Production method of sand-capping material
By carbonating and granulating steelmaking slag with a water-soluble resin binder, the method addresses slow settling and elution issues, improving carbon dioxide fixation and maintaining water clarity in aquatic environments.
Patent Information
- Application Number
- JP2023049685
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing methods for using steelmaking slag in aquatic environments face issues with slow settling, wide dispersion, turbidity, and alkaline component elution, leading to pH changes and cloudiness in seawater, and insufficient carbon dioxide fixation efficiency.
A method involving carbonating steelmaking slag with an average particle size of 7.00 mm or less and adding a water-soluble resin as a binder during granulation to form a sand-covering material, ensuring a specific particle size distribution and preventing alkaline component elution.
Enhances carbon dioxide fixation efficiency and prevents alkaline component elution in aquatic environments, maintaining water clarity and structural integrity of the sand-covering material.
Smart Images

Figure 2024138949000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a sand-capping material. [Background technology]
[0002] Steelmaking slag, a by-product of the steel production process, contains a large amount of calcium oxide and is therefore expected to be effective in fixing carbon dioxide, a greenhouse gas, as calcium carbonate. In recent years, various technologies have been proposed for fixing carbon dioxide using steelmaking slag.
[0003] Initially, the carbonated steelmaking slag obtained by the above-mentioned fixation technology was considered to be used as road base material, which is the main application of the road base material. Here, road base material is required to have a certain particle size or more in order to maintain the required strength. On the other hand, in order to fix more carbon dioxide in steelmaking slag, it is preferable that the specific surface area of the steelmaking slag is large, so it is preferable to use finely divided steelmaking slag. In order to use such steelmaking slag in which carbon dioxide is fixed as road base material, it is necessary to achieve both a particle size suitable for carbon dioxide fixation and the strength required for road base material, which is a difficult problem in reality.
[0004] As one of the applications of carbon dioxide fixed using fine steelmaking slag, for example, the following Patent Documents 1 to 3 propose applications in aquatic environments such as as a sand-capping material, backfill material, and environmental conservation material. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2012-131651 A [Patent Document 2] JP 2005-320230 A [Patent Document 3] Patent Publication No. 2021-80111 [Patent Document 4] JP 2007-31220 A [Patent Document 5] JP 2008-100893 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the present inventors have concerns regarding the use in aquatic environments (particularly in marine areas) proposed in the above Patent Documents 1 to 3, including the following points.
[0007] That is, since steelmaking slag has a small particle size, it has a slow settling speed when it is dumped into the sea, and it spreads over a wide area, which may cause the seawater to become turbid for a long time. Even if the steelmaking slag settles, it will be carried away by the tidal current for a long time, and the steelmaking slag will wear away from each other. As a result, the carbonated surface layer will be scraped off, creating a new surface, which may cause the alkaline components of the steelmaking slag (e.g., hydroxide ions) to dissolve. When the alkaline components dissolve in the seawater, the pH of the seawater increases, and magnesium ions in the seawater precipitate as magnesium hydroxide, a white solid. This causes the seawater to become turbid.
[0008] The above Patent Documents 1 to 3 do not mention any measures against the elution of alkaline components due to such wear.
[0009] Furthermore, in the above-mentioned Patent Document 4, a technology is proposed for using powdered slag generated in the steel manufacturing process as a part of various aggregates or roadbed materials, or as an alternative raw material for natural sand, in which powdered slag containing 20% or more by mass of particles with an undersize of 5 mm or less is adjusted to a specified moisture content and granulated by mechanical stirring while supplying carbon dioxide gas. Since the particle size of the slag increases by granulating the slag, it is expected that the settling rate will also increase when the slag is dumped into the sea.
[0010] However, powdered slag containing 20% by mass or more of particles with an undersize particle size of 5 mm or less cannot be said to have a particle size sufficient to efficiently fix carbon dioxide, and there is still room for improvement in terms of improving the efficiency of fixation of carbon dioxide.
