Rubber composition for tire and tire

The rubber composition addresses the balance of wet grip, warm-up, and breaking strength by using rosin-modified phenolic resin and silica, enhancing tire performance and processability.

JP2024139430AActive Publication Date: 2024-10-09THE YOKOHAMA RUBBER CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023050367
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09
Estimated Expiration
2043-03-27

AI Technical Summary

Technical Problem

Existing tire compositions face challenges in balancing wet grip performance, warm-up performance, breaking strength, and processability, with high filler content leading to decreased breaking strength and increased low temperature hardness, and high softening point resins affecting operability and warm-up performance.

Method used

A rubber composition incorporating 1 to 60 parts by mass of rosin-modified phenolic resin with an acid value less than 30 mgKOH/g and nitrogen adsorption specific surface area of 100-300 m^2/g, along with 30 to 300 parts by mass of silica, enhances compatibility and improves wet grip, warm-up, and breaking strength, while maintaining excellent processability.

Benefits of technology

The composition achieves improved wet grip, warm-up, and breaking strength, with enhanced processability, making it suitable for tire applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139430000001
    Figure 2024139430000001
Patent Text Reader

Abstract

To solve the problem that a tire for traveling on a dry road surface and a tire for traveling on a wet road surface are prepared as a pneumatic tire for racing, an optimal tire is selected according to weather in travel and the state of the road surface, there is a method that a large amount of a filler having a high specific surface area and a resin (high softening point resin) having a high softening point are blended as the tire for racing for traveling on the wet road surface, but abrasion resistance and warm-up performance deteriorate.SOLUTION: A rubber composition for a tire is formed by blending 1 to 60 pts.mass of a rosin-modified phenol resin having an acid value of less than 30 mgKOH / g and 30 to 300 pts.mass of silica having a nitrogen adsorption specific surface area of 100 to 300 m2 / g, with 100 pts.mass of diene-based rubber.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a rubber composition for tires and a tire using the same, and more particularly to a rubber composition for tires which has improved wet grip performance, warm-up performance (grip performance at low temperatures) and breaking strength, and is also excellent in processability, and a tire using the same. [Background technology]

[0002] Generally, tires are required to have a wide range of performance characteristics, and among these, they are required to maintain high levels of grip performance and wear resistance. On the other hand, pneumatic tires for racing are prepared for dry roads and for wet roads, and the optimum tire is selected according to the weather and road conditions during driving. Here, racing tires for wet roads contain a large amount of filler with a high specific surface area and resin with a high softening point (high softening point resin) to improve wet grip performance. However, when a large amount of filler with a high specific surface area is blended, the breaking strength decreases, which deteriorates the abrasion resistance, and when a large amount of resin with a high softening point is blended, the low-temperature hardness increases, which deteriorates the operability and the warm-up performance.

[0003] In addition, the following Patent Document 1 describes a method for producing a rubber composition having a CTAB specific surface area of ​​100 to 400 m with respect to 100 parts by mass of a diene rubber containing a styrene-butadiene copolymer rubber having a glass transition temperature (Tg) of -20°C or higher. 2 This paper discloses a rubber composition for tires, which is obtained by compounding 75 to 200 parts by mass of silica having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more with 5 to 50 parts by mass of a terpene phenol resin having an acid value of 30 mgKOH / g or more and a hydroxyl value of 5 mgKOH / g or more. However, it does not disclose or suggest a rosin-modified phenol resin having an acid value of less than 30 mgKOH / g, which will be described below.

[0004] In addition, when a vulcanizing agent, a vulcanization accelerator, etc. are added to the rubber composition for tires described in Patent Document 1 below and the rubber composition is kneaded, for example, with an open roll, the rubber composition tends to adhere to the roll, and there was a need to improve its processability. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 6791278 Summary of the Invention [Problem to be solved by the invention]

[0006] Therefore, an object of the present invention is to provide a rubber composition for tires which has improved wet grip performance, warm-up performance and breaking strength as well as excellent processability, and a tire using the same. [Means for solving the problem]

[0007] As a result of extensive research, the inventors have discovered that the above-mentioned problems can be solved by blending specific amounts of a rosin-modified phenolic resin having an acid value within a specific range and a silica having a nitrogen adsorption specific surface area (N2SA) within a specific range with a diene-based rubber, and have thus completed the present invention.

