacetyl group-containing monomers, etc. These functional group-containing monomers can be used alone or in combination of two or more kinds.

[0024] The content of the functional group-containing monomer (a2) in the copolymerization component of the acrylic resin (A) is usually 50% by weight or less, preferably 40% by weight or less, more preferably 30% by weight or less of the total copolymerization component (a). If the content is too high, the storage stability tends to decrease, or crosslinking tends to progress before the drying process, which tends to cause problems in coating properties. If the content is too low, the amount of ethylenically unsaturated groups introduced tends to decrease, and the peelability after irradiation with active energy rays tends to decrease.

[0025] The acrylic resin (A) of the present invention preferably uses a hydroxyl-containing monomer (a2-1) as the functional group-containing monomer (a2). By using the hydroxyl-containing monomer (a2-1) as the copolymerization component (a) of the acrylic resin (A), the acrylic resin (A) has a structural portion derived from the hydroxyl-containing monomer (a2), i.e., a hydroxyl group. This hydroxyl group serves as a reaction site when introducing an ethylenically unsaturated group, which will be described later, and also serves as a reaction site with the crosslinking agent (C), which will be described later.

[0026] The hydroxyl group-containing monomer (a2-1) is preferably a hydroxyl group-containing (meth)acrylate monomer, and specific examples thereof include (meth)acrylic acid hydroxyalkyl esters such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate, and caprolactone-modified monomers such as caprolactone-modified 2-hydroxyethyl (meth)acrylate. Examples of the monomers include oxyalkylene-modified monomers such as diethylene glycol (meth)acrylate and polyethylene glycol (meth)acrylate, primary hydroxyl group-containing monomers such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing monomers such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate and 3-chloro-2-hydroxypropyl (meth)acrylate, and tertiary hydroxyl group-containing monomers such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate. These may be used alone or in combination of two or more. Among the above hydroxyl group-containing monomers, primary hydroxyl group-containing monomers are preferred, and 2-hydroxyethyl (meth)acrylate and 4-hydroxybutyl (meth)acrylate are particularly preferred, because they have excellent reactivity with the ethylenically unsaturated compound and crosslinking agent (C) described below.

[0027] The content of the hydroxyl group-containing monomer (a2-1) in the entire copolymerization component (a) of the acrylic resin (A) is usually 0.1 to 60% by weight, preferably 1 to 50% by weight, more preferably 3 to 40% by weight, and particularly preferably 7 to 30% by weight. If the content is too high, crosslinking may proceed before the drying step, which may lead to problems in coatability, whereas if the content is too low, the amount of ethylenically unsaturated groups described below may also be reduced, resulting in an insufficient decrease in adhesive strength, which may lead to increased contamination of the workpiece.

[0028] Examples of the carboxy group-containing monomer include (meth)acrylic acid, (meth)acrylic acid dimer, crotonic acid, maleic acid, maleic anhydride, fumaric acid, citraconic acid, glutaconic acid, itaconic acid, acrylamido-N-glycolic acid, cinnamic acid, etc. Among these, (meth)acrylic acid is preferably used in terms of copolymerizability.

[0029] The content of the carboxyl group-containing monomer in the entire copolymerization component (a) of the acrylic resin (A) is usually 30% by weight or less, preferably 10% by weight or less, and more preferably 5% by weight or less. If the content is too high, the processed member tends to be easily deteriorated, storage stability tends to decrease, and crosslinking tends to proceed before the drying process, causing problems in coatability.

[0030] Examples of the amino group-containing monomer include aminoethyl (meth)acrylate, N,N-dimethylaminoethyl (meth)acrylate, and N,N-dimethylaminopropyl (meth)acrylate.

[0031] The content of the amino group-containing monomer in the entire copolymerization component (a) of the acrylic resin (A) is usually 30% by weight or less, preferably 25% by weight or less, more preferably 20% by weight or less, based on the entire copolymerization component. If the content is too high, crosslinking may proceed before the drying step, which may cause problems in coatability.

[0032] Examples of the glycidyl group-containing monomer include glycidyl methacrylate and allyl glycidyl methacrylate.

[0033] The content of the glycidyl group-containing monomer in the entire copolymerization component (a) of the acrylic resin (A) is usually 20% by weight or less, preferably 10% by weight or less, and more preferably 5% by weight or less. If the content is too high, crosslinking proceeds before the drying step, and problems with coatability tend to occur.

[0034] Examples of the sulfonic acid group-containing monomer include olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, 2-acrylamido-2-methylolpropane sulfonic acid, styrene sulfonic acid, and salts thereof.

[0035] The content of the sulfonic acid group-containing monomer in the entire copolymerization component (a) of the acrylic resin (A) is usually 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less. If the content is too high, crosslinking proceeds before the drying step, and problems with coatability tend to occur.

[0036] Examples of the acetoacetyl group-containing monomer include 2-(acetoacetoxy)ethyl (meth)acrylate and allyl acetoacetate.

[0037] The content of the acetoacetyl group-containing monomer in the entire copolymerization component (a) of the acrylic resin (A) is usually 10% by weight or less, preferably 5% by weight or less, and more preferably 1% by weight or less. If the content is too high, crosslinking may proceed before the drying step, which may cause problems in the coatability.

[0038] [Amide group-containing monomer (a3)] The acrylic resin (A) of the present invention preferably uses an amide group-containing monomer (a3) ​​as the copolymerization component (a). Examples of the amide group-containing monomer (a3) ​​include (meth)acrylamide-based monomers such as methoxydimethylpropanamide, ethoxymethyl(meth)acrylamide, n-butoxymethyl(meth)acrylamide, (meth)acryloylmorpholine, dimethyl(meth)acrylamide, diethyl(meth)acrylamide, dimethylaminopropyl(meth)acrylamide, (meth)acrylamide, and N-methylol(meth)acrylamide. Among these, (meth)acryloylmorpholine is particularly preferred in terms of reducing adhesive strength after exposure to high temperatures and then irradiation with active energy rays.

[0039] The content of the amide group-containing monomer (a3) ​​in the entire copolymerization component (a) of the acrylic resin (A) is usually 1 to 30% by weight, preferably 5 to 25% by weight, and more preferably 8 to 18% by weight. If the content is too small, the adhesive strength after exposure to high temperatures and irradiation with active energy rays tends to be insufficient. In addition, the amide group-containing monomer (a3) ​​often has a high glass transition temperature, and if the content is too large, the glass transition temperature of the polymer increases, which tends to result in insufficient reduction in adhesive strength after exposure to high temperatures and irradiation with active energy rays.

