Thermal conductive material

A thermally conductive material combining flaky carbon, organic compounds, and spherical materials addresses issues of thermal conductivity and dispersibility, enhancing thermal conductivity and heat dissipation.

JP2024139339APending Publication Date: 2024-10-09OSAKA GAS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2023050230
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing thermally conductive materials, such as crystalline carbon and inorganic materials, face issues with thermal conductivity, compatibility with resins, and agglomeration, leading to difficulties in kneading, molding, and strength, while nanocarbon materials have low usability and dispersibility when combined with resins.

Method used

A thermally conductive material is developed using a specific combination of flaky carbon with a thickness of 1 nm to 100 nm, an organic compound with hydrophilic and carbon-affinity hydrophobic groups, and approximately spherical materials with a diameter of 5 μm or more, along with a resin component, to enhance thermal conductivity and dispersibility.

Benefits of technology

The material achieves excellent thermal conductivity and heat dissipation by preventing agglomeration of flaky carbon and improving dispersibility, resulting in improved thermal conductivity and heat dissipation properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139339000001
    Figure 2024139339000001
  • Figure 2024139339000002
    Figure 2024139339000002
  • Figure 2024139339000003
    Figure 2024139339000003
Patent Text Reader

Abstract

To provide a thermal conductive material with superior thermal conductivity.SOLUTION: The present invention provides a thermal conductive composition.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a thermally conductive material. [Background technology]

[0002] Carbon materials having crystallinity, such as graphite and carbon nanotubes, are used as thermal conductive materials because they have high thermal conductivity (see, for example, Patent Document 1). These carbon materials often do not achieve as high thermal conductivity as expected because of the high thermal resistance between the resin and carbon. Furthermore, these carbon materials have low affinity with resin, so if the amount of added carbon materials is increased to improve thermal conductivity, problems arise in kneading, molding, strength, and the like.

[0003] On the other hand, inorganic materials such as alumina are often used as thermal conductive materials. However, these inorganic materials have some issues compared to carbon-based materials, such as lower thermal conductivity and a higher specific gravity.

[0004] A graphene sheet is a two-dimensional monolayer sheet in which carbon atoms are arranged in a honeycomb lattice pattern, and is also the building block of graphite, fullerenes, carbon nanotubes, etc. Flake-like carbon (which also includes graphene sheets) in which graphene sheets are stacked to a thickness of about 100 nm or less has attracted attention as a new material that can be used in a variety of applications due to its unique physical properties.

[0005] Nanocarbon materials such as flake carbon have extremely high thermal conductivity, but the finer the structure, the more likely they are to agglomerate, making it difficult to fully utilize their usability and difficult to fully improve their thermal conductivity and heat dissipation.

[0006] Nanocarbon materials have issues with usability, such as the difficulty of creating a film from them alone and of turning them into paints. When combined with resins, depending on the compatibility, they tend not to disperse (they cannot be applied as a paint, they do not have enough strength as a sheet, etc.), and their thermal conductivity tends to drop significantly.

[0007] The coating and sheeting are preferably insulating. [Prior art documents] [Patent documents]

[0008] [Patent Document 1] International Publication No. 2014 / 080743 Summary of the Invention [Problem to be solved by the invention]

[0009] An object of the present invention is to provide a thermally conductive material having excellent thermal conductivity. [Means for solving the problem]

[0010] The present inventors have discovered that a thermally conductive material with excellent thermal conductivity can be produced by using a combination of a specific organic compound, thick flaky carbon, and specific nanofibers.

[0011] Based on this finding, the present inventors conducted further research and completed the present invention.

[0012] The present invention provides the following thermally conductive material.

[0013] The present invention encompasses the following thermally conductive compositions and thermally conductive composites.

[0014] Section 1. 1. A thermally conductive composition comprising: (A) flaky carbon having a thickness of 1 nm to 100 nm; (B) an organic compound having a hydrophilic group and a carbon-affinic hydrophobic group; (C) at least one material selected from the group consisting of inorganic materials and carbon materials, which is approximately spherical and has a diameter of 5 μm or more; (D) a resin component; A thermally conductive composition comprising:

[0015] Section 2. 2. The thermally conductive composition according to item 1, wherein the hydrophilic group is at least one type of hydrophilic group selected from the group consisting of the following general formulae (1) to (4):

[0016] [ka]

[0017] [Formula (1) represents an alcoholic hydroxyl group or a phenolic hydroxyl group.

[0018] In formula (2), R represents a divalent organic group, and both oxygen atoms represent ether bonds.

[0019] In formula (3), X1 represents a hydrogen atom, an alkali metal, NH4, or an organic ammonium.

[0020] In formula (4), X2 represents a hydrogen atom, an alkali metal, NH4, an organic ammonium, or an alkyl group. Section 3. 2. The thermally conductive composition according to item 1, wherein the hydrophilic group is a phenolic hydroxyl group or a polyoxyethylene group.

[0021] Section 4. 2. The thermally conductive composition according to item 1, wherein the carbon affinity hydrophobic group is at least one carbon affinity hydrophobic group selected from the group consisting of an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and a polyoxyalkylene group having 3 or more carbon atoms.

[0022] Section 5. 2. The thermally conductive composition according to claim 1, wherein the carbon-philic hydrophobic group is an aryl group having two or more aromatic rings.

[0023] Section 6. 2. The thermally conductive composition according to claim 1, wherein the (C) material is at least one material selected from the group consisting of aluminum oxide (alumina), zinc oxide, magnesium oxide, magnesium carbonate, boron nitride, silicon nitride, aluminum nitride, and graphite.

[0024] Section 7. The (A) flaky carbon and the (C) material are The (C) material is a thermally conductive composite supported by the (A) flaky carbon. Item 1. The thermal conductive composition according to item 1.

[0025] Section 8. A paint containing the thermal conductive composition according to item 7, or The coating film formed by the paint.

[0026] Section 9. 8. A resin molded article comprising the thermal conductive composition according to item 7.

[0027] Section 10. A method for producing a thermally conductive composite, comprising the steps of: (1) comprising a step of mixing (A) a dispersion liquid containing flaky carbon having a thickness of 1 nm to 100 nm, and 1 part by mass of the flaky carbon with (C) 0.1 parts by mass to 100 parts by mass of at least one material that is approximately spherical and has a diameter of 5 μm or more and is selected from the group consisting of inorganic materials and carbon materials, (B) an organic compound having a hydrophilic group and a carbon-affinic hydrophobic group; (D) a resin component, Method for manufacturing a thermally conductive composite. Effect of the Invention

[0028] The thermally conductive material of the present invention contains a specific organic compound, and a combination of thick flaky carbon and specific nanofibers, and has excellent thermal conductivity. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0029] The present invention will be described in detail below.

[0030] The embodiments of the present invention are intended to provide a better understanding of the gist of the invention, and unless otherwise specified, do not limit the content of the invention.

[0031] In this specification, the terms "comprise" and "containing" are concepts which encompass all of "comprise," "consist essentially of," and "consist only of."

[0032] In this specification, when a numerical range is indicated as "A to B," it means "A or more and B or less."

[0033] In this specification, the designations parts, % etc. are generally used.

[0034] In this specification, unless otherwise specified, all parts by mass or % by mass (wt%) are used.

[0035] [1] Thermal conductive materials The thermally conductive composition (thermally conductive material) of the present invention is composed of flaky carbon having a thickness of 1 nm to 100 nm, a thermally conductive spherical material, and a resin.

[0036] The thermally conductive composition of the present invention comprises: (A) flaky carbon having a thickness of 1 nm to 100 nm; (B) an organic compound having a hydrophilic group and a carbon-affinic hydrophobic group; (C) at least one material selected from the group consisting of inorganic materials and carbon materials, which is approximately spherical and has a diameter of 5 μm or more; (D) a resin component.

[0037] (1-1) Flake carbon The thermally conductive composition of the present invention contains (A) flaky carbon having a thickness of 1 nm to 100 nm.

[0038] The flaky carbon is preferably thin so that the thermal conductive composition (thermal conductive material) has excellent thermal conductivity and heat dissipation. The thickness of the flaky carbon is 1 nm to 100 nm, and preferably 1 nm to 20 nm. By setting the thickness of the flaky carbon within the above range, a thermal conductive material having sufficient thermal conductivity and heat dissipation can be obtained.

[0039] The content of flaky carbon having a thickness of 1 nm to 10 nm is preferably 80% or more, more preferably 90% or more, based on the total number of flaky carbon being 100% (mass conversion). The flaky carbon may contain flaky carbon having a thickness of more than 10 nm. The thickness of most of the flaky carbon is preferably 10 nm or less.

[0040] The thickness of the flaky carbon is measured by observation using a transmission electron microscope (TEM).

[0041] Flaky carbon also includes graphene sheets.

[0042] The flaky carbon is preferably flaky carbon having a layered structure in which 300 or less layers (i.e., 1 to 300 layers) of graphene are stacked, and more preferably flaky carbon having a layered structure in which 1 to 60 layers of graphene are stacked.

[0043] The content of flaky carbon having 1 to 30 lamination layers is preferably 80% or more, and more preferably 90% or more, based on the total number of flaky carbon being 100% (mass conversion). The flaky carbon may include thick flaky carbon. In the flaky carbon, the thickness of the multiple flaky carbons is preferably 30 layers or less.

[0044] The lamination of flaky carbon is calculated based on the thickness measured by observation with a transmission electron microscope (TEM).

[0045] Flaky carbon usually has a planar shape with many convex and concave angles, and it is difficult to define its size in general terms other than its thickness.

[0046] In this specification, the size of a single piece of flaky carbon is defined as the distance between the most distant convex angles of that piece of flaky carbon.

