Optical film with process film, wound body, method for manufacturing optical film with process film, and method for manufacturing process film
A self-adhesive thermoplastic resin-based process film allows for efficient recycling by eliminating the need for adhesive layers, maintaining film quality and purity, addressing the recycling challenges posed by conventional adhesive-based process films.
Patent Information
- Application Number
- JP2023049807
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
The adhesive layer on conventional process films hinders the recycling of discarded process films, leading to impurities and different material characteristics, thus affecting the quality and purity of recycled materials.
The use of a self-adhesive process film composed of a single type of thermoplastic resin, which allows for easy separation and recycling without the need for additional adhesive layers, maintaining material purity.
Enables recycling of process films with minimal impurities, ensuring the same functional properties as the original film, thus improving material quality and reducing recycling costs.
Smart Images

Figure 2024139033000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to an optical film with a processing film, a roll formed by winding an optical film with a processing film, a method for manufacturing an optical film with a processing film, and a method for manufacturing a processing film. [Background technology]
[0002] Optical films such as polarizers and polarizing plates may have their surfaces damaged or contaminated during their manufacturing process or during transportation after manufacturing. To prevent this, a processing film that serves to temporarily protect the surface of the optical film is attached to the surface of the optical film (see, for example, Patent Document 1). The processing film generally has an adhesive layer and is attached to the surface of the optical film by its adhesive force. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Patent Publication No. 2021-6638 Summary of the Invention [Problem to be solved by the invention]
[0004] After completing its role, the process film is peeled off and discarded. When the process film is peeled off, the adhesive layer remains on the process film side, not on the optical film side. Here, when attempting to recycle the process film using the discarded process film as a raw material, the components of the adhesive layer become impurities for the material forming the process film, so the recycled process film will have different characteristics or quality from the original process film. In other words, the adhesive layer used to bond the process film to the optical film hinders the recycling of the process film.
[0005] Therefore, an object of the present invention is to provide an optical film with a process film, which is provided with a process film that does not hinder recycling in terms of the purity of the raw material when discarded process film is used as the raw material for recycling the process film. Another object of the present invention is to provide a roll in which the optical film with the process film is rolled up. Another object of the present invention is to provide a method for manufacturing the optical film with the process film. Another object of the present invention is to provide a method for manufacturing the process film. [Means for solving the problem]
[0006] The present invention provides an optical film with a process film, comprising an optical film and a process film having self-adhesive properties, the optical film and the process film being in contact with each other and bonded together, the process film comprising one type of thermoplastic resin.
[0007] Since the process film of this optical film with process film is composed of one type of thermoplastic resin, when recycling after disposal, there is no need for the trouble of sorting or the like to increase the purity as a raw material.
[0008] The optical film with the processing film of the present invention may have one or more of the following characteristics.
[0009] The process film may be a single layer or may be made up of multiple layers.
[0010] The optical film may be a polarizing plate.
[0011] The process film may be attached to the optical film such that the difference between the peel strength of one surface of the process film to the optical film and the peel strength of the other surface of the process film to the optical film is 0.02 N / 25 mm or more, and the surface with the greater peel strength is in contact with the optical film.
[0012] The process film may have a peel strength from the optical film of 0.06 N / 25 mm or more on a surface that is in contact with the optical film, and may have a peel strength from the optical film of 0.04 N / 25 mm or less on a surface that is not in contact with the optical film.
[0013] The haze of the casting film may be 6.0% or less.
[0014] The thermoplastic resin may contain at least one copolymer selected from the group consisting of ethylene-α-olefin copolymers and ethylene-(meth)acrylate copolymers. Here, the density of the ethylene-α-olefin copolymer is 0.880 g / cm 3 More than 0.915g / cm 3 or less, and the density of the ethylene-(meth)acrylate copolymer may be 0.935 g / cm 3 It may be more than that.
[0015] The ethylene-α-olefin copolymer may include a copolymer derived from at least one selected from the group consisting of ethylene-1-hexene and ethylene-1-butene. The ethylene-(meth)acrylate copolymer may be an ethylene-methyl methacrylate copolymer.
[0016] The present invention also provides a roll obtained by rolling up the above-mentioned optical film with a processing film.
[0017] The present invention also provides a manufacturing method for producing the above-mentioned optical film with a process film, the manufacturing method comprising the steps of subjecting one side of the process film to corona treatment, and laminating the process film and the optical film with the one side facing the optical film.
[0018] In this manufacturing method, the process film may have a peel strength from the optical film on one side of 0.04 N / 25 mm or less before the corona treatment, and a peel strength from the optical film on one side of 0.06 N / 25 mm or more after the corona treatment.
