Adhesive, and article using the same

A water-based adhesive with cellulose fibers and nanofibers swells upon water absorption, addressing the challenge of easy peeling and adhesiveness, enhancing recyclability by facilitating adhesive removal.

JP2024139331APending Publication Date: 2024-10-09DKS CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2023050219
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing adhesives containing cellulose fibers do not effectively absorb water to facilitate easy peeling after adhesion.

Method used

A water-based adhesive composition comprising a water-based resin and cellulose fibers, with cellulose nanofibers being preferred, that swells upon water absorption to enable easy peeling.

Benefits of technology

The adhesive composition maintains adhesiveness while allowing for easy removal by swelling upon water absorption, facilitating recycling by enabling the adhesive layer to be peeled off from the adherend.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139331000001
    Figure 2024139331000001
Patent Text Reader

Abstract

To provide an adhesive which is made to absorb water after adhesion and is used for application of peeling.SOLUTION: An adhesive is made to absorb water after adhesion and used for application of peeling, contains (A) an aqueous resin and (B) a cellulose fiber, and contains 0.1 to 10 pts.mass of the cellulose fiber with respect to 100 pts.mass of the aqueous resin.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an adhesive used in applications where adhesion is followed by water absorption and then peeling, and to an article using the adhesive. [Background technology]

[0002] In recent years, there has been a demand for adhesives that are easily peelable from the standpoint of recycling, etc. For example, Patent Document 1 discloses the use of an aqueous dispersion of cellulose nanofibers as an easily peelable adhesive composition that has high adhesive strength and does not require special treatment for peeling.

[0003] Patent Document 2 discloses a pressure-sensitive adhesive composition having excellent adhesion and removability, which is obtained by blending modified cellulose fibers with a matrix resin such as an acrylic pressure-sensitive adhesive.

[0004] Patent Document 3 discloses an adhesive composition that contains cellulose nanofibers and a resin such as an acrylic resin, a urethane resin, or an epoxy resin, as an adhesive composition having a high ratio of shear strength to peel strength. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2017-025130 A [Patent Document 2] JP 2020-076075 A [Patent Document 3] JP 2020-152829 A Summary of the Invention [Problem to be solved by the invention]

[0006] The above Patent Documents 1 to 3 disclose adhesives containing cellulose fibers as adhesives having releasability, but do not disclose their use in applications where the adhesive is peeled off by absorbing water after adhesion.

[0007] An object of an embodiment of the present invention is to provide an adhesive that is used in applications where adhesion is followed by water absorption and subsequent peeling. [Means for solving the problem]

[0008] The present invention includes the embodiments set forth below. [1] An adhesive used in applications where adhesion is followed by water absorption and peeling, the adhesive comprising (A) an aqueous resin and (B) cellulose fibers, the cellulose fibers being contained in an amount of 0.1 to 10 parts by mass per 100 parts by mass of the aqueous resin. [2] The adhesive according to [1], wherein the aqueous resin contains a water-dispersible resin. [3] The adhesive according to [2], wherein the water-dispersible resin comprises an anionic water-dispersible resin and / or a nonionic water-dispersible resin. [4] The adhesive described in any one of [1] to [3], wherein the cellulose fibers contain cellulose nanofibers. [5] The adhesive according to any one of [1] to [4], wherein the cellulose fibers have anionic groups. [6] The adhesive according to any one of [1] to [5], which is a primer. [7] An article comprising a first member, a second member, and an adhesive layer formed from the adhesive according to any one of [1] to [6], which bonds the first member and the second member. Effect of the Invention

[0009] In the case of the adhesive according to the embodiment of the present invention, the cellulose fibers swell when they are allowed to absorb water after bonding, so that the adhesive can be easily peeled off. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The adhesive according to the embodiment is obtained by blending (A) an aqueous resin and (B) cellulose fibers.

[0011] [(A) Water-based resin] The aqueous resin is a component (adhesive component) that exerts adhesive properties in the adhesive. Therefore, the adhesive according to the embodiment can be said to be a mixture of an aqueous adhesive containing an aqueous resin and cellulose fibers or an aqueous dispersion thereof. By blending cellulose fibers, it is possible to impart peelability by swelling of the cellulose fibers when absorbing water while maintaining the adhesive properties of the aqueous resin.

