Electrophotographic photoreceptor, process cartridge, electrophotographic device, and method of manufacturing electrophotographic photoreceptor

By integrating fluorine atom-containing resin particles with a specific polymer A in the surface layer, potential fluctuations in electrophotographic photoreceptors are suppressed, enhancing dispersibility and maintaining image quality and lifespan.

JP2024139416APending Publication Date: 2024-10-09CANON KK

Patent Information

Application Number
JP2023050344
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing electrophotographic photoreceptors experience significant potential fluctuations during long-term use, despite having improved abrasion resistance through the use of fluorine atom-containing resin particles, which affect image quality and lifespan.

Method used

Incorporating fluorine atom-containing resin particles with a specific polymer A having a structural unit represented by formula (1) into the surface layer, which acts as a dispersant to enhance dispersibility and suppress charge accumulation, thereby reducing potential fluctuations.

Benefits of technology

The solution results in an electrophotographic photoreceptor with excellent dispersibility and reduced potential fluctuations during repeated long-term use, maintaining image quality and extending the photoreceptor's lifespan.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139416000001_ABST
    Figure 2024139416000001_ABST
Patent Text Reader

Abstract

To provide an electrophotographic photoreceptor which comprises a surface layer that features superior dispersibility of fluorine atom-containing resin particles and suppresses electric potential variations associated with repetitive use.SOLUTION: An electrophotographic photoreceptor is provided, comprising a surface layer containing fluorine atom-containing resin particles, a binder resin, and a polymer having a specific repeating unit.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to an electrophotographic photoreceptor, a process cartridge and an electrophotographic apparatus having the electrophotographic photoreceptor, and a method for manufacturing the electrophotographic photoreceptor. [Background technology]

[0002] As electrophotographic photoreceptors mounted in electrophotographic devices, those containing an organic photoconductive material (charge generating material) are widely used. In recent years, there has been a demand for improving the mechanical durability (wear resistance) of electrophotographic photoreceptors in order to extend the life of the electrophotographic photoreceptors and improve image quality during repeated use.

[0003] As a technique for improving the wear resistance of an electrophotographic photoreceptor, there is a method of incorporating fluorine atom-containing resin particles in the surface layer of the electrophotographic photoreceptor to reduce friction between the surface layer and a contact member such as a cleaning blade. Patent Document 1 discloses a technique for forming a surface layer using a dispersion liquid of fluorine atom-containing resin particles such as polytetrafluoroethylene resin particles as a coating liquid for the surface layer.

[0004] In addition, when preparing a dispersion liquid of fluorine-containing resin particles, a method is known in which a fluorine-containing (meth)acrylic polymer is used as a dispersant for the fluorine-containing resin particles in order to improve dispersibility. Patent Documents 2 and 3 disclose a technique for improving the dispersibility of fluorine-containing resin particles by using a fluorine-containing (meth)acrylic polymer having a specific structure as a dispersant.

[0005] Patent Document 4 discloses an electrophotographic photoreceptor having an outermost surface layer containing a fluorine-based graft polymer and fluorine-containing resin particles, the fluorine-based graft polymer containing a structural unit having an acidic group with a pKa of 3 or less. [Prior art documents] [Patent documents]

[0006] [Patent Document 1] Japanese Patent Application Publication No. 06-332219 [Patent Document 2] JP 2012-189715 A [Patent Document 3] JP 2009-104145 A [Patent Document 4] Patent Publication No. 2021-47236 Summary of the Invention [Problem to be solved by the invention]

[0007] However, in the techniques disclosed in Patent Document 2 and Patent Document 3, while a surface layer excellent in dispersibility of fluorine-containing resin particles can be obtained, there are cases where potential fluctuations cannot be sufficiently suppressed during long-term repeated use of an electrophotographic photoreceptor. In particular, in an electrophotographic photoreceptor having a surface layer excellent in abrasion resistance for the purpose of extending the life of the electrophotographic photoreceptor, there is a problem that potential fluctuations become large during long-term repeated use. Therefore, there is room for improvement in suppressing potential fluctuations during long-term repeated use of an electrophotographic photoreceptor.

[0008] One aspect of the present disclosure is to provide an electrophotographic photoreceptor in which potential fluctuations during long-term repeated use are suppressed. Another aspect of the present disclosure is directed to providing a process cartridge having the electrophotographic photosensitive member mounted thereon, and an electrophotographic apparatus having the process cartridge. Another aspect of the present disclosure is directed to providing a method for producing the electrophotographic photoreceptor. [Means for solving the problem]

[0009] According to one embodiment of the present disclosure, there is provided an electrophotographic photoreceptor having a surface layer, the surface layer containing fluorine atom-containing resin particles, a binder material, and a polymer A having a structural unit represented by the following formula (1): [ka] (In formula (1), R11 represents a hydrogen atom or a methyl group, R 12 and R 13 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms, n is 0 to 3, Rf 1 each independently represents a perfluoroalkylene group having 1 to 5 carbon atoms or a perfluoroalkylidene group having 1 to 5 carbon atoms; Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms. The present invention provides an electrophotographic photoreceptor comprising: According to another aspect of the present disclosure, there is provided a process cartridge that integrally supports the electrophotographic photosensitive member and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably attachable to a main body of an electrophotographic apparatus. According to another aspect of the present disclosure, there is provided an electrophotographic apparatus having the electrophotographic photoreceptor, a charging unit, an exposure unit, a developing unit, and a transfer unit. According to another aspect of the present disclosure, there is provided a method for producing the electrophotographic photoreceptor. Effect of the Invention

[0010] According to one embodiment of the present disclosure, it is possible to provide an electrophotographic photoreceptor in which the dispersibility of fluorine-containing resin particles in the surface layer is excellent and potential fluctuation during long-term repeated use is suppressed. [Brief description of the drawings]

[0011] [Figure 1] FIG. 1 is a schematic diagram illustrating an example of a configuration of an electrophotographic photoreceptor according to the present disclosure. [Diagram 2] FIG. 1 is a diagram showing an example of a polishing machine using a polishing sheet. [Diagram 3] 1 is a diagram showing an example of a schematic configuration of a process cartridge equipped with an electrophotographic photosensitive member of the present disclosure, and an electrophotographic apparatus equipped with the process cartridge. [Figure 4] FIG. 2 is a schematic diagram illustrating an example of a process cartridge having the electrophotographic photoreceptor of the present disclosure. [Diagram 5] 1 is a schematic diagram illustrating an example of an electrophotographic apparatus having an electrophotographic photoreceptor according to the present disclosure. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] The present disclosure will be described in detail below with reference to preferred embodiments. As a result of investigations by the present inventors, it has been found that by incorporating fluorine atom-containing resin particles, a binder material, and a polymer A having a structural unit represented by the following formula (1) in the surface layer of an electrophotographic photoreceptor, it is possible to obtain an electrophotographic photoreceptor in which the dispersibility of the fluorine atom-containing resin particles in the surface layer is excellent and potential fluctuation during long-term repeated use is suppressed. [ka] (In formula (1), R 11 represents a hydrogen atom or a methyl group, R 12 and R 13 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms, n is 0 to 3, Rf 1 each independently represents a perfluoroalkylene group having 1 to 5 carbon atoms or a perfluoroalkylidene group having 1 to 5 carbon atoms; Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms.

[0013] The polymer A may or may not contain a structural unit having an acidic group with a pKa of 3 or less, but it is preferable that it does not contain such a structural unit. The pKa of an acidic group is determined by a measurement using a known method such as titration. Examples of acidic groups with a pKa of 3 or less include a sulfonic acid group (methanesulfonic acid: pKa-2.6), a phosphonic acid group (first dissociation: pKa 1.5), a phosphoric acid group (first dissociation: pKa 2.12), and a fluorinated alkyl carboxylic acid group (e.g., trifluoroacetic acid: pKa-0.25, difluoroacetic acid: pKa 1.24, and monofluoroacetic acid: pKa 2.66).

[0014] Here, the present inventors believe that the polymer A having the structural unit represented by the formula (1) functions as a dispersant for fluorine-containing resin particles in the process of preparing a surface layer coating liquid for forming a surface layer of an electrophotographic photoreceptor. The present inventors also believe that the polymer A having the structural unit represented by the formula (1) functions as a dispersant for fluorine-containing resin particles in the process of forming a coating film using the surface layer coating liquid, and drying and / or curing the coating film to form the surface layer.

[0015] The present inventors speculate as follows why the electrophotographic photoreceptor of the present disclosure has excellent dispersibility of the fluorine atom-containing resin particles in the surface layer and excellent effect of suppressing potential fluctuation during long-term repeated use. An electrophotographic photoreceptor having a surface layer containing fluorine-containing resin particles and a dispersant tends to have a large potential fluctuation during long-term repeated use. This is due to the -(CF2) of the dispersant attached to the fluorine-containing resin particles contained in the surface layer. n This is thought to be because electric charges tend to accumulate in the chains. As a result of the investigations by the present inventors, -(CF2) n When the surface layer contains a polymer having a structural unit containing a - chain, -(CF2) n -Chain and-(CF2) n It was found that the presence of an oxygen atom between the -(CF2) chain has the effect of suppressing charge trapping. n - The greater the number of carbon atoms in the chain, the more easily electric charges accumulate, and in some cases the effect of suppressing potential fluctuations may not be sufficient. As a result of further investigations by the present inventors, it has been found that by incorporating polymer A having a structural unit represented by the above formula (1) in the surface layer, charge trapping is suppressed, and an electrophotographic photoreceptor in which potential fluctuations during long-term repeated use are suppressed can be obtained.

[0016] The formula (1) contains a urethane bond. It is considered that the formula (1) contains a urethane bond, and therefore the urethane bond acts as a dispersant for fluorine-containing resin particles in the process of preparing a coating liquid for a surface layer for forming a surface layer of an electrophotographic photoreceptor, and in the process of forming the surface layer by forming a coating film using the coating liquid for the surface layer and drying and / or curing the coating film, and then has an excellent effect of suppressing potential fluctuation during long-term repeated use of the electrophotographic photoreceptor. The inventors believe that this is because the urethane bond in the formula (1) contained in the polymer A in the surface layer is broken by the discharge that the electrophotographic photoreceptor receives during long-term repeated use of the electrophotographic photoreceptor, thereby eliminating the charge accumulation in the polymer A and suppressing potential fluctuation. In addition, Rf in the formula (1) 1 are each independently a perfluoroalkylene group having 1 to 5 carbon atoms or a perfluoroalkylidene group having 1 to 5 carbon atoms, Rf 2 is a perfluoroalkyl group having a carbon number of 1 to 5. By doing so, it is believed that accumulation of electric charge in the structural unit represented by the formula (1) can be suppressed. Furthermore, n in the formula (1) is set to be equal to or greater than 0 and equal to or less than 3. By doing so, it is believed that accumulation of electric charge in the structural unit represented by the formula (1) can be suppressed. In addition, R in the formula (1) 12 and R 13 are each independently a single bond or an alkylene group having from 1 to 3 carbon atoms. By doing so, it is considered that the difference in surface energy between the structural unit represented by formula (1) and the fluorine-containing resin particles becomes small, and the structural unit is easily attached to the fluorine-containing resin particles.

