Block olefin-modified polyvinyl alcohol and method for producing the same

The block olefin-modified polyvinyl alcohol addresses affinity and adhesion issues by integrating a polyolefin resin with α-methylstyrene groups into polyvinyl alcohol, achieving high hydrophilicity and compatibility with hydrophobic materials for filtration and separation applications.

JP2024139419AInactive Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023050352
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Hydrophilic materials applied to hydrophobic materials suffer from low affinity and adhesion issues, leading to destabilization and insufficient hydrophilicity when used in porous membranes for aqueous liquid treatments.

Method used

A block olefin-modified polyvinyl alcohol is developed by incorporating a polyolefin resin with α-methylstyrene groups into a polyvinyl alcohol resin, creating a material with both hydrophilic and hydrophobic properties.

Benefits of technology

The block olefin-modified polyvinyl alcohol exhibits excellent affinity with hydrophobic materials while maintaining high hydrophilicity, suitable for applications in medical and industrial filtration and separation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139419000002
    Figure 2024139419000002
  • Figure 2024139419000001
    Figure 2024139419000001
Patent Text Reader

Abstract

To provide block olefin-modified polyvinyl alcohol which has excellent compatibility with a hydrophobic material, in a state having a hydrophilic group.SOLUTION: Block olefin-modified polyvinyl alcohol has a constitutional unit derived from a polyvinyl alcohol-based resin, and a constitutional unit derived from a polyolefin resin having an α-methyl styrene group.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a block olefin-modified polyvinyl alcohol, and more particularly to a block olefin-modified polyvinyl alcohol having excellent affinity with hydrophobic materials while having hydrophilic groups. [Background technology]

[0002] Hydrophobic resin materials are generally used as materials for films and fibers. However, materials for forming porous membranes used in the treatment of various aqueous liquids, such as medical and industrial filtration and separation, require high hydrophilicity, and studies have been conducted on coating hydrophobic resin materials with hydrophilic materials or alloying them with highly hydrophilic resins (Patent Documents 1 and 2). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2015-29926 A [Patent Document 2] Japanese Patent Application Publication No. 5-202240 Summary of the Invention [Problem to be solved by the invention]

[0004] However, when a hydrophobic material is coated with a hydrophilic material, the hydrophilic material may fall off during use due to low affinity for the material and insufficient adhesion. Furthermore, when a hydrophobic material and a hydrophilic material are alloyed, mutual exclusion occurs due to low affinity, making the mixed phase unstable or causing localization, making it impossible to form the desired shape, or insufficient hydrophilicity.

[0005] Therefore, attempts have been made to solve the above problems by partially incorporating a hydrophobic structure into a hydrophilic material to improve the affinity between the hydrophobic material and the hydrophilic material. However, when a hydrophobic structure is incorporated into a hydrophilic material, although the affinity with the hydrophobic material is improved, the effect of imparting the desired hydrophilicity is reduced.

[0006] Under these circumstances, an object of the present invention is to provide a block olefin-modified polyvinyl alcohol that has excellent affinity with hydrophobic materials while having hydrophilic groups. [Means for solving the problem]

[0007] However, in view of these circumstances, the present inventors conducted extensive research and discovered that by introducing a polyolefin resin having an α-methylstyrene group in a block manner into a polyvinyl alcohol resin, it is possible to produce a material that has excellent affinity with hydrophobic materials while still having hydrophilic groups, and thus completed the present invention.

[0008] That is, the present invention has the following aspects. [1] A block olefin-modified polyvinyl alcohol having a structural unit derived from a polyvinyl alcohol resin and a structural unit derived from a polyolefin resin having an α-methylstyrene group. [2] The block olefin-modified polyvinyl alcohol according to [1], wherein the polyolefin having an α-methylstyrene group is a polyethylene having an α-methylstyrene group at its terminal. [3] The block olefin-modified polyvinyl alcohol according to [2], wherein the content of the ethylene monomer units is 1 to 20 mol % based on the total of the vinyl alcohol monomer units and the ethylene monomer units. [4] The block olefin-modified polyvinyl alcohol according to any one of [1] to [3], which has a weight average molecular weight of 10,000 to 1,000,000. [5] A method for producing block olefin-modified polyvinyl alcohol obtained by saponifying a reaction product of a polyvinyl ester resin obtained by living polymerization with a polyolefin resin having an α-methylstyrene group. [6] The method for producing a block olefin-modified polyvinyl alcohol according to [5], wherein the polyvinyl ester-based resin is a polyvinyl acetate-terminated cobalt complex obtained by living polymerization using a cobalt living control agent. Effect of the Invention

[0009] The block olefin-modified polyvinyl alcohol of the present invention, in the state in which it has hydrophilic groups, becomes a material that has excellent affinity with hydrophobic materials. [Brief description of the drawings]

[0010] [Figure 1] 1 is a graph showing the relationship between the ethylene modification rate and the water contact angle in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described below based on examples of the mode for carrying out the present invention. However, the present invention is not limited to the embodiment described below.