[0012] The water-based resin refers to a resin that disperses or dissolves in water, and includes water-dispersible resins and water-soluble resins. As the water-based resin, either water-dispersible resin or water-soluble resin may be used, or both may be used in combination. It is preferable to use a water-dispersible resin. That is, in one embodiment, the water-based resin contains a water-dispersible resin. In that case, the water-based resin is preferably mainly composed of a water-dispersible resin, and the amount of the water-dispersible resin in 100% by mass of the water-based resin is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass.

[0013] The water-dispersible resin refers to a resin that forms an emulsion or suspension by emulsifying or dispersing it in water as a dispersion medium. Therefore, the water-dispersible resin may be a resin contained in an emulsion in which the resin, which is the dispersoid, is liquid (i.e., a water-based emulsion resin), or a resin contained in a suspension in which the resin, which is the dispersoid, is solid (i.e., a water-based suspension resin).

[0014] The water-dispersible resin is preferably a water-based emulsion resin. The water-based emulsion may be a forced emulsification type or a self-emulsification type. The forced emulsification type refers to a type that is forcedly emulsified by a surfactant. The self-emulsification type refers to a type that is made self-dispersible by adding a hydrophilic group or a hydrophilic segment in the molecule.

[0015] Examples of the water-dispersible resin include water-dispersible urethane resin, water-dispersible acrylic resin, water-dispersible vinyl acetate resin, water-dispersible polyester resin, water-dispersible polyepoxy resin, water-dispersible polystyrene resin, etc. Any one of these may be used alone, or two or more of them may be used in combination.

[0016] The water-dispersible urethane resin is obtained by reacting a polyol with a polyisocyanate, and a known urethane emulsion can be used as an example. The polyol can be at least one selected from the group consisting of polyester polyol, polyether polyol, polycarbonate polyol, polybutadiene polyol, etc. In addition, together with or instead of these polyols, low molecular weight polyols such as ethylene glycol, diethylene glycol, triethylene glycol, tetraethylene glycol, propanediol, dipropylene glycol, tripropylene glycol, butanediol, pentanediol, hexanediol, neopentyl glycol, glycerin, trimethylolpropane, ditrimethylolpropane, pentaerythritol, bisphenol A, etc. may be used.

[0017] Examples of polyisocyanates include aliphatic polyisocyanates such as tetramethylene diisocyanate, dodecamethylene diisocyanate, hexamethylene diisocyanate, and lysine diisocyanate, alicyclic diisocyanates such as hydrogenated diphenylmethane diisocyanate (hydrogenated MDI), isophorone diisocyanate, and methylcyclohexylene diisocyanate, aromatic polyisocyanates such as tolylene diisocyanate, diphenylmethane diisocyanate (MDI), 1,5-naphthylene diisocyanate, and xylylene diisocyanate, as well as modified and polynuclear polyisocyanates thereof. Any of these may be used alone or in combination of two or more.

[0018] The water-dispersible acrylic resin is a resin obtained by using (meth)acrylic acid and / or (meth)acrylic acid ester as a monomer, and may be a copolymer using other monomers such as ethylene, styrene, etc. together with these monomers, and a known acrylic emulsion can be used as an example. Examples of the (meth)acrylic acid ester include (meth)acrylic acid alkyl esters such as methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, and butyl (meth)acrylate, and (meth)acrylic acid aryl esters such as benzyl (meth)acrylate, etc.

[0019] The water-dispersible vinyl acetate resin is a resin obtained using vinyl acetate as a monomer, and may be a copolymer of vinyl acetate and other monomers. For example, a known vinyl acetate emulsion can be used.

[0020] The water-dispersible polyester resin is a polycondensate obtained by dehydrating and condensing a polyvalent carboxylic acid and a polyol to form an ester bond, and as an example, a known polyester emulsion can be used.

[0021] The water-dispersible polyepoxy resin and the water-dispersible polystyrene resin are also not particularly limited, and for example, known polyepoxy emulsions and polystyrene emulsions can be used.

[0022] The water-dispersible resin may be anionic, nonionic, or cationic, or may be a suitable combination of these. In one embodiment, the water-dispersible resin contains an anionic water-dispersible resin and / or a nonionic water-dispersible resin. In that case, the water-dispersible resin is preferably composed mainly of an anionic water-dispersible resin and / or a nonionic water-dispersible resin, and the amount of the anionic water-dispersible resin and / or the nonionic water-dispersible resin in 100% by mass of the water-dispersible resin is preferably 70% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more, and may be 100% by mass.