[0017] <Fluorine atom-containing resin particles> The surface layer of the electrophotographic photoreceptor of the present disclosure contains fluorine atom-containing resin particles. The content of the fluorine atom-containing resin particles in the surface layer is preferably 5% by mass or more and 40% by mass or less with respect to the total mass of the surface layer. Specifically, when the surface layer is a charge transport layer, the content of the fluorine atom-containing resin particles in the charge transport layer is preferably 5% by mass or more and 20% by mass or less, and when the surface layer is a protective layer, the content of the fluorine atom-containing resin particles in the protective layer is preferably 20% by mass or more and 40% by mass or less with respect to the total mass of the protective layer. Examples of the resin contained in the fluorine atom-containing resin particles used in the present disclosure include the following. Polytetrafluoroethylene resin, polychlorotrifluoroethylene resin, polytetrafluoroethylenepropylene resin, polyvinyl fluoride resin, polyvinylidene fluoride resin, or polydichlorodifluoroethylene resin. It is also preferable to use particles containing a plurality of the above resins. Among the above, from the viewpoint of improving dispersibility, it is more preferable that the fluorine atom-containing resin particles are polytetrafluoroethylene (PTFE) resin. In cross-sectional observation of the surface layer, the arithmetic mean of the major axis of the primary particles (average primary particle size) measured from a secondary electron image by a scanning electron microscope is preferably 150 nm or more and 300 nm or less from the viewpoint of improving dispersibility and suppressing potential fluctuation. Furthermore, the fluorine atom-containing resin particles preferably have an average primary particle size of 180 nm or more and 250 nm or less. The fluorine atom-containing resin particles preferably have an average circularity (average circularity) of 0.75 or more, calculated from the area and perimeter of primary particles measured from a secondary electron image obtained by a scanning electron microscope. In order to ensure that the measured values ​​of the average primary particle size and average circularity of the fluorine atom-containing resin particles contained in the surface layer of the electrophotographic photoreceptor of the present disclosure fall within the above ranges, fluorine atom-containing resin particles whose average primary particle size and average circularity values ​​calculated by the following methods fall within the above ranges can be used.

[0018] (Method of measuring average primary particle size and average roundness) That is, in the examples of the present disclosure, the average particle size and average roundness of the fluorine-containing resin particles contained in the surface layer of the electrophotographic photoreceptor were measured using a field emission scanning electron microscope (FE-SEM) as follows. The fluorine-containing resin particles were attached to a commercially available carbon conductive tape, and the fluorine-containing resin particles not attached to the conductive tape were removed with compressed air, followed by platinum deposition. The deposited fluorine-containing resin particles were observed using an FE-SEM (S-4700) manufactured by Hitachi High-Technologies Corporation. The measurement conditions for the FE-SEM were as follows: Acceleration voltage: 2 kV WD: 5mm Magnification: 20,000 times Number of pixels: 1280 pixels vertically, 960 pixels horizontally (size of one pixel: 5 nm) The Feret's diameters of 100 particles were determined from the obtained images using ImageJ (open source software from the National Institutes of Health (NIH)), and the average value was calculated to obtain the average particle size. Similarly, the area and circumference were determined, and the circularity was calculated from the following formula (II), and the average value was calculated to obtain the average circularity. Circularity = 4 × π × (area) ÷ (perimeter squared) Formula (II) The fluorine atom-containing resin particles of the present disclosure may be used alone or in combination of two or more kinds.

[0019] <Polymer A having a structural unit represented by formula (1)> The surface layer of the electrophotographic photoreceptor of the present disclosure contains a polymer A having a structural unit represented by the following formula (1). [ka] In the previous formula (1), R 11 R represents a hydrogen atom or a methyl group. 12 and R 13 R each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms. 12 and / or R 13When Rf is an alkylene having 4 or more carbon atoms, the difference in surface energy between the structural unit represented by the formula (1) and the fluorine-containing resin particles becomes large, so that the structural unit is unlikely to adhere sufficiently to the fluorine-containing resin particles, and dispersibility tends to be insufficient. n is 0 or more and 3 or less. 1 each independently represents a perfluoroalkylene group having 1 to 5 carbon atoms or a perfluoroalkylidene group having 1 to 5 carbon atoms; Rf 2 Rf represents a perfluoroalkyl group having 1 to 5 carbon atoms. 1 and / or Rf 2 When the number of carbon atoms is 6 or more, accumulation of electric charge in the structural unit represented by the formula (1) cannot be sufficiently suppressed, and potential fluctuations cannot be sufficiently suppressed during long-term repeated use of the electrophotographic photoreceptor. In addition, in the formula (1), Rf 1 and Rf 2 From the viewpoint of improving the dispersibility of the fluorine-containing resin particles, the total number of carbon atoms in Rf is preferably 6 or more and 9 or less. 1 and Rf 2 The total number of carbon atoms is more preferably 6 or more and 8 or less.

[0020] Rf in the formula (1) 1 Examples of the structure include the structures shown below. [ka]

[0021] In addition, Rf in the formula (1) 2 Examples of the structure include the structures shown below. [ka]

[0022] In the polymer A contained in the surface layer of the electrophotographic photoreceptor of the present disclosure, the content of the structural unit represented by the formula (1) is preferably 5% by number or more and 50% by number or less with respect to the total structural units contained in the polymer A, from the viewpoint of improving the dispersibility of the fluorine atom-containing resin particles. The content of the structural unit represented by the formula (1) is preferably 0.070% by mass or more and 32.4% by mass or less with respect to the total structural units contained in the polymer A. Furthermore, the content of the structural unit represented by the formula (1) is more preferably 20% by number or more and 45% by number or less with respect to the total structural units contained in the polymer A. Furthermore, the content of the structural unit represented by the formula (1) is more preferably 0.30% by mass or more and 28.2% by mass or less with respect to the total structural units contained in the polymer A.

[0023] The weight average molecular weight of the polymer A having the structural unit represented by the formula (1) contained in the surface layer of the electrophotographic photoreceptor of the present disclosure is preferably 16,000 or more and 300,000 or less from the viewpoint of improving the dispersibility of the fluorine-containing resin particles and suppressing potential fluctuation. Furthermore, the weight average molecular weight of the polymer A having the structural unit represented by the formula (1) is more preferably 40,000 or more and 250,000 or less.

[0024] The weight average molecular weight of the polymer A having the structural unit represented by the formula (1) can be measured and calculated by the following method. (Weight average molecular weight measured by GPC) The weight average molecular weight according to the present disclosure is measured by gel permeation chromatography (GPC) as follows. First, a sample is dissolved in tetrahydrofuran (THF) at room temperature for 24 hours. The resulting solution is then filtered through a solvent-resistant membrane filter "Maeshori Disk" (manufactured by Tosoh Corporation) with a pore size of 0.2 μm to obtain a sample solution. The sample solution is adjusted so that the concentration of components soluble in THF is approximately 0.8 mass%. This sample solution is used to perform measurements under the following conditions. Equipment: HLC8120 GPC (detector: RI) (Tosoh Corporation) Column: 7 columns of Shodex KF-801, 802, 803, 804, 805, 806, 807 (Showa Denko Co., Ltd.) Eluent: Tetrahydrofuran (THF) ·Flow rate: 1.0ml / min Oven temperature: 40.0℃ Sample injection volume: 0.10ml In calculating the molecular weight of the sample, a molecular weight calibration curve prepared using standard polystyrene resins (e.g., trade names "TSK Standard Polystyrene F-850, F-450, F-288, F-128, F-80, F-40, F-20, F-10, F-4, F-2, F-1, A-5000, A-2500, A-1000, A-500" manufactured by Tosoh Corporation) is used.

[0025] The content of the polymer A having the structural unit represented by the formula (1) in the surface layer relative to the fluorine atom-containing resin particles is preferably from 2 to 10% by mass, more preferably from 4 to 8% by mass, from the viewpoints of improving dispersibility and suppressing potential fluctuation.

[0026] The polymer A is preferably a polymer having a structural unit represented by the above formula (1) and a structural unit represented by the following formula (2). [ka] (In formula (2), Y A1 represents an unsubstituted alkylene group, Y B represents an unsubstituted alkylene group, an alkylene group substituted with a halogen atom, an alkylene group substituted with a hydroxyl group, an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), or a divalent linking group derived by combining one or more of these groups or bonds with -O- or -S-, or a single bond; Z A represents a structure represented by formula (2A), a cyano group, or a phenyl group, R 21 , R 22each independently represents a hydrogen atom or a methyl group, m is an integer between 25 and 150. [ka] (In formula (2A), Z A1 represents an alkyl group having 1 to 4 carbon atoms.

[0027] In formula (2), Y B When represents an ester bond, -Y A1 -Y B -CH2- is -Y A1 -CO-O-CH2- and Y A1 -O-CO-CH2-, preferably -Y A1 In addition, in formula (2), Y B When represents an amide bond, -Y A1 -Y B -CH2- is -Y A1 -NH-CO-CH2- and Y A1 -CO-NH-CH2- is acceptable, and preferably -Y A1 In addition, in formula (2), Y B When is a urethane bond, -Y A1 -Y B -CH2- is -Y A1 -NH-CO-O-CH2- and Y A1 -O-CO-NH-CH2-, preferably -Y A1 -NH-CO-O-CH2-. In addition, -Y A1 -Y B - is -Y A1 -(Y A2 ) b -(Y A3 ) c -(Y A4 ) d -(Y A5 ) e -(Y A6 ) f It is preferred that the compound has the structure represented by the formula: (Y A1represents an unsubstituted alkylene group, Y A2 represents a methylene group substituted with at least one atom selected from the group consisting of a hydroxy group and a halogen atom, Y A3 represents an unsubstituted alkylene group, Y A4 represents an ester bond, an amide bond or a urethane bond, Y A5 represents an unsubstituted alkylene group, Y A6 represents an oxygen atom or a sulfur atom, b, c, d, e and f each independently represent 0 or 1.

[0028] It is preferable that the polymer A has, as structural units, only the structural unit represented by the formula (1) and the structural unit represented by the formula (2).

[0029] In the formula (2), [ka] is preferably not an acidic group having a pKa of 3 or less.

[0030] In the formula (2), [ka] is preferably not -SO3H.

[0031] In polymer A having a structural unit represented by formula (1) and a structural unit represented by formula (2), the molar ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) is preferably 1:19 to 1:1, and more preferably 1:4 to 9:11.

[0032] Examples of the structural unit represented by the formula (2) include those having the structures shown in Table 2 below. [Table 1-1] [Table 1-2]

[0033] <Electrophotographic photoreceptor> An example of the layer structure of the electrophotographic photoreceptor of the present disclosure is shown in Figure 1. In Figure 1, an undercoat layer 102, a charge generation layer 103, a charge transport layer 104, and a surface layer 105 are laminated on a support 101. The photosensitive layer may be a laminated type photosensitive layer having a charge generation layer and a charge transport layer, or may be a single-layer type photosensitive layer containing a charge generation material and a charge transport material. The surface layer of the electrophotographic photoreceptor of the present disclosure contains fluorine atom-containing resin particles, a binder material, and a polymer A having a structural unit represented by the above formula (1). The method for manufacturing the electrophotographic photoreceptor of the present disclosure includes a method of preparing the coating liquid for each layer described later, coating the desired layers in order, and drying the coating liquid. In this case, the coating liquid can be applied by dip coating, spray coating, inkjet coating, roll coating, die coating, blade coating, curtain coating, wire bar coating, ring coating, etc. Among these, dip coating is preferred from the viewpoint of efficiency and productivity. The configuration of the electrophotographic photoreceptor of the present disclosure will be described below.

[0034] <Support> The support of the electrophotographic photoreceptor is preferably conductive (conductive support). The shape of the support may be cylindrical, belt-like, or sheet-like. Of these, a cylindrical support is preferable. The surface of the support may be subjected to electrochemical treatment such as anodization, blasting, cutting, or the like. The support is preferably made of a metal, a resin, or a glass. Examples of the metal include aluminum, iron, nickel, copper, gold, stainless steel, and alloys thereof. Among these, an aluminum support using aluminum is preferred. In addition, it is preferable to impart electrical conductivity to the resin or glass by a process such as mixing with or coating with an electrically conductive material.