[0040] [Other copolymerizable monomers (a4)] Examples of the other copolymerizable monomers (a4) include vinyl carboxylate ester monomers such as vinyl acetate, vinyl propionate, vinyl stearate, and vinyl benzoate; aromatic ring-containing monomers such as phenyl(meth)acrylate, benzyl(meth)acrylate, phenoxyethyl(meth)acrylate, phenyldiethylene glycol(meth)acrylate, 2-hydroxy-3-phenoxypropyl(meth)acrylate, styrene, and α-methylstyrene; biphenyloxy structure-containing (meth)acrylic acid ester monomers such as biphenyloxyethyl(meth)acrylate; 2-methoxyethyl(meth)acrylate, 2-ethoxyethyl(meth)acrylate, and the like. acrylate, methoxydiethylene glycol (meth)acrylate, ethoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, polypropylene glycol mono(meth)acrylate, and other monomers containing an alkoxy group or an oxyalkylene group; acrylonitrile, methacrylonitrile, vinyl chloride, vinylidene chloride, alkyl vinyl ether, vinyl toluene, vinylpyridine, vinylpyrrolidone, itaconic acid dialkyl ester, fumaric acid dialkyl ester, allyl alcohol, acrylic chloride, methyl vinyl ketone, allyl trimethyl ammonium chloride, dimethyl allyl vinyl ketone, and the like. These may be used alone or in combination of two or more.

[0041] The content of the other copolymerizable monomer (a4) in the copolymerization component (a) of the acrylic resin (A) is usually 40% by weight or less, preferably 30% by weight or less, more preferably 25% by weight or less of the entire copolymerization component (a). If the content of the other copolymerizable monomer (a4) is too high, the adhesive properties tend to be easily deteriorated.

[0042] In the present invention, the (meth)acrylic resin (A) is produced by polymerizing an alkyl group-containing (meth)acrylate (a1), a functional group-containing monomer (a2) other than an amide group, an amide group-containing monomer (a3), and, if necessary, other copolymerizable monomers (a4) as copolymerization components (a). As such a polymerization method, a conventionally known method such as solution radical polymerization, suspension polymerization, bulk polymerization, emulsion polymerization, etc. is usually appropriately performed. Among them, the production by solution radical polymerization is preferable because the acrylic resin (A) can be safely and stably produced with any monomer composition.

[0043] In the solution radical polymerization, for example, monomer components such as an alkyl group-containing (meth)acrylate (a1), a functional group-containing monomer other than an amide group (a2), an amide group-containing monomer (a3), and, if necessary, other copolymerizable monomers (a4), as well as a polymerization initiator, are mixed or dropped into an organic solvent, and polymerization is carried out under reflux or usually at 50 to 98° C. for about 0.1 to 20 hours.

[0044] Examples of the organic solvent used in the polymerization reaction include aromatic hydrocarbons such as toluene and xylene, aliphatic hydrocarbons such as hexane, esters such as ethyl acetate and butyl acetate, aliphatic alcohols such as n-propyl alcohol and isopropyl alcohol, and ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclohexanone. The amount of the organic solvent used is usually 10 to 900 parts by weight per 100 parts by weight of the copolymerization components.

[0045] As the polymerization initiator, a conventional radical polymerization initiator can be used. Specific examples of the polymerization initiator include azo-based polymerization initiators such as azobisisobutyronitrile and azobisdimethylvaleronitrile, and peroxide-based polymerization initiators such as benzoyl peroxide, lauroyl peroxide, di-tert-butyl peroxide and cumene hydroperoxide.

[0046] In addition, the acrylic resin (A) preferably has a structural portion derived from the hydroxyl group-containing monomer (a2-1), i.e., has a hydroxyl group, in terms of reactivity with the ethylenically unsaturated compound and the crosslinking agent (C) described below. When the acrylic resin (A) has a hydroxyl group, it reacts with the ethylenically unsaturated compound, and an ethylenically unsaturated group can be introduced into the acrylic resin (A), and a crosslinked structure is formed by the reaction with the crosslinking agent (C), which tends to improve the adhesive strength before the irradiation with active energy rays.

[0047] When the acrylic resin (A) has hydroxyl groups, the content of the hydroxyl groups is usually 0.01 to 20% by weight, preferably 0.05 to 10% by weight, and more preferably 0.1 to 5% by weight, based on the acrylic resin (A). If the content of hydroxyl groups is too low, the cohesive strength of the adhesive decreases, which tends to cause glue residue, and if the content of hydroxyl groups is too high, the flexibility and adhesive strength of the adhesive decrease, which tends to cause lifting between the adhesive and the workpiece.

[0048] The glass transition temperature (Tg) of the acrylic resin (A) is preferably −60 to 0° C., particularly preferably −55 to −10° C., and further preferably −50 to −30° C. If the glass transition temperature is too high, the adhesive strength reduction after exposure to high temperatures and subsequent irradiation with active energy rays tends to be insufficient, whereas if the glass transition temperature is too low, the adhesive strength tends to be insufficient.

[0049] The above glass transition temperature (Tg) is a value calculated by applying the glass transition temperature and weight fraction of each monomer constituting the acrylic resin (A) as a homopolymer to the following Fox's formula.

[0050]

number

[0051] Here, the glass transition temperature when the monomers constituting the acrylic resin (A) are made into a homopolymer is usually measured by a differential scanning calorimeter (DSC) and can be measured by a method in accordance with JIS K 7121-1987 or JIS K 6240.

[0052] The weight-average molecular weight of the acrylic resin (A) is usually 100,000 to 2,000,000, preferably 150,000 to 1,500,000, particularly preferably 200,000 to 1,200,000, and especially preferably 300,000 to 1,000,000. If the weight-average molecular weight is too small, the staining of the workpiece tends to increase, whereas if it is too large, the coatability tends to decrease and there is also a tendency for it to be disadvantageous in terms of cost.

[0053] Furthermore, the dispersity (weight average molecular weight / number average molecular weight) of the acrylic resin (A) is preferably 20 or less, particularly preferably 10 or less, further preferably 8 or less, and particularly preferably 6 or less. If the dispersity is too high, there is a tendency for contamination of the workpiece to increase. The lower limit of the dispersity is usually 1.1 in view of production limitations.

[0054] The weight average molecular weight of the acrylic resin (A) is a weight average molecular weight calculated based on the molecular weight of standard polystyrene. The weight average molecular weight was measured by a high performance liquid chromatograph (Waters Japan, "Waters 2695 (main body)" and "Waters 2414 (detector)") using a Shodex GPC KF-806L column (molecular weight exclusion limit: 2×10 7 , Separation range: 100~2×10 7 The number average molecular weight is measured by using three columns in series (100 / column, theoretical plate number: 10,000 plates / column, filler material: styrene-divinylbenzene copolymer, filler particle size: 10 μm), and the number average molecular weight can also be obtained in the same way.

[0055] The viscosity of the acrylic resin (A) at 25°C is preferably 5 to 10,000 mPa·s, more preferably 100 to 5,000 mPa·s. If the viscosity is outside the above range, the coatability tends to decrease. The viscosity is measured using an E-type viscometer.

[0056] The acrylic resin (A) may be used as it is, but in the present invention, it is preferable that the acrylic resin (A) further has an ethylenically unsaturated group. When the acrylic resin (A) has an ethylenically unsaturated group, the ethylenically unsaturated group is polymerized and hardened when irradiated with active energy rays, and the adhesive strength is reduced. Therefore, when the adhesive composition containing the acrylic resin (A) is made into an adhesive sheet, it can be given easy peeling property.

