Polyurethane foam for doll core material and manufacturing method of doll
A polyurethane foam with specific hardness and elongation properties addresses the issues of wool detachment and insertion in doll manufacturing, providing stable wool adherence and efficient production.
Patent Information
- Application Number
- JP2023049846
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing methods for manufacturing dolls using wool as core material face issues such as wool easily coming off and difficulty in inserting wool into core materials, particularly with expanded polystyrene and thermosetting foam sponge.
A polyurethane foam with a C hardness of 3 to 40 and tensile elongation at break of 30 to 200% is used as a core material, made by reacting a polyol component, preferably polyether polyol, with a polyisocyanate component, especially aromatic polyisocyanate, allowing easy adherence and retention of wool through needle implantation.
The polyurethane foam effectively adheres wool to the core material, preventing it from coming off, and facilitates efficient manufacturing of dolls by ensuring stable wool attachment.
Smart Images

Figure 2024139060000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a polyurethane foam for use as a core material for dolls and a method for producing dolls. [Background technology]
[0002] In recent years, there has been an increasing demand for dolls that resemble pet animals. Conventionally, a method for manufacturing such dolls involves cutting wool into a lump and molding it into a desired shape. This method requires a large amount of wool as it uses wool as the core material. In addition, skilled techniques are required to mold the doll into the desired shape, and it takes a long time to complete the process. Known methods of using core materials other than wool include, for example, a method of attaching wool to a polystyrene foam core material (see Patent Document 1), and a method of attaching felt-like wool to a thermosetting foam sponge core material by inserting a needle into the core material (see Patent Document 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Utility Model Registration No. 3090778 [Patent Document 1] JP 2012-249741 A Summary of the Invention [Problem to be solved by the invention]
[0004] The method described in Patent Document 1 has the problem that the wool easily comes off from the core material, while the method described in Patent Document 2 has the problem that it is difficult to pierce the core material with a needle, and the attached wool easily comes off from the core material. The object of the present invention is to provide a polyurethane foam for use as a core material for dolls, which allows easy application of wool to the core material and prevents the wool from falling out, and a method for producing a doll using said polyurethane foam. [Means for solving the problem]
[0005] The present inventors conducted extensive research to solve the above problems and arrived at the present invention. That is, the present invention is as follows. [1] A polyurethane foam for use as a core material for dolls, which is obtained by reacting a polyol component with a polyisocyanate component, and has a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%. [2] The polyurethane foam for doll core material described in [1], wherein the polyol component contains polyether polyol. [3] The polyurethane foam for doll core material according to [1] or [2], wherein the polyisocyanate component contains an aromatic polyisocyanate. [4] A method for manufacturing a doll using the polyurethane foam for a doll core material described in any one of [1] to [3], comprising a step of implanting felt-like wool into the core material made of the polyurethane foam with a needle. Effect of the Invention
[0006] According to the present invention, it is possible to provide a polyurethane foam for doll cores which allows wool to be easily attached to the core and prevents the attached wool from falling out, and a method for producing dolls using said polyurethane foam. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0007] <Polyurethane foam> The polyurethane foam of the present invention is a polyurethane foam obtained by reacting a polyol component with a polyisocyanate component. The polyurethane foam of the present invention has a C hardness of 3 to 40 and a tensile elongation at break of 30 to 200%.
[0008] Examples of the polyol component (A) that is a material for polyurethane foam include polyether polyol (A1) and polyester polyol (A2).
[0009] The polyether polyol (A1) may be a polyol obtained by adding an alkylene oxide to an active hydrogen-containing compound. Specific examples of the polyether polyol (A11) include a polyol obtained by adding an alkylene oxide (hereinafter also referred to as AO) to a polyhydric alcohol, a polyol (A12) obtained by adding an AO to an amine, and a polyol (A13) obtained by adding an AO to a polyhydric phenol.
[0010] Examples of the polyhydric alcohol (a1) constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol include dihydric alcohols having 2 to 20 carbon atoms, trihydric alcohols having 3 to 20 carbon atoms, and tetrahydric to octahydric alcohols having 5 to 20 carbon atoms. Examples of the dihydric alcohol having 2 to 20 carbon atoms include linear or branched aliphatic diols and alicyclic diols. Examples of the linear or branched aliphatic diols include alkylene glycols, specifically ethylene glycol, 1,2- or 1,3-propylene glycol, 1,3- or 1,4-butanediol, 1,6-hexanediol, and neopentyl glycol. Examples of the alicyclic diol include cycloalkylene glycols, and specific examples thereof include cyclohexanediol and cyclohexanedimethanol. Examples of trihydric alcohols having 3 to 20 carbon atoms include aliphatic triols, and specific examples thereof include glycerin, trimethylolpropane, trimethylolethane, and hexanetriol. Examples of the tetrahydric to octahydric polyalcohols having 5 to 20 carbon atoms include aliphatic polyols and sugars. Examples of the aliphatic polyols include alkane polyols such as pentaerythritol, sorbitol, mannitol, sorbitan, diglycerin, and dipentaerythritol, alkane triols, intramolecular dehydration products of alkane polyols, and intermolecular dehydration products of alkane triols and / or alkane polyols. Examples of the sugars include sucrose, glucose, mannose, fructose, methyl glucoside, and derivatives thereof.