[0035] <Conductive layer> A conductive layer may be provided on the support. By providing the conductive layer, scratches and irregularities on the surface of the support can be concealed and light reflection on the surface of the support can be controlled. The conductive layer preferably contains conductive particles and a resin. The conductive particles may be made of a material such as metal oxide, metal, or carbon black. Examples of metal oxides include zinc oxide, aluminum oxide, indium oxide, silicon oxide, zirconium oxide, tin oxide, titanium oxide, strontium titanate, magnesium oxide, antimony oxide, bismuth oxide, etc. Examples of metals include aluminum, nickel, iron, nichrome, copper, zinc, silver, etc. Among these, it is preferable to use metal oxide particles as the conductive particles, and it is particularly preferable to use titanium oxide particles, tin oxide particles, or zinc oxide particles. When metal oxide particles are used as the conductive particles, the surfaces of the metal oxide particles may be treated with a silane coupling agent or the like, or the metal oxide particles may be doped with an element such as phosphorus or aluminum or an oxide thereof. The conductive particles may have a laminated structure having a core particle and a coating layer that covers the core particle. Examples of the core particle include titanium oxide particles, barium sulfate particles, zinc oxide particles, etc. Examples of the coating layer include metal oxide particles such as tin oxide. Furthermore, when metal oxide particles are used as the conductive particles, the volume average particle size thereof is preferably 1 nm or more and 500 nm or less, and more preferably 3 nm or more and 400 nm or less. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, and alkyd resin. The conductive layer may further contain silicone oil, resin particles, a masking agent such as titanium oxide, and the like.

[0036] The conductive layer can be formed by preparing a conductive layer coating solution containing the above-mentioned materials and solvent, forming this coating film on a support, and drying it. Examples of the solvent used in the conductive layer coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Examples of the dispersion method for dispersing the conductive particles in the conductive layer coating solution include a method using a paint shaker, a sand mill, a ball mill, and a liquid collision type high-speed disperser. The thickness of the conductive layer is preferably from 1 μm to 50 μm, and particularly preferably from 3 μm to 40 μm.

[0037] <Undercoat layer> In the present disclosure, an undercoat layer may be provided on the support or the conductive layer. By providing an undercoat layer, the adhesion function between layers can be improved and a charge injection blocking function can be imparted. The undercoat layer preferably contains a resin. Alternatively, the undercoat layer may be formed as a cured film by polymerizing a composition containing a monomer having a polymerizable functional group. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, acrylic resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl phenol resin, alkyd resin, polyvinyl alcohol resin, polyethylene oxide resin, polypropylene oxide resin, polyamide resin, polyamic acid resin, polyimide resin, polyamideimide resin, and cellulose resin. Examples of the polymerizable functional group contained in the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylated methylol group, an epoxy group, a metal alkoxide group, a hydroxy group, an amino group, a carboxy group, a thiol group, a carboxylic anhydride group, and a carbon-carbon double bond group.

[0038] For the purpose of improving electrical properties, the undercoat layer may further contain an electron transport material, metal oxide particles, metal particles, a conductive polymer, etc. Among these, it is preferable to use an electron transport material and metal oxide particles. Examples of the electron transport substance include a quinone compound, an imide compound, a benzimidazole compound, a cyclopentadienylidene compound, a fluorenone compound, a xanthone compound, a benzophenone compound, a cyanovinyl compound, an aryl halide compound, a silole compound, a boron-containing compound, etc. An electron transport substance having a polymerizable functional group may be used as the electron transport substance, and the undercoat layer may be formed as a cured film by copolymerizing the electron transport substance with the monomer having the polymerizable functional group described above. Metal oxide particles include particles of indium tin oxide, tin oxide, indium oxide, titanium oxide, strontium titanate, zinc oxide, aluminum oxide, etc. Silicon dioxide particles can also be used. Metal particles include particles of gold, silver, aluminum, etc.

[0039] The metal oxide particles contained in the undercoat layer may be surface-treated with a surface treatment agent such as a silane coupling agent. The surface treatment of the metal oxide particles can be carried out by a common method, such as a dry method or a wet method. In the dry method, metal oxide particles are stirred in a mixer capable of high-speed stirring, such as a Henschel mixer, while an alcohol aqueous solution, an organic solvent solution, or an aqueous solution containing a surface treatment agent is added to the metal oxide particles to uniformly disperse them, and then the particles are dried. In the wet method, the metal oxide particles and the surface treatment agent are stirred in a solvent or dispersed in a sand mill using glass beads or the like, and the solvent is removed by filtration or distillation under reduced pressure. After the solvent is removed, it is preferable to further bake the mixture at 100° C. or higher.

[0040] The undercoat layer may further contain additives, for example, known materials such as metal particles such as aluminum particles, conductive material particles such as carbon black, charge transport materials, metal chelate compounds, and organometallic compounds. The undercoat layer can be formed by preparing a coating solution for the undercoat layer containing the above-mentioned materials and solvent, forming a coating film of this on a support or a conductive layer, and drying and / or curing it. Examples of the solvent used in the coating liquid for the undercoat layer include organic solvents such as alcohols, sulfoxides, ketones, ethers, esters, halogenated aliphatic hydrocarbons, aromatic compounds, etc. In the present disclosure, it is preferable to use an alcohol-based or ketone-based solvent. Examples of a dispersion method for preparing a coating solution for the undercoat layer include methods using a homogenizer, an ultrasonic disperser, a ball mill, a sand mill, a roll mill, a vibration mill, an attritor, and a liquid collision type high-speed disperser. The thickness of the undercoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, and particularly preferably 0.3 μm or more. The thickness of the undercoat layer is preferably 50 μm or less, more preferably 40 μm or less, more preferably 30 μm or less, more preferably 10 μm or less, and particularly preferably 5 μm or less.

[0041] <Photosensitive layer> The photosensitive layer of an electrophotographic photoreceptor is mainly classified into (1) a laminated type photosensitive layer and (2) a single-layer type photosensitive layer. (1) The laminated type photosensitive layer is a photosensitive layer having a charge generation layer containing a charge generation material and a charge transport layer containing a charge transport material. (2) The single-layer type photosensitive layer is a photosensitive layer containing both a charge generation material and a charge transport material.

[0042] (1) Laminated photosensitive layer The laminated type photosensitive layer has a charge generating layer and a charge transport layer.

[0043] (1-1) Charge generation layer The charge generating layer preferably contains a charge generating material and a resin. Examples of the charge generating material include azo pigments, perylene pigments, polycyclic quinone pigments, indigo pigments, and phthalocyanine pigments. Among these, azo pigments and phthalocyanine pigments are preferred. Among phthalocyanine pigments, oxytitanium phthalocyanine pigments, chlorogallium phthalocyanine pigments, and hydroxygallium phthalocyanine pigments are preferred. The content of the charge generating material in the charge generating layer is preferably from 40% by mass to 85% by mass, and more preferably from 60% by mass to 80% by mass, based on the total mass of the charge generating layer. Examples of the resin include polyester resin, polycarbonate resin, polyvinyl acetal resin, polyvinyl butyral resin, acrylic resin, silicone resin, epoxy resin, melamine resin, polyurethane resin, phenol resin, polyvinyl alcohol resin, cellulose resin, polystyrene resin, polyvinyl acetate resin, polyvinyl chloride resin, etc. Among these, polyvinyl butyral resin is more preferable. The charge generating layer may further contain additives such as an antioxidant and an ultraviolet absorbing agent, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, and benzophenone compounds. The charge generating layer can be formed by preparing a coating solution for the charge generating layer containing the above-mentioned materials and solvent, forming a coating film of this on the undercoat layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, sulfoxide-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. The thickness of the charge generating layer is preferably from 0.1 μm to 1 μm, and more preferably from 0.15 μm to 0.4 μm.

[0044] (1-2) Charge transport layer The charge transport layer preferably contains a charge transport material and a binder material. When a protective layer described later is not provided, the charge transport layer becomes the surface layer of the electrophotographic photoreceptor. In this case, the charge transport layer contains fluorine atom-containing resin particles, a binder material, and a polymer A having a structural unit represented by the above formula (1). Examples of the charge transport material include polycyclic aromatic compounds, heterocyclic compounds, hydrazone compounds, styryl compounds, enamine compounds, triarylamine compounds, resins having groups derived from these materials, etc. Among these, triarylamine compounds are preferred. The content of the charge transport material in the charge transport layer is preferably from 25% by weight to 70% by weight, and more preferably from 30% by weight to 55% by weight, based on the total weight of the charge transport layer. As the binding material, a thermoplastic resin (hereinafter, also referred to as "resin") is used. Examples of the thermoplastic resin include polyester resin, polycarbonate resin, acrylic resin, polystyrene resin, etc. Among these, polycarbonate resin and polyester resin are preferable. As the polyester resin, polyarylate resin is particularly preferable. The content ratio (mass ratio) of the charge transport material to the resin is preferably from 4:10 to 20:10, and more preferably from 5:10 to 12:10. The content of the fluorine-containing resin particles in the charge transport layer is preferably 5% by weight to 20% by weight, and more preferably 7% by weight to 10% by weight.

[0045] The charge transport layer may also contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, etc. Specific examples of such additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, silicone oils, polystyrene resin particles, polyethylene resin particles, and boron nitride particles. The charge transport layer can be formed by preparing a coating solution for the charge transport layer containing the above-mentioned materials and solvent, forming the coating film on the charge generating layer, and drying it. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. Among these solvents, ether-based solvents or aromatic hydrocarbon-based solvents are preferred. The thickness of the charge transport layer is preferably from 5 μm to 50 μm, more preferably from 8 μm to 40 μm, and particularly preferably from 10 μm to 30 μm.

[0046] (2) Single-layer photosensitive layer The single-layer type photosensitive layer can be formed by preparing a coating solution for the photosensitive layer containing a charge generating material, a charge transporting material, a resin and a solvent, forming a coating film of this on the undercoat layer, and drying it. The charge generating material, the charge transporting material and the resin are the same as the examples of materials in "(1) Multi-layer type photosensitive layer" above.

[0047] <Protective layer> In the present disclosure, a protective layer may be provided on the photosensitive layer. By providing a protective layer, durability can be improved. When a protective layer is provided, the protective layer becomes the surface layer of the electrophotographic photoreceptor. In this case, the protective layer contains fluorine atom-containing resin particles, a binder material, and a polymer A having a structural unit represented by the above formula (1). The protective layer may be formed as a cured film by polymerizing a composition containing, for example, a monomer having a polymerizable functional group, which is a raw material of the binding material. Examples of the reaction include thermal polymerization reaction, photopolymerization reaction, and radiation polymerization reaction. Examples of the polymerizable functional group of the monomer having a polymerizable functional group include an isocyanate group, a blocked isocyanate group, a methylol group, an alkylmethylol group, an epoxy group, a metal alkoxyl group, a hydroxyl group, an amino group, a carboxyl group, a thiol group, a carboxylic anhydride group, and a group containing a carbon-carbon double bond. Examples of the group containing a carbon-carbon double bond include an acryloyl group and a methacryloyl group. A monomer having a charge transporting ability may be used as the monomer having a polymerizable functional group. Here, the cured product of the monomer having a polymerizable functional group is the binder material of the protective layer. As the monomer having a polymerizable functional group, it is preferable to use a hole transporting compound having a chain polymerizable functional group.

