Laminate and method for manufacturing the same
A laminate with a polycarbonate resin layer and a cured active energy ray-curable resin layer addresses adhesion and weather resistance issues, providing enhanced scratch resistance and hardness for diverse applications.
Patent Information
- Application Number
- JP2023049917
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing laminates with hard coat layers on polycarbonate resins suffer from inadequate adhesion, weather resistance, and scratch resistance, despite improvements in surface hardness.
A laminate structure comprising a polycarbonate resin layer with a specific structural unit derived from a dihydroxy compound and a layer formed by curing an active energy ray-curable resin composition containing mono- or polypentaerythritol poly(meth)acrylate and trifunctional or higher functional urethane (meth)acrylate, with optional additives for enhanced adhesion and weather resistance.
The laminate achieves excellent surface hardness, scratch resistance, and adhesion between layers, along with improved weather resistance, suitable for various applications including automotive components and medical products.
Smart Images

Figure 2024139115000001 
Figure 2024139115000002 
Figure 2024139115000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having a layer obtained by curing an active energy ray-curable resin composition on a substrate such as a film, sheet or molded article made of a polycarbonate resin, and to a method for producing the same. [Background technology]
[0002] Polycarbonate resins are excellent in transparency, heat resistance and mechanical strength, and are therefore widely used in the fields of automobile parts, medical parts, containers such as films, sheets and bottles, building materials, various housing materials for mobile phones and the like, optical disc substrates and plastic lenses.
[0003] However, polycarbonate resin has a drawback that it is easily scratched because its surface hardness is lower than that of glass, and the inherent transparency or appearance of the resin is significantly impaired, making it difficult to use plastic substrates in fields that require scratch resistance. Therefore, in order to solve the abrasion resistance of the surface of these polycarbonate resins, it has been proposed to obtain a polycarbonate resin with high surface hardness by using isosorbide and carrying out an ester exchange reaction with diphenyl carbonate (Patent Document 1). Also, a method has been proposed to obtain a polycarbonate resin by copolymerizing isosorbide with an alicyclic dihydroxy compound (Patent Document 2).
[0004] However, although these polycarbonate resins have excellent optical properties, processability, mechanical properties, and light resistance, their scratch resistance is not satisfactory. A laminate having a hard coat layer laminated thereon has been proposed to improve the scratch resistance of these polycarbonate resins (Patent Documents 3 to 4). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent No. 6349866 [Patent Document 2] JP 2008-24919 A [Patent Document 3] JP 2009-102537 A [Patent Document 4] JP 2016-68438 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, although the laminates described in Patent Documents 3 and 4 have improved surface hardness and scratch resistance due to the hard coat layer, the adhesion after a weather resistance test was insufficient.
[0007] An object of the present invention is to provide a laminate that is excellent in surface hardness, scratch resistance, adhesion between a substrate and a hard coat layer, and weather resistance, and a method for producing the same. [Means for solving the problem]
[0008] As a result of intensive research aimed at solving the above problems, the present inventors have found that a laminate having the configuration of the present invention can solve the above problems. That is, the present invention is as follows. [1] A laminate having a layer A containing a polycarbonate resin and a layer B obtained by curing an active energy ray-curable resin composition, wherein at least one of the outermost layers is the layer B, The polycarbonate resin has a structural unit (a) derived from a dihydroxy compound having a structure represented by the following general formula (1): The active energy ray-curable resin composition contains a mono- or polypentaerythritol poly(meth)acrylate (c) represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d), A laminate, wherein a ratio of the mono- or polypentaerythritol poly(meth)acrylate (c) is 10 to 90 mass% and a ratio of the urethane (meth)acrylate compound (d) is 10 to 90 mass% relative to the total mass of the active energy ray-curable compound in the active energy ray-curable resin composition.
[0009] [ka]
[0010] [ka]
[0011] [In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., a group represented by CH2=CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH2=CR-CO(O(CH2)5C=O) y -O-, R represents a hydrogen atom or a methyl group, and y represents an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.]
[0012] [2] The laminate according to [1], wherein the urethane (meth)acrylate compound (d) is a urethane (meth)acrylate compound having a nurate skeleton. [3] The laminate according to [1] or [2], wherein at least one of X in the formula (2) is a (meth)acryloyloxy group modified with caprolactone.
[0013] [4] The laminate according to any one of [1] to [3], wherein the active energy ray-curable resin composition contains at least one of an ultraviolet absorber (e) and a hindered amine-based light stabilizer (f). [5] The laminate according to any one of [1] to [4], which is used as an automobile component. [6] A method for producing a laminate having a layer A containing a polycarbonate resin and a layer B obtained by curing an active energy ray-curable resin composition, wherein at least one of the outermost layers is the layer B, and applying the active energy ray-curable resin composition onto at least one surface of the layer A, and then irradiating the active energy ray to form the layer B. The polycarbonate resin has a structural unit (a) derived from a dihydroxy compound having a structure represented by the following general formula (1): The active energy ray-curable resin composition contains a mono- or polypentaerythritol poly(meth)acrylate (c) represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d), A method for producing a laminate, wherein a proportion of the mono- or polypentaerythritol poly(meth)acrylate (c) is 10 to 90 mass% and a proportion of the urethane (meth)acrylate compound (d) is 10 to 90 mass% relative to a total mass of the active energy ray-curable compounds in the active energy ray-curable resin composition.
[0014] [ka]
[0015] [ka]
[0016] [In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., a group represented by CH2=CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH2=CR-CO(O(CH2)5C=O) y -O-, R represents a hydrogen atom or a methyl group, and y represents an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.] Effect of the Invention
[0017] According to the present invention, a laminate can be obtained which has excellent surface hardness, scratch resistance, adhesion between the substrate (layer A) and the hard coat (layer B), and weather resistance, and it is possible to provide resin molded products which can be used in a wide range of fields, such as automobile parts, medical parts, films, sheets, containers such as bottles, building materials, various housing materials for smartphones, optical disc substrates, and plastic lenses. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0018] The following describes in detail the embodiments of the present invention. However, the following description of the components is a representative example of the embodiment of the present invention, and the present invention is not limited to these contents. In this specification, the term "(meth)acryloyl group" is a general term for acryloyl group and methacryloyl group. The same applies to "(meth)acryl" and "(meth)acrylate". In addition, in this specification, a numerical range expressed by "to" includes the numerical values before and after it as the lower limit and upper limit.
[0019] 1.Laminate The laminate of the present invention is a laminate having a layer (layer A) containing the specific polycarbonate resin described below, and a layer (layer B) formed by curing a specific active energy ray-curable resin composition. The layer A is a layer containing a polycarbonate resin having a structural unit (a) derived from a dihydroxy compound having a structure represented by the following general formula (1) (hereinafter, sometimes referred to as "dihydroxy compound (1)").
[0020] [ka]
[0021] The layer B is a layer obtained by curing an active energy ray-curable resin composition containing mono- or polypentaerythritol poly(meth)acrylate (c) represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d).
[0022] [ka]
[0023] In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., a group represented by CH2=CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH2=CR-CO(O(CH2)5C=O) y It is a group represented by -O-, where R represents a hydrogen atom or a methyl group, and y represents an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.
[0024] The layer A in the laminate of the present invention may have any desired form and shape, and examples thereof include a film, a sheet, or a molded article.
[0025] In the laminate of the present invention, in order to obtain the effects of the present invention, such as surface chemical resistance and scratch resistance, at least one of the outermost layers must be layer B. There are no particular limitations on the arrangement of layers A and B. Each layer may be formed adjacent to the other layers, or may have another layer between the layers, such as a primer layer, which further improves adhesion.
[0026] 2.A layer The polycarbonate resin (A) constituting the layer A has a structural unit (a) derived from a dihydroxy compound (1), and preferably further has a structural unit (b) derived from a dihydroxy compound other than the dihydroxy compound (1).
[0027] (1) Polycarbonate resin and polycarbonate resin composition based on the same The polycarbonate resin for obtaining the laminate of the present invention and the polycarbonate resin composition based thereon will be described in detail below.
[0028] [Polycarbonate resin] <Raw materials> (Dihydroxy compound (1)) The polycarbonate resin used in the present invention (hereinafter sometimes referred to as "polycarbonate resin (A)") contains a structural unit (a) derived from a dihydroxy compound (1) in at least a part of its structure.
[0029] Dihydroxy compounds (1) include isosorbide, isomannide, and isoidite, which are stereoisomers. Of these dihydroxy compounds (1), isosorbide, which is abundant and easily available as a resource and is obtained by dehydration condensation of sorbitol produced from various starches, is most preferred in terms of availability, ease of production, and moldability. These dihydroxy compounds (1) may be used alone or in combination of two or more.
[0030] The polycarbonate resin (A) preferably has, as part of its structure, a structural unit (b) derived from another dihydroxy compound, and more preferably, this structural unit (b) is a structural unit derived from at least one compound selected from the group consisting of an aliphatic dihydroxy compound, an alicyclic dihydroxy compound, and a heterocyclic dihydroxy compound.
[0031] Among the other dihydroxy compounds, it is particularly preferable to contain a structural unit derived from an aliphatic dihydroxy compound. It is also preferable to contain a structural unit derived from an alicyclic dihydroxy compound, in which case flexibility can be imparted to the resulting polycarbonate resin (A).