[0019] The present invention also provides a manufacturing method for a process film, the manufacturing method comprising a step of crushing the process film peeled off from the optical film with the process film, and melt-extruding the crushed process film to form a new process film.The present invention also provides an optical film with a process film, the optical film with a process film, comprising a process film having self-adhesive properties manufactured by the manufacturing method and an optical film, the absolute value of the difference between the haze of the process film to be crushed in the manufacturing method and the haze of the process film manufactured by the manufacturing method is 3.0% or less. Effect of the Invention
[0020] According to the present invention, it is possible to provide an optical film with a process film, which is provided with a process film that does not hinder recycling in terms of the purity of the raw material when discarded process film is used as a raw material for recycling the process film. It is also possible to provide a roll in which the optical film with the process film is rolled up. It is also possible to provide a method for manufacturing the optical film with the process film. It is also possible to provide a method for manufacturing the process film. [Brief description of the drawings]
[0021] [Figure 1] FIG. 2 is a cross-sectional view of an optical film with a processing film. [Diagram 2] FIG. 2 is a cross-sectional view of a polarizing plate with a processing film. [Diagram 3] FIG. 2 is a cross-sectional view of a laminate of sheets of optical film with a process film attached thereto. [Figure 4] FIG. 2 is a side view of a roll of the optical film with a processing film attached. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Optical films such as polarizers and polarizing plates are long when manufactured, and there is a risk that the surface may be damaged or contaminated during the manufacturing process or transportation after manufacturing. To prevent this, a process film that plays a role of temporarily protecting the surface is attached to the surface of the optical film. In this specification, the optical film to which the process film is attached is called an "optical film with a process film". The optical film with a process film of the present invention includes an optical film and a process film having self-adhesive properties, and both films are attached in contact with each other. Since the process film of the present invention is a film having self-adhesive properties containing one type of thermoplastic resin, it is easy to maintain a high purity state as a raw material for recycling after it has completed its role as a process film and is discarded. Hereinafter, a preferred embodiment of the present invention will be described in detail with reference to the drawings. In addition, the same parts or corresponding parts in each figure are given the same reference numerals, and duplicated explanations will be omitted.
[0023] <Optical film with processing film> As shown in Fig. 1, the optical film with processing film 1A of this embodiment includes an optical film 3A and a processing film 2 having self-adhesive properties. The optical film 3A and the processing film 2 are in contact with each other and bonded together. The optical film 3A may be a retardation film, a polarizer, a polarizing plate, etc., and Fig. 2 shows an example in which the optical film is a polarizing plate 3B.
[0024] <Processing film> The process film 2 may be a single layer or may be made up of multiple layers. When the process film is made up of multiple layers, all layers contain one type of thermoplastic resin. The meaning of "one type" will be described later. All layers are made of the same thermoplastic resin composition. Here, the same thermoplastic resin composition means that the type and molecular weight of the thermoplastic resin contained in the thermoplastic resin composition, and the type and content of additives added to the thermoplastic resin are all the same. In other words, the raw materials (e.g., pelletized resin composition) used for film formation of the process film 2 are the same.
[0025] In addition, when all layers are formed from the same thermoplastic resin composition, the physical properties of each layer may be different. The crystallinity and orientation of the thermoplastic resin composition after film formation can be manipulated by adjusting the temperature during film formation. By manipulating these physical properties, the peeling force of the processing film 2 against the optical film 3A can be adjusted. Even if each layer is formed into a film under different forming conditions, all layers are in a molten state of a homogeneous thermoplastic resin composition during melt extrusion, so that by reproducing the film under the same forming conditions, a multilayer processing film having the same function as before the regeneration can be obtained again.
[0026] The casting film 2 has self-adhesive properties. In this specification, "self-adhesive properties" refers to a property in which the casting film has a peel strength (adhesion strength) sufficient to adhere to an adherend by itself without the need for a separate means for adhesion (such as a pressure-sensitive adhesive layer or adhesive layer) between the casting film and the adherend, and the adhesion state can be maintained.
[0027] The processing film 2 is laminated directly onto the optical film 3A, and the peeling force of the processing film 2 against the optical film is greater than 0 N / 25 mm. If the peeling force is 0 N / 25 mm, the processing film and the optical film in the optical film with the processing film are not in close contact with each other, causing problems such as lifting during transportation or cutting in the manufacturing process and reduced durability of the optical film in a humid and hot environment during transportation.