[0057] The method for introducing an ethylenically unsaturated group into the acrylic resin (A) may be to react the acrylic resin (A) with an ethylenically unsaturated group-containing compound, for example, (i) A method of reacting a hydroxyl group of the acrylic resin (A) with an isocyanate group-containing ethylenically unsaturated compound; (ii) A method of reacting a hydroxyl group of the acrylic resin (A) with (meth)acrylic anhydride; (iii) A method of reacting a hydroxyl group of the acrylic resin (A) with an ethylenically unsaturated group-containing carboxylic acid, (iv) A method of reacting a carboxy group of the acrylic resin (A) with a vinyl ether group-containing (meth)acrylic acid ester, Among them, method (i) is preferred from the viewpoint of reactivity. The preferred method (i) will now be described.

[0058] In the above method (i), the hydroxyl group derived from the hydroxyl group-containing monomer (a2-1) in the acrylic resin (A) reacts with the isocyanate group of the isocyanate group-containing ethylenically unsaturated compound, and an ethylenically unsaturated group containing an ethylenically unsaturated bond and a urethane bond is introduced into the acrylic resin (A), thereby obtaining an acrylic resin containing an ethylenically unsaturated group.

[0059] [Isocyanate group-containing ethylenically unsaturated compounds] The isocyanate group-containing ethylenically unsaturated compound is a monomer having an isocyanate group and a polymerizable ethylenically unsaturated group. Examples of the isocyanate group-containing ethylenically unsaturated compound include 2-(meth)acryloyloxyethyl isocyanate, 3-(meth)acryloyloxy-n-propyl isocyanate, 2-(meth)acryloyloxyisopropyl isocyanate, 4-(meth)acryloyloxy-n-butyl isocyanate, 2-(meth)acryloyloxy-tert-butyl isocyanate, 2-(meth)acryloyloxybutyl-4-isocyanate, 2-(meth)acryloyloxybutyl-3-isocyanate, 2-(meth)acryloyloxybutyl-2-isocyanate, and 2-(meth)acryloyloxybutyl-1-isocyanate. Examples of the isocyanate include 5-(meth)acryloyloxy-n-pentyl isocyanate, 6-(meth)acryloyloxy-n-hexyl isocyanate, 7-(meth)acryloyloxy-n-heptyl isocyanate, 2-(isocyanatoethyloxy)ethyl (meth)acrylate, 3-(meth)acryloyloxyphenyl isocyanate, 4-(meth)acryloyloxyphenyl isocyanate, 1,1-bis((meth)acryloyloxymethyl)methyl isocyanate, 1,1-bis((meth)acryloyloxymethyl)ethyl isocyanate, and 2'-pentenoyl-4-oxyphenyl isocyanate. These may be used alone or in combination of two or more. Among these compounds, (meth)acrylate monomers are preferred in terms of ease of synthesis and availability of raw materials, and 2-methacryloyloxyethyl isocyanate, 2-acryloyloxyethyl isocyanate, 2-(isocyanatoethyloxy)ethyl methacrylate, 2-(isocyanatoethyloxy)ethyl acrylate, and 1,1-bis(acryloyloxymethyl)ethyl isocyanate are more preferred.

[0060] The ratio of the acrylic resin (A) to the isocyanate group-containing ethylenically unsaturated compound in the reaction between them is appropriately set in consideration of the ratio between the hydroxyl group and the isocyanate group, and varies depending on the types of the two compounds. Generally, the ratio of the isocyanate group-containing ethylenically unsaturated compound is 10 to 100 mol %, preferably 20 to 97 mol %, and particularly preferably 30 to 95 mol %, per 100 mol % of the hydroxyl group-containing monomer (a2-1) in the acrylic resin (A).

[0061] The reaction between the two compounds may be carried out in the presence of a reaction catalyst, and the reaction rate can be adjusted by the amount of the reaction catalyst added. The reaction catalyst may be a known reaction catalyst. Specific examples of the reaction catalyst include dibutyltin dilaurate, copper naphthenate, cobalt naphthenate, zinc naphthenate, triethylamine, 1,4-diazabicyclo[2.2.2]octane, zirconium acetylacetonate, titanium diisopropoxybis(ethylacetoacetate), and a mixture of bismuth tris(2-ethylhexanoate) and 2-ethylhexanoic acid. One of these reaction catalysts may be used alone, or two or more may be used in combination.

[0062] The reaction temperature when reacting the two compounds is preferably 25 to 100° C., more preferably 30 to 60° C. The reaction time is preferably 30 minutes to 50 hours, more preferably 3 hours to 20 hours.

[0063] When reacting the two compounds, a polymerization inhibitor may be added to the reaction system as necessary. As the polymerization inhibitor, a commonly used one can be used, for example, a phenol-based compound, a hydroquinone-based compound, etc. Specific examples of the polymerization inhibitor include hydroquinone, methoxyhydroquinone, catechol, p-tert-butylcatechol, cresol, 2,6-di-tert-butyl-4-methylphenol (BHT), etc. In addition, when reacting the two compounds, known additives may be added depending on the purpose.

[0064] The addition reaction rate between the hydroxyl group derived from the hydroxyl group-containing monomer (a2-1) of the acrylic resin (A) and the isocyanate group of the isocyanate group-containing ethylenically unsaturated compound, that is, the urethane conversion rate, is preferably 5 to 99%, more preferably 10 to 90%. If the urethane conversion rate is too low, the adhesive strength after irradiation with active energy rays such as ultraviolet rays tends to be difficult to decrease sufficiently, and if the urethane conversion rate is too high, the urethane reaction does not go to completion, and unreacted isocyanate group-containing ethylenically unsaturated compound tends to remain.

[0065] The urethane conversion rate can be calculated, for example, from the ratio of the amount (mol) of isocyanate groups in the isocyanate group-containing ethylenically unsaturated compound to the amount (mol) of hydroxyl groups in the acrylic resin (A). It is determined that 100% of the charged isocyanate groups have reacted by confirming the disappearance of the peak of the isocyanate groups by IR measurement. Another method for calculating the urethane conversion rate is to calculate it from the integral ratio of the structure derived from the hydroxyl group-containing monomer (a2-1) before and after the urethane conversion reaction by 1H-NMR measurement.

[0066] In the above, the method (i) which is a preferred embodiment for introducing an ethylenically unsaturated group into the acrylic resin (A) has been described. However, in the above methods (ii) to (iv), an ethylenically unsaturated group can also be introduced into the acrylic resin (A) by following a conventional method.

[0067] When the acrylic resin (A) has an ethylenically unsaturated group, the content of the ethylenically unsaturated group is usually 5 to 250 mmol / 100 g, preferably 30 to 200 mmol / 100 g, and more preferably 50 to 160 mmol / 100 g. If the content of the ethylenically unsaturated group is too small, the peelability by irradiation with active energy rays tends to decrease, and if the content of the ethylenically unsaturated group is too large, the adhesive strength before irradiation with active energy rays tends to decrease.