[0048] The hole transporting compound having a chain polymerizable functional group is more preferably a compound represented by the following formula (CT-1) or (CT-2). [ka] (In the above formula (CT-1), Ar 11 ~Ar 13 are each independently a substituted aryl group or an unsubstituted aryl group. The substituent that the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by any one of the following formulas (P-1) to (P-3). However, the compound represented by the formula (CT-1) has at least one monovalent functional group represented by any one of the following formulas (P-1) to (P-3). [ka] (In the formula (CT-2), Ar 21 ~Ar 24 are each independently a substituted aryl group or an unsubstituted aryl group; Ar 25is a substituted arylene group or an unsubstituted arylene group. The substituent that the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3). The substituent that the substituted arylene group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3). However, the compound represented by formula (CT-2) has at least one monovalent functional group represented by any of the following formulas (P-1) to (P-3). [ka] (In the formula (P-1), Z 11 is a single bond or an alkylene group having 1 to 6 carbon atoms; X 11 is a hydrogen atom or a methyl group. [ka] (In the formula (P-2), Z 21 is a single bond or an alkylene group having 1 to 6 carbon atoms. [ka] (In the formula (P-3), Z 31 is a single bond or an alkylene group having 1 to 6 carbon atoms. The content of the fluorine-containing resin particles in the protective layer is preferably 20% by mass or more and 40% by mass or less, based on the total mass of the protective layer, and more preferably 25% by mass or more and 35% by mass or less.

[0049] The protective layer preferably contains a compound represented by the following formula (3): In addition, in preparing a coating liquid for the surface layer, the compound represented by the following formula (3) is preferably a liquid compound from the viewpoint of use as a dispersion medium. [ka] In the formula (3), R 31R is an alkyl group or a fluoroalkyl group. 32 is a fluoroalkyl group. 31 is preferably a fluoroalkyl group.

[0050] Examples of the compound represented by the formula (3) include methyl nonafluorobutyl ether, ethyl nonafluorobutyl ether, 1,1,1,2,3,4,4,5,5,5-decafluoro-3-methoxy-2-(trifluoromethyl)pentane 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether, etc. Among them, 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether is preferred from the viewpoints of improving dispersibility and suppressing potential fluctuation.

[0051] In terms of suppressing potential fluctuation, the content of the compound represented by the formula (3) in the protective layer is preferably from 1 ppm to 10 ppm. The method for measuring the content of the compound represented by the formula (3) in the protective layer includes, for example, a method using GCMS analysis. The surface layer on the electrophotographic photoreceptor is scraped off with a razor or the like to obtain a film mass as a measurement sample. The measurement sample is analyzed by GCMS to measure the content of the compound represented by the formula (3) contained in the surface layer. As an apparatus for GCMS analysis, for example, GCMS-QP2000 (manufactured by Shimadzu Corporation) can be used. In the examples of the present disclosure, after obtaining a measurement sample by the above-mentioned method, the content of the compound represented by the formula (3) was measured using the above-mentioned GCMS apparatus.

[0052] The protective layer may contain additives such as antioxidants, ultraviolet absorbers, plasticizers, leveling agents, etc. Specific examples of additives include hindered phenol compounds, hindered amine compounds, sulfur compounds, phosphorus compounds, benzophenone compounds, siloxane-modified resins, and silicone oils. The protective layer can be formed by preparing a coating solution for the protective layer containing the above-mentioned materials and solvent, forming the coating film on the photosensitive layer, and drying and / or curing the coating film. Examples of the solvent used in the coating solution include alcohol-based solvents, ketone-based solvents, ether-based solvents, sulfoxide-based solvents, ester-based solvents, and aromatic hydrocarbon-based solvents. The thickness of the protective layer is preferably 0.50 μm or more and 10 μm or less, and more preferably 1 μm or more and 7 μm or less.

[0053] <Surface treatment of electrophotographic photoreceptor> In the present disclosure, the surface of the electrophotographic photoreceptor may be processed. By performing the surface processing, the behavior of the cleaning means (cleaning blade) that is brought into contact with the electrophotographic photoreceptor can be more stabilized. Examples of the surface processing method include a method of pressing a mold having a convex portion against the surface of the electrophotographic photoreceptor to transfer the shape, a method of imparting a convex and concave shape by mechanical polishing, or a method of colliding a powder with the surface of the electrophotographic photoreceptor to roughen the surface. In this way, by providing concave or convex portions on the surface layer of the electrophotographic photoreceptor, the behavior of the cleaning means that is brought into contact with the electrophotographic photoreceptor can be more stabilized. The recesses or protrusions may be formed over the entire surface of the electrophotographic photoreceptor, or may be formed on a portion of the surface of the electrophotographic photoreceptor. When the recesses or protrusions are formed on a portion of the surface of the electrophotographic photoreceptor, it is preferable that the recesses or protrusions are formed over at least the entire contact area with the cleaning means (cleaning blade). When forming recesses, a mold having protrusions corresponding to the recesses is pressed against the surface of the electrophotographic photosensitive member to transfer the shape, thereby forming the recesses on the surface of the electrophotographic photosensitive member.

[0054] <Polishing tools used for mechanical polishing> A known means can be used for mechanical polishing. In general, an abrasive tool is brought into contact with an electrophotographic photoreceptor, and one or both of them are moved relatively to polish the surface of the electrophotographic photoreceptor. The abrasive tool is a polishing member having a base material and a layer in which abrasive grains are dispersed in a binder resin. Examples of the abrasive grains include particles of aluminum oxide, chromium oxide, diamond, iron oxide, cerium oxide, corundum, silica stone, silicon nitride, boron nitride, molybdenum carbide, silicon carbide, tungsten carbide, titanium carbide, and silicon oxide. The particle size of the abrasive grains is preferably 0.01 to 50 μm, and more preferably 1 to 15 μm. If the particle size of the abrasive grains is too small, the polishing power becomes weak, and it becomes difficult to increase the F / C ratio of the outermost surface of the electrophotographic photoreceptor. These abrasive grains can be used alone or in combination of two or more types. When two or more types are mixed, the materials and particle sizes may be different or the same. The binder resin for dispersing the abrasive grains used in the polishing tool may be a known thermoplastic resin, thermosetting resin, reactive resin, electron beam curing resin, ultraviolet curing resin, visible light curing resin, or antifungal resin. Examples of the thermoplastic resin include vinyl chloride resin, polyamide resin, polyester resin, polycarbonate resin, amino resin, styrene-butadiene copolymer, urethane elastomer, and polyamide-silicone resin. Examples of the thermosetting resin include phenol resin, phenoxy resin, epoxy resin, polyurethane resin, polyester resin, silicone resin, melamine resin, and alkyd resin. An isocyanate-based curing agent may also be added to the thermoplastic resin. The thickness of the layer of the polishing tool, in which the abrasive grains are dispersed in the binder resin, is preferably 1 μm or more and 100 μm or less. If the layer is too thick, the layer is likely to have uneven thickness, which results in uneven surface roughness of the polished object. On the other hand, if the layer is too thin, the abrasive grains are likely to fall off. The shape of the substrate of the abrasive tool is not particularly limited. In the examples of the present disclosure, a sheet-shaped substrate is used to efficiently abrade a cylindrical electrophotographic photoreceptor, but other shapes may be used. (Hereinafter, the abrasive tool of the present disclosure will also be referred to as an abrasive sheet.) The material of the substrate of the abrasive tool is also not particularly limited. For example, the material of the sheet-shaped substrate may be paper, woven fabric, nonwoven fabric, or plastic film. The abrasive tool can be obtained by coating a base material with a coating material in which the above-mentioned abrasive grains, binder resin, and a solvent capable of dissolving the binder resin are mixed and dispersed, followed by drying.

[0055] <Polishing equipment> FIG. 2 shows an example of a polishing device for an electrophotographic photoreceptor according to the present disclosure. FIG. 2 shows an apparatus for polishing a cylindrical electrophotographic photoreceptor using an abrasive sheet. In FIG. 2, the abrasive sheet 2-1 is wound around a hollow shaft 2-6, and a motor (not shown) is arranged to apply tension to the abrasive sheet 2-1 in the direction opposite to the direction in which the abrasive sheet 2-1 is fed around the shaft 2-6. The abrasive sheet 2-1 is fed in the direction of the arrow, passes through guide rollers 2-2a and 2-2b and a backup roller 2-3, and the abrasive sheet 2-1 after polishing is taken up by a motor (not shown) around a take-up means 2-5 via guide rollers 2-2c and 2-2d. Polishing is performed by constantly pressing the abrasive sheet 2-1 against the object to be treated (electrophotographic photoreceptor before polishing) 2-4. Since the abrasive sheet 2-1 is often insulating, it is preferable to use an earthed or conductive material for the part in contact with the abrasive sheet 2-1. The feed speed of the polishing sheet 2-1 is preferably in the range of 10 to 1000 mm / min. If the feed rate is too low, the binder resin may adhere to the surface of the polishing sheet 2-1, which may cause deep scratches on the surface of the workpiece 2-4. The workpiece 2-4 is placed at a position facing the backup roller 2-3 via the polishing sheet 2-1. The backup roller 2-3 is preferably an elastic body from the viewpoint of improving the uniformity of the surface roughness of the workpiece 2-4. At this time, the workpiece 2-4 and the backup roller 2-3 are pressed against each other via the polishing sheet 2-1 at a desired set value for a predetermined time, and the surface of the workpiece 2-4 is polished. The rotation direction of the workpiece 2-4 may be the same as or opposite to the direction in which the polishing sheet 2-1 is fed. The rotation direction may also be changed during polishing. The pressure of the backup roller 2-3 against the workpiece 2-4 is 0.005 to 15 N / m, depending on the hardness of the backup roller 2-3 and the polishing time. 2 is preferred. The surface roughness of the electrophotographic photoreceptor can be adjusted by appropriately selecting the feed speed of the polishing sheet 2-1, the pressing pressure of the backup roller 2-3, the abrasive grain type of the polishing sheet, the film thickness of the binder resin of the polishing sheet, the thickness of the substrate, etc.

[0056] <Measurement of the maximum height Rmax in JIS B0601 1982> The surface roughness of the electrophotographic photoreceptor can be measured by known means. For example, the following can be mentioned. Surface roughness meters such as the Surf Coater SE3500 type surface roughness measuring instrument manufactured by Kosaka Laboratory Ltd. A non-contact three-dimensional surface measuring machine, Micro Map 557N, manufactured by Hishikawa System Co., Ltd. Microscopes capable of acquiring three-dimensional shapes, such as the ultra-depth shape measuring microscopes VK-8550 and VK-9000 manufactured by Keyence Corporation. In the present disclosure, among the indices of surface roughness, the maximum height Rmax in JIS B0601 1982 defined by the Japanese Industrial Standard JIS is used as the polishing depth L (μm). Also, in the present disclosure, for the range of the 5 mm square section of the electrophotographic photoreceptor cut out as a specimen for X-ray photoelectron spectroscopy described later, Rmax is measured in advance. The measurement is performed arbitrarily at three locations in the 5 mm square range, and the average value is adopted as the polishing depth L (μm).

[0057] <Process cartridge, electrophotographic apparatus> The electrophotographic photoreceptor of the present disclosure may be one of the components of a process cartridge or an electrophotographic apparatus. The process cartridge integrally supports at least one means selected from the group consisting of the electrophotographic photoreceptor described so far, a charging means, a developing means, a transfer means, and a cleaning means, and is detachable from the electrophotographic apparatus main body. Further, the electrophotographic apparatus is characterized by having the electrophotographic photoreceptor, a charging means, an exposure means, a developing means, and a transfer means described so far.