[0047] The size of the flaky carbon is preferably 20 nm or more, more preferably 100 nm or more, and even more preferably 200 nm or more. By using flaky carbon of the above size in the thermal conductive material, the thermal conductivity and heat dissipation can be further improved. The upper limit of the size of the flaky carbon is preferably large in terms of excellent thermal conductivity and heat dissipation. The upper limit of the size of the flaky carbon is not particularly limited, and is usually about 100 μm.

[0048] The size of the flaky carbon is measured by observation using a transmission electron microscope (TEM).

[0049] Flake carbon content In the thermal conductive composition (thermal conductive material) of the present invention, the content of flaky carbon is not particularly limited. From the viewpoint of thermal conductivity and heat dissipation, the content of flaky carbon is preferably 50% by mass to 99.5% by mass, and more preferably 60% by mass to 99.2% by mass, based on 100% by mass of the total amount of the thermal conductive composition (thermal conductive material).

[0050] (1-2) Organic compounds having hydrophilic groups and carbon-compatible hydrophobic groups The thermally conductive composition of the present invention contains (B) an organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group.

[0051] In a thermal conductive composition (thermal conductive material), by using an organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group, the flake carbon that maintains the graphene structure can be maintained in a uniformly dispersed state without agglomeration.

[0052] The organic compound can also function as a dispersant for uniformly dispersing the flaky carbon.

[0053] The organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group is not particularly limited, and a wide variety of organic compounds (preferably water-soluble compounds) that can function as dispersants for flaky carbon can be used.

[0054] Carbon-philic hydrophobic groups in organic compounds In the thermally conductive composition, the carbon-philic hydrophobic group is preferably at least one carbon-philic hydrophobic group selected from the group consisting of an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and a polyoxyalkylene group having 3 or more carbon atoms.

[0055] In the thermally conductive composition, the carbon-philic hydrophobic group is preferably an aryl group having two or more aromatic rings, or an organic compound having two or more aromatic rings in one molecule.

[0056] The carbon affinity hydrophobic group in the organic compound is not particularly limited, and is preferably an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, a polyoxyalkylene group having 3 or more carbon atoms, or the like.

[0057] The organic compound having a hydrophilic group and a carbon affinity hydrophobic group can contain one or more of these hydrophobic groups. When the organic compound having a hydrophilic group and a carbon affinity hydrophobic group has multiple hydrophobic groups, the multiple hydrophobic groups may be the same or different.

[0058] Alkyl group The alkyl group is preferably a chain alkyl group or a branched alkyl group. From the viewpoint of affinity with carbon, the alkyl group is preferably a chain alkyl group. From the viewpoint of affinity with carbon, the number of carbon atoms of the alkyl group is preferably 6 or more, more preferably 8 to 28, and further preferably 10 to 22.

[0059] The alkyl group is preferably a hexyl group, an octyl group, a decyl group, a undecyl group, a dodecyl group (or a lauryl group), a tridecyl group, a tetradecyl group (or a myristyl group), a pentadecyl group, a hexadecyl group (or a cetyl group), an octadecyl group, an icosyl group, or the like.

[0060] The alkyl group may or may not have a substituent. The substituent is preferably a cycloalkyl group (described later), an aryl group (described later), an aralkyl group, or the like.

[0061] The aralkyl group as the substituent of the alkyl group is preferably an aralkyl group having 7 to 14 carbon atoms and containing an aryl group (described later) and an alkyl group having 1 to 6 carbon atoms, and more preferably a benzyl group, a phenethyl group, or the like.

[0062] The substituent of the alkyl group is not particularly limited, and may have a group derived from a fluorene structure (such as a fluorenyl group).

[0063] When importance is placed on water solubility, the alkyl group substituent is preferably a phenyl group, etc. When importance is placed on compatibility with the flaky carbon, the alkyl group substituent is preferably a naphthyl group, a fluorenyl group, etc.

[0064] Alkenyl group The number of carbon atoms in the alkenyl group is preferably 4 or more, more preferably 6 to 100, and even more preferably 8 to 30, from the viewpoints of affinity with carbon and water solubility of the compound.

[0065] The alkenyl group is preferably an oleyl group, a linoleyl group, or the like.

[0066] The alkenyl group may or may not have a substituent. The substituent is preferably an alkyl group, a cycloalkyl group (described later), an aryl group (described later), an aralkyl group (described above), or the like.

[0067] The alkyl group as the substituent of the alkenyl group is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group, a butyl group, a tert-butyl group, or the like.

[0068] The substituent of the alkenyl group is not particularly limited, and may have a group derived from a fluorene structure (such as a fluorenyl group).

[0069] When importance is placed on water solubility, the substituent of the alkenyl group is preferably a phenyl group, etc. When importance is placed on compatibility with the flaky carbon, the substituent of the alkenyl group is preferably a naphthyl group, a fluorenyl group, etc.

[0070] Cycloalkyl group The cycloalkyl group is preferably a cycloalkyl group having 5 to 10 carbon atoms, more preferably 5 to 8 carbon atoms, and even more preferably 5 to 6 carbon atoms, and particularly preferably a cyclopentyl group, cyclohexyl group, or the like.

[0071] The cycloalkyl group may or may not have a substituent. The substituent is preferably an alkyl group, an aryl group (as described above), an aralkyl group (as described above), or the like.

[0072] The alkyl group as a substituent of the cycloalkyl group is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group, a butyl group, a tert-butyl group, or the like.

[0073] The substituent of the cycloalkyl group is not particularly limited, and may have a group derived from a fluorene structure (such as a fluorenyl group).

[0074] When importance is placed on water solubility, the substituent of the cycloalkyl group is preferably a phenyl group, etc. When importance is placed on compatibility with the flaky carbon, the substituent of the cycloalkyl group is preferably a naphthyl group, a fluorenyl group, etc.

[0075] Aryl Group The aryl group is preferably an aryl group having a carbon number of 6 to 18, more preferably 6 to 14. The aryl group may be any of a monocyclic aryl group, a condensed ring aryl group, and a polycyclic aryl group, and preferably, a phenyl group, a naphthyl group, an anthracenyl group, a phenanthrenyl group, a biphenyl group, a terphenyl group, a fluorenyl group, a pyrenyl group, a triphenylenyl group, or the like.

[0076] From the viewpoint of affinity with carbon, the aryl group is preferably an aryl group having two or more aromatic rings (a fused aryl group and a polycyclic aryl group) or having two or more aromatic rings in one molecule.

[0077] The aryl group may or may not have a substituent. The substituent is preferably an alkyl group, a cycloalkyl group (as described above), an aralkyl group (as described above), or the like.

[0078] The alkyl group as a substituent of the aryl group is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group, a butyl group, a tert-butyl group, or the like.

[0079] The substituent of the aryl group is not particularly limited, and may have a group derived from a fluorene structure (such as a fluorenyl group).

[0080] Polyoxyalkylene group with 3 or more carbon atoms Polyoxyethylene groups are generally hydrophilic.

[0081] Polyoxyethylene groups, polyoxypropylene groups, polyoxybutylene groups and other polyoxyalkylene groups having 3 or more carbon atoms become more hydrophobic as the degree of polymerization increases, and thus function as hydrophobic groups.

[0082] The polyoxyethylene group is preferably a polyoxypropylene group having a degree of polymerization of 4 or more, a polyoxybutylene group having a degree of polymerization of 3 or more, or the like.

[0083] When polyoxyethylene-polyoxypropylene, polyoxyethylene-polyoxybutylene, or the like is used as an organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group, the polyoxypropylene group and the polyoxybutylene group can also function as a hydrophobic group.

[0084] The polyoxyalkylene group having 3 or more carbon atoms may or may not have a substituent. The substituent is preferably an alkyl group, a cycloalkyl group (described above), an aralkyl group (described above), an aryl group (described above), or the like.

[0085] The alkyl group as a substituent of the polyoxyalkylene group having 3 or more carbon atoms is preferably an alkyl group having 1 to 6 carbon atoms, and more preferably a methyl group, an ethyl group, a propyl group, a butyl group, a tert-butyl group, or the like.

[0086] The substituent of the polyoxyalkylene group having 3 or more carbon atoms is not particularly limited, and may have a group derived from a fluorene structure (such as a fluorenyl group).

[0087] When importance is placed on water solubility, the substituent of the polyoxyalkylene group having 3 or more carbon atoms is preferably a phenyl group, etc. When importance is placed on compatibility with flaky carbon, the substituent of the polyoxyalkylene group having 3 or more carbon atoms is preferably a naphthyl group, a fluorenyl group, etc.

[0088] From the viewpoint of affinity with carbon, the carbon-affinity hydrophobic group in the organic compound is preferably an aryl group, a polyoxyalkylene group having 3 or more carbon atoms, etc., more preferably an aryl group, and even more preferably an aryl group having two or more aromatic rings (a fused aryl group and a polycyclic aryl group) or having two or more aromatic rings in one molecule of the organic compound.

[0089] The carbon affinity hydrophobic group in the organic compound is preferably a naphthyl group, anthracenyl group, phenanthrenyl group, biphenyl group, terphenyl group, fluorenyl group, pyrenyl group, triphenylenyl group, a polyoxypropylene group having a degree of polymerization of 4 or more, a polyoxybutylene group having a degree of polymerization of 3 or more, or the like.

[0090] Hydrophilic groups in organic compounds In the thermally conductive composition, the hydrophilic group possessed by the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is not particularly limited, so long as it can increase the solubility in water of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group.

[0091] The hydrophilic group possessed by the organic compound having a hydrophilic group and a carbon affinity hydrophobic group is preferably at least one hydrophilic group selected from the group consisting of the following general formulas (1) to (4), from the viewpoints of the water solubility of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group, the dispersibility of the flaky carbon, the thermal conductivity, and the heat dissipation properties, etc.