[0028] The peel strength of the surface of the processing film 2 that is in contact with the optical film 3A from the optical film 3A is preferably 0.06 N / 25 mm or more, more preferably 0.08 N / 25 mm or more, and even more preferably 0.10 N / 25 mm or more. If the peel strength is 0.06 N / 25 mm or more, the adhesion to the optical film 3A is high, and partial peeling of the processing film 2 is unlikely to occur. In particular, when the optical film 3A is a polarizing plate that includes a polarizer, the polarizer is unlikely to tear along the stretching direction (parallel to the stretching direction) during storage in a rolled state.
[0029] In general, the peeling force is preferably 1.5 N / 25 mm or less, but particularly when the optical film 3A is a polarizer in which iodine is adsorbed and oriented in a polyvinyl alcohol-based resin film, the peeling force is preferably 0.5 N / 25 mm or less. When the peeling force of the process film 2 from the optical film 3A is equal to or less than the upper limit described above, the process film 2 can be easily peeled from the optical film 3A, and the optical film can be prevented from being broken or damaged.
[0030] The peel strength of the processing film 2 on the side of the processing film-attached optical film 1A that is not in contact with the optical film 3A from the optical film 3A is preferably 0.04 N / 25 mm or less, more preferably 0.03 N / 25 mm or less, and even more preferably 0.02 N / 25 mm or less. If the peel strength is 0.04 N / 25 mm or less, when a plurality of processing film-attached optical films 1A are stacked in the thickness direction, adhesion of other processing film-attached optical films 1A to the optical film 3A is prevented.
[0031] More specifically, examples of "an embodiment in which a plurality of optical films with processing films 1A are stacked in the thickness direction" include a laminate 7 of sheets (FIG. 3) and a roll 8 (FIG. 4) described below. These have an integrated structure in which the optical films with processing films 1A are directly stacked, and are stored in this state. At this time, as shown in FIG. 3, the process film 2 of one optical film with processing films 1A is in contact with the surface of the optical film 3A of another optical film with processing films 1A, and is stored for a long period of time in the state of the laminate 7.
[0032] Here, the difference between the peel strength of one side of the processing film 2 and the peel strength of the other side of the processing film 2 with respect to the optical film 3A is preferably 0.02 N / 25 mm or more, more preferably 0.04 N / 25 mm or more, and even more preferably 0.06 N / 25 mm or more. At the same time, it is preferable that the side with the larger peel strength is bonded to the optical film 3A so as to contact the optical film 3A. By satisfying these requirements, unintended adhesion and peeling are suppressed. For example, when the optical film 3A is a polarizing plate, the polarizing plate is mechanically conveyed in a state where multiple overlapping plates are conveyed in the panel bonding process when only one should be conveyed, or the adhesive layer interface in the polarizing plate is peeled off when the overlapping polarizing plates are pulled apart. In addition, if the peel strength at the interface between the laminated processing film-attached optical films 1A is 0.04 N / 25 mm or less, the effect is further enhanced.
[0033] The haze of the processing film 2, which is measured in accordance with JIS K 7136:2000 after being attached to glass via an acrylic adhesive, is preferably 6.0% or less, more preferably 5.0% or less, and even more preferably 4.5% or less. If the haze is 6.0% or less, the processing film has a sufficiently high transparency and is unlikely to be an obstacle when automatically inspecting the optical film 1A with the processing film. In other words, when inspecting the optical film 3A for defects, inspection is possible even in a state where the processing film 2 is attached.
[0034] The material forming the casting film 2 is not particularly limited as long as it is a thermoplastic resin composition. The thermoplastic resin composition contains a polymer component and an additive. The additives may be one type or two or more types as long as they are uniform within the casting film 2.
[0035] The process film 2 contains one type of thermoplastic resin. Here, "one type" means that (i) when the process film 2 is a single layer, the polymer components are uniformly distributed throughout, and the polymer components constituting the thermoplastic resin may be a single polymer component or may be in a state where multiple types of polymer components are uniformly distributed. Also, "one type" means that (ii) when the process film 2 is made up of multiple layers, the same polymer components are uniformly distributed throughout all layers, and the polymer components constituting the thermoplastic resin may be a single polymer component or may be in a state where multiple types of polymer components are uniformly distributed. The state of (ii) is achieved by using the same raw materials for each layer before film formation.
[0036] The polymer component is not particularly limited as long as it is any thermoplastic resin, but is preferably a copolymer. It is more preferably a copolymer using ethylene as a monomer before polymerization, and more preferably at least one copolymer selected from the group consisting of ethylene-α-olefin copolymers and ethylene-(meth)acrylate copolymers. The ethylene-α-olefin copolymer preferably contains a copolymer derived from at least one selected from the group consisting of ethylene-1-hexene and ethylene-1-butene. The ethylene-(meth)acrylate copolymer is preferably an ethylene-methyl methacrylate copolymer.
