Regenerated styrene resin expanded molding, regenerated expandable styrene resin particle, and regenerate pre-expanded styrene resin particle

By adjusting the Z-average and Z+1 average molecular weights of recycled styrenic resin foam molded products, the mechanical strength is enhanced, making them suitable for various applications, including insulation and packaging.

JP2024139517APending Publication Date: 2024-10-09SEKISUI PLASTICS CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2023050489
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Recycled styrenic resin foam molded products exhibit lower strength compared to those made without using recycled materials, limiting their effectiveness in applications requiring high mechanical strength.

Method used

The solution involves adjusting the Z-average molecular weight (Mz) and Z+1 average molecular weight (Mz+1) of recycled styrenic resin foam molded products to specific ranges, typically between 370,000 to 5 million and 2 million to 15 million, respectively, by incorporating a polymerization process with a peroxyalkyl ester peroxide initiator and controlled addition of styrenic and polyfunctional monomers.

Benefits of technology

This approach results in recycled styrenic resin foam molded products with high mechanical strength, comparable to those made from non-recycled materials, suitable for applications such as insulation and packaging materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139517000001
    Figure 2024139517000001
Patent Text Reader

Abstract

To provide a regenerated expandable styrene resin expanded molding capable of exerting high strength, a regenerate expandable styrene resin particle capable of becoming a raw material of a regenerated expandable styrene resin expanded molding capable of exerting high strength, and a regenerated pre-expanded styrene resin particle capable of becoming a raw material of a regenerated expandable styrene resin expanded molding capable of exerting high strength.SOLUTION: A regenerated styrene resin expanded molding by an embodiment of the present invention is a regenerated styrene resin expanded molding molded from a regenerated pre-expanded styrene resin particle constituted by pre-expanding the regenerated expandable styrene resin particle, where the Z-average molecular weight Mz is 370,000-5,000,000, and the Z+1 average molecular weight Mz+1 is 2,000,000-15,000,000.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to recycled styrene-based resin foamed molded articles, recycled expandable styrene-based resin particles, and recycled pre-expanded styrene-based resin particles. [Background technology]

[0002] Since foamed molded articles are lightweight and have excellent heat insulating properties and mechanical strength, they are widely used as heat insulating materials for houses and automobiles, heat retaining materials for building materials, embankment materials for polystyrene foam civil engineering, transport packaging materials for fish boxes and food containers, cushioning materials, etc. Among them, in-mold foamed molded articles manufactured from expandable particles (typically expandable polystyrene-based resin particles or pre-expanded styrene-based resin particles obtained by pre-expanding them) are widely used because of the advantage that they are easy to obtain the desired shape. Such foamed molded articles are composed of a plurality of expandable particles fused to each other.

[0003] On the other hand, the amount of plastic waste is increasing year by year. Most plastic waste is disposed of by incineration or landfilling, but it has become a major social problem, such as environmental pollution, global warming, and a lack of landfill sites. For this reason, there is a strong social demand for the reuse of plastic waste, and various methods for recycling plastic waste are being considered, such as with the enforcement of the Home Appliance Recycling Law. Among the various recycling methods proposed, material recycling, in which plastic waste is reused as plastic components of products, has attracted attention from the viewpoints of resource circulation and reducing environmental load, and such material recycling is also being considered for styrene resin foam moldings.

[0004] As a material recycling method for styrene-based resin foam moldings, several methods have been proposed for producing recycled expandable styrene-based resin particles, which are obtained by melting and extruding recovered raw materials to form recovered pellets, and then impregnating the pellets with a foaming agent.

[0005] Methods have been reported for obtaining recycled expandable styrene resin particles by impregnating or pressurizing and then impregnating recycled resin pellets molded from recovered styrene resin foam molded products with a blowing agent (Patent Documents 1 to 4). Also, methods have been reported for obtaining recycled expandable styrene resin particles by adding styrene monomer to recycled resin pellets molded from recovered styrene resin foam molded products, polymerizing the pellets, and then impregnating or pressurizing and then impregnating the pellets with a blowing agent (Patent Documents 5 to 8).