[0092] [ka]

[0093] Formula (1) represents an alcoholic hydroxyl group or a phenolic hydroxyl group.

[0094] In formula (2), R represents a divalent organic group, and both oxygen atoms represent ether bonds.

[0095] In formula (3), X1 represents a hydrogen atom, an alkali metal, NH4, or an organic ammonium.

[0096] In formula (4), X2 represents a hydrogen atom, an alkali metal, NH4, an organic ammonium, or an alkyl group.

[0097] In the thermally conductive composition, the hydrophilic group is preferably a phenolic hydroxyl group or a polyoxyethylene group.

[0098] The organic compound having a hydrophilic group and a carbon affinity hydrophobic group can contain one or more of these hydrophilic groups. When the organic compound having a hydrophilic group and a carbon affinity hydrophobic group uses a plurality of hydrophilic groups, the organic compound may contain a plurality of the same hydrophilic groups, may use a plurality of hydrophilic groups represented by the same general formula, or may use a plurality of hydrophilic groups represented by different general formulas.

[0099] Hydrophilic group of general formula (1) In the general formula (1), -OH can be either an alcoholic hydroxyl group or a phenolic hydroxyl group.

[0100] In general formula (1), -OH is preferably an alcoholic hydroxyl group from the viewpoints of water solubility of organic compounds having a hydrophilic group and a carbon-affinity hydrophobic group, dispersibility of flaky carbon, thermal conductivity, heat dissipation, and the like.

[0101] In general formula (1), when -OH contains a phenolic hydroxyl group (particularly when it contains multiple phenolic hydroxyl groups), it necessarily contains a benzene ring which has excellent hydrophobicity, and as a whole, the water solubility of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the dispersibility of the flaky carbon, the thermal conductivity, the heat dissipation, etc. are excellent.

[0102] From the viewpoint of water solubility in particular, the compound having the hydrophilic group of general formula (1) preferably has a group in which two or more phenolic hydroxyl groups are bonded to a benzene ring, and more preferably has a catechol (1,2-benzenediol) structure, a resorcinol (1,3-benzenediol) structure, a hydroquinone (1,4-benzenediol) structure, a hydroxyquinol (1,2,4-benzenetriol) structure, a phloroglucinol (1,3,5-benzenetriol) structure, or a pyrogallol (1,2,3-benzenetriol) structure.

[0103] Compounds having a hydrophilic group of general formula (1) are also included in natural products such as polyphenols and tannic acid, and are particularly preferably those having a pyrogallol (1,2,3-benzenetriol) structure or a catechol (1,2-benzenediol) structure, which have excellent water solubility.

[0104] Tannic acid is an organic compound that has two or more aromatic rings in one molecule and has a pyrogallol (1,2,3-benzenetriol) structure.

[0105] Hydrophilic group of general formula (2) In the general formula (2), the divalent organic group represented by R is not particularly limited, and is preferably a divalent hydrocarbon group. The divalent hydrocarbon group is preferably an aliphatic hydrocarbon group (an alkylene group (or an alkylidene group), a cycloalkylene group, an alkylene (or an alkylidene)-cycloalkylene group, a bicycloalkylene group or a tricycloalkylene group, etc.), an aromatic hydrocarbon group (an arylene group, an alkylene (or an alkylidene)-arylene group, etc.), etc.

[0106] In the general formula (2), the alkylene group (or alkylidene group) represented by the group R is preferably an alkylene group, more preferably C 1-8 is preferably an alkylene group, more preferably C 1-4 An alkylene group is particularly preferably C 2-4 An alkylene group, most preferably C 2-3 An alkylene group. The alkylene group (or alkylidene group) is preferably a methylene group, an ethylene group, an ethylidene group, a trimethylene group, a propylene group, a propylidene group, a tetramethylene group, an ethylethylene group, a butan-2-ylidene group, a 1,2-dimethylethylene group, a pentamethylene group, a pentane-2,3-diyl group, or the like.

[0107] In the general formula (2), the cycloalkylene group represented by the group R is preferably C 5-10 is a cycloalkylene group, more preferably C5-8 A cycloalkylene group. The cycloalkylene group is preferably a cyclopentylene group, a cyclohexylene group, a methylcyclohexylene group, a cycloheptylene group, or the like.

[0108] In the general formula (2), the alkylene (or alkylidene)-cycloalkylene group represented by the group R is preferably an alkylene-cycloalkylene group, more preferably C 1-6 Alkylene-C 5-10 A cycloalkylene group, more preferably C 1-4 Alkylene-C 5-8Cycloalkylene group. The alkylene (or alkylidene)-cycloalkylene group is preferably a methylene-cyclohexylene group, an ethylene-cyclohexylene group, an ethylene-methylcyclohexylene group, an ethylidene-cyclohexylene group, or the like.

[0109] In the general formula (2), the bi- or tricycloalkylene group represented by the group R is preferably a norbornane-diyl group or the like.

[0110] In the general formula (2), the arylene group represented by the group R is preferably C 6-10 An arylene group is preferably a phenylene group, a naphthalenediyl group, or the like.

[0111] In the general formula (2), the alkylene (or alkylidene)-arylene group represented by the group R is preferably an alkylene-arylene group, more preferably C 1-6 Alkylene-C 6-20 An arylene group, more preferably C 1-4 Alkylene-C 6-10 An arylene group, particularly preferably C 1-2 An alkylene-phenylene group. The alkylene (or alkylidene)-arylene group is preferably a methylene-phenylene group, an ethylene-phenylene group, an ethylene-methylphenylene group, an ethylidenephenylene group, or the like.

[0112] In the general formula (2), the divalent organic group represented by R is preferably a divalent aliphatic hydrocarbon group, and particularly preferably an alkylene group (e.g., a C alkylene group such as a methylene group or an ethylene group). 1-4 alkylene groups, etc.

[0113] The alkylene (or alkylidene)-cycloalkylene group and the alkylene (alkylidene)-arylene group are groups represented by "-Ra-Rb-".

[0114] In the formula, Ra represents an alkylene group or an alkylidene group each bonded to an oxygen atom in general formula (2), and Rb represents a cycloalkylene group or an arylene group.

[0115] The hydrophilic group represented by formula (2) is not particularly limited, and preferably, -OC2H4O-, -OC3H6O-, -OCH2O-, etc. can be used.

[0116] The hydrophilic group represented by the general formula (2) may preferably have a plurality of such groups (preferably 3 to 100 groups).

[0117] The hydrophilic group represented by the general formula (2) is preferably a polyoxymethylene group, a polyoxyethylene group, a polyoxypropylene group, or the like.

[0118] When the hydrophilic group represented by general formula (2) has a structure in which three or more hydrophilic groups represented by general formula (2) are polymerized, the hydrophilicity decreases and the hydrophobicity increases as the number of carbon atoms in R increases (preferably, the number of carbon atoms is 3 or more). The hydrophilic group represented by general formula (2) is preferably -OC2H4O-, -OCH2O-, etc., which can maintain hydrophilicity even when the degree of polymerization increases.

[0119] Hydrophilic group of general formula (3) In the general formula (3), the alkali metal represented by X1 is not particularly limited, and is preferably sodium, potassium, lithium, or the like.

[0120] In the general formula (3), the organic ammonium represented by X1 is preferably a quaternary ammonium, more preferably tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, or the like.

[0121] The hydrophilic group represented by the general formula (3) is not particularly limited, and is preferably -SO3 - H + , -SO3 - Na + , -SO3 -K + , -SO3 - Li + , -SO3 - NH4 + , -SO3 - N(CH3)4 + , -SO3 - N(C2H5)4 + , -SO3 - N(C3H7)4 + , -SO3 - N(C4H9)4 + etc.

[0122] Hydrophilic group of general formula (4) In the general formula (4), the alkali metal and organic ammonium represented by X2 are preferably those exemplified as the hydrophilic group in the general formula (3).

[0123] In the general formula (4), the alkyl group represented by X2 is preferably a chain alkyl group or a branched alkyl group. From the viewpoint of affinity with carbon, the alkyl group is preferably a chain alkyl group. From the viewpoint of affinity with carbon, the number of carbon atoms of the alkyl group is preferably 1 to 2.

[0124] The hydrophilic group represented by the general formula (4) is not particularly limited, and is preferably -COOH, -COONa, -COOK, -COOLi, -COONH4, -COON(CH3)4, -COON(C2H5)4, or -COON(C3H7)4. + , -COON(C4H9)4 + etc.

[0125] The hydrophilic group in the organic compound is preferably a hydrophilic group represented by general formula (2) from the viewpoints of water solubility of an organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group, pH-independent stability, dispersibility of flaky carbon, thermal conductivity, and heat dissipation.

[0126] When an organic compound has a hydrophilic group having multiple identical hydrophilic groups represented by general formula (2), that is, when the compound has a polymerized structure, the hydrophilicity of the water-soluble compound increases as the degree of polymerization increases for compounds having two or fewer carbon atoms, whereas the hydrophobicity of the compound increases as the degree of polymerization increases for compounds having three or more carbon atoms.

[0127] In an organic compound having a hydrophilic group and a carbon affinity hydrophobic group, the number of carbon atoms in the constituent parts other than the hydrophilic group (such as hydrophobic groups) is preferably 6 or more, and more preferably 8 to 18, from the viewpoints of the water solubility of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group, the dispersibility of the flaky carbon, thermal conductivity, heat dissipation, etc.

[0128] When a nonionic material (such as a nonionic surfactant) is used as the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the HLB value of the nonionic material is preferably 12 or more, and more preferably 13 to 19, from the viewpoints of the water solubility of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the dispersibility of the flaky carbon, thermal conductivity, heat dissipation, and the like.

