Polyvinyl alcohol-based resin, method for producing the same, and polyvinyl ester-based polymer and method for producing the same
By incorporating specific structural units into polyvinyl alcohol resin, the resin achieves superior gas barrier and moldability, addressing productivity and residual monomer issues, resulting in a high-performance packaging material.
Patent Information
- Application Number
- JP2023049610
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Polyvinyl alcohol resins face challenges in achieving high gas barrier properties and moldability due to chain transfer reactions during polymerization, leading to poor productivity and residual monomer issues.
Introducing structural units represented by general formulas (1) and/or (2) into polyvinyl alcohol resin, using a compound with structure (3) as a copolymerization monomer, which improves gas barrier properties and moldability while minimizing residual monomer content.
The modified polyvinyl alcohol resin exhibits excellent gas barrier properties under high humidity, low melting point, and enhanced moldability, with improved productivity due to reduced residual monomer amounts.
Smart Images

Figure 2024138893000014 
Figure 2024138893000001 
Figure 2024138893000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyvinyl alcohol resin, a method for producing the same, and a polyvinyl alcohol The present invention relates to a steric polymer and a method for producing the same. [Background technology]
[0002] Polyvinyl ester polymers have been widely used as raw materials for polyvinyl alcohol resins. Polyvinyl alcohol resin is a type of polyvinyl ester such as polyvinyl acetate. It is a crystalline water-soluble polymer material obtained by saponifying a methacrylic polymer. Using the solubility and film properties (strength, oil resistance, film-forming ability, oxygen gas barrier properties, etc.), Used as a turbidifying agent, surfactant, textile processing agent, various binders, paper processing agent, adhesive, film, etc. It has been done.
[0003] In addition, to prevent food and medicine from deteriorating or spoiling due to oxygen in the air, Gas barrier properties (especially oxygen barrier properties) are required for packaging materials. Polyvinyl alcohol resins, which have excellent gas barrier properties, transparency, and aroma retention, are also useful as packaging materials. Fat is used.
[0004] On the other hand, polyvinyl alcohol resin has a high melting point and poor moldability, and moisture dissipates in high humidity conditions. It is known that the crystallinity and gas barrier properties of the polymer are reduced by the addition of molecules. A method of improving moldability by lowering the melting point of polyvinyl alcohol resin and a method of improving moldability by modifying polyvinyl alcohol resin For example, Patent Document 1 discloses a method for improving the barrier properties of polyvinyl acetate. By introducing an alicyclic skeleton into alcohol resin, the glass transition temperature (Tg) is increased, and the It is described that the barrier properties are improved under high temperatures. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2008-202048 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the monomers such as 2-norbornene described in Patent Document 1 are radically copolymerized. When the ethylenediamine is introduced into polyvinyl alcohol resin, chain transfer reaction to 2-norbornene occurs during polymerization. This reaction occurs very easily, making it difficult to control the modification rate and degree of polymerization. If the modification rate is low, the melting point is not lowered much, and it is difficult to improve moldability. -Olefins such as norbornene are used in combination with vinyl ester monomers such as vinyl acetate. It has poor polymerization properties, and 2-norbornene tends to remain at the end of polymerization, which creates problems in terms of productivity. Ta.
[0007] In the present invention, therefore, under such circumstances, the present invention aims to obtain a copolymerized monomer remaining in the polymerization process. Polyvinyl alcohol has very little mer, excellent productivity, and excellent gas barrier properties and moldability. Polyvinyl ester resin and its manufacturing method, and its raw material polyvinyl ester resin and its manufacturing method The present invention aims to provide a manufacturing method thereof. [Means for solving the problem]
[0008] However, the present inventors have discovered that a structural unit represented by general formula (1) and / or general formula (2) The introduction of ethylenediaminetetraacetate into polyvinyl alcohol resin improves gas barrier properties and moldability under high humidity conditions. It is possible to produce a copolymer by using a compound having the structure of the general formula (3) as a copolymerization monomer. By this, the polyvinyl alcohol resin is formed into a compound having a structure represented by the general formula (1) and / or the general formula (2). It is possible to modify the copolymer, and the amount of copolymerized monomer remaining at the end of polymerization is small. We have discovered and completed the present invention.
