Method for manufacturing composite body
The use of polyamide resin foam with controlled moisture content and a thermosetting resin layer addresses curing failures and molding shrinkage issues, enhancing productivity and mechanical strength in composite production.
Patent Information
- Application Number
- JP2023049654
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Existing methods for manufacturing composite molded products face challenges in balancing productivity with the prevention of molding shrinkage and curing failures due to exothermic reactions in thermosetting resin foam pieces, leading to prolonged molding cycles and decreased productivity.
A method involving the use of a core material composed of polyamide resin foam with a moisture content of 0.1 to 5% and a closed cell ratio of 80% or more, combined with a thermosetting resin layer, to suppress curing failures and maintain mechanical strength.
The method enables the production of composites with enhanced productivity by preventing curing defects and cell destruction, while maintaining excellent bending strength and shortening the molding cycle.
Smart Images

Figure 2024138927000001 
Figure 2024138927000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a composite and a core material used in the method. [Background technology]
[0002] 2. Description of the Related Art Composites of thermosetting resins and foams obtained by foaming resins are lightweight and have mechanical strength, and are therefore used in a variety of applications.
[0003] For example, Patent Document 1 describes a method for producing a composite molded product of a foamed small piece molded product obtained by molding a thermoplastic resin foamed small piece and a cured thermosetting resin, with the objective of providing a method for producing a composite molded product that is lightweight and has high compressive strength and bending strength, and is characterized by including the steps of placing a foamed small piece molded product having interconnected voids and a porosity within a specific range in a mold having a sealable internal space of a predetermined shape, sealing and reducing the pressure in the internal space, introducing a thermosetting resin liquid raw material into the reduced pressure internal space and impregnating the liquid raw material into the voids of the foamed small piece molded product, and curing the liquid raw material.
[0004] Patent Document 2, which aims to provide a composite molded body that is lightweight and has high bending strength, describes a composite molded body made of a plurality of resin foam pieces and a cured thermosetting resin, in which a cured thermosetting resin is formed between the resin foam pieces, the cured thermosetting resin constituting the composite molded body has a porosity in a specific range, and the bending elastic modulus E (MPa) and density ρ (kg / m 3 ) satisfies a specific formula. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2014-193539 A [Patent Document 2] JP 2015-17190 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, when the composite molded body described in Patent Documents 1 and 2 is laminated with a thermosetting resin on a resin foam piece, if an attempt is made to shorten the molding cycle in consideration of productivity, molding shrinkage may easily occur depending on the type of resin of the resin foam piece due to the exothermic curing reaction of the thermosetting resin. On the other hand, if an attempt is made to suppress the heat generated by the curing reaction in order to prevent molding shrinkage, there is a problem that the molding cycle of the composite molded body becomes longer, resulting in a decrease in productivity.
[0007] Furthermore, in a casting process in which a liquid thermosetting resin material is filled into a mold for molding, depending on the type of resin in the foamed resin pieces, the liquid thermosetting resin material may not cure properly.
[0008] The problem to be solved by the present invention is to provide a method for producing a composite material which is excellent in productivity and capable of suppressing curing defects, and a core material used in the production method. [Means for solving the problem]
[0009] The inventors have discovered that the above-mentioned problems can be solved by using a core material that is made of a polyamide-based resin foam and has a moisture content within a specific range in a method for manufacturing a composite having a core material and a thermosetting resin layer provided on at least a portion of the surface of the core material. That is, the present invention is as follows. <1> A method for producing a composite having a core material and a thermosetting resin layer provided on at least a portion of the surface of the core material, the method comprising the steps of: placing a core material made of a polyamide resin foam and having a moisture content of 0.1 to 5 mass % in a molding die; filling the molding die with a thermosetting resin liquid raw material; and curing the thermosetting resin liquid raw material to form a thermosetting resin layer on at least a portion of the surface of the core material. <2> The method for manufacturing a composite according to <1>, wherein the thermosetting resin layer contains a reinforcing fiber sheet material. <3> The method for manufacturing a composite according to <1> or <2>, wherein the closed cell ratio of the polyamide-based resin foam is 80% or more. <4> The method for manufacturing a composite according to any one of <1> to <3>, wherein the melting point of the polyamide-based resin constituting the polyamide-based resin foam is 160 to 285°C. <5> The method for manufacturing a composite according to any one of <1> to <4>, wherein the core material is composed of composite particles in which reinforcing fibers are adhered to the surface of particulate polyamide-based resin foam via an uncured thermosetting resin. <6> A core material used in the method for manufacturing a composite according to any one of <1> to <5>, wherein the core material is composed of a polyamide-based resin foam, and the moisture content of the core material is 0.1 to 5% by mass.
Advantages of the Invention
[0010] According to the present invention, it is possible to provide a method for manufacturing a composite excellent in productivity and capable of suppressing curing defects, and a core material used in the manufacturing method.