[0006] However, recycled styrene-based resin foamed moldings produced using such recycled expandable styrene-based resin particles have the problem that they have lower strength than foamed styrene-based resin moldings produced without using recycled raw materials. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Patent No. 3044942 [Patent Document 2] Patent No. 4234832 [Patent Document 3] Patent No. 4261676 [Patent Document 4] Patent No. 6788428 [Patent Document 5] Patent No. 4052193 [Patent Document 6] JP 2006-160905 A [Patent Document 7] Patent No. 4912567 [Patent Document 8] Patent No. 5128246 [Patent Document 9] JP 2007-211230 A Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above-mentioned problems in the conventional art, and an object of the present invention is to provide a recycled expandable styrene-based resin foam molded product capable of exhibiting high strength, to provide recycled expandable styrene-based resin particles that can be used as a raw material for recycled expandable styrene-based resin foam molded products capable of exhibiting high strength, and to provide recycled pre-expanded styrene-based resin particles that can be used as a raw material for recycled expandable styrene-based resin foam molded products capable of exhibiting high strength. [Means for solving the problem]

[0009] The present inventors have conducted intensive studies to solve the above problems. As a result, it has been found that the mass average molecular weight Mw of the recycled styrene-based resin foamed molding is not significantly reduced, while the Z average molecular weight Mz and the Z+1 average molecular weight Mz+1 are significantly reduced, compared to the mass average molecular weight Mw of the styrene-based resin foamed molding that does not use recycled raw materials. The Z average molecular weight Mz and the Z+1 average molecular weight Mz+1 are average molecular weights that emphasize the influence of high molecular weight components, and the Z+1 average molecular weight Mz+1 is an average molecular weight that particularly emphasizes the influence of high molecular weight components, compared to the mass average molecular weight Mw. Therefore, the inventors have focused on the Z average molecular weight Mz and the Z+1 average molecular weight Mz+1 of the recycled styrene-based resin foamed molding, particularly the Z+1 average molecular weight Mz+1, and further studied how to adjust them to a predetermined range. As a result, a recycled styrene-based resin foamed molding in which the Z average molecular weight Mz and the Z+1 average molecular weight Mz+1 are both large values ​​within a predetermined range has been completed, and this recycled styrene-based resin foamed molding has been able to solve the above problems. Furthermore, the present inventors have also perfected recycled expandable styrene-based resin particles and recycled pre-expanded styrene-based resin particles which can be used as raw materials for such recycled styrene-based resin foamed moldings.

[0010] [1] The recycled styrene-based resin foamed molded product according to an embodiment of the present invention is a recycled styrene-based resin foamed molded product molded from recycled pre-expanded styrene-based resin particles obtained by pre-expanding recycled expandable styrene-based resin particles, and has a Z-average molecular weight Mz of 370,000 to 5,000,000 and a Z+1 average molecular weight Mz+1 of 2,000,000 to 15,000,000. [2] The recycled styrene-based resin foam molded article according to the above item [1] may have an average maximum bending strength of 0.33 MPa or more. [3] In the recycled styrene-based resin foamed molding described in [1] or [2] above, the recycled expandable styrene-based resin particles may be obtained by injecting and impregnating a blowing agent into recycled styrene-based resin particles (A) obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing the mixture in the presence of a polymerization initiator. [4] In the recycled styrene-based resin foamed molding described in [3] above, the ratio of the amount of the recycled styrene-based resin raw material particles (a) to the total amount of the recycled styrene-based resin raw material particles (a) and the styrene-based monomer may be 50 mass% or more. [5] In the recycled styrene-based resin foamed molded article according to the above [3] or [4], the polymerization initiator may contain a peroxyalkyl ester-based peroxide having a 10-hour half-life temperature of 65°C or higher. [6] In the recycled styrene-based resin foam molded product according to any one of [3] to [5] above, the content of the polyfunctional monomer per 100 parts by mass of the styrene-based monomer may be 0.001 to 0.049 parts by mass. [7] The recycled expandable styrene-based resin particles according to an embodiment of the present invention are obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a), polymerizing the mixture in the presence of a polymerization initiator to produce recycled styrene-based resin particles (A), and then injecting and impregnating the recycled styrene-based resin particles with a blowing agent. The recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles give a recycled styrene-based resin foamed molding having a Z-average molecular weight Mz of 370,000 to 5,000,000 and a Z+1 average molecular weight Mz+1 of 2,000,000 to 15,000,000. [8] In the recycled expandable styrene-based resin particles described in [7] above, the polymerization initiator may contain a peroxyalkyl ester-based peroxide having a 10-hour half-life temperature of 65°C or higher. [9] In the recycled expandable styrene-based resin particles according to the above [7] or [8], the content of the polyfunctional monomer per 100 parts by mass of the styrene-based monomer may be 0.001 to 0.049 parts by mass.