[0037] The density of ethylene-α-olefin copolymer is 0.880 g / cm 3 More than 0.915g / cm 3 It is preferable that the density is 0.890 g / cm or less. 3 More than 0.910g / cm 3The density of the ethylene-(meth)acrylate copolymer is preferably 0.935 g / cm or less. 3 It is preferable that the content is 0.938 g / cm or more. 3 More preferably, it is equal to or greater than this.
[0038] The thermoplastic resin composition forming the casting film 2 may contain an additive. The type of additive is not particularly limited, but it is preferable that the casting film contains an antistatic agent. When the casting film contains an antistatic agent, it is possible to prevent problems, particularly when the optical film is a polarizing plate, in which peeling electrification disturbs the alignment of the liquid crystal in the liquid crystal panel when the casting film is peeled off from the polarizing plate after panel lamination, causing defects in the image display device, and problems in which the surface of the polarizing plate is contaminated by peeling electrification.
[0039] The thickness of the casting film 2 is not particularly limited, but is preferably 20 μm or more, and more preferably 30 μm or more, and is preferably 150 μm or less, and more preferably 100 μm or less.
[0040] <Optical film> The optical film 3A may be any of various optical films (films having optical properties) that can be incorporated into liquid crystal displays and organic EL displays. The optical film 3A may be an optical film having a single layer structure or an optical film having a multilayer structure.
[0041] Specific examples of the optical film having a single layer structure include optically functional films such as a polarizer, a retardation film, a brightness enhancing film, an anti-glare film, an anti-reflection film, a diffusion film, and a light collecting film.
[0042] Examples of the optical film having a multilayer structure include a laminate in which the optical films having the above-mentioned single-layer structure are laminated on each other via a pressure-sensitive adhesive layer or an adhesive layer, and examples of the laminate include a polarizing plate and a retardation plate. The laminate may include a protective film in addition to the films exemplified in the above-mentioned single-layer optical film.
[0043] (Polarizing plate) In the present invention, the polarizing plate includes at least a protective film, an adhesive layer, and a polarizer. The polarizing plate may further include other films or layers, and may have protective films on both sides of the polarizer, and may further have a pressure-sensitive adhesive layer and a release liner. The processing film of the polarizing plate with a processing film is preferably provided on the protective film side of the polarizing plate.
[0044] As shown in FIG. 2, the polarizing plate with processing film 1B is a laminate of a processing film 2 and a polarizing plate 3B, and the polarizing plate 3B includes, in order from closest to the processing film 2, a protective film 4, an adhesive layer 5, and a polarizer 6.
[0045] The polarizer may be, for example, a film in which a dichroic dye is adsorbed and aligned on a polyvinyl alcohol-based resin film, or a cured film in which a dichroic dye is aligned in a polymerizable liquid crystal compound and the polymerizable liquid crystal compound is polymerized. The thickness of the polarizer 6 is usually 1 μm to 30 μm, and from the viewpoint of thinning the polarizing plate 3B, it is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less.
[0046] The protective film 4 is preferably made of a resin selected from the group consisting of cyclic polyolefin resins, polycarbonate resins, cellulose resins, polyester resins, and (meth)acrylic resins. The thickness of the protective film 4 is usually 1 μm to 150 μm, preferably 5 μm to 100 μm, and more preferably 5 μm to 60 μm. The thickness may be 50 μm or less, and even 30 μm or less. Reducing the thickness of the protective film 4 is advantageous for reducing the thickness of the polarizing plate 3B and the display device including the same.
[0047] The adhesive for forming the adhesive layer 5 may be a water-based adhesive or an active energy ray-curable adhesive.
[0048] <Optical film sheet with processing film> When the optical film 3A is a polarizing plate, the optical film with processing film 1A may be stored and used in the form of, for example, a long sheet, but it is preferable that it is cut into a size according to the screen size of the image display device to which it is applied, and made into a sheet-like laminate 7 of sheets as shown in Fig. 3. If the peeling force of the processing film 2 satisfies the above-mentioned relationship, adhesion force is exerted in the part of the laminate 7 where adhesion force should be exerted (between the processing film 2 and the optical film 3A in any optical film with processing film 1A), and adhesion force is not exerted in the part where adhesion force should not be exerted (between overlapping optical films with processing films 1A), so that when one optical film with processing film 1A is to be picked up from the laminate 7, only one piece can be picked up reliably.