[0032] (Aliphatic dihydroxy compounds) The aliphatic dihydroxy compound may be either a linear aliphatic dihydroxy compound or a branched aliphatic dihydroxy compound. As the linear aliphatic dihydroxy compound, a linear aliphatic dihydroxy compound having preferably 2 to 30 carbon atoms, more preferably 3 to 20 carbon atoms, and even more preferably 3 to 10 carbon atoms is used. As the branched aliphatic dihydroxy compound, a branched aliphatic dihydroxy compound having preferably 3 to 30 carbon atoms, more preferably 3 to 20 carbon atoms, and even more preferably 4 to 12 carbon atoms is used.
[0033] Specific examples of the linear aliphatic dihydroxy compound include ethylene glycol, 1,3-propanediol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12-dodecanediol, hydrogenated dilinoleyl glycol, hydrogenated dioleyl glycol, etc. Among these, 1,3-propanediol, 1,4-butanediol, 1,6-pentanediol, and 1,9-nonanediol are preferred in terms of heat resistance, polymerizability, and availability.
[0034] Specific examples of branched aliphatic dihydroxy compounds include 1,3-butylene glycol, 2-methyl-1,3-propanediol, neopentyl glycol, 2-ethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol, 2,2,4-trimethyl-1,6-hexanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, 2,4-diethyl-1,5-pentanediol, 1,2-hexane glycol, 1,2-octyl glycol, 2-ethyl-1,3-hexanediol, 2,3-diisobutyl-1,3-propanediol, 2,2-diisoamyl-1,3-propanediol, and 2-methyl-2-propyl-1,3-propanediol. Among these, neopentyl glycol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-diethyl-1,3-propanediol, and 2,4-diethyl-1,5-pentanediol are preferred in terms of heat resistance, polymerizability, and availability.
[0035] (alicyclic dihydroxy compounds) The alicyclic dihydroxy compound is not particularly limited, but usually includes a compound having a 5-membered ring structure or a 6-membered ring structure. When the alicyclic dihydroxy compound has a 5-membered ring structure or a 6-membered ring structure, the heat resistance of the resulting polycarbonate resin (A) may be high. The 6-membered ring structure may be fixed to a chair or boat shape by a covalent bond. The number of carbon atoms contained in the alicyclic dihydroxy compound is usually 70 or less, preferably 50 or less, and more preferably 30 or less. If the number of carbon atoms is excessively large, the heat resistance is high, but the synthesis becomes difficult, the purification becomes difficult, and the cost tends to be high. The smaller the carbon number, the easier it is to purify and the easier it is to obtain.
[0036] Specific examples of the alicyclic dihydroxy compound having a 5-membered ring structure or a 6-membered ring structure include cyclohexanedimethanols, tricyclodecane dimethalins, pentacyclopentadecanedimethanols, decalin dimethanols, tricyclotetradecane dimethanols, norbornane dimethanols, adamantane dimethanols, cyclohexanediols, tricyclodecanediols, pentacyclopentadecanediols, decalin diols, tricyclotetradecanediols, norbornanediols, and adamantanediols.
[0037] Among the specific examples of the alicyclic dihydroxy compounds described above, cyclohexanedimethanols, tricyclodecane dimethanols, adamantanediols, and pentacyclopentadecanedimethanols are preferred, and from the viewpoints of availability and ease of handling, 1,4-cyclohexanedimethanol, 1,3-cyclohexanedimethanol, 1,2-cyclohexanedimethanol, and tricyclodecane dimethanol are particularly preferred. The above-mentioned exemplary compounds are merely examples of other dihydroxy compounds that can be used in the present invention, and the present invention is not limited thereto. These other dihydroxy compounds may be used alone or in combination of two or more.
[0038] When the polycarbonate resin (A) has the structural unit (b), the molar ratio of the structural unit (a) to the structural unit (b) in the polycarbonate resin (A) can be set to any ratio. By adjusting the molar ratio, the impact strength (e.g., Charpy notched impact strength) may be improved, and further, it is possible to obtain a polycarbonate resin (A) having a desired glass transition temperature.
[0039] The proportion of the structural unit (a) in the polycarbonate resin (A) is preferably from 25 to 95 mol %, more preferably from 30 to 90 mol %, and even more preferably from 40 to 80 mol %, based on all structural units derived from dihydroxy compounds.
[0040] (carbonic acid diester) The polycarbonate resin (A) can be obtained by polycondensing a dihydroxy compound including the dihydroxy compound (1) and a carbonic acid diester as raw materials through an ester exchange reaction. Examples of the carbonic acid diester used include diphenyl carbonate, substituted diphenyl carbonate such as ditolyl carbonate, dimethyl carbonate, diethyl carbonate, and di-t-butyl carbonate. Among them, diphenyl carbonate and substituted diphenyl carbonate are preferred, and diphenyl carbonate is particularly preferred. Note that the carbonic acid diester may contain impurities such as chloride ions, which may inhibit the polymerization reaction or deteriorate the hue of the resulting polycarbonate resin (A). Therefore, it is preferable to use a diester purified by distillation or the like, as necessary.
[0041] The carbonic acid diester is used in a molar ratio of preferably 0.90 to 1.20, more preferably 0.95 to 1.10, further preferably 0.96 to 1.10, and particularly preferably 0.98 to 1.04, based on the total amount of dihydroxy compounds used in the melt polymerization. If the molar ratio is 0.90 or more, the number of terminal hydroxyl groups in the produced polycarbonate resin (A) is not excessively increased, the thermal stability of the polymer is improved, and coloring during molding is less likely to occur. In addition, the rate of the ester exchange reaction is less likely to decrease, making it easier to obtain a desired high molecular weight product.
[0042] Moreover, if this molar ratio is 1.20 or less, the transesterification reaction rate is improved under the same conditions, and it becomes easy to produce a polycarbonate resin (A) with a desired molecular weight. In addition, the amount of residual diester carbonate in the produced polycarbonate resin (A) is reduced. This residual diester carbonate may be undesirable as it may cause odor during molding or in the molded product, and may increase the thermal history during the polymerization reaction, which may result in deterioration of the hue and weather resistance of the obtained polycarbonate resin (A). Therefore, a reduction in the amount of residual diester carbonate is preferable in that these problems are less likely to occur.
[0043] Furthermore, if the molar ratio of the carbonate diester to the total dihydroxy compounds is increased, the amount of the residual carbonate diester in the obtained polycarbonate resin (A) increases, and this may absorb ultraviolet light and deteriorate the light resistance of the polycarbonate resin (A), which is not preferable. The concentration of the carbonate diester remaining in the polycarbonate resin (A) is preferably 200 ppm by mass or less, more preferably 100 ppm by mass or less, particularly preferably 60 ppm by mass or less, and particularly preferably 30 ppm by mass or less. However, in reality, the polycarbonate resin (A) may contain unreacted carbonate diester, and the lower limit of the concentration of the unreacted carbonate diester in the polycarbonate resin (A) is usually 1 ppm by mass.
[0044] <Production method of polycarbonate resin (A)> The polycarbonate resin (A) is obtained by polycondensing a dihydroxy compound including the dihydroxy compound (1) with a carbonic acid diester through an ester exchange reaction. The dihydroxy compound and the carbonic acid diester as raw materials are preferably mixed uniformly in a raw material preparation tank or the like before the ester exchange reaction.
[0045] The mixing temperature is usually 80°C or higher, preferably 90°C or higher, and its upper limit is usually 250°C or lower, preferably 200°C or lower, and more preferably 150°C or lower. Of these, 100°C or higher and 120°C or lower are suitable. If the mixing temperature is above the lower limit, a sufficient dissolution rate is easily obtained, the solubility is unlikely to be insufficient, and problems such as solidification are unlikely to occur. If the mixing temperature is below the upper limit, the dihydroxy compound is unlikely to be thermally deteriorated, so that the color of the resulting polycarbonate resin is unlikely to deteriorate, and the light resistance is unlikely to be adversely affected.
[0046] The polycarbonate resin (A) is preferably produced by melt polymerization in multiple stages using a catalyst using multiple reactors. The reason for carrying out melt polymerization in multiple reactors is that in the early stage of the melt polymerization reaction, since the monomer contained in the reaction liquid is large, it is important to suppress the volatilization of the monomer while maintaining the required polymerization rate, and in the later stage of the melt polymerization reaction, it is important to sufficiently distill off the by-produced monohydroxy compound in order to shift the equilibrium to the polymerization side. In this way, in order to set different polymerization reaction conditions, it is preferable to use multiple reactors arranged in series from the viewpoint of production efficiency. As described above, the number of the reactors may be at least two or more, but from the viewpoint of production efficiency, it is preferably three or more, more preferably three to five, and particularly preferably four.
[0047] The reaction may be carried out in any of a batch system, a continuous system, or a combination of a batch system and a continuous system. Furthermore, in order to suppress the amount of monomer distilled, it is effective to use a reflux condenser in the polymerization reactor, and the effect is particularly large in a reactor in the early stage of polymerization where there is a large amount of unreacted monomer components. The temperature of the coolant introduced into the reflux condenser can be appropriately selected depending on the monomer used, but the temperature of the coolant introduced into the reflux condenser is usually 45 to 180°C, preferably 80 to 150°C, and particularly preferably 100 to 130°C at the inlet of the reflux condenser. If the temperature of the coolant introduced into the reflux condenser is below the upper limit, the reflux amount increases and the effect is improved, and if it is above the lower limit, the efficiency of distilling off the monohydroxy compound that should be distilled off tends to improve. As the refrigerant, hot water, steam, heat transfer oil, etc. are used, with steam and heat transfer oil being preferred.
[0048] In order to maintain an appropriate polymerization rate and suppress distillation of monomers while not impairing the hue, thermal stability, light resistance, etc. of the finally obtained polycarbonate resin (A), it is important to select the type and amount of the above-mentioned catalyst. In producing the polycarbonate resin (A), if there are two or more reactors, the reactors may have a plurality of reaction stages with different conditions, or the temperature or pressure may be changed continuously.