[0068] The content of the ethylenically unsaturated group can be calculated from the following formula. Ethylenically unsaturated group content (mmol / 100g) = Hydroxyl groups (mmol) contained in 100 g of acrylic resin (A) before the addition of ethylenically unsaturated groups × addition reaction rate (%) / weight (g) of 100 g of acrylic resin (A) after the addition of ethylenically unsaturated groups × 100

[0069] When the acrylic resin (A) has an ethylenically unsaturated group, the glass transition temperature (Tg) is preferably −65 to 0° C., particularly −60 to −10° C., further preferably −55 to −20° C., and particularly preferably −51 to −30° C. If the glass transition temperature is too high, the adhesiveness tends to decrease, and if it is too low, the contamination of the workpiece tends to increase. The glass transition temperature (Tg) can be calculated by the method described above.

[0070] Furthermore, when the acrylic resin (A) has an ethylenically unsaturated group, the weight-average molecular weight is usually 100,000 to 2,000,000, preferably 150,000 to 1,500,000, particularly preferably 200,000 to 1,200,000, and especially preferably 300,000 to 1,000,000. If the weight-average molecular weight is too small, the staining of the workpiece tends to increase, whereas if it is too large, the coatability tends to decrease and there is also a tendency for it to be disadvantageous in terms of cost.

[0071] Furthermore, when the acrylic resin (A) has an ethylenically unsaturated group, the degree of dispersion (weight average molecular weight / number average molecular weight) is preferably 20 or less, particularly preferably 15 or less, further preferably 10 or less, and particularly preferably 7 or less. If the degree of dispersion is too high, the contamination of the workpiece tends to increase. The lower limit of the degree of dispersion is usually 1.1 from the viewpoint of production limitations.

[0072] When the acrylic resin (A) has an ethylenically unsaturated group, the weight average molecular weight and the dispersity can be measured according to the above-mentioned method.

[0073] When the acrylic resin (A) has an ethylenically unsaturated group, the viscosity at 25°C is preferably 5 to 10,000 mPa·s, more preferably 500 to 5,000 mPa·s. If the viscosity is outside the above range, the coatability tends to decrease. The viscosity is measured using an E-type viscometer.

[0074] Even when the acrylic resin (A) has an ethylenically unsaturated group, it is preferable that the acrylic resin (A) has a structural portion derived from the hydroxyl group-containing monomer (a2-1), i.e., has a hydroxyl group, from the viewpoint of reactivity with the crosslinking agent (C) described later.

[0075] When the acrylic resin (A) has an ethylenically unsaturated group, the hydroxyl group content is usually 0.01 to 10% by weight, preferably 0.05 to 8% by weight, and more preferably 1 to 5% by weight. If the hydroxyl group content is too low, the cohesive strength of the adhesive decreases, which tends to cause glue residue, and if the hydroxyl group content is too high, the flexibility and adhesive strength of the adhesive decrease, which tends to cause lifting between the adhesive and the workpiece.

[0076] [Antioxidant (B)] The pressure-sensitive adhesive composition of the present invention contains an antioxidant (B), and the antioxidant (B) contains a primary antioxidant (B1) and a secondary antioxidant (B2) (excluding the antioxidant (B1)).

[0077] The primary antioxidant (B1) is preferably a dimer, trimer, or tetramer, and more preferably has no bonding site at the ortho position of the hydroxyl group. The steric hindrance at the ortho position of the hydroxyl group has a significant effect on the reaction rate with radicals. It is said that the greater the steric hindrance of the hydroxyl group, the faster the reaction rate of the radicals becomes, but the number of radicals per mole decreases, so it is important to have an appropriate level of steric hindrance. Specific examples of the dimer, trimer, or tetramer primary antioxidant include ADK STAB AO-20, ADK STAB AO-50, ADK STAB AO-60, ADK STAB AO-330, ADK STAB AO-30, ADK STAB AO-40, ADK STAB AO-80 (all manufactured by ADEKA), IRGANOX1010, IRGANOX1035, IRGANOX1098, IRGANOX1330, IRGANOX1425WL, IRGANOX245, IRGANOX259, IRGANOX3114 (manufactured by BASF Japan Ltd.), Yoshinox BB (manufactured by Mitsubishi Chemical Corporation), and ANTAGE W-300 (manufactured by Kawaguchi Chemical Industry Co., Ltd.).

[0078] The content of the primary antioxidant (B1) is usually 0.01 to 10% by weight, preferably 0.05 to 8% by weight, more preferably 1 to 3% by weight. If the content of the primary antioxidant is too low, the reduction in adhesive strength after heating and irradiation with active energy rays tends to be insufficient, while if the content of the primary antioxidant is too high, it tends to bleed out to the adherend interface or substrate interface, resulting in a decrease in adhesive strength to the adherend and a deterioration in adhesion to the substrate interface.

[0079] The secondary antioxidant (B2) used in the present invention is a phosphorus-based antioxidant. The secondary antioxidant (B2) may be used alone or in combination of two or more different secondary antioxidants.

[0080] Examples of phosphorus-based antioxidants include phosphite-based antioxidants, specifically Irgaphos 38, Irgaphos 126, Irgaphos 168 (all manufactured by BASF), Sumilizer GP (manufactured by Sumitomo Chemical), Adeka STAB PEP-8, Adeka STAB PEP-36, Adeka STAB HP-10, Adeka STAB 2112, Adeka STAB 1178, Adeka STAB 1500, Adeka STAB 135A, Adeka STAB 3010, Adeka STAB C, Adeka STAB TPP (all manufactured by ADEKA), etc. The antioxidant may be in a solid or liquid form.

[0081] The content of the secondary antioxidant (B2) is usually 0.1 to 2.0% by weight, preferably 0.2 to 1.5% by weight, and more preferably 0.5 to 1.25% by weight, based on 100 parts by mass of the acrylic copolymer (A). If the content of the secondary antioxidant is too low, the adhesive strength after heating and irradiation with active energy rays tends to be insufficient, while if the content of the secondary antioxidant is too high, it tends to bleed out to the adherend interface or substrate interface, resulting in a decrease in adhesive strength to the adherend and a deterioration in adhesion to the substrate interface.

[0082] The blending ratio of the primary antioxidant (B1) to the secondary antioxidant (B2) is preferably primary antioxidant (B1):secondary antioxidant (B2)=1:0.02 to 1:5, more preferably 1:0.1 to 1:3, and even more preferably 1:0.5 to 1:2. If the blending ratio of the secondary antioxidant is too low, radical generation from hydroperoxide cannot be suppressed, and the adhesive strength reduction after irradiation with active energy rays becomes insufficient, whereas if the blending ratio of the secondary antioxidant is too high, i.e., the amount of the primary antioxidant is too low, hydrogen abstraction from the polymer cannot be suppressed, and the adhesive strength reduction after irradiation with active energy rays becomes insufficient.

[0083] Other antioxidants include sulfur-based antioxidants, amine-based antioxidants, and hindered amine-based antioxidants, which may be used alone or in combination of two or more.

