Non-aqueous electrolyte secondary battery and manufacturing method thereof
The method improves Li precipitation resistance and high-temperature storage characteristics in non-aqueous electrolyte secondary batteries by optimizing the capacity ratio of negative to positive electrodes and applying voltage to decompose a Li compound on the battery case, ensuring uniform Li ion distribution.
Patent Information
- Application Number
- JP2023050052
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Non-aqueous electrolyte secondary batteries, particularly those with a wound electrode body, face challenges in Li precipitation resistance and high-temperature storage characteristics, especially when the number of turns is large.
A manufacturing method involving a wound electrode body with a specific capacity ratio of negative to positive electrodes, a coating layer containing a Li compound on the battery case inner surface, and controlled voltage application to decompose the Li compound and supply ions to the outermost negative electrode.
The method enhances Li precipitation resistance and high-temperature storage characteristics by ensuring uniform Li ion distribution and reducing capacity deterioration.
Smart Images

Figure 2024139211000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a non-aqueous electrolyte secondary battery. The present invention also relates to a method for producing the non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, nonaqueous electrolyte secondary batteries such as lithium ion secondary batteries have been suitably used as portable power sources for personal computers, mobile terminals, and the like, and as power sources for driving vehicles such as electric vehicles (BEVs), hybrid electric vehicles (HEVs), and plug-in hybrid electric vehicles (PHEVs), among others.
[0003] A nonaqueous electrolyte secondary battery typically includes an electrode assembly in which a positive electrode and a negative electrode are insulated by a separator. One common form of the electrode assembly is a wound electrode assembly in which a laminate of a positive electrode, a negative electrode, and a separator is wound. A technique is known in which a metallic lithium foil or the like is placed in a battery case of a nonaqueous electrolyte secondary battery including a wound electrode assembly, and lithium ions are released into the nonaqueous electrolyte (see, for example, Patent Document 1, etc.). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 05-144473 Summary of the Invention [Problem to be solved by the invention]
[0005] In recent years, there has been a demand for a non-aqueous electrolyte secondary battery with a higher capacity for use as a power source for driving a vehicle. As a measure for increasing the capacity, there is a method of increasing the number of windings (i.e., the number of turns) in order to make the wound electrode body multi-layered. As a result of intensive research by the present inventors, it has been found that there is room for improvement in the Li precipitation resistance and high-temperature storage characteristics of the non-aqueous electrolyte secondary battery, especially when the number of turns of the wound electrode body is large.
[0006] Therefore, an object of the present invention is to provide a nonaqueous electrolyte secondary battery including a wound electrode body, which has a nonaqueous electrolyte that is excellent in Li deposition resistance and high-temperature storage characteristics. [Means for solving the problem]
[0007] The method for producing a nonaqueous electrolyte secondary battery disclosed herein includes the steps of: preparing an assembly in which a wound electrode body in which a laminate including a positive electrode, a negative electrode, and a separator interposed between them is wound, and a nonaqueous electrolyte is housed in a metal battery case, wherein the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more, the outermost periphery of the wound electrode body is the negative electrode, and the inner surface of the battery case has a coating layer containing a Li compound; applying a voltage between the battery case and the negative electrode so as to decompose the Li compound, thereby supplying Li ions from the Li compound to the negative electrode at the outermost periphery of the wound electrode body; and applying a voltage between the positive electrode and the negative electrode to perform an initial charge.
[0008] According to such a configuration, it is possible to provide a nonaqueous electrolyte secondary battery including a wound electrode body, which has excellent Li deposition resistance and high-temperature storage characteristics.
[0009] The nonaqueous electrolyte secondary battery disclosed herein includes a wound electrode assembly in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween is wound, a nonaqueous electrolyte, and a metal battery case that houses them. The ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more. The nonaqueous electrolyte secondary battery has a high Li element accumulation region on the inner surface of the battery case.
[0010] According to such a configuration, a nonaqueous electrolyte secondary battery including the wound electrode body has excellent Li deposition resistance and high-temperature storage characteristics. [Brief description of the drawings]
[0011] [Figure 1] 2 is a flowchart showing each step of a method for producing a lithium ion secondary battery according to one embodiment of the present invention. [Diagram 2] 4 is a cross-sectional view showing a schematic internal structure of an assembly prepared in an assembly preparation step of a manufacturing method according to one embodiment of the present invention. FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view taken along line XX in FIG. 2. [Figure 4] 3 is a schematic exploded view showing the configuration of the wound electrode body of FIG. 2. [Diagram 5] 1 is a cross-sectional view showing a schematic internal structure of a lithium-ion secondary battery obtained by a manufacturing method according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. Matters not mentioned in this specification but necessary for carrying out the present invention can be understood as design matters for a person skilled in the art based on the prior art in the relevant field. The present invention can be carried out based on the contents disclosed in this specification and the technical common sense in the relevant field. In addition, in the following drawings, members and parts having the same function are described with the same reference numerals. Furthermore, the dimensional relationships (length, width, thickness, etc.) in each drawing do not reflect the actual dimensional relationships. In addition, the numerical range expressed as "A to B" in this specification includes A and B.