[0049] <Physical properties of polycarbonate resin (A)> Preferred physical properties of the polycarbonate resin (A) are shown below. (glass transition temperature) The glass transition temperature (Tg) of the polycarbonate resin (A) is preferably less than 155°C. If the glass transition temperature of the polycarbonate resin (A) is less than 155°C, it is less likely to be discolored, and it is easy to improve the impact strength. In this case, the mold temperature can be set to a certain degree low when transferring the shape of the mold surface to the molded product during molding. Therefore, the temperature regulator that can be selected is less likely to be limited, and the transferability of the mold surface is good.
[0050] The glass transition temperature of the polycarbonate resin (A) is more preferably lower than 145°C, and further preferably lower than 135°C. The glass transition temperature of the polycarbonate resin (A) is usually 90° C. or higher, and preferably 95° C. or higher. Methods for making the glass transition temperature of the polycarbonate resin (A) less than 155°C include reducing the proportion of the structural unit (a) in the polycarbonate resin (A), selecting an alicyclic dihydroxy compound with low heat resistance as another dihydroxy compound used in the production of the polycarbonate resin (A), and reducing the proportion of structural units derived from aromatic dihydroxy compounds such as bisphenol compounds in the polycarbonate resin (A).
[0051] (Polycarbonate resin composition) In forming the layer A, an additive may be blended with the polycarbonate resin (A) to form a polycarbonate resin composition, as long as the object of the present invention is not impaired. Examples of additives used in the polycarbonate resin composition include ultraviolet absorbers, light stabilizers, release agents, lubricants, antioxidants, flame retardants, flame retardant assistants, hydrolysis inhibitors, antistatic agents, foaming agents, fillers such as inorganic fillers, and colorants such as dyes and pigments.
[0052] (Manufacturing method of polycarbonate resin molded product (layer A)) The polycarbonate resin molded article (hereinafter, sometimes simply referred to as "molded article") which is layer A of the laminate of the present invention can be produced by various methods using the above-mentioned polycarbonate resin (A) or polycarbonate resin composition (hereinafter, sometimes collectively referred to as "polycarbonate resin composition, etc."). The molded article can also be produced by injection molding. In the case of injection molding, a mold corresponding to the shape of the molded article can be used to produce a molded article of a complex shape. Injection molding is performed by an injection molding machine, and suitable molding conditions are set according to the resin composition used and the product shape. Examples of molding conditions include cylinder temperature, mold temperature, injection pressure, pressure dwell, screw rotation speed, cushion amount, injection speed, injection time, pressure dwell time, and cooling time.
[0053] In the production of molded articles by injection molding, the cylinder temperature is preferably 200° C. to 300° C., more preferably 210° C. to 280° C., particularly preferably 220° C. to 270° C., and most preferably 230° C. to 260° C. If the cylinder temperature is equal to or lower than the upper limit, the resin composition is less likely to undergo thermal decomposition, and the molded article is less likely to become discolored, whereas if the cylinder temperature is equal to or higher than the lower limit, the melt viscosity of the polycarbonate resin composition or the like does not become too high, and molding defects and optical distortion tend to be less likely to occur. The mold temperature is preferably 40° C. to 120° C., more preferably 50° C. to 100° C., and particularly preferably 60° C. to 80° C. If the mold temperature is equal to or lower than the upper limit, the productivity of molded products tends to improve, while if it is equal to or higher than the lower limit, optical distortion tends to be small.
[0054] In the present invention, the molded article (layer A) can be obtained by controlling the ratio of the structural unit (a) derived from the dihydroxy compound (1) to the total dihydroxy compounds within a specific range as described above, and also by controlling the cylinder temperature and the mold temperature within the above-mentioned specific range. The molded article of the present invention can be produced by using these means alone or in appropriate combination.
[0055] The molded article of the present invention may have a decorative film layer or a printed layer laminated on at least one side thereof. By providing the decorative film layer or the printed layer, it is possible to obtain excellent effects such as improving the appearance of the molded article and improving the scratch resistance of the surface on which the decorative film layer or the printed layer is present. The lamination of the in-mold decorative film or the printed layer can be performed by a conventionally known method.
[0056] According to the present invention, it is possible to provide a laminate molded using a polycarbonate resin composition having excellent surface hardness and impact resistance. This laminate can be used for a wide range of applications as described above, and is particularly suitable for optical applications.
[0057] 3.B layer Layer B in the laminate of the present invention is a layer obtained by curing an active energy ray-curable resin composition (hereinafter sometimes simply referred to as "curable resin composition") containing mono- or polypentaerythritol poly(meth)acrylate (c) (hereinafter sometimes simply referred to as "component (c)") represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d) (hereinafter sometimes simply referred to as "component (d)").
[0058] [ka]
[0059] In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., a group represented by CH2=CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH2=CR-CO(O(CH2)5C=O) y It is a group represented by -O-, where R represents a hydrogen atom or a methyl group, and y represents an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.
[0060] <Mono- or polypentaerythritol poly(meth)acrylate (c)> The component (c) is one of the active energy ray-curable compounds contained in the curable resin composition for forming the B layer. By using the component (c), the curable resin composition exhibits good curability when irradiated with active energy rays, and a cured film (layer B) having a high crosslink density and excellent scratch resistance and chemical resistance can be formed.
[0061] Specific examples of the component (c) include pentaerythritol tri(meth)acrylate, EO-modified pentaerythritol tri(meth)acrylate, PO-modified pentaerythritol tri(meth)acrylate, caprolactone-modified pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, EO-modified pentaerythritol tetra(meth)acrylate, PO-modified pentaerythritol tetra(meth)acrylate, caprolactone-modified pentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, (Meth)acrylate, EO modified dipentaerythritol tri(meth)acrylate, PO modified dipentaerythritol tri(meth)acrylate, caprolactone modified dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, EO modified dipentaerythritol tetra(meth)acrylate, PO modified dipentaerythritol tetra(meth)acrylate, caprolactone modified dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, EO modified dipenta Erythritol penta(meth)acrylate, PO modified dipentaerythritol penta(meth)acrylate, caprolactone modified dipentaerythritol penta(meth)acrylate, dipentaerythritol hexa(meth)acrylate, EO modified dipentaerythritol hexa(meth)acrylate, PO modified dipentaerythritol hexa(meth)acrylate, caprolactone modified dipentaerythritol hexa(meth)acrylate, tripentaerythritol tetra(meth)acrylate, EO modified tripentaerythritol tetra(meth)acrylate ) acrylate, PO modified tripentaerythritol tetra(meth)acrylate, caprolactone modified tripentaerythritol tetra(meth)acrylate, tripentaerythritol penta(meth)acrylate, EO modified tripentaerythritol penta(meth)acrylate, PO modified tripentaerythritol penta(meth)acrylate, caprolactone modified tripentaerythritol penta(meth)acrylate, tripentaerythritol hexa(meth)acrylate, EO modified tripentaerythritol hexa(meth)acrylate,Examples of the tripentaerythritol hexa(meth)acrylate include PO-modified tripentaerythritol hexa(meth)acrylate, caprolactone-modified tripentaerythritol hepta(meth)acrylate, EO-modified tripentaerythritol hepta(meth)acrylate, PO-modified tripentaerythritol hepta(meth)acrylate, caprolactone-modified tripentaerythritol hepta(meth)acrylate, tripentaerythritol octa(meth)acrylate, EO-modified tripentaerythritol octa(meth)acrylate, PO-modified tripentaerythritol octa(meth)acrylate, and caprolactone-modified tripentaerythritol octa(meth)acrylate. Here, "EO" means ethylene oxide, and "PO" means propylene oxide. These can be used alone or in combination of two or more.
[0062] Among them, from the viewpoint of the balance between weather resistance and scratch resistance of the cured film, dipentaerythritol poly(meth)acrylate is preferred, and caprolactone-modified dipentaerythritol poly(meth)acrylate is more preferred. As the dipentaerythritol poly(meth)acrylate, from the viewpoint of the weather resistance of the cured film, dipentaerythritol penta(meth)acrylate and dipentaerythritol hexa(meth)acrylate are preferred, and caprolactone-modified dipentaerythritol penta(meth)acrylate and caprolactone-modified dipentaerythritol hexa(meth)acrylate are more preferred.
[0063] In the general formula (2), from the viewpoint of scratch resistance of the cured film, a (meth)acryloyl group modified with caprolactone (CH2=CR-CO(O(CH2)5C=O) yIn -O-), y is preferably 5 or less, more preferably 3 or less, and even more preferably 2 or less. The number of (meth)acryloyl groups modified with caprolactone is 1 or more and 2n+2 or less on average per molecule of the mono- or polypentaerythritol poly(meth)acrylate modified with caprolactone, with the lower limit being preferably 2 or more from the viewpoint of weather resistance. The upper limit is preferably 2n+1, more preferably 2n, from the viewpoint of scratch resistance and weather resistance of the cured film.
[0064] The blending amount of the (c) component is preferably 10% by mass or more, more preferably 25% by mass or more, and particularly preferably 40% by mass or more, based on the total amount of the curable resin composition. The greater the blending amount of the (c) component, the greater the scratch resistance and chemical resistance of the cured film. The smaller the blending amount of the (c) component, the greater the weather resistance of the cured film.