[0084] The secondary antioxidant (B2) may contain an antioxidant other than the above phosphorus-based antioxidants, and examples thereof include sulfur-based antioxidants. Specific examples of sulfur-based antioxidants include ADK STAB AO-412S, ADK STAB AO-503 (manufactured by ADEKA Corporation), Irganox PS 802 FL (manufactured by BASF Corporation), Sumilizer MB (manufactured by Sumika Chemtex Corporation), DLTP "Yoshitomi", DSTP "Yoshitomi", DMTP "Yoshitomi", DTTP "Yoshitomi" (manufactured by API Corporation), etc. The antioxidant may be in a solid or liquid form.

[0085] [Crosslinking agent (C)] In order to improve the adhesive strength before irradiation with active energy rays, it is preferable to further contain a crosslinking agent (C) in the resin composition of the present invention. As described above, the crosslinking agent (C) reacts with the functional group in the acrylic resin (A) to form a crosslinked structure, and examples thereof include isocyanate-based crosslinking agents, epoxy-based crosslinking agents, aziridine-based crosslinking agents, melamine-based crosslinking agents, aldehyde-based crosslinking agents, amine-based crosslinking agents, and metal chelate-based crosslinking agents. Among these, it is preferable to use an isocyanate-based crosslinking agent in terms of improving the adhesiveness to the adherend and reactivity with the acrylic resin (A).

[0086] The isocyanate-based crosslinking agent contains at least two isocyanate groups, and examples thereof include aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate, and xylylene diisocyanate, aliphatic polyisocyanates such as hexamethylene diisocyanate, alicyclic polyisocyanates such as isophorone diisocyanate and hydrogenated diphenylmethane diisocyanate, and biuret and isocyanurate forms thereof, as well as adducts which are reaction products with low-molecular active hydrogen-containing compounds such as ethylene glycol, propylene glycol, neopentyl glycol, trimethylolpropane, and castor oil. Among these, aromatic polyisocyanates and adducts of aromatic polyisocyanates and trimethylolpropane are preferred in terms of drug resistance and reactivity with functional groups, and adducts of tolylene diisocyanate and trimethylolpropane are particularly preferred.

[0087] Examples of the epoxy crosslinking agent include 1,3-bis(N,N'-diglycidylaminomethyl)cyclohexane, N,N,N',N'-tetraglycidyl-m-xylylenediamine, ethylene glycol diglycidyl ether, 1,6-hexanediol diglycidyl ether, trimethylolpropane diglycidyl ether, diglycidyl aniline, and diglycidylamine.

[0088] Examples of the aziridine crosslinking agent include diphenylmethane-4,4'-bis(1-aziridinecarboxamide), trimethylolpropane tri-β-aziridinylpropionate, tetramethylolmethane tri-β-aziridinylpropionate, toluene-2,4-bis(1-aziridinecarboxamide), triethylenemelamine, bisisophthaloyl-1-(2-methylaziridine), tris-1-(2-methylaziridine)phosphine, and trimethylolpropane tri-β-(2-methylaziridine)propionate.

[0089] Examples of the melamine-based crosslinking agent include melamine; methylolmelamine derivatives such as amino group-containing methylolmelamine, imino group-containing methylolmelamine, and hexamethylolmelamine obtained by condensing melamine with formaldehyde; and alkylated methylolmelamines such as partially or completely alkylated methylolmelamine and imino group-containing partially or completely alkylated methylolmelamine obtained by reacting a methylolmelamine derivative with a lower alcohol such as methyl alcohol or butyl alcohol to partially or completely etherify the methylolmelamine derivative.

[0090] Examples of the aldehyde crosslinking agent include aldehyde compounds that liberate aldehyde in an aqueous solution, such as formaldehyde, acetaldehyde, propionaldehyde, butylaldehyde, glyoxal, glutaraldehyde, dialdehyde starch, hexamethylenetetramine, 1,4-dioxane-2,3-diol, 1,3-bis(hydroxymethyl)-2-imidazolidine, dimethylol urea, N-methylol acrylamide, urea formalin resin, and melamine formalin resin, and aromatic aldehyde compounds, such as benzaldehyde, 2-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, and m-hydroxybenzaldehyde.

[0091] Examples of the amine-based crosslinking agent include 4,4'-methylene-bis(2-chloroaniline), modified 4,4'-methylene-bis(2-chloroaniline), and diethyltoluenediamine.

[0092] The above-mentioned metal chelate crosslinking agent includes, for example, chelate compounds whose metal atom is aluminum, zirconium, titanium, zinc, iron, tin, etc., and aluminum chelate compounds are preferred from the viewpoint of performance.As aluminum chelate compounds, for example, diisopropoxyaluminum monooleyl acetoacetate, monoisopropoxyaluminum bisoleyl acetoacetate, monoisopropoxyaluminum monooleate monoethyl acetoacetate, diisopropoxyaluminum monolauryl acetoacetate, diisopropoxyaluminum monostearyl acetoacetate, diisopropoxyaluminum monoisostearyl acetoacetate, etc. can be mentioned.

[0093] The crosslinking agent (C) may be used alone or in combination of two or more kinds.

[0094] The content of the crosslinking agent (C) is usually preferably 0.01 to 20 parts by weight, particularly preferably 0.2 to 10 parts by weight, and further preferably 0.2 to 3 parts by weight, based on 100 parts by weight of the acrylic resin (A). If the crosslinking agent (C) is too little, the cohesive strength of the adhesive decreases, which tends to cause glue residue, while if the crosslinking agent (C) is too much, the flexibility and adhesive strength of the adhesive decrease, which tends to cause lifting between the processed member.

[0095] [Other ingredients] The pressure-sensitive adhesive composition of the present invention may further contain, for example, an ethylenically unsaturated compound in terms of peelability after irradiation with active energy rays, within a range that does not impair the effects of the present invention. The pressure-sensitive adhesive composition of the present invention may further contain additives such as antistatic agents, polymerization inhibitors, plasticizers, fillers, pigments, diluents, antioxidants, ultraviolet absorbers, ultraviolet stabilizers, tackifier resins, and photopolymerization initiators. These additives may be used alone or in combination of two or more. In particular, the polymerization inhibitor is effective in maintaining the stability of the pressure-sensitive adhesive layer. The content of the polymerization inhibitor when it is added is not particularly limited, but is preferably 0.01 to 5% by weight. In addition to the additives, a small amount of impurities contained in the manufacturing raw materials of the components of the pressure-sensitive adhesive composition may be contained.

[0096] [Adhesive composition] Thus, the pressure-sensitive adhesive composition of the present invention can be obtained by mixing the acrylic resin (A), the antioxidant (B), preferably the crosslinking agent (C), and, if necessary, other components. The content of the acrylic resin (A) in the entire pressure-sensitive adhesive composition is usually 50% by weight or more, preferably 60% by weight or more, and particularly preferably 70% by weight or more. If the content is too low, it becomes difficult to obtain the effects of the present invention.

[0097] The pressure-sensitive adhesive composition of the present invention is preferably used as a pressure-sensitive adhesive sheet for temporarily protecting the surface of a workpiece, such as an electronic substrate, a semiconductor wafer, a processed glass product, a metal plate, a plastic plate, etc. The pressure-sensitive adhesive sheet has a pressure-sensitive adhesive layer in which the pressure-sensitive adhesive composition is crosslinked. The pressure-sensitive adhesive sheet will now be described.