Embodiments for Carrying Out the Invention
[0011] Hereinafter, the present invention will be described in detail. In this specification, the term "A to B" regarding the description of numerical values means "A or more and B or less" (when A < B) or "A or less and B or more" (when A > B). In the present invention, a combination of preferred embodiments is a more preferred embodiment.
[0012] [Method for Manufacturing a Composite] The method for producing a composite of the present invention (hereinafter also simply referred to as "the method for producing a composite") is a method for producing a composite having a core material and a thermosetting resin layer provided on at least a portion of the surface of the core material, in which the core material (hereinafter also simply referred to as "core material") made of polyamide resin foam (hereinafter also simply referred to as "foam") and having a moisture content of 0.1 to 5 mass % is placed in a molding die, and then a thermosetting resin liquid raw material is filled into the molding die and the thermosetting resin liquid raw material is cured to form a thermosetting resin layer on at least a portion of the surface of the core material.
[0013] The method for producing the composite of the present invention includes at least the following steps. Step (A): A step of placing a core material made of a polyamide-based resin foam and having a moisture content of 0.1 to 5% by mass in a molding die; Step (B): filling a liquid thermosetting resin raw material into a mold; Step (C): A step of curing the thermosetting resin liquid raw material to form a thermosetting resin layer on at least a portion of the surface of the core material.
[0014] <Core material> The core material is made of a polyamide-based resin foam, which is formed by foaming a polyamide-based resin as a base resin. The moisture content of the core material is 0.1 to 5% by mass from the viewpoint of suppressing poor curing of the thermosetting resin liquid raw material constituting the thermosetting resin layer and obtaining a composite having excellent mechanical strength, particularly bending strength. From the above viewpoint, the moisture content of the core material is preferably 0.3 to 4.7% by mass, more preferably 0.5 to 4.5% by mass. A core material having a moisture content in the above range is suitably used for producing a composite. The moisture content of the core material can be adjusted by a drying step in which a polyamide resin foam is dried when producing the polyamide resin foam. The moisture content of the core material can be measured by heating the polyamide resin foam to a temperature of 235°C using a thermal moisture vaporizer to vaporize the moisture inside the foam, and then guiding the resulting moisture to a Karl Fischer moisture meter (e.g., "CA-200" manufactured by Mitsubishi Chemical Analytech Co., Ltd.) connected to the thermal moisture vaporizer.
[0015] The reason why the core material is made of a polyamide-based resin foam and has a moisture content within a specific range can suppress poor curing of the thermosetting resin liquid raw material that constitutes the thermosetting resin layer is not clear, but it is presumed as follows. The core material is made of a polyamide-based resin foam, and the destruction of the cell structure of the foam that forms the core material, which is caused by the exothermic reaction of the thermosetting resin, can be suppressed. As a result, it is not necessary to gradually progress the exothermic reaction of the thermosetting resin, and it is considered that the molding cycle of the composite molded body is not lengthened and the productivity is not reduced. In addition, in cast molding, particularly when cast molding is performed under reduced pressure using a core material made of a polyamide-based resin foam, there is a tendency for poor curing (dry spots) to occur, but it is considered that by setting the moisture content of the core material within a specific range, poor curing of the thermosetting resin liquid raw material can be suppressed.
[0016] (Polyamide resin foam) The polyamide resin foam of the present invention contains a polyamide resin as a base resin. Examples of polyamide resins that serve as the base resin for the polyamide resin foam include polyamides and polyamide copolymers, with polyamide copolymers being preferred. Polyamides include, for example, poly(6-aminohexanoic acid), also known as poly(caprolactam) (polycaproamide, nylon 6), poly(laurolactam) (nylon 12), poly(hexamethylene adipamide) (nylon 66), poly(7-aminoheptanoic acid) (nylon 7), poly(8-aminooctanoic acid) (nylon 8), poly(9-aminononanoic acid) (nylon 9), poly(10-aminodecanoic acid) (nylon 10), poly(11-aminounsodium EDTA) (nylon 11), poly(12-aminobutanoic acid) (nylon 12), poly(1 ... Examples of homopolymers include poly(hexamethylene sebacamide) (nylon 11), poly(hexamethylene sebacamide) (nylon 610), poly(decamethylene sebacamide) (nylon 1010), poly(hexamethylene azelamide) (nylon 69), poly(tetramethylene adipamide) (nylon 46), poly(tetramethylene sebacamide) (nylon 410), poly(pentamethylene adipamide) (nylon 56), and poly(pentamethylene sebacamide) (nylon 510). The term "polyamide copolymer" refers to a copolymer having two or more repeating units, and at least a part of each repeating unit has an amide bond. Examples of polyamide copolymers include polycaproamide / polyhexamethylene adipamide copolymer (nylon 6 / 66), caprolactam / hexamethylenediaminoadipic acid / lauryl lactam (nylon 6 / 66 / 12), and caprolactam / lauryl lactam copolymer (nylon 6 / 12). The polyamide resin may be one of these polyamides and polyamide copolymers, or two or more of them may be combined. Among the above polyamide resins, it is preferable to use a polyamide resin that is a combination of one or more of nylon 6, nylon 66, nylon 6 / 66, and nylon 6 / 66 / 12, and more preferably one or two of nylon 6 / 66 and nylon 6 / 66 / 12. In addition, polyamides and polyamide copolymers incorporating plant-derived raw materials can also be used as the polyamide resins. Polyamide resins are generally hygroscopic, and when placed in water at 23°C in a solid state, their saturated water absorption rate is higher the fewer the number of carbon atoms per amide group in the repeating unit, with nylon 6 having a saturated water absorption rate of about 11.5%, and nylon 66 having a saturated water absorption rate of about 9.5%.