[0009] That is, the gist of the present invention is the following [1] to [6]. [1] Having a structural unit represented by the following general formula (1) and / or the following general formula (2): A polyvinyl alcohol resin characterized by:
[0010] [ka]
[0011] [ka]
[0012] (In the above formula (2), R 1 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .) [2] The structural units represented by the above general formula (1) and / or the above general formula (2) are contained in a resin. The monomer structural units are contained in an amount of 0.1 to 30 mol % based on the total amount of the monomer structural units. [1] The polyvinyl alcohol resin according to claim 1. [3] [1] or [2], characterized in that the degree of saponification is 80 to 99.9 mol% or less. The polyvinyl alcohol resin according to claim 1. [4] Any one of [1] to [3], characterized in that the average degree of polymerization is 200 to 5,000. The polyvinyl alcohol resin according to claim 1. [5] A polyvinyl ester having a structural unit represented by the above general formula (2). Polymers based on methacrylic acid. [6] The structural unit represented by the above general formula (2) is The polyvinyl ester-based copolymer according to [5] above is contained in an amount of 0.1 to 30 mol %. Polymer. [7] A compound having a structural unit represented by the above general formula (1) and / or the above general formula (2). The method for producing the polyvinyl alcohol resin according to claim 1, comprising the steps of: The method is characterized by comprising a step of saponifying a polyvinyl ester polymer having a structural unit The present invention relates to a method for producing a polyvinyl alcohol-based resin. [8] The polyvinyl chloride according to [5] or [6], having a structural unit represented by the above general formula (2). The present invention relates to a method for producing a vinyl ester polymer, the method comprising the steps of: and a compound represented by the formula (1): Method for producing tere polymers.
[0013] [ka]
[0014] (In the above formula (3), R 2 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .) [1] Radical polymerization of a vinyl ester monomer and a compound represented by the above general formula (3) In the step of carrying out the above, a solution containing the compound represented by the general formula (3) is continuously added dropwise. The method for producing a polyvinyl ester polymer according to [8], Effect of the Invention
[0015] The polyvinyl alcohol-based resin of the present invention has high gas barrier properties under high humidity conditions and is therefore suitable for use in foods and pharmaceuticals. The polyvinyl chloride of the present invention can be suitably used as a gas barrier layer for packaging materials such as those described above. Nyl alcohol-based resins have a low melting point and excellent moldability. In addition, by using a compound having the structure of general formula (3) as a monomer, polyvinyl alcohol can be obtained. The resin can be modified with the structure of general formula (1) and / or general formula (2), Furthermore, the amount of copolymerization monomer remaining at the end of polymerization is small, resulting in excellent productivity. BEST MODE FOR CARRYING OUT THEINVENTION
[0016] The present invention will be described in more detail below. (sometimes referred to as "PVA resin") is a polyvinyl alcohol resin that contains vinyl. a structure represented by the following general formula (1) and / or general formula (2): The present invention is characterized by having a unit. Each of the components of the present invention will be described below.
[0017] [Vinyl alcohol structural unit] The PVA resin of the present invention has at least a vinyl alcohol structural unit. The cholesteryl structural unit is obtained by saponifying the structural unit derived from the vinyl ester monomer. Examples of vinyl ester monomers include vinyl formate, vinyl acetate, and propylene. Vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, Vinyl acrylate, vinyl laurate, vinyl stearate, vinyl benzoate, Versatile Among them, vinyl acetate is preferably used from an economical viewpoint.
[0018] The content of vinyl alcohol units in the polyvinyl alcohol resin is not particularly limited. However, it is preferably 40 mol % or more and less than 99.9 mol % based on 100 mol % of all structural units. More preferably, the ratio is 50 mol % or more and 99 mol % or less, and further preferably, 60 mol % or more. If the content is less than 40 mol %, the gas barrier properties will be insufficient. There may be cases where this occurs.
[0019] [Structural unit represented by general formula (1)] The structural unit represented by the following general formula (1) is 2-(allyloxymethyl)acrylic acid or a structural unit derived from a salt thereof or a 2-(allyloxymethyl)acrylic acid ester, The structural units derived from vinyl alcohol or vinyl ester monomers are lactonized to form The structural unit obtained is sodium 2-(allyloxymethyl)acrylic acid salt. Examples of the salts include ammonium salts, lithium salts, potassium salts, calcium salts, and magnesium salts. As the (allyloxymethyl) acrylic acid ester, 2-(allyloxymethyl) acrylate is methyl acrylate, ethyl 2-(allyloxymethyl)acrylate, ethyl 2-(allyloxymethyl)acrylate ) n-Propyl acrylate, 2-(allyloxymethyl)i-propyl acrylate, 2- (Allyloxymethyl)acrylate n-Butyl, 2-(Allyloxymethyl)acrylic acid i-Butyl, 2-(allyloxymethyl)acrylate t-Butyl, 2-(allyloxymethyl)acrylate 2-(allyloxymethyl)acrylate n-pentyl, 2-(allyloxymethyl)acrylate n-hexyl, 2-(allyloxymethyl) cyclohexyl acrylate, etc., but from an economical point of view Of these, methyl 2-(allyloxymethyl)acrylate is preferably used.