[0098] [Adhesive sheet] The pressure-sensitive adhesive sheet of the present invention usually has a base sheet, a pressure-sensitive adhesive layer made of the pressure-sensitive adhesive composition of the present invention, and a release film. In the method of producing such a pressure-sensitive adhesive sheet, the pressure-sensitive adhesive composition of the present invention is first applied directly onto a release film or a base sheet, either as is or after adjusting the concentration with an appropriate organic solvent. Then, the composition is dried, for example, by heating at 80 to 105°C for 0.5 to 10 minutes, and then attached to a base sheet or a release film to obtain a pressure-sensitive adhesive sheet. In addition, in order to balance the adhesive properties, aging may be further performed after drying.

[0099] Examples of the base sheet include sheets made of at least one synthetic resin selected from the group consisting of polyester resins such as polyethylene naphthalate, polyethylene terephthalate, polybutylene terephthalate, and polyethylene terephthalate / isophthalate copolymers; polyolefin resins such as polyethylene, polypropylene, and polymethylpentene; polyethylene fluoride resins such as polyvinyl fluoride, polyvinylidene fluoride, and polyethylene fluoride; polyamides such as nylon 6 and nylon 6,6; vinyl polymers such as polyvinyl chloride, polyvinyl chloride / vinyl acetate copolymer, ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, polyvinyl alcohol, and vinylon; cellulose resins such as cellulose triacetate and cellophane; acrylic resins such as polymethyl methacrylate, polyethyl methacrylate, polyethyl acrylate, and polybutyl acrylate; polystyrene; polycarbonate; polyarylate; and polyimide; metal foils such as aluminum, copper, and iron; paper such as fine paper and glassine paper; and woven fabrics and nonwoven fabrics made of glass fiber, natural fibers, synthetic fibers, and the like. These substrate sheets can be used as a single layer or as a multi-layered body in which two or more types are laminated. Among these, a sheet made of a synthetic resin is preferred from the viewpoint of weight reduction, etc.

[0100] Furthermore, as the release film, for example, various synthetic resin sheets, papers, woven fabrics, nonwoven fabrics, etc. exemplified above as the base material sheets can be used which have been subjected to a release treatment.

[0101] The method for applying the pressure-sensitive adhesive composition is not particularly limited as long as it is a common application method, and examples thereof include roll coating, die coating, gravure coating, comma coating, and screen printing.

[0102] The thickness of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is usually preferably from 4 to 200 μm, and more preferably from 5 to 100 μm.

[0103] The aging conditions are generally a temperature of room temperature (23°C) to 70°C, and a time of 1 to 30 days. Specifically, the aging may be performed under conditions such as 1 to 20 days at 23°C, 3 to 10 days at 23°C, or 1 to 7 days at 40°C.

[0104] The gel fraction of the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet is preferably 10 to 99% by weight from the viewpoint of adhesiveness, particularly preferably 20 to 97% by weight, and further preferably 40 to 95% by weight. If the gel fraction is too low, the adhesive strength to the workpiece tends to decrease, whereas if the gel fraction is too high, the adhesive strength to the workpiece tends to decrease.

[0105] The gel fraction is a measure of the degree of crosslinking (degree of hardening) and is calculated, for example, by the following method: The adhesive sheet is attached to a SUS mesh sheet (200 mesh), the adhesive sheet is wrapped, and then immersed in a sealed container containing ethyl acetate for 24 hours. The gel fraction is calculated from the change in weight of the adhesive layer before and after immersion in ethyl acetate using the following formula. Gel fraction (wt%) = weight (g) of adhesive layer after immersion in ethyl acetate / Weight of adhesive layer before immersion in ethyl acetate (g) x 100

[0106] The gel fraction of the pressure-sensitive adhesive layer can be adjusted to fall within the above range by adjusting the type and amount of the crosslinking agent (C), for example.

[0107] By irradiating the pressure-sensitive adhesive layer of the pressure-sensitive adhesive sheet of the present invention with active energy rays, the ethylenically unsaturated groups contained in the pressure-sensitive adhesive layer are polymerized to harden the pressure-sensitive adhesive layer, resulting in a decrease in adhesive strength and enabling peeling.

[0108] As the active energy ray, generally, light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, electromagnetic waves such as X-rays and gamma rays, as well as electron beams, proton beams, neutron beams, etc. can be used. From the viewpoints of curing speed, availability of irradiation equipment, cost, etc., ultraviolet rays are preferred.

[0109] The cumulative dose of ultraviolet light is usually 50 to 3,000 mJ / cm 2 , preferably 100 to 1,000 mJ / cm 2 The irradiation time varies depending on the type of light source, the distance between the light source and the adhesive layer, the thickness of the adhesive layer, and other conditions, but may usually be several seconds, or in some cases a fraction of a second.

[0110] The adhesive strength of the pressure-sensitive adhesive sheet varies depending on the type of substrate sheet, the type of workpiece, etc., but is preferably 3.0 N / 25 mm or more, more preferably 4.0 N / 25 mm or more before irradiation with active energy rays. The upper limit of the adhesive strength before irradiation with active energy rays is usually 100 N / 25 mm. The adhesive strength after irradiation with active energy rays is preferably 0.3 N / 25 mm or less, and more preferably 0.1 N / 25 mm or less.

[0111] The pressure-sensitive adhesive sheet of the present invention is also heated at 150° C. for 1 hour and then irradiated with ultraviolet light (accumulated irradiation amount 250 mJ / cm 2 ). 2 ) is preferably 1 N / 25 mm or less, and more preferably 0.5 N / 25 mm or less.

[0112] Furthermore, the pressure-sensitive adhesive sheet of the present invention is heated at 175° C. for 1 hour and then irradiated with ultraviolet light (accumulated irradiation amount 250 mJ / cm 2 ) is preferably 1 N / 25 mm or less, and more preferably 0.7 N / 25 mm or less.

[0113] The adhesive composition of the present invention is useful as a peelable adhesive sheet, for example, by laminating an adhesive sheet using the adhesive composition as an adhesive layer to a workpiece, temporarily protecting the surface of the workpiece, and then irradiating it with active energy rays, which hardens the adhesive layer and reduces the adhesive strength, allowing it to be easily peeled off from the workpiece.Furthermore, since the adhesive sheet of the present invention has excellent heat resistance, even if it is subjected to a heating process of, for example, 150°C or higher, particularly 175°C or higher after being attached to the surface of the workpiece, it exhibits excellent peelability with reduced adhesive strength and no adhesive residue by subsequent irradiation with active energy rays. EXAMPLES

[0114] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention. Note that "%" and "parts" are based on weight.