[0013] In this specification, the term "secondary battery" refers to an electricity storage device that can be repeatedly charged and discharged, and includes so-called storage batteries and electricity storage elements such as electric double layer capacitors. In addition, in this specification, the term "lithium ion secondary battery" refers to a secondary battery that uses lithium ions as a charge carrier and realizes charging and discharging by the transfer of charge associated with the lithium ions between the positive and negative electrodes.
[0014] As shown in the flowchart of FIG. 1, the method for producing a nonaqueous electrolyte secondary battery according to this embodiment includes a step of preparing an assembly in which a wound electrode body, in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween, is wound, and a nonaqueous electrolyte is housed in a metal battery case (hereinafter also referred to as an "assembly preparation step") S101, in which the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more, the outermost periphery of the wound electrode body is the negative electrode, and the inner surface of the battery case has a coating layer containing a Li compound; a step of applying a voltage between the battery case and the negative electrode so as to decompose the Li compound, and supplying Li ions from the Li compound to the negative electrode at the outermost periphery of the wound electrode body (hereinafter also referred to as a "voltage application step") S102; and a step of applying a voltage between the positive electrode and the negative electrode to perform initial charging (hereinafter also referred to as an "initial charging step") S103.
[0015] Hereinafter, the steps of the method for manufacturing a nonaqueous electrolyte secondary battery according to this embodiment will be described in detail using a flat prismatic lithium ion secondary battery having a flat wound electrode body and a flat battery case as an example, but it is not intended that the present invention be limited to the embodiment described above.
[0016] The assembly 100 prepared in the assembly preparation step S101 is shown in Figures 2 to 4. Figure 2 is a cross-sectional view showing a schematic internal structure of the assembly 100. Figure 3 is a cross-sectional view of the assembly 100 taken along line XX in Figure 2. Figure 4 is a schematic exploded view showing the configuration of the wound electrode body 20.
[0017] 2 and 3, the assembly 100 includes a flat-shaped wound electrode body 20, a non-aqueous electrolyte 80, and a battery case (i.e., an outer container) 30 that houses the wound electrode body 20 and the non-aqueous electrolyte 80. Note that Figs. 2 and 3 do not accurately represent the amount of non-aqueous electrolyte 80.
[0018] 2 and 4, the wound electrode body 20 has a configuration in which a laminate in which a positive electrode sheet 50 and a negative electrode sheet 60 are stacked with two long first separators 70 interposed therebetween is wound in the longitudinal direction. The positive electrode sheet 50 has a configuration in which a positive electrode active material layer 54 is formed along the longitudinal direction on one or both sides (both sides here) of a long positive electrode current collector 52. The negative electrode sheet 60 has a configuration in which a negative electrode active material layer 64 is formed along the longitudinal direction on one or both sides (both sides here) of a long negative electrode current collector 62. The positive electrode active material layer-free portion 52a (i.e., a portion where the positive electrode active material layer 54 is not formed and the positive electrode current collector 52 is exposed) and the negative electrode active material layer-free portion 62a (i.e., a portion where the negative electrode active material layer 64 is not formed and the negative electrode current collector 62 is exposed) are formed so as to protrude outward from both ends in the winding axis direction (i.e., the sheet width direction perpendicular to the longitudinal direction) of the wound electrode body 20. The positive electrode active material layer-free portion 52a and the negative electrode active material layer-free portion 62a are joined to the positive electrode current collector 42a and the negative electrode current collector 44a, respectively.
[0019] In this embodiment, the outermost periphery of the wound electrode body 20 is the negative electrode 60. Therefore, as shown in Fig. 4, in the wound electrode body 20, the positive electrode 50 is located on the inner periphery side (in other words, on the winding axis side).
[0020] The greater the number of windings of the wound electrode body 20, the greater the effect of improving the Li precipitation resistance and the high-temperature storage characteristics. Therefore, the number of windings of the wound electrode body 20 is preferably 4 turns (in other words, 4 times) or more, more preferably 10 turns or more, even more preferably 20 turns or more, even more preferably 25 turns or more, and particularly preferably 30 turns or more. The number of windings of the wound electrode body 20 may be 100 turns or less, 70 turns or less, or 50 turns or less.
[0021] The ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 (negative electrode 60 / positive electrode 50) is 1.2 or more. When the capacity ratio is 1.2 or more, the Li precipitation resistance of the obtained lithium ion secondary battery 200 can be improved. From the viewpoint of higher Li precipitation resistance, the capacity ratio is preferably 1.3 or more. On the other hand, the capacity ratio may be less than 2.0, 1.8 or less, or 1.5 or less. Note that the capacity of the positive electrode 50 and the capacity of the negative electrode 60 are both theoretical capacities and can be calculated according to a known method.
[0022] A known positive electrode current collector used in lithium ion secondary batteries may be used as the positive electrode current collector 52 constituting the positive electrode sheet 50, and an example of such a positive electrode current collector is aluminum foil, etc. The thickness of the positive electrode current collector 52 is not particularly limited and is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0023] The positive electrode active material layer 54 contains a positive electrode active material. As the positive electrode active material, a known positive electrode active material used in a lithium ion secondary battery may be used. Specifically, for example, as the positive electrode active material, a lithium composite oxide, a lithium transition metal phosphate compound, or the like may be used. The crystal structure of the positive electrode active material is not particularly limited, and may be a layered structure, a spinel structure, an olivine structure, or the like.