[0008] That is, the present invention relates to a rubber composition comprising 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g and a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m per 100 parts by mass of a diene rubber. 2 The present invention provides a rubber composition for tires, which is characterized by comprising 30 to 300 parts by mass of silica having a molecular weight of 1.0 to 1.2 g / g. Effect of the Invention

[0009] The rubber composition for tires of the present invention comprises, per 100 parts by mass of diene rubber, 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g and a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m 2 The rubber composition is characterized by being blended with 30 to 300 parts by mass of silica having a molecular weight of 1.0 to 1.2 g / g. This makes it possible to provide a rubber composition for tires that has improved wet grip performance, warm-up performance, and breaking strength as well as excellent processability, and a tire using the same.

[0010] The rosin-modified phenolic resin used in the present invention has excellent compatibility with diene rubber, and because of its low acid value, it allows the alkaline components in the rubber composition (e.g., vulcanization accelerators) to fully function, improving dry grip performance, warm-up performance and breaking strength. It is also believed that the processability can be improved because the carboxyl groups that act to adhere to metal surfaces are reduced. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will now be described in further detail.

[0012] (Diene rubber) The diene rubber used in the present invention may be any diene rubber that can be blended into a normal rubber composition, such as natural rubber (NR), isoprene rubber (IR), butadiene rubber (BR), styrene-butadiene copolymer rubber (SBR), acrylonitrile-butadiene copolymer rubber (NBR), etc. These may be used alone or in combination of two or more. There are no particular limitations on the molecular weight or microstructure, and the diene rubber may be terminally modified with amine, amide, silyl, alkoxysilyl, carboxyl, hydroxyl, etc., or may be epoxidized. Among these diene rubbers, SBR is preferred in terms of the effects of the present invention. For example, in the case of racing applications, the blending amount of SBR is preferably 80 parts by mass or more, more preferably 100 parts by mass.

[0013] (rosin modified phenolic resin) The rosin modified phenolic resin used in the present invention can be a reaction product of a rosin-based resin, a phenol, formaldehyde and a polyol. Examples of rosin-based resins include unmodified rosins such as gum rosin, tall oil rosin, and wood rosin; polymerized rosins derived from unmodified rosin; disproportionated products or hydrogenated products of unmodified rosin or polymerized rosin; and unsaturated carboxylic acid-modified rosins obtained by reacting unmodified rosin or polymerized rosin with an unsaturated carboxylic acid. Examples of the phenols include phenol; alkylphenols such as methylphenol (cresol), butylphenol, pentylcresol, octylphenol, nonylphenol, decylphenol, dodecylphenol, tetradecylphenol, and hexyldecylphenol; and the like. Examples of formaldehyde include formalin and paraformaldehyde. Examples of polyols include diols such as ethylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, and 3-methyl-1,5-pentanediol; triols such as glycerin, trimethylolpropane, and trimethylolethane; and tetraols such as pentaerythritol, diglycerin, ditrimethylolpropane, and ditrimethylolethane.

[0014] The amounts of the rosin resin, formaldehyde, phenols, and polyol used are not particularly limited, and may be appropriately determined in consideration of, for example, the desired molecular weight, softening point, etc. In addition, the reaction method may be, for example, a method in which the rosin resin, phenols / formaldehyde (condensate), and polyol are charged all at once and reacted, and the reaction temperature is usually about 100 to 300° C., and the reaction time is usually about 1 to 24 hours.