[0011] The AO constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol preferably has 2 to 4 carbon atoms, and specific examples thereof include ethylene oxide (hereinafter sometimes abbreviated as EO), propylene oxide (hereinafter sometimes abbreviated as PO), and butylene oxide (hereinafter sometimes abbreviated as BO). PO and BO may be linear or branched. One type of AO may be used, or two or more types may be used. AO is preferably EO, PO, or a combination of PO and EO. When two or more types of AO are used in combination, the addition form may be block or random.
[0012] Examples of the amine (a2) constituting the polyol (A12) obtained by adding AO to an amine include ammonia, linear or branched aliphatic amines, aromatic amines, alicyclic amines, and heterocyclic amines, and those having 2 to 8 active hydrogens are preferred. Examples of linear or branched aliphatic amines include alkanolamines having 2 to 20 carbon atoms (monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, aminoethylethanolamine, etc.), alkylamines having 1 to 20 carbon atoms (n-butylamine, octylamine, etc.), alkylenediamines having 2 to 6 carbon atoms (ethylenediamine, propylenediamine, hexamethylenediamine, etc.), and polyalkylenepolyamines having 4 to 20 carbon atoms (those in which the alkylene group has 2 to 6 carbon atoms, specifically, diethylenetriamine, triethylenetetramine, etc.). Examples of the aromatic amine include aromatic amines having 6 to 20 carbon atoms (aniline, phenylenediamine, tolylenediamine, xylylenediamine, diethyltoluenediamine, methylenedianiline, diphenyletherdiamine, etc.). Examples of the alicyclic amine include alicyclic amines having 4 to 20 carbon atoms (such as isophoronediamine, cyclohexylenediamine, and dicyclohexylmethanediamine). Examples of the heterocyclic amine include heterocyclic amines having 4 to 20 carbon atoms (such as piperazine, aminoethylpiperazine, and those described in JP-B-55-21044). Examples of the AO constituting the polyol (A12) obtained by adding AO to an amine include the same AO as those constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol.
[0013] Examples of the polyhydric phenol (a3) constituting the polyol (A13) obtained by adding AO to a polyhydric phenol include monocyclic polyhydric phenols, bisphenols, condensates of phenol and formaldehyde (novolaks), polyphenols, and combinations of two or more of these. Examples of the monocyclic polyhydric phenols include pyrogallol, hydroquinone, and phloroglucinone. Examples of the bisphenols include bisphenol A, bisphenol F, and bisphenol sulfone. Examples of the polyphenols include those described in U.S. Pat. No. 3,265,641. Examples of the AO constituting the polyol (A13) obtained by adding an AO to a polyhydric phenol include the same AO as those constituting the polyol (A11) obtained by adding an AO to a polyhydric alcohol.
[0014] The polyether polyol (A1) is preferably a polyol (A11) obtained by adding AO to a polyhydric alcohol, more preferably a polyol obtained by adding AO to a dihydric to tetrahydric alcohol, and even more preferably a polyol obtained by adding AO to glycerin, a polyol obtained by adding AO to pentaerythritol, and a polyol obtained by adding AO to sorbitol.
[0015] Polyether polyol (A1) can be obtained by the reaction of adding AO to active hydrogen-containing compound, and the addition reaction can be carried out by a known method. The catalyst used when adding AO to active hydrogen-containing compound can be alkali catalyst (KOH, CsOH, etc.), catalyst described in JP-A-2000-344881 (tris(pentafluorophenyl)borane, etc.), catalyst described in JP-A-11-120300 (magnesium perchlorate, etc.).
[0016] Examples of the polyester polyol (A2) include polyester polyols (A21) of polyhydric alcohols and polycarboxylic acids or ester-forming derivatives thereof, condensation products (A22) of carboxylic anhydrides and AO, AO adducts (A23) of the polyester polyols (A21) or the condensation products (A22), polylactone polyols (A24), and polycarbonate polyols (A25).