[0024] Examples of the lithium composite oxide include lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0025] In this specification, the term "lithium nickel cobalt manganese composite oxide" includes oxides containing Li, Ni, Co, Mn, and O as constituent elements, as well as oxides containing one or more additional elements other than those. Examples of such additional elements include transition metal elements and typical metal elements such as Mg, Ca, Al, Ti, V, Cr, Y, Zr, Nb, Mo, Hf, Ta, W, Na, Fe, Zn, and Sn. The additional element may be a semimetal element such as B, C, Si, or P, or a nonmetal element such as S, F, Cl, Br, or I. This also applies to the above-mentioned lithium nickel composite oxide, lithium cobalt composite oxide, lithium manganese composite oxide, lithium nickel manganese composite oxide, lithium nickel cobalt aluminum composite oxide, and lithium iron nickel manganese composite oxide.
[0026] Examples of the lithium transition metal phosphate compound include lithium iron phosphate (LiFePO4), lithium manganese phosphate (LiMnPO4), and lithium manganese iron phosphate.
[0027] These positive electrode active materials may be used alone or in combination of two or more. The positive electrode active material is preferably a lithium nickel cobalt manganese based composite oxide.
[0028] The average particle diameter (median diameter: D50) of the positive electrode active material is not particularly limited, but is, for example, 0.05 μm to 25 μm, preferably 1 μm to 20 μm, and more preferably 3 μm to 15 μm. The average particle diameter (D50) of the positive electrode active material can be determined, for example, by a laser diffraction scattering method.
[0029] The content of the positive electrode active material in the positive electrode active material layer 54 (i.e., the content of the positive electrode active material relative to the total mass of the positive electrode active material layer 54) is not particularly limited, but is, for example, 80 mass % or more, preferably 85 mass % or more, and more preferably 90 mass % or more.
[0030] The positive electrode active material layer 54 may contain a component (i.e., an optional component) other than the positive electrode active material. Examples of the optional component include a conductive material, a binder, and the like. As the conductive material, for example, a carbon material such as carbon black (e.g., acetylene black), carbon nanotubes (CNT), graphite, and the like may be suitably used. As the binder, for example, polyvinylidene fluoride (PVDF) and the like may be used. When CNT is used as the conductive material, the positive electrode active material layer 54 may further contain a dispersant for CNT.
[0031] The content of the conductive material in the positive electrode active material layer 54 is not particularly limited, but is preferably from 0.1% by mass to 15% by mass, and more preferably from 0.5% by mass to 13% by mass. The content of the binder in the positive electrode active material layer 54 is not particularly limited, but is preferably from 1% by mass to 15% by mass, and more preferably from 1.5% by mass to 10% by mass.
[0032] The thickness of the positive electrode active material layer 54 is not particularly limited, but is, for example, from 10 μm to 300 μm, and preferably from 20 μm to 200 μm.
[0033] The positive electrode sheet 50 may contain an insulating layer (not shown) at the boundary between the positive electrode active material layer non-forming portion 52a and the positive electrode active material layer 54. The insulating layer contains, for example, ceramic particles.
[0034] A known negative electrode current collector used in lithium ion secondary batteries may be used as the negative electrode current collector 62 constituting the negative electrode sheet 60, and an example of such a collector is copper foil. The thickness of the negative electrode current collector 62 is not particularly limited and is, for example, 5 μm or more and 35 μm or less, and preferably 7 μm or more and 20 μm or less.
[0035] The negative electrode active material layer 64 contains a negative electrode active material. As the negative electrode active material, for example, a carbon material such as graphite, hard carbon, soft carbon, etc. The graphite may be natural graphite or artificial graphite, or may be amorphous carbon-coated graphite in which graphite is coated with an amorphous carbon material.
[0036] The average particle diameter (median diameter: D50) of the negative electrode active material is not particularly limited, but is, for example, 0.1 μm to 50 μm, preferably 1 μm to 25 μm, and more preferably 5 μm to 20 μm. The average particle diameter (D50) of the negative electrode active material can be determined, for example, by a laser diffraction scattering method.
[0037] The negative electrode active material layer 64 may contain components other than the active material, such as a binder, a thickener, etc. As the binder, for example, styrene butadiene rubber (SBR), polyvinylidene fluoride (PVDF), etc. may be used. As the thickener, for example, carboxymethyl cellulose (CMC), etc. may be used.
[0038] The content of the negative electrode active material in the negative electrode active material layer 64 is preferably 90% by mass or more, and more preferably 95% by mass or more and 99% by mass or less. The content of the binder in the negative electrode active material layer 64 is preferably 0.1% by mass or more and 8% by mass or less, and more preferably 0.5% by mass or more and 3% by mass or less. The content of the thickener in the negative electrode active material layer 64 is preferably 0.3% by mass or more and 3% by mass or less, and more preferably 0.5% by mass or more and 2% by mass or less.