[0017] The polyamide copolymer may be a block copolymer in which a certain amount of amides of the same repeating unit are followed by a certain amount of amides of different types, or a random copolymer in which different types of amides are randomly repeated, but is preferably a random copolymer. If the polyamide copolymer is a random copolymer, it becomes possible to mold the expanded beads at a relatively low molding pressure when molding them in a mold.
[0018] The melting point of the polyamide resin constituting the polyamide resin foam is preferably 160 to 285° C., more preferably 170 to 240° C., and even more preferably 175 to 200° C., from the viewpoint of improving the heat resistance of the composite and facilitating temperature control during foaming. In addition, when the melting point is within the above range, the composite can withstand the exothermic curing reaction of the thermosetting resin during molding. The melting point of the polyamide resin constituting the polyamide resin foam is the value obtained as the peak apex temperature of the melting peak of the DSC curve obtained at a heating rate of 10°C / min by heat flux differential scanning calorimetry, using "the case where the melting temperature is measured after a certain heat treatment" (the heating rate and cooling rate in the condition adjustment of the test piece are both 10°C / min) as the condition adjustment of the test piece based on JIS K 7121:1987. When the DSC curve has multiple melting peaks, the peak apex temperature of the melting peak with the largest area is adopted as the melting temperature. Note that the polyamide resin test piece can be stored, for example, in a desiccator and then vacuum-suctioned to prevent hydrolysis under high temperature and high humidity conditions. In addition, when the polyamide resin is a mixture of two or more polyamide resins, or a mixture of a polyamide resin and another thermoplastic resin, the mixture can be used as the test piece.
[0019] The base resin may contain other thermoplastic resins in addition to the polyamide resin, so long as the purpose and effect of the present invention are not impaired. Examples of other thermoplastic resins include polyethylene resins, polypropylene resins, polystyrene resins, vinyl acetate resins, thermoplastic polyester resins, acrylic acid ester resins, methacrylic acid ester resins, modified polyphenylene ether resins, polycarbonate resins, polyacetal resins, polybutylene terephthalate resins, polysulfone resins, polyethersulfone resins, polyamideimide resins, polyetherimide resins, and polyetheretherketone resins. From the viewpoint of obtaining a composite having excellent lightness and mechanical strength, the content of thermoplastic resin other than polyamide-based resin in the base resin is preferably 10% by mass or less, more preferably 5% by mass or less, and even more preferably 3% by mass or less. It is particularly preferable that the base resin consists of only polyamide-based resin.
[0020] The base resin constituting the polyamide resin foam may be appropriately blended with various additives, such as commonly used antistatic agents, conductivity imparting agents, lubricants, ultraviolet absorbers, flame retardants, metal deactivators, crystal nucleating agents, colorants, and fillers, as necessary. The amount of each of these additives to be added varies depending on the purpose of use of the composite, but is preferably 25 parts by mass or less, more preferably 15 parts by mass or less, even more preferably 10 parts by mass or less, and even more preferably 5 parts by mass or less, relative to 100 parts by mass of the base resin constituting the polyamide resin foam.
[0021] <Closed bubble rate> From the viewpoint of maintaining the light weight of the composite, the closed cell ratio of the polyamide-based resin foam is preferably 80% or more, more preferably 85% or more, and even more preferably 90% or more. The closed cell ratio of a polyamide resin foam is the ratio of the volume of closed cells to the volume of all cells in the foam, and can be determined using an air comparison type specific gravity meter in accordance with ASTM-D2856-70.
[0022] Examples of the polyamide-based resin foam constituting the core material include expanded beads or expanded bead groups which are particulate foams, extruded foams obtained by extrusion, expanded bead moldings obtained by molding the expanded beads in a mold, etc. Among these, expanded bead moldings are preferred because they can form any core material according to the shape of the composite molding.