[0012] In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". In the present invention, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also means that "it is preferably greater than X" or "it is preferably less than Y".

[0013] In the present invention, the term "mainly" refers to the component that constitutes the majority in the target object, and generally, it is preferably 50% by mass or more of the target object, more preferably 60% by mass or more, even more preferably 70% by mass or more, particularly preferably 80% by mass or more, and especially preferably 90% by mass or more, and may be 100% by mass. In the present invention, "(meth)acrylic" means acrylic or methacrylic, and "(meth)acrylate" means acrylate or methacrylate, respectively. In the present invention, the term "film" includes "tape" and "sheet".

[0014] <<Block olefin modified polyvinyl alcohol>> The block olefin-modified polyvinyl alcohol according to one embodiment of the present invention (hereinafter, sometimes referred to as "this block-modified PVA") is polyvinyl alcohol modified in blocks with polyolefin, and is usually polyvinyl alcohol modified at the end of the main chain with polyolefin. Note that polyvinyl alcohol may also be simply referred to as "PVA".

[0015] The present block modified PVA contains structural units derived from a PVA resin and structural units derived from a polyolefin resin having an α-methylstyrene group, and preferably has these structural units as the main components.

[0016] The PVA resin is obtained by saponifying a polyvinyl ester resin, and the structural units derived from the PVA resin include a vinyl alcohol monomer unit, and the structural units derived from the polyolefin resin include an ethylene monomer unit.

[0017] In the present block modified PVA, the content of ethylene monomer units relative to the total of vinyl alcohol monomer units and ethylene monomer units (hereinafter referred to as "ethylene modification rate") is preferably 1 to 20 mol%, more preferably 2 to 18 mol%, and further preferably 5 to 15 mol%. When the content of ethylene monomer units is within this range, high hydrophilicity can be exhibited while maintaining affinity with hydrophobic materials. The content of ethylene monomer units in the present block modified PVA can be measured, for example, by the method for calculating the ethylene modification rate described in the Examples below.

[0018] The average saponification degree of the block modified PVA is usually 95 mol% or more, preferably 97 mol% or more, more preferably 99 mol% or more. If the average saponification degree is too low, the hydrophilicity tends to decrease, and the upper limit of the average saponification degree is 100 mol%. The average saponification degree is measured in accordance with JIS K 6726.

[0019] The weight-average molecular weight of the block-modified PVA is preferably from 10,000 to 1,000,000, more preferably from 20,000 to 500,000, even more preferably from 30,000 to 400,000, and particularly preferably from 40,000 to 300,000. When the weight-average molecular weight is within this range, the balance between processability and water resistance is excellent. The weight average molecular weight of the present block modified PVA can be measured, for example, by the method described in the Examples below.

[0020] The polydispersity of the present block modified PVA is preferably 1-10, more preferably 1-5, and further preferably 1-3. The dispersity of the present block modified PVA can be measured, for example, by the method described in the Examples below.

[0021] The water contact angle of the present block modified PVA is preferably 58° or more, more preferably 59° or more, and further preferably 60° or more. The upper limit is usually 150°, and preferably 90° or less. The water contact angle of the present block modified PVA can be measured, for example, by the method described in the Examples below.

[0022] Compared with random olefin-modified PVA with the same number of olefin monomer units, this block-modified PVA has a higher water contact angle and is believed to have a higher affinity with hydrophobic materials despite having many hydrophilic groups.

[0023] <<Production method of block olefin modified PVA>> This block modified PVA can be obtained by saponifying the reaction product of a polyvinyl ester resin obtained by living polymerization and a polyolefin resin having an α-methylstyrene group.

[0024] Specifically, the method includes (1) a step of preparing a polyolefin resin having an α-methylstyrene group and a polyvinyl ester resin obtained by living polymerization, (2) a step of obtaining a reaction product of the polyolefin resin having an α-methylstyrene group and the vinyl ester resin, and (3) a step of saponifying the reaction product. Each step will be described below.