[0049] <Optical film roll with processing film> The optical film with processing film 1A may be stored and used in the form of, for example, a long sheet. As shown in Fig. 4, the sheet-like optical film with processing film 1A is preferably wound around a core 9 to form a roll 8.
[0050] The roll of the retardation film with the processing film can be applied to the production of a laminated film, for example, as follows. A processing film is attached to the retardation film continuously formed into a long shape in order to prevent deformation of the roll during storage and adhesion of the retardation films to each other, and the retardation film with the processing film is rolled up. The retardation film with the processing film is then pulled out from the roll, and after the processing film is peeled off, it is laminated to a polarizer or another retardation film.
[0051] The roll of the polarizer with the processing film can be used to manufacture a polarizing plate, for example, as follows. A processing film is attached to a polarizer that has been continuously molded into a long shape in order to prevent the polarizers from sticking to each other or from developing wrinkles due to moisture changes during storage, and the polarizer with the processing film is then rolled up. The polarizer with the processing film is then pulled out from the roll, and after the processing film is peeled off, it is stuck to other protective films and optical compensation films such as retardation films that have also been pulled out from the roll.
[0052] In addition, the roll of the polarizing plate with the processing film can be applied to the manufacture of a liquid crystal panel, for example, as follows. A processing film is attached to a polarizing plate continuously molded into a long shape to prevent the surface from being scratched during transportation in a later process, and the polarizing plate with the processing film is rolled up. Then, the polarizing plate with the processing film is pulled out from the roll, and the polarizing plate surface is laminated with another protective film or an optical compensation film such as a retardation film, which is also pulled out from the roll, or a pressure-sensitive adhesive film for laminating to a liquid crystal cell. Then, the laminate is laminated to a liquid crystal cell. The processing film is peeled off after the laminate is laminated to the liquid crystal cell.
[0053] <Method of manufacturing optical film with processing film> The optical film 1A with processing film is produced by a production method including a step of subjecting one side of the processing film 2 to corona treatment and a step of bonding the processing film 2 and the optical film 3A together with the other side facing the optical film 3A.
[0054] The conditions of the corona treatment can be set appropriately, and the peel strength of the process film 2 from the optical film 3A can be adjusted by the conditions of the corona treatment. As described above, the peel strength of one side of the optical film 3A before the corona treatment is preferably 0.04 N / 25 mm or less. Moreover, the peel strength of one side of the optical film 3A after the corona treatment is preferably 0.06 N / 25 mm or more.
[0055] Pellets of the thermoplastic resin composition as raw material can be melt extruded in a conventional manner to form a single-layered casting film, or the same pellets can be co-extruded to form a multi-layered casting film.
[0056] <Recycling of processing film> The process film 2 is used by being stuck to the optical film 3A, and is peeled off and discarded after use. The discarded process film 2 can be collected and recycled. The collected process film 2 can be crushed and melt-extruded to form a new process film. According to this manufacturing method, the process film can be recycled. Here, "recyclable" means that the new film obtained by crushing and melt-extruding the process film can have the same functions as the film before recycling. Therefore, the new process film can be reused as a process film by laminating it on an optical film.
[0057] Here, "having equivalent functions" means, for example, that the optical properties are equivalent. A specific example of an optical property is haze. The absolute value of the difference between the haze of the process film before recycling and the haze of the process film after recycling is preferably 3.0% or less, more preferably 1.0% or less, and even more preferably 0.5% or less. Here, "difference in haze" does not mean the rate of change of the haze value (%) after recycling from the haze value (%) before recycling, but means the simple difference in value expressed as a percentage.
[0058] Conventional casting films are made by laminating an adhesive layer on a base film that does not have self-adhesiveness, and are attached to the surface of the optical film by the adhesive force. When such casting films are recycled, the components of the adhesive layer become impurities in the material that forms the casting film, so there is a problem that the recycled casting film has different characteristics or quality from the original casting film. However, it is very costly to provide a process for removing the adhesive layer for recycling.
[0059] In contrast, the processing film 2 of the present embodiment is configured to contain one type of thermoplastic resin, and therefore does not require the effort of separation or the like to increase the purity of the raw material when recycled.
[0060] Although the preferred embodiments of the present invention have been described above, the present invention is not limited to the above-described embodiments. EXAMPLES
[0061] The present invention will be described in more detail below with reference to examples and comparative examples. Note that the present invention is not limited to the following examples. Note that "%" and "parts" in the description are by mass% and parts by mass unless otherwise specified.