[0015] The rosin-modified phenolic resin used in the present invention must have an acid value adjusted to less than 30 mgKOH / g. The method of adjusting the acid value to less than 30 mgKOH / g is not particularly limited, but a suitable embodiment is, for example, a method of esterifying the rosin-modified phenolic resin prepared as described above or a commercially available rosin-modified phenolic resin (usually having an acid value of 30 mgKOH / g or more) to reduce the acid value to less than 30 mgKOH / g. The esterification may be carried out by a conventional method, using a polyhydric alcohol as the alcohol, and can be carried out at a reaction temperature of 150 to 300°C. Since the use of a dihydric alcohol such as ethylene glycol results in a resin with a low softening point, it is preferable to use a trihydric or higher alcohol. The acid value can be adjusted by the amount of alcohol charged. The rosin-modified phenolic resin prepared by the above suitable embodiment contains an ester bond inside, which increases the compatibility with diene rubber, and further enhances the effect of the rosin-modified phenolic resin. The acid value of the rosin-modified phenolic resin used in the present invention is preferably from 5 to 25 mgKOH / g, and more preferably from 10 to 20 mgKOH / g.

[0016] The rosin-modified phenolic resin used in the present invention preferably has a weight-average molecular weight of 2000 to 5000, more preferably 2500 to 4500, from the viewpoint of further enhancing the effects of the present invention. The softening point is preferably 100 to 160°C, more preferably 110 to 150°C. The weight-average molecular weight in the present invention means a weight-average molecular weight in terms of polystyrene analyzed by gel permeation chromatography (GPC). The softening point is measured in accordance with JIS K6220-1.

[0017] (silica) The silica used in the present invention has a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m 2 / g. Silica's N2SA is 100m 2 If it is less than 1 / g, the wet grip performance is deteriorated, and the breaking strength is reduced, resulting in poor abrasion resistance. Silica's N2SA is also 300m 2 If it exceeds 1 / g, the processability deteriorates. The more preferred N2SA of the silica used in the present invention is 130 to 270 m 2 / g. N2SA shall be measured in accordance with JIS K6217-2.

[0018] (Mixing ratio) The rubber composition of the present invention comprises, per 100 parts by mass of diene rubber, 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g and a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m 2 The silica is blended in an amount of 30 to 300 parts by mass / g. If the amount of the rosin-modified phenolic resin is less than 1 part by mass, the amount is too small to achieve the effects of the present invention, whereas if it exceeds 60 parts by mass, the warm-up performance is reduced and the breaking strength is reduced, resulting in poor wear resistance. The amount of the rosin-modified phenolic resin to be mixed is preferably 5 to 55 parts by mass, and more preferably 10 to 50 parts by mass, based on 100 parts by mass of the diene rubber. The amount of silica added is preferably 50 to 270 parts by mass, and more preferably 70 to 240 parts by mass, based on 100 parts by mass of the diene rubber.

[0019] (Silane coupling agent) From the viewpoint of further improving the effects of the present invention, the rubber composition for tires of the present invention preferably contains 2 to 20 mass % of a silane coupling agent relative to the silica, and it is more preferable that the silane coupling agent be represented by the following composition formula (2). (A) a (B) b (C) c (D) d (R1) e SiO (4-2a-b-c-d-e) / 2 (2) (In formula (2), A represents a divalent organic group containing a sulfide group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, R1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and the relationships 0 ≦ a < 1, 0 < b < 1, 0 < c < 3, 0 ≦ d < 1, 0 ≦ e < 2, and 0 < 2a + b + c + d + e < 4 are satisfied.)

[0020] The silane coupling agent (polysiloxane) represented by formula (2) and a method for producing the same are disclosed, for example, in International Publication WO2014 / 002750 pamphlet and are known.

[0021] In the above formula (2), A represents a divalent organic group containing a sulfide group. Among them, it is preferably a group represented by the following formula (12). * -(CH2) n -S x -(CH2) n - * (12) In the above formula (12), n represents an integer of 1 to 10, and among them, it is preferably an integer of 2 to 4. In the above formula (12), x represents an integer of 1 to 6, and among them, it is preferably an integer of 2 to 4. In the above formula (12), * indicates the bonding position. Specific examples of the group represented by the above formula (12) include, for example, * -CH2-S2-CH2- * 、 * -C2H4-S2-C2H4- * 、 * -C3H6-S2-C3H6- * 、 * -C4H8-S2-C4H8- * 、 * -CH2-S4-CH2- * 、 * -C2H4-S4-C2H4- * 、 * -C3H6-S4-C3H6- * 、 * -C4H8-S4-C4H8- * and the like.