[0065] <Urethane (meth)acrylate compound (d)> Component (d) is one of the active energy ray curable compounds contained in the curable resin composition for forming layer B, and includes a urethane (meth)acrylate compound containing three or more (meth)acryloyl groups in one molecule. By using component (d), it is possible to impart toughness to the cured film of the curable resin composition, improve adhesion, and further improve the weather resistance of the cured film (layer B).
[0066] Examples of the (d) component include a urethane (meth)acrylate compound (hereinafter simply referred to as "component (d12)") obtained by reacting a diisocyanate (d1) having two isocyanate groups with a hydroxy(meth)acrylate (d2) having two or more (meth)acryloyloxy groups and a hydroxy group, and a urethane (meth)acrylate compound (hereinafter simply referred to as "component (d34)") obtained by reacting a polyisocyanate (d3) having three or more isocyanate groups with a hydroxy(meth)acrylate (d4) having one or more (meth)acryloyloxy groups and a hydroxy group.
[0067] (Component (d12)) The diisocyanate (d1) is not particularly limited, and examples thereof include aliphatic, alicyclic, or aromatic diisocyanates. Specific examples include isophorone diisocyanate, tetramethylene diisocyanate, hexamethylene diisocyanate, xylylene diisocyanate, triene diisocyanate, polymeric MDI, naphthalene diisocyanate, tetramethyl xylylene diisocyanate, trimethylhexamethylene diisocyanate, lysine diisocyanate methyl ester, hydrogenated xylylene diisocyanate, hydrogenated diphenylmethane diisocyanate, diphenylmethane diisocyanate, methylenebis(4,1-cyclohexylene)-diisocyanate, 1,3-bis(isocyanate Examples of the diisocyanates include methyl)cyclohexane, tolylene diisocyanate (e.g., 2,4-tolylene diisocyanate), phenylene diisocyanate (1,4-phenylene diisocyanate), diphenyl diisocyanate (e.g., 4,4-diphenyl diisocyanate, 3,3-dimethyl-4,4-diphenylene diisocyanate), diphenylmethane diisocyanate (4,4-diphenylmethane diisocyanate), dicyclohexylmethane diisocyanate, naphthalene diisocyanate (e.g., 1,5-naphthalene diisocyanate), and xylylene diisocyanate. Among these, from the viewpoint of the weather resistance of the cured film obtained, aliphatic or alicyclic diisocyanates are more preferable. These may be used alone or in combination of two or more.
[0068] The hydroxy(meth)acrylate (d2) is not particularly limited, and examples thereof include glycerin di(meth)acrylate, pentaerythritol tri(meth)acrylate, dipentaerythritol penta(meth)acrylate, ditrimethylolpropane tri(meth)acrylate, etc. Among these, pentaerythritol tri(meth)acrylate and dipentaerythritol penta(meth)acrylate are more preferred from the viewpoint of excellent curability and surface hardness. These may be used alone or in combination of two or more.
[0069] Furthermore, as a raw material for the urethane (meth)acrylate compound, a diol having two hydroxyl groups in the molecule may be used. The diol to be used is not particularly limited, and examples thereof include low molecular weight diols, polyether diols, polycaprolactone dipolyols, polycarbonate dipolyols, etc.
[0070] Specific examples of low molecular weight polyols include aliphatic diols such as 1,2-ethanediol (ethylene glycol), 1,2-propanediol (propylene glycol), diethylene glycol, 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, 3-methyl-1,5-pentanediol, neopentyl glycol, glycerin, and trimethylolpropane, and alicyclic diols such as cyclohexanedidimethanol and 2,2'-bis(4-hydroxycyclohexyl)propane. Examples of polyether diols include aliphatic polyether polyols obtained by ring-opening polymerization of the above-mentioned aliphatic diols and alkylene oxides having 2 to 4 carbon atoms, such as ethylene oxide, propylene oxide, and tetrahydrofuran. Examples of polycaprolactone diols include aliphatic polycaprolactone polyols obtained by ring-opening polymerization of the above-mentioned aliphatic diols and ε-caprolactone. Examples of polycarbonate diols include polycarbonate polyols, which are polycondensates of aliphatic or alicyclic diols having 4 to 8 carbon atoms, such as 1,4-butanediol, 1,5-pentanediol, 1,6-hexanediol, and 1,4-cyclohexanedimethanol, and alkylene carbonates having 2 to 5 carbon atoms, such as ethylene carbonate and propylene carbonate, and are obtained by polycondensation and dealkylene glycol reaction. These may be used alone or in combination of two or more kinds.
[0071] (Component (d34)) The polyisocyanate (d3) is not particularly limited, and may be, for example, an aliphatic, alicyclic or aromatic polyisocyanate.Specific examples include adducts of the various diisocyanate compounds listed in the diisocyanate (d1) with polyol compounds such as trimethylolpropane, and isocyanate derivatives such as biuret and isocyanurate of diisocyanate compounds.Of these, polyisocyanates derived from hexamethylene diisocyanate and isophorone diisocyanate are preferred from the viewpoint of weather resistance and excellent hardness of the cured coating film. Commercially available products include Duranate D-201, TPA-100, TKA-100, 24A-100, 22A-75P, P301-75E, MHG-80B, etc. manufactured by Asahi Kasei Corporation, Coronate HX, 2715, etc. manufactured by Tosoh Corporation, Takenate D160N, D-170N, D-170HN, D-172N, D-177N manufactured by Mitsui Chemicals, Inc., and Vestanat T-1890 manufactured by EVONIK. These may be used alone or in combination of two or more kinds.
[0072] The hydroxy(meth)acrylate (d4) is not particularly limited, and examples thereof include, in addition to the hydroxy(meth)acrylate (d2), hydroxyalkyl(meth)acrylates such as 2-hydroxyethyl(meth)acrylate, 2-hydroxypropyl(meth)acrylate, and 4-hydroxybutyl(meth)acrylate, cyclohexanedimethanol mono(meth)acrylate, and 2-hydroxy-3-acryloyloxypropyl methacrylate. Among these, 2-hydroxyethyl(meth)acrylate, 4-hydroxybutyl(meth)acrylate, pentaerythritol tri(meth)acrylate, and dipentaerythritol penta(meth)acrylate are more preferred from the viewpoint of excellent surface hardness and adhesion. These hydroxy(meth)acrylates (d4) may be used alone or in combination of two or more.
[0073] The synthesis method of the component (d) is not particularly limited, and a known synthesis method of polyurethane can be adopted. For example, the component (d12) can be obtained by mixing a diisocyanate (d1) with a polyurethane catalyst, and then dropping and reacting a hydroxy (meth) acrylate (d2) at 50 to 90°C. The component (d34) can be obtained by mixing a polyisocyanate (d3) with a polyurethane catalyst, and then dropping and reacting a hydroxy (meth) acrylate (d4) at 50 to 90°C.
[0074] As the polyurethane catalyst, an amine catalyst, an organometallic catalyst, etc. can be used. As the amine catalyst, triethylamine, N,N-dimethylcyclohexylamine, dimethanolamine, etc. can be used. As the organometallic catalyst, an organotin compound is preferably used, and examples thereof include stannous octoate, stannous laurate, dibutyltin dilaurate, dibutyltin dimaleate, dibutyltin diacetate, dioctyltin diacetate, etc. These may be used alone or in combination of two or more. Among these, from the viewpoint of obtaining a high catalytic effect with a small amount, an organometallic catalyst is preferred, and dibutyltin dilaurate is more preferred. In addition, in order to facilitate temperature control during synthesis and to reduce the viscosity of the obtained component (d) to improve workability, the reaction solution may be diluted with a solvent or the like as necessary.
[0075] When synthesizing the component (d12) of the component (d), in addition to the diisocyanate (d1) and the hydroxy(meth)acrylate (d2), a hydroxy group-containing compound other than the hydroxy(meth)acrylate (d2) may be used. The ratio of diisocyanate (d1) to hydroxy(meth)acrylate (d2) when producing the (d12) component is not particularly limited. However, it is preferable that the ratio of the total amount of isocyanate groups contained in the diisocyanate (d1) to the total amount of hydroxy groups contained in the hydroxy(meth)acrylate (d2) is 0.5≦(total amount of isocyanate groups) / (total amount of hydroxy groups)<0.9. When the ratio is 0.5 or more, the molecular weight of the obtained (d12) component does not become too low, and volume shrinkage during curing is small, which is preferable. In addition, when the ratio is less than 0.9, the molecular weight of the obtained (d12) component does not become too high, and gelation due to thickening during synthesis can be prevented. It is more preferable that the (total amount of isocyanate groups) / (total amount of hydroxy groups) is 0.65 to 0.85. The amount of hydroxy groups and the amount of isocyanate groups are values calculated by multiplying the number of each functional group contained in one molecule by the number of moles used.
[0076] The weight average molecular weight of component (d) is preferably 5500 to 60000. When the weight average molecular weight of component (d) is within the above range, it becomes easy to achieve both scratch resistance and weather resistance of the obtained cured film. The weight average molecular weight of component (d) is more preferably 5500 to 30000, and further preferably 5500 to 25000. When the weight average molecular weight is 5500 or more, the weather resistance of the obtained cured film becomes good.