[0129] When a non-ionic material is used as an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, if the hydrophobic group is the same (if the affinity with flaky carbon is about the same), the HLB value of the non-ionic material is preferably a high HLB value.

[0130] The organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group is not particularly limited.

[0131] As the organic compound having a hydrophilic group and a carbon affinity hydrophobic group, an aromatic water-soluble compound, a non-aromatic water-soluble compound, or the like is preferably used, and an aromatic water-soluble compound is more preferably used.

[0132] The organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is preferably polyoxyethylene lauryl ether, polyoxyethylene decyl ether, polyoxypropylene decyl ether, polyoxyethylene lauryl ether, polyoxyethylene naphthyl ether, polyoxypropylene lauryl ether, polyoxypropylene naphthyl ether, polyoxyethylene myristyl ether, polyoxypropylene myristyl ether, polyoxyethylene cetyl ether, polyoxypropylene cetyl ether, polyoxyethylene octylphenyl ether, polyoxypropylene octylphenyl ether, polyoxyethylene undecylphenyl ether, polyoxyethylene oct ... ether, polyoxypropylene undecyl phenyl ether, polyoxyethylene tridecyl phenyl ether, polyoxypropylene tridecyl phenyl ether, polyoxyethylene pentadecyl phenyl ether, polyoxypropylene pentadecyl phenyl ether, polyoxyethylene polyoxypropylene glycol, polyoxypropylene polyglyceryl ether, sodium cholate, potassium cholate, sodium dodecyl sulfonate, potassium dodecyl sulfonate, sodium dilauroyl glutamic acid lysine, potassium dilauroyl glutamic acid lysine, decaglycerol laurate, and n-decyl alcohol.

[0133] As the organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group, preferably polyoxyethylene alkyl ethers manufactured by Kao Corporation, such as Emulgen 103, Emulgen 104P, Emulgen 105, Emulgen 106, Emulgen 108, Emulgen 109P, Emulgen 120, Emulgen 123P, Emulgen 130K, Emulgen 147, Emulgen 150, Emulgen 210P, and Emulgen 220, can be used.

[0134] As the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, preferably, polyoxyethylene octylphenyl ethers such as Triton X-100, Triton X-114, Triton X-305, and Triton X-405 manufactured by The Dow Chemical Company can be used.

[0135] As the organic compound having a hydrophilic group and a carbon affinity hydrophobic group, polyoxyethylene naphthyl ethers such as Noigen EN and Noigen EN-10 manufactured by Daiichi Kogyo Seiyaku Co., Ltd. can be preferably used.

[0136] Content of organic compounds having hydrophilic groups and carbon-affinity hydrophobic groups In the thermal conductive composition (thermal conductive material) of the present invention, the content of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group is not particularly limited. From the viewpoint of imparting sufficient thermal conductivity and heat dissipation to the thermal conductive material, the content of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group is preferably 0.5% by mass to 50% by mass, more preferably 0.8% by mass to 40% by mass, based on 100% by mass of the total amount of the thermal conductive composition (thermal conductive material).

[0137] In the thermal conductive composition (thermal conductive material), from the viewpoint of imparting sufficient thermal conductivity and heat dissipation to the thermal conductive material, the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is preferably 1 part by mass to 100 parts by mass, and more preferably 2 parts by mass to 80 parts by mass, per 100 parts by mass of flaky carbon.

[0138] In a thermally conductive composition (thermally conductive material), when the content of an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is small, the surface of the flaky carbon is coated with an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group.

[0139] In a thermally conductive composition (thermally conductive material), when the content of an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is high, the composition has a configuration in which flaky carbon is dispersed in the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group.

[0140] In either case of the thermally conductive composition (thermal conductive material), the presence of an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group around the flaky carbon suppresses the aggregation of the flaky carbon, thereby making it possible to obtain a material with excellent thermal conductivity and heat dissipation properties.

[0141] (1-3) Spherical material The thermally conductive composition of the present invention contains (C) at least one material (spherical material) which is approximately spherical and has a diameter of 5 μm or more, and is selected from the group consisting of inorganic materials and carbon materials.

[0142] In the thermally conductive composition, (C) the spherical material is preferably at least one material selected from the group consisting of aluminum oxide (alumina), zinc oxide, magnesium oxide, magnesium carbonate, boron nitride, silicon nitride, aluminum nitride, and graphite.

[0143] In the thermally conductive composition, the (A) flaky carbon and the (C) spherical material are preferably a thermally conductive composite in which the (A) flaky carbon is supported on the (C) spherical material.

[0144] The spherical material is an inorganic material or a carbon material.

[0145] In thermally conductive compositions (thermally conductive materials), the use of spherical materials together with flaky carbon has the effect of suppressing the orientation of the flaky carbon and generating a thermal conduction path along the surface of the spherical materials.

[0146] When the thermal conductive composition (thermal conductive material) is molded into a sheet, the thermal conductivity in the thickness direction tends to be smaller than in the in-plane direction. By using spherical materials in the thermal conductive composition (thermal conductive material), the thermal conductivity in the thickness direction can be strengthened.

[0147] In thermally conductive compositions (thermally conductive materials), by using a highly insulating material as the spherical material and using highly dispersible flake carbon, it is possible to improve thermal conductivity while creating a state with low electrical conductivity.

[0148] The spherical material is approximately spherical in order to provide the thermal conductive composition (thermal conductive material) with excellent thermal conductivity and heat dissipation, and has a diameter of 5 μm or more, preferably 7 μm to 300 μm, and more preferably 10 μm to 200 μm. By setting the diameter of the spherical material within the above range, a thermal conductive material having sufficient thermal conductivity and heat dissipation can be obtained.

[0149] (1-4) Resin component The thermally conductive composition of the present invention contains a resin component (D).

[0150] The resin component is preferably a thermoplastic resin, a thermosetting resin, a rubber, or the like.

[0151] The thermosetting resin is preferably polyurethane, epoxy resin, phenol resin, melamine resin, urea resin, unsaturated polyester resin, alkyd resin, thermosetting polyimide, or the like.

[0152] The thermoplastic resin preferably used is a polyolefin such as polyethylene or polypropylene, polyvinyl chloride, an ethylene-vinyl acetate copolymer, polystyrene, polyvinyl acetate, polyurethane, polytetrafluoroethylene, an acrylonitrile-butadiene-styrene resin, an acrylonitrile-styrene resin, an acrylic resin, or polyvinyl alcohol.

[0153] The present invention includes a coating material that includes a thermally conductive composition.

[0154] The present invention includes a coating film formed by a paint containing a thermally conductive composition.

[0155] The present invention includes a resin molded article comprising a thermally conductive composition.

[0156] The shape of the thermally conductive composition (thermally conductive material) is not particularly limited, and is preferably a coating film, a sheet, a lump, a fiber, or the like.

[0157] The thermally conductive composition (thermally conductive material) of the present invention is a material that not only has excellent thermal conductivity but also has excellent heat dissipation properties.

[0158] The thermally conductive composition (thermally conductive material) of the present invention not only has excellent thermal conductivity, but also dissipates heat after being heated, making it possible to more quickly dissipate heat and cool the temperature.

[0159] The thermally conductive composition (thermally conductive material) of the present invention functions as a thermally conductive heat dissipating material.

[0160] Since the thermally conductive composite of the present invention has excellent thermal conductivity and heat dissipation properties, it is preferably used for applications such as thermally conductive grease for electronic materials, thermally conductive paint for electronic materials, thermally conductive rubber for electronic materials, thermally conductive paint for LEDs, paint for heat sinks, and coatings for various heat exchangers.

[0161] [2] Method for producing thermally conductive composition The present invention includes an invention related to a method for making a thermally conductive composition.

[0162] The method for producing the thermally conductive composite (thermally conductive composition) of the present invention includes the steps of: (1) comprising a step of mixing (A) a dispersion liquid containing flaky carbon having a thickness of 1 nm to 100 nm, and 1 part by mass of the flaky carbon with (C) 0.1 parts by mass to 100 parts by mass of at least one material that is approximately spherical and has a diameter of 5 μm or more and is selected from the group consisting of inorganic materials and carbon materials, The thermal conductive composite is (B) an organic compound having a hydrophilic group and a carbon-affinic hydrophobic group; (D) a resin component.

[0163] In a method for producing a thermal conductive composition, 1 part by mass of flaky carbon ((A) flaky carbon having a thickness of 1 nm to 100 nm) is mixed with 0.1 parts by mass to 100 parts by mass of a spherical material ((C) approximately spherical with a diameter of 5 μm or more, and at least one material selected from the group consisting of inorganic materials and carbon materials) and a resin component.

[0164] (2-1) Method for producing flaky carbon dispersion liquid, which is a part of the thermal conductive composite In a dispersion (flaky carbon dispersion) containing flaky carbon, an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, and a solvent, the flaky carbon, the hydrophilic group, and the organic compound having a carbon-affinity hydrophobic group are as described above.

[0165] The solvent used to prepare the flaky carbon dispersion liquid is preferably water as the main solvent, from the viewpoints of the dispersibility of the flaky carbon, the thermal conductivity and heat dissipation properties of the resulting thermal conductive material, and the like.

[0166] The flaky carbon dispersion may contain components other than water as necessary. The components other than water may be, for example, organic solvents such as alcohol. The components other than water may be used to increase the solubility of compounds having hydrophilic and hydrophobic groups when producing the flaky carbon. The components other than water are added in a range that does not remove the organic compounds from the carbon surface and provides good peeling and dispersion.

[0167] The water content in the solvent used is not particularly limited, and from the viewpoints of the dispersibility of the flaky carbon, the thermal conductivity and heat dissipation properties of the resulting thermal conductive material, etc., the water content is preferably 70 mass% or more (70 mass% to 100 mass%), and more preferably 75 mass% to 100 mass%, of the total amount of the solvent being 100 mass%.