[0025] <Regarding process (1)> First, a polyolefin resin having an α-methylstyrene group and a polyvinyl ester resin obtained by living polymerization are prepared as necessary.

[0026] [Polyolefin resin containing α-methylstyrene groups] Examples of polyolefins in the polyolefin resin having an α-methylstyrene group include polyethylene and polypropylene, which can be used alone or in combination of two or more. Among them, polyethylene is preferably used because it is easy to modify PVA.

[0027] The polyolefin resin having an α-methylstyrene group is preferably a polyethylene having an α-methylstyrene group at its terminal. When the polyolefin resin is a polyethylene having an α-methylstyrene group at its terminal, it tends to be easily introduced into the PVA resin in the form of blocks.

[0028] PVA-based resins are obtained by saponifying polyvinyl ester-based resins, and by having an α-methylstyrene group having an unsaturated group at the end of the polyolefin, the reactivity with the end of the polyvinyl ester-based resin can be improved.

[0029] A preferred example of a polyolefin having an α-methylstyrene group at its end, which has an unsaturated group, is 1,3-diisopropenylbenzene-terminated polyethylene.

[0030] [Living polymerized polyvinyl ester resin] Polyvinyl ester resins are usually obtained by polymerizing vinyl ester monomers, and such polyvinyl ester resins become PVA resins by saponification.

[0031] Examples of the vinyl ester monomer include aliphatic vinyl esters such as vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl versatate, and vinyl trifluoroacetate, and aromatic vinyl esters such as vinyl benzoate. Among these, aliphatic vinyl esters having 3 to 20 carbon atoms are preferred, more preferably 4 to 10 carbon atoms, and even more preferably 4 to 7 carbon atoms, and particularly preferably vinyl acetate. These are usually used alone, but multiple types may be used simultaneously as necessary.

[0032] The polymerization reaction is preferably carried out by living radical polymerization, for example, by using a known radical polymerization initiator such as azobisisobutyronitrile, acetyl peroxide, benzoyl peroxide, lauroyl peroxide, etc. in combination with a cobalt catalyst as a living radical control agent. The radical polymerization initiator is preferably an azo-based polymerization initiator, more preferably 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and the cobalt catalyst is preferably a divalent organic cobalt complex, more preferably cobalt acetylacetonate.

[0033] The amount of the radical polymerization initiator added is preferably 0.00001 to 0.2 mol %, more preferably 0.00005 to 0.02 mol %, and further preferably 0.0001 to 0.002 mol % parts by mass based on the total amount of the vinyl ester monomer and the radical polymerization initiator initially charged.

[0034] The amount of the living radical controller added is preferably 0.00001 to 0.1 mol %, more preferably 0.00005 to 0.01 mol %, and further preferably 0.0001 to 0.001 mol %, based on the total amount of the vinyl ester monomer and the living radical controller initially charged.

[0035] The polymerization temperature is preferably 0 to 60° C., and more preferably 10 to 50° C. The polymerization time is not particularly limited since it varies depending on the polymerization temperature, and it is preferable to carry out the polymerization until the polymerization rate reaches 10% or more, more preferably 15% or more, and further preferably 20% or more.

[0036] As the living polymerized polyvinyl ester resin, a polyvinyl acetate-terminated cobalt complex is particularly preferred.

[0037] In addition to the vinyl ester monomers, other unsaturated monomers may also be polymerized within the limits not impairing the effects of the present invention. The amount of other unsaturated monomers introduced into the PVA resin is usually 20 mol % or less, preferably 10 mol % or less, and particularly preferably 5 mol % or less. The lower limit is 0 mol %.

[0038] Examples of the other unsaturated monomers include unsaturated acids such as (meth)acrylic acid, crotonic acid, maleic acid, maleic anhydride, and itaconic acid, or their salts or mono- or dialkyl esters; nitriles such as (meth)acrylonitrile; amides such as (meth)acrylamide; olefin sulfonic acids such as ethylene sulfonic acid, allyl sulfonic acid, and methallyl sulfonic acid, or their salts; alkyl vinyl ethers; N-acrylamidomethyltrimethylammonium chloride, allyl trimethylammonium chloride, dimethylallyl vinyl ketone, N-vinylpyrrolidone, vinyl chloride, vinylidene chloride, polyoxyethylene (meth)allyl ether, and polyoxypropylene (meth)allyl ether. Examples of the polyoxyalkylene (meth)allyl ether include polyoxyalkylene (meth)acrylates such as polyoxyethylene (meth)acrylate and polyoxypropylene (meth)acrylate, polyoxyalkylene (meth)acrylamides such as polyoxyethylene (meth)acrylamide and polyoxypropylene (meth)acrylamide, polyoxyethylene (1-(meth)acrylamide-1,1-dimethylpropyl) ester, polyoxyethylene vinyl ether, polyoxypropylene vinyl ether, polyoxyethylene allylamine, polyoxypropylene allylamine, polyoxyethylene vinylamine, polyoxypropylene vinylamine, 3,4-diacetoxybutene, etc. These can be used alone or in combination of two or more.

