Piano black tone injection molded article, injection molding metal mold, and evaluation method for scratch resistance thereof

By mirror-polishing injection molds with controlled abrasive particle sizes and evaluating scratch resistance through a Gakushin-type test, the method enhances piano black-like resin products' scratch resistance across different resin types without additional coatings or fillers, maintaining appearance and reducing costs.

JP2024138972AInactive Publication Date: 2024-10-09MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023049713
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for achieving piano black-like resin molded products with improved scratch resistance either require post-processing with a clear coat film, increasing costs, or are limited to specific resin materials like polyamide, and do not effectively enhance scratch resistance for other commonly used resins such as acrylic and polycarbonate.

Method used

Molding piano black-like products using a mirror-polished injection mold with controlled abrasive particle sizes to enhance surface smoothness, followed by a Gakushin-type abrasion test to evaluate scratch resistance, without the need for additional coatings or filler addition.

Benefits of technology

This method improves scratch resistance without additional processing steps or material limitations, maintaining aesthetic quality and reducing manufacturing costs, while enhancing the resilience of various resin types.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024138972000001
    Figure 2024138972000001
  • Figure 2024138972000002
    Figure 2024138972000002
Patent Text Reader

Abstract

To improve scratch resistance of a piano black tone resin molded article without using a resin material for enhancing hardness and without carrying out a formation processing of a protective film by the following process.SOLUTION: When forming a piano black tone injection molded article, the molded article is formed using a metal mold whose surface is subjected to mirror polishing with a coarse abrasive material without affecting appearance quality of the molded article. As to whether scratch resistance is improved or not, a predetermined Gakushin type wear test is conducted on the molded article, and an evaluation is made by determining whether a difference of measured values of L * value of a surface of the molded body before and after the test falls within a predetermined range.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a piano black-toned injection-molded article having improved scratch resistance (hereinafter also referred to as "scratch resistance"). [Background technology]

[0002] Piano black parts, which have a high-gloss finish in black like the surface of a piano, are used in passenger car parts and panels of home appliances such as televisions because of their luxurious appearance. In the past, the piano black look was often reproduced by painting the surface of a resin molded product; however, painting tends to leave the surface of the molded product with an orange peel look, and requires the use of solvents that are difficult to handle. In addition, there is a demand for a finish with a higher appearance than that achieved by painting. For these reasons, a method has been developed to mold resin molded products with a piano black appearance using raw colorants, that is, materials that color the resin composition itself and give it a glossy finish, without using solvents.

[0003] However, resin molded products made using a raw coloring material have the material exposed as it is on the piano black surface, and therefore have the problem of lower scratch resistance compared to products that are painted. A known technology aimed at solving such problems and a means for solving such problems is to form a molded article with a black surface by injection molding, and then form a clear coat film on the surface of this molded article in a post-processing step, thereby protecting the surface of the black molded article with the clear coat film and thereby improving the scratch resistance of the molded article surface (see, for example, Patent Document 1). It is also known that polyamide resin is used as the material for molded products with a piano black appearance, and a special filler (cellulose fiber) is mixed into the resin material when it is polymerized, thereby increasing the hardness of the molded product surface and improving its scratch resistance (see, for example, Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] JP 2012-236175 A [Patent Document 2] JP 2015-51631 A Summary of the Invention [Problem to be solved by the invention]

[0005] Among the above-mentioned conventional techniques, the former requires a step of coating the surface of the molded article with a clear coat film in addition to a step of molding a black molded article by injection molding, and this poses the problem of increased manufacturing costs depending on the shape of the molded article. The latter method is to mix a special filler into the resin material before molding, which increases the hardness of the molded product and improves its scratch resistance, but it is limited to molded products that use polyamide resin as the material.Acrylic resin and polycarbonate resin are mainly used as materials for piano black molded products, but this technology cannot be applied to moldings that use materials other than polyamide resin.

[0006] In view of the above problems, an object of the present invention is to improve the scratch resistance of a piano black-colored resin molded product without requiring post-processing to increase the surface hardness and without limiting the materials used. [Means for solving the problem]

[0007] In order to solve the above problems, the present invention includes the following aspects. [1] A piano black injection-molded product having a surface L* value of 0.01 to 5.00, wherein when the surface of the molded product is subjected to the following Gakushin type abrasion test, the difference between the L* value of the molded product surface after the test and the L* value before the test is 1.56 or less. (Gakushin-type abrasion test) The Gakushin type abrasion tester specified in "JISK5701-1 6.2.3 Abrasion resistance" was used, and the following items among the test conditions specified in the same regulation were set as follows. Wear element: Kanakin No. 3 Speed:3000mm / min Weight: 500g Number of round trips: 200 [2] A mold for molding a piano black-colored injection-molded product, in which the mold surface to be filled with a resin composition is polished with an abrasive having an average particle size of 3.1 μm to 5.2 μm. [3] A method for producing a piano black-toned injection-molded product, comprising filling the injection molding die according to [2] above with a resin composition to produce a molded product. [4] A method for evaluating the scratch resistance of a piano black-toned injection-molded product, comprising: subjecting a piano black-toned injection-molded product having a surface L* value of 0.01 to 5.00 to the Gakushin-type abrasion test described above; and judging the scratch resistance of the injection-molded product from the difference between the L* value of the surface of the molded product after the test and the L* value before the test.