[0077] The weight average molecular weight of the component (d) is a weight average molecular weight (Mw) calculated using standard polystyrene standards and measured by gel permeation chromatography (GPC) under the following conditions: Equipment: Tosoh Corporation high-speed GPC equipment HLC-8320GPC type UV detector: Tosoh UV-8320 ·Flow rate: 0.35mL / min ·Inlet temperature: 40℃ Oven temperature: 40℃ ·RI temperature: 40℃ ·UV wavelength: 254nm Sample injection volume: 10μL Columns: Three columns connected in the order of (1) to (3). (1) TSKgel superHZM-M (4.6mm ID x 15cm L) manufactured by Tosoh Corporation (2) TSKgel superHZM-M (4.6mm ID x 15cm L) manufactured by Tosoh Corporation (3) TSKgel HZ2000 (4.6mm ID x 15cm L) manufactured by Tosoh Corporation Guard column: Tosoh Corporation TSKguardcolumn SuperHZ-L (4.6mm ID x 3.5cm L) Solvent: THF (tetrahydrofuran) (stabilizer: BHT (dibutylhydroxytoluene)) Sample concentration: Resin content adjusted to 0.2% by mass
[0078] As the component (d), from the viewpoints of the balance between the weather resistance and scratch resistance of the cured film and the adhesion to the substrate, the component (d34) is preferred, and a urethane (meth)acrylate compound obtained using the polyisocyanate (d3), which is an isocyanurate, is more preferred.
[0079] The blending amount of the (d) component is preferably 10% by mass or more, more preferably 15% by mass or more, and particularly preferably 30% by mass or more, based on the total amount of the curable resin composition. The higher the blending amount of the (d) component, the higher the toughness and flexibility of the cured film. The lower the blending amount of the (d) component, the higher the coating hardness and chemical resistance of the cured film.
[0080] <Other monomers> The active energy ray-curable resin composition of the present invention may contain, in addition to the components (c) and (d), a (meth)acrylate compound other than the components (c) and (d) as another active energy ray-curable compound. Examples of the other active energy ray-curable compounds include monofunctional (meth)acrylates having a polymerizable unsaturated bond such as (meth)acrylates, polyfunctional (meth)acrylates, polyester (meth)acrylates, and epoxy (meth)acrylates, and may be appropriately selected depending on the required performance of the cured film.
[0081] Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, butyl (meth)acrylate, propyl (meth)acrylate, n-butyl (meth)acrylate, i-butyl (meth)acrylate, t-butyl (meth)acrylate, hexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, morpholyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, glycidyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, and the like. ) acrylate, diethylaminoethyl (meth)acrylate, tricyclodecane (meth)acrylate, polyethylene glycol mono(meth)acrylate, cyclohexyl (meth)acrylate, tetrahydrofurfuryl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyl (meth)acrylate, isobornyl (meth)acrylate, allyl (meth)acrylate, 2-ethoxyethyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyl (meth)acrylate and other mono(meth)acrylates, and adducts of phthalic anhydride and 2-hydroxyethyl (meth)acrylate, and the like.
[0082] Examples of the polyfunctional (meth)acrylate include neopentyl glycol di(meth)acrylate, ethylene glycol di(meth)acrylate, polyethylene glycol (number of repeating units (hereinafter referred to as "n") = 2 to 15) di(meth)acrylate, polypropylene glycol (n = 2 to 15) di(meth)acrylate, polybutylene glycol (n = 2 to 15) di(meth)acrylate, 2,2-bis(4-(meth)acryloxyethoxyphenyl)propane, 2,2-bis(4-(meth)acryloxydiethoxyphenyl)propane, and the like. Examples of the acrylates include propane, trimethylolpropane diacrylate, bis(2-(meth)acryloxyethyl)-hydroxyethyl-isocyanurate, trimethylolpropane tri(meth)acrylate, tris(2-(meth)acryloxyethyl)isocyanurate, pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate.
[0083] Examples of polyester poly(meth)acrylates include polyester (meth)acrylates obtained by reacting trimethylolethane with succinic acid and (meth)acrylic acid, and polyester (meth)acrylates obtained by reacting trimethylolpropane with succinic acid, ethylene glycol, and (meth)acrylic acid. Examples of epoxy (meth)acrylates include glycidyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate glycidyl ether, 2-hydroxypropyl (meth)acrylate glycidyl ether, and 2-hydroxybutyl (meth)acrylate glycidyl ether. These can be used alone or in combination of two or more. Among these, tris(2-(meth)acryloxyethyl)isocyanurate is preferred from the viewpoint of weather resistance.
[0084] <Ultraviolet absorber (e)> The curable resin composition preferably contains an ultraviolet absorber (e) from the viewpoint of weather resistance. Benzophenone-based ultraviolet absorbers are more preferable from the viewpoint of being contained in a large amount in the curable resin composition. Also, triazine-based or benzotriazole-based ultraviolet absorbers are more preferable from the viewpoint of preventing yellowing of the A layer.
[0085] Examples of the ultraviolet absorber (e) include triazine-based compounds, benzophenone-based compounds, benzotriazole-based compounds, phenyl benzoate-based compounds, phenyl salicylate-based compounds, and anilide oxalate-based compounds. Examples of triazine compounds include 2-[4-{(2-hydroxy-3-dodecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-{(2-hydroxy-3-tridecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-{4-(octyl-2-methylethanoate)oxy-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-{(2-hydroxy-3-dodecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-{(2-hydroxy-3-tridecyloxypropyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and the like. Examples of benzophenone compounds include 2,4-dihydroxybenzophenone, 2-hydroxy-4-methoxy-benzophenone, and the like. Examples of benzotriazole compounds include 2-(2H-benzotriazol-2-yl)-4,6-bis(I-methyl-1-phenylethyl)phenol and 2-(2H-benzotriazol-2-yl)-6-(1-methyl-1-phenylethyl)-4-(1,1,3,3-tetramethylbutyl)phenol. Examples of the phenyl benzoate compounds include phenyl salicylate, p-tert-butylphenyl salicylate, and p-(1,1,3,3-tetramethylbutyl)phenyl salicylate. Examples of the phenyl salicylate compounds include phenyl salicylates, 3-hydroxyphenylbenzoate, and phenylene-1,3-dibenzoate. Examples of the oxalic acid anilide compounds include 2-ethoxy-2'-ethyloxalanilide, 2-ethoxy-2'-dodecyloxalanilide, and the like.
[0086] Among these, triazine-based compounds or anilide oxalates are preferred, from the viewpoint that the curable resin composition has good curability and a cured film having high surface hardness can be obtained, and 2-[4-{(2-hydroxy-3-dodecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, 2-[4-{(2-hydroxy-3-tridecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine, and 2-ethoxy-2'-dodecyloxalanilide are more preferred. These can be used alone or in combination of two or more. Furthermore, from the viewpoint of the scratch resistance of the cured film, it is preferable to use a combination of 2-[4-{(2-hydroxy-3-dodecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine and 2-[4-{(2-hydroxy-3-tridecyloxy-propyl)oxy}-2-hydroxyphenyl]-4,6-bis(2,4-dimethylphenyl)-1,3,5-triazine.
[0087] The content of the ultraviolet absorber (e) in the curable resin composition is preferably high from the viewpoint of weather resistance, and is preferably low from the viewpoint of scratch resistance. The content of the ultraviolet absorber (e) in the curable resin composition is preferably 0.5 parts by mass or more and 20 parts by mass or less, and more preferably 0.5 parts by mass or more and 5 parts by mass or less, based on 100 parts by mass of the active energy ray-curable compound.
[0088] <Hindered amine light stabilizers (f)> From the viewpoint of weather resistance, the curable resin composition preferably contains a hindered amine-based light stabilizer (f). These may be used alone or in combination of two or more kinds.
[0089] Examples of the hindered amine light stabilizer (f) include a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name: Adeka STAB (registered trademark; the same applies below) LA-63P), manufactured by ADEKA Corporation; Condensation product of butanetetracarboxylic acid, 2,2,6,6-pentamethyl-4-piperidinol, and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name: Adeka STAB LA-68P), condensation product of 1,1-dimethylethyl hydroperoxide and octane manufactured by BASF, bis(2,2,6,6-tetramethyl-1-( octyloxy)-4-piperidinyl) ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane (e.g., Tinuvin (trade name; the same applies below) 123), 2-butyl-2-[3,5-di(tert-butyl)-4-hydroxybenzyl]malonate bis(1,2,2,6,6-pentamethyl-4-piperidyl) (trade name: Tinuvin 144), 2,4-bis[N-butyl-N-(1- cyclohexyloxy-2,2,6,6-tetramethylpiperidin-4-yl)amino]-6-(2-hydroxyethylamine)-1,3,5-triazine (trade name: Tinuvin 152), a mixture of bis(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate and methyl(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (trade name: Tinuvin 292), and the like. Among these, a condensate of 1,2,3,4-butanetetracarboxylic acid, 1,2,2,6,6-pentamethyl-4-piperidinol, and β,β,β,β-tetramethyl-3,9-(2,4,8,10-tetraoxaspiro[5,5])undecane)diethanol (trade name: Adeka STAB (registered trademark; the same applies hereinafter) LA-63P), 1,1-dimethylethyl hydroperoxide and octyl ether (trade name: Adeka STAB (registered trademark; the same applies hereinafter) LA-63P), and 1,2,3,4-butanetetracarboxylic acid and 1,2,2,6,6-pentamethyl-4-piperidinol (trade name: Adeka STAB (registered trademark; the same applies hereinafter) LA-63P) are preferred because they provide a curable resin composition with good curability and can maintain weather resistance for a long period of time. Preferred are decanedioic acid condensates with octane, decanedioic acid bis(2,2,6,6-tetramethyl-1-(octyloxy)-4-piperidinyl) ester, reaction products of 1,1-dimethylethyl hydroperoxide with octane (for example, TINUVIN (trade name; the same applies below) 123), and a mixture of bis(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate and methyl(1,2,2,6,6-pentamethylpiperidin-4-yl) sebacate (trade name: TINUVIN 292).