[0023] <<Appearance of honey>> The apparent density of the polyamide-based resin foam is preferably 10 kg / m from the viewpoint of easily obtaining a composite having excellent light weight and mechanical strength. 3 More preferably, 20 kg / m 3 More preferably, 30 kg / m 3 More preferably, 40 kg / m 3 and preferably 200 kg / m 3 Less than or equal to 150 kg / m 3 More preferably, 100 kg / m or less 3 More preferably, 75 kg / m or less 3 The following is the result. The apparent density of the polyamide foam can be measured by external dimensions or by a submersion method. When the polyamide-based resin foam is in the form of foamed particles, the apparent density is measured by the following method (submersion method). When left for 24 hours or more under conditions of 50% relative humidity, 23°C, and 1 atm, the volume is approximately 500 cm 3 The mass W1 of the foamed beads is measured, a measuring cylinder containing water at a temperature of 23°C is prepared, and the foamed beads of mass W1 are submerged in the measuring cylinder using a wire net. Taking into account the volume of the wire net, the volume V1 [cm2] of the foamed beads is read from the rise in the water level. 3 ] and divide the mass W1 [g] of the expanded beads by the volume V1 (W1 / V1) to obtain the apparent density [g / cm 3 ] is required.
[0024] The polyamide-based resin foam constituting the core material is not particularly limited as long as it is obtained by foaming the above-mentioned base resin, but it may be composed of composite particles in which reinforcing fibers are attached to the surface of particulate polyamide-based resin foam (polyamide-based expanded particles) obtained by foaming the above-mentioned base resin via an uncured thermosetting resin.
[0025] Examples of the thermosetting resin in the composite particles include unsaturated polyester resins, epoxy resins, vinyl ester resins, phenol resins, polyamide resins, urea resins, melamine resins, polyimide resins, diallyl phthalate resins, urethane resins, etc. Among these, the thermosetting resin is preferably one or more types selected from the group consisting of unsaturated polyester resins and epoxy resins, and more preferably one or more types selected from epoxy resins, from the viewpoint of excellent adhesion to the base resin constituting the polyamide resin foam.
[0026] The unsaturated polyester resin is preferably an unsaturated polyester resin obtained by dissolving a condensation product obtained from an unsaturated polycarboxylic acid and a polyhydric alcohol in a vinyl monomer. Examples of the unsaturated polycarboxylic acid include maleic anhydride, fumaric acid, adipic acid, phthalic anhydride, and isophthalic acid. Examples of the polyhydric alcohol include ethylene glycol, 1,3-butylene glycol, diethylene glycol, and propylene glycol. Examples of the vinyl monomer include styrene monomers.
[0027] Examples of epoxy resins include bisphenol type epoxy resins such as bisphenol A type epoxy resins, bisphenol F type epoxy resins, and bisphenol S type epoxy resins; novolac type epoxy resins such as phenol novolac type epoxy resins and cresol novolac type epoxy resins; alicyclic epoxy resins; glycidyl ether type epoxy resins; glycidylated amine type epoxy resins; halogenated epoxy resins; and addition polymers of epoxy group-containing monomers or oligomers such as glycidylated polyesters, glycidylated polyurethanes, and glycidylated acrylics.
[0028] Examples of reinforcing fibers in the composite particles include glass fibers, carbon fibers, vinylon fibers, polyester fibers, ceramic fibers, steel fibers, stainless steel (SUS) fibers, aluminum fibers, boron fibers, etc. Among these, from the viewpoints of high strength, versatility, economy, etc., one or more types selected from the group consisting of glass fibers, carbon fibers, and vinylon fibers are preferred, and one or more types selected from the group consisting of glass fibers and carbon fibers are more preferred.
[0029] The composite particles preferably contain a curing agent capable of reacting with the thermosetting resin to produce a cured product. The curing agent is not particularly limited as long as it can react with the thermosetting resin to produce a cured product. When an unsaturated polyester resin is used as the thermosetting resin, it is preferable to use a peroxide as a curing agent (polymerization initiator). As the peroxide, organic peroxides such as benzoyl peroxide, lauroyl peroxide, methyl ethyl ketone peroxide, peroxy perbenzoate, peroxy ketal, dicumyl peroxide, etc. are preferably used. These peroxides are used alone or as a mixture of two or more. In addition to the peroxide, a chain transfer agent may be used. Examples of the curing agent for the epoxy resin include acid anhydrides such as methylhexahydrophthalic anhydride, phenolic resins such as novolac type phenolic resins and cresol novolac type epoxy resins, phthalic anhydride derivatives, dicyandiamide, amine compounds, imidazole compounds, aluminum chelates, and amine complexes of Lewis acids such as BF3. These are used alone or as a mixture of two or more.
[0030] The composite particles can be produced, for example, by the following method. The expanded polyamide resin particles obtained by expanding the base resin are mixed with a thermosetting resin and a curing agent by stirring or the like to prepare a thermosetting resin dispersion in which the thermosetting resin and the curing agent are uniformly dispersed. The expanded polyamide resin particles are mixed with the thermosetting resin dispersion, and reinforcing fibers are further added and mixed to obtain the composite particles.