[0017] Examples of the polyhydric alcohol constituting the polyester polyol (A21) of a polyhydric alcohol and a polycarboxylic acid or an ester-forming derivative thereof include the same polyhydric alcohols as the polyhydric alcohols (a1) constituting the polyol (A11). Examples of the polycarboxylic acids and ester-forming derivatives constituting the polyester polyol (A21) include polycarboxylic acids such as aliphatic polycarboxylic acids having 4 to 18 carbon atoms (e.g., succinic acid, adipic acid, sebacic acid, glutaric acid, azelaic acid, etc.), aromatic polycarboxylic acids having 8 to 18 carbon atoms (e.g., terephthalic acid, isophthalic acid, orthophthalic acid, trimellitic acid, pyromellitic acid), and alicyclic polycarboxylic acids having 8 to 15 carbon atoms (e.g., cyclohexane-1,4-dicarboxylic acid, etc.); acid anhydrides such as maleic anhydride and phthalic anhydride; and lower alkyl esters (wherein the alkyl group has 1 to 4 carbon atoms) such as dimethyl terephthalate.
[0018] The carboxylic anhydride constituting the condensation reaction product (A22) of the carboxylic anhydride and AO may be the same as the acid anhydride described in the polyester polyol (A21). The AO constituting the condensation reaction product (A22) of the carboxylic anhydride and AO may be the same as the AO constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol.
[0019] Examples of the AO constituting the polyester polyol (A21) or the AO adduct (A23) of the condensation reaction product (A22) include the same AO constituting the polyol (A11) and the like.
[0020] The polylactone polyol (A24) may be one obtained by ring-opening polymerization of lactone (e.g., ε-caprolactone) using a polyhydric alcohol as an initiator. The polyhydric alcohol constituting the polylactone polyol (A24) may be the same as the polyhydric alcohol (a1) constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol.
[0021] The polycarbonate polyol (A25) may be a reaction product of a polyhydric alcohol and an alkylene carbonate, etc. The polyhydric alcohol constituting the polycarbonate polyol (A25) may be the same as the polyhydric alcohol (a1) constituting the polyol (A11) obtained by adding AO to a polyhydric alcohol.
[0022] As the polyester polyol (A2), polyester polyols of natural origin may be used, such as those containing castor oil, castor oil derivatives, and mixtures thereof.
[0023] The polyol component (A) may contain a polyol other than the polyether polyol (A1) and the polyester polyol (A2). Examples of the polyol other than (A1) and (A2) include a polyhydric alcohol (A3) having no polyoxyalkylene unit, a polymer polyol (A4), and an AO adduct of an amine (A5).
[0024] Examples of the polyhydric alcohol (A3) having no polyoxyalkylene unit include the same as the polyhydric alcohol (a1) constituting the polyol (A11).
[0025] Examples of the polymer polyol (A4) include those obtained by polymerizing an ethylenically unsaturated monomer (p) in a polyol in the presence of a radical polymerization initiator, and dispersing the polymer particles in the polyol. Such polymer polyols are preferred in terms of dispersion stability, and can be obtained by the methods described in, for example, U.S. Patent No. 3,383,351 and Japanese Patent Publication No. 39-25737.
[0026] Examples of the polyol used in the production of the polymer polyol (A4) include polyether polyol (A1), polyester polyol (A2) and polyhydric alcohol (A3) having no polyoxyalkylene unit.
[0027] As the radical polymerization initiator used in the production of the polymer polyol (A4), one that generates free radicals to initiate polymerization can be used, and examples of such initiators include azo compounds [2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(2-methylbutyronitrile)], organic peroxides [dibenzoyl peroxide, dicumyl peroxide, benzoyl peroxide, lauroyl peroxide, and persuccinic acid], and inorganic peroxides [persulfates, perborates, and the like]. These may be used alone or in combination of two or more.
[0028] Examples of the ethylenically unsaturated monomer used in the production of the polymer polyol (A4) include unsaturated nitriles (p1), aromatic ring-containing monomers (p2), (meth)acrylic acid esters (p3), and other ethylenically unsaturated monomers (p4), etc. These monomers may be used alone or in combination of two or more. Examples of the (p1) include acrylonitrile and methacrylonitrile. Examples of the (p2) include styrene, α-methylstyrene, hydroxystyrene, and chlorostyrene. Examples of (p3) include those composed of C, H and O atoms, such as (meth)acrylic acid alkyl esters (alkyl group having 1 to 24 carbon atoms) [methyl (meth)acrylate, butyl (meth)acrylate, nonyl (meth)acrylate, decyl (meth)acrylate, dodecyl (meth)acrylate, eicosyl (meth)acrylate, docosyl (meth)acrylate, etc.], hydroxyalkyl (carbon number: 2 to 5) (meth)acrylates [hydroxyethyl (meth)acrylate, etc.] and hydroxypolyoxyalkylene mono(meth)acrylates [alkylene group having 2 to 4 carbon atoms, polyoxyalkylene chain having number average molecular weight of 200 to 1000, etc.]. Examples of (p4) include ethylenically unsaturated carboxylic acids and derivatives thereof [(meth)acrylic acid, (meth)acrylamide, etc.], aliphatic or alicyclic hydrocarbon monomers [alkene (ethylene, propylene, norbornene, etc.) and alkadienes (butadiene, etc.)], fluorine-based vinyl monomers [fluorine-containing (meth)acrylates (perfluorooctylethyl methacrylate, perfluorooctylethyl acrylate, etc.)], chlorine-based vinyl monomers (vinylidene chloride, etc.), nitrogen-containing vinyl monomers other than (meth)acrylamide [nitrogen-containing (meth)acrylates (diaminoethyl methacrylate, morpholinoethyl methacrylate, etc.)], and vinyl-modified silicones. Among these, from the viewpoint of moldability, the above (p1) and (p2) are preferred, and acrylonitrile and / or styrene are more preferred.