[0023] Examples of anionic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which anionic groups such as carboxyl groups and sulfonic acid groups have been introduced into the resin. Examples of nonionic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which nonionic hydrophilic groups or hydrophilic segments such as polyethylene glycol have been introduced into the resin. Examples of cationic water-dispersible resins include aqueous emulsion resins and / or aqueous suspension resins in which cationic groups such as quaternary ammonium bases have been introduced into the resin.

[0024] [(B) Cellulose fiber] The cellulose fibers may be cellulose fibers having a number average fiber diameter of more than 500 nm on the order of μm, or cellulose nanofibers having a number average fiber diameter of 500 nm or less, or a combination of both.

[0025] From the viewpoint of not impairing the initial adhesiveness, it is preferable to use cellulose nanofibers as the cellulose fibers. Also, from the viewpoint of increasing the degree of swelling when water is absorbed after adhesion and enhancing the effect of improving releasability, it is preferable to use cellulose nanofibers as the cellulose fibers. That is, in one embodiment, the cellulose fibers contain cellulose nanofibers. In this case, it is preferable that the cellulose fibers are mainly composed of cellulose nanofibers, and the amount of cellulose nanofibers in 100% by mass of cellulose fibers is preferably 50% by mass or more, more preferably 70% by mass or more, even more preferably 90% by mass or more, and may be 100% by mass.

[0026] The number average fiber diameter of the cellulose nanofibers is preferably from 1 to 500 nm, more preferably from 1.5 to 200 nm, even more preferably from 2 to 100 nm, even more preferably from 2.5 to 50 nm, and even more preferably from 3 to 20 nm.

[0027] The average aspect ratio of the cellulose nanofibers is not particularly limited, but is preferably 10-1,000, more preferably 50-700, even more preferably 100-500, and even more preferably 200-400.

[0028] The number average fiber diameter and average aspect ratio of cellulose nanofibers can be determined by observation using an atomic force microscope (AFM). For example, after casting an aqueous dispersion of cellulose nanofibers on a mica substrate, 10 AFM images are taken using an atomic force microscope (AFM, manufactured by Hitachi High-Tech Corporation), and 25 cellulose nanofibers are selected from the images and their fiber diameters and lengths are measured. From the obtained fiber diameter and fiber length data, the arithmetic mean of each is calculated to determine the number average fiber diameter [nm] and number average fiber length [nm], and the average aspect ratio is calculated according to the following formula. Average aspect ratio = number average fiber length [nm] / number average fiber diameter [nm]

[0029] The cellulose nanofiber preferably has a cellulose type I crystal structure. The cellulose type I crystal structure is the crystalline form of natural cellulose, and the cellulose fiber (B) has water insolubility and can maintain its fibrous form in water due to the cellulose type I crystal structure. The cellulose type I crystal structure can be identified by the presence of typical peaks at two positions, around 2θ=14° to 17° and around 2θ=22° to 23°, in a diffraction profile obtained by wide-angle X-ray diffraction image measurement.

[0030] As the cellulose fibers (preferably cellulose nanofibers), unmodified cellulose fibers to which no anionic groups have been introduced may be used, but it is preferable to use cellulose fibers having anionic groups. That is, in one embodiment, it is preferable that the cellulose fibers have anionic groups, and more preferably, cellulose nanofibers having anionic groups are used as the cellulose fibers. By having anionic groups, it is possible to increase the degree of swelling when water is absorbed after adhesion, thereby enhancing the effect of improving the peelability.

[0031] Examples of the anionic group include at least one selected from the group consisting of a carboxy group, a phosphate group, a sulfonate group, a nitrate group, a borate group, and a sulfate group. These anionic groups may be directly or indirectly bonded to a glucose unit, which is a structural unit of a cellulose molecule. When indirectly bonded, for example, an alkylene group having 1 to 4 carbon atoms may be present between the glucose unit and the anionic group. One or more anionic groups may be bonded to all glucose units constituting the cellulose molecule, or one or more anionic groups may be bonded to a part of the glucose units constituting the cellulose molecule.