[10] The recycled pre-expanded styrene-based resin particles according to an embodiment of the present invention are obtained by pre-expanding the recycled expandable styrene-based resin particles described in any one of [7] to [9] above. Effect of the Invention

[0011] According to the present invention, it is possible to provide recycled expandable styrene-based resin foam molded products capable of exhibiting high strength, recycled expandable styrene-based resin particles that can be used as a raw material for recycled expandable styrene-based resin foam molded products capable of exhibiting high strength, and recycled pre-expanded styrene-based resin particles that can be used as a raw material for recycled expandable styrene-based resin foam molded products capable of exhibiting high strength. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, embodiments of the present invention will be described, but the present invention is not limited to these embodiments.

[0013] In this specification, "(meth)acrylic" means acrylic and / or methacrylic, and "(meth)acrylate" means acrylate and / or methacrylate.

[0014] <<A. Recycled styrene resin foam molding>> The recycled styrene-based resin foamed molded article according to the embodiment of the present invention is molded from recycled pre-expanded styrene-based resin particles obtained by pre-expanding recycled expandable styrene-based resin particles.

[0015] The recycled styrene-based resin foamed molded article typically contains recycled expandable styrene-based resin particles (hereinafter sometimes simply referred to as "expanded particles") obtained by further expanding recycled pre-expanded styrene-based resin particles.

[0016] A recycled styrene-based resin foamed molded article is typically composed of a plurality of foamed particles fused to one another.

[0017] The recycled styrene-based resin foam molded article according to the embodiment of the present invention has a Z-average molecular weight Mz of 370,000 to 5,000,000, preferably 370,000 to 4,500,000, and more preferably 370,000 to 4,000,000.

[0018] The recycled styrene-based resin foam molded article according to the embodiment of the present invention has a Z+1 average molecular weight Mz+1 of 2 million to 15 million, preferably 2 million to 12 million, and more preferably 2 million to 10 million.

[0019] The recycled styrene-based resin foamed moldings according to the embodiments of the present invention can exhibit high strength equivalent to that of styrene-based resin foamed moldings produced without using recycled raw materials by adjusting the Z-average molecular weight Mz and the Z+1-average molecular weight Mz+1 to be within the above ranges.

[0020] The recycled styrene-based resin foam molded product according to the embodiment of the present invention can exhibit an average maximum bending strength equivalent to that of a styrene-based resin foam molded product manufactured without using recycled raw materials. The recycled styrene-based resin foam molded product according to the embodiment of the present invention has a density of, for example, 0.0167 g / cm 3 In the case of the flexural strength, the average maximum bending strength is preferably 0.33 MPa or more, more preferably 0.34 MPa or more, further preferably 0.35 MPa or more, and particularly preferably 0.36 MPa or more. The upper limit of the average maximum bending strength is preferably as high as possible, but in reality, it is typically 0.37 MPa or less.

[0021] The recycled styrene-based resin foam molded article can be typically produced by charging recycled pre-expanded styrene-based resin particles into a mold having a predetermined shape according to the purpose and performing in-mold foam molding. More specifically, in-mold foam molding includes (i) filling recycled pre-expanded styrene-based resin particles into a closed mold having a large number of small holes, (ii) heating and foaming the recycled pre-expanded styrene-based resin particles with a heat medium (e.g., pressurized steam, etc.) to obtain foamed particles, and (iii) filling the voids between the foamed particles by the heating and foaming, and fusing the foamed particles together to integrate them. The density of the recycled styrene-based resin foam molded article can be appropriately set according to the purpose. The density of the recycled styrene-based resin foam molded article can be adjusted, for example, by previously adjusting the bulk expansion ratio of the pre-expanded styrene-based resin particles filled in the mold, or by adjusting the amount of recycled pre-expanded styrene-based resin particles filled in the mold.