[0029] The weight ratios of the (p1), (p2), (p3) and (p4) in the ethylenically unsaturated monomers can be changed depending on the required physical properties of the polyurethane, and are not particularly limited. An example is as follows. Based on the total weight of (p), the (p1) and / or (p2) is preferably 50 to 100% by weight, more preferably 80 to 100% by weight. The weight ratio of (p1) to (p2) is not particularly limited, but is preferably 100 / 0 to 20 / 80. The (p3) is preferably 0 to 50% by weight, more preferably 0 to 20% by weight, based on the total weight of (p). The (p4) is preferably 0 to 10% by weight, more preferably 0 to 5% by weight.
[0030] The content of the ethylenically unsaturated monomer in the polymer polyol (A4) is preferably 50% by weight or less, more preferably 3 to 30% by weight, based on the weight of (A4) from the viewpoint of moldability.
[0031] The amine constituting the AO adduct of amine (A5) includes ammonia, linear or branched aliphatic amines, aromatic amines, alicyclic amines and heterocyclic amines, and those having 2 to 8 active hydrogens are preferred. Examples of linear or branched aliphatic amines include alkanolamines having 2 to 20 carbon atoms (monoethanolamine, diethanolamine, triethanolamine, isopropanolamine, aminoethylethanolamine, etc.), alkylamines having 1 to 20 carbon atoms (n-butylamine, octylamine, etc.), alkylenediamines having 2 to 6 carbon atoms (ethylenediamine, propylenediamine, hexamethylenediamine, etc.), and polyalkylenepolyamines having 4 to 20 carbon atoms (those in which the alkylene group has 2 to 6 carbon atoms, specifically, diethylenetriamine, triethylenetetramine, etc.). Examples of the aromatic amine include aromatic amines having 6 to 20 carbon atoms (aniline, phenylenediamine, tolylenediamine, xylylenediamine, diethyltoluenediamine, methylenedianiline, diphenyletherdiamine, etc.). Examples of the alicyclic amine include alicyclic amines having 4 to 20 carbon atoms (such as isophoronediamine, cyclohexylenediamine, and dicyclohexylmethanediamine). Examples of the heterocyclic amine include heterocyclic amines having 4 to 20 carbon atoms (such as piperazine, aminoethylpiperazine, and those described in JP-B-55-21044).
[0032] In addition to (A1) to (A5), the polyol component (A) may include polydiene polyols such as polybutadiene polyols and hydrogenated products thereof; acrylic polyols (hydroxyl group-containing vinyl polymers described in JP-A-58-57413 and JP-A-58-57414, etc.); natural fat-and-oil based polyols such as castor oil; modified products of natural fat-and-oil based polyols such as castor oil modified products (polyhydric alcohol transesterification products, hydrogenated products, etc.); active hydrogen compounds (including mono-ols) containing terminal radically polymerizable functional groups described in International Publication WO98 / 44016; modified polyols obtained by jump-splitting polyether polyols with alkylene dihalides such as methylene dihalide; OH-terminated prepolymers of polyether polyols; and the like.
[0033] The polyol component (A) preferably contains a polyether polyol (A1) from the viewpoint of facilitating the preparation of a polyurethane foam having a C hardness of 3 to 40 and a tensile elongation at break of 30 to 200%.
[0034] From the viewpoint of facilitating the preparation of a polyurethane foam having a C hardness of 3 to 40 and a tensile elongation at break of 30 to 200%, the polyol component (A) preferably contains a polyol having a number average molecular weight Mn of 400 to 10,000, more preferably a polyol having an Mn of 700 to 8,000, and even more preferably a polyol having an Mn of 1,000 to 7,000.
[0035] The content of oxyethylene units based on the total weight of the polyol component (A) is preferably 0 to 70% by weight, more preferably 0 to 40% by weight, and further preferably 5 to 25% by weight, from the viewpoint of moldability and productivity of polyurethane foam. The content of oxyethylene units contained in the component (A) is calculated from the weight ratio of oxyethylene units contained in the component (A). Methods for adjusting the content of oxyethylene units contained in the component (A) within the above range include adjusting the amount of EO charged when producing the polyol having EO used as the component (A) and adjusting the amount of the polyol having EO used.