[0062] (Production Examples 1 to 8: Production of Process Films A to H) Pellet A shown in Table 1 was melt-extruded at a resin temperature of 180°C, and then cooled and solidified while being wound up on a chill roll through which a cooling liquid of roll temperature 30°C was passed, to obtain a 100μm thick process film A. Pellet B to H shown in Table 1 were also subjected to the same procedure to obtain 100μm thick process films B to H.
[0063] [Table 1]
[0064] (Production Example 9: Production of Process Film I) A polyethylene terephthalate film (thickness: 38 μm) having a 20 μm thick adhesive layer was used as the casting film I. The casting film I had a thickness of 58 μm.
[0065] (Production Example 10: Production of Process Film J) Toretec (registered trademark) 7332, a multi-layer polyolefin protective film having weak adhesive strength and manufactured by Toray Advanced Film Co., Ltd., was prepared and used as a processing film J. The processing film J had a thickness of 30 μm.
[0066] (Production Example 11: Production of Polarizing Plate A) Protective film 1 (50 μm thick cyclic polyolefin resin (norbornene resin) film [trade name "ZEONOR" manufactured by Zeon Corporation]), polarizer (23 μm thick polyvinyl alcohol (PVA)-iodine polarizing film), and protective film A in the table below were laminated in this order using an ultraviolet-curing adhesive, and then a 20 μm thick (meth)acrylic adhesive and a release film were laminated in this order to the surface of protective film 1. Protective film A was produced as follows.
[0067] -Preparation of protective film A A (meth)acrylic resin was prepared, which is a copolymer of methyl methacrylate and methyl acrylate copolymerized at a weight ratio of 96:4. Also prepared were acrylic rubber particles having an average particle size of 240 nm up to the elastic body of the intermediate layer, which is a three-layer structure in which the innermost layer is made of a hard polymer polymerized with methyl methacrylate using a small amount of allyl methacrylate, the intermediate layer is made of a soft elastic body mainly composed of butyl acrylate and further polymerized with styrene and a small amount of allyl methacrylate, and the outermost layer is made of a hard polymer polymerized with methyl methacrylate using a small amount of ethyl acrylate.
[0068] The above (meth)acrylic resin and the above acrylic rubber particles were blended in a weight ratio of 70:30, and pellets were prepared to which a benzotriazole-based ultraviolet absorber was added. While melt-kneading the pellets in a twin-screw extruder, 0.05 parts by weight of stearic acid, a lubricant, was added to 100 parts by weight of the pellets, and mixed to obtain pellets of a (meth)acrylic resin composition. The pellets were fed into a single-screw extruder of 65 mmφ and extruded through a T-shaped die set at 275°C, and both sides of the extruded film-like molten resin were sandwiched between two polishing rolls with mirror surfaces set at 45°C and cooled to produce a (meth)acrylic resin film with a thickness of 80 μm. This was designated "protective film A".
[0069] (Production Examples 12 to 16: Production of Polarizing Plates B to F) Polarizing plates B to F were produced in the same manner as in Production Example 11, except that protective film A was changed to protective films B to F (see Table 2). The method for producing protective film E is as follows.
[0070] - Preparation of protective film E When the temperature of the esterification reactor reached 200°C, 86.4 parts by mass of terephthalic acid and 64.6 parts by mass of ethylene glycol were charged, and 0.017 parts by mass of antimony trioxide, 0.064 parts by mass of magnesium acetate tetrahydrate, and 0.16 parts by mass of triethylamine were charged as catalysts while stirring. Next, the temperature was increased under pressure and a pressure esterification reaction was carried out under conditions of a gauge pressure of 0.34 MPa and 240°C, after which the esterification reactor was returned to normal pressure and 0.014 parts by mass of phosphoric acid was added. Further, the temperature was increased to 260°C over 15 minutes, and 0.012 parts by mass of trimethyl phosphate was added. Next, after 15 minutes, a dispersion treatment was carried out using a high-pressure disperser, and after 15 minutes, the obtained esterification reaction product was transferred to a polycondensation reactor and a polycondensation reaction was carried out under reduced pressure at 280°C.
[0071] After the polycondensation reaction was completed, the mixture was filtered using a Naslon filter with a 95% cut diameter of 5 μm, extruded from a nozzle in the form of a strand, cooled and solidified using cooling water that had been previously filtered (pore diameter: 1 μm or less), and cut into pellets. The intrinsic viscosity of the resulting polyethylene terephthalate resin (A) was 0.62 dl / g, and it contained substantially no inert particles or internally precipitated particles. (Hereinafter, this will be abbreviated as PET (A)).