[0115] [Production of acrylic resin (A-1)] A 4-neck round-bottom flask equipped with a reflux condenser, a stirrer, nitrogen gas blowing and a thermometer was charged with 65 parts of ethyl acetate, and the internal temperature was raised to the boiling point to start the reaction. The above-prepared 2-ethylhexyl acrylate (2EHA) 70 parts, 2-hydroxyethyl acrylate (HEA) 17 parts, acryloylmorpholine (ACMO) 10 parts, and azobisisobutyronitrile (AIBN) 0.045 parts as a polymerization initiator were dropped over 2 hours. After reacting for one hour, 2-hydroxyethyl acrylate (HEA) 3 parts and 7.5 parts of ethyl acetate solution were added and reacted at reflux temperature for 0.5 hours. Further, 7.5 parts of ethyl acetate solution containing 1% AIBN were added and reacted at reflux temperature for 2 hours, and 30 parts of ethyl acetate solution containing 0.3% AIBN were added again and reacted at reflux temperature for 2 hours, after which the reaction was stopped and diluted with ethyl acetate to obtain an acrylic resin (A1) solution. To the acrylic resin (A1) solution obtained above, 2-methacryloyloxyethyl isocyanate (hereinafter referred to as "MOI") (manufactured by Showa Denko KK) and dibutyltin dilaurate as a urethanization catalyst were appropriately added, and the mixture was reacted at 50°C for 18 hours, after which 0.02 parts of MEHQ was added to obtain an ethylenically unsaturated group-containing acrylic resin (A-1) solution (solid content 45.9%, viscosity 4900mPa·s / 25°C, acrylic resin (A-1): weight average molecular weight (Mw) 780,000, dispersity (Mw / Mn) 5.5). The urethanization rate of HEA by MOI was 90mol%, the content of ethylenically unsaturated groups was 125mmol / 100g, and the number of parts of MOI per 100 parts of acrylic resin (A1) was 24.1 parts.

[0116] [Table 1]

[0117] [Antioxidant (B)] The following were prepared as a primary antioxidant (B1) and other primary antioxidants (B'1). (B1-1) Irganox 1010 (pentaerythritol tetrakis(3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate), manufactured by BASF Japan Ltd.) (B1-2) Yoshinox BB (4,4'-butylidenebis6-tert-butyl-3-methylphenol, manufactured by Mitsubishi Chemical Corporation) (B1-3) Yoshinox 425 (2,2'-methylenebis 6-tert-butyl-4-ethylphenol, manufactured by Mitsubishi Chemical Corporation) (B'1-1) Yoshinox BHT (2,6-di-t-butyl-p-cresol, manufactured by API Corporation)

[0118] The following were prepared as secondary antioxidant (B2) and other secondary antioxidants (B'2). (B2-1) Irgafos 168 (Tris(2,4-di-tert-butylphenyl)phosphite, manufactured by BASF Japan Ltd.) (B'2-1) DLTP "Yoshitomi" (dilauryl thiodipropionate, API Corporation) (B'2-2) DSTP "Yoshitomi" (distearyl thiodipropionate, API Corporation) (B'2―3) DMTP "Yoshitomi" (dimyristyl thiodipropionate, API Corporation)

[0119] [Crosslinking agent (C)] The following was prepared as the crosslinking agent (C-1). Takenate D101E (adduct of tolylene diisocyanate and trimethylolpropane, manufactured by Mitsui Chemicals)

[0120] [Photopolymerization initiator] The following photopolymerization initiators were prepared: Omnirad127 (2-hydroxy-1-(4-(2-hydroxy-2-methylpropionyl)benzyl)phenyl)-2-methylpropan-1-one, manufactured by IGM Resins Omnirad379EG (2-Dimethylamino-2-(4-methyl-benzyl)-1-(4-morpholin-4-yl-phenyl)-butan-1-one, IGM Resins)

[0121] <Examples 1 to 4 and Comparative Examples 1 to 11> To 100 parts of the acrylic resin prepared as described above, the antioxidant (B), the crosslinking agent (C) and the photopolymerization initiator were added and mixed as shown in Table 2 below, and the resultant was adjusted with ethyl acetate to a solid content concentration (resin content) of 30% by weight to obtain a pressure-sensitive adhesive composition solution.

[0122] [Table 2]

[0123] The adhesive composition solution obtained above was used to prepare an adhesive sheet as described below, and the adhesive strength was measured and evaluated. The evaluation results are shown in Table 3.

[0124] <Adhesive sheet (S1) (for gel fraction measurement)> The adhesive composition solution obtained above was applied to a heavy release 38 μm polyester-based release sheet (manufactured by Mitsui Chemicals Tocello: Lumirror (registered trademark) SP03-38BU) so that the thickness after drying would be 25 μm, and after drying at 100° C. for 5 minutes, this was bonded to a light release 38 μm polyester-based release sheet (manufactured by Mitsui Chemicals Tocello: Lumirror (registered trademark) SP01-38BU) and aged for 3 days in an environment of 40° C. to obtain an adhesive sheet (S1) for gel fraction measurement.

[0125] <Adhesive sheet (S2) (for measuring adhesive strength)> The adhesive composition solution obtained above was applied to a polyimide film (film thickness 50 μm) ("Kapton 200H" manufactured by Toray DuPont Co., Ltd.) so that the thickness after drying would be 25 μm, and after drying at 100° C. for 5 minutes, the film was attached to a 38 μm polyester-based release sheet with a light peeling property (Lumirror (registered trademark) SP01-38BU manufactured by Mitsui Chemicals Tocello Co., Ltd.) and aged for 3 days in an environment of 40° C. to obtain an adhesive sheet (S2) for adhesive strength measurement.

[0126] [Gel fraction] The pressure-sensitive adhesive sheet (S1) was cut to 40 mm x 40 mm, and the light release 38 μm polyester release sheet was peeled off, and the pressure-sensitive adhesive layer side was attached to a 50 mm x 100 mm SUS mesh sheet (200 mesh). Next, the heavy release 38 μm polyester release sheet was peeled off, and the SUS mesh sheet was folded back from the center in the longitudinal direction to encase the sample. The sample was immersed in a sealed container containing 250 g of ethyl acetate for 24 hours, and the gel fraction was calculated from the weight change of the pressure-sensitive adhesive layer before and after immersion in ethyl acetate using the following formula. Gel fraction (%) = (weight (g) of adhesive layer after immersion in ethyl acetate) / Weight of adhesive layer before immersion in ethyl acetate (g) × 100

[0127] [Room temperature adhesive strength before exposure to active energy rays] A 25 mm x 100 mm test piece was prepared from the above adhesive sheet (S2), and the light release 38 μm polyester-based release sheet was peeled off. The test piece was then pressure-attached to an alkali-free glass plate (Corning Eagle XG) by rolling a 2 kg rubber roller back and forth twice in an atmosphere of 23°C and 50% RH, and allowed to stand for 30 minutes in the same atmosphere. The 180 degree peel strength (N / 25 mm) was then measured at a peel speed of 300 mm / min.

[0128] [Room temperature adhesive strength after exposure to active energy rays (high pressure mercury lamp)] A 25mm x 100mm test piece was prepared from the above pressure sensitive adhesive sheet (S2), the 38μm polyester release sheet was peeled off, and the piece was pressed and attached to an alkali-free glass plate (Corning, Eagle XG) by rolling a 2kg rubber roller back and forth twice in an atmosphere of 23°C and 50%RH, and left to stand in the same atmosphere for 30 minutes. After that, the piece was irradiated with ultraviolet light (accumulated irradiation amount 250mJ / cm2) from the non-alkali-free glass plate side using one 80W high pressure mercury lamp. 2 ) and allowed to stand for 30 minutes in an atmosphere of 23°C and 50% RH, after which the 180° peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min.