[0036] The polyisocyanate component (B) constituting the polyurethane foam of the present invention includes divalent or higher (preferably divalent to octavalent) organic polyisocyanates. Specific examples thereof include aromatic polyisocyanates, linear or branched aliphatic polyisocyanates, alicyclic polyisocyanates, araliphatic polyisocyanates, and modified products thereof.
[0037] Examples of aromatic polyisocyanates include aromatic diisocyanates having 6 to 16 carbon atoms excluding the carbon in the NCO group (this also applies to the following polyisocyanates), aromatic triisocyanates having 6 to 20 carbon atoms, and crude products of these isocyanates, such as 2,4- or 2,6-tolylene diisocyanate (hereinafter abbreviated as TDI), 1,3- or 1,4-phenylene diisocyanate, 2,4'- or 4,4'-diphenylmethane diisocyanate (hereinafter abbreviated as MDI), polymethylene polyphenylene polyisocyanate (crude MDI), naphthylene-1,5-diisocyanate, and triphenylmethane-4,4',4''-triisocyanate.
[0038] The linear or branched aliphatic polyisocyanate is, for example, a linear or branched aliphatic diisocyanate having 6 to 10 carbon atoms, such as 1,6-hexamethylene diisocyanate, 2,2,4-trimethylhexamethylene diisocyanate, and lysine diisocyanate.
[0039] The alicyclic polyisocyanate is an alicyclic diisocyanate having 6 to 16 carbon atoms, such as isophorone diisocyanate, 4,4'-dicyclohexylmethane diisocyanate, 1,4-cyclohexane diisocyanate, and norbornane diisocyanate.
[0040] The aralkyl polyisocyanate is an aralkyl diisocyanate having 8 to 12 carbon atoms, such as xylylene diisocyanate and α,α,α',α'-tetramethylxylylene diisocyanate.
[0041] The modified polyisocyanate includes modified products containing a urethane group, a carbodiimide group, an allophanate group, a urea group, a biuret group, an isocyanurate group, and an oxazolidone group, and examples thereof include carbodiimide-modified MDI.
[0042] From the viewpoint of productivity of polyurethane foam, the polyisocyanate component (B) is preferably an aromatic polyisocyanate, more preferably MDI, crude MDI, or modified products of these isocyanates. The polyisocyanate component (B) may be used alone or in combination of two or more kinds.
[0043] The isocyanate group content (NCO%) of the polyisocyanate component (B) as a whole is preferably from 20 to 50% from the viewpoint of moldability of the polyurethane foam.
[0044] The isocyanate index [(number of NCO groups / number of OH groups in polyol)×100] in producing a polyurethane foam is preferably 50 to 300, more preferably 70 to 150, and even more preferably 90 to 110, from the viewpoint of moldability of the polyurethane foam.
[0045] The polyurethane foam of the present invention has a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%. By having a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%, it is possible to provide a polyurethane foam for doll core material that allows wool to be easily attached to the core material and prevents the attached wool from coming off. If the resilience modulus is outside the above range and / or if the tensile breaking elongation is outside the above range, the attached wool may easily come off.
[0046] The C hardness of polyurethane foam can be measured by a method using an Asker rubber hardness tester type C specified in JIS K7312, and the tensile breaking elongation of polyurethane foam can be measured by a method for measuring tensile strength specified in JIS K6400-5. From the viewpoints of facilitating adhesion of wool to the core material and preventing the wool from coming off, the polyurethane foam has a C hardness of preferably 5 to 35, more preferably 10 to 30. From the viewpoints of facilitating adhesion of wool to the core material and preventing the wool from coming off, the polyurethane foam has a tensile breaking elongation of preferably 50 to 160%, more preferably 70 to 120%.
[0047] A polyurethane foam having a C hardness of 3 to 40 and a tensile elongation at break of 30 to 200% can be obtained, for example, by adjusting the type and amount of the polyol component (A) and the type and amount of the polyisocyanate component (B). It can be easily prepared by using at least one member selected from the group consisting of polyether polyol (A1) and polyester polyol (A2) and using an aromatic polyisocyanate as the polyisocyanate component (B).
[0048] The polyurethane foam of the present invention can be produced by a process comprising the steps of: preparing a composition for producing polyurethane foam comprising a polyol component (A) and a polyisocyanate component (B) (step 1); and reacting the composition (step 2).
[0049] The content of the polyol component (A) in the composition for producing polyurethane foam is preferably 40 to 90% by weight, more preferably 50 to 80% by weight, based on the total weight of the composition. The content of the polyisocyanate component (B) in the composition for producing polyurethane foam is preferably 10 to 60% by weight, more preferably 20 to 50% by weight, based on the total weight of the composition.