[0011] In addition, as carbon dioxide gas penetrates the slag from its surface, it reacts with the calcium oxide in the slag and is immobilized. However, when carbon dioxide gas is supplied during granulation, although immobilization progresses on the surface of the granules, the reaction may not proceed sufficiently inside the granules, and there is still room for improvement in terms of measures against the elution of alkali due to wear.
[0012] Therefore, the present invention has been made in consideration of the above problems, and an object of the present invention is to provide a method for manufacturing a sand-capping material that can fix carbon dioxide more efficiently and prevent the leaching of alkali even when placed in an aquatic environment. [Means for solving the problem]
[0013] In order to solve the above problems, the present inventors conducted intensive research and came up with the idea of separating the process of fixing carbon dioxide in steelmaking slag to carbonate the steelmaking slag from the process of granulating the steelmaking slag, and of including a substance that can prevent the elution of alkali when granulating the steelmaking slag, thereby completing the present invention. The gist of the present invention, which was completed based on these findings, is as follows.
[0014] (1) A method for producing a sand-capping material using steelmaking slag, comprising: a carbonation step of fixing carbon dioxide to the steelmaking slag having an average particle size of 7.00 mm or less to carbonate the steelmaking slag; and a granulation step of adding a water-soluble resin as a binder component to the carbonated steelmaking slag, and then granulating the steelmaking slag to which the water-soluble resin has been added to produce a sand-capping material. A method for producing a sand-covering material, comprising: (2) The method for producing a sand-capping material described in (1), wherein the mass ratio of the sand-capping material having a particle size of 2 mm or less in the obtained sand-capping material is 30 mass% or less relative to the total mass of the sand-capping material. (3) The method for producing a sand-capping material described in (1) or (2), wherein the water-soluble resin is at least one of a water-soluble acrylic resin, a water-soluble polyurethane resin, a water-soluble polyester resin, a water-soluble epoxy resin, a water-soluble ceramic resin, or a water-soluble silicone resin. (4) The method for producing a sand-capping material described in (1) or (2), wherein the average particle size of the steelmaking slag subjected to the carbonation process is 1.00 mm or less. (5) The method for producing a sand-capping material according to (1) or (2), wherein the total content of free CaO and Ca(OH)2 in the steelmaking slag subjected to the carbonation process is more than 0.9 mass%. (6) The method for producing a sand-capping material according to (1) or (2), wherein the average particle size of the obtained sand-capping material is within a range of 1.0 mm to 5.0 mm. Effect of the Invention
[0015] As described above, according to the present invention, it is possible to fix carbon dioxide more efficiently, and also to prevent the elution of alkali even when the biomass is placed in an aquatic environment. [Brief description of the drawings]
[0016] [Figure 1] 1 is a flow chart showing an example of a flow of a method for producing a sand-covering material according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings.
[0018] (About the manufacturing method of sand-capping materials) The method for producing a sand-capping material according to the present embodiment relates to a method for producing a sand-capping material using steelmaking slag generated in a steel manufacturing process. As shown in FIG. 1, the method for producing the sand-capping material includes a carbonation step (step S11) and a granulation step (step S13).
[0019] <Carbonation step (step S11)> The carbonation step (step S11) in the method for producing a sand-capping material according to this embodiment is a step of fixing carbon dioxide to the steelmaking slag to carbonate the steelmaking slag. Through this step, carbonated steelmaking slag (hereinafter, sometimes simply referred to as "carbonated slag") can be obtained.
[0020] Examples of steelmaking slag include converter slag, pretreatment slag, decarburization slag, dephosphorization slag, desulfurization slag, desiliconization slag, electric furnace reduction slag, electric furnace oxidation slag, secondary refining slag, ingot casting slag, etc. In the carbonation step (step S11) according to this embodiment, the various steelmaking slags described above can be used alone or in combination.