[0058] FIG. 3 shows an example of the schematic configuration of an electrophotographic apparatus having a process cartridge equipped with an electrophotographic photoreceptor. A cylindrical (drum-shaped) electrophotographic photoreceptor 201 is driven to rotate around an axis 202 in the direction of an arrow at a predetermined peripheral speed (process speed). The surface of the electrophotographic photoreceptor 201 is charged to a predetermined positive or negative potential by a charging means 203 during the rotation process. Note that, although a roller charging method using a roller-type charging member is shown in FIG. 3, a charging method such as a corona charging method, a proximity charging method, or an injection charging method may be adopted. Exposure light 204 is irradiated from an exposure means (not shown) onto the charged surface of the electrophotographic photoreceptor 201, and an electrostatic latent image corresponding to the target image information is formed. The exposure light 204 is light whose intensity is modulated in response to a time-series electric digital image signal of the target image information, and is output from an image exposure means such as a slit exposure or a laser beam scanning exposure. The electrostatic latent image formed on the surface of the electrophotographic photoreceptor 201 is developed (normal development or reversal development) with toner on a developing member 213 contained in a developing means 205, and a toner image is formed on the surface of the electrophotographic photoreceptor 201. The toner image formed on the surface of the electrophotographic photoreceptor 201 is transferred to a transfer material 207 by a transfer means 206. At this time, a bias voltage of a polarity opposite to the charge held by the toner is applied to the transfer means 206 from a bias power source (not shown). When the transfer material 207 is paper, the transfer material 207 is taken out from a paper feed section (not shown) and fed between the electrophotographic photoreceptor 201 and the transfer means 206 in synchronization with the rotation of the electrophotographic photoreceptor 201. The transfer material 207 onto which the toner image has been transferred from the electrophotographic photoreceptor 201 is separated from the surface of the electrophotographic photoreceptor 201 and conveyed to a fixing means 208, where the toner image is fixed, and the image is printed out as an image formed product (print, copy) outside the electrophotographic device. The electrophotographic device may have a cleaning means 209 for removing deposits such as toner remaining on the surface of the electrophotographic photoreceptor 201 after transfer. Also, a so-called cleanerless system may be used in which the above-mentioned deposits are removed by the developing means or the like without providing a separate cleaning means. A process cartridge can be formed by housing a plurality of components selected from the above-mentioned electrophotographic photosensitive member 201, charging means 203, developing means 205, cleaning means 209, etc. in a container and supporting them integrally. In addition, the process cartridge can be configured to be detachable from the main body of the electrophotographic apparatus.For example, it may be configured as follows. At least one selected from the charging means 203, the developing means 205, and the cleaning means 209 is integrally supported together with the electrophotographic photosensitive member 201 to form a cartridge. This can be made into a process cartridge 211 that can be detachably attached to the main body of the electrophotographic device using a guide means 212 such as a rail of the main body of the electrophotographic device. The electrophotographic device may have a charge removing mechanism that performs charge removal processing on the surface of the electrophotographic photosensitive member 201 with pre-exposure light 210 from a pre-exposure means (not shown). Also, a guide means 212 such as a rail may be provided to attach and detach the process cartridge 11 to the main body of the electrophotographic device. The electrophotographic device of the present disclosure is characterized by having the electrophotographic photosensitive member 201, the charging means 203, the exposure means, the developing means 205, and the transfer means 206.

[0059] FIG. 4 shows the configuration of a process cartridge equipped with the electrophotographic photosensitive member of the present disclosure, and FIG. 5 shows an example of a schematic configuration of an electrophotographic apparatus having the process cartridge of FIG. In FIG. 4, a cylindrical electrophotographic photoreceptor 1 is rotated in the direction of the arrow at a predetermined peripheral speed. The peripheral surface of the rotated electrophotographic photoreceptor 1 is uniformly charged to a predetermined positive or negative potential by charging means 2. Next, the charged peripheral surface of the electrophotographic photoreceptor 1 is subjected to exposure light (image exposure light) 3 output from exposure means (not shown) such as slit exposure or laser beam scanning exposure. In this way, an electrostatic latent image corresponding to a target image is formed sequentially on the peripheral surface of the electrophotographic photoreceptor 1. The voltage applied to the charging means (such as a charging roller) 2 may be either a voltage in which an AC component is superimposed on a DC component, or a voltage consisting of only a DC component. The electrostatic latent image formed on the peripheral surface of the electrophotographic photoreceptor 1 is developed into a toner image by the toner contained in the developer of the developing means 4. Next, the toner images formed and carried on the peripheral surface of the electrophotographic photoreceptor 1 are sequentially transferred to a transfer material (paper, intermediate transfer body, etc.) 6 by a transfer bias from a transfer means (transfer roller, etc.) 5. The transfer material 6 is fed in synchronization with the rotation of the electrophotographic photoreceptor 1. The surface of the electrophotographic photoreceptor 1 after the toner image transfer is subjected to a charge removal process using pre-exposure light 7 from a pre-exposure means (not shown), and then the surface is cleaned by removing the residual toner from the electrophotographic photoreceptor 1 by a cleaning means 8, and the electrophotographic photoreceptor 1 is repeatedly used for image formation. The pre-exposure means may be placed before or after the cleaning step, and the pre-exposure means is not necessarily required. The electrophotographic photoreceptor 1 may be mounted in an electrophotographic apparatus such as a copying machine or a laser beam printer. In addition, a process cartridge 9 configured by housing a plurality of components such as the electrophotographic photoreceptor 1, the charging means 2, the developing means 4, and the cleaning means 8 in a container and supporting them integrally may be configured to be detachably attached to the main body of the electrophotographic apparatus. In FIG. 4, the electrophotographic photoreceptor 1, the charging means 2, the developing means 4, and the cleaning means 8 are supported integrally to form a process cartridge 9 that is detachably attached to the main body of the electrophotographic apparatus.

[0060] Next, an electrophotographic apparatus equipped with the electrophotographic photoreceptor of the present disclosure will be described. An example of the configuration of the electrophotographic apparatus of the present disclosure is shown in Fig. 5. A yellow process cartridge 17, a magenta process cartridge 18, a cyan process cartridge 19, and a black process cartridge 20 corresponding to the respective colors of yellow, magenta, cyan, and black are arranged side by side along the intermediate transfer body 10. The diameter, constituent materials, developer, charging method, and other means of the electrophotographic photosensitive member do not necessarily need to be uniform for each color. When the image formation operation starts, toner images of each color are sequentially superimposed on the intermediate transfer body 10 according to the image formation process described above. In parallel, transfer paper 11 is sent out from paper feed tray 13 by paper feed path 12 and fed to secondary transfer means 14 in synchronization with the rotation of the intermediate transfer body. The toner image on the intermediate transfer body 10 is transferred to the transfer paper 11 by a transfer bias from secondary transfer means 14. The toner image transferred onto the transfer paper 11 is transported along the paper feed path 12, fixed on the transfer paper by fixing means 15, and discharged from paper discharge section 16. The electrophotographic photoreceptor of the present disclosure can be used in laser beam printers, LED printers, copiers, facsimiles, and multifunction machines thereof. EXAMPLES

[0061] The present disclosure will be described in more detail below using examples and comparative examples, but is not limited thereto. In the following description of the examples, "parts" are by mass unless otherwise specified.

[0062] <Synthesis of polymer A having a structural unit represented by formula (1)> Polymer A (hereinafter also referred to as "graft copolymer") having a structural unit represented by the formula (1) in the present disclosure was synthesized as follows. The (meth)acrylate compound and macromonomer compound used in the synthesis examples below can be produced by referring to, for example, JP-A-2009-104145.

[0063] (Graft copolymer 1) 48.2 parts by mass of 1H,1H-heptadecafluoro(2,5-dimethyl-3,6-dioxanonan-1-ol) (manufactured by Apollo Scientific), 15.5 parts by mass of 2-isocyanatoethyl methacrylate (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.012 parts by mass of hydroquinone monomethyl ether (manufactured by Tokyo Chemical Industry Co., Ltd.), 0.3 parts by mass of zirconium(IV) acetylacetonate (manufactured by Sigma-Aldrich), and 100 parts by mass of n-butyl acetate were mixed in a glass flask equipped with a stirrer, reflux condenser, nitrogen gas inlet tube, thermostatic bath, and thermometer at 20°C under a nitrogen atmosphere for 30 minutes, and then heated to 50°C and reacted for 24 hours to obtain a perfluoro structure-containing monomer represented by the following formula (M-1). [ka] 6.37 parts of the obtained perfluoro structure-containing monomer, 180 parts of a macromonomer (number average molecular weight 6,000) represented by the following formula (A), 0.473 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) (trade name: OTAZO-15, manufactured by Otsuka Chemical Co., Ltd.), and 338 parts of n-butyl acetate were mixed in a glass flask equipped with a stirrer, a reflux condenser, a nitrogen gas inlet tube, a thermostatic bath, and a thermometer at 20 ° C. under a nitrogen atmosphere for 30 minutes, and then the reaction liquid was heated to 85 to 90 ° C. and reacted for 5 hours. The reaction was stopped by cooling with ice, and 1500 parts of 2-propanol were added to obtain a precipitate. The precipitate was washed with a mixed solvent of n-butyl acetate: 2-propanol = 1:5, and dried at a temperature of 80 ° C. and a reduced pressure of 1325 Pa or less for 3 hours to obtain a graft copolymer 1. The resulting graft copolymer 1 was subjected to GPC measurement by the above-mentioned method, and the weight average molecular weight was calculated to be 150,000. [ka]

[0064] (Graft copolymer 2) Graft copolymer 2 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was replaced with 5.21 parts of the perfluoro structure-containing monomer represented by formula (M-2): The weight average molecular weight of the obtained graft copolymer 2 was calculated to be 150,000. [ka]

[0065] (Graft copolymer 3) Graft copolymer 3 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was replaced with 6.87 parts of the perfluoro structure-containing monomer represented by formula (M-3) below. The weight average molecular weight of the obtained graft copolymer 3 was calculated to be 150,000. [ka]

[0066] (Graft Copolymer 4) Graft copolymer 4 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was replaced with 4.05 parts of the perfluoro structure-containing monomer represented by formula (M-4) below. The weight average molecular weight of the obtained graft copolymer 4 was calculated to be 150,000. [ka]

[0067] (Graft Copolymer 5) Graft copolymer 5 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was replaced with 7.87 parts of the perfluoro structure-containing monomer represented by formula (M-5) below. The weight average molecular weight of the obtained graft copolymer 5 was calculated to be 150,000. [ka]

[0068] (Graft Copolymer 6) Graft copolymer 6 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 1.02 parts and the macromonomer represented by formula (A) was changed to 230 parts. The weight average molecular weight of the obtained graft copolymer 6 was calculated to be 150,000.

[0069] (Graft Copolymer 7) Graft copolymer 7 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 1.27 parts and the macromonomer represented by formula (A) was changed to 228 parts. The weight average molecular weight of the obtained graft copolymer 7 was calculated to be 150,000.

[0070] (Graft Copolymer 8) Graft copolymer 8 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 5.10 parts and the macromonomer represented by formula (A) was changed to 192 parts. The weight average molecular weight of the obtained graft copolymer 8 was calculated to be 150,000.

[0071] (Graft Copolymer 9) Graft copolymer 9 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 11.47 parts and the macromonomer represented by formula (A) was changed to 132 parts. The weight average molecular weight of the obtained graft copolymer 9 was calculated to be 150,000.

[0072] (Graft Copolymer 10) Graft copolymer 10 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 12.75 parts and the macromonomer represented by formula (A) was changed to 120 parts. The weight average molecular weight of the obtained graft copolymer 10 was calculated to be 150,000.

[0073] (Graft Copolymer 11) Graft copolymer 11 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 14.02 parts and the macromonomer represented by formula (A) was changed to 108 parts. The weight average molecular weight of the obtained graft copolymer 11 was calculated to be 150,000.

[0074] (Graft Copolymer 12) Graft copolymer 12 was obtained in the same manner as graft copolymer 1, except that 4.725 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) was used. The weight average molecular weight of the obtained graft copolymer 12 was calculated to be 15,000.

[0075] (Graft Copolymer 13) Graft copolymer 13 was obtained in the same manner as graft copolymer 1, except that 2.363 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) was used. The weight average molecular weight of the obtained graft copolymer 13 was calculated to be 30,000.