[0072] On the other hand, 10 parts by mass of dried ultraviolet absorber (2,2'-(1,4-phenylene)bis(4H-3,1-benzoxazinon-4-one) and 90 parts by mass of particle-free PET (A) (intrinsic viscosity 0.62 dl / g) were mixed and kneaded using an extruder to obtain polyethylene terephthalate resin (B) containing an ultraviolet absorber (hereinafter abbreviated as PET (B)).
[0073] As the raw material for the intermediate layer of the base film, 90 parts by mass of PET (A) resin pellets containing no particles and 10 parts by mass of PET (B) resin pellets containing an ultraviolet absorber were dried under reduced pressure (1 Torr) at 135 ° C for 6 hours, and then fed to an extruder (for intermediate layer II layer), and PET (A) was dried by a conventional method and fed to an extruder (for outer layer I layer and outer layer III layer), respectively, and melted at 285 ° C. These two types of polymers were filtered with a stainless steel sintered filter medium (nominal filtration accuracy 10 μm particle 95% cut) and laminated in a two-type three-layer merging block, extruded into a sheet shape from a die, and then wrapped around a casting drum with a surface temperature of 30 ° C using an electrostatic casting method, cooled and solidified, and an unstretched film was made. At this time, the discharge amount of each extruder was adjusted so that the thickness ratio of I layer, II layer, and III layer was 10:80:10.
[0074] Next, the unstretched PET film was coated on both sides with a 0.08 g / m coating after drying by the reverse roll method. 2 After the adhesiveness-modifying coating liquid was applied so that the thickness became 100 μm, the coating was dried at 80° C. for 20 seconds.
[0075] The unstretched film with the coating layer formed thereon was introduced into a tenter stretching machine, and while the ends of the film were held by clips, it was introduced into a hot air zone at a temperature of 125°C and stretched 4.0 times in the width direction. Next, while maintaining the width stretched in the width direction, it was treated at a temperature of 225°C for 10 seconds, and further relaxed by 3.0% in the width direction to obtain a uniaxially stretched PET film with a film thickness of about 80 μm. This was named "protective film E".
[0076] (Production Example 17: Production of Polarizing Plate G) The same protective film 1 and polarizer as in Production Example 11 were bonded together using an ultraviolet-curable adhesive, and then a (meth)acrylic pressure sensitive adhesive having a thickness of 20 μm was bonded to the surface of the protective film 1.
[0077] [Table 2]
[0078] <Example 1> (1) Preparation of a polarizing plate with a process film (without corona treatment) The process film A produced in Production Example 1 was bonded to the surfaces of the protective films A to F of the polarizing plates A to F produced in Production Example 11, and to the polarizer side surface of the polarizing plate G, using a roll laminating device, to produce polarizing plates with the process film.
[0079] (2) Preparation of polarizing plate with process film (with corona treatment) Discharge rate of 100 W·min / m on one side of the process film A produced in Manufacturing Example 1 2 Corona treatment was performed at a voltage of 500 W (output 500 W / electrode width 500 mm, film transport speed 10 m / min), and the corona-treated surface was bonded to the protective film A-E sides of polarizing plates A-E produced in Production Example 11 and to the polarizer side surface of polarizing plate G using a roll laminating device to produce polarizing plates with process film.
[0080] (3) Evaluation of adhesion to polarizing plates The polarizing plate with the processing film obtained above was left to stand for one week under conditions of a temperature of 23°C and a humidity of 55% RH. The polarizing plate with the processing film after standing was cut into a strip of 25 mm width x 100 mm length, and the release film was peeled off and the plate was attached to a soda glass with a thickness of 1.1 mm via the adhesive layer of the polarizing plate. The processing film was peeled off in the length direction at a peel angle of 180° and a peel speed of 300 mm / min, and the peel force was measured. The average value of the obtained peel forces was taken as the peel force of the processing film.
[0081] (4) Haze evaluation One side of the casting film was attached to glass via a 25 μm thick acrylic adhesive. The haze was measured using a haze meter HR-150 manufactured by Murakami Color Research Laboratory Co., Ltd. under the conditions of glass surface incidence and JIS K 7136:2000. The measured value obtained was taken as the haze of the casting film.
[0082] (5) Evaluation of haze after remolding The processing film was cut into pieces of about 10 mm x 10 mm, fed into an extruder, melt-extruded at a resin temperature of 180°C, and cooled and solidified while being wound up on a chill roll through which a cooling liquid of 30°C had been passed, to obtain a new processing film with a thickness of 100 μm (process film J was 30 μm). The haze of the obtained remolded processing film was measured in the same manner as in the above-mentioned measurement method.