[0050] The composition for producing polyurethane foam may contain components other than the polyol component (A) and the polyisocyanate component (B). Such components include a catalyst component (C), a blowing agent (D), a foam stabilizer (E), and auxiliary components (F) other than the above. Each of these may be used alone or in combination of two or more.
[0051] Examples of the catalyst component (C) include tertiary amines, carboxylates of tertiary amines, metal carboxylates, and organometallic compounds. The catalyst component (C) may be used alone or in combination of two or more.
[0052] Examples of tertiary amines and tertiary amine carboxylates include triethylenediamine, N-ethylmorpholine, diethylethanolamine, N,N,N',N'-tetramethylhexamethylenediamine, 1,2-dimethylimidazole, 1-isobutyl-2-methylimidazole, 1,8-diazabicyclo-[5,4,0]-undecene-7 (carboxylate) and bis(dimethylaminoethyl)ether (carboxylate), and polyamines obtained by polycondensation of methylamine and linear or branched diol having 4 to 8 carbon atoms ("Kao Raiser P200" manufactured by Kao Corporation). Examples of the metal carboxylate include potassium acetate, potassium octoate, and stannous octoate. Examples of the organometallic compounds include stannous octoate, dibutyl stannous dilaurate, and lead octoate.
[0053] The content of catalyst component (C) in the composition for producing polyurethane foam is preferably 0 to 5% by weight, more preferably 0.1 to 2.5% by weight, from the viewpoint of production efficiency and the like.
[0054] The blowing agent (D) preferably contains water, more preferably only water. The content of the blowing agent (D) is preferably 0.1 to 5.0% by weight, more preferably 0.5 to 4.0% by weight, based on the weight of the polyol component (A). When water is used as the blowing agent (D), hydrogen atom-containing halogenated hydrocarbons, low boiling point hydrocarbons, liquefied carbon dioxide gas, etc. may be used in combination, if necessary.
[0055] As the foam stabilizer (E), any known foam stabilizer used in the production of polyurethane foams can be used, and preferred examples include silicone foam stabilizers. Examples of silicone foam stabilizers include polyether-modified dimethylsiloxane foam stabilizers ("SZ-1328", "SZ-1346", and "SF-2962" manufactured by Dow Toray Industries, Inc., and "L-3640" manufactured by Momentive Performance Materials, Inc.), and dimethylsiloxane foam stabilizers ("TEGOSTAB B8738LF2" and "TEGOSTAB B8715LF2" manufactured by EVONIK, etc.). The amount of the foam stabilizer (E) used is preferably 3% by weight or less, and more preferably 2% by weight or less, based on the total weight of the polyol component (A) from the viewpoint of moldability.
[0056] Examples of the auxiliary component (F) include colorants, flame retardants, age resistors, and antioxidants. Examples of the colorants include dyes and pigments. Examples of the flame retardants include phosphate esters and halogenated phosphate esters. Examples of the age resistors include triazole-based and benzophenone-based age resistors. Examples of the antioxidants include hindered phenol-based and hindered amine-based antioxidants. The amounts of these auxiliary components used are, based on the weight of the polyol component (A), preferably 5.0% by weight or less of the colorant from the viewpoints of curability and the mechanical properties of the polyurethane foam, preferably 30% by weight or less of the flame retardant from the viewpoints of curability and the mechanical properties of the polyurethane foam, and more preferably 15% by weight or less of the antioxidant from the viewpoints of curability and the mechanical properties of the polyurethane foam, and more preferably 2.0% by weight or less of the antioxidant from the viewpoints of curability and the mechanical properties of the polyurethane foam, and more preferably 1.0% by weight or less of the antioxidant.
[0057] The composition for producing polyurethane foam can be prepared by mixing the polyol component (A) and the polyisocyanate component (B) as well as the components added as required [catalyst component (C), blowing agent (D), foam stabilizer (E) and auxiliary component (F)] by a known method such as using a mixing vessel equipped with a stirrer. There is no restriction on the order of mixing these components, but it is preferable to prepare a polyol composition containing the polyol component (A) and the components added as required, and to obtain the composition for producing polyurethane foam by mixing the obtained polyol composition with the polyisocyanate component (B).
[0058] The step of reacting the composition for producing a polyurethane foam (step 2) can be carried out in a mold. The mold used may be one having a desired shape, or one having an undesired shape. When a mold having an undesired shape is used, a step of cutting the polyurethane foam obtained in step 2 into the desired shape to prepare a core material may be carried out.
[0059] The polyurethane foam of the present invention has a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%, so that it is easy to cover the core with wool and the covered wool is unlikely to come off, making it suitable for use as a core for wool dolls. In the present invention, the "doll" includes those in the shape of a human being, those in the shape of an animal, etc.