[0039] The thickness of the negative electrode active material layer 64 is not particularly limited, but is, for example, not less than 10 μm and not more than 300 μm, and preferably not less than 20 μm and not more than 200 μm.
[0040] The first separator 70 may be a porous sheet (film) made of a resin such as polyethylene (PE), polypropylene (PP), polyester, cellulose, or polyamide. Such a porous sheet may have a single-layer structure or a laminated structure of two or more layers (for example, a three-layer structure in which a PP layer is laminated on both sides of a PE layer). A heat-resistant layer (HRL) may be provided on the surface of the first separator 70. The thickness of the first separator 70 is not particularly limited, but is, for example, 5 μm to 50 μm, and preferably 10 μm to 30 μm.
[0041] The nonaqueous electrolyte 80 typically contains a nonaqueous solvent and a supporting salt (electrolyte salt). As the nonaqueous solvent, various organic solvents such as carbonates, ethers, esters, nitriles, sulfones, and lactones that are used in general electrolytes of lithium ion secondary batteries can be used without any particular limitation. Among them, carbonates and esters are preferable, and specific examples thereof include ethylene carbonate (EC), propylene carbonate (PC), diethyl carbonate (DEC), dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), methyl acetate, and methyl propionate. Such nonaqueous solvents can be used alone or in appropriate combination of two or more.
[0042] As the supporting salt, for example, a lithium salt such as LiPF6, LiBF4, lithium bis(fluorosulfonyl)imide (LiFSI) (preferably LiPF6) can be suitably used. The concentration of the supporting salt is preferably 0.7 mol / L or more and 1.3 mol / L or less.
[0043] The nonaqueous electrolyte 80 may contain various additives other than the above-mentioned components, such as film-forming agents such as vinylene carbonate (VC) and oxalate complexes; gas generating agents such as biphenyl (BP) and cyclohexylbenzene (CHB); and thickeners, as long as the effects of the present invention are not significantly impaired.
[0044] The battery case 30 has a case body 32 and a lid 34. The case body 32 has a flattened rectangular parallelepiped shape, and one of its faces (the upper face in the figure) is an opening. The lid 34 has a substantially rectangular shape that fits the shape of the opening. The lid 34 is provided with a positive electrode terminal 42 and a negative electrode terminal 44 for external connection, and a thin-walled safety valve 36 that is set to release the internal pressure when the internal pressure of the battery case 30 rises to a predetermined level or higher. The lid is also provided with an injection hole (not shown) for injecting the non-aqueous electrolyte 80. The positive electrode terminal 42 is electrically connected to the positive electrode current collector plate 42a. The negative electrode terminal 44 is electrically connected to the negative electrode current collector plate 44a.
[0045] In a voltage application step S102 described later, a current is passed between the battery case 30 and the negative electrode 60, so the battery case 30 has electrical conductivity. Therefore, the material of the battery case 30 is a metal (e.g., aluminum, stainless steel, nickel-plated steel, etc.). The battery case 30 is preferably made of aluminum because it has good electrical conductivity, thermal conductivity, strength, and is lightweight.
[0046] According to the study by the present inventor, when the wound electrode body is multi-layered, the uniform diffusion of Li ions is likely to be insufficient, and the salt concentration becomes uneven in the negative electrode at the outermost periphery of the wound electrode body, which has been found to cause a decrease in high-temperature storage characteristics (particularly, capacity deterioration when left at high temperatures for a long period of time). Therefore, in this embodiment, in order to supply Li ions to the negative electrode 60 at the outermost periphery of the wound electrode body 20, the inner surface of the battery case 30 (particularly the inner surface of the case body 32) has a coating layer 90 containing a Li compound. The Li compound is a compound that can be decomposed by application of a voltage to release Li ions in the voltage application step S102 described later. A suitable example of the Li compound is at least one selected from the group consisting of lithium carbonate, lithium chloride, lithium nitrate, lithium dihydrogen carbonate, and lithium phosphate, and among them, lithium carbonate is preferable. By using such a Li compound, it is possible to release more Li ions at a lower cost than using a lithium ion donor (typically, a compound that can be used as a positive electrode active material) that releases Li ions without decomposition by application of a voltage.
[0047] The coating layer 90 may contain only a Li compound, or may contain other components. For example, when the coating layer 90 contains a conductive material (e.g., carbon black, etc.) in addition to a Li compound, the Li compound contained in the coating layer 90 can be efficiently electrolyzed. The content of the conductive material in the coating layer 90 is, for example, 1 mass % to 20 mass %, and preferably 5 mass % to 15 mass %.
[0048] The coating layer 90 may be formed on any inner surface of the battery case 30 as long as it can release Li ions to the non-aqueous electrolyte 80. The position of the coating layer 90 on the inner surface of the battery case 30 is not particularly limited. Typically, at least a part (preferably the entirety) of the coating layer 90 is in contact with the non-aqueous electrolyte 80. In the illustrated example, the coating layer 90 is formed on the inner surface of the case main body 32, which faces the flat surface of the wound electrode body 20. In this case, it is particularly easy to supply Li ions to the negative electrode 60 at the outermost periphery of the wound electrode body 20. The wound electrode body 20 has a flat portion and R portions at both ends thereof, and the flat surface of the wound electrode body 20 refers to the main surface of this flat portion (i.e., the surface with the largest area). The flat surface of the wound electrode body 20 does not have to be completely flat.