[0168] As the solvent, only water may be used. As the solvent, an organic solvent may not necessarily be used. As the solvent, from the viewpoint of further improving the solubility of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group in water, it is preferable to use an organic solvent such as methanol, ethanol, 2-propanol, tert-butyl alcohol, etc.; glycols such as ethylene glycol, etc.; glycerin; 2-methoxyethanol, etc.

[0169] The content of the organic solvent in the solvent used is preferably 30 mass% or less (0 to 30 mass%), and more preferably 5 mass% to 25 mass%, based on 100 mass% of the total amount of the solvent, from the viewpoints of the solubility of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the thermal conductivity and heat dissipation properties of the obtained thermal conductive material, etc.

[0170] In the flaky carbon dispersion, the content of flaky carbon is not particularly limited, and from the viewpoint of ease of composition of the thermal conductive material, the content is preferably 20 mass% or less, more preferably 0.0001 mass% to 15 mass%, and even more preferably 0.001 mass% to 10 mass%, based on the total amount of the flaky carbon dispersion being 100 mass%.

[0171] The solvent content is not particularly limited, and from the viewpoint of ease of composition of the thermal conductive material, it is preferably 40% by mass to 99.9998% by mass, more preferably 63% by mass to 99.998% by mass, and even more preferably 85% by mass to 99.98% by mass, with the total amount of the flaky carbon dispersion liquid being 100% by mass.

[0172] The method for producing the flaky carbon dispersion is not particularly limited, and preferably, flaky carbon and an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group are added to a solvent.

[0173] The method for producing a flaky carbon dispersion preferably involves adding flaky carbon to a dispersion of an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, or adding an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group to a dispersion of flaky carbon, or simultaneously adding the flaky carbon and the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group to a solvent.

[0174] <Grinding method (shearing treatment)> From the viewpoint of further improving the dispersibility of the flaky carbon, making it less likely to agglomerate, and further enhancing the thermal conductivity and heat dissipation properties of the obtained thermal conductive material, preferably, a composition containing a carbonaceous material having a layered structure (a material for producing flaky carbon, described below) and an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is placed between a rotating turntable and a plate placed approximately parallel to the turntable, and the carbonaceous material in the composition is subjected to a shearing treatment (grinding method) while adjusting the shortest distance between the turntable and the plate to 200 μm or less.

[0175] The shearing treatment causes the carbonaceous material having a layered structure to be atomized, so that the carbonaceous material having a layered structure can be efficiently exfoliated while maintaining the graphene structure, and the treatment time can be reduced.

[0176] The rotating plate and the plate are arranged approximately parallel to each other during the shearing process, and may not be strictly parallel. Specifically, the angle between the axis perpendicular to the rotating plate and the axis perpendicular to the plate is preferably 10° or less, more preferably 5° or less. The axis perpendicular to the rotating plate and the axis perpendicular to the plate are preferably strictly parallel.

[0177] The shortest distance between the two faces when the shearing treatment is performed is not particularly limited as long as the carbonaceous material having a layered structure can be sufficiently sliced, and is preferably 200 μm or less, more preferably 1 μm to 50 μm, and even more preferably 2 μm to 30 μm.

[0178] The rotating disk and the disk are installed approximately parallel to each other, and the distance between the rotating disk and the disk may vary depending on the location. In this case, the shortest distance between the rotating disk and the disk means the shortest distance between the rotating disk and the disk. It is not necessary to leave a gap between the rotating disk and the disk in advance, and the material to be processed may be sandwiched between the rotating disk and the disk, or the rotating disk and the disk may be brought into contact with each other, and a carbonaceous material having a layered structure may be sandwiched between the rotating disk and the disk, thereby widening the gap between the rotating disk and the disk.

[0179] The shearing treatment can be carried out using any device that has a mechanism for rotating a disk-like object, and is preferably carried out using a millstone, a vibration mixer, a spin coater, a grinder, or the like.

[0180] The size of the rotating disk and the disk used is not particularly limited, but from the viewpoint of scale-up, mass production, etc., it is preferably 100 mm to 10,000 mm, and more preferably 150 mm to 6,000 mm.

[0181] The rotation speed of the rotating disk during the shear treatment is not particularly limited, and is preferably within a range that can sufficiently exfoliate the carbonaceous material having a layered structure, more preferably 1,000 ppm to 10,000 ppm, and even more preferably 1,500 ppm to 5,000 ppm.

[0182] By performing the shearing treatment, the carbonaceous material having a layered structure can be brought into contact with the plate, and the carbonaceous material having a layered structure can be brought into contact with another carbonaceous material having a layered structure, and shear can be applied to the carbonaceous material having a layered structure in a direction parallel to the graphene layer of the carbonaceous material having a layered structure.

[0183] By reducing the shortest distance between the rotating disks in the shearing treatment and increasing the rotation speed of the rotating disks, it is possible to make the conditions stronger, and the carbonaceous material having a layered structure can be more efficiently exfoliated and the treatment time can be further reduced. The shearing operation is preferably performed once or more, and more preferably three or more times.

[0184] The temperature at which the shear treatment is carried out is not particularly limited and is a temperature at which the carbonaceous material having a layered structure can be sufficiently exfoliated, and is preferably 0° C. or higher, more preferably 0° C. to 100° C., and even more preferably 20° C. to 95° C. The temperature at which the shear treatment is carried out is preferably a condition at which the solubility of an organic compound having a hydrophilic group and a hydrophobic group having a high affinity with carbon is high.

[0185] The temperature at which the shearing treatment is carried out is preferably a higher temperature when the solubility increases at a higher temperature. When a water-soluble compound having a cloud point is used, the temperature at which the shearing treatment is carried out is preferably maintained at a temperature equal to or lower than the cloud point.

[0186] In order to thoroughly contact the carbonaceous material having a layered structure with the organic compound having a hydrophilic group and a hydrophobic group having high affinity for carbon before the shearing treatment is performed, it is preferable to stir the material in advance using a stirrer, ultrasonic disperser or the like before preparing the composition, so that the organic compound having a hydrophilic group and a hydrophobic group having high affinity for carbon is allowed to blend with the surface of the carbonaceous material having a layered structure.

[0187] When graphite oxide is used as the carbonaceous material having a layered structure, the graphite oxide exists as an oxide of flaky carbon in the dispersion that has been subjected to shear treatment. When graphite oxide is used as the carbonaceous material having a layered structure, it is preferable to perform a reduction treatment as a post-treatment. Various methods such as chemical reduction and electrochemical reduction can be used for the reduction treatment, and chemical reduction is preferable.

[0188] The reduction treatment is preferably a chemical reduction using a reducing agent such as hydrazine, sodium borohydride, etc. The amount of the reducing agent is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, per 1 part by mass of the flaky carbon oxide.

[0189] The reduction treatment is preferably performed with heating during reduction, which makes the reduction easier. The heating temperature is preferably 40°C to 200°C, more preferably 50°C to 150°C, and further preferably 60°C to 120°C.

[0190] The reduction time of the reduction treatment is preferably about 10 minutes to 64 hours, more preferably about 30 minutes to 48 hours, and further preferably about 1 hour to 24 hours. The reduction time is preferably set so that the graphene structure is not excessively destroyed.

[0191] According to the manufacturing method of the present invention, flaky carbon is obtained as a flaky carbon dispersion. In the manufacturing method, an organic compound having a hydrophilic group and a hydrophobic group having a high affinity with carbon is contained, and the flaky carbon dispersion also contains an organic compound having a hydrophilic group and a hydrophobic group having a high affinity with carbon. The organic compound having a hydrophilic group and a hydrophobic group having a high affinity with carbon is adsorbed on the surface of the flaky carbon, and can disperse the flaky carbon in a high concentration in an isolated manner in a solvent, and also functions as a dispersant in the flaky carbon dispersion.

[0192] An organic compound having a hydrophilic group and a hydrophobic group that has a high affinity for carbon exhibits sufficient thermal conductivity and heat dissipation by remaining on the surface of the flaky carbon.

[0193] In conventional methods involving oxidation and reduction treatment, it was not possible to form a flaky carbon dispersion on a plastic substrate because the plastic substrate was hydrolyzed during the reduction treatment and the flaky carbon aggregated when the reduction treatment was performed, meaning that it could not exist as a dispersion.

[0194] The manufacturing method of the present invention makes it possible to form a flake-shaped carbon dispersion on a substrate without hydrolysis of plastic substrates such as polyethylene terephthalate (PET) by incorporating an organic compound having a hydrophilic group and a hydrophobic group that has high affinity with carbon and carrying out a specific treatment.

[0195] <High pressure dispersion method (pressure treatment)> Flaky carbon dispersion liquid can be produced by subjecting a composition containing a carbonaceous material having a layered structure and an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group to a pressure treatment of 30 MPa or more (high-pressure dispersion method).

[0196] When the high-pressure dispersion method is adopted, a composition containing a carbonaceous material having a layered structure and an organic compound having a hydrophilic group and a hydrophobic group having high affinity with carbon is preferably subjected to a pressure treatment of 30 MPa or more.

[0197] The pressure treatment causes the carbonaceous material having a layered structure to be atomized, so that the carbonaceous material having a layered structure can be efficiently flaked while maintaining the graphene structure, and the treatment time can be reduced.

[0198] The pressure level when carrying out the pressure treatment is not particularly limited as long as it can sufficiently exfoliate the carbonaceous material having a layered structure, and is preferably 30 MPa or more, more preferably 50 MPa to 400 MPa, and even more preferably 100 MPa to 300 MPa.