[0008] The present inventors have conducted research into improving the scratch resistance of piano black-toned molded products by appropriately controlling the transferability of the mold used to mold the molded product, rather than by coating the surface of the molded product with a protective film or by mixing a filler into a resin material and molding it, in other words, by increasing the surface hardness of the molded product itself. Specifically, the surface of the mold for molding piano black-toned molded products is generally polished with fine abrasives, i.e., mirror polished, and this mirror polishing makes the surface of the molded product glossy and smooth. Piano black-toned molded products were molded using molds with different degrees of mirror polishing, i.e., molds with surfaces polished with abrasives of different particle sizes, and their scratch resistance was evaluated.

[0009] As a result, it was found that the scratch resistance of the molded product varies depending on the degree of mirror polishing of the mold surface. More specifically, it was found that even if molding is performed using a mold whose surface has been polished with a coarser abrasive than the abrasive conventionally used to polish the surface of molds, as long as the coarseness of the abrasive is within a certain range, the molded product obtained will have the same degree of gloss when visually inspected, a beautiful appearance, and it can be determined that there is no difference in appearance quality; and when the scratch resistance of molded products molded using a mold whose surface has been polished with a fine abrasive and that molded using a mold whose surface has been polished with a coarse abrasive were evaluated by friction tests, the latter had better scratch resistance.

[0010] Based on the above findings, the present invention aims to improve the scratch resistance of molded products by adjusting the degree of mirror polishing of the surface of the mold used to mold piano black-toned molded products and appropriately controlling the transferability to the molded product surface. In order to objectively determine whether or not this scratch resistance has been imparted, an evaluation method was adopted in which a specified abrasion test was performed on the molded product, the L* value of the molded product surface before and after the test was measured with a colorimeter, and whether or not scratch resistance has been imparted was judged from the difference in the measured L* values. This evaluation method can be applied to evaluate the scratch resistance of molded articles that exhibit gloss, in addition to the piano black molded articles.

[0011] As described later, a prescribed Gakushin type abrasion test was conducted on a piano black molded article whose surface L* value was measured to be in the range of 0.01 to 5.00. It was confirmed in the examples of the present invention that if the difference between the L* value of the molded article surface after the test and the L* value before the test was 1.56 or less, preferably 1.08 or less, and more preferably 0.50 or less, the molded article would have high scratch resistance, would be less susceptible to scratches on the surface, and would be less noticeable even if scratches did occur. It was also confirmed that polishing the surface of a mold for molding piano black-colored molded products with an abrasive having an average particle size of 3.1 μm to 5.2 μm increases the scratch resistance of the molded products produced using this mold. Effect of the Invention

[0012] According to the present invention, the scratch resistance of a molded article formed using a piano black-colored molded article can be increased simply by treating the surface condition of the mold for forming the article. Therefore, compared to conventional two-layer structures in which a protective film is formed on the surface of the molded article, it is possible to design the molded article in any shape and to reduce manufacturing costs. Furthermore, there is no need for the conventional process of mixing additives into the resin material to increase the hardness of the molded product, and it is possible to mold piano black-toned molded products with a beautiful appearance without limiting the resin material used and without impairing the physical properties and texture of the resin material that serves as the base for molding, and it is also possible to increase the scratch resistance of the molded products. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] A preferred embodiment of the piano black molded article of the present invention will be described with reference to the following examples, although the present invention is not limited to the following examples. EXAMPLES

[0014] Example 1 Using PMMA resin (acrylic resin), a piano black molded product was formed by injection molding into a square plate-like product in plan view, measuring 40 mm in length and width and 1.0 mm in thickness. The surface of the mold for molding the above molded product, which was to be filled with the molten resin, was mirror-finished with diamond abrasive (compound) No. 3000 having an average particle size of 5.2 μm. The mold surface is polished uniformly, and the specified polishing roughness (arithmetic mean height Sa) of the mold surface after polishing is 8.0 nm. As the PMMA resin material, ACRYPET (registered trademark) PTN0023 (manufactured by Mitsubishi Chemical Corporation) was used. The resin material used was of a grade that contains a black pigment that produces a piano black color. The resin material was heated to a resin temperature of 240°C and melted and injected into the mold, with the mold temperature set at 80°C, and cured in the mold to form a piano black molded product for testing. Three test molded products were molded.