[0049] Here, the wound electrode body 20 has a pair of (i.e., two) flat surfaces. Two of the inner surfaces of the battery case 30 face these two flat surfaces, respectively. In the illustrated example, a coating layer 90 is formed on one of the inner surfaces of the battery case 30 and faces one of the flat surfaces of the wound electrode body 20. The coating layer 90 is preferably provided on two surfaces of the inner surface of the battery case 30 that face the flat surfaces of the wound electrode body 20. In this case, the Li precipitation resistance and high-temperature storage characteristics of the obtained lithium-ion secondary battery 200 are further improved.
[0050] The coating layer 90 is not in contact with the wound electrode body 20 and is separated therefrom. The coating layer 90 is insulated from the wound electrode body 20 via a second separator 72. The second separator 72 may be the same as or similar to the first separator 70. The second separator 72 may be wound around the wound electrode body 20 and surround the outer periphery of the wound electrode body 20. Alternatively, the second separator 72 may have a bag shape and house the wound electrode body 20 inside. Note that the method of insulating the coating layer 90 from the wound electrode body 20 is not limited to this.
[0051] The assembly 100 can be prepared, for example, as follows. First, a battery case 30 including a case body 32 and a lid 34, and a coating liquid containing a Li compound are prepared. The coating liquid may be a solution or a dispersion liquid. The coating liquid is applied to the inner surface of the case body 32 of the battery case 30, and dried to form a coating layer 90. Meanwhile, a positive terminal 42, a negative terminal 44, a positive current collector 42a, and a negative current collector 44a are attached to the lid 34 of the battery case 30.
[0052] The wound electrode body 20 is produced according to a known method. For example, a positive electrode sheet 50, a negative electrode sheet 60, and two first separator sheets 70 are prepared. Using a known winding machine, the positive electrode sheet 50 and the negative electrode sheet 60 are wound while being stacked so that the first separator sheet 70 is interposed between them. The obtained wound body is processed into a flat shape by pressing from its side direction, and the wound electrode body 20 is produced.
[0053] The positive electrode current collector 42a and the negative electrode current collector 44a are attached to the prepared wound electrode body 20 by resistance welding, ultrasonic welding, or the like. This connects the wound electrode body 20 to the lid 34 of the battery case 30. A second separator 72 is prepared and the second separator 72 is abutted against the wound electrode body 20. The wound electrode body 20 is inserted into the case body 32 from the opening of the case body 32. At this time, the second separator 72 is positioned between the wound electrode body 20 and the coating layer 90 on the inner surface of the case body 32. Thereafter, the case body 32 and the lid 34 are sealed by laser welding or the like.
[0054] The non-aqueous electrolyte 80 is prepared according to a known method. The non-aqueous electrolyte 80 is poured into the battery case 30 through the pouring hole in the lid 34 of the battery case 30, and the pouring hole is sealed. In this manner, the assembly 100 can be obtained.
[0055] Next, the voltage application step S102 will be described. The voltage application step S102 can be performed using a known voltage application device (not shown). Specifically, for example, terminals of a voltage application device (for example, a charger, etc.) are attached to the battery case 30 and the negative electrode terminal 44, respectively, and a voltage is applied between the battery case 30 and the negative electrode 60. At this time, the voltage is applied with the battery case 30 as the anode and the negative electrode 60 as the cathode.
[0056] The magnitude of the voltage is appropriately set according to the type of Li compound, specifically, the decomposition start potential of the Li compound, and preferably, a voltage equal to or higher than the decomposition start potential of the Li compound is selected. The voltage applied in the voltage application step S102 is 4.10 V to 4.50 V (vs Li + / Li), and more preferably 4.20V to 4.35V (vsLi + / Li).
[0057] This voltage application decomposes the Li compound, and Li ions are released from the Li compound into the nonaqueous electrolyte 80. These Li ions move to the negative electrode 60 at the outermost periphery of the wound electrode body 20, and the Li ions are supplied to the negative electrode 60. In this manner, the voltage application step S102 can be performed.
[0058] Here, by using a compound that is decomposed by application of voltage as the Li compound, the Li ions can be supplied efficiently. Also, by supplying Li ions to the negative electrode 60 at the outermost periphery of the wound electrode body 20, it is possible to eliminate unevenness in the salt concentration in the negative electrode 60, thereby improving the high-temperature storage characteristics of the resulting lithium-ion secondary battery 200.
[0059] Next, the initial charging step S103 will be described. The initial charging step S103 can be performed according to a known method using a known voltage application device (not shown). The voltage application device may be the same as that used in the voltage application step S102.
[0060] Specifically, for example, terminals of a voltage application device are attached to the positive electrode terminal 42 and the negative electrode terminal 44, respectively, and a voltage is applied between the positive electrode 50 and the negative electrode 60. At this time, the voltage is applied with the positive electrode 50 as the anode and the negative electrode 60 as the cathode. The voltage application may be appropriately set depending on the configuration of the assembly (particularly, the type of positive electrode active material, the type of negative electrode active material, the composition of the non-aqueous electrolyte 80, etc.), and known conditions may be used.