[0022] In the above formula (2), B represents a monovalent hydrocarbon group having 5 to 20 carbon atoms, and specific examples thereof include a hexyl group, an octyl group, a decyl group, etc. B is preferably a monovalent hydrocarbon group having 5 to 10 carbon atoms.

[0023] In the above formula (2), C represents a hydrolyzable group, specific examples of which include an alkoxy group, a phenoxy group, a carboxyl group, an alkenyloxy group, etc. Among these, a group represented by the following formula (13) is preferred. * -OR 2 (13) In the above formula (13), R 2 represents an alkyl group having 1 to 20 carbon atoms, an aryl group having 6 to 10 carbon atoms, an aralkyl group (arylalkyl group) having 6 to 10 carbon atoms, or an alkenyl group having 2 to 10 carbon atoms, and among these, an alkyl group having 1 to 5 carbon atoms is preferable. Specific examples of the alkyl group having 1 to 20 carbon atoms include, for example, a methyl group, an ethyl group, a propyl group, a butyl group, a hexyl group, an octyl group, a decyl group, and an octadecyl group. Specific examples of the aryl group having 6 to 10 carbon atoms include, for example, a phenyl group and a tolyl group. Specific examples of the aralkyl group having 6 to 10 carbon atoms include, for example, a benzyl group and a phenylethyl group. Specific examples of the alkenyl group having 2 to 10 carbon atoms include, for example, a vinyl group, a propenyl group, and a pentenyl group. In the above formula (13), * indicates the bond position.

[0024] In the above formula (2), D represents an organic group containing a mercapto group, and is preferably a group represented by the following formula (14). * -(CH2) m -SH (14) In the above formula (14), m represents an integer of 1 to 10, and among these, an integer of 1 to 5 is preferable. In the above formula (14), * indicates the bond position. Specific examples of the group represented by the above formula (14) include:* -CH2SH, * -C2H4SH, * -C3H6SH, * -C4H8SH, * -C5H 10 SH, * -C6H 12 SH, * -C7H 14 SH, * -C8H 16 SH, * -C9H 18 SH, * -C 10 H 20 SH and the like can be mentioned.

[0025] In the above formula (2), R1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms.

[0026] In the above formula (2), the relationships of 0 ≦ a < 1, 0 < b < 1, 0 < c < 3, 0 ≦ d < 1, 0 ≦ e < 2, and 0 < 2a + b + c + d + e < 4 are satisfied.

[0027] In the above formula (2), a is preferably 0 < a ≦ 0.50 for the reason that the effects of the present invention are improved. In the above formula (2), b is preferably 0 < b, and more preferably 0.10 ≦ b ≦ 0.89 for the reason that the effects of the present invention are improved. In the above formula (2), c is preferably 1.2 ≦ c ≦ 2.0 for the reason that the effects of the present invention are improved. In the above formula (2), d is preferably 0.1 ≦ d ≦ 0.8 for the reason that the effects of the present invention are improved.

[0028] The weight average molecular weight of the above polysiloxane is preferably 500 to 2300, and more preferably 600 to 1500 for the reason that the effects of the present invention are improved. The molecular weight of the above polysiloxane in the present invention is determined in terms of polystyrene by gel permeation chromatography (GPC) using toluene as a solvent. The mercapto equivalent of the polysiloxane as determined by the acetic acid / potassium iodide / potassium iodate addition-sodium thiosulfate solution titration method is preferably 550 to 700 g / mol, and more preferably 600 to 650 g / mol, from the viewpoint of excellent vulcanization reactivity.