[0199] The pressurization treatment can be carried out using a high-pressure dispersion device, a supercritical water production device, etc. The high-pressure dispersion device can disperse flaky carbon by applying mechanical pressure, while the supercritical water production device can increase the pressure of the system by heating the water.

[0200] Depending on the pressure treatment, for example, (i) causing two or more of the carbonaceous material dispersions to collide with each other; (ii) colliding the carbonaceous material dispersion with a metal or ceramic material (a high-hardness material such as silicon carbide or alumina); (iii) subjecting the carbonaceous material dispersion to a cross-sectional area of ​​1 cm 2 Passing through the following spaces It is possible to carry out the following processing.

[0201] By carrying out the (i) treatment and the (ii) treatment, it is possible to make the pressurizing conditions stronger, so that the carbonaceous material having a layered structure can be exfoliated more efficiently and the treatment time can be further reduced.

[0202] (iii) By carrying out the treatment, it is possible to more appropriately exfoliate a carbonaceous material having a layered structure while better maintaining the graphene structure.

[0203] The pressurizing operation is preferably carried out once or more, and more preferably, ten or more times.

[0204] The pressing temperature is not particularly limited, and may be set to a temperature at which the carbonaceous material having a layered structure can be sufficiently exfoliated.

[0205] The pressing temperature is preferably 0°C to 100°C, and more preferably 20°C to 95°C, in the cases of the (i) treatment and the (ii) treatment.

[0206] In the case of the treatment (iii), when pressure is applied mechanically, the pressurizing temperature is preferably 0° C. to 100° C. In the case of the treatment (iii), when pressure is generated by the supercritical state of water, the pressurizing temperature is preferably 373° C. to 700° C., and more preferably 380° C. to 450° C.

[0207] When the pressure treatment is performed, it is preferable to perform an ultrasonic dispersion treatment as a preliminary treatment (pretreatment) to atomize the carbonaceous material having a layered structure. The preliminary treatment (pretreatment) has the effect of preventing clogging, etc.

[0208] The output of the ultrasonic dispersion treatment is not particularly limited, and from the viewpoint of flaking the carbonaceous material having a layered structure, it is preferably stronger than that of a normal ultrasonic dispersion treatment (about 40 W to 50 W). The output of the ultrasonic dispersion treatment is preferably 100 W or more, more preferably 300 W to 20,000 W, and even more preferably 400 W to 18,000 W.

[0209] The ultrasonic dispersion temperature is not particularly limited as long as it is a temperature at which the carbonaceous material having a layered structure can be sufficiently exfoliated, and is preferably 0°C to 80°C, and more preferably 10°C to 70°C.

[0210] The ultrasonic dispersion time is not particularly limited and may be a time that can sufficiently exfoliate the carbonaceous material having a layered structure, and is preferably about 1 to 600 minutes, and more preferably about 3 to 120 minutes.

[0211] As a pre-treatment or post-treatment of these treatments, dispersion treatment using ordinary mechanical stirring, an emulsifying device, or other dispersion treatment using other dispersion devices such as a bead mill may be used in combination.

[0212] When graphite oxide is used as the carbonaceous material having a layered structure, the graphite oxide is present as an oxide of flaky carbon in the dispersion that has been subjected to pressure treatment. When graphite oxide is used as the carbonaceous material having a layered structure, it is preferable to perform a reduction treatment as a post-treatment. Various methods such as chemical reduction and electrochemical reduction can be used for the reduction treatment, and chemical reduction is preferable.

[0213] The reduction treatment is preferably a chemical reduction using a reducing agent such as hydrazine, sodium borohydride, etc. The amount of the reducing agent is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, and even more preferably 0.5 to 3 parts by mass, per 1 part by mass of the flaky carbon oxide.

[0214] The reduction treatment is preferably performed with heating during reduction, which makes the reduction easier. The heating temperature is preferably 40°C to 200°C, more preferably 50°C to 150°C, and further preferably 60°C to 120°C.

[0215] The reduction time of the reduction treatment is preferably about 10 minutes to 64 hours, more preferably about 30 minutes to 48 hours, and further preferably about 1 hour to 24 hours. The reduction time is preferably set so that the graphene structure is not excessively destroyed.

[0216] The method for producing the flaky carbon dispersion is preferably a grinding method, from the viewpoints of the thermal conductivity and heat dissipation of the thermally conductive composite (thermally conductive composition).

[0217] Conventionally, when producing flaky carbon by a wet method, a water dispersion containing an oxide of flaky carbon and an aqueous solvent is subjected to a reduction treatment. In the conventional method, it is difficult to maintain the graphene structure, and the obtained flaky carbon aggregates severely, making it difficult to obtain a flaky carbon water dispersion. The conventional method also has a problem in terms of safety.

[0218] When performing conventional high-pressure treatment, it is possible to obtain an aqueous dispersion of flaky carbon, but the resulting flaky carbon is easily destroyed, production tends to take a long time, and lumps that fail to peel off may remain.

[0219] According to the manufacturing method of the present invention for producing a flaky carbon dispersion, by using an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, it is possible to obtain flaky carbon in a uniformly dispersed state (flaky carbon dispersion) without the flaky carbon maintaining the graphene structure agglomerating.

[0220] According to the method for producing a flaky carbon dispersion liquid of the present invention, the obtained flaky carbon is not easily broken, flaky carbon can be obtained in a short time, and lumps that have not been peeled off are unlikely to remain. In the method for producing a flaky carbon dispersion liquid of the present invention, the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group functions as a dispersant for uniformly dispersing the flaky carbon.

[0221] In the method for producing the flaky carbon dispersion of the present invention, the content of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group is not particularly limited. From the viewpoint of being easily incorporated into the composition of the thermal conductive material, the content of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group is preferably 0.00001 mass% to 99.9 mass%, more preferably 0.0001 mass% to 50 mass%, and even more preferably 0.001 mass% to 30 mass%, based on the total amount of the flaky carbon dispersion being 100 mass%.

[0222] In the manufacturing method of the flaky carbon dispersion liquid of the present invention, the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group in the flaky carbon dispersion is not particularly limited, and from the viewpoint of ease of composition into the thermal conductive material, it is preferably 1 part by mass to 100 parts by mass, more preferably 2 parts by mass to 80 parts by mass, per 100 parts by mass of the flaky carbon.

[0223] The smaller the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the greater the content of the carbonaceous material having a layered structure, which makes it easier to improve the thermal conductivity and heat dissipation of the thermal conductive material and makes it easier to process at low cost.

[0224] The higher the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group, the easier it is for flaking (delamination) to occur, and there is a tendency for flaky carbon to be obtained more efficiently. If the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group is high, the viscosity of the thermal conductive material may increase, and the flaking efficiency may decrease.

[0225] From the viewpoint of a balance between the thermal conductivity, heat dissipation, cost, and efficiency of flaking of the thermally conductive material, it is preferable to appropriately set the content of the organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group.

[0226] In the production method, when a carbonaceous material dispersion is used, the content of the organic compound having a hydrophilic group and a carbon-affinity hydrophobic group in the carbonaceous material dispersion is preferably within the above-mentioned range.

[0227] By adopting a shearing method as a method for producing a flaky carbon dispersion, the direction of force application is parallel to the surface direction of the carbonaceous material having a layered structure, and processing can be performed in a narrow space. Compared with conventional production methods using high-speed stirring, ultrasonic treatment, high-pressure treatment, etc., the shearing method causes less destruction, can obtain larger-sized flaky carbon (e.g., flaky carbon with a size of 1 μm or more), has good peeling efficiency, can perform processing in a short time (few passes), and is less likely to leave thick lumps that have not been peeled off.

[0228] The carbonaceous material having a layered structure is not particularly limited, and is preferably natural graphite, artificial graphite, expanded graphite, amorphous graphite, graphite oxide, or the like.

[0229] The graphite oxide to be used may be graphite oxidized with one or more oxidizing agents such as sulfuric acid, nitric acid, potassium permanganate, hydrogen peroxide, etc. For example, when graphite oxide is obtained by the Hummers process, graphite is immersed in concentrated sulfuric acid, potassium permanganate is added to oxidize the graphite, and the reaction product is quenched with dilute sulfuric acid and / or hydrogen peroxide, and then washed with distilled water, whereby oxygen atoms are bonded to carbon atoms and oxygen atoms are introduced between layers to obtain graphite oxide.

[0230] When it is desired to obtain high-purity flaky carbon that does not contain heteroatoms such as oxygen, it is preferable to use graphite as the raw material, and more preferably, natural graphite and expanded graphite are used.

[0231] When using expanded graphite, it is preferable to use expanded graphite with less oxidation of the graphene structure. When using expanded graphite, it may be heat-treated at about 300°C to 1,000°C for about 10 seconds to 5 hours before use. By the heat treatment, it is possible to obtain expanded graphite that has been appropriately expanded.

[0232] When ease of production is important, graphite oxide is preferably used. By using graphite oxide, solvent molecules can be easily inserted between layers, and it is easy to exfoliate only in the layer direction. By using graphite oxide, the efficiency of exfoliation and dispersibility are improved, and the processing time can be shortened. When graphite oxide is used, a reduction process is required later.

[0233] From the viewpoint of further maintaining the graphene structure, electrical conductivity, and strength of the flaky carbon, it is preferable to use natural graphite, artificial graphite, expanded graphite, amorphous graphite, etc.

[0234] From the viewpoint of further improving the dispersibility of flaky carbon in the flaky carbon dispersion liquid, amorphous graphite is preferably used.

[0235] From the viewpoints of crystallinity, purity, and structural maintenance of the flaky carbon, it is preferable to use natural graphite, artificial graphite, expanded graphite, graphite oxide, etc.