[0061] This makes it possible to obtain the lithium ion secondary battery 200. After the initial charging step S103, a step of performing an aging treatment on the lithium ion secondary battery 200 may be further performed. The aging treatment can further eliminate unevenness in the salt concentration in the negative electrode 60 at the outermost periphery of the wound electrode body 20, and thus can further improve the high-temperature storage characteristics. The aging treatment is preferably performed at 60°C or higher in a charged state where the potential of the negative electrode 60 is 0.5V or higher. The aging temperature is more preferably 60°C to 80°C. The aging time is, for example, 1 hour or more, and preferably 5 hours to 48 hours.
[0062] The lithium ion secondary battery 200 obtained as described above has excellent high-temperature storage characteristics. Specifically, the capacity degradation when placed under high temperatures for a long period of time is suppressed. Therefore, the lithium ion secondary battery 200 has excellent durability. In addition, the lithium ion secondary battery 200 also has excellent Li precipitation resistance.
[0063] In the completed lithium ion secondary battery 200, the Li compound in the coating layer 90 is decomposed. Therefore, the portion where the coating layer 90 was present contains the remaining Li compound and decomposed products of the Li compound, and therefore may remain as a region with a high abundance ratio of the Li element. FIG. 5 shows a schematic cross-sectional view of the lithium ion secondary battery 200 corresponding to FIG. 3. As shown in FIG. 5, the lithium ion secondary battery 200 may have a high Li element accumulation region 92 on the inner surface of the battery case 30. In this specification, the "high Li element accumulation region" refers to a region on the inner surface of the battery case 30 where there is an attachment, and the attachment contains the Li element. The attachment may contain, in particular, a Li compound or a decomposed product of the Li compound. In the attachment, the ratio of Li atoms to all atoms may be 5 atomic % or more, or 10 atomic % or more. This ratio of Li atoms can be measured by a known method (e.g., ICP emission spectroscopy, etc.).
[0064] From another perspective, the lithium ion secondary battery 200 disclosed herein includes a wound electrode assembly 20 formed by winding a laminate including a positive electrode 50, a negative electrode 60, and a first separator 70 interposed therebetween, a nonaqueous electrolyte 80, and a metal battery case 30 that houses them. The ratio of the capacity of the negative electrode 60 to the capacity of the positive electrode 50 is 1.2 or more. The lithium ion secondary battery 200 has a high Li element accumulation region 92 on the inner surface of the battery case 30.
[0065] The lithium ion secondary battery 200 can be used for various purposes. Specific applications include portable power sources for personal computers, portable electronic devices, portable terminals, etc.; power sources for driving vehicles such as electric vehicles (BEVs), hybrid vehicles (HEVs), and plug-in hybrid vehicles (PHEVs); and storage batteries for small power storage devices, among which a power source for driving vehicles is preferable. The lithium ion secondary battery 200 can also be used in the form of a battery pack in which a plurality of batteries are typically connected in series and / or in parallel.
[0066] The above describes, as an example, a rectangular lithium ion secondary battery 200 including a flat wound electrode body 20. However, the lithium ion secondary battery can also be configured as a cylindrical lithium ion secondary battery or the like.
[0067] The secondary battery according to this embodiment can be constructed as a non-aqueous electrolyte secondary battery other than a lithium ion secondary battery in accordance with a known method.
[0068] Examples of the present invention will be described in detail below, but it is not intended that the present invention be limited to those shown in these examples.
[0069] Example 1 An aluminum battery case was prepared. This battery case included a case body and a lid, and had a rectangular parallelepiped shape. The lid was provided with an injection hole. A paste containing lithium carbonate and acetylene black (AB) in a mass ratio of 90:10 was prepared. The paste was applied to one of the inner surfaces with the largest area of the battery case body, and then dried. This formed a coating layer containing lithium carbonate and AB.
[0070] LiNi as a positive electrode active material powder 0.5 Co 0.2 Mn 0.3 O2 (NCM), acetylene black (AB) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were mixed in a mass ratio of NCM:AB:PVdF=90:5:5. This resulted in the preparation of a slurry for forming a positive electrode active material layer. This slurry was applied to both sides of an aluminum foil and then dried to form a positive electrode active material layer. The total basis weight of both sides at this time was 10 mg / cm. 2 Next, the positive electrode active material layer was 3 A positive electrode sheet was obtained by rolling and pressing the sheet so as to obtain a positive electrode sheet.
[0071] A negative electrode active material layer forming slurry was prepared by mixing natural graphite (C) as a negative electrode active material, styrene butadiene rubber (SBR) as a binder, and carboxymethyl cellulose (CMC) as a thickener with ion-exchanged water in a mass ratio of C:SBR:CMC=97:2:1. This slurry was applied to both sides of a copper foil and then dried to form a negative electrode active material layer. The total weight of both sides was 9 mg / cm. 2 Next, the negative electrode active material layer was 3 A roll press treatment was performed so that a negative electrode sheet was obtained.