[0032] The carboxyl group as the anionic group includes not only the acid type (-COOH) but also the salt type, i.e., carboxylate group (-COOX, where X is a cation that forms a salt with a carboxylic acid), and the acid type and the salt type may be mixed. Similarly, the phosphate group, sulfonic acid group, nitrate group, borate group, and sulfate group include not only the acid type but also the salt type, and the acid type and the salt type may be mixed. The salt is not particularly limited, and examples thereof include alkali metal salts such as sodium salts and potassium salts, alkaline earth metal salts such as magnesium salts and calcium salts, onium salts such as ammonium salts and phosphonium salts, and amine salts such as primary amines, secondary amines, and tertiary amines.

[0033] When the cellulose fiber has an anionic group, the amount of the anionic group is not particularly limited, and may be, for example, 0.5 to 4.0 mmol / g or 1.0 to 3.0 mmol / g per dry mass of the cellulose fiber. For example, in the case of a carboxy group, the amount of the anionic group is determined by preparing 60 mL of a cellulose fiber-containing slurry adjusted to a concentration of 0.1 to 1% by mass, adjusting the pH to about 2.5 with a 0.1 mol / L aqueous hydrochloric acid solution, dropping a 0.05 mol / L aqueous sodium hydroxide solution, measuring the electrical conductivity, and continuing until the pH becomes about 11. The amount of sodium hydroxide consumed in the neutralization stage of the weak acid where the change in electrical conductivity is gradual (V) according to the following formula. The phosphate group can also be measured by the same electrical conductivity measurement. Other anionic groups may also be measured by a known method. In this specification, the "dry mass" refers to the mass after drying at 140°C until the mass change rate per minute is 0.05% or less. Amount of anionic group (mmol / g) = V (mL) × [0.05 / mass of cellulose fiber (g)]

[0034] In one embodiment, examples of cellulose nanofibers having carboxy groups as anionic groups include oxidized cellulose nanofibers obtained by oxidizing hydroxyl groups of glucose units in cellulose molecules, and carboxymethylated cellulose nanofibers obtained by carboxymethylating hydroxyl groups of glucose units in cellulose molecules.

[0035] Oxidized cellulose nanofibers include those in which the hydroxyl group at the C6 position of the glucose unit in the cellulose molecule is selectively oxidized to a carboxyl group. Oxidized cellulose nanofibers are obtained by oxidizing natural cellulose such as wood pulp using a co-oxidant in the presence of an N-oxyl compound and subjecting it to defibration (fine processing). As the N-oxyl compound, a compound having a nitroxy radical, which is generally used as an oxidation catalyst, is used, for example, a piperidine nitroxyoxy radical, and in particular, 2,2,6,6-tetramethylpiperidinooxy radical (TEMPO) or 4-acetamide-TEMPO is preferred. Cellulose fibers oxidized and finely divided with TEMPO are generally called TEMPO-oxidized cellulose nanofibers (TOCN). The oxidized cellulose nanofibers may have an aldehyde group or a ketone group in addition to the carboxyl group.

[0036] When cellulose fibers are defibrated to obtain cellulose nanofibers, the defibration may be performed after or before the introduction of anionic groups. The defibration can be performed by treating an aqueous dispersion of cellulose fibers using, for example, a homomixer, a high-pressure homogenizer, an ultrasonic dispersion processor, a beater, a disk refiner, a conical refiner, a double disk refiner, a grinder, or the like under high-speed rotation, to obtain an aqueous dispersion of cellulose nanofibers.

[0037] [glue] The adhesive according to the embodiment is an aqueous adhesive containing the aqueous resin and cellulose fibers. Therefore, the adhesive is a liquid adhesive containing water as well as the aqueous resin and cellulose fibers. The cellulose fibers are water-insoluble and are dispersed in water, which is a dispersion medium. When the aqueous resin is used, the aqueous resin is dispersed in water, which is a dispersion medium. Therefore, in this case, the adhesive is an aqueous dispersion containing the aqueous resin and cellulose fibers dispersed in water, which is a dispersion medium.

[0038] The above-mentioned aqueous dispersion contains water as a dispersion medium, but the dispersion medium may be water alone, or may contain water-soluble organic solvents such as ethanol and isopropyl alcohol together with water to the extent that the effect is not impaired. When an organic solvent is contained, the amount of water in 100% by mass of the dispersion medium is preferably 70% by mass or more, more preferably 80% by mass or more, even more preferably 90% by mass or more, and even more preferably 100% by mass. The dispersion medium may be an aqueous solution containing an acid, an alkali, or a salt thereof, as long as the effect is not impaired.