[0021] In the carbonation step (step S11) according to this embodiment, the average particle size of the steelmaking slag used is 7.00 mm or less. If the average particle size of the steelmaking slag used exceeds 7.00 mm and is no longer fine, the specific surface area of the steelmaking slag is too small to improve the reaction efficiency with carbon dioxide, and therefore the fixation efficiency of carbon dioxide cannot be improved. By using a steelmaking slag with an average particle size of 7.00 mm or less, the specific surface area of the steelmaking slag can be made sufficiently large, and the fixation efficiency of carbon dioxide can be improved. In the carbonation step according to this embodiment, the average particle size of the steelmaking slag used is preferably 1.00 mm or less. By using a steelmaking slag with an average particle size of 1.00 mm or less, it is possible to cause a reaction with carbon dioxide in a larger portion of the steelmaking slag, and as a result, the fixation efficiency of carbon dioxide can be further improved.
[0022] On the other hand, there is no particular lower limit for the average particle size of the steelmaking slag used. However, the smaller the average particle size of the steelmaking slag used, the easier it is to granulate in the subsequent granulation process, and at the same time, the cost of the crushing and sieving processes required to adjust the average particle size to a smaller size increases. In addition, the smaller the average particle size, the higher the dust generation, which significantly worsens the working environment, and therefore requires a great deal of cost for dust prevention measures during handling. Taking these points into consideration, the lower limit for the average particle size of the steelmaking slag used is substantially about 15 μm.
[0023] The average particle size of the steelmaking slag can be measured, for example, as follows. That is, the average particle size can be obtained by performing measurement in accordance with the laser diffraction and scattering method (JIS Z8825:2022). However, when the particle size of the steelmaking slag is large and exceeds the measurement range of the laser diffraction and scattering method, the average particle size can be obtained by performing particle size distribution measurement in accordance with the sieving test (JIS Z8815:1994). In this embodiment, the weighted volume-based average diameter according to the moment notation method of expressing particle size measurement results (JIS Z8819:2019) is obtained as the average particle size.
[0024] In addition, the steelmaking slag to be subjected to the carbonation step (step S11) according to this embodiment preferably has a total content of free CaO and Ca(OH)2 of more than 0.9 mass%. In the carbonation step, the calcium content in the steelmaking slag reacts with carbon dioxide through a chemical reaction represented by the following reaction formula (1), thereby immobilizing carbon dioxide. This reaction forms a layer containing carbonate from the surface of the steelmaking slag toward the inside. Ca 2+ +CO3 2- → CaCO3···Reaction equation (1)
[0025] Therefore, it is preferable that the steelmaking slag to be subjected to the carbonation step contains more calcium, since it is possible to fix a larger amount of carbon dioxide. Such an effect can be significantly exhibited when the total content of free CaO and Ca(OH)2 in the steelmaking slag to be subjected to the carbonation step exceeds 0.9 mass%. From this viewpoint, it is preferable that the total content of free CaO and Ca(OH)2 in the steelmaking slag to be subjected to the carbonation step exceeds 0.9 mass%. The total content of free CaO and Ca(OH)2 in the steelmaking slag to be subjected to the carbonation step is more preferably 2.0 mass% or more.
[0026] Here, the above "free CaO and Ca(OH)2" refers to CaO and Ca(OH)2 dispersed in the steelmaking slag. The total content of free CaO and Ca(OH)2 can be measured by a measurement method such as the ethylene glycol method or the tribromophenol method.
[0027] The specific method for carbonating the steelmaking slag as described above is not particularly limited, and various carbonation treatment methods can be used, including the methods disclosed in the above Patent Documents 1 to 3 and Patent Document 5. Furthermore, the specific treatment conditions in these carbonation treatment methods are also not particularly limited.
[0028] The carbonated slag produced by this process is subjected to a subsequent granulation process. It is preferable that the obtained carbonated slag is subjected to the subsequent granulation process before the moisture contained therein is completely removed.