[0022] The heat-foaming temperature (substantially the temperature of the heat transfer medium) is preferably 90°C to 150°C, more preferably 110°C to 130°C. The heat-foaming time is preferably 5 seconds to 50 seconds, more preferably 10 seconds to 50 seconds. The molding vapor pressure of the heat-foaming (gauge pressure of the heat transfer medium blowing in) is preferably 0.04 MPa to 0.1 MPa, more preferably 0.06 MPa to 0.08 MPa. If the heat-foaming is performed under such conditions, the expanded particles can be well fused to each other.

[0023] If necessary, the recycled pre-expanded styrene resin particles may be aged before molding into a recycled styrene resin foamed molded article. The aging temperature of the recycled pre-expanded styrene resin particles is preferably 20°C to 60°C. If the aging temperature is too low, an excessively long aging time may be required. If the aging temperature is too high, the blowing agent in the recycled pre-expanded styrene resin particles may dissipate, resulting in a decrease in moldability.

[0024] The expansion ratio of the expanded beads in the recycled styrene-based resin foamed molded product is preferably 2 times or more and less than 110 times, more preferably 5 times to 90 times, further preferably 10 times to 85 times, and particularly preferably 15 times to 80 times.

[0025] The recycled styrene-based resin foam molded product according to the embodiment of the present invention is lightweight and has excellent heat insulation properties and mechanical strength, and is therefore suitable for use as wall insulation material, floor insulation material, roof insulation material, automobile insulation material, heat insulation material for hot water tanks, heat insulation material for piping, heat insulation material for solar systems, heat insulation material for water heaters, containers for food and industrial products (e.g., food containers such as fish boxes, return boxes), cushioning material, floats, blocks, packaging material for fish and agricultural products, etc., molded bodies for embankments, core material for tatami mats, core material for cushions, aggregate for concrete, etc.

[0026] The recycled pre-expanded styrene resin particles are obtained by expanding the recycled expandable styrene resin particles to a desired bulk expansion ratio (bulk density) using water vapor or the like. The bulk expansion ratio of the recycled pre-expanded styrene resin particles is preferably 2 to 150 times, more preferably 2 to less than 100 times, more preferably 5 to 90 times, even more preferably 10 to 85 times, and particularly preferably 15 to 83 times. The bulk density is the reciprocal of the bulk expansion ratio. By having the bulk expansion ratio of the recycled pre-expanded styrene resin particles within the above range, blocking during expansion and molding can be more effectively prevented, and further, the electrostatic charge during expansion and molding can be suppressed while exhibiting better fusion properties and surface properties, and a recycled styrene resin foam molded article with less static electricity can be molded.

[0027] The recycled expandable styrene-based resin particles are preferably obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing the mixture in the presence of a polymerization initiator to obtain recycled styrene-based resin particles (A), from the viewpoint of being able to more effectively exert the effects of the present invention, and then pressurizing and impregnating the particles with a blowing agent.

[0028] The recycled styrene-based resin particles (A) are obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing them in the presence of a polymerization initiator.

[0029] The recycled styrene-based resin raw material particles (a) may be of one type only, or of two or more types.

[0030] As the material for the recycled styrene-based resin raw material particles (a), any suitable recycled styrene-based resin can be used within the scope that does not impair the effects of the present invention. Examples of such recycled styrene-based resins include recycled products of plastic materials used in polystyrene foam (molded products, block molded products, etc.), foam sheets (tray containers, broken sheets, etc.), home appliances, packaging containers, cushion beads, etc.