[0029] The polysiloxane preferably has 2 to 50 siloxane units (-Si-O-) because this improves the effects of the present invention.

[0030] The polysiloxane skeleton does not contain any metals other than silicon atoms (for example, Sn, Ti, Al).

[0031] The above polysiloxane can be produced by known methods, for example, according to the method disclosed in International Publication WO2014 / 002750.

[0032] It is also possible to use a known silane coupling agent other than the silane coupling agent represented by formula (2), or to use the silane coupling agent represented by formula (2) in combination with another known silane coupling agent.

[0033] (Liquid aromatic vinyl-conjugated diene rubber) The rubber composition for tires of the present invention is preferably blended with a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher. Such liquid aromatic vinyl-conjugated diene rubber can improve wet grip performance and abrasion resistance. In addition, the liquid aromatic vinyl-conjugated diene rubber is compatible with diene rubber and can improve the dispersibility of the rosin-modified phenolic resin used in the present invention, thereby enhancing the effects of the present invention. As the liquid aromatic vinyl-conjugated diene rubber, liquid styrene-butadiene copolymer (liquid SBR) is preferred. The liquid SBR has a weight average molecular weight of 2000 to 40000, preferably 3000 to 20000. The glass transition temperature of the liquid SBR is -40°C or higher, more preferably -20°C to -5°C, as described above. As the liquid SBR, commercially available liquids can be used, such as RICON 100 manufactured by Cray Valley and L-SBR 820 manufactured by Kuraray Co., Ltd. The Tg referred to in the present invention is the midpoint temperature of the transition region measured by differential scanning calorimetry (DSC) at a temperature rise rate of 20°C / min. The liquid aromatic vinyl-conjugated diene rubber used in the present invention is liquid at 23° C. Therefore, it is distinguished from the diene rubber which is solid at this temperature. The amount of the liquid aromatic vinyl-conjugated diene rubber compounded is preferably 5 to 40 parts by mass, and more preferably 10 to 30 parts by mass, per 100 parts by mass of the diene rubber.

[0034] (Other ingredients) In addition to the above-mentioned components, the rubber composition of the present invention may contain various additives that are generally compounded in rubber compositions, such as vulcanizing or crosslinking agents, vulcanizing or crosslinking accelerators, zinc oxide, various fillers such as carbon black, clay, talc, calcium carbonate, and aluminum hydroxide, antioxidants, and plasticizers, and these additives can be kneaded in a general manner to form a composition and used for vulcanization or crosslinking. The amounts of these additives may be conventional general amounts as long as they do not go against the object of the present invention. When aluminum hydroxide is used, it is preferably 10 parts by mass or more, more preferably 15 to 70 parts by mass, per 100 parts by mass of diene rubber.

[0035] The rubber composition of the present invention is suitable for use in tire treads, particularly cap treads, preferably treads for racing tires, particularly cap treads, because it enhances wet grip performance, warm-up performance and breaking strength, and is also excellent in processability. The tire of the present invention is preferably a pneumatic tire, and can be filled with air, an inert gas such as nitrogen, or other gases. EXAMPLES

[0036] The present invention will be further described below with reference to examples and comparative examples, but the present invention is not limited to the following examples.

[0037] Standard Example 1, Examples 1 to 7, and Comparative Examples 1 to 5 Sample preparation In the formulation (parts by mass) shown in Table 1, the components other than the vulcanization accelerator and sulfur were kneaded in a 1.7-liter closed Banbury mixer for 5 minutes, and the rubber was discharged outside the mixer and cooled at room temperature. The rubber was then placed back into the mixer, and the vulcanization accelerator and sulfur were added, followed by further roll kneading to obtain a rubber composition. The obtained rubber composition was then press-vulcanized in a specified mold at 160°C for 20 minutes to obtain a vulcanized rubber test piece, and the physical properties of the vulcanized rubber test piece were measured by the test methods shown below.