[0129] [Adhesive strength after heating at 150℃ and before exposure to active energy rays] A 25mm x 100mm test piece was prepared from the above adhesive sheet (S2), the 38μm polyester release sheet with light release was peeled off, and the piece was pressed and attached to an alkali-free glass plate (Corning, Eagle XG) by rolling a 2kg rubber roller back and forth twice in an atmosphere of 23°C and 50%RH, and then heat-treated at 150°C for 1 hour. The stainless steel plate with the heat-treated adhesive sheet attached was left to stand for 1 hour in an atmosphere of 23°C and 50% relative humidity, and then the 180° peel strength (N / 25mm) was measured at a peel speed of 300mm / min. Evaluation was performed as follows. 〇7N / 25mm or more × Less than 7N / 25mm

[0130] [Adhesive strength after heating at 150℃ and exposure to active energy rays] A test piece of 25 mm x 100 mm was prepared from the above adhesive sheet (S2), the light release 38 μm polyester-based release sheet was peeled off, and the piece was pressed and attached to an alkali-free glass plate (Corning, Eagle XG) by rolling a rubber roller weighing 2 kg back and forth twice under an atmosphere of 23 ° C and 50% RH, and then heat-treated at 150 ° C for 1 hour. The stainless steel plate to which the heat-treated adhesive sheet was attached was left for 1 hour under an atmosphere of 23 ° C and 50% relative humidity, and then irradiated with ultraviolet light (cumulative irradiation amount 250 mJ / cm 2 ) from the alkali-free glass plate side using one 80 W high-pressure mercury lamp, and left for 30 minutes under an atmosphere of 23 ° C and 50% RH, and the 180-degree peel strength (N / 25 mm) was measured at a peel speed of 300 mm / min. Evaluation was performed as follows. 〇 0.5N / 25mm or less × Larger than 0.5N / 25mm

[0131] [Table 3]

[0132] [Adhesive strength after heating at 175℃ and before exposure to active energy rays] A 25mm x 100mm test piece was prepared from the above adhesive sheet (S2), the 38μm polyester release sheet with light release was peeled off, and the piece was pressed and attached to an alkali-free glass plate (Corning, Eagle XG) by rolling a 2kg rubber roller back and forth twice in an atmosphere of 23°C and 50%RH, and then heat-treated at 175°C for 1 hour. The stainless steel plate with the heat-treated adhesive sheet attached was left to stand for 1 hour in an atmosphere of 23°C and 50% relative humidity, and then the 180° peel strength (N / 25mm) was measured at a peel speed of 300mm / min. Evaluation was performed as follows. 〇7N / 25mm or more × Less than 7N / 25mm

[0133] [Adhesive strength after heating to 175℃ and exposure to active energy rays] A 25mm x 100mm test piece was prepared from the above adhesive sheet (S2), the light release 38μm polyester release sheet was peeled off, and the piece was pressed and attached to an alkali-free glass plate (Corning, Eagle XG) by rolling a 2kg rubber roller back and forth twice under an atmosphere of 23°C and 50%RH, and then heat-treated at 175°C for 1 hour. The stainless steel plate to which the heat-treated adhesive sheet was attached was left for 1 hour under an atmosphere of 23°C and 50% relative humidity, and then irradiated with ultraviolet light (cumulative irradiation amount 250mJ / cm2) from the alkali-free glass plate side using one 80W high-pressure mercury lamp, and left for 30 minutes under an atmosphere of 23°C and 50%RH, and the 180° peel strength (N / 25mm) was measured at a peel speed of 300mm / min. Evaluation was performed as follows. 〇 0.7N / 25mm or less × 0.7N / 25mm or larger

[0134] [Table 4]

[0135] From the above evaluation results, it was found that Examples 1 to 4 had sufficient adhesive strength before irradiation with active energy rays, had excellent heat resistance, and even when exposed to high temperatures, the adhesive strength was reduced after irradiation with active energy rays, there was no adhesive residue, and they had excellent peelability. In contrast, the adhesive strength reduction after exposure to high temperatures and subsequent irradiation with active energy rays was insufficient in Comparative Examples 1 to 3, 5, 6, 9, and 11. Also, in Comparative Examples 4, 8, and 10, the adhesive strength before irradiation with active energy rays was reduced. From this, it can be seen that in order to maintain sufficient adhesive strength before exposure to active energy rays while reducing the adhesive strength after exposure to high temperatures, it is important to contain a primary antioxidant and a secondary antioxidant, and in particular, it is important to use in combination a primary antioxidant that is a dimer, trimer, or tetramer and does not have a bonding site at the ortho position of the hydroxyl group with a phosphorus-based secondary antioxidant. [Industrial Applicability]

[0136] The pressure-sensitive adhesive composition of the present invention can be suitably used as a pressure-sensitive adhesive sheet for temporary surface protection during processing of electronic substrates, semiconductor wafers, processed glass products, metal plates, plastic plates, and the like.

Claims

1. An active energy ray-curable pressure-sensitive adhesive composition comprising an acrylic resin (A) and an antioxidant (B), wherein the antioxidant (B) comprises a primary antioxidant (B1) and a secondary antioxidant (B2) (excluding the antioxidant (B1)), the primary antioxidant (B1) is a dimer, trimer or tetramer, and the secondary antioxidant (B2) is a phosphorus-based antioxidant.

2. 2. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) has a structural unit derived from an alkyl group-containing (meth)acrylate (a1) and a structural unit derived from a functional group-containing monomer other than an amide group (a2).

3. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1 , wherein the acrylic resin (A) has a structural unit derived from an amide group-containing monomer (a3).

4. 2. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) further contains an ethylenically unsaturated group.

5. 2. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the acrylic resin (A) has an ethylenically unsaturated group content of 5 to 250 mmol / 100 g.

6. 2. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, wherein the primary antioxidant (B1) has no bonding site at the ortho-position of the hydroxyl group.

7. The active energy ray-curable pressure-sensitive adhesive composition according to claim 1, further comprising a crosslinking agent (C).

8. 9. A pressure-sensitive adhesive sheet comprising a pressure-sensitive adhesive layer crosslinked with the active energy ray-curable pressure-sensitive adhesive composition according to claim 1.

9. 10. The pressure-sensitive adhesive sheet according to claim 9, wherein the pressure-sensitive adhesive layer is cured and becomes peelable by irradiation with active energy rays.

Citation Information

Patent Citations

  • Adhesive composition for conductive member

    JP2017025212A

  • Ultraviolet-curable hot-melt adhesive

    JP2019218480A

  • Active energy ray-curable adhesive composition and adhesive sheet, and use thereof

    WO2019225719A1

  • Pressure-sensitive adhesive sheet

    WO2020162330A1

  • Masking material

    JP2019145575A