[0029] <Granulation process (step S13)> The granulation step (step S13) in the method for producing a sand-capping material according to this embodiment is a step of granulating carbonated steelmaking slag to produce a sand-capping material. In granulating the steelmaking slag, the material to be granulated may be kneaded in advance using various kneaders, etc., prior to granulation by the granulator.
[0030] Here, in the granulation step (step S13) according to this embodiment, when the carbonated steelmaking slag is granulated, a water-soluble resin is added to the steelmaking slag as a binder component.
[0031] The water-soluble resin added to the carbonated steel slag during granulation is liquid during granulation, but becomes solid after granulation is completed and the slag is dried, and is an irreversible resin that will not return to a liquid state even if new water is added. In other words, the water-soluble resin is a component that will not dissolve in water for a long period of time once it has solidified.
[0032] For example, the above-mentioned Patent Document 3 discloses the addition of auxiliary materials such as lignin sulfonic acid or its metal salts, molasses, and starch to steelmaking slag, but these substances do not have the above-mentioned irreversibility, and even if they are in a solidified state, they may dissolve when new moisture is added. Therefore, when such substances are used as binder components, there is a concern that the steelmaking slag granulated using the binder components may disintegrate as the binder components dissolve.
[0033] However, when a water-soluble resin is used as a binder component, the water-soluble resin forms liquid bridges during granulation, binding the fine carbonated slag to be granulated and creating an environment in which it is easy to granulate. In addition, when granulation is completed and the water-soluble resin dries and solidifies, solid bridges are formed, making it possible to obtain very strong granulated material. As a result, the obtained granulated material (i.e., sand capping material) does not collapse for a long period of time even after immersion in seawater, and the form in which the fine carbonated slag is granulated together can be maintained for a long period of time, making it possible to obtain granulated material that is less susceptible to wear.
[0034] The surface of the granulated material thus obtained (i.e., sand-capping material) is coated with a water-soluble resin, which prevents the elution of alkaline components from the steelmaking slag. In addition, the resin coating makes the material resistant to wear, so that even if the material is placed in an aquatic environment for a long period of time, the elution of alkaline components can be prevented, and the clouding of seawater can be prevented.
[0035] Examples of water-soluble resins that can be used as the binder component include at least one of water-soluble acrylic resins, water-soluble polyurethane resins, water-soluble polyester resins, water-soluble epoxy resins, water-soluble ceramic resins, and water-soluble silicone resins. In addition, a polymer obtained by polymerizing a plurality of types of water-soluble resins as described above so as not to lose water solubility may be used. In addition, in consideration of environmental impact, it is preferable that the resin component has biodegradable properties.
[0036] By using water-soluble resins such as the various resins exemplified above, it is possible to improve the work efficiency. In addition to the water-soluble resin, by adding water as necessary, it is possible to obtain a more uniform sand-capping material.
[0037] In addition, in order to sufficiently dry the granulated material, it is possible to secure a long drying time. However, since the granulation time is also lengthened with the lengthening of the drying time, it becomes necessary to secure a site area for drying, and there is a possibility that the production efficiency will not improve. Alternatively, in order to sufficiently dry the granulated material, it is possible to set the drying temperature at a high temperature. However, in order to set the drying temperature at a high temperature, more energy is consumed, which is not environmentally preferable. However, since water-soluble resins, including the various resins exemplified above, have a quick-drying property, it is not necessary to secure an excessive drying temperature or drying time, and the production efficiency can be improved.
[0038] Furthermore, by using water-soluble resins such as the various resins exemplified above, it becomes possible to maintain the strength of the sand-capping material in an aqueous environment. As mentioned above, water-soluble resins dissolve in water when not solidified, but after drying, the resins dispersed in water approach and fuse together to form solid bridges between the carbonated slag particles, losing their water-soluble function. This prevents the resin component, which is the binder component, from dissolving and diffusing in an aqueous environment, and makes it possible to maintain the fine carbonated slag particles in a bonded state.