[0236] When emphasis is placed on the crystallinity, strength, structural maintenance, etc. of the flaky carbon, it is preferable to use artificial graphite.

[0237] In the method for producing a flaky carbon dispersion, the content of the carbonaceous material having a layered structure in the system when a shearing process is performed between a rotating rotating disk and a disk installed approximately parallel to the rotating disk while maintaining the shortest distance between the two surfaces at 200 μm or less is not particularly limited. The content of the carbonaceous material having a layered structure is preferably 20 mass% or less, more preferably 0.0001 mass% to 15 mass%, and even more preferably 0.001 mass% to 10 mass%, based on the total amount of the composition used to produce the flaky carbon dispersion being 100 mass%.

[0238] The thinner the content of the carbonaceous material having a layered structure, the easier it is for flaking (delamination) to occur, flaky carbon can be obtained more efficiently, the number of processing steps can be reduced, and shear processing and the like can be easily performed while maintaining an appropriate viscosity.

[0239] The higher the content of the carbonaceous material having a layered structure, the better the productivity. From the viewpoint of the balance of the efficiency of flaking the carbonaceous material having a layered structure, viscosity, productivity, etc., the content of the carbonaceous material having a layered structure is preferably set appropriately. When a carbonaceous material dispersion is used, the content of the carbonaceous material having a layered structure in the flaky carbon dispersion is preferably set within the above range.

[0240] When producing the flaky carbon dispersion liquid, a carbonaceous material having a layered structure is preferably subjected to a specific treatment in the coexistence of an organic compound having a hydrophilic group and a carbon-affinitive hydrophobic group.

[0241] From the viewpoints of the efficiency of flaking the carbonaceous material having a layered structure, the thermal conductivity and heat dissipation properties of the resulting flaky carbon, etc., a specific treatment is preferably performed on a carbonaceous material dispersion containing a carbonaceous material having a layered structure and an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group.

[0242] The solvent may be any of the solvents described above. The solvent used to prepare the carbonaceous material dispersion (carbonaceous material dispersion liquid, or carbonaceous material coating film) may be any of the solvents described above.

[0243] When a specific treatment is performed using a carbonaceous material dispersion liquid using a solvent, the total amount of the solvent in the carbonaceous material dispersion liquid is not particularly limited. The total amount of the solvent in the carbonaceous material dispersion liquid is preferably 40% by mass to 99.9998% by mass, more preferably 63% by mass to 99.998% by mass, and even more preferably 85% by mass to 99.98% by mass, based on 100% by mass of the total amount of the carbonaceous material dispersion liquid, from the viewpoints of the exfoliation efficiency of the carbonaceous material having a layered structure, the solubility of the organic compound having a hydrophilic group and a carbon affinity hydrophobic group, and the like.

[0244] When a specific process is performed using a carbonaceous material dispersion using a solvent, the carbonaceous material dispersion may be prepared by adding a carbonaceous material having a layered structure to an organic compound dispersion having a hydrophilic group and a carbon-affinity hydrophobic group, or by adding an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group to a carbonaceous material dispersion having a layered structure, or by simultaneously adding a carbonaceous material having a layered structure and an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group to a solvent.

[0245] (2-2) Spherical material As the spherical material, preferably, aluminum oxide (alumina), zinc oxide, magnesium oxide, magnesium carbonate, boron nitride, silicon nitride, aluminum nitride, graphite, or the like is used.

[0246] (2-3) A step of mixing the flaky carbon dispersion liquid and the spherical material The thermally conductive composite of the present invention is produced by (1) mixing (A) a dispersion liquid containing flaky carbon having a thickness of 1 nm to 100 nm, and 0.1 parts by mass to 100 parts by mass of (C) at least one material that is approximately spherical and has a diameter of 5 μm or more and is selected from the group consisting of inorganic materials and carbon materials, for 1 part by mass of the flaky carbon.

[0247] In the step of mixing the flaky carbon dispersion liquid and the spherical material, the flaky carbon and the spherical material may be added separately to the resin.

[0248] In the process of mixing the flaky carbon dispersion liquid with the spherical material, by supporting the flaky carbon on the spherical material (thermal conductive composite), it is possible to improve the thermal conductivity of the thermal conductive material and suppress the orientation of the thermal conductive composition.

[0249] In the step of mixing the flaky carbon dispersion with the spherical material, the flaky carbon dispersion is mixed with the dried spherical material.

[0250] In the step of mixing the flaky carbon dispersion and the spherical material, an aqueous dispersion of the flaky carbon and a dispersion of the spherical material are mixed.

[0251] In the step of mixing the flaky carbon dispersion liquid and the spherical material, one of the materials may be a wet solid prepared by filtration, centrifugation, or the like.

[0252] In the process of mixing the flaky carbon dispersion liquid and the spherical material, both may be made into wet solids and mixed by applying strong shear.

[0253] The solvent for the dispersion is preferably water.

[0254] In the step of mixing the flaky carbon dispersion liquid and the spherical material, a dispersion liquid in which one or both of the solvents are replaced with an organic solvent, or a wet solid thereof may be used. In the step of mixing the flaky carbon dispersion liquid and the spherical material, a water-insoluble resin may be added.

[0255] The present invention is not limited to these examples in any way.

[0256] The present invention can be embodied in various forms without departing from the spirit and scope of the present invention. EXAMPLES

[0257] The present invention will be specifically described below with reference to examples.

[0258] The present invention is not limited to the following specific examples.

[0259] <(i) Flake-like carbon water dispersion, (ii) Spherical alumina-containing epoxy resin> Example 1 500 g of natural graphite ((A) flaky carbon with a thickness of 1 nm to 100 nm, manufactured by Ito Graphite Industries Co., Ltd.), 50 g of tannic acid ((B) an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group), and 10,000 g of water were mixed and processed in a ceramic grinder for one pass. The obtained dispersion had a solid content of 5.5% by weight, of which the carbon content was 5.0% by mass.

[0260] 100 g of acetone was added to 20 g of this dispersion containing 1 g of carbon, filtered, and then 100 g of acetone was added again and filtered to replace the water with acetone, thereby finally obtaining a dispersion containing 5.0 mass % of carbon.

[0261] A total of 1 g of an epoxy resin ((D) resin component) composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride was added to 1 g of spherical alumina ((C) approximately spherical and having a diameter of 5 μm or more, at least one material selected from the group consisting of inorganic materials and carbon materials, diameter 10 μm), and then 0.4 g (1 part by weight per 50 parts by weight of alumina) of an acetone dispersion containing 5% by weight of the flaky carbon was added (thermal conductive composition, thermal conductive composite). After distilling off the acetone, the mixture was hot pressed at 150° C. to produce a plate-shaped molded product (thermal conductive material).

[0262] Example 2 The experiment was carried out in the same manner as in Example 1, except that 0.8 g (2 parts by weight per 50 parts by weight of alumina) of the acetone dispersion was added.

[0263] Example 3 The experiment was carried out in the same manner as in Example 1, except that 1.2 g (3 parts by weight per 50 parts by weight of alumina) of the acetone dispersion was added.

[0264] Example 4 The experiment was carried out in the same manner as in Example 1, except that 2.0 g (5 parts by weight per 50 parts by weight of alumina) of the acetone dispersion was added.

[0265] Example 5 The experiment was carried out in the same manner as in Example 1, except that 4.0 g (10 parts by weight per 50 parts by weight of alumina) of the acetone dispersion was added.

[0266] Example 6 The experiment was carried out in the same manner as in Example 1, except that 8.0 g (20 parts by weight per 50 parts by weight of alumina) of the acetone dispersion was added.

[0267] <(i) Flake-like carbon water dispersion + spherical alumina, (ii) epoxy resin> Example 7 An experiment was carried out in the same manner as in Example 1, except that 0.4 g of the acetone dispersion (1 part by weight per 50 parts by weight of alumina) was first added to 1 g of spherical alumina and dried, and then the remaining components were added.

[0268] Example 8 An experiment was carried out in the same manner as in Example 2, except that 0.8 g of the acetone dispersion (2 parts by weight per 50 parts by weight of alumina) was first added to 1 g of spherical alumina and dried, and then the remaining components were added.

[0269] Example 9 An experiment was carried out in the same manner as in Example 5, except that 4.0 g of acetone dispersion (10 parts by weight per 50 parts by weight of alumina) was first added to 1 g of spherical alumina and dried, and then the remaining components were added.

[0270] Table 1 shows the thermal conductivity versus the amount of flaky carbon added, with the total of alumina and epoxy resin taken as 100.

[0271] [Table 1]

[0272] (Comparative Example 1, no flaky carbon) A total of 1 g of an epoxy resin composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride was added to 1 g of spherical alumina (diameter 10 μm), and then the mixture was hot-pressed at 150° C. to produce a plate-shaped molded product.

[0273] (Comparative Example 2, no spherical material) 500 g of natural graphite (manufactured by Ito Graphite Industries Co., Ltd.), 50 g of tannic acid, and 10,000 g of water were mixed and processed once with a ceramic grinder. The obtained dispersion had a solid content of 5.5% by weight, of which the carbon content was 5.0% by mass.

[0274] 100 g of acetone was added to 20 g of this dispersion containing 1 g of carbon, filtered, and then 100 g of acetone was added again and filtered to replace the water with acetone, thereby finally obtaining a dispersion containing 5.0 mass % of carbon.

[0275] 2.0 g of the dispersion (0.1 g of flaky carbon) was added to a total of 0.9 g of an epoxy resin composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride, and after distilling off the acetone, the mixture was hot-pressed at 150°C to produce a plate-shaped molded product.