[0020] [ka]
[0021] [Structural unit represented by formula (2)] R in the structural unit represented by the following general formula (2) 1 is a metal atom, hydrogen atom, or carbon number 1 is an alkyl group having a carbon number of 1 to 6, preferably a hydrogen atom, a methyl group, or an ethyl group, and particularly preferably Most often it is a methyl group. The structural unit represented by the general formula (2) is 2-(allyloxymethyl)acrylic acid or or a structural unit derived from 2-(allyloxymethyl)acrylic acid ester. Salts of 2-(allyloxymethyl)acrylic acid include sodium salts, lithium salts, potassium salts, and Examples of the salt include 2-(allyloxymethyl)acrylamide, calcium salt, and magnesium salt. The acrylate esters include methyl 2-(allyloxymethyl)acrylate, methyl 2-(allyl 2-(allyloxymethyl)acrylate n-propyl , 2-(allyloxymethyl)acrylate i-propyl, 2-(allyloxymethyl)acrylate n-Butyl acrylate, 2-(allyloxymethyl) isobutyl acrylate, 2-(allyl 2-(allyloxymethyl)acrylate n-pentene n-Hexyl, 2-(allyloxymethyl)acrylate, 2-(allyloxymethyl)acrylate ) cyclohexyl acrylate, etc., but from an economical point of view, 2-(allyloxy Methyl)acrylate is preferably used.
[0022] [ka]
[0023] (In the above formula (2), R 1 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .)
[0024] The PVA resin of the present invention is represented by the above general formula (1) and / or the above general formula (2). The structural unit is contained in an amount of 0.1 to 30 mol % based on the total amount of monomer structural units in the resin. It is preferable that the content of the aryl group is 0.5 to 20 mol %, particularly preferably 1 to 10 mol %. do. When the content is within the above specific range, the gas barrier property tends to be good and the productivity tends to be excellent. In addition, the structural unit represented by the above general formula (1) and the structural unit represented by the above general formula (2) are preferably used. The proportion of structural units present is preferably such that the structural units represented by the above general formula (1) are more abundant.
[0025] [Ethylene structural unit] The PVA resin of the present invention, especially when copolymerized with ethylene, has a low crystallinity of the copolymer. The lower melting point is preferable because it makes melt molding easier. The ratio of the ethylene structural unit to the total amount of structural units is usually 1 to 70 mol %, preferably 1 It is preferably from 0 to 60 mol %, more preferably from 25 to 50 mol %.
[0026] [Other structural units] In addition, the PVA resin of the present invention is usually 10 mol % or less within a range that does not impair the gist of the invention. In the above, a copolymerizable ethylenically unsaturated monomer other than ethylene may be copolymerized. Such monomers include olefins such as propylene, 1-butene, and isobutene; Acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) ) Unsaturated acids such as itaconic acid, their salts, or mono- or di-alkyl ethers having 1 to 18 carbon atoms Acrylamide, N-alkylacrylamide with 1 to 18 carbon atoms, N,N-diacrylamide Methylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylic Amidopropyldimethylamine, its salts and its quaternary salts; C1-18 N-alkyl methacrylamide, N,N-dimethyl methacrylamide arylamide, 2-methacrylamidopropanesulfonic acid or its salt, methacrylamide Methacrylamides such as propyldimethylamine, its salts and its quaternary salts; N-vinyl Pyrrolidone, N-vinylformamide, N-vinylacetamide, and other N-vinylamides Vinyl cyanides such as acrylonitrile and methacrylonitrile; Alkenes with 1 to 18 carbon atoms alkyl vinyl ether, hydroxyalkyl vinyl ether, alkoxyalkyl vinyl ether vinyl ethers such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinyl halides such as vinyl silane, vinyl bromide, etc.; vinyl trimethoxysilane, vinyl methyl Vinyl silanes such as dimethoxysilane and vinyldimethoxysilane; Allyl acetate; 2-acetate Methylallyl;3,4-Diacetoxy-1-butene;Vinyl ethylene carbonate;Chloride Allyl;Allyl alcohol;2-Methylallyl alcohol;Dimethylallyl alcohol; 3,4-Dihydroxy-1-butene; Trimethyl-(3-acrylamido-3-dimethyl) Propyl)-ammonium chloride; acrylamido-2-methylpropanesulfonic acid, etc. Examples include:
[0027] The degree of saponification of the polyvinyl alcohol resin of the present invention is usually 80 mol % or more, preferably It is preferably 90 mol % or more, and more preferably 98 mol % or more.
[0028] The average degree of polymerization of the polyvinyl alcohol resin of the present invention (measured in accordance with JIS K 6726) The standard is usually 200-5000, more preferably 300-3000, and especially 500-2200. It is preferable that there is.