[0039] In the granulation process according to this embodiment, it is preferable that the carbonated slag to be subjected to the process is granulated so that the mass proportion of sand capping material having a particle size of 2 mm or less in the sand capping material obtained after granulation is reduced to 30 mass% or less of the total mass of the sand capping material.
[0040] Here, it is difficult to uniquely determine the amount of water-soluble resin to be added, and it varies depending on the moisture content and average particle size of the carbonated slag to be granulated, the total amount of the carbonated slag, the amount of moisture to be added as necessary, the average particle size required for the sand capping material after granulation, the range of allowable mixing time, etc. Therefore, it is preferable to carry out verification in advance using the carbonated slag and granulator to be used in actual operation, and to optimize in advance the amount to be added that allows the particles of the carbonated slag to be used to be bonded together without excessive excess or deficiency, and the specific values of the various granulation parameters as described above.
[0041] Here, the granulator used in the granulation step is not particularly limited, and various types of rolling granulators such as a briquette machine, a pan pelletizer, a drum mixer, a rotary mixer, etc. can be used.
[0042] Even if a part of the steelmaking slag is granulated in the carbonation process carried out prior to the granulation process, the granulated state of the carbonated slag is eliminated by kneading the carbonated slag in the granulation process within about one hour after the carbonation process is completed so as not to advance the solidification reaction of the granulated material. Therefore, the carbonated slag is granulated while being coated with the water-soluble resin.
[0043] <Average particle size of sand-capping material> In the method for producing a sand-capping material according to the present embodiment, the sand-capping material produced through the above-mentioned steps preferably has an average particle size in the range of 1.0 mm to 5.0 mm. By making the average particle size of the sand-capping material 1.0 mm or more, the settling speed when thrown into water is increased, preventing turbidity, and preventing the sand-capping material from being washed away by tidal currents, etc., while further preventing wear of the sand-capping material. The average particle size of the obtained sand-capping material is more preferably 1.2 mm or more, and even more preferably 1.5 mm or more. On the other hand, by making the average particle size of the sand-capping material 5.0 mm or less, it becomes easier for organisms to burrow in the sand, which is favorable from the viewpoint of increasing organisms. The average particle size of the obtained sand-capping material is more preferably 4.0 mm or less, and even more preferably 3.5 mm or less.
[0044] Here, the average particle size of the obtained sand-capping material can be measured in the same manner as the average particle size of the steelmaking slag described above.
[0045] Furthermore, it is preferable that the average particle size of the obtained sand capping material is within the above range, and the mass ratio of sand capping material with a particle size of 2 mm or less is 30 mass% or less of the total mass of the sand capping material. By reducing the particle size of 2 mm or less to 30 mass% or less of the total, it is possible to further reduce the proportion of sand capping material that may collapse due to wear. The mass ratio of sand capping material with a particle size of 2 mm or less is more preferably 20 mass% or less of the total mass of the sand capping material.
[0046] The mass proportion of sand-capping material with a particle size of 2 mm or less can be measured in accordance with the sieve analysis test (JIS Z8815:1994).
[0047] The method for manufacturing a sand-capping material according to this embodiment has been described in detail above. EXAMPLES
[0048] Next, the method for manufacturing the sand-capping material according to the present embodiment will be specifically described with reference to examples and comparative examples. Note that the examples shown below are merely examples of the method for manufacturing the sand-capping material according to the present embodiment, and the method for manufacturing the sand-capping material according to the present embodiment is not limited to the examples below.
[0049] In the test examples shown below, steelmaking slag with a particle size of 0 to 25 mm and containing 1.6 mass % or 0.7 mass % free CaO, and steelmaking slag that had been classified to have the average particle size shown in Table 1 below were used. A: Steelmaking slag with a total content of free CaO and Ca(OH)2 of 1.6% by mass B: Steelmaking slag with a total content of free CaO and Ca(OH)2 of 0.7% by mass
[0050] Using each of the prepared steelmaking slags, 10 kg of steelmaking slag and 1 L of water were charged into a mortar mixer with a capacity of 55 L. After that, carbon dioxide gas with a purity of 95% was continuously introduced into the mortar mixer at a flow rate of 4 L / min, and the mortar mixer was operated (stirred) for 4 hours to carry out a carbonation treatment.