[0039] <Regarding step (2)> The polyvinyl ester resin obtained by living polymerization (hereinafter may be referred to as "polyvinyl ester resin component") prepared as above is reacted with a polyolefin resin having an α-methylstyrene group (hereinafter may be referred to as "polyolefin resin component") to obtain a reaction product. The polyvinyl ester resin component, particularly the polyvinyl ester resin living polymerized using a living radical control agent, has a polymerization active group at its terminal, and is therefore highly reactive with a polyolefin having an α-methylstyrene group having an unsaturated group at its terminal.

[0040] The reaction temperature between the polyvinyl ester resin component and the polyolefin resin component is preferably 20 to 80°C, more preferably 30 to 70°C, and further preferably 40 to 60°C.

[0041] The reaction time is not particularly limited since it varies depending on the reaction temperature, but it is usually 10 minutes to 5 hours, and preferably 30 minutes to 2 hours.

[0042] If necessary, the reaction may be stopped by adding a reaction stopper such as dinitrobenzene.

[0043] <Regarding step (3)> The reaction product obtained in the above step (2) is saponified, but the saponification method is not particularly limited and can be any known method. That is, the saponification can be carried out using an alkali catalyst or an acid catalyst in a state where the polyvinyl ester polymer is dissolved in an alcohol or water / alcohol solvent. As the alkali catalyst, for example, hydroxides or alcoholates of alkali metals such as potassium hydroxide, sodium hydroxide, sodium methylate, sodium ethylate, potassium methylate, and lithium methylate can be used. Generally, transesterification using an alkali catalyst in an absolute alcohol solvent is preferably used in terms of reaction rate and ability to reduce impurities such as fatty acid salts. The saponification step is preferably carried out after the extraction step (extraction of the reaction product from the reaction solution) from the viewpoint of the purity of the present block-modified PVA obtained.

[0044] By saponifying the reaction product, the present block modified PVA can be obtained.

[0045] <Other ingredients> In addition, the present block modified PVA may contain other components such as other resin components, various additives such as polymerization inhibitors, antioxidants, corrosion inhibitors, crosslinking accelerators, UV absorbers, plasticizers, pigments, stabilizers, and fillers, metals, and resin particles, as long as the effects of the present invention are not impaired. These may be used alone or in combination of two or more. In addition, small amounts of impurities contained in the manufacturing raw materials of the constituent components may be contained.

[0046] The content of the other components is preferably 20% by mass or less, particularly preferably 10% by mass or less, and further preferably 5% by mass or less, based on the block modified PVA. The lower limit is usually 0% by mass.

[0047] <Application> This block-modified PVA has excellent affinity with hydrophobic materials while retaining hydrophilic groups, and can therefore be used in a wide range of applications in various fields, including medical and industrial fields, such as antithrombotic materials and membrane fouling prevention materials. In addition, this block-modified PVA is expected to be used to hydrophobize the surface of hydrophilic materials and as a compatibilizer for incompatible polymers. EXAMPLES

[0048] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.

[0049] The ethylene modification rate, number average molecular weight, weight average molecular weight, dispersity, and water contact angle of the PVA obtained in the examples and comparative examples were measured as follows. The results are shown in Table 1 below.

[0050] (Calculation of ethylene modification rate) The modification rate of ethylene monomer units was calculated from the comparison of the integral ratio of the peak (4.9 to 5.1 ppm) derived from the main chain methine of the vinyl ester to the peak (1.2 to 1.4 ppm) derived from ethylene using 1H-NMR (Ascend NMR 400, manufactured by Bruker Japan). The modification rate of ethylene monomer units was calculated from the comparison of the integral ratio of the peak (4.9 to 5.1 ppm) derived from the main chain methine of the vinyl ester to the peak (1.2 to 1.4 ppm) derived from ethylene using 1H-NMR (Bruker Japan, Ltd.).