[0031] <Thermosetting resin layer> The thermosetting resin layer is provided on at least a part of the surface side of the core material. The thermosetting resin layer is formed by curing a liquid thermosetting resin raw material, and is made of a cured product of the thermosetting resin. The thickness of the thermosetting resin layer can be appropriately set, but from the viewpoint of achieving both light weight and strength, it is preferably 0.5 to 20 mm, and more preferably 1 to 10 mm.
[0032] As the thermosetting resin, those exemplified as the thermosetting resin in the composite particles described above can be used. Among these, the thermosetting resin is preferably one or more selected from the group consisting of unsaturated polyester resins and epoxy resins, and more preferably one or more selected from unsaturated polyester resins. As the thermosetting resin, commercially available products may be used, and examples of the unsaturated polyester resin include those manufactured by Nippon U-PICA Co., Ltd. under the trade names "4015", "4072", "5116", and "5126". Examples of the epoxy resin include those manufactured by DIC Corporation under the trade name "EPICLON".
[0033] The thermosetting resin layer preferably contains a curing agent capable of reacting with the thermosetting resin to produce a cured product. The curing agent is not particularly limited as long as it reacts with the thermosetting resin to harden and produce a cured product of the thermosetting resin, and the curing agent may be any of the curing agents exemplified above that can react with the thermosetting resin in the composite particles to produce a cured product.
[0034] The thermosetting resin layer preferably includes a reinforcing fiber sheet material. The reinforcing fiber sheet material is a sheet of reinforcing fibers. As the reinforcing fibers constituting the reinforcing fiber sheet material, those exemplified as the reinforcing fibers in the composite particles can be used. Among these, from the viewpoints of high strength, versatility, economic efficiency, etc., one or more types selected from the group consisting of glass fiber, carbon fiber, and vinylon fiber are preferred, and one or more types selected from the group consisting of glass fiber and carbon fiber are more preferred. The thickness of the reinforcing fiber sheet material can be appropriately changed depending on the intended use of the composite, but can be about 1 to 3 mm.
[0035] <Process (A)> The method for producing a composite of the present invention includes a step of placing a core material composed of the polyamide resin foam in a molding die.
[0036] The method for placing the core material composed of the polyamide-based resin foam in the mold is not particularly limited, and it can be placed in a desired position in the mold by a conventionally known method.
[0037] The molding die is not particularly limited as long as it can be filled with a thermosetting resin liquid raw material after placing a core material composed of a polyamide-based resin foam. For example, a molding die composed of a lower die and an upper die, which together form a molding space, can be used.
[0038] When the thermosetting resin layer includes a reinforcing fiber sheet material, the reinforcing fiber sheet material can be placed in the mold in step (A). For example, when the reinforcing fiber sheet material of the thermosetting resin layer is placed in a part of the core material made of a polyamide-based resin foam, the core material with the reinforcing fiber sheet material placed at a desired position can be placed in the mold, or the core material can be placed in the mold after the reinforcing fiber sheet material is placed at a desired position in the mold. When the reinforcing fiber sheet material of the thermosetting resin layer is placed around the entire periphery of the core material made of a polyamide-based resin foam, the entire periphery of the core material can be covered with the reinforcing fiber sheet material and placed in the mold. In addition, when a mold consisting of a lower mold and an upper mold is used, the reinforcing fiber sheet material is placed on the lower mold, the core material is placed on the reinforcing fiber sheet material, and the reinforcing fiber sheet material is further placed on the core material, and the lower mold and the upper mold are moved relative to each other so that the reinforcing fiber sheet material on the core material comes into contact with the upper mold, and the lower mold and the upper mold are closed, whereby the reinforcing fiber sheet material and the core material can be placed in the mold.
[0039] <Process (B)> The method for producing a composite of the present invention includes a step of filling a liquid thermosetting resin raw material into a mold, that is, a step of filling a liquid thermosetting resin raw material into a mold in which a core material made of a polyamide-based resin foam is placed.
[0040] The method for filling the mold with the thermosetting resin liquid raw material is not particularly limited, but from the viewpoint of improving the adhesion between the core material and the reinforcing fiber sheet material and from the viewpoint of not leaving air in the composite, it is preferable to reduce the pressure inside the mold and fill the mold with the thermosetting resin liquid raw material so that the thermosetting resin liquid raw material does not remain. The method for reducing the pressure inside the mold is not particularly limited, and examples include a method of reducing the pressure by suction with a vacuum pump. In addition, when the pressure is reduced during molding and the thermosetting resin liquid raw material is filled, particularly when a polyamide-based resin foam is used as the core material, there is a tendency for poor curing to occur. If such poor curing occurs, there is a risk of the strength of the composite being locally reduced. In the present invention, it has been found that this poor curing is related to the reduced pressure suction during filling and the moisture content of the polyamide-based resin foam, and is caused by moisture concentration at the reduced pressure suction port, and can be solved by using a polyamide-based resin foam with a specific moisture content as the core material.