[0039] In the above adhesive, the amount of cellulose fiber is 0.1 to 10 parts by mass relative to 100 parts by mass of the aqueous resin. When the amount of cellulose fiber is 0.1 part by mass or more, the degree of swelling when water is absorbed after adhesion can be increased, thereby improving the peelability. Furthermore, when the amount of cellulose fiber is 10 parts by mass or less, the coatability of the adhesive is good. The amount of cellulose fiber relative to 100 parts by mass of the aqueous resin is more preferably 0.2 to 9 parts by mass, even more preferably 0.3 to 6 parts by mass, even more preferably 0.5 to 5 parts by mass, and even more preferably 0.6 to 3 parts by mass.

[0040] In the adhesive, the content (concentration) of the aqueous resin is not particularly limited and may be, for example, 1 to 70 mass % or 5 to 50 mass %. The content (concentration) of the cellulose fiber is also not particularly limited and may be, for example, 0.001 to 7 mass % or 0.005 to 5 mass %.

[0041] The adhesive according to the embodiment may contain additives such as a colorant, a filler, a preservative, an antifoaming agent, a film-forming aid, an antiblocking agent, a flow improver, a viscosity adjuster, an adhesion imparting agent, a conductive agent, an antioxidant, a light stabilizer, and an ultraviolet absorbing agent, in addition to the above-mentioned aqueous resin, cellulose fiber, and water.

[0042] In the adhesive according to the embodiment, after the adhesive is used to adhere the adherend, the adhesive layer in a dry state is allowed to absorb water, causing the cellulose fibers contained in the adhesive layer to swell. This makes it easier for the adherend to peel off at the interface with the adhesive layer, and the adherend can be easily peeled off. Water absorption into the adhesive layer (i.e., taking in water into the adhesive layer) can be achieved by treating the adhesive layer with water, such as by immersing the part including the adhesive layer in water or spraying water on it.

[0043] In one embodiment, the adhesive can be used as a primer (i.e., undercoat adhesive). In detail, the adhesive is applied as a primer onto a substrate, and a topcoat paint is applied thereon to form a coating film (one or more coating films including an intermediate coating). When recycling a substrate from the product thus obtained, the adhesive layer formed as a primer can be treated with water as described above to absorb water, so that the coating film including the adhesive layer can be easily peeled off from the substrate. When the coating film is peeled off after absorbing water, the adhesive layer may peel off together with the coating film, or the adhesive layer may remain on the substrate side. Even if the adhesive layer remains on the substrate side, the remaining adhesive layer can be peeled off and removed by further treating with water to absorb water, and the substrate can be recycled. In addition, when the adhesive layer remains on the coating film, the adhesive layer remaining on the coating film may be further treated with water to peel off and remove the adhesive layer from the coating film, thereby recycling the coating film.

[0044] The substrate is not particularly limited, and examples thereof include inorganic substrates such as glass plates and concrete, etc. In addition, examples thereof include synthetic resin substrates such as films, sheets, and plates made of synthetic resins such as polyester (PET, PEN, etc.), polyvinylidene chloride, polyvinyl chloride, polyethylene, polypropylene, polycarbonate, polystyrene, polyacrylate, and polyolefin, and organic substrates such as wood substrates.

[0045] The method for applying the adhesive is not particularly limited, and the adhesive can be applied by, for example, a knife coater, a roll coater, a spray, or the like.

[0046] The thickness of the adhesive layer is not particularly limited and may be, for example, 0.1 to 500 μm, or 0.5 to 100 μm.

[0047] An article according to one embodiment includes an adhesive layer formed from the adhesive. That is, the article includes a first member and a second member as adherends, and an adhesive layer that bonds the first member and the second member, the adhesive layer being formed from the adhesive. The adhesive layer is formed by applying and drying the adhesive, and is therefore formed from the non-volatile content of the adhesive.

[0048] The first and second members as the adherends are materials that form part of an article, and their shapes are not particularly limited. For example, one of the first and second members may be a substrate for the primer application, and the other may be a coating film formed by a topcoat paint. The substrates may be bonded together with the adhesive. EXAMPLES

[0049] Examples will be described in detail below together with comparative examples, but the present invention is not limited to these examples.

[0050] Details of the components used in the examples and comparative examples are as follows.