[0060] The method for producing a doll using the polyurethane foam of the present invention includes a step of tufting felt-like wool with a needle into a core material made of the polyurethane foam of the present invention.
[0061] The core material may be the polyurethane foam of the present invention as it is, or may be prepared by cutting the polyurethane foam of the present invention into a desired shape. The process of implanting felt-like wool into the core material with a needle can be carried out, for example, by wrapping small pieces of wool fiber around the surface of the core material while penetrating the inside of the core material with a needle to adhere it in a felt-like form (see JP 2012-249641 A). EXAMPLES
[0062] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0063] <Examples 1 to 4, Comparative Example 3> A polyol composition was prepared by mixing the components listed in Table 1 except for the polyisocyanate component (B), to which the amount of polyisocyanate component (B) listed in Table 1 was added so that the NCO index was 100. The mixture was stirred for 8 seconds at 4000 rpm using a Homo Disper (a mixer manufactured by Tokushu Kika Co., Ltd.), and then the mixture was poured into an aluminum mold measuring 300 mm (length) × 300 mm (width) × 100 mm (height) and thermostated at 40°C, and molded with a cure time (the time from pouring in the raw materials to demolding) of 3 minutes. In Table 1, "composition for producing polyurethane foam" is described as "polyurethane foam composition."
[0064] <Comparative Example 1> The core material of Comparative Example 1 was made of polystyrene foam. The polystyrene foam used was a commercially available product (manufactured by Daiso Industries Co., Ltd., product name: polystyrene foam brick (white)).
[0065] <Comparative Example 2> A commercially available wool mat (made of polyethylene, manufactured by Daiso Industries Co., Ltd., product name: Starter Set for Wool Felt) was used as Comparative Example 2.
[0066] <Evaluation method> (Preparation of evaluation samples) For each core material, a rectangular parallelepiped sample measuring 9 cm in length, 5 cm in width, and 2 cm in thickness was cut out and used as an evaluation sample. (Measurement of physical properties of core material) The C hardness and tensile elongation at break of the evaluation samples of the examples and comparative examples were measured. The C hardness was measured by the method specified in JIS K7312 using an Asker rubber hardness tester type C, and the tensile breaking elongation was measured by the method specified in JIS K6400-5.
[0067] (Evaluation of needle penetration; measurement of needle penetration length (mm) required to break through a surface) A sample for evaluation was prepared, a wool felt needle (size: extra fine, manufactured by HJ Co.) was held in the hand, and the needle was slowly inserted into the surface of the foam at a 45° angle. When it felt like the needle had broken through the surface, the hand was stopped and the length of the needle tip that had penetrated into the foam at that point was measured with a ruler. The test was performed three times, and the average value was recorded in the table as the needle penetration length (mm). The shorter the needle length required to penetrate the surface, the easier it is felt to penetrate the foam, and so the shorter the measured needle penetration length (mm) the easier it is to penetrate the foam.
[0068] (Evaluation of the resistance of implanted hair (transplanted hair) to falling out) (1) Measurement of maximum tensile load (g) of grafted hair (1-1) Hair transplantation Wool felt (Wool Full Feel Natural Color 84, Fujikyu Co., Ltd.) was cut to a length of 4 cm and divided into 0.05 g portions. A 1 cm long line was drawn on the evaluation sample of each example with an oil-based marker, and a bundle of divided wool felt pieces was placed on top so that the center of the bundle (a part 2 cm long from the tip of the wool) was on the marker line. A wool felt needle (size: extra fine, HJ Co., Ltd.) was pierced 50 times along the marker line to implant the wool felt into the evaluation sample. (1-2) Measurement of maximum tensile load (g) The wool was clipped with a paper clip and attached to the hook of a digital hanging scale (BDS-H50K, manufactured by Ito Co., Ltd.) fixed with a clamp, and the foam was slowly pulled to read the maximum tensile load (g) applied to the flock. The test was carried out three times, and the average value was calculated as the maximum tensile load (g) of the flock. The results are shown in the table. The greater the maximum tensile load (g) of the flock, the less likely it is to fall out.