[0015] The L* value of the surface of each of the three test molded products was measured using a spectrophotometer (SE-7700, manufactured by Nippon Denshoku Industries Co., Ltd.) The median L* value of the three test molded products was 4.01.

[0016] Next, the three test molded pieces were subjected to a Gakushin type abrasion test. The Gakushin type abrasion test was performed using a Gakushin type abrasion tester specified in "JIS K5701-1 6.2.3 Abrasion resistance", using Kanakin No. 3 as the abrasion element (friction element) specified in the same specification, with a weight set to 500g, the movement speed of the abrasion element set to 3000mm / min, and the number of reciprocations set to 200, and the surface of the test molded product was rubbed in accordance with the test process specified in the same specification. The L* value of the surface of each of the three test molded articles after the test was measured using the colorimeter. The median L* value of the three test molded articles after the test was 3.92. The difference in L* value before and after the test was 0.30.

[0017] Example 2 Except for using a mold whose surface was mirror-finished with diamond abrasive (compound) No. 5000 (#5000) with an average particle size of 3.1 μm, the molding of the test molded product, measurement of the L* value of the surface, execution of the Gakushin-type abrasion test, and measurement of the L* value after the test were carried out in the same manner as in Example 1. The prescribed polishing roughness (Sa arithmetic mean height) of the mold surface after polishing was 5.0 nm. The median L* values ​​before and after the test were 3.71 and 4.15, respectively, with a difference of 0.44.

[0018] Example 3 Except for using a mold whose surface was mirror-finished with diamond abrasive (compound) No. 8000 (#8000) with an average particle size of 1.5 μm, the molding of the test molded product, measurement of the L* value of the surface, execution of the Gakushin-type abrasion test, and measurement of the L* value after the test were carried out in the same manner as in Example 1. The prescribed polishing roughness (Sa arithmetic mean height) of the mold surface after polishing was 3.0 nm. The median L* values ​​before and after the test were 3.10 and 4.18, respectively, with a difference of 1.08.

[0019] Comparative Example 1 Except for using a mold whose surface was mirror-finished with diamond abrasive (compound) No. 10000 (#10000) with an average particle size of 0.9 μm, the molding of the test molded product, measurement of the L* value of the surface, execution of the Gakushin-type abrasion test, and measurement of the L* value after the test were carried out in the same manner as in Example 1. The prescribed polishing roughness (Sa arithmetic mean height) of the mold surface after polishing was 2.5 nm. The median L* values ​​before and after the test were 3.02 and 4.74, respectively, with a difference of 1.72. The results of measuring the L* values ​​of the above-mentioned Examples and Comparative Examples are shown in Table 1.

[0020] [Table 1]

[0021] When the appearance of the molded products of each of the above-mentioned Examples and Comparative Examples was visually inspected, all of the molded products had a beautiful, glossy, jet black appearance before the Gakushin-type friction test. It was possible to judge that the appearance quality of all the molded products was the same within the range of visual inspection. When the appearance of the molded products after the Gakushin-type friction test was visually inspected, the molded products of Examples 1 and 2 had the same glossy appearance as before the test. On the other hand, the molded product of Example 3 had lost a little more gloss than before the test, but no scratches were found on the surface. It was confirmed that the molded product of Comparative Example 1 had lost more gloss than before the test and had numerous scratches on its surface.

[0022] Example 4 Using Bioengineering PC resin (polycarbonate resin), a piano black molded product was molded by injection molding in the same manner as in Example 1. As the bioengineering PC resin, DURABIO (registered trademark) D7010SR (manufactured by Mitsubishi Chemical Corporation) was used. The resin material used was of a grade that contains a black pigment that produces a piano black color. The molding die used was the same as that used in Example 1. In the same manner as in each of the above-mentioned Examples and Comparative Examples, test molded products were molded, the L* value of the surface was measured, a Gakushin type abrasion test was conducted, and the L* value after the test was measured. The median L* values ​​before and after the test were 3.22 and 3.92, respectively, with a difference of 0.70.

[0023] Example 5 Using the same bioengineering PC resin as in Example 4 and the molding die of Example 2, test molded products were molded, the L* value of the surface was measured, a Gakushin type abrasion test was conducted, and the L* value after the test was measured in the same manner as in each of the above examples and comparative examples. The median L* values ​​before and after the test were 2.70 and 4.26, respectively, with a difference of 1.56.