[0051] [Water-based resin] Water-based resin 1: "Superflex 460" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / carbonate-based, non-volatile content 38% by mass)

[0052] Water-based resin 2: "Superflex 150" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / ester-ether type, non-volatile content 30% by mass)

[0053] Water-based resin 3: "Superflex 210" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (anionic urethane emulsion / ester-based, non-volatile content 35% by mass)

[0054] Water-based resin 4: "Superflex 500M" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (nonionic urethane emulsion / ester-based, non-volatile content 45% by mass)

[0055] Water-based resin 5: "Superflex 620" manufactured by Daiichi Kogyo Seiyaku Co., Ltd. (cationic urethane emulsion / ester type, non-volatile content 30% by mass)

[0056] Water-based resin 6: "Movinyl 730L" manufactured by Japan Coating Resins Co., Ltd. (nonionic acrylic emulsion, non-volatile content 46% by mass)

[0057] Water-based resin 7: "Movinyl 51" manufactured by Japan Coating Resins Co., Ltd. (nonionic vinyl acetate emulsion, non-volatile content 50% by mass)

[0058] Water-based resin 8: GOO Chemical Industry Co., Ltd.'s "Pluscoat RZ-105" (anionic polyester emulsion, non-volatile content 25% by mass)

[0059] [Cellulose fiber] Cellulose fiber 1: TEMPO-oxidized cellulose nanofibers obtained by Production Example 1 below, having a number average fiber diameter of 3 nm, an average aspect ratio of 300, and a carboxy group amount of 2.0 mmol / g. [Production Example 1] 150 mL of water, 0.25 g of sodium bromide, and 0.025 g of TEMPO were added to 2 g of softwood pulp, and the mixture was thoroughly stirred to disperse the mixture. Then, a 13% by mass aqueous solution of sodium hypochlorite (co-oxidant) was added so that the amount of sodium hypochlorite was 5.2 mmol / g per 1.0 g of the pulp, and the reaction was started. Since the pH decreased as the reaction proceeded, a 0.5 N aqueous solution of sodium hydroxide was added dropwise to maintain the pH at 10 to 11, and the reaction was continued until no change in pH was observed (reaction time: 120 minutes). After the reaction was completed, 0.1 N hydrochloric acid was added to adjust the pH to 2, and the mixture was purified by repeatedly filtering and washing with water to obtain cellulose fibers with an oxidized fiber surface. The mixture was diluted to a cellulose fiber concentration of 2% by mass by adding pure water, and the pH was adjusted to 7 by adding 10% by mass of sodium hydroxide. The mixture was treated once at a pressure of 100 MPa using a high-pressure homogenizer (H11, manufactured by Sanwa Engineering Co., Ltd.) to prepare cellulose fiber 1.

[0060] Cellulose fiber 2: TEMPO-oxidized cellulose nanofibers obtained by Production Example 2 below, having a number average fiber diameter of 3 nm, an average aspect ratio of 300, and a carboxy group amount of 2.0 mmol / g. [Production Example 2] Cellulose fibers 2 were obtained in the same manner as in Production Example 1, except that in the neutralization step, tetrabutylammonium hydroxide was used instead of sodium hydroxide.

[0061] Cellulose fiber 3: phosphorylated cellulose nanofibers obtained by Production Example 3 described below, having a number average fiber diameter of 3 nm, an average aspect ratio of 200, and a phosphate group amount of 2.5 mmol / g. [Production Example 3] It was prepared by the method described in Production Example 1 of JP 2020-100845 A. That is, 100 g of urea, 55.3 g of sodium dihydrogen phosphate dihydrate, and 41.3 g of disodium hydrogen phosphate were dissolved in 110 g of water. Then, 100 g of softwood bleached kraft pulp was added and reacted at 140 ° C. for 2 hours. Next, the fibers were taken out and washed with water, and then a 2N aqueous solution of sodium hydroxide was added as a neutralizing agent to adjust the pH to 12 to 13, and the fibers were washed with water again. After that, the fibers were dehydrated and then diluted with water so that the cellulose fiber concentration was 2.0% by mass. Then, as a micro-refining treatment step, a treatment with a microfluidizer (150 MPa, 10 passes) was performed to obtain cellulose fibers 3.