[0029] The polyvinyl alcohol resin of the present invention has a glass transition point (Tg) of usually 75 to 180° C. The reaction temperature is preferably 78 to 140° C., and particularly preferably 82 to 120° C. The PVA resin according to the present invention when copolymerized usually has a glass transition temperature (Tg) of 60 to 1 The temperature is 60°C, preferably 65 to 130°C, and particularly preferably 70 to 110°C. The higher the glass transition temperature (Tg), the better the gas barrier properties. The transition point (Tg) was measured using a differential scanning calorimeter during the second heating (second-time heating). (temperature).
[0030] Next, the method for producing the polyvinyl alcohol resin of the present invention will be described. The polyvinyl chloride having the structural units represented by the general formula (1) and / or the general formula (2) of the present invention The method for producing the aryl alcohol resin is not particularly limited, but may be a method represented by the general formula (2 ) by saponifying a polyvinyl ester polymer having a structural unit represented by the formula It is preferable to use a polyvinyl copolymer having a structural unit represented by the general formula (2). The ester polymer is prepared by laminating a vinyl ester monomer and a compound represented by the general formula (3). It is preferable that the polymer is produced by dichloromethane polymerization. The above manufacturing method will now be described in detail.
[0031] [Method of producing polyvinyl ester polymer having a structural unit represented by general formula (2) (polymerization combination process)] First, the compound represented by the following general formula (3) will be described. R in the compound represented by the following general formula (3) 2 is a metal atom, a hydrogen atom, or a carbon atom having 1 to 1 6 alkyl group, preferably a hydrogen atom, a methyl group, or an ethyl group, and particularly preferably is a methyl group. Specific examples of the compound represented by the following general formula (3) include 2-(allyloxymethyl) 2-(allyloxymethyl)acrylic acid, sodium 2-(allyloxymethyl)acrylate, 2-(allyloxymethyl)acrylate lithium, 2-(allyloxymethyl)acrylate potassium, 2- Calcium (allyloxymethyl)acrylate, 2-(allyloxymethyl)acrylic acid Magnesium, 2-(allyloxymethyl) acrylate, 2-(allyloxymethyl) 2-(allyloxymethyl)acrylate n-propyl 2-(allyloxymethyl)acrylate 2-(allyloxymethyl)acrylic acid i-propyl, 2-(allyloxymethyl)acrylic acid n -Butyl, 2-(allyloxymethyl)acrylate i-Butyl, 2-(allyloxymethyl)acrylate 2-(allyloxymethyl)acrylate n-pentyl, 2-(allyloxymethyl)acrylate n-pentyl (Allyloxymethyl)acrylate n-Hexyl, 2-(Allyloxymethyl)acrylate cyclohexyl acrylate, and the like, preferably 2-(allyloxymethyl)methyl acrylate. It is.
[0032] [ka]
[0033] (In the above formula (3), R 2 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .)
[0034] [Polymerization process] Radical polymerization of vinyl ester monomers and the compound represented by the above general formula (3) The method is not particularly limited, and may be bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization, or emulsion polymerization. Although known methods such as polymerization can be used, solution polymerization is usually carried out. The method of feeding the monomer components during radical polymerization is not particularly limited, and may be a single feeding method, a separate feeding method, or the like. Any method such as batch feeding or continuous feeding can be used, but the polymer produced during polymerization is generally Since the compound represented by formula (3) is uniformly incorporated, the compound represented by general formula (3) is It is preferable to continuously add the solution containing the compound dropwise. In the case of copolymerizing ethylene, for example, pressurized polymerization of ethylene can be adopted. By adjusting the pressure of ethylene, it is possible to control the amount of ethylene introduced. Although it depends on the desired ethylene content, the pressure is usually 1 to 80 kg / cm 2 is selected from.
[0035] Solvents used in such radical polymerization are usually methanol, ethanol, propane, etc. Lower alcohols such as polyol and butanol, ketones such as acetone and methyl ethyl ketone Examples of esters include methyl acetate, ethyl acetate, and butyl acetate. The amount of the solvent used is determined according to the desired degree of polymerization and the chain structure of the solvent. The transfer constant should be taken into consideration when selecting the appropriate solvent. For example, when the solvent is methanol, the solvent / mono The mass ratio is selected from the range of about 0.01 to 10, preferably about 0.05 to 3. It is selected. The polymerization initiator used in such radical polymerization is, for example, 2,2'-azobisisopropyl butyronitrile, acetyl peroxide, benzoyl peroxide, lauryl peroxide, and other known radicals. Polymerization initiator, 2,2'-azobis(2,4-dimethylvaleronitrile), 2,2'-azobis(2,4-dimethylvaleronitrile) Radical polymerization for low-temperature polymerization of benzobis(4-methoxy-2,4-dimethylvaleronitrile) etc. The amount of the polymerization initiator used varies depending on the type of initiator, and cannot be determined in general. The polymerization rate is not limited to a specific value, and can be selected arbitrarily. For example, azoisobutyronitrile and peroxy acid When acetyl chloride is used, the amount is 0.001 to 0.2 mol% based on the vinyl ester monomer. is preferable, and 0.01 to 0.1 mol % is particularly preferable.