[0076] (Graft Copolymer 14) Graft copolymer 14 was obtained in the same manner as graft copolymer 1, except that 0.709 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) was used. The weight average molecular weight of the obtained graft copolymer 14 was calculated to be 100,000.

[0077] (Graft Copolymer 15) Graft copolymer 15 was obtained in the same manner as for graft copolymer 1, except that 0.394 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) was used. The weight average molecular weight of the obtained graft copolymer 15 was calculated to be 180,000.

[0078] (Graft Copolymer 16) Graft copolymer 16 was obtained in the same manner as for graft copolymer 1, except that 0.322 parts of 1,1'-azobis(1-acetoxy-1-phenylethane) was used. The weight average molecular weight of the obtained graft copolymer 16 was calculated to be 220,000.

[0079] (Graft Copolymer 17) Graft copolymer 17 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was replaced with 5.48 parts of the perfluoro structure-containing monomer represented by formula (M-6) below. The weight average molecular weight of the obtained graft copolymer 17 was calculated to be 150,000. [ka]

[0080] (Graft Copolymer 18) Graft copolymer 18 was obtained in the same manner as graft copolymer 1, except that the perfluoro structure-containing monomer represented by formula (M-1) was changed to 9.14 parts of the perfluoro structure-containing monomer represented by formula (M-7) below. The weight average molecular weight of the obtained graft copolymer 18 was calculated to be 150,000. [ka]

[0081] <Preparation of Electrophotographic Photoreceptor> Example 1-1 (Support 1) A cylindrical aluminum cylinder (JIS-A3003, aluminum alloy, outer diameter 30.6 mm, length 370 mm, thickness 1 mm) was used as a support (conductive support). It was ultrasonically cleaned in a cleaning solution of pure water containing detergent (product name: Chemicol CT, Tokiwa Chemical Co., Ltd.), and then the cleaning solution was washed away. It was further ultrasonically cleaned in pure water and degreased, and this was used as support 1.

[0082] (Undercoat layer 1) Zinc oxide particles (specific surface area: 19 m 2 / g, powder resistance: 4.7×10 6 100 parts of the solubility in water (Ω·cm) was stirred and mixed with 500 parts of toluene, to which 0.8 parts of a silane coupling agent (compound name: N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane, product name: KBM602, Shin-Etsu Chemical Co., Ltd.) was added and stirred for 6 hours. Thereafter, the toluene was distilled off under reduced pressure, and the mixture was dried by heating at 130°C for 6 hours to obtain surface-treated zinc oxide particles A. Next, 15 parts of butyral (product name: BM-1, manufactured by Sekisui Chemical Co., Ltd.) as a polyol and 15 parts of blocked isocyanate (product name: Duranate TPA-B80E, non-volatile content 80 mass%, manufactured by Asahi Kasei Chemicals Co., Ltd.) were dissolved in a mixed solvent of 73.5 parts of methyl ethyl ketone and 73.5 parts of 1-butanol. 80.8 parts of surface-treated zinc oxide particles A and 0.81 parts of 2,3,4-trihydroxybenzophenone (manufactured by Tokyo Chemical Industry Co., Ltd.) were added to this solution, and the mixture was dispersed in a sand mill device using glass beads with a diameter of 0.8 mm under an atmosphere of 23±3°C for 3 hours. After the dispersion treatment, 0.01 parts of silicone oil (product name: SH28PA, manufactured by Toray Dow Corning Co., Ltd. (formerly Toray Dow Corning Silicones Co., Ltd.)) and 5.6 parts of cross-linked polymethyl methacrylate (PMMA) particles (product name: Techpolymer SSX-103, manufactured by Sekisui Chemical Co., Ltd., average primary particle size: 3 μm) were added and stirred to prepare a coating solution for the undercoat layer. The obtained coating liquid for undercoat layer was dip-coated onto the support 1 to form a coating film, and the coating film was dried at 160° C. for 30 minutes to form an undercoat layer 1 having a thickness of 18 μm.

[0083] (Charge generation layer 1) Four parts of hydroxygallium phthalocyanine crystals (charge generating material) having strong peaks at Bragg angles 2θ±0.2° at 7.4° and 28.1° in CuKα characteristic X-ray diffraction, and 0.04 parts of a compound represented by the following formula (E) were added to a solution prepared by dissolving 2 parts of polyvinyl butyral (product name: S-LEC BX-1, manufactured by Sekisui Chemical Co., Ltd.) in 100 parts of cyclohexanone. The solution was then dispersed for 1 hour in an atmosphere of 23±3°C using a sand mill using glass beads with a diameter of 1 mm, and after the dispersion treatment, 100 parts of ethyl acetate was added to prepare a coating solution for a charge generating layer. This charge generating layer coating liquid was dip coated onto the undercoat layer 1, and the resulting coating was dried at 90° C. for 10 minutes to form a charge generating layer 1 having a thickness of 0.15 μm. [ka]

[0084] (Charge transport layer 1) A coating solution for a charge transport layer was prepared by dissolving 60 parts of a compound represented by the following formula (F), 30 parts of a compound represented by the following formula (G), 10 parts of a compound represented by the following formula (H), 100 parts of a bisphenol Z-type polycarbonate resin (product name: Iupilon Z400, manufactured by Mitsubishi Engineering Plastics Corporation), and 0.2 parts of a polycarbonate having a structural unit represented by the following formula (I) (viscosity average molecular weight Mv: 20,000) in a mixed solvent of 272 parts of o-xylene, 256 parts of methyl benzoate, and 272 parts of dimethoxymethane. This charge transport layer coating liquid was dip coated onto the charge generating layer 1 to form a coating film, and the resulting coating film was dried at 115° C. for 50 minutes to form a charge transport layer 1 having a thickness of 18 μm. [ka] [ka] [ka] [ka] (In formula (I), 0.95 and 0.05 are the molar ratios (copolymerization ratios) of the two structural units.)

[0085] (protective layer) 3 kg of commercially available polytetrafluoroethylene resin particles (average primary particle size 210 nm, average circularity 0.85) were placed in a stainless steel container with a width of 400 mm, depth of 400 mm, and height of 50 mm, and dried at 150°C for 3 hours in a high-temperature incubator (model: SPH-102, manufactured by Espec Corporation) to obtain polytetrafluoroethylene resin particles A. A dispersant solution was prepared by dissolving 2.20 parts of the above-mentioned graft copolymer 1 in a mixed solvent consisting of 100 parts of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether (product name: AE-3000, manufactured by AGC Corporation) and 100 parts of 1-propanol. To the obtained dispersant solution, 40 parts of polytetrafluoroethylene resin particles A were added, and the mixture was passed through a high-pressure disperser (product name: Microfluidizer M-110EH, manufactured by Microfluidics, Inc., USA) to obtain a polytetrafluoroethylene resin particle dispersion. To the obtained polytetrafluoroethylene resin particle dispersion, 75.4 parts of a hole transporting compound represented by the following formula (B), 21.9 parts of a compound represented by the following formula (C), and 100 parts of 1-propanol were added. Then, the mixture was filtered with a Polyflon filter (product name: PF-040, manufactured by Advantec Toyo Co., Ltd.) to prepare a polytetrafluoroethylene resin particle dispersion (coating liquid for protective layer). [ka] [ka] This protective layer coating solution was applied by dip coating on the charge transport layer to form a coating film, and the resulting coating film was dried at 40°C for 5 minutes. After drying, the coating film was irradiated with an electron beam for 1.6 seconds under a nitrogen atmosphere at an acceleration voltage of 70 kV and an absorbed dose of 15 kGy. Then, in a nitrogen atmosphere, heat treatment was performed for 15 seconds under conditions such that the temperature of the coating film reached 135°C. The oxygen concentration from the irradiation of the electron beam to the heat treatment for 15 seconds was 15 ppm. Next, the coating film was naturally cooled in the atmosphere until the temperature reached 25°C, and then heat treatment was performed for 1 hour under conditions such that the coating film reached 105°C, forming a surface layer (protective layer) with a thickness of 5 μm. The content of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether in the surface layer was 5 ppm. In this manner, an electrophotographic photoreceptor having a support and a surface layer before surface polishing was prepared.

[0086] <Surface treatment of electrophotographic photoreceptor> (Polishing of electrophotographic photoreceptor before surface polishing) The surface of the electrophotographic photoreceptor before the surface shape formation was polished using the polishing device shown in Figure 2 under the following conditions. Abrasive sheet feed speed: 400mm / min Rotational speed of electrophotographic photoreceptor: 450 rpm Pressing of electrophotographic photoreceptor onto backup roller: 3.5mm Rotation direction of the abrasive sheet and electrophotographic photoreceptor; With Backup roller; outer diameter 100mm, Asker C hardness 25 The polishing sheet A to be attached to the polishing device was made by mixing the polishing grains used in GC3000 and GC2000 manufactured by Riken Corundum Co., Ltd. GC3000 (polishing sheet surface roughness Ra0.83μm) GC2000 (abrasive sheet surface roughness Ra1.45μm) Abrasive sheet A (abrasive sheet surface roughness Ra1.12μm) The polishing time using the polishing sheet A was 20 seconds.

[0087] (Measurement of polishing depth L (μm)) The maximum height Rmax of the electrophotographic photoreceptor after polishing was measured according to JIS B 0601 1982 using a surface roughness measuring instrument Surfcorder SE3500 manufactured by Kosaka Laboratory Co., Ltd. The measurement conditions were set as follows. The measurement was performed at three arbitrary locations within a 5 mm square range, and the average value was adopted as the polishing depth L (μm). The polishing depth L of the electrophotographic photoreceptor after surface polishing was 0.75 μm. In Examples 1-2 to 1-16 described later, the polishing depth L of all electrophotographic photoreceptors subjected to surface processing was 0.75 μm. (Measurement conditions) Detector: R2μm Stylus: 0.7mN diamond stylus Filter: 2CR Cutoff value: 0.08mm Measurement length: 2.5mm Feed speed: 0.1mm

[0088] [Examples 1-2 to 1-16, Comparative Examples 1-1 to 1-2] An electrophotographic photoreceptor was produced in the same manner as in Example 1-1, except that in forming the protective layer, the graft copolymer 1 was changed to the graft copolymer shown in Table 3. The content of 1,1,2,2-tetrafluoroethyl-2,2,2-trifluoroethyl ether in the surface layer is shown in Table 3.

[0089] [Table 2]

[0090] Example 2-1 (Support 2) A cylindrical aluminum cylinder (JIS-A3003, aluminum alloy, outer diameter 30 mm, length 357.5 mm, wall thickness 0.7 mm) was used as a support (conductive support). It was ultrasonically cleaned in a cleaning solution of pure water containing detergent (product name: Chemicol CT, Tokiwa Chemical Co., Ltd.), and then the cleaning solution was washed away. It was further ultrasonically cleaned in pure water and degreased, and this was used as support 2.

[0091] (Undercoat layer 2) Zinc oxide particles (average particle size: 70 nm, specific surface area: 15 m 2 To this was added 0.75 parts of a silane coupling agent (compound name: N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, product name: KBM603, manufactured by Shin-Etsu Chemical Co., Ltd.), and the mixture was stirred for 2 hours. Thereafter, the tetrahydrofuran was distilled off under reduced pressure, and the mixture was dried by heating at 120°C for 3 hours to obtain surface-treated zinc oxide particles. Next, 25 parts of butyral (product name: BM-1, manufactured by Sekisui Chemical Co., Ltd.) as a polyol and 22.5 parts of blocked isocyanate (product name: Sumidur BL-3173, manufactured by Sumitomo Bayer Urethane Co., Ltd.) were dissolved in 142 parts of methyl ethyl ketone. To this solution, 100 parts of the surface-treated zinc oxide particles and 1 part of alizarin were added, and the mixture was dispersed in a sand mill using glass beads with a diameter of 1 mm for 5 hours. After the dispersion treatment, 0.008 parts of dioctyltin dilaurate and 6.5 parts of silicone resin particles (Tospearl 145, manufactured by GE Toshiba Silicones) were added and stirred to prepare a coating liquid for an undercoat layer. The obtained coating liquid for undercoat layer was dip-coated onto the support 2 to form a coating film, and the coating film was dried at 190° C. for 24 minutes to form an undercoat layer 2 with a thickness of 15 μm.