[0062] Cellulose fiber 4: Unmodified cellulose nanofibers having a number average fiber diameter of 35 nm and an average aspect ratio of 250, obtained by Production Example 4 described below. [Production Example 4] 50.0 g of softwood pulp was dispersed in 950.0 g of water, pulverized in a household mixer, defibrated in a stone mill, and further water was added to obtain an aqueous dispersion with a cellulose fiber concentration of 2% by mass. The obtained 2% by mass aqueous dispersion was treated with a microfluidizer (150 MPa, 1 pass) to obtain cellulose fiber 4.

[0063] [Preparation of adhesive] Adhesives of Examples 1 to 14 and Comparative Examples 1 to 3 were prepared by mixing aqueous resin emulsions (aqueous resins 1 to 8) and aqueous dispersions of cellulose fibers (cellulose fibers 1 to 4) according to the formulations shown in Table 1 below. The formulations in Table 1 are the mass ratios of the aqueous resin and the nonvolatile content of the cellulose fibers, and the nonvolatile content of the resin is shown as 100 parts by mass. Each adhesive was prepared by diluting with water so that the concentration of the nonvolatile content of the resin was 10% by mass (however, 5% by mass in Comparative Example 1).

[0064] The obtained adhesive was evaluated for water absorption rate (mass), water absorption rate (thickness), adhesion (before water absorption), and peelability (after water absorption) using the following evaluation methods.

[0065] [Water absorption rate (mass)] The adhesive was applied to a release paper and dried at 40°C for 24 hours to obtain a film with a dry thickness of 500 μm. The obtained film was cut into 2 cm x 4 cm to obtain a test piece. The test piece was conditioned at 23°C and 50% relative humidity for 24 hours, and then its mass (Wd) was measured. The test piece was immersed in ion-exchanged water at room temperature for 24 hours, then removed from the ion-exchanged water, and the water droplets on the surface were wiped off, and the mass (W) of the test piece was immediately measured. The water absorption rate (mass) was calculated using the following formula. Water absorption rate (mass) = {(W-Wd) / Wd}×100

[0066] [Water absorption rate (thickness)] Similarly to the water absorption rate (mass), a test piece was prepared, and the thickness (Dd) of the obtained test piece was measured after conditioning it at 23°C and a relative humidity of 50% for 24 hours. In addition, the test piece was immersed in ion-exchanged water at room temperature for 24 hours, and the thickness (D) of the test piece was measured immediately after removing it from the ion-exchanged water. The water absorption rate (thickness) was calculated by the following formula and evaluated according to the following evaluation criteria. Water absorption rate (thickness) = {(D-Dd) / Dd} x 100 <Evaluation criteria> ○: Water absorption rate (thickness) value is 50 or more △: Water absorption rate (thickness) value is 20 or more and less than 50 ×: Water absorption rate (thickness) value is less than 20

[0067] [Adhesiveness (before water absorption)] The adhesive was applied to a substrate and dried at 80° C. for 10 minutes to form a coating film having a dry thickness of 20 μm. As the substrate, a glass plate was used in Examples 1 to 8 and Comparative Examples 1 and 2, and a corona-treated PET film was used in Examples 9 to 14 and Comparative Example 3. Next, a photocurable resin liquid was applied onto the coating film and dried at 80°C for 10 minutes to form a photocurable resin layer with a dry thickness of 20 μm, thereby obtaining a laminate. As the photocurable resin liquid, a mixed liquid prepared by mixing a photocurable resin oligomer ("New Frontier R-1220" manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) with a photopolymerization initiator ("Omnirad 184" manufactured by IGM Resins BV) at 3 mass% was used. The obtained laminate was irradiated with ultraviolet light to prepare a test piece. The ultraviolet light irradiation conditions were a nitrogen atmosphere (oxygen concentration 0.3%), a high-pressure mercury lamp of 80 W / cm, and an integrated illuminance of 250 mJ / cm. 2 The line speed was 5 m / min and the power was 2 kW. A cross-cut peel test was carried out on the prepared test pieces in accordance with JIS K5400 8.5.2:1990. A cross-cut adhesion score of 70 or more out of 100 cross-cuts was evaluated as "Good", a score of 20 or more but less than 70 was evaluated as "Good", and a score of less than 20 was evaluated as "Poor".

[0068] [Removability (after water absorption)] Similar to the adhesion (before water absorption), test pieces were prepared, immersed in 80°C ion-exchanged water for 24 hours, removed from the ion-exchanged water, and dried at 40°C for 24 hours, after which a cross-cut peel test was carried out in accordance with JIS K5400 8.5.2:1990. Of the 100 cross-cuts, an increase of 30 or more peeled spots compared to the test results before water absorption was marked as "Good", an increase of 15 to less than 30 was marked as "Good", and an increase of less than 15 was marked as "Poor".