[0069] (2) Method for evaluating remaining hair grafts For the evaluation samples after the measurement of the maximum tensile load (g) in (1-2) above, the percentage of hairs remaining [amount of hairs remaining in the sample after (1-2) / amount of hairs in the sample after (1-1) and before (1-2)] was visually judged and evaluated according to the following criteria. The evaluation was performed three times, and the result with the highest percentage of hairs remaining was recorded as the result of this evaluation in the table (for example, if the result was ◎, ◯, or ×, ◎ was recorded). A higher percentage of hairs remaining is preferable. ◎: The percentage of hair that remains is more than 1 / 2 〇: The percentage of hair grafts remaining is more than 1 / 3, but less than 1 / 2 △: The percentage of hair grafts remaining is more than 1 / 10 and less than 1 / 3 ×: The percentage of remaining grafted hair is 1 / 10 or less
[0070] Each component listed in Table 1 is described below. <Polyol component (A)> (A-1): A block-addition type polyoxyethylene propylene polyol obtained by adding 85.3 moles of PO to 1 mole of glycerin using potassium hydroxide as a catalyst (catalyst amount 0.3% by weight (based on the weight of the reaction product)) at a reaction temperature of 95°C to 130°C, then adding 21.8 moles of EO, and then removing the potassium hydroxide by a conventional method. Hydroxyl value 28.0, terminal EO unit content 16%. (A-2): A block-addition type polyoxyethylene propylene polyol obtained by adding 67.4 moles of PO to 1 mole of glycerin using potassium hydroxide as a catalyst (catalyst amount 0.3% by weight (based on the weight of the reaction product)) at a reaction temperature of 95°C to 130°C, then adding 22.7 moles of EO, and then removing the potassium hydroxide by a conventional method. Hydroxyl value 33.5, terminal EO unit content 20%. (A-3): A random addition type polyoxyethylene propylene polyol obtained by reacting 1 mole of glycerin with a mixture of 34.6 moles of PO and 111.4 moles of EO at a reaction temperature of 95°C to 130°C using potassium hydroxide as a catalyst, and then removing the potassium hydroxide by a conventional method. Functionality 3.0, hydroxyl value 24, EO content 70%. (A-4): A polyoxypropylene polyol obtained by adding 8.7 moles of PO to 1 mole of sorbitol using potassium hydroxide as a catalyst (amount of catalyst used: 0.3% by weight (based on the weight of the reaction product)) at a reaction temperature of 95°C to 130°C, and then removing the potassium hydroxide by a conventional method. Functionality: 6.0, hydroxyl value: 490, EO content: 0%. (A-5): A polymer polyol obtained by copolymerizing acrylonitrile and styrene in a polymerization ratio of 7:3 in a block-addition type polyoxyethylene polyoxypropylene polyol (functionality 3.0, hydroxyl value 34.0, terminal EO unit content 14.0%) obtained by adding 72.6 mol of PO and then 15.9 mol of EO to 1 mol of glycerin at a reaction temperature of 95°C to 130°C using potassium hydroxide as a catalyst, and then removing the potassium hydroxide by a conventional method. Polymer content 32%, hydroxyl value 22.0. (A-6): A polyoxypropylene polyol obtained by adding 7.2 moles of PO to 1 mole of pentaerythritol using potassium hydroxide as a catalyst (amount of catalyst used: 0.3% by weight (based on the weight of the reaction product)) at a reaction temperature of 95°C to 130°C, and then removing the potassium hydroxide by a conventional method. Functional group number: 4.0, hydroxyl value: 404, EO unit content: 0%
[0071] <Catalyst component (C)> (C-1): "DABCO NE1070" manufactured by Evonik: an aliphatic tertiary amine composition. (C-2): "DABCO NE300" manufactured by Evonik: an aliphatic tertiary amine composition. (C-3) Polyamine obtained by polycondensation of methylamine and 1,6-hexanediol (Kao Corporation, "Kao Raiser P200") <Crosslinking agent>: Triethanolamine <Foaming agent (D)> (D-1):Water <Foam stabilizer> (E-1): Evonik "TEGOSTAB B8715LF2" <Polyisocyanate component (B)> (B-1): Modified MDI "CEF-403" manufactured by Tosoh Corporation, NCO%=28.2
[0072] [Table 1]
[0073] According to the examples using a core material made of polyurethane foam with a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%, the needle penetration length was longer and the maximum tensile load of the hair was larger than those of the comparative examples. As a result, it was found that the polyurethane foam of the present invention can provide a urethane foam for doll core material that makes it easy to attach wool to the core material and prevents the attached wool from falling out.
Claims
1. A polyurethane foam obtained by reacting a polyol component with a polyisocyanate component, The polyurethane foam for use as a core material for dolls has a C hardness of 3 to 40 and a tensile breaking elongation of 30 to 200%.
2. 2. The polyurethane foam for doll cores according to claim 1, wherein said polyol component comprises a polyether polyol.
3. 3. The polyurethane foam for use as a doll core material according to claim 1, wherein the polyisocyanate component comprises an aromatic polyisocyanate.
4. A method for manufacturing a doll using the polyurethane foam for doll core material according to claim 1 or 2, comprising the steps of: The method for manufacturing a doll includes a step of using a needle to implant felt-like wool into the core material made of polyurethane foam.
Citation Information
Patent Citations
Felt doll, core member sheet for manufacturing felt doll, and method of manufacturing felt doll
JP2012249741A
Animal mascot toys
JP3090778U