[0072] In addition, polyolefin porous membranes were prepared as two first separators and one second separator. The prepared positive electrode sheet and negative electrode sheet were laminated with the first separator interposed therebetween. The obtained laminate was wound 30 turns to prepare a wound electrode body. At this time, the outermost periphery of the wound electrode body was set to be the negative electrode. Furthermore, a second separator sheet was wound around the outermost periphery of the wound electrode body, and the outermost negative electrode was covered with the second separator sheet.
[0073] Terminals were attached to this electrode body, and the electrode body was attached to the lid of the battery case. After that, the electrode body was housed in the battery case body, and the battery case and the lid were hermetically sealed. The negative electrode on the outermost periphery of the wound electrode body faced the coating layer. In addition, in the wound electrode body, the capacity ratio of the negative electrode to the positive electrode (negative electrode / positive electrode) was 1.2.
[0074] A mixed solvent containing ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a volume ratio of 25:40:35 was prepared. A non-aqueous electrolyte was prepared by dissolving LiPF6 in this mixed solvent at a concentration of 1.1 mol / L. The prepared non-aqueous electrolyte was injected into the battery case through the injection hole, and the injection hole was sealed to obtain an assembly.
[0075] A commercially available charger was prepared. Using this charger, a voltage of 4.3 V (vsLi) was applied between the battery case and the negative electrode of the assembly, with the battery case as the anode and the negative terminal as the cathode.+ A voltage of ( / Li) was applied. As a result, lithium carbonate in the coating layer on the inner surface of the battery case was decomposed, and Li ions were inserted into the outermost negative electrode of the wound electrode body.
[0076] Next, using this charger, with the positive electrode terminal as the anode and the negative electrode terminal as the cathode, the assembly was subjected to constant current charging up to 4.15 V at a current value of 0.1 C, and then discharged at a constant current down to 3 V. This charge and discharge was performed twice as the initial charge. The capacity at the time of the second discharge was measured and taken as the initial capacity.
[0077] After discharging the obtained lithium ion secondary battery down to 2 V, it was subjected to an aging treatment for 12 hours in a constant temperature layer at 60 °C. In this way, the lithium ion secondary battery for evaluation of Example 1 was obtained.
[0078] 〔Example 2〕 A lithium ion secondary battery for evaluation was obtained in the same manner as in Example 1, except that the capacity ratio of the negative electrode to the positive electrode (negative electrode / positive electrode) was changed to 1.3.
[0079] 〔Comparative Example 1〕 A lithium ion secondary battery for evaluation was obtained in the same manner as in Example 1, except that the capacity ratio of the negative electrode to the positive electrode (negative electrode / positive electrode) was changed to 1.1.
[0080] 〔Comparative Example 2〕 A lithium ion secondary battery for evaluation was obtained in the same manner as in Example 1, except that no voltage was applied between the battery case and the negative electrode.
[0081] 〔Comparative Example 3〕 A lithium ion secondary battery for evaluation was obtained in the same manner as in Example 1, except that a coating layer containing lithium carbonate and AB was not formed on the inner surface of the battery case and no voltage was applied between the battery case and the negative electrode.
[0082] Each of the lithium ion secondary batteries for evaluation prepared above was adjusted to SOC 50% in a temperature environment of 25°C. Then, it was placed in a temperature environment of -10°C, and 200 cycles of charging and discharging were repeated for each lithium ion secondary battery for evaluation, with one cycle being charging at 20C for 10 seconds and discharging at 2C for 100 seconds. Then, it was placed in a temperature environment of 25°C, and the discharge capacity was measured in the same manner as the initial capacity. The capacity retention rate (%) was calculated from the formula: (discharge capacity after charge and discharge cycle / initial capacity) x 100. The results are shown in Table 1. Note that this charge and discharge cycle is a condition that is likely to cause metallic lithium precipitation, so the higher the capacity retention rate, the less capacity reduction due to metallic lithium precipitation has occurred, and the higher the Li precipitation resistance of the lithium ion secondary battery.
[0083] <High temperature storage characteristic evaluation> Each of the lithium ion secondary batteries for evaluation prepared above was adjusted to SOC 80% in a temperature environment of 25°C. Each of the lithium ion secondary batteries for evaluation was placed in a thermostatic chamber at 60°C and stored for 60 days. Thereafter, the discharge capacity after storage was measured in the same manner as for the initial capacity. The capacity retention rate (%) was calculated from the formula: (discharge capacity after high-temperature storage / initial capacity) x 100. The results are shown in Table 1. Note that a higher capacity retention rate means a higher durability of the lithium ion secondary battery.
[0084] [Table 1]
[0085] As shown in Table 1, by setting the capacity ratio of the negative electrode to the positive electrode to 1.2 or more, providing a coating layer containing lithium carbonate on the inner surface of the battery case, and applying a voltage between the battery case and the negative electrode at which lithium carbonate decomposes to supply lithium ions to the negative electrode at the outermost periphery of the wound electrode assembly, it is found that both Li precipitation resistance and high-temperature storage characteristics are excellent. Therefore, it is found that the manufacturing method for a nonaqueous electrolyte secondary battery disclosed herein can provide a nonaqueous electrolyte secondary battery including a wound electrode assembly, which has a nonaqueous electrolyte that is excellent in Li precipitation resistance and high-temperature storage characteristics.