[0051] In this test example, the following four types of binder components were prepared. a1: Water-soluble polyurethane acrylic resin, water-based VATON Top Clear (manufactured by Otani Paint Co., Ltd.) A2: Water-based ceramic silicone resin paint, water-based Ceramic Silicone (manufactured by SK Chemical Co., Ltd.) b:molasses c: starch d: Pulp waste liquor
[0052] To the carbonated slag prepared as above, a binder component equivalent to 8% of the mass of the carbonated slag was added, and water equivalent to 5-10% of the carbonated slag was further added, and the mixture was kneaded in a kneader for 10 minutes. The kneaded carbonated slag was placed in a pan pelletizer with a diameter of 400 mm, and tumbling granulated while adding water appropriately with a water sprinkler. The obtained granulated material was dried for 6 hours in a dryer set at a temperature of 105°C to obtain a sand capping material. The average particle size of each obtained sand capping material and the mass ratio of sand capping material with a particle size of 2 mm or less were measured according to the method described above.
[0053] The obtained sand-capping materials were evaluated from the viewpoints of immobilized carbon dioxide and abrasion resistance. The obtained results are summarized in Table 1 below.
[0054] [Method for evaluating carbon dioxide fixation efficiency] Regarding the efficiency of carbon dioxide fixation, the amount of carbon dioxide before and after carbonation was quantified according to the method for quantifying carbon dioxide in "Methods for Chemical Analysis of Gypsum (JIS R9101:2018)," and the mass concentration of carbon dioxide fixed by the carbonation process was calculated from the difference in the quantitative values before and after the carbonation process. Samples with a mass concentration of carbon dioxide of less than 0.5% by mass were deemed to have failed.
[0055] [Wear resistance evaluation method] The abrasion resistance was evaluated as follows. 100g of each of the obtained sand-capping materials was placed in a 2L plastic container, and 1L of artificial seawater with a pH adjusted to 8.5 was poured in. Each container was stirred at 200 rpm for 1 hour using a shaker to vigorously fluidize and wear down the sand-capping materials in the container.
[0056] After stirring, the pH of the artificial seawater in the plastic container was measured. After the sand capping material and artificial seawater were sieved through a sieve with 2 mm mesh, the sand capping material and artificial seawater below the sieve were filtered through a glass fiber filter paper with a pore size of 1 μm, and the mass after drying was measured to determine the amount of suspended solids (SS). Those with a suspended solid amount of 200 mg / L or more, those with a pH of 9.5 or more after stirring, and those with a suspended solid amount of 200 mg / L or more and a pH of 9.5 or more after stirring were deemed to have failed the test.
[0057] [Table 1]
[0058] As is clear from Table 1 above, the sand-capping materials corresponding to the examples of the present invention exhibit excellent carbon dioxide fixation efficiency and also have excellent abrasion resistance, while the sand-capping materials corresponding to the comparative examples of the present invention are insufficient in at least one of the carbon dioxide fixation efficiency or abrasion resistance.
[0059] Although the preferred embodiment of the present invention has been described in detail above with reference to the accompanying drawings, the present invention is not limited to such an example. It is clear that a person having ordinary knowledge in the technical field to which the present invention pertains can conceive of various modified or altered examples within the scope of the technical ideas described in the claims, and it is understood that these also naturally belong to the technical scope of the present invention.