[0036] The reaction temperature of such radical polymerization is about 20°C to the boiling point depending on the solvent and pressure used. It is not necessary to carry out the polymerization at a constant temperature until the end of the polymerization. This may be changed by adding additional polymerization initiator. The polymerization time is preferably 1 to 20 hours, more preferably 2 to 12 hours, in the case of a batchwise polymerization. In this case, the average residence time in the polymerization vessel is preferably 2 to 10 hours, more preferably 2 to 8 hours. If the residence time is too short, it becomes difficult to control the polymerization to achieve high productivity (high polymerization rate). On the other hand, if it is too long, it is not preferable because it causes problems in terms of productivity. If necessary, a polymerization inhibitor may be added to terminate the polymerization. Examples of the polymerization inhibitor include: Examples of the amine include, but are not limited to, hydroquinone, aniline, anthracene, nitrobenzene, Dinitrobenzene, trinitrobenzene, benzonitrile, benzophenone, N,N-di Examples of suitable amines include methylformamide, cinnamic alcohol, cinnamic acid, and sorbic acid. In the case of the above, unreacted monomers and the like are removed by distillation.
[0037] The polyvinyl ester polymer of the present invention has the structural unit represented by the above general formula (2) as a resin. It is preferable that the content of the monomer structural units in the copolymer is 0.1 to 30 mol %, and particularly The content is preferably 0.5 to 20 mol %, and more preferably 1 to 10 mol %. If the polyvinyl alcohol obtained by saponifying the polyvinyl ester polymer falls within a specific range, Coal-based resins tend to have good gas barrier properties and excellent productivity, and are therefore preferred.
[0038] [Polyvinyl alkenyl having structural units represented by general formula (1) and / or general formula (2)] Manufacturing method of coal resin (saponification process)] The polyvinyl chloride having the structural units represented by the general formula (1) and / or the general formula (2) of the present invention The hydroxyl alcohol-based resin is produced by the saponification process described below, The polyvinyl ester polymer having the structural unit represented by the formula (I) is saponified. It is preferred. The polyvinyl ester polymer having the structural unit represented by the general formula (2) obtained above The mixture is mixed in batches using a mixer or kneader, or continuously on a belt or in a column. To become. The saponification is carried out by subjecting the polyvinyl ester having the structural unit represented by the general formula (2) obtained above to saponification. The olefin polymer is dissolved in alcohol or water-containing alcohol, and reacted with the solvent in the presence of an alkali or acid catalyst. The alcohols are methanol, ethanol, propanol, tert-butyl alcohol, and Among them, methanol is particularly preferred. The concentration of the polymer is appropriately selected depending on the viscosity of the system, but is usually selected from the range of 4 to 60% by mass. do.
[0039] The catalyst used for saponification is not particularly limited, and examples thereof include sodium hydroxide, potassium hydroxide, etc. methyl, sodium methylate, sodium ethylate, potassium methylate, lithium methylate Alkaline catalysts such as hydroxides and alcoholates of alkali metals such as sulfuric acid, hydrochloric acid, nitric acid, etc. Examples of the acid catalyst include acid, methanesulfonic acid, zeolite, and cation exchange resin. The amount of the saponification catalyst to be used is appropriately selected depending on the saponification method, the desired degree of saponification, etc. However, when an alkali catalyst is used, a poly(ethylene glycol) having a structural unit represented by the general formula (2) is used. The amount is usually 0.01 to 5 mol % based on the total amount of monomer structural units of the vinyl ester polymer, and preferably A content of 0.2 to 1.7 mol % is preferable.
[0040] The reaction temperature for the saponification reaction is not particularly limited, but is preferably 10 to 80° C., and more preferably 10 to 80° C. The temperature is preferably 20 to 70° C. The saponification reaction is usually carried out for 0.5 to 5 hours. These conditions are appropriately adjusted to obtain the desired degree of saponification.
[0041] After completion of saponification, the obtained slurry is subjected to solid-liquid separation by a known method, and methyl acetate and methanol are separated. The mixture is washed with water or the like, and if necessary, stranded and then pelletized, and dried to obtain the product of the present invention. Polyvinyl alcohol having structural units represented by general formula (1) and / or general formula (2) A copolymer resin is obtained. In addition, when an alkaline catalyst is used, the alkaline catalyst is neutralized with an acid such as acetic acid after saponification. It is preferable that the alkali is neutralized to promote lactonization, and polyvinyl alcohol is obtained. The structural unit represented by the general formula (1) in the coal-based resin increases.