[0086] Although the specific examples of the present invention have been described in detail above, these are merely examples and do not limit the scope of the claims. The technology described in the claims includes various modifications and changes of the specific examples exemplified above.
[0087] That is, the nonaqueous electrolyte secondary battery disclosed herein comprises the following items [1] to [9]. [1] A process for preparing an assembly in which a wound electrode body in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween is wound, and a non-aqueous electrolyte are housed in a metal battery case, wherein the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more, the outermost periphery of the wound electrode body is the negative electrode, and the inner surface of the battery case has a coating layer containing a Li compound; applying a voltage between the battery case and the negative electrode so as to decompose the Li compound, thereby supplying Li ions from the Li compound to the negative electrode at the outermost periphery of the wound electrode body; and applying a voltage between the positive electrode and the negative electrode to perform an initial charge; The method for producing a non-aqueous electrolyte secondary battery includes the steps of: [2] The manufacturing method according to item [1], wherein the number of turns of the wound electrode body is 20 turns or more. [3] The manufacturing method according to item [1] or [2], wherein the coating layer is formed on the inner surface of the battery case, the surface facing the flat surface of the wound electrode body. [4] The method according to any one of items [1] to [3], wherein the coating layer further contains a conductive material. [5] The method according to any one of items [1] to [4], wherein a ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.3 or more. [6] The method according to any one of items [1] to [5], wherein the Li compound is at least one selected from the group consisting of lithium carbonate, lithium chloride, lithium nitrate, lithium dihydrogen carbonate, and lithium phosphate. [7] The method according to item [6], wherein the Li compound is lithium carbonate. [8] The method according to any one of items [1] to [7], further comprising a step of performing an aging treatment at a temperature of 60° C. or higher in a charged state in which the potential of the negative electrode is 0.5 V or higher after the initial charge. [9] A wound electrode body in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween is wound. a non-aqueous electrolyte, and A metal battery case that houses these Equipped with The ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more; The inner surface of the battery case has a high Li element accumulation region. Nonaqueous electrolyte secondary battery. [Explanation of symbols]
[0088] 20 Wound electrode body 30 Battery case 36 Safety valve 42 Positive terminal 42a Positive current collector 44 Negative terminal 44a Negative current collector plate 50 Positive electrode sheet (positive electrode) 52 Positive electrode current collector 52a Portion where positive electrode active material layer is not formed 54 Cathode active material layer 60 Negative electrode sheet (negative electrode) 62 Negative electrode current collector 62a Part where negative electrode active material layer is not formed 64 Negative electrode active material layer 70 First separator sheet (separator) 72 Second separator sheet (separator) 80 Non-aqueous electrolytes 90 Coating layer 92 Lithium-rich region 100 assemblies 200 Lithium-ion secondary battery
Claims
1. a step of preparing an assembly in which a wound electrode body in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween is wound, and a non-aqueous electrolyte are housed in a metal battery case, wherein the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more, the outermost periphery of the wound electrode body is the negative electrode, and the inner surface of the battery case has a coating layer containing a Li compound; A step of applying a voltage between the battery case and the negative electrode so as to decompose the Li compound, thereby supplying Li ions from the Li compound to the negative electrode at the outermost periphery of the wound electrode body; and A step of applying a voltage between the positive electrode and the negative electrode to perform an initial charge; The method for producing a non-aqueous electrolyte secondary battery includes the steps of:
2. The manufacturing method according to claim 1 , wherein the number of turns of the wound electrode body is 20 turns or more.
3. The manufacturing method according to claim 1 , wherein the coating layer is formed on an inner surface of the battery case, the surface facing the flat surface of the wound electrode body.
4. The method according to claim 1 , wherein the coating layer further contains a conductive material.
5. The method according to claim 1 , wherein the ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.3 or more.
6. The method according to claim 1, wherein the Li compound is at least one selected from the group consisting of lithium carbonate, lithium chloride, lithium nitrate, lithium dihydrogen carbonate, and lithium phosphate.
7. The method according to claim 6 , wherein the Li compound is lithium carbonate.
8. The method according to claim 1 , further comprising the step of performing an aging treatment at a temperature of 60° C. or higher in a charged state in which the potential of the negative electrode is 0.5 V or higher after the initial charging.
9. a wound electrode body in which a laminate including a positive electrode, a negative electrode, and a separator interposed therebetween is wound; a non-aqueous electrolyte, and A metal battery case that houses these Equipped with The ratio of the capacity of the negative electrode to the capacity of the positive electrode is 1.2 or more; The inner surface of the battery case has a high Li element accumulation region. Nonaqueous electrolyte secondary battery.
Citation Information
Patent Citations
Secondary battery
JP1995135024A
Aging treatment method for lithium secondary battery
JP2000340262A
Battery
JP2007258029A
Lithium ion battery before pre-doping and manufacturing method of lithium ion battery
JP2008192540A
Lithium ion secondary battery and method for manufacturing the same
JP2011054324A