[0092] (Charge generation layer 2) Next, 15 parts of chlorogallium phthalocyanine crystals having strong diffraction peaks at Bragg angles (2θ±0.2°) of at least 7.4°, 16.6°, 25.5°, and 28.3° for CuKα characteristic X-rays, 10 parts of vinyl chloride-vinyl acetate copolymer resin (VMCH, manufactured by Nippon Union Carbide Co., Ltd.), and 300 parts of n-butyl alcohol were mixed and dispersed for 4 hours in a sand mill using glass beads with a diameter of 1 mm to prepare a coating solution for the charge generating layer. This charge generating layer coating liquid was dip coated onto the undercoat layer 2, and the resulting coating was dried at 150° C. for 5 minutes to form a charge generating layer 2 having a thickness of 0.2 μm.

[0093] (Charge transport layer 2) 3 kg of commercially available polytetrafluoroethylene resin particles (average primary particle size 210 nm, average circularity 0.85) were placed in a stainless steel container with a width of 400 mm, depth of 400 mm, and height of 50 mm, and dried at 150°C for 3 hours in a high-temperature incubator (model: SPH-102, manufactured by Espec Corporation) to obtain polytetrafluoroethylene resin particles A. Next, 10 parts of polytetrafluoroethylene resin particles A, 0.50 parts of the above-mentioned graft copolymer 1, and 24 parts of tetrahydrofuran were mixed with stirring for 48 hours while maintaining the liquid temperature at 20° C., to obtain mixed liquid A. Next, 53.2 parts of N,N'-bis(3-methylphenyl)-N,N'-diphenylbenzidine, 14.1 parts of bisphenol Z type polycarbonate resin (viscosity average molecular weight 40,000), and 0.26 parts of 2,6-di-t-butyl-4-methylphenol as an antioxidant were mixed, and 250 parts of tetrahydrofuran was mixed and dissolved to obtain preparation B. Preparation A was added to preparation B and mixed with stirring, and then passed through a high-pressure disperser (product name: Microfluidizer M-110EH, manufactured by Microfluidics, Inc., USA) to obtain a dispersion. Then, fluorine-modified silicone oil (product name: FL-100, manufactured by Shin-Etsu Silicones) was added to the dispersion to a concentration of 5 ppm, and the mixture was filtered through a Polyflon filter (product name: PF-040, manufactured by Advantech Toyo Co., Ltd.) to prepare a coating liquid for the charge transport layer. This charge transport layer coating liquid was dip-coated onto the charge generating layer 2 to form a coating film, and the resulting coating film was dried at 150° C. for 25 minutes to form a charge transport layer with a thickness of 30 μm. In this manner, an electrophotographic photoreceptor was prepared.

[0094] [Examples 2-2 to 2-16, Comparative Examples 2-1 to 2-2] An electrophotographic photoreceptor was produced in the same manner as in Example 2-1, except that in forming the charge transport layer, the graft copolymer 1 was changed to the graft copolymer shown in Table 4.

[0095] [Table 3]

[0096] <Evaluation of Electrophotographic Photoreceptor> The electrophotographic photoreceptors obtained in Examples 1-1 to 1-16, 2-1 to 2-16, and Comparative Examples 1-1 to 1-2, and 2-1 to 2-2 were evaluated as follows.

[0097] [Evaluation device 1-1] The electrophotographic photoreceptors prepared in Examples 1-1 to 1-16 and Comparative Examples 1-1 to 1-2 were mounted on a copying machine, imagePRESS C800 (product name), manufactured by Canon Inc., and evaluated. In detail, the above-mentioned evaluation device was placed in an environment of a temperature of 23°C and a relative humidity of 50% RH, and the prepared electrophotographic photosensitive member was attached to a magenta process cartridge, which was then attached to the station of the magenta process cartridge, and evaluation was performed.

[0098] [Evaluation device 1-2] The electrophotographic photoreceptors prepared in Examples 1-1 to 1-16 and Comparative Examples 1-1 to 1-2 were installed in a modified copy machine, imagePRESS C800 (product name), manufactured by Canon Inc., and evaluated. The charging means of the modified machine was a charging means of a type that applies a voltage in which an AC voltage is superimposed on a DC voltage to a roller-type contact charging member (charging roller), and the exposure means was an exposure means of a laser image exposure type (wavelength 680 nm). In detail, the above-mentioned evaluation device was placed in an environment of a temperature of 23°C and a relative humidity of 50% RH, and the prepared electrophotographic photosensitive member was attached to a magenta process cartridge, which was then attached to the station of the magenta process cartridge, and evaluation was performed. The charging conditions were adjusted so that the charging potential was −800V and the exposure potential was −300V, and the charging potential and the exposure amount of the exposure means were adjusted. The surface potential of the electrophotographic photoreceptor was measured by removing the developing cartridge from the evaluation device and inserting a potential measuring device therein. The potential measuring device is configured by arranging a potential measuring probe (product name: model 6000B-8, manufactured by Trek Japan Co., Ltd.) at the developing position of the developing cartridge. The position of the potential measuring probe relative to the electrophotographic photoreceptor was set to the center of the electrophotographic photoreceptor in the bus direction, with a gap of 3 mm from the surface of the electrophotographic photoreceptor. Furthermore, the potential of the center of the electrophotographic photoreceptor was measured using a surface potential meter (product name: model 344, manufactured by Trek Japan Co., Ltd.).

[0099] [Evaluation device 2-1] The electrophotographic photoreceptors prepared in Examples 2-1 to 2-16 and Comparative Examples 2-1 to 2-2 were mounted on a copying machine imageRUNNER iR-ADV C5051 manufactured by Canon Inc. and evaluated. In detail, the above-mentioned evaluation device was placed in an environment of a temperature of 23° C. and a relative humidity of 50% RH, and the prepared electrophotographic photosensitive member was attached to a cyan process cartridge, which was then attached to the station of the cyan process cartridge, and evaluation was performed.

[0100] [Evaluation device 2-2] The electrophotographic photoreceptors prepared in Examples 2-1 to 2-16 and Comparative Examples 2-1 to 2-2 were attached to a modified copy machine imageRUNNER iR-ADV C5051 manufactured by Canon Inc. (the charging means was a type in which a voltage in which an AC voltage was superimposed on a DC voltage was applied to a roller-type contact charging member (charging roller), and the exposure means was a laser image exposure method (wavelength 780 nm)) and evaluated. In detail, the above-mentioned evaluation device was placed in an environment of a temperature of 23° C. and a relative humidity of 50% RH, and the prepared electrophotographic photosensitive member was attached to a cyan process cartridge, which was then attached to the station of the cyan process cartridge, and evaluation was performed. The charging conditions were adjusted so that the charging potential was −700V and the exposure potential was −200V, and the charging potential and the exposure amount of the exposure means were adjusted. The surface potential of the electrophotographic photoreceptor was measured by removing the developing cartridge from the evaluation device and inserting a potential measuring device therein. The potential measuring device was configured by arranging a potential measuring probe (product name: model 6000B-8, manufactured by Trek Japan Co., Ltd.) at the developing position of the developing cartridge, and the position of the potential measuring probe relative to the electrophotographic photoreceptor was the center of the electrophotographic photoreceptor in the bus direction, with a gap of 3 mm from the surface of the electrophotographic photoreceptor. Furthermore, the potential at the center of the electrophotographic photoreceptor was measured using a surface potential meter (product name: model 344, manufactured by Trek Japan Co., Ltd.).

[0101] (Initial image evaluation) The image evaluation was carried out using the above-mentioned evaluation device 1-1 and evaluation device 2-1. A solid white image was output using A4-sized gloss paper, and the number of image defects, i.e., black spots, due to poor dispersion contained in the area of ​​one circumference of the electrophotographic photoreceptor of the output image was visually evaluated according to the following evaluation ranks. The area of ​​one circumference of the electrophotographic photoreceptor is a rectangular area whose length is 297 mm, which is the long side length of A4 paper, and whose width is 94.2 mm, which is one circumference of the electrophotographic photoreceptor. In addition, in this disclosure, ranks A, B, C, and D are levels at which the effects of this disclosure are obtained, and among them, rank A was judged to be an excellent level. On the other hand, rank E was judged to be a level at which the effects of this disclosure are not obtained. A: No black spots at all B: 1 to 3 black dots less than 1.5 mm in diameter, and no black dots 1.5 mm or more in diameter C: 1 to 3 black dots less than 1.5 mm in diameter, and 1 to 2 black dots 1.5 mm or more in diameter D: 4 to 5 black dots less than 1.5 mm in diameter, and 2 or less black dots 1.5 mm or more in diameter E: 6 or more black spots less than 1.5 mm in diameter, or 3 or more black spots 1.5 mm or more in diameter The results of the evaluation are shown in Table 6.

[0102] (Evaluation of potential fluctuations during repeated use) The potential fluctuation evaluation during repeated use was carried out using the above-mentioned evaluation device 1-2 and evaluation device 2-2. The cartridge equipped with the electrophotographic photoreceptor was attached to the evaluation device, and the photoreceptor was repeatedly used by passing 10,000 sheets of paper. In the station where the electrophotographic photoreceptor was installed, a single-color character image with a printing rate of 1% was repeatedly formed on 10,000 sheets of A4-sized plain paper. The initial dark area potential at this time was compared with the dark area potential after the repeated image formation of 10,000 sheets, and this was taken as the potential fluctuation value (ΔVd). In addition, the initial light area potential was compared with the light area potential after the repeated image formation of 10,000 sheets, and this was taken as the potential fluctuation value (ΔVl). After passing 10,000 sheets of paper, the cartridge was left for 5 minutes, the developing cartridge was replaced with a potential measuring device, and the light area potential (Vlb) and dark area potential (Vdb) after repeated use were measured. The difference between the dark area potential after repeated use and the initial dark area potential (Vda) was taken as the dark area potential fluctuation (ΔVd=|Vdb|-|Vda|). The difference between the light area potential after repeated use and the initial light area potential (Vla) was taken as the light area potential fluctuation (ΔVl=|Vlb|-|Vla|). In the evaluation using evaluation device 1-2, the light area potential fluctuation was measured after repeated use of 100,000 sheets, 300,000 sheets, and 500,000 sheets. In the evaluation using evaluation device 2-2, the light area potential fluctuation was measured after repeated use of 100,000 sheets. In the present disclosure, it is determined that the smaller the change in bright area potential is, the greater the effect of the present disclosure is.