[0090] The content of the hindered amine light stabilizer (f) in the curable resin composition is preferably from 0.1 to 5 parts by mass, and more preferably from 0.5 to 2 parts by mass, based on 100 parts by mass of the active energy ray-curable compound.
[0091] <Photopolymerization initiator> The curable resin composition is applied to the A layer, and then cured by irradiating it with active energy rays such as light to form the B layer. When an electron beam or hard X-ray having a relatively high energy is used as the active energy ray, the curable resin composition can be cured without adding a photopolymerization initiator to the curable resin composition. On the other hand, when other active energy rays such as ultraviolet rays or soft X-rays are used for curing, it is preferable to add a photopolymerization initiator to the curable resin composition.
[0092] When a photopolymerization initiator is contained in the curable resin composition, a wide variety of known photopolymerization initiators can be used, but preferred examples include alkylphenone compounds such as α-hydroxyacetophenone (α-hydroxyphenyl ketone), α-aminoacetophenone, and benzil ketal; acylphosphine oxide compounds; oxime ester compounds; oxyphenylacetic acid esters; benzoin ethers; aromatic ketones (benzophenones); ketone / amine compounds; and benzoylformic acid and its ester derivatives.
[0093] Specifically, for example, benzoin methyl ether, benzoin ethyl ether, benzoin propyl ether, benzoin butyl ether, diethoxyacetophenone, benzyl dimethyl ketal, 2-hydroxy-2-methylpropiophenone, 1-hydroxycyclohexyl phenyl ketone, benzophenone, 2,4,6-trimethylbenzoin diphenylphosphine oxide, 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, Michler's ketone, N,N-dimethylaminobenzoic acid isoamyl, 2-chlorothioxanthone, 2,4-diethylthioxanthone, benzoylformic acid, benzoylformic acid methyl, and benzoylformic acid ethyl. These photopolymerization initiators may be used alone or in combination of two or more.
[0094] Among these, it is preferable to use α-hydroxyphenyl ketones such as 2-hydroxy-2-methylpropiophenone and 1-hydroxycyclohexyl phenyl ketone as at least a part of the photopolymerization initiator, since it is possible to minimize the decrease in curability, they are easily available, and they are less likely to cause coloration, etc.
[0095] In particular, in order to improve the curability of the curable resin composition, α-aminophenyl ketones such as 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone and 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one; benzophenones such as benzophenone, Michler's ketone, 2-chlorothioxanthone, isopropylthioxanthone, and 2,4-diethylthioxanthone; benzoylformic acid (esters) such as methyl benzoylformate, benzoylformic acid, and ethyl benzoylformate; and oxime esters such as CGI242 (manufactured by Ciba) and OXE01 (manufactured by Ciba) are preferred. Furthermore, it is more preferable to use 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, benzophenone, methyl benzoylformate, or the like, and it is particularly preferable to use 2-methyl-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butan-1-one, methyl benzoylformate.
[0096] When the curable resin composition contains a photopolymerization initiator, the content of the photopolymerization initiator is preferably 2 to 6.5 parts by mass, more preferably 2.5 to 5.5 parts by mass, based on 100 parts by mass of the active energy ray curable compound. When the content of the photopolymerization initiator is equal to or more than the lower limit, the curability of the curable resin composition is excellent, and when the content is equal to or less than the upper limit, the physical properties of the cured film (layer B) are improved.
[0097] <Inorganic particles> The curable resin composition can contain inorganic particles. In addition, by containing the inorganic particles and a (meth)acryloyl copolymer having a high crosslinking density, a curable resin composition capable of forming a hard coat layer having higher hardness can be provided.
[0098] The average primary particle size of the inorganic particles is preferably 1 nm to 200 nm, more preferably 150 nm or less, and even more preferably 100 nm or less, in view of good transparency of the cured film. The lower limit of the average primary particle size of the inorganic particles is more preferably 5 nm or more, and even more preferably 10 nm or more, in view of easy availability of raw materials.
[0099] The movement of the inorganic particles in the above range is dominated by thermal diffusion rather than gravity-induced sedimentation, so that the particles can be stably dispersed in the curable resin composition, and further, when a cured film (layer B) is formed, the inorganic particles can be effectively present on the surface. In addition, the smaller the average primary particle size of the inorganic particles, the better the optical properties tend to be. The average primary particle size of inorganic particles refers to the average size of particles observed with an electron microscope such as a TEM.
[0100] Examples of inorganic particles include silica (including organosilica sol), alumina, titania, zeolite, mica, synthetic mica, calcium oxide, zirconium oxide, zinc oxide, magnesium fluoride, smectite, synthetic smectite, vermiculite, ITO (indium oxide / tin oxide), ATO (antimony oxide / tin oxide), tin oxide, indium oxide, antimony oxide, etc. These inorganic particles may contain only one type, or may contain two or more types in combination. Among them, silica (including organosilica sol) is preferably used because the raw material is easily available, the particle surface is easily modified, and dispersion stability is easily ensured.
[0101] From the viewpoints of the transparency of layer B, the weather resistance of the laminate, and the laminate itself, it is preferable that the colloidal silica obtained by dispersing silica in water is surface-modified colloidal silica. To modify colloidal silica, a compound having a hydrolyzable silicon group or a compound having a silicon group bonded with a hydroxyl group can be used. Each of these compounds may be one type or two or more types. In the compound having a hydrolyzable silicon group, silanol groups are generated by hydrolysis, and these silanol groups react with and bond to the silanol groups present on the surface of the colloidal silica to generate surface-modified colloidal silica.
[0102] Examples of the silicon group-containing compound include tetramethoxysilane, tetraethoxysilane, methyltrimethoxysilane, ethyltrimethoxysilane, phenyltrimethoxysilane, dimethyldimethoxysilane, trimethylmethoxysilane, β-(meth)acryloyloxyethyltrimethoxysilane, γ-(meth)acryloyloxypropyltrimethoxysilane, γ-(meth)acryloyloxypropyltriethoxysilane, γ-(meth)acryloyloxypropylmethyldimethoxysilane, vinylolimethoxysilane, vinyltriethoxysilane, vinylmethyldimethoxysilane, p-vinylphenyltrimethoxysilane, β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, γ-aminopropyltrimethoxysilane, γ-styryltrimethoxysilane, p-styryltrimethoxysilane, 3-mercaptopropylmethyldimethoxysilane, and 3-mercaptopropyltrimethoxysilane.
[0103] In addition, modified silicon group-containing compounds such as derivatives in which a polyfunctional (meth)acrylate or a high molecular weight (meth)acrylate is added to a silane having a mercapto group, and derivatives in which a polyfunctional (meth)acrylate having a hydroxyl group is added to a silane having an isocyanate group may also be used. The surface modification of colloidal silica can be carried out by reacting the colloidal silica with a compound containing a hydrolyzable silicon group, a catalyst, and water at 20 to 100° C. for 1 to 40 hours.
[0104] Examples of the catalyst used in the surface modification reaction include inorganic acids such as hydrochloric acid, hydrofluoric acid, hydrobromic acid, sulfuric acid, nitric acid, and phosphoric acid; organic acids such as formic acid, acetic acid, oxalic acid, p-toluenesulfonic acid, acrylic acid, and methacrylic acid; alkali; aluminum acetylacetonate, aluminum 2,2,6,6-tetramethyl-3,5-heptanedionate, aluminum diisopropoxide ethylacetoacetate, aluminum diisobutoxide ethylacetoacetate, boric acid butoxide, dibutyltin dilaurate, and dibutyltin dioctate.
[0105] The amount of these catalysts used is preferably 0.0001 to 5 parts by mass, and more preferably 0.01 to 1 part by mass, per 100 parts by mass of the total amount of colloidal silica and the hydrolyzable silicon group-containing compound. The amount of water in the surface modification reaction is preferably 0.5 to 100 equivalents, and more preferably 1 to 30 equivalents, relative to the hydrolyzable silicon group. Moreover, of the colloidal silica, acidic colloidal silica is preferable among acidic and basic colloidal silica.
[0106] The content of the inorganic particles in the curable resin composition is preferably 5 parts by mass or more, more preferably 10 parts by mass or more, and even more preferably 20 parts by mass or more, and is preferably 70 parts by mass or less, more preferably 50 parts by mass or less, and even more preferably 40 parts by mass or less, relative to 100 parts by mass of the active energy ray-curable compound.
[0107] <Preparation method> The curable resin composition can be prepared by mixing and stirring the above-mentioned components using a conventional stirrer. If necessary, the composition can be prepared by mixing the components together with a solvent, a polymerization initiator, an additive, and the like. The solvent used in the preparation of the curable resin composition is not particularly limited, and is appropriately selected in consideration of the (meth)acryloyl copolymer, the polyfunctional (meth)acrylate, the material of the substrate that serves as the base for coating, the coating method of the composition, and the like. Specific examples of solvents that can be used include aromatic solvents such as toluene and xylene; ketone-based solvents such as methyl ethyl ketone, acetone, methyl isobutyl ketone and cyclohexanone; ether-based solvents such as diethyl ether, isopropyl ether, tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, propylene glycol monomethyl ether, anisole and phenetole; ester-based solvents such as ethyl acetate, butyl acetate, isopropyl acetate and ethylene glycol diacetate; amide-based solvents such as dimethylformamide, diethylformamide and N-methylpyrrolidone; cellosolve-based solvents such as methyl cellosolve, ethyl cellosolve and butyl cellosolve; alcohol-based solvents such as methanol, ethanol, propanol, isopropanol and butanol; and halogen-based solvents such as dichloromethane and chloroform.