[0051] (Measurement of number average molecular weight, weight average molecular weight, and dispersity (molecular weight distribution)) The number average molecular weight (Mn) and weight average molecular weight (Mw) of PVA were measured using a high-speed GPC device (Shimadzu Corporation, HLC-8420GPC) under the following measurement conditions. Column: Showa Denko GPC standard column "HFIP-806M" 2 columns connected in series Standard sample: Polymethyl methacrylate Solvent and mobile phase: Sodium trifluoroacetate-HFIP solution (concentration 5 mM) Flow rate: Sample line 1.0mL / min, Reference line 0.5mL / min ·Temperature: 40℃ Sample solution concentration: 10mg / 10mL (filtered with a non-aqueous 0.2μL filter) ·Injection volume: 50μL Detector: RI

[0052] (Water contact angle measurement) The obtained PVA was used to prepare a 4% aqueous solution, which was then cast onto a PET film and dried at 25°C for one week to obtain a film with a thickness of 100 μm. After conditioning the film at 25°C and 55% RH for one week, the contact angle of a water droplet was measured using a DropMaster DM-500 manufactured by Kyowa Interface Science Co., Ltd. The contact angle was automatically measured using the analysis software FAMAS on an image taken 2 seconds after the water droplet was dropped. Each sample was measured 10 times, and the average value of 8 points excluding the maximum and minimum values ​​was calculated.

[0053] <Example 1> A block olefin modified PVA was produced through the following steps.

[0054] [Living radical polymerization of poly(vinyl acetate)] 200g of vinyl acetate and 0.08g of cobalt (II) acetylacetonate as a living control agent were added to a flask equipped with a stirring blade, and nitrogen bubbling was performed for 30 minutes. Then, 0.26g of 2,2'-azobis (4-methoxy-2,4-dimethylvaleronitrile) was added as a radical polymerization initiator, and nitrogen bubbling was performed for another 30 minutes. The temperature was raised while stirring under a nitrogen atmosphere, and polymerization was performed by adjusting the temperature of the reaction solution to 30°C. When the polymerization rate reached 23%, the polymerization was stopped by cooling, and a vinyl acetate solution of polyvinyl acetate terminal cobalt complex was obtained.

[0055] [Reaction of polyvinyl acetate terminal cobalt complex with polyolefin resin having α-methylstyrene group] In a flask equipped with a stirring blade, 80 mL of toluene and 6.8 g of 1,3-diisopropenylbenzene-terminated polyethylene were added, and nitrogen was bubbled for 30 minutes. After that, the temperature was raised to dissolve the 1,3-diisopropenylbenzene-terminated polyethylene in toluene, and the temperature was adjusted to 50°C. The entire amount of the vinyl acetate solution of the polyvinyl acetate-terminated cobalt complex prepared above was added, and the reaction was allowed to proceed for 1 hour. Thereafter, 0.2 g of dinitrobenzene was added to terminate the reaction, 100 g of an aqueous solution of acetic acid (2%) was added, and the aqueous layer was removed by a separation operation. The organic layer was then distilled off with an evaporator to obtain a mixture of the reaction product of the polyvinyl acetate-terminated cobalt complex and the 1,3-diisopropenylbenzene-terminated polyethylene, and unreacted 1,3-diisopropenylbenzene-terminated polyethylene. The resulting mixture was washed with methanol, and the remaining vinyl acetate was removed using an evaporator. The mixture was then dissolved in ethyl acetate and allowed to stand overnight. After that, the unreacted 1,3-diisopropenylbenzene-terminated polyethylene was removed by Buchner filtration, yielding a reaction product of a polyvinyl acetate-terminated cobalt complex and 1,3-diisopropenylbenzene-terminated polyethylene.

[0056] [Saponification of the reactant] The reaction product of the polyvinyl acetate-terminated cobalt complex and 1,3-diisopropenylbenzene-terminated polyethylene was added to the flask, saponified with sodium hydroxide, washed with methanol, and dried in a vacuum dryer at 50°C for 8 hours to obtain the desired block ethylene-modified PVA. The resulting block ethylene modified PVA had a weight average molecular weight of 250,000, an ethylene modification rate of 3 mol %, and a saponification degree of 99 mol %.