[0038] Wet grip performance: In accordance with JIS K6394:2007, tan δ(0°C) was measured using a viscoelasticity spectrometer (manufactured by Toyo Seiki Seisakusho) under conditions of an elongation deformation rate of 10±2%, a vibration frequency of 20 Hz, and a temperature of 0°C. The results were expressed as an index, with Standard Example 1 being 100. A larger index indicates better wet grip performance. Hardness (20° C.): Measured at 20° C. in accordance with JIS K6253. The results are expressed as an index, with the value of Standard Example 1 being 100. A smaller index indicates better warm-up performance. Breaking strength: According to JIS K6251, a No. 3 dumbbell-shaped sample piece was punched out from the vulcanized rubber test piece, and a tensile test was carried out at a tensile speed of 500 mm / min to measure the breaking elongation (%). The results were expressed as an index, with the value of Standard Example 1 being 100. A larger index indicates better breaking strength and better abrasion resistance. Processability: The adhesion during roll kneading was evaluated according to the following criteria. Good: The rubber peels off without applying any force and no rubber remains on the roll. △: You need to use force to peel the rubber off, but no rubber remains on the roll. ×: The rubber needs to be peeled off with force, and some of it remains on the roll. The results are shown in Table 1.

[0039] [Table 1]

[0040] *1: SBR (Nipol NS522 manufactured by ZS Elastomers Co., Ltd.) *2: Silica 1 (Evonik Ultrasil 7000GR (N2SA=171m 2 / g) *3: Silica 2 (Solvay Zeosil 1085GR, N2SA=86m 2 / g) *4: Carbon black (Seast 9, manufactured by Tokai Carbon Co., Ltd.) *5: Aluminum hydroxide (BF013 manufactured by Nippon Light Metal Co., Ltd.) *6: Resin 1 (Yasuhara Chemical Co., Ltd. YS Polystar S145, phenol-modified terpene resin, acid value = 0 mg KOH / g) *7: Resin 2 (Tamanol 803L, rosin-modified phenolic resin, acid value = 52 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *8: Resin 3 (Marquid No. 5, maleic acid modified rosin resin, acid value = 19 mg KOH / g, manufactured by Arakawa Chemical Industries, Ltd.) *9: Resin 4 (Arakawa Chemical Industries, Ltd., Pencel KK, rosin ester resin, acid value = 19 mg KOH / g) *10: Resin 5 (rosin modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. Acid value = 15 mg KOH / g) *11: Resin 6 (rosin modified phenolic resin: reaction product of rosin, phenols, formaldehyde and polyol. Acid value = 17 mg KOH / g) *12: Silane coupling agent 1 (Si69 manufactured by Evonik) *13: Silane coupling agent 2 (a silane coupling agent prepared by the method disclosed in International Publication WO2014 / 002750 and satisfying the composition formula (2) above. Composition formula = (-C3H6-S4-C3H6-) 0.083 (-C8H 17 ) 0.667 (-OC2H5) 1.50 (-C3H6SH) 0.167 SiO 0.75 , average molecular weight=860) *14: Liquid SBR (RICON 100 manufactured by Cray Valley, weight average molecular weight = 6400, Tg = -15℃) *15: Oil (Extract No. 4 S manufactured by Showa Shell Sekiyu K.K.) *16: Stearic acid (Beads Stearic Acid YR manufactured by NOF Corporation) *17: Zinc oxide (3 types of zinc oxide manufactured by Seido Chemical Industry Co., Ltd.) *18: Anti-aging agent (Flexis 6PPD) *19: Vulcanization accelerator 1 (Sansera DG manufactured by Sanshin Chemical Industry Co., Ltd.) *20: Vulcanization accelerator 2 (Noccela CZ-G manufactured by Ouchi Shinko Chemical Industry Co., Ltd.) *21: Sulfur (Kinka-in oil-filled fine sulfur manufactured by Tsurumi Chemical Industry Co., Ltd.)