[0108] These solvents may be used alone or in combination of two or more of them. Among these solvents, ester-based solvents, ether-based solvents, alcohol-based solvents and ketone-based solvents are preferably used.
[0109] Various additives may be added to the curable resin composition as necessary, including commonly used additives such as antioxidants, anti-yellowing agents, bluing agents, pigments, leveling agents, defoamers, thickeners, anti-settling agents, antistatic agents, and anti-fogging agents.
[0110] Examples of the leveling agent include compounds containing a perfluoroalkyl group or a perfluoroalkylene skeleton, and compounds containing a polydimethylsiloxane structure. The content of the leveling agent in the curable resin composition is preferably 0 to 5 parts by mass, more preferably 0 to 2 parts by mass, and even more preferably 0 to 1 part by mass, relative to 100 parts by mass of the active energy ray-curable compound, from the viewpoints of transparency, coating appearance, adhesion, and hardness.
[0111] In addition, when the layer A contains a functional group that can be cured by light or heat, it may be more preferable to cure the layer A by irradiating with active energy rays or by heating. The layer A may be in the form of a molded article (article), or another layer may be interposed between the layer A and the layer B.
[0112] The method of applying the curable resin composition is not particularly limited, but is preferably applied by spin coating, dip coating, flow coating, spray coating, bar coating, gravure coating, roll coating, blade coating, air knife coating, etc. From the viewpoints of the applicability of the curable resin composition, the smoothness and uniformity of the coating film, and the adhesion of the cured film (layer B) to layer A, it is preferable to apply the composition by adding an organic solvent. In addition, in order to reduce the viscosity, the curable resin composition may be heated or diluted with a subcritical fluid.
[0113] After forming a coating film on at least one surface of Layer A by the above-mentioned coating method, volatile components are removed by heating and drying as necessary, and then a layer consisting of a cured film, i.e., Layer B, is obtained by, for example, irradiating the coating film with active energy rays.
[0114] When active energy rays are used to obtain a cured film, examples of the irradiation method include ultraviolet rays emitted from light sources such as xenon lamps, low-pressure mercury lamps, high-pressure mercury lamps, ultra-high-pressure mercury lamps, metal halide lamps, carbon arc lamps, and tungsten lamps, and active energy rays (electron beams, EB) such as electron beams, α rays, β rays, and γ rays usually extracted from particle accelerators of 20 to 2000 kV. As active energy rays, ultraviolet rays are preferred in terms of good curability and productivity. As the ultraviolet ray source, high-pressure mercury lamps, metal halide lamps, etc. can be used. The ultraviolet ray is ultraviolet ray of 100 nm or more and 400 nm or less at 100 mJ / cm. 2 More than 5000mJ / cm2 It is preferable to irradiate the active energy rays so as to satisfy the following conditions: The atmosphere for irradiating the active energy rays may be air or an inert gas such as nitrogen or argon.
[0115] The thickness of the B layer after curing is preferably 2 μm or more, more preferably 3 μm or more, and even more preferably 4 μm or more from the viewpoint of ensuring high hardness. Also, the thickness of the B layer is preferably 40 μm or less, more preferably 30 μm or less, even more preferably 25 μm or less, and particularly preferably 20 μm or less from the viewpoint of dimensional stability in which distortion (cracks) of the B layer due to cure shrinkage is unlikely to occur, and from the viewpoint of moist heat resistance in which distortion (cracks) of the B layer is unlikely to occur in a moist heat environment.
[0116] In the laminate, layer B may be formed on only one side of layer A, or on both sides of layer A. Also, layer B may be directly laminated on layer A. In the production of the laminate, the application and curing of the curable resin composition may be performed only once or may be performed multiple times. By repeating the application and curing of the curable resin composition multiple times, warping of the laminate can be prevented. EXAMPLES
[0117] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as the gist of the present invention is not exceeded. In the following examples, "parts" refers to "parts by mass." The physical properties of the laminates obtained in the following examples were evaluated by the following methods.
[0118] (1) Molding of polycarbonate resin (production of layer A) A mold with a cavity of 100 mm width, 100 mm length, and 1.0 mm thickness, and one fan gate of 40 mm width and 0.8 mm thickness was attached to an injection molding machine with a clamping force of 200 ton manufactured by Meiki Seisakusho Co., Ltd., and plates were molded using polycarbonate resin (A-1 to A-2) under the conditions of a mold temperature of 80°C, injection pressure of 180 to 250 MPa, holding pressure of 60 to 80 MPa, holding time of 2 seconds, and cooling time of 30 seconds, to obtain a polycarbonate resin molded product (layer A).
[0119] (2) Synthesis of urethane (meth)acrylate compound (component (d)) [Synthesis Example 1] Synthesis of urethane (meth)acrylate compound (UA1) In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and an air inlet, 222.3 parts (1.00 mol) of isophorone diisocyanate and 300 ppm of dibutyltin dilaurate were charged and dissolved by heating to 70° C. Then, air was introduced into the liquid, and 934.9 parts (2.10 mol) of pentaerythritol triacrylate and 2.1 parts of methylethylhydroquinone were charged and reacted at the same temperature for 5 hours. The reaction was terminated when it was confirmed that the residual isocyanate group was 0.3%, and a hexafunctional urethane acrylate compound (UA1) was obtained.
[0120] [Synthesis Example 2] Synthesis of urethane (meth)acrylate compound (UA2) In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and an air inlet, 333.5 parts (0.50 mol) of isophorone diisocyanate trimer, 558.3 parts of ethyl acetate, and 300 ppm of dibutyltin dilaurate were charged and dissolved by heating to 70 ° C. Then, air was introduced into the liquid, and 703.4 parts (1.58 mol) of pentaerythritol triacrylate and 1.06 parts of methylethylhydroquinone were charged and reacted at the same temperature for 5 hours. The reaction was terminated after confirming that the residual isocyanate group was 0.3%, and a 9-functional urethane acrylate compound (UA2) was obtained. The solid content of the resulting mixed liquid was 65 mass %.
[0121] [Comparative Synthesis Example 1] Synthesis of urethane (meth)acrylate compound (UA3) In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a dropping funnel with a heat retention function, 265 parts (1.00 mol) of dicyclohexylmethane diisocyanate and 300 ppm of di-n-butyltin dilaurate were charged and heated to 50°C. Then, 800 g (1 mol) of polycarbonate diol (trade name: Kuraray Polyol C-770, manufactured by Kuraray Co., Ltd., weight average molecular weight 800) was dropped as a diol compound over 4 hours. After the dropwise addition, the mixture was stirred at 50°C for 2 hours and heated to 70°C over 1 hour. Then, 232 g (2 mol) of 2-hydroxyethyl acrylate (HEA) was dropped over 2 hours, and the reaction was continued for another 2 hours. The reaction was terminated after confirming that the residual isocyanate group was 0.3%, and a bifunctional urethane acrylate compound (UA3) was obtained.
[0122] [Comparative Synthesis Example 2] Synthesis of urethane (meth)acrylate compound (UA4) In a four-neck flask equipped with a thermometer, a stirrer, a water-cooled condenser, and a dropping funnel with a heat retention function, 265 parts (1.00 mol) of dicyclohexylmethane diisocyanate and 300 ppm of di-n-butyltin dilaurate were charged and heated to 50°C. Then, 800 g (1 mol) of polyether diol (trade name: PTG850SN, manufactured by Hodogaya Chemical Co., Ltd., weight average molecular weight 800) was dropped as a diol compound over 4 hours. After the dropwise addition, the mixture was stirred at 50°C for 2 hours and heated to 70°C over 1 hour. Then, 232 g (2 mol) of 2-hydroxyethyl acrylate (HEA) was dropped over 2 hours, and the reaction was continued for another 2 hours. The reaction was terminated after confirming that the residual isocyanate group was 0.3%, and a bifunctional urethane acrylate compound (UA4) was obtained.
[0123] (3) Preparation of active energy ray-curable resin composition [Formulation Example 1] Preparation of active energy ray-curable resin composition A composition containing mono- or polypentaerythritol poly(meth)acrylate modified with caprolactone, in which n=1 in the structure of formula (2), two of six Xs are "caprolactone-modified (meth)acryloyloxy groups" and the remaining four Xs are "(meth)acryloyloxy groups", and is modified with caprolactone), KAYARAD DPCA-20 manufactured by Nippon Kayaku Co., Ltd., ARONIX M315 manufactured by Toagosei Co., Ltd., and the solution of the urethane acrylate compound (UA1) obtained in Synthesis Example 1 were mixed in a solid content ratio of 54:13:33, and 2.5 parts of benzophenone as a photopolymerization initiator and Omnirad 1.2 parts of TPO (manufactured by IGM), 1.2 parts of Tinuvin 400 (manufactured by BASF) as an ultraviolet absorber, 3.6 parts of Adeka STAB LA-63P (manufactured by ADEKA) as a hindered amine light stabilizer, and 0.01 parts of BYK-333 (manufactured by BYK-Chemie) as a leveling agent were added, and the mixture was diluted with propylene glycol monomethyl ether to a solids content of 24%, to obtain an active energy ray-curable resin composition (B-1).
[0124] (4) Method for applying active energy ray-curable resin composition The obtained active energy ray curable resin composition (B-1) was applied by air spray onto the layer A obtained in (1) above so that the film thickness after drying would be 6 μm, and the coating film was dried by heating in an oven at 80° C. for 3 minutes. Next, in the air, ultraviolet rays having a wavelength of 340 nm or more and 380 nm or less were irradiated at 100 mW / cm using a high-pressure mercury lamp. 2 , 800mJ / cm 2 The laminate was then exposed to light at a wavelength of 1000 nm to obtain a laminate covered with a cured film (layer B).