[0069] [Table 1]

[0070] The results are shown in Table 1. Examples 1 to 8 and Comparative Examples 1 and 2 are examples in which glass plates were used as the substrate. In this case, Comparative Example 2, which contained only aqueous resin 1 as the adhesive component and no cellulose fiber, had excellent adhesion before water absorption, but had a low water absorption rate when immersed in water and poor peelability after water absorption. In Comparative Example 1, the viscosity of the mixed liquid was high and coating was difficult, so evaluations of water absorption rate (mass), water absorption rate (thickness), adhesion, and peelability were not performed, and are shown as "-" in Table 1.

[0071] In contrast, in Examples 1 to 8, in which cellulose fibers 1 to 4 were blended with water-based resins 1 and 2, the adhesiveness before water absorption was excellent, the thickness change after immersion in water was large, and the peelability after water absorption was excellent. Comparing Examples 1 to 3 and Example 4, with respect to the type of cellulose fiber, the one into which an anionic group was introduced had higher water absorption rate (mass) and water absorption rate (thickness) than the unmodified one. In addition, the water absorption rate (mass) and water absorption rate (thickness) improved as the amount of cellulose fiber increased, but the coatability tended to decrease.

[0072] Examples 9 to 14 and Comparative Example 3 are examples in which a PET film was used as the substrate. In Comparative Example 3, which contained only aqueous resin 6 as an adhesive component and no cellulose fiber, the adhesiveness before water absorption was excellent, but the change in thickness when immersed in water was small, and the peelability after water absorption was poor.

[0073] In contrast, in Examples 9 to 14, in which cellulose fiber 1 was blended together with water-based resins 3 to 8, the adhesiveness before water absorption was excellent, the thickness change after immersion in water was large, and the peelability after water absorption was excellent. Comparing Examples 9 to 11, it was found that, regarding the type of urethane emulsion as the water-based resin, nonionic tended to be better than cationic, and anionic tended to be better than nonionic in terms of adhesiveness before water absorption and peelability after water absorption.

[0074] In the evaluation of adhesion (before water absorption) and peelability (after water absorption), the adhesion between the adhesive layer and the photocured resin layer was good in all of the Examples and Comparative Examples, and no peeling was observed at the interface between the adhesive layer and the photocured resin layer.

[0075] In addition, the various numerical ranges described in the specification can be arbitrarily combined with their upper and lower limits, and all such combinations are considered to be preferred numerical ranges described in the specification. In addition, a numerical range described as "X to Y" means from X to Y.

[0076] Although several embodiments of the present invention have been described above, these embodiments are presented as examples and are not intended to limit the scope of the invention. These embodiments can be implemented in various other forms, and various omissions, substitutions, and modifications can be made without departing from the gist of the invention. These embodiments and their omissions, substitutions, modifications, etc. are included in the scope and gist of the invention as well as the invention and its equivalents described in the claims.

Claims

1. An adhesive used in applications where the adhesive is peeled off by absorbing water after adhesion, (A) an aqueous resin and (B) cellulose fibers, The adhesive comprises 0.1 to 10 parts by mass of the cellulose fibers relative to 100 parts by mass of the aqueous resin.

2. The adhesive of claim 1 , wherein the water-based resin comprises a water-dispersible resin.

3. The adhesive of claim 2 , wherein the water-dispersible resin comprises an anionic water-dispersible resin and / or a nonionic water-dispersible resin.

4. The adhesive of claim 1 , wherein the cellulose fibers comprise cellulose nanofibers.

5. The adhesive of claim 1 , wherein the cellulose fibers have anionic groups.

6. The adhesive of claim 1 which is a primer.

7. An article comprising a first member, a second member, and an adhesive layer formed from the adhesive according to any one of claims 1 to 6, which bonds the first member and the second member.

Citation Information

Patent Citations

  • Removable type pressure-sensitive adhesive

    JP1998001654A

  • Re-releasable sheet

    JP2018053220A

  • Adhesive composition

    JP2020076075A

  • Adhesive composition, and method for increasing value of ratio between shear bond strength and peel strength

    JP2020152829A

  • Adhesive agent composition and adhesive agent

    WO2016076115A1