[0041] <Process (C)> The method for producing a composite of the present invention includes a step of curing a thermosetting resin liquid raw material to form a thermosetting resin layer on at least a portion of the surface of a core material, i.e., a step of curing a thermosetting resin liquid raw material filled in a mold in which a core material made of a polyamide-based resin foam is placed, to form a thermosetting resin layer on at least a portion of the surface of the core material.
[0042] The method for curing the thermosetting resin liquid raw material is not particularly limited, and the thermosetting resin liquid raw material can be cured by heating or a curing reaction using a conventionally known method. The thermosetting resin liquid raw material preferably contains a curing agent that can react with the thermosetting resin to produce a cured product. The curing agent is not particularly limited as long as it can react with the thermosetting resin to cure and produce a cured product of the thermosetting resin, and the curing agents exemplified as curing agents that can react with the thermosetting resin in the composite particles to produce a cured product can be used.
[0043] The thermosetting resin liquid raw material hardens during or after filling the mold with the thermosetting resin liquid raw material, forming a thermosetting resin layer. When the mold is filled with the thermosetting resin liquid raw material under reduced pressure, the thermosetting resin liquid raw material tends to harden easily after the reduced pressure in the mold is released.
[0044] When the core material is composed of a composite particle molded body in which reinforcing fibers are attached to the surface of the expanded polyamide resin particles via an uncured thermosetting resin, the uncured thermosetting resin present on the surface of the expanded polyamide resin particles is also cured in step (C). When the core material is composed of the composite particle molded body, the reinforcing fibers are also present around the expanded polyamide resin particles, resulting in superior mechanical strength. EXAMPLES
[0045] The present invention will be described in detail below with reference to examples, but the present invention is not limited thereto.
[0046] The polyamide resin, expanded particles, composite particles, core material, and composites in the examples and comparative examples were measured and evaluated by the following methods.
[0047] [Measurement and Evaluation] <Melting point of polyamide resin> The melting point of the polyamide resin constituting the expanded beads was measured by heat flux differential scanning calorimetry based on JIS K 7121:1987. Under the condition of a nitrogen inflow rate of 30 mL / min, the resin was heated and melted from 30°C to a temperature 30°C higher than the end of the melting peak at a heating rate of 10°C / min (first temperature rise), then held at that temperature for 10 minutes, cooled to 30°C at a cooling rate of 10°C / min, and heated and melted again at a heating rate of 10°C / min to a temperature 30°C higher than the end of the melting peak. The melting point was determined as the peak apex temperature of the melting peak of the second DSC curve. Note that a high-sensitivity differential scanning calorimeter "EXSTAR DSC7020" (manufactured by SII Nano Technology Co., Ltd.) was used as the measuring device. The resin used as the test piece was placed in a desiccator in a nitrogen atmosphere to avoid high temperature and high humidity conditions and to prevent hydrolysis, and then vacuumed to a moisture content of 1000 mass ppm or less and stored for 24 hours before the melting point was measured. When a DSC curve has multiple melting peaks, the peak apex temperature of the melting peak with the largest area was used as the melting point.
[0048] <Moisture content of expanded particles, composite particles and core material> The moisture content of the expanded beads, composite particles, and core material was measured by heating the polyamide resin foam to a temperature of 235°C using a heating moisture vaporizer to vaporize the moisture inside the expanded beads, composite particles, and core material, and then guiding the resulting moisture to a Karl Fischer moisture meter ("CA-200" manufactured by Mitsubishi Chemical Analytech Co., Ltd.) connected to the heating moisture vaporizer.
[0049] <Apparent density of polyamide resin foam> The apparent density of the expanded polyamide resin particles and the composite particles obtained using the same was determined as follows. The bulk volume of the expanded polyamide resin particles was approximately 500 cm3 after being left for 24 hours or more under the conditions of 50% relative humidity, 23°C, and 1 atm. 3 The mass W1 of the particle was measured, a measuring cylinder containing water at a temperature of 23°C was prepared, and the particle of mass W1 was submerged in the measuring cylinder using a wire net. Taking into account the volume of the wire net, the volume V1 [cm 3] and divide the particle mass W1 [g] by the volume V1 (W1 / V1) to obtain the apparent density [g / cm 3 ] was requested.