[0103] The results of the evaluation are shown in Table 5. [Table 4]

[0104] The disclosure of this embodiment includes the following configurations and methods. (Configuration 1) An electrophotographic photoreceptor having a surface layer, The surface layer is Fluorine atom-containing resin particles; A binding material; A polymer A having a structural unit represented by the following formula (1); An electrophotographic photoreceptor comprising: [ka] (In formula (1), R 11 represents a hydrogen atom or a methyl group, R 12 and R 13 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms, n is 0 to 3, Rf 1 each independently represents a perfluoroalkylene group having 1 to 5 carbon atoms, or a perfluoroalkylidene group having 1 to 5 carbon atoms, Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms. (Configuration 2) Rf in the formula (1) 1 and Rf 2 2. The electrophotographic photoreceptor according to claim 1, wherein the total number of carbon atoms in (Configuration 3) The electrophotographic photoreceptor according to Configuration 1, wherein the content of the structural unit represented by formula (1) in the polymer A is from 5% by number to 50% by number by number with respect to all structural units in the polymer A. (Configuration 4) 2. The electrophotographic photoreceptor according to claim 1, wherein the weight average molecular weight of the polymer A is 16,000 or more and 300,000 or less. (Configuration 5) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the content of the polymer A in the surface layer is from 2% by mass to 10% by mass based on the mass of the fluorine-containing resin particles in the surface layer. (Configuration 6) The electrophotographic photoreceptor according to Configuration 1, wherein the polymer A further has a structural unit represented by the following formula (2): [ka] (In formula (2), Y A1represents an unsubstituted alkylene group, Y B represents an unsubstituted alkylene group, an alkylene group substituted with a halogen atom, an alkylene group substituted with a hydroxyl group, an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), or a divalent linking group derived by combining one or more selected from these groups and bonds with -O- or -S-, or a single bond, Z A represents a structure represented by the following formula (2A), a cyano group, or a phenyl group, R 21 , and R 22 each independently represents a hydrogen atom or a methyl group, m is an integer between 25 and 150. [ka] (In formula (2A), Z A1 represents an alkyl group having 1 to 4 carbon atoms. (Configuration 7) The electrophotographic photoreceptor according to Constitution 6, wherein the polymer A has, as structural units, only the structural unit represented by formula (1) and the structural unit represented by formula (2). (Configuration 8) The electrophotographic photoreceptor according to Configuration 7, wherein the ratio of the structural unit represented by formula (1) to the structural unit represented by formula (2) in the polymer A is from 1:19 to 1:1 in terms of molar ratio. (Configuration 9) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the content of the fluorine atom-containing resin particles in the surface layer is from 5% by mass to 40% by mass, both inclusive, based on the total mass of the surface layer. (Configuration 10) 2. The electrophotographic photoreceptor according to claim 1, wherein the binder material is a cured product of a hole transporting compound having a chain polymerizable functional group. (Configuration 11) 11. The electrophotographic photoreceptor according to Configuration 10, wherein the hole transporting compound having a chain polymerizable functional group is a compound represented by the following formula (CT-1) or (CT-2): [ka] (In the above formula (CT-1), Ar 11 ~Ar 13 each independently represents a substituted aryl group or an unsubstituted aryl group, and the substituent that the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by any one of the following formulas (P-1) to (P-3), with the proviso that the compound represented by the formula (CT-1) has at least one monovalent functional group represented by any one of the following formulas (P-1) to (P-3). [ka] (In the formula (CT-2), Ar 21 ~Ar 24 each independently represents a substituted aryl group or an unsubstituted aryl group; Ar 25 represents a substituted arylene group or an unsubstituted arylene group, the substituent which the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3), the substituent which the substituted arylene group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3), and the compound represented by formula (CT-2) has at least one monovalent functional group represented by any of the following formulas (P-1) to (P-3). [ka] (In the formula (P-1), Z 11 represents a single bond or an alkylene group having 1 to 6 carbon atoms; X 11 represents a hydrogen atom or a methyl group. [ka] (In the formula (P-2), Z 21 represents a single bond or an alkylene group having 1 to 6 carbon atoms. [ka] (In the formula (P-3), Z 31 represents a single bond or an alkylene group having 1 to 6 carbon atoms. (Configuration 12) 2. The electrophotographic photoreceptor according to Configuration 1, wherein the polymer A does not have a structural unit having an acidic group with a pKa of 3 or less. (Configuration 13) 12. The electrophotographic photoreceptor according to claim 11, wherein the surface layer further contains a compound represented by the following formula (3): [ka] (In formula (3), R 31 represents an alkyl group or a fluoroalkyl group, R 32 represents a fluoroalkyl group. (Configuration 14) A process cartridge integrally supporting the electrophotographic photosensitive member according to any one of configurations 1 to 13 and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and being detachably mountable to a main body of an electrophotographic apparatus. (Configuration 15) 14. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to any one of Configurations 1 to 13, a charging unit, an exposing unit, a developing unit, and a transferring unit. (Method 1) A method for producing an electrophotographic photoreceptor according to any one of configurations 1 to 13, comprising the steps of: The manufacturing method comprises: A step of preparing a coating liquid for a surface layer, the coating liquid containing the polymer A, at least one selected from a binder material and a raw material for a binder material, and fluorine atom-containing resin particles; and a step of forming a coating film of the coating liquid for the surface layer, and drying and / or curing the coating film to form the surface layer; having 2. A method for producing an electrophotographic photoreceptor comprising the steps of: [Explanation of symbols]

[0105] 101 Support 102 Undercoat layer 103 Charge generating layer 104 Charge transport layer 105 Surface layer (protective layer) 201 Electrophotographic photoreceptor 202 Axis 203 Charging means 204 Exposure light 205 Developing means 206 Transcription means 207 Transfer material 208 Fixing means 209 Cleaning methods 210 Pre-exposure light 211 Process cartridge 212 Guidance means 1. Electrophotographic photoreceptor 2. Charging means 3 Exposure light (image exposure light) 4. Developing Method 5 Transfer Method 6 Transfer material 7 Pre-exposure light 8 Cleaning Method 9 Process cartridge 10 Intermediate transfer body 11 Transfer paper 12 Paper feed path 13 Paper feed tray 14 Secondary transfer means 15 Fixing Method 16 Paper ejection section 17 Yellow process cartridge 18 Magenta process cartridge 19 Cyan process cartridge 20 Black process cartridge

Claims

1. An electrophotographic photoreceptor having a surface layer, The surface layer is Fluorine atom-containing resin particles; A binding material; A polymer A having a structural unit represented by the following formula (1), An electrophotographic photoreceptor comprising: [Formula 1] (In formula (1), R 11 represents a hydrogen atom or a methyl group, R 12 and R 13 each independently represents a single bond or an alkylene group having 1 to 3 carbon atoms, n is 0 to 3, Rf 1 each independently represents a perfluoroalkylene group having 1 to 5 carbon atoms, or a perfluoroalkylidene group having 1 to 5 carbon atoms, Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms.

2. Rf in the formula (1) 1 and Rf 2 The electrophotographic photoreceptor according to claim 1 , wherein the total number of carbon atoms in the formula (I) is 6 or more and 9 or less.

3. 2 . The electrophotographic photoreceptor according to claim 1 , wherein the content of the structural unit represented by formula (1) in the polymer A is 5% by number or more and 50% by number or less based on all structural units in the polymer A.

4. 2. The electrophotographic photoreceptor according to claim 1, wherein the weight average molecular weight of the polymer A is from 16,000 to 300,000.

5. 2 . The electrophotographic photoreceptor according to claim 1 , wherein the content of the polymer A in the surface layer is from 2% by mass to 10% by mass with respect to the mass of the fluorine atom-containing resin particles in the surface layer.

6. The electrophotographic photoreceptor according to claim 1 , wherein the polymer A further has a structural unit represented by the following formula (2): [chemical 2] (In formula (2), Y A1 represents an unsubstituted alkylene group, Y B represents an unsubstituted alkylene group, an alkylene group substituted with a halogen atom, an alkylene group substituted with a hydroxyl group, an ester bond (-COO-), an amide bond (-NHCO-), a urethane bond (-NHCOO-), or a divalent linking group derived by combining one or more selected from these groups and bonds with -O- or -S-, or a single bond, Z A represents a structure represented by the following formula (2A), a cyano group, or a phenyl group, R 21 , and R 22 each independently represents a hydrogen atom or a methyl group, m is an integer between 25 and 150. [C3] (In formula (2A), Z A1 represents an alkyl group having 1 to 4 carbon atoms.

7. The electrophotographic photoreceptor according to claim 6 , wherein the polymer A has, as structural units, only the structural unit represented by the formula (1) and the structural unit represented by the formula (2).

8. 8. The electrophotographic photoreceptor according to claim 7, wherein the ratio of the structural unit represented by the formula (1) to the structural unit represented by the formula (2) in the polymer A is from 1:19 to 1:1 in terms of molar ratio.

9. 2 . The electrophotographic photoreceptor according to claim 1 , wherein the content of the fluorine atom-containing resin particles in the surface layer is from 5% by mass to 40% by mass with respect to the total mass of the surface layer.

10. 2. The electrophotographic photoreceptor according to claim 1, wherein the binder material is a cured product of a hole transporting compound having a chain polymerizable functional group.

11. The electrophotographic photoreceptor according to claim 10, wherein the hole transporting compound having a chain polymerizable functional group is a compound represented by the following formula (CT-1) or (CT-2): [C4] (In the above formula (CT-1), Ar 11 ~Ar 13 each independently represents a substituted aryl group or an unsubstituted aryl group, and the substituent that the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by any one of the following formulas (P-1) to (P-3), with the proviso that the compound represented by the formula (CT-1) has at least one monovalent functional group represented by any one of the following formulas (P-1) to (P-3). [C5] (In the above formula (CT-2), Ar 21 ~Ar 24 each independently represents a substituted aryl group or an unsubstituted aryl group; Ar 25 represents a substituted arylene group or an unsubstituted arylene group, a substituent which the substituted aryl group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3), a substituent which the substituted arylene group may have is an alkyl group having 1 to 6 carbon atoms, or a monovalent functional group represented by the following formulas (P-1) to (P-3), and the compound represented by formula (CT-2) has at least one monovalent functional group represented by any of the following formulas (P-1) to (P-3). [C6] (In the formula (P-1), Z 11 represents a single bond or an alkylene group having 1 to 6 carbon atoms; X 11 represents a hydrogen atom or a methyl group. [C7] (In the formula (P-2), Z 21represents a single bond or an alkylene group having 1 to 6 carbon atoms. [C8] (In the formula (P-3), Z 31 represents a single bond or an alkylene group having 1 to 6 carbon atoms.

12. 2. The electrophotographic photoreceptor according to claim 1, wherein the polymer A does not have a structural unit having an acidic group having a pKa of 3 or less.

13. The electrophotographic photoreceptor according to claim 11, wherein the surface layer further contains a compound represented by the following formula (3): [C9] (In formula (3), R 31 represents an alkyl group or a fluoroalkyl group; R 32 represents a fluoroalkyl group.

14. 14. A process cartridge which integrally supports the electrophotographic photosensitive member according to any one of claims 1 to 13 and at least one means selected from the group consisting of a charging means, a developing means, and a cleaning means, and is detachably mountable to a main body of an electrophotographic apparatus.

15. 14. An electrophotographic apparatus comprising the electrophotographic photoreceptor according to claim 1, a charging unit, an exposing unit, a developing unit, and a transferring unit.

16. A method for producing an electrophotographic photoreceptor according to any one of claims 1 to 13, comprising the steps of: The manufacturing method comprises: A step of preparing a coating liquid for a surface layer, the coating liquid containing the polymer A, at least one selected from a binder material and a raw material for a binder material, and fluorine atom-containing resin particles; and a step of forming a coating film of the coating liquid for the surface layer, and drying and / or curing the coating film to form the surface layer; having 2. A method for producing an electrophotographic photoreceptor comprising the steps of:

Citation Information

Patent Citations

  • Electrophotographic sensitive and electrophotographic device having the same

    JP1994332219A

  • Electrophotographic photosensitive member, method of manufacturing electrophotographic photosensitive member, process cartridge, and electrophotographic apparatus

    JP2009104145A

  • Electrophotographic photoreceptor, method for manufacturing electrophotographic photoreceptor, image forming apparatus and process cartridge

    JP2012189715A

  • Electrophotographic photoreceptor, process cartridge, and image forming device

    JP2021047236A

Cited By

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP7868767B1

  • Electrophotographic photoreceptor, process cartridge, and image forming apparatus

    JP7907815B1