[0042] The polyvinyl chloride having the structural units represented by the general formula (1) and / or the general formula (2) of the present invention In order to use vinyl alcohol resins for various applications, different properties must be added to them. It may be mixed with other PVA-based resins. Such other PVA-based resins include those having different degrees of saponification, different degrees of polymerization, and modified Examples of the modified polysiloxane include those having different groups and those having different degrees of modification. For the purpose of adjusting the viscosity, unmodified PVA resin and ethylene-vinyl alcohol copolymer are used. may be mixed.
[0043] [Additives] The polyvinyl chloride having the structural units represented by the general formula (1) and / or the general formula (2) of the present invention In order to use the vinyl alcohol resin for various applications, it is necessary to , lubricants, inorganic salts (e.g. hydrotalcite, etc.), plasticizers (e.g. ethylene glycol, Aliphatic polyhydric alcohols such as glycerol and hexanediol), oxygen absorbents, heat stabilizers agents, light stabilizers, antioxidants, UV absorbers, colorants, antistatic agents, surfactants, antibacterial agents, Anti-blocking agents, slip agents, fillers (e.g. inorganic fillers, etc.), other resins (e.g. Polyolefin, polyamide, etc.) may be contained. EXAMPLES
[0044] The present invention will be described in more detail below with reference to examples and comparative examples. The present invention is not limited to the following examples. In the following examples and comparative examples, the units "parts" and "components" are used. "%" is by weight unless otherwise specified.
[0045] <Example 1> [Polymerization process] A reactor equipped with a stirrer, a thermometer, a reflux condenser, and a sample inlet was charged with 120 parts by mass of vinyl acetate, 60 parts by mass of methanol, distilled AOMA (manufactured by Nippon Shokubai Co., Ltd., 2-(allyloxymethyl) The reactor was immersed in a water bath to heat the water. The mixture was heated until the liquid boiled. 2,2'-azobisisobutyric acid was used as the radical initiator. 0.12 parts by mass of ethyl nitrile was added to the mixture to initiate polymerization. The mixed monomer of A and vinyl acetate was added dropwise at a rate of 10.5 parts by mass / hr. The monomer mixture was prepared in advance so that the weight ratio of AOMA to vinyl acetate was 6:94. After polymerization for 1.5 hours, heating was stopped and m- The polymerization was terminated by adding 0.03 parts by mass of dinitrobenzene and 200 parts by mass of methanol. The polymerization rate was 28%. In order to remove the methanol and vinyl acetate, the methanol and vinyl acetate were distilled off under reduced pressure. By adding methanol, the remaining vinyl acetate is expelled and the modified polyvinyl acetate is formed. A part of this methanol solution was collected and dried to obtain modified polyvinyl acetate (poly The resulting modified polyvinyl acetate was 1 1H-NMR measurement The modification rate was calculated by the above calculation, and the AOMA modification rate was found to be 1.6 mol%. The total amount of AOMA added before the start of polymerization and the amount of AOMA added dropwise during polymerization is the polymer. This is consistent with the modification rate (1.6 mol%) calculated assuming that all of the It can be said that almost all of the AOMA present in the complex was consumed. [Saponification process] Next, the methanol solution of the modified polyvinyl acetate was diluted with methanol until the concentration reached 8% by mass. The modified polyvinyl acetate methanol solution was diluted with 400 parts by mass (as modified polyvinyl acetate). The reactor was immersed in a water bath until the internal temperature reached 65°C. The mixture was heated to a temperature of 8.5°C. A 3.5% by mass solution of sodium hydroxide in methanol was added to the mixture. The saponification reaction was started by adding 5 parts by mass of ethyl alcohol. As the saponification reaction proceeded, the saponified product precipitated. Stirring was continued as it was. After the addition of the methanol solution of sodium hydroxide, the mixture was stirred for 1.5 hours. The precipitated saponification product was then filtered off and charged again into the reactor, where 240 mass of methanol was added. The mixture was heated to 65° C. and a 3.5% by mass solution of sodium hydroxide in methanol was added. The saponification reaction was completed by adding 8.5 parts by mass of ethanol and reacting for 2.5 hours. 0.36 parts by mass of acetic acid was added to neutralize the mixture, and the mixture was suction filtered while being washed with methanol. The saponification product was taken out, and 1000 mass of methanol was added to the saponification product and incubated at 65°C for 30 minutes. The saponified product was washed by stirring. After washing, the saponified product was taken out by suction filtration and then Dry in an air dryer at 50°C for 12 hours to obtain the AOMA-modified polyvinyl alcohol resin. I got fat.
[0046] <Example 2> In the polymerization step, the dropping rate was 10.7 parts by mass / hr. The weight ratio of AOMA to vinyl acetate was 8:92, and the polymerization time was 2 hours. The polymerization was stopped at 29%. The modified polyvinyl acetate obtained was of 1 The modification rate of AOMA was calculated by measuring H-NMR, and it was found to be 2.7 mol This value is the amount of AOMA charged before the start of polymerization and the amount of AOMA added dropwise during polymerization. The modification rate (2.7 moles) was calculated assuming that the total amount of %), indicating that the AOMA present in the polymerization system was almost completely consumed.