[0125] (5) Adhesion For the laminate obtained in (4) above, the adhesion between the cured film (layer B) and the substrate (layer A) was evaluated in accordance with the cross-cut peel test of JIS K-5400 (number of cross-cuts: 100). ◯: The number of cured films remaining after the cross-cut peel test was 100 / 100. ×: The number of cured films remaining after the cross-cut peel test was 99 / 100 or less.
[0126] (6) Hot water resistance The laminate obtained in (4) above was left to stand in a warm bath adjusted to a temperature of 80°C for 8 hours, and then removed, and the adhesion between the cured film (layer B) and the substrate (layer A) was evaluated by the method in (5) above. ◯: The number of cured films remaining after the cross-cut peel test was 100 / 100. ×: The number of cured films remaining after the cross-cut peel test was 99 / 100 or less.
[0127] (7) Pencil hardness: The laminate obtained in (4) above was measured using a JIS-compliant pencil hardness tester (manufactured by Taiyu Kizai Co., Ltd.) based on the conditions of JIS K-5400, and the pencil hardness was evaluated based on the hardest pencil grit that did not cause scratches. The pencil hardness of the laminate is preferably 2H or more, and more preferably, the hardness of the laminate is improved by two or more steps (for example, from F to 2H) compared to the hardness of the A layer. If the pencil hardness is less than H, the obtained molded product may be easily scratched and the appearance may be easily damaged. In addition, if the hardness of the laminate is improved by less than two steps compared to the hardness of the A layer, the cost-effectiveness of forming the hard coat layer (B layer) may be easily impaired. The pencil hardness is expressed in the order of 7H, 6H, 5H, 4H, 3H, 2H, H, F, HB, B, 2B, 3B, and 4B from the hardest to the hardest. In the present invention, H or more is considered to be acceptable.
[0128] (8) Scratch resistance 150 g / cm2 on the surface of the cured film of the laminate obtained in (4) above 2 A scratch test was performed by moving steel wool #0000 back and forth 20 times under a load of 1000 g / m. The haze value was measured before and after the scratch test using a haze meter (product name: HM-65W, manufactured by Murakami Color Research Laboratory Co., Ltd.), and the scratch resistance was evaluated based on the following criteria. ⊚: The increased haze value is 0% or more and less than 0.5%. ◯: The increased haze value is 0.5% or more and less than 1.0%. △: The increased haze value is 1.0% or more and less than 2.0%. ×: The increased haze value is 2.0% or more.
[0129] (9) Weather resistance The weather resistance test for the laminate obtained in (4) was carried out in accordance with JIS B7753 using a Sunshine Weather Meter S60 manufactured by Suga Test Instruments Co., Ltd. The light source was a Sunshine Carbon Arc (Ultra Long Life Carbon 4 pairs) with a discharge voltage of 50 V and a discharge current of 60 A, and the surface of the cured film of the laminate was irradiated and sprayed (rainfall) under the conditions of a black panel temperature of 63°C and a relative humidity of 50%. The surface spray (rainfall) time was 12 minutes / hour, and a type A glass filter was used. After 2000 hours and 3000 hours of testing, the appearance was evaluated based on the following criteria. ⊚: No cracking, whitening, or peeling of the cured film occurs after 3000 hours of evaluation. ◯: In the evaluation after 2000 hours, none of the following occurred: cracks, whitening, or peeling of the cured film. In the evaluation after 3000 hours, at least one of the following occurred: cracks, whitening, or peeling of the cured film. ×: At least one of cracks, whitening, and peeling of the cured film occurs after 2000 hours of evaluation.
[0130] The abbreviations for compounds used in the following examples are as follows. (Polycarbonate resin) A-1: Isosorbide / 1,4-cyclohexanedimethanol = 70 / 30 mol% copolymer polycarbonate (Mitsubishi Chemical Corporation: Durabio D7340R) A-2: Bisphenol A polycarbonate (Teijin Ltd., PANLITE L-1225Z) DHPA: Dipentaerythritol penta / hexaacrylate ·PETA: Pentaerythritol tri / tetraacrylate ·PGM: Propylene glycol monomethyl ether
[0131] [Example 1] A layer A was formed using the polycarbonate resin (A-1) by the method (1) above, and a layer B was formed on the surface of the layer A by the method (4) above using the active energy ray resin composition (B-1) to obtain a laminate. The results of evaluating the obtained laminate according to the methods (5) to (9) above are shown in Table 1.
[0132] [Examples 2 to 8, Comparative Examples 1 to 7] A laminate was obtained in the same manner as in Example 1, except that the polycarbonate resin and the active energy ray-exposed resin composition shown in Tables 1 and 2 were used. The evaluation results of the obtained laminate are shown in Tables 1 and 2.
[0133] [Table 1]
[0134] [Table 2]
[0135] The laminates of Examples 1 to 8 were superior to the laminates shown in the Comparative Examples in terms of adhesion, durability, hardness, weather resistance, and other evaluation items, with no △, ×, or fail marks in each characteristic evaluation. Among them, Examples 1, 4, 7, and 8 were particularly excellent in weather resistance, and Examples 2, 3, and 6 were particularly excellent in surface hardness. On the other hand, the active energy ray curable resin compositions of Comparative Examples 1 to 4 did not contain either the component (c) or the component (d), and therefore were insufficient in any of adhesion, hardness, and weather resistance. In Comparative Example 5, the amount of the component (c) was small, and therefore the scratch resistance was insufficient, and in Comparative Example 6, the amount of the component (d) was small, and therefore the weather resistance was insufficient. Comparative Example 7 is a laminate using bisphenol A type polycarbonate that does not contain the structural unit (a) derived from the dihydroxy compound, but the pencil hardness of the laminate was HB, and the molded product was easily scratched, and the weather resistance was also insufficient. [Industrial Applicability]
[0136] A laminate having a layer (layer A) containing the polycarbonate resin of the present invention and a layer (layer B) obtained by curing an active energy ray-curable resin composition containing mono- or polypentaerythritol poly(meth)acrylate represented by the general formula (2) and a tri- or higher functional urethane (meth)acrylate compound, is excellent in surface hardness, adhesion between layers A and B, and weather resistance, and can provide resin molded products that are applicable in a wide range of fields, such as automobile parts, medical parts, films, sheets, containers such as bottles, building materials, various housing materials for mobile phones, optical disc substrates, and plastic lenses.
Claims
1. A laminate having a layer A containing a polycarbonate resin and a layer B obtained by curing an active energy ray-curable resin composition, at least one of the outermost layers being the layer B, The polycarbonate resin has a structural unit (a) derived from a dihydroxy compound having a structure represented by the following general formula (1): The active energy ray-curable resin composition contains a mono- or polypentaerythritol poly(meth)acrylate (c) represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d), a ratio of the mono- or polypentaerythritol poly(meth)acrylate (c) to a total mass of the active energy ray-curable compound in the active energy ray-curable resin composition is 10 to 90 mass%, and a ratio of the urethane (meth)acrylate compound (d) is 10 to 90 mass%, based on the total mass of the active energy ray-curable compound in the active energy ray-curable resin composition. 【Chemistry 1】 【Chemistry 2】 [In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., CH 2 =CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH 2 =CR-CO(O(CH 2 ) 5 C=O) y -O-, where R is a hydrogen atom or a methyl group, and y is an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.]
2. The laminate according to claim 1 , wherein the urethane (meth)acrylate compound (d) is a urethane (meth)acrylate compound having a nurate skeleton.
3. 3. The laminate according to claim 1, wherein at least one of X's in the formula (2) is a (meth)acryloyloxy group modified with caprolactone.
4. The laminate according to claim 1 or 2, wherein the active energy ray-curable resin composition contains at least one of an ultraviolet absorber (e) and a hindered amine-based light stabilizer (f).
5. The laminate according to claim 1 or 2, which is used as an automobile component.
6. A method for producing a laminate having a layer A containing a polycarbonate resin and a layer B obtained by curing an active energy ray-curable resin composition, wherein at least one of the outermost layers is the layer B, comprising the steps of: and applying the active energy ray-curable resin composition onto at least one surface of the layer A, and then irradiating the layer A with active energy rays to form the layer B. The polycarbonate resin has a structural unit (a) derived from a dihydroxy compound having a structure represented by the following general formula (1): The active energy ray-curable resin composition contains a mono- or polypentaerythritol poly(meth)acrylate (c) represented by the following general formula (2) and a tri- or higher functional urethane (meth)acrylate compound (d), a ratio of the mono- or polypentaerythritol poly(meth)acrylate (c) to a total mass of the active energy ray-curable compound in the active energy ray-curable resin composition is 10 to 90 mass%, and a ratio of the urethane (meth)acrylate compound (d) is 10 to 90 mass%. 【Chemistry 3】 【Chemistry 4】 [In formula (2), "4+2n" X's each independently represent a (meth)acryloyloxy group (i.e., CH 2 =CR-COO-, where R represents a hydrogen atom or a methyl group), a (meth)acryloyloxy group modified with caprolactone (i.e., CH 2 =CR-CO(O(CH 2 ) 5 C=O) y -O-, where R is a hydrogen atom or a methyl group, and y is an integer of 1 to 5.) and a hydroxy group. Also, n is an integer of 0 to 4.]
Citation Information
Patent Citations
Polycarbonate resin molding improved in wearing resistance and weatherability and production thereof
JP1995247383A
Laminate
JP2014240200A
Laminated body
JP2016068438A
Bus switching control system
JP1988049866A
Polycarbonate copolymer and method for producing the same
JP2008024919A