[0050] <Closed cell ratio of polyamide resin expanded particles, composite particles and core material> The closed cell ratio of the polyamide resin foamed particles, composite particles, and core material was measured by the following method. According to procedure C described in ASTM-D2856-70, the true volume Vx of a sample consisting of the polyamide resin foamed particles, composite particles, or core material (the sum of the volume of the resin constituting the composite particles or core material and the total volume of the bubbles in the closed cell part in the sample) was measured. To measure this true volume Vx, an air comparison specific gravity meter "930" manufactured by Toshiba Beckman Co., Ltd. was used. Next, the closed cell ratio was calculated by the following formula (1), and the arithmetic average of the five measurement results was obtained. Closed cell ratio (%)=(Vx-W / ρ)×100 / (Va-W / ρ) (1) Vx: The true volume (cm) of the sample measured by the above method 3 ) Va: Apparent volume of the sample (cm 3 ) W: Mass of the measurement sample (g) ρ: Density of the resin that constitutes the sample (g / cm 3 )
[0051] <Core density> The density of the core material was determined by measuring the mass and volume of three core materials, calculating the apparent density, and taking the arithmetic average value thereof.
[0052] <Porosity of core material> The porosity of the core material was measured by the following method. A rectangular parallelepiped test piece cut from the center of the core material was submerged in a graduated cylinder containing ethanol, and the true volume Vc [L] of the test piece was calculated from the rise in the ethanol liquid level. In addition, the apparent volume Vd [L] was calculated from the outer dimensions of the test piece (length 25 mm × width 25 mm × height 100 mm). The porosity of the core material was calculated from the calculated true volume Vc and apparent volume Vd using the following formula (2). Porosity (%)=[(Vd-Vc) / Vd]×100 (2)
[0053] <Surface thickness of thermosetting resin layer> The surface thickness of the thermosetting resin layer was measured by the following method: the obtained composite was cut perpendicularly to the longitudinal direction at three locations, and the thermosetting resin layer was measured at six locations equally spaced along the circumferential direction on each cut surface, and the arithmetic average value of the thicknesses obtained at 18 locations was taken as the surface thickness of the thermosetting resin layer.
[0054] <Complex cycle time> The time required from placing the core material in the mold until the composite having a thermosetting resin layer formed on the surface of the core material was removed from the mold was measured and defined as the cycle time of the composite.
[0055] <Whether or not the cells of the core material in the composite are destroyed> The presence or absence of destruction of the cells of the core material in the composite was examined by cutting out five test pieces, each measuring 100 mm x 100 mm x the thickness of the part excluding the thermosetting resin layer part, from a total of five places, namely the center and the four corners (excluding the R part), of the molded composite, so as not to include the thermosetting resin layer. The state of the particles on any of the cut surfaces of the cut-out foamed beads was observed by visual observation, and the number of particles with destroyed bubbles in the foamed beads was counted. The ratio of the number of foamed beads with destroyed bubbles to the number of all foamed beads on the cut surface was calculated, and the lowest value among the values obtained from the five test pieces was taken as the destruction rate of the foamed beads, and the destruction of the cells of the core material in the composite was evaluated according to the following criteria. A: The destruction rate of foam particles is less than 50%. B: The destruction rate of the foam particles is 50% or more.
[0056] <Whether or not dry spots form in the complex> The presence or absence of dry spots, which are voids caused by insufficient curing of the composite, was confirmed by visual inspection.
[0057] <Bending properties of composite> The composite was measured for 1.0 mm deflection bending load and maximum yield point load in accordance with JIS K 7171:2006, specifically by the following method. First, a test piece of width 50 mm × length 400 mm × thickness 300 mm was cut out from each composite. When the thickness of the test piece was less than the above range, the test piece was used as it was. The cut test piece was left in a constant room at room temperature of 23 ° C. and humidity of 50% for 24 hours or more, and then the deflection-bending load curve (SS curve) was measured using a tabletop precision universal testing machine "Autograph AGS-10kNG" manufactured by Shimadzu Corporation under the conditions of a support distance of 300 mm, a radius R of the indenter of 5.0 mm, a radius R of the support table of 2.0 mm, a test speed of 5 mm / min, a room temperature of 23 ° C., and a humidity of 50%. The load at the deflection amount of 1.0 mm (1.0 mm deflection load (N)) of the SS curve was measured, and the average value of the measured values of 5 or more points was adopted as the measurement result, and the following criteria were used for evaluation. A: 1.0mm deflection load (N) is 170N or more B: 1.0mm deflection load (N) is less than 170N
[0058] [Raw materials] The materials used for the composite are shown below. <Expanded particles> PA1: Polyamide resin foam particles ·PA2: Polyamide resin foam particles PA3: Polyamide resin foam particles PA4: Polyamide resin foam particles PLA1: Polylactic acid foam particles <Thermosetting resin> Thermosetting resin A: "EPICLON850" manufactured by DIC Corporation Thermosetting resin 1: Product name "4072PT-3" manufactured by Japan U-Pica Corporation <Hardening agent> Hardener A: 1,3-bisaminomethylcyclohexane Hardener B: 2-ethyl-4-methylimidazole Hardener 1: NOF Corporation's product name "Percure AH" Hardener 2: NOF Corporation's product name "Percure HB" <Reinforced fiber> Reinforced fiber: Glass reinforced fiber, milled fiber manufactured by Central Glass Co., Ltd., product name "EFK80-31 / T" Reinforced fiber sheet 1: Glass fiber sheet, manufactured by GRP Japan Co., Ltd., product name "Combiflow S450 / V250 / S450" Reinforced fiber sheet 2: Glass fiber sheet, manufactured by SHINDO Co., Ltd., product name "NCF Q880G"
[0059] Manufacturing Examples 1 to 5 The thermosetting resin and the curing agent shown in Table 1 were mixed by stirring to obtain a thermosetting resin dispersion. The expanded particles and the thermosetting resin dispersion shown in Table 1 were mixed. Furthermore, the reinforcing fibers shown in Table 1 were added and mixed to obtain composite particles. The measurement results of the composite particles are shown in Table 1.