[0047] <Comparative Example 1> As a general-purpose polyvinyl alcohol resin, Gohsenol NL-05 (Mitsubishi Chemical Corporation) ) fully saponified polyvinyl alcohol, degree of polymerization: 500) was used.
[0048] <Comparative Example 2> [Polymerization process] A reactor equipped with a stirrer, a thermometer, a reflux condenser, and a sample inlet was charged with 100 parts by mass of vinyl acetate, 3.38 parts by mass of norbornene (molar ratio of vinyl acetate to norbornene: 97:3), The reactor was immersed in a water bath and the water bath was heated to bring the liquid inside to a boil. The mixture was heated until the reaction temperature reached 100°C. 0.0% 2,2'-azobisisobutyronitrile was used as a radical initiator. After polymerization for 5 hours, heating was stopped and polymerization was continued. Add 0.005 parts by mass of m-dinitrobenzene and 200 parts by mass of methanol as a terminator. The polymerization was terminated by adding 100% ethyl acetate. The polymerization rate was 33%. To remove the norbornene and 2-norbornene, methanol and vinyl acetate were distilled off under reduced pressure. When the viscosity increases, add methanol to remove the remaining vinyl acetate. The mixture was poured out to obtain a methanol solution of modified polyvinyl acetate. [Saponification process] The saponification step was carried out in the same manner as in Example 1 to obtain modified polyvinyl alcohol. The molar ratio of the 2-norbornene-derived units in the polymer was 2.1 mol %. The number of moles of AOMA in Examples 1 and 2 was less than that of 2-norbornene charged at the time of the reaction. It was found that a large amount of 2-norbornene remained at the end of the polymerization compared to when .
[0049] The polyvinyl ester polymers and polyvinyl The following measurements were performed on the alcohol-based resin and the polyvinyl alcohol-based resin used in Comparative Example 1. The results are shown in Table 1.
[0050] [Measurement method] <Measurement of polymerization rate> Approximately 1 to 2 g of the polymerized liquid sample in the reactor was weighed out into an aluminum cup and dried in a 140°C oven. After drying for 30 minutes at 40°C, the amount of the sample remaining in the aluminum cup was used to determine the resin fraction at the end of polymerization. The weight of the reacted monomer was calculated from the resin fraction measurement results, and the weight of the charged monomer was calculated. The polymerization rate was calculated by dividing the total weight of the monomer dropped and the amount of the monomer dropped.
[0051] <Modification rate of 2-(allyloxymethyl)methyl acrylate (AOMA) in polyvinyl acetate Measurements > The content of AOMA in polyvinyl acetate (AOMA modification rate) is 1 Measured by H-NMR The measurement was performed using a Bruker Ascend 400 instrument at a temperature of 23°C. The solvent is CDCl. 3 Tetramethylsilane was used as the internal standard. 3.3-4.3 ppm The peak is the methylene (CH 2 ) Two and the methyl of the ester group (CH 3 ) for a total of seven hydrogen atom peaks (for the above structural unit) Inside H a , the integral value a) in Figure 1, and the peaks at 4.6 ppm to 5.3 ppm are acetic acid. The peak of methine (CH) of the vinyl structural unit (H in the above structural unit) b , the product in Fig. 1 b) is the fractional value.
[0052] [ka]
[0053] <Measurement of modification rate of 2-norbornene modified PVOH> According to the method described in Patent Document JP 2008-202048, 1 Calculated from H-NMR Ta
[0054] <Measurement of average degree of polymerization> The average degree of polymerization was analyzed in accordance with JIS K 6726-1994.
[0055] <Melt point and glass transition point (Tg) measurement> Polyvinyl alcohol resin was measured using a differential scanning calorimeter (TA Instruments, "Q 2000"), 2 Flow rate 50ml / min, modulation amplitude 5℃ / min, modulation The cycle was 6 seconds, and the temperature was raised from -50°C to 260°C at 5°C / min, and then lowered to -5°C at 5°C / min. Cool to 0℃ and hold for 3 minutes, then heat again from -50℃ to 260℃ at 5℃ / min and measure. The glass transition temperature was determined from the reversing heat flow during the second heating process. The melting point was determined from the melting peak of total heat flow.