[0031] The recycled styrene-based resin raw material particles (a) may contain any suitable recycled resin other than the recycled styrene-based resin, as long as the effect of the present invention is not impaired. Examples of such other recycled resins include recycled resins of AS resin, ABS resin, HIPS (high impact polystyrene); polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), and polycarbonate (PC); polyamide resins such as nylon (PA); and polyolefin resins such as polyethylene (linear low density polyethylene (LLDPE), low density polyethylene (LDPE), high density polyethylene (HDPE), polypropylene (PP), and EVA (ethylene-vinyl acetate copolymer). The other resins may be one type or two or more types. In this specification, the above-mentioned recycled resins of AS resin, ABS resin, and HIPS (high impact polystyrene) are not included in the category of the above-mentioned recycled styrene-based resins.

[0032] As the recycled styrene-based resin raw material particles (a), molded products made from products under the trade names "EPSREM" and "ESLENE BEAD RNW" manufactured by Sekisui Plastics Co., Ltd. may be used.

[0033] The recycled styrene-based resin raw material particles (a) may be a pulverized product obtained by pulverizing a recycled resin obtained by heating and / or reducing the volume of a used expanded styrene-based resin. The recycled styrene-based resin raw material particles may be pelletized by extrusion molding the pulverized product, or may be pelletized by further pulverizing the pellets. Alternatively, the recycled styrene-based resin raw material particles may be a reduced-volume recovered product using a solvent such as limonene.

[0034] The recycled styrene resin raw material particles (a) are preferably pellets obtained by melt extrusion, which is a method in which crushed products, ingots, foamed particles, etc. of used styrene resin are fed to a resin feeder, melted in the resin feeder, extruded from small holes in a die attached to the tip of the resin feeder, and then cooled to obtain pellets.

[0035] The pellets obtained by the melt extrusion method are preferably at least one type selected from extruded strand pellets obtained by extruding used expanded styrene-based resin with an extruder and strand cutting it, underwater cut pellets obtained by an underwater cutting method in which used expanded styrene-based resin is extruded with an extruder and simultaneously cut in water, and hot cut pellets obtained by a hot cutting method in which used expanded styrene-based resin particles are cut and cooled immediately after coming out of the die of an extruder.

[0036] As the recycled styrene-based resin raw material particles (a), the pellets obtained by the above-mentioned melt extrusion method may be used as they are, or they may be made into so-called "mini-pellets" by melt extrusion or the like again to obtain pellets of smaller size.

[0037] The recycled styrene-based resin raw material particles (a) may be a shrinkage or molten product of a styrene-based resin that is obtained by coarsely crushing used styrene-based resin into an appropriate size as necessary, and then subjecting the resin to heat shrinkage, bubble destruction shrinkage due to compression, shrinkage due to frictional heat, melting, or the like.

[0038] Examples of used expanded styrene resin include molded products obtained by molding expandable styrene resin into a mold and products obtained by heating and expanding the molded products.

[0039] The recycled styrene-based resin raw material particles (a) may contain finely powdered inorganic substances and / or organic lubricants, which typically function as cell regulators.

[0040] Examples of fine powder inorganic substances include talc, calcium carbonate, and silica. Here, talc typically refers to a mixture mainly composed of silicon oxide and magnesium oxide, and containing trace amounts of aluminum oxide, iron oxide, etc.

[0041] The average particle size of the finely powdered inorganic material is preferably 100 μm or less, and more preferably 30 μm or less.

[0042] The content of the fine powder inorganic material is preferably 0.1 to 5% by mass, and more preferably 0.5 to 2% by mass, relative to the recycled styrene-based resin raw material particles (a).

[0043] Examples of organic lubricants include liquid paraffin; polyethylene glycol; silicone oils such as dimethylpolysiloxane, methylphenylpolysiloxane, and methylhydrogenpolysiloxane; higher fatty acid bisatomids such as methylene bisstearylamide, ethylene bisstearylamide, and ethylene bisoleic acid amide; and metal salts of higher fatty acids such as zinc stearate, magnesium stearate, and zinc oleate.

[0044] The content of the organic lubricant relative to the recycled styrene-based resin raw material particles (a) is preferably 0.01% by mass to 2.0% by mass, more preferably 0.02% by mass to 1.8% by mass, and in some cases, even more preferably 0.02% by mass to 0.2% by mass, and particularly preferably 0.02% by mass to 0.1% by mass.

[0045] A specific method for including a