[0060] [Table 1]
[0061] Examples 1 to 3, Comparative Example 1, and Reference Examples 1 to 2 The composite particles shown in Table 2 were molded at the compression ratio and molding temperature shown in Table 2 to obtain a core material having a length of 450 mm, a width of 300 mm, and a thickness of 27 mm and a moisture content shown in Table 2. The thermosetting resin and curing agent shown in Table 2 were mixed by stirring to obtain a thermosetting resin liquid raw material. A composite was formed by using a mold consisting of an upper mold and a lower mold, with the dimensions of the molding space formed by the upper mold and the lower mold being 460 mm long, 310 mm wide, and 30 mm thick. Specifically, a reinforcing fiber sheet 1 was placed in the lower mold, a reinforcing fiber sheet 2 was placed on the reinforcing fiber sheet 1, the core material was placed on the reinforcing fiber sheet 2, the reinforcing fiber sheet 2 was further placed on the core material, and the reinforcing fiber sheet 1 was placed on the reinforcing fiber sheet 2, and the lower mold and the upper mold were moved relative to each other so that the reinforcing fiber sheet 1 and the upper mold were in contact with each other, and the lower mold and the upper mold were closed, thereby placing the reinforcing fiber sheet materials 1 and 2 and the core material in the mold (step (A)). The liquid thermosetting resin raw material was filled in the mold by decompression and suction with a vacuum pump from a first pipe connected from a thermosetting resin liquid raw material storage tank to the inside of the mold through a second pipe connected from inside the mold to the outside of the mold (step (B)). Then, during or after the filling of the thermosetting resin liquid raw material, the thermosetting resin liquid raw material was cured by a curing reaction, and the curing of the thermosetting resin liquid raw material was completed. After the thermosetting resin liquid raw material was filled, the reduced pressure suction was released before the curing reaction was completed. After that, when the surface temperature of the composite reached room temperature (25°C), the composite was removed from the mold, and a composite was obtained in which a thermosetting resin layer was formed by the cured thermosetting resin on the surface of the core material (step (C)). The measurement and evaluation results of the composite are shown in Table 2.
[0062] [Table 2]
[0063] From Table 2, it can be seen that the composites obtained in the examples can suppress poor curing. It can also be seen that there is no destruction of the cells of the core material in the composite, and it is possible to shorten the molding time. It can also be seen that the obtained composites have excellent bending properties. [Industrial Applicability]
[0064] The method for producing a composite body according to the present invention and the core material used in the production method can suppress poor curing, are free from cell destruction in the core material in the composite body, and have excellent bending properties.
Claims
1. A method for producing a composite having a core material and a thermosetting resin layer provided on at least a portion of a surface of the core material, comprising the steps of: A core material made of a polyamide resin foam and having a moisture content of 0.1 to 5% by mass is placed in a mold, and then Filling the mold with a liquid thermosetting resin material; The thermosetting resin liquid raw material is cured to form a thermosetting resin layer on at least a part of the surface of the core material. A method for producing the composite.
2. The method of claim 1 , wherein the thermosetting resin layer comprises a reinforcing fiber sheet material.
3. The method for producing a composite according to claim 1, wherein the polyamide resin foam has a closed cell rate of 80% or more.
4. The method for producing a composite according to claim 1, wherein the melting point of the polyamide resin constituting the polyamide resin foam is 160 to 285°C.
5. The method for producing a composite according to claim 1 , wherein the core material is composed of composite particles in which reinforcing fibers are attached to the surface of a particulate polyamide-based resin foam via an uncured thermosetting resin.
6. A core material used in the method for producing the composite according to any one of claims 1 to 5, The core material is made of a polyamide resin foam, The core material has a moisture content of 0.1 to 5% by mass.
Citation Information
Patent Citations
Resin foam sheet, resin composite, and method for producing resin composite
JP2018053079A
Polyamide resin foam particles for core material of fiber-reinforced resin composites
JP7203256B1
Method of producing composite molding
JP2014193539A
Composite molding
JP2015017190A