[0276] (Comparative Example 3, no spherical material) 500 g of natural graphite (manufactured by Ito Graphite Industries Co., Ltd.), 50 g of tannic acid, and 10,000 g of water were mixed and processed once with a ceramic grinder. The obtained dispersion had a solid content of 5.5% by weight, of which the carbon content was 5.0% by mass.

[0277] 100 g of acetone was added to 20 g of this dispersion containing 1 g of carbon, filtered, and then 100 g of acetone was added again and filtered to replace the water with acetone, thereby finally obtaining a dispersion containing 5.0 mass % of carbon.

[0278] 4.0 g of the dispersion (0.2 g of flaky carbon) was added to a total of 0.8 g of an epoxy resin composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride, and after distilling off the acetone, the mixture was hot-pressed at 150°C to produce a plate-shaped molded product.

[0279] In Examples 1 to 6, the thermal conductivity was dramatically improved by adding flaky carbon, compared to alumina alone (Comparative Example 1).

[0280] In Examples 5 and 6, the thermal conductivity was improved by adding alumina, which does not have a high thermal conductivity by itself, compared to flaky carbon alone (Comparative Examples 2 and 3).

[0281] Examples 7 to 9 In Examples 7 to 9, first, a flaky carbon aqueous dispersion was mixed with spherical alumina to allow it to be supported (forming a thermally conductive composite), and then the mixture was mixed with an epoxy resin composition. As a result, the thermal conductivity was improved compared to when an epoxy resin composition containing spherical alumina was mixed with a flaky carbon aqueous dispersion (Examples 1, 2, and 5).

[0282] It can be assumed that by first contacting the flaky carbon with the alumina (forming a thermally conductive composite), a thermally conductive path is created on the surface of the alumina.

[0283] Example 9 500 g of natural graphite ((A) flaky carbon with a thickness of 1 nm to 100 nm, manufactured by Ito Graphite Industries Co., Ltd.), 50 g of tannic acid ((B) an organic compound having a hydrophilic group and a carbon-affinity hydrophobic group), and 10,000 g of water were mixed and processed in a ceramic grinder for one pass. The obtained dispersion had a solid content of 5.5% by weight, of which the carbon content was 5.0% by mass.

[0284] 100 g of acetone was added to 20 g of this dispersion containing 1 g of carbon, filtered, and then 100 g of acetone was further added and filtered to replace the water with acetone, thereby finally obtaining a dispersion containing 5.0 mass % of carbon.

[0285] A total of 1 g of an epoxy resin ((D) resin component) composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride was added to 1 g of spherical boron nitride ((C) approximately spherical and having a diameter of 5 μm or more, at least one material selected from the group consisting of inorganic materials and carbon materials, diameter 12 μm), and then 4.0 g (10 parts by weight per 50 parts by weight of alumina) of an acetone dispersion containing 5% by weight of the flaky carbon was added (thermal conductive composition, thermal conductive composite). After distilling off the acetone, the mixture was hot pressed at 150° C. to produce a plate-shaped molded product (thermal conductive material).

[0286] (Comparative Example 4, no flaky carbon) A total of 1 g of an epoxy resin composition consisting of bisphenol A glycidyl ether and 4-methylphthalic anhydride was added to 1 g of spherical boron nitride (diameter 12 μm), and then the mixture was hot-pressed at 150° C. to produce a plate-shaped molded product.

[0287] Example 10 The test was carried out in the same manner as in Example 9, except that the spherical boron nitride was replaced with spherical zinc oxide (diameter 20 μm).

[0288] (Comparative Example 5, no flaky carbon) The test was carried out in the same manner as in Comparative Example 4, except that the spherical boron nitride was changed to spherical zinc oxide (diameter 20 μm).

[0289] Example 11 The test was carried out in the same manner as in Example 9, except that the spherical boron nitride was replaced with spherical zinc oxide (diameter 50 μm).

[0290] (Comparative Example 6, no flaky carbon) The test was carried out in the same manner as in Comparative Example 4, except that the spherical boron nitride was changed to spherical zinc oxide (diameter 50 μm).

[0291] Example 12 The test was carried out in the same manner as in Example 9, except that the spherical boron nitride was changed to spherical graphite (diameter 50 μm).

[0292] (Comparative Example 7, no flaky carbon) The test was carried out in the same manner as in Comparative Example 4, except that the spherical boron nitride was changed to spherical graphite (diameter 50 μm).

[0293] Example 13 The test was carried out in the same manner as in Example 9, except that the spherical boron nitride was changed to spherical graphite (diameter 100 μm).

[0294] (Comparative Example 8, no flaky carbon) The test was carried out in the same manner as in Comparative Example 4, except that the spherical boron nitride was changed to spherical graphite (diameter 100 μm).

[0295] [Table 2]

[0296] In Comparative Example 4, spherical boron nitride was added, and the thermal conductivity in the thickness direction was higher than that of Comparative Example 1 (single alumina) or Comparative Example 4 (plate-like alumina).

[0297] In Example 9, when a flaky carbon aqueous dispersion was mixed with an epoxy resin composition containing spherical boron nitride, the thermal conductivity in the in-plane direction was approximately eight times that of Comparative Example 4 (spherical boron nitride only), and the thermal conductivity in the thickness direction, which was high even with boron nitride alone, was improved by approximately two times (Table 2).

[0298] In Example 10, the thermal conductivity was improved by 6.4 times in the thickness direction and by 9.4 times in the in-plane direction as compared with Comparative Example 5.

[0299] In Example 11, the thermal conductivity was improved by 4.8 times in the thickness direction and 10.3 times in the in-plane direction compared to Comparative Example 6.

[0300] In Examples 10 and 11, in comparison with the comparative example, the thermal conductivity in the in-plane direction increased by about 10 times, and the thermal conductivity in the thickness direction, which was 1 W / m K or less, also improved significantly.

[0301] In Example 12, the thermal conductivity was improved by 2.5 times in the thickness direction and 4.9 times in the in-plane direction compared to Comparative Example 7.

[0302] In Example 13, the thermal conductivity was improved by 1.5 times in the thickness direction and 2.2 times in the in-plane direction compared to Comparative Example 8.

[0303] In Examples 12 and 13, the thermal conductivity was higher than that of the comparative examples, and the thermal conductivity was further improved even when mixed with spherical carbon, which also had a high thermal conductivity in the thickness direction.

[0304] In this way, a dramatic improvement in thermal conductivity was observed by adding flake carbon to the spherical thermal conductive material. Furthermore, a further improvement in thermal conductivity is expected by first coating the spherical thermal conductive material with flake carbon.

[0305] [Industrial Applicability] The present invention makes it possible to produce a thermally conductive material that has excellent thermal conductivity in both the thickness direction and the in-plane direction by using a specific organic compound in combination with thick flake-like carbon and spherical thermally conductive material.

Claims

1. 1. A thermally conductive composition comprising: (A) Thin flake carbon with a thickness of 1 nm to 100 nm; (B) an organic compound having a hydrophilic group and a carbon affinity hydrophobic group; (C) at least one material selected from the group consisting of inorganic materials and carbon materials, which is approximately spherical and has a diameter of 5 μm or more; (D) Resin component A thermally conductive composition comprising:

2. 2. The thermally conductive composition according to claim 1, wherein the hydrophilic group is at least one hydrophilic group selected from the group consisting of the following general formulas (1) to (4): 【Chemistry 1】 [Formula (1) represents an alcoholic hydroxyl group or a phenolic hydroxyl group. In formula (2), R represents a divalent organic group, and both oxygen atoms represent ether bonds. In formula (3), X 1 is a hydrogen atom, an alkali metal, NH 4 or organic ammonium. In formula (4), X 2 is a hydrogen atom, an alkali metal, NH 4 , organic ammonium, or alkyl group.

3. 2. The thermally conductive composition according to claim 1, wherein the hydrophilic group is a phenolic hydroxyl group or a polyoxyethylene group.

4. 2. The thermally conductive composition of claim 1, wherein the carbon affinity hydrophobic group is at least one carbon affinity hydrophobic group selected from the group consisting of an alkyl group, an alkenyl group, a cycloalkyl group, an aryl group, and a polyoxyalkylene group having 3 or more carbon atoms.

5. 10. The thermally conductive composition of claim 1, wherein the carbon-philic hydrophobic group is an aryl group having two or more aromatic rings.

6. 2. The thermally conductive composition of claim 1, wherein the (C) material is at least one material selected from the group consisting of aluminum oxide (alumina), zinc oxide, magnesium oxide, magnesium carbonate, boron nitride, silicon nitride, aluminum nitride, and graphite.

7. The (A) flaky carbon and the (C) material are The (C) material is a thermally conductive composite supported by the (A) flaky carbon.

10. The thermally conductive composition of claim 1.

8. A paint comprising the thermally conductive composition according to claim 7; or The coating film formed by the paint.

9. A resin molded article comprising the thermally conductive composition according to claim 7.

10. A method for producing a thermally conductive composite, comprising the steps of: (1) comprising a step of mixing (A) a dispersion liquid containing flaky carbon having a thickness of 1 nm to 100 nm, and 0.1 parts by mass to 100 parts by mass of (C) at least one material that is approximately spherical and has a diameter of 5 μm or more and is selected from the group consisting of inorganic materials and carbon materials, per part by mass of the flaky carbon; (B) an organic compound having a hydrophilic group and a carbon affinity hydrophobic group; (D) a resin component, Method for manufacturing a thermally conductive composite.

Citation Information

Patent Citations

  • Thermal interface materials with mixed aspect ratio particle dispersion

    JP2017519888A

  • Member for fixation and fixation device

    JP2018165807A

  • Heat conduction material

    JP2020164637A

  • Thermally conductive elastomer composition and thermally conductive molded body

    JP2021008527A

  • Inorganic powder composition, resin composition containing the same and heat radiation material

    JP2021181381A