[0060] The embodiments disclosed herein are illustrative and not restrictive in all respects. The above embodiments may be omitted, substituted, or modified in various forms without departing from the scope of the appended claims, the technical scope of the present invention as described below, and the spirit thereof. For example, the components of the above embodiments can be arbitrarily combined within a range that does not impair the effects of the components. Furthermore, the arbitrary combination naturally provides the actions and effects of each of the components in the combination, and also provides other actions and effects that are obvious to a person skilled in the art from the description of this specification.
[0061] In addition, the effects described in this specification are merely explanatory or exemplary, and are not limiting. In other words, the technology according to the present invention may achieve other effects that are apparent to a person skilled in the art from the description of this specification, in addition to or in place of the above effects.
[0062] The following configurations also fall within the technical scope of the present invention. (1) A method for producing a sand-capping material using steelmaking slag, a carbonation step of fixing carbon dioxide to the steelmaking slag having an average particle size of 7.00 mm or less to carbonate the steelmaking slag; A granulation process in which a water-soluble resin is added as a binder component to the carbonated steelmaking slag, and the steelmaking slag to which the water-soluble resin has been added is granulated to form a sand-capping material; A method for producing a sand-covering material, comprising: (2) The method for producing a sand-capping material according to (1), wherein the mass ratio of the sand-capping material having a particle size of 2 mm or less in the obtained sand-capping material is 30 mass% or less relative to the total mass of the sand-capping material. (3) The method for producing a sand-capping material according to (1) or (2), wherein the water-soluble resin is at least one of a water-soluble acrylic resin, a water-soluble polyurethane resin, a water-soluble polyester resin, a water-soluble epoxy resin, a water-soluble ceramic resin, or a water-soluble silicone resin. (4) The method for producing a sand-capping material according to any one of (1) to (3), wherein the steelmaking slag subjected to the carbonation step has an average particle size of 1.00 mm or less. (5) The method for producing a sand-capping material according to any one of (1) to (4), wherein the total content of free CaO and Ca(OH)2 in the steelmaking slag subjected to the carbonation step is more than 0.9 mass%. (6) The method for producing a sand-capping material according to any one of (1) to (5), wherein the average particle size of the obtained sand-capping material is within a range of 1.0 mm to 5.0 mm.
Claims
1. A method for producing a sand-capping material using steelmaking slag, a carbonation step of fixing carbon dioxide to the steelmaking slag having an average particle size of 7.00 mm or less to carbonate the steelmaking slag; A granulation process in which a water-soluble resin is added as a binder component to the carbonated steelmaking slag, and the steelmaking slag to which the water-soluble resin has been added is granulated to form a sand-capping material; A method for producing a sand-covering material, comprising:
2. The method for producing a sand-capping material according to claim 1, wherein a mass ratio of the sand-capping material having a particle size of 2 mm or less in the obtained sand-capping material is 30 mass% or less with respect to a total mass of the sand-capping material.
3. The method for producing a sand-capping material according to claim 1 or 2, wherein the water-soluble resin is at least one of a water-soluble acrylic resin, a water-soluble polyurethane resin, a water-soluble polyester resin, a water-soluble epoxy resin, a water-soluble ceramic resin, and a water-soluble silicone resin.
4. The method for producing a sand-capping material according to claim 1 or 2, wherein the steelmaking slag subjected to the carbonation step has an average particle size of 1.00 mm or less.
5. Free CaO and Ca(OH) of the steelmaking slag subjected to the carbonation process 2 The method for producing a sand-capping material according to claim 1 or 2, wherein the total content is more than 0.9% by mass.
6. The method for producing a sand-capping material according to claim 1 or 2, wherein the average particle size of the obtained sand-capping material is within a range of 1.0 mm to 5.0 mm.
Citation Information
Patent Citations
Environmental preservation material for water area and its using method
JP2005320230A
Method of granulating slag and granulated slag
JP2007031220A
Method for stabilizing treatment of powdered steelmaking slag and stabilized steelmaking slag
JP2008214149A
Method for manufacturing modified steel-making slag
JP2012131651A
Slag shaped body and slag shaped body production method
JP2021080111A