[0083] <Examples 2 to 5 and Comparative Examples 1 to 4> The evaluation was carried out in the same manner as in Example 1, except that the process film A was changed to the process films B to I.
[0084] <Comparative Example 5> The evaluation was performed in the same manner as in Example 1, except that the process film A was changed to the process film J, and the thickness of the process film after remolding in the evaluation of the haze after remolding was changed to 30 μm.
[0085] The evaluation results are shown in the following Table 3. The casting films of Examples 1 to 5 having the desired peel strength had a haze of 6.0% or less, and the absolute value of the difference between the haze and the haze of the casting film after remolding was 3.0% or less.
[0086] [Table 3] [Industrial Applicability]
[0087] The present invention can be used for protecting the surface of an optical film. [Explanation of symbols]
[0088] 1A...optical film with processing film, 1B...polarizing plate with processing film, 2...processing film, 3A...optical film, 3B...polarizing plate, 4...protective film, 5...adhesive layer, 6...polarizer, 7...laminate of sheets, 8...roll, 9...winding core.
Claims
1. The optical film and the process film having self-adhesive properties are included, the optical film and the process film are bonded to each other in contact with each other, The processing film comprises one kind of thermoplastic resin.
2. 2. The optical film with a process film according to claim 1, wherein the process film is a single layer.
3. 2. The optical film with a process film according to claim 1, wherein the process film comprises a plurality of layers.
4. The optical film with a processing film according to claim 1 , wherein the optical film is a polarizing plate.
5. the difference between the peel strength of one surface of the process film relative to the optical film and the peel strength of the other surface of the process film relative to the optical film is 0.02 N / 25 mm or more; 2. The optical film with a processing film according to claim 1, wherein the processing film is attached to the optical film such that the surface having a larger peel strength is in contact with the optical film.
6. 2. The optical film with a processing film according to claim 1, wherein the processing film has a peel strength from the optical film of a surface in contact with the optical film of 0.06 N / 25 mm or more.
7. 7. The optical film with a processing film according to claim 6, wherein the processing film has a peel strength from the optical film of a surface not in contact with the optical film of 0.04 N / 25 mm or less.
8. 8. The optical film with a casting film according to claim 1, wherein the casting film has a haze of 6.0% or less.
9. 2. The optical film with a processing film according to claim 1, wherein the thermoplastic resin comprises at least one copolymer selected from the group consisting of ethylene-α-olefin copolymers and ethylene-(meth)acrylate copolymers.
10. The density of the ethylene-α-olefin copolymer is 0.880 g / cm 3 0.915g / cm or more 3 The optical film with the processing film according to claim 9, wherein:
11. The density of the ethylene-(meth)acrylate copolymer is 0.935 g / cm 3 The optical film with the processing film according to claim 9 .
12. 10. The optical film with a processing film according to claim 9, wherein the ethylene-α-olefin copolymer comprises a copolymer derived from at least one selected from the group consisting of ethylene-1-hexene and ethylene-1-butene.
13. 10. The optical film with the processing film according to claim 9, wherein the ethylene-(meth)acrylate copolymer is an ethylene-methyl methacrylate copolymer.
14. 2. A roll comprising the optical film with the processing film according to claim 1 rolled up.
15. A method for producing the optical film with a process film according to claim 1, comprising the steps of: A process of subjecting one side of the film to a corona treatment; and laminating the process film and the optical film together with the one surface facing the optical film.
16. 16. The manufacturing method according to claim 15, wherein the peel strength of the process film on one side to the optical film before the corona treatment is 0.04 N / 25 mm or less, and the peel strength of the process film on one side to the optical film after the corona treatment is 0.06 N / 25 mm or more.
17. A method for producing a process film, comprising the steps of: A manufacturing method comprising a step of crushing the process film peeled off from the process film-attached optical film according to claim 1 and melt-extruding the crushed process film to form a new process film.
18. An optical film with a processing film, comprising an optical film and a processing film having self-adhesive properties, the processing film being manufactured by the manufacturing method according to claim 17, 18. An optical film with a process film, wherein the absolute value of the difference between the haze of the process film to be crushed in the manufacturing method according to claim 17 and the haze of the process film manufactured by the manufacturing method according to claim 17 is 3.0% or less.
Citation Information
Patent Citations
Anti-static surface protective film
JP2021006638A
Cited By
Polarizing laminate and optical lens
WO2025116030A1