[0041] From the results in Table 1, the rubber composition of the example contains 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g and a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m relative to 100 parts by mass of diene rubber. 2It was found that, compared with Reference Example 1, the wet grip performance, warm-up performance and breaking strength were improved, and the processability was also excellent. In contrast, in Comparative Example 1, the acid value of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention, and therefore the wet grip performance was deteriorated. Comparative Example 2 was an example in which a maleic acid modified rosin resin was used, and therefore the warm-up performance was deteriorated. Comparative Example 3 is an example in which a rosin ester resin was used, and therefore the wet grip performance and warm-up performance were deteriorated. In Comparative Example 4, the nitrogen adsorption specific surface area (N2SA) of silica was below the lower limit specified in the present invention, and therefore the warm-up performance and breaking strength were deteriorated. In Comparative Example 5, the amount of the rosin-modified phenolic resin exceeded the upper limit specified in the present invention, and therefore the warm-up performance and breaking strength were deteriorated.

[0042] The present disclosure includes the following inventions. Invention [1]: A rubber composition comprising 100 parts by mass of diene rubber, 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g and a nitrogen adsorption specific surface area (N2SA) of 100 to 300 m 2 2. A rubber composition for tires, comprising 30 to 300 parts by mass of silica having a molecular weight of 1 / g. Invention [2]: The silica is further mixed with 2 to 20 mass% of a silane coupling agent, The rubber composition for tires according to Invention 1, wherein the silane coupling agent is represented by the following composition formula (2): (A) a (B) b (C) c (D) d (R1) e SiO (4-2a-b-c-d-e) / 2 (2) (In formula (2), A represents a divalent organic group containing a sulfide group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms; 0≦a<1, 0 <b<1、0<c<3、0≦d<1、0≦e<2、かつ0<2a+b+c+d+e<4の関係を満たす。)Invention [3]: The rubber composition according to Invention 1 or 2, further comprising a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher. Invention [4]: ​​A rubber composition according to any one of Inventions 1 to 3, further comprising 10 parts by mass or more of aluminum hydroxide per 100 parts by mass of the diene rubber. Invention [5]: A tire using the rubber composition for tires according to any one of Inventions 1 to 4 in a cap tread.

Claims

1. A rubber composition according to claim 1, further comprising: 1 to 60 parts by mass of a rosin-modified phenolic resin having an acid value of less than 30 mgKOH / g per 100 parts by mass of diene rubber; and a nitrogen adsorption specific surface area (N 2 SA) is 100 to 300 m 2 30 to 300 parts by mass of silica having a molecular weight of 1 / g are blended in the rubber composition for tires.

2. The silica is further mixed with a silane coupling agent in an amount of 2 to 20% by mass, 2. The rubber composition for tires according to claim 1, wherein the silane coupling agent is represented by the following composition formula (2): (A) a (B) b (C) c (D) d (R1) e SiO (4-2a-b-c-d-e) / 2 (2) (In formula (2), A represents a divalent organic group containing a sulfide group, B represents a monovalent hydrocarbon group having 5 to 10 carbon atoms, C represents a hydrolyzable group, D represents an organic group containing a mercapto group, and R1 represents a monovalent hydrocarbon group having 1 to 4 carbon atoms, and the relationships 0≦a<1, 0<b<1, 0<c<3, 0≦d<1, 0≦e<2, and 0<2a+b+c+d+e<4 are satisfied.)

3. 2. The rubber composition for tires according to claim 1, further comprising a liquid aromatic vinyl-conjugated diene rubber having a glass transition temperature (Tg) of -40°C or higher.

4. 2. The rubber composition for tires according to claim 1, further comprising 10 parts by mass or more of aluminum hydroxide per 100 parts by mass of the diene rubber.

5. A tire using the rubber composition for tires according to claim 1 in a cap tread.

Citation Information

Patent Citations

  • Flame-retardant chlorinated polyethylene waterproof roll and preparation method thereof

    CN110539540A

  • Light-colored low-molecular-weight phenol-modified rosin ester

    JP2002526592A

  • Rubber composition for tire

    JP2009051975A

  • Adhesive tape

    JP2017200978A

  • Rubber composition for tires and pneumatic tire using same

    JP6791278B2