[0057] <Example 2> Polymerization was carried out in the same manner as in Example 1, except that the amount of cobalt(II) acetylacetonate was 0.24 g and the amount of 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile) was 0.78 g. The polymerization was terminated at a polymerization rate of 7%, to obtain a vinyl acetate solution of polyvinyl acetate-terminated cobalt complex. Similarly to Example 1, the vinyl acetate solution of the polyvinyl acetate-terminated cobalt complex was added to a solution of 4.85 g of 1,3-diisopropenylbenzene-terminated polyethylene in 200 g of toluene and reacted, and a saponification reaction was carried out similarly to Example 1 to obtain the target block ethylene-modified PVA. The weight average molecular weight was 47,000, the ethylene modification rate was 10 mol %, and the saponification degree was 99 mol %.

[0058] <Comparative Example 1> Vinyl acetate was polymerized in the same manner as in Example 1, and the polymerization was terminated when the polymerization rate reached 22%, and a saponification reaction was carried out in the same manner as in Example 1 without reacting it with 1,3-diisopropenylbenzene-terminated polyethylene to obtain unreacted PVA. The weight average molecular weight was 240,000, the ethylene modification rate was 0 mol%, and the saponification degree was 99 mol%.

[0059] <Comparative Example 2> [Preparation of random ethylene modified PVA] An autoclave was charged with 460 g of vinyl acetate and 75 g of methanol, and the inside of the system was once replaced with nitrogen gas and then replaced with ethylene. The temperature was raised to 67°C while stirring, ethylene was pressurized so that the partial pressure became 1.0 MPa, a solution of 0.82 g of 2,2'-azobisisobutyronitrile dissolved in 10 g of methanol was added, and the internal temperature was maintained at 67°C for 4 hours while stirring, thereby carrying out a polymerization reaction. Thereafter, a solution of 0.082 g of sorbic acid dissolved in 100 g of methanol was added and cooled to terminate the polymerization. Unreacted vinyl acetate was removed by repeatedly removing volatile matter and adding methanol under reduced pressure at 40°C to obtain a methanol solution of random ethylene-modified polyvinyl acetate. The solution was then saponified with sodium hydroxide, washed with methanol, and dried for 8 hours in a hot air dryer at 100°C to obtain a random ethylene-modified PVA with a weight-average molecular weight of 52,000, an ethylene modification rate of 7 mol%, and a degree of saponification of 99 mol%.

[0060] [Table 1]

[0061] As can be seen from the results in Table 1, the water contact angle increases as the ethylene modification rate increases. However, compared to Comparative Example 2, which is a random ethylene-modified PVA, Examples 1 and 2, which are block ethylene-modified PVAs, had larger water contact angles than resins with similar ethylene modification rates, as shown in FIG. 1. Therefore, as shown in FIG. 1, which shows the relationship between the ethylene modification rate and the water contact angle in the examples and comparative examples, it is considered that the block olefin modified PVA of the present invention has a higher affinity with hydrophobic materials than resins having hydrophilic groups to the same extent, such as random ethylene modified PVA. [Industrial Applicability]

[0062] The block olefin-modified PVA of the present invention has excellent affinity with hydrophobic materials while retaining hydrophilic groups, and is therefore expected to be used in a wide range of fields, including medical and industrial applications.

Claims

1. A block olefin-modified polyvinyl alcohol having a structural unit derived from a polyvinyl alcohol resin and a structural unit derived from a polyolefin resin having an α-methylstyrene group.

2. 2. The block olefin-modified polyvinyl alcohol according to claim 1, wherein the polyolefin having an α-methylstyrene group is a polyethylene having an α-methylstyrene group at its terminal.

3. 3. The block olefin-modified polyvinyl alcohol according to claim 2, wherein the content of the ethylene monomer units is 1 to 20 mol % based on the total of the vinyl alcohol monomer units and the ethylene monomer units.

4. The block olefin-modified polyvinyl alcohol according to any one of claims 1 to 3, having a weight average molecular weight of 10,000 to 1,000,000.

5. The present invention relates to a method for producing a block olefin-modified polyvinyl alcohol, which is obtained by saponifying a reaction product of a polyvinyl ester resin obtained by living polymerization with a polyolefin resin having an α-methylstyrene group.

6. 6. The method for producing a block olefin-modified polyvinyl alcohol according to claim 5, wherein the polyvinyl ester resin is a polyvinyl acetate-terminated cobalt complex obtained by living polymerization using a cobalt living control agent.

Citation Information

Patent Citations

  • Hydrophilic polymer alloy, fiber and porous membrane comprising same, and their production

    JP1993202240A

  • Method of immobilizing resin compound in hollow fiber membrane

    JP2015029926A