[0056] <Oxygen transmission rate (OTR) measurement> A 10% by weight aqueous solution of polyvinyl alcohol resin was prepared, and the surface of the polyvinyl alcohol resin was corona-treated. The dry thickness was measured using a bar coater on a polyethylene terephthalate film (thickness 38 μm). The coated film was dried (120°C x 5 minutes) to obtain a thickness of 3 μm. A polyvinyl alcohol resin film layer was formed on the PET film. The polyvinyl alcohol resin film layer was removed from the film. The oxygen transmission rate (OTR) of the layer was evaluated. Oxygen permeability (OTR, cc 3μm / m 2 ·day·atm) is at 23℃ and humidity 8 Under the condition of 0% RH, an oxygen permeability measuring device (MOCON "OX-TRAN") was used. The measurements were taken.
[0057] [Table 1]
[0058] The film using the polyvinyl alcohol resin of Example 1 was the same as the polyvinyl alcohol resin of Comparative Examples 1 and 2. It was found that the gas barrier properties were superior to those of polyvinyl alcohol-based resins. do. The film using the polyvinyl alcohol-based resin of Example 2 was the same as that using the polyvinyl alcohol-based resin of Comparative Example 1. It has better gas barrier properties than the case where an alcohol-based resin is used. It has the same gas barrier properties as the polyvinyl alcohol resin. However, the polyvinyl alcohol resin of Example 1 was similar to the polyvinyl alcohol resins of Comparative Examples 1 and 2. It can be seen that the melting point is lower and moldability is excellent compared to other resins.
[0059] In addition, in the production of the polyvinyl alcohol resins in Examples 1 and 2, Compared to polyvinyl alcohol resin production, the amount of copolymerization monomer remaining is small, resulting in superior productivity. It is clear that this is possible. [Industrial Applicability]
[0060] The polyvinyl alcohol resin of the present invention has excellent elasticity not only under dry conditions but also under high humidity conditions. Since the gas barrier properties are good even when the film is made of this resin, it is possible to prevent food contamination even when it is a single layer. As a packaging material for various products, pharmaceuticals, industrial chemicals, and agricultural chemicals It is also useful to laminate a single layer or two or more layers of other resin layers to form the PVA-based film of the present invention. When a laminate having at least one layer containing a resin is formed, the resin is easily oxidized under high humidity conditions. This prevents the deterioration of gas barrier properties and increases mechanical strength, so the quality of the product is not affected by oxygen. It is suitable as a packaging material for articles that may deteriorate. [Brief description of the drawings]
[0061] [Figure 1] 1 is a 1H-NMR chart of the polyvinyl ester polymer of Example 1.
Claims
1. Having a structural unit represented by the following general formula (1) and / or the following general formula (2): A polyvinyl alcohol resin characterized by the above. [Formula 1] [Case 2] (In the above formula (2), R 1 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .)
2. The structural units represented by the above general formula (1) and / or the above general formula (2) are incorporated into the resin.
2. The copolymer according to claim 1, wherein the content of the monomer unit is 0.1 to 30 mol % based on the total amount of the monomer unit. The polyvinyl alcohol resin is described above.
3. 2. The polyvinyl chloride according to claim 1, wherein the degree of saponification is 80 to 99.9 mol %. Alcohol-based resin.
4. 2. The polyvinyl acetate composition according to claim 1, wherein the average degree of polymerization is from 200 to 5,000. Alcohol-based resin.
5. A polyvinyl ester-based compound characterized by having a structural unit represented by the above general formula (2). Polymer.
6. The structural unit represented by the above general formula (2) is 6. The polyvinyl ester polymer according to claim 5, wherein the content is 0.1 to 30 mol %. body.
7. Claims having a structural unit represented by the above general formula (1) and / or the above general formula (2).
1. A method for producing the polyvinyl alcohol-based resin according to claim 1, comprising: The method is characterized by comprising a step of saponifying a polyvinyl ester polymer having a structural unit. A method for producing a polyvinyl alcohol resin.
8. The polyvinyl ester polymer according to claim 5, which has a structural unit represented by the general formula (2). The present invention relates to a method for producing a copolymer, the method comprising the steps of: A process for producing a polyvinyl ester polymer, comprising a step of radically polymerizing a Construction method. [C3] (In the above formula (3), R 2 is a metal atom, a hydrogen atom, or an alkyl group having 1 to 6 carbon atoms. .)
9. A vinyl ester monomer and a compound represented by the above general formula (3) are radically polymerized. In the step, a solution containing the compound represented by the general formula (3) is continuously added dropwise. The method for producing a polyvinyl ester polymer according to claim 8,
Citation Information
Patent Citations
Production of vinyl ester polymer and production of vinyl alcohol polymer
JP1992227904A
Diene-based carboxylate anion and salt thereof, and polymerizable or curable composition thereof
JP2012107208A
Carboxylic acid polymer composition
JP2014181252A
Diene carboxylic acid anion and salt thereof and polymer thereof or curable composition
JP2016166233A
Method for manufacturing modified resin
JP2020050832A
Cited By
Polymer, production method therefor, and composition, aqueous solution, molded body, and packaging containing polymer.