[0024] Comparative Example 2 Using the same bioengineering PC resin as in Example 4 and the mold of Comparative Example 1, test molded products were molded, the L* value of the surface was measured, a Gakushin-type abrasion test was conducted, and the L* value after the test was measured in the same manner as in each of the previous Examples and Comparative Examples. The median L* values ​​before and after the test were 2.22 and 8.52, respectively, with a difference of 6.30.

[0025] Comparative Example 3 Using the same bioengineering PC resin as in Example 4 and the mold of Example 3, test molded products were molded, the L* value of the surface was measured, a Gakushin type abrasion test was conducted, and the L* value after the test was measured in the same manner as in each of the above examples and comparative examples. The median L* values ​​before and after the test were 2.32 and 6.26, respectively, with a difference of 3.94. The results of measuring the L* values ​​of the above-mentioned Examples and Comparative Examples are shown in Table 2.

[0026] [Table 2]

[0027] When the appearance of the molded products of each of the above-mentioned Examples and Comparative Examples was visually inspected, all of the molded products had a beautiful, glossy, jet black appearance before the Gakushin-type friction test. It was possible to judge that the appearance quality of all the molded products was the same within the range of visual inspection. When the appearances of the molded products after the Gakushin-type friction test were visually inspected, the molded product of Example 4 had the same glossy appearance as before the test. The molded product of Example 5 had lost some gloss, but no scratches were found on the surface. The molded product of Comparative Example 2 had no gloss and had numerous scratches that stood out as white marks on the surface, and it was confirmed that the molded product of Comparative Example 3 had numerous scratches on its surface, although fewer than Comparative Example 2.

[0028] From the results of the Examples and Comparative Examples, it was confirmed that even when molding products using the molds of each Example, which have a coarser mirror finish than the molds used in Comparative Examples 1 and 2, it is possible to mold piano black-colored molded products with the same appearance quality as the Comparative Examples. It was confirmed that the molded products of each Example, in which the degree of mirror polishing was rough, as in Examples 1 to 5, had better scratch resistance than the molded products of the Comparative Examples, and that the surface of the molded product was less likely to be scratched, and even if scratches were made, they could be made inconspicuous. In particular, it was confirmed that the molded products made using the molds whose surfaces were polished with abrasives having average particle sizes of 5.2 μm and 3.71 μm, used in molding in Examples 1 and 2 and Examples 4 and 5, maintained a beautiful appearance without scratches even after the Gakushin-type abrasion test. It is considered that mirror-polishing the surface of the mold for molding piano black-like molded products with abrasives having the above particle sizes is effective in improving the scratch resistance of the molded products.

Claims

1. A piano black-toned injection molded product having a surface L* value of 0.01 to 5.00, wherein when the surface of this molded product is subjected to the following Gakushin type abrasion test, the difference between the L* value of the molded product surface after the test and the L* value before the test is 1.56 or less. (Gakushin-type abrasion test) A Gakushin type abrasion tester specified in "JIS K5701-1 6.2.3 Abrasion resistance" was used, and the following items among the test conditions specified in the same specification were set as follows. Wear element: Kanakin No. 3 Speed: 3000mm / min Weight: 500g Number of round trips: 200

2. The injection molding die is for molding a piano black-toned injection molded product, and the surface of the die to be filled with a resin composition is polished with an abrasive having an average particle size of 3.1 μm to 5.2 μm.

3. A method for producing an injection-molded product having a piano black tone, comprising filling the injection mold according to claim 2 with a resin composition to produce a molded product.

4. A method for evaluating the scratch resistance of a piano black injection-molded product, comprising the steps of: A method for evaluating the scratch resistance of a piano black-toned injection molded product, in which the following Gakushin type abrasion test is performed on a piano black-toned injection molded product having a surface L* value of 0.01 to 5.00, and the scratch resistance of the injection molded product is determined from the difference between the L* value of the molded product surface after the test and the L* value before the test. (Gakushin-type abrasion test) A Gakushin type abrasion tester specified in "JIS K5701-1 6.2.3 Abrasion resistance" was used, and the following items among the test conditions specified in the same specification were set as follows. Wear element: Kanakin No. 3 Speed: 3000mm / min Weight: 500g Number of round trips: 200

Citation Information

Patent Citations

  • Piano black molding

    JP2012236175A

  • Injection-molded product, and production method thereof

    JP2015051631A

Cited By

  • Game machine

    JP2024159850A

  • Game machine

    JP2024161101A

  • Game machine

    JP2024161102A

  • Game machine

    JP2024161103A

  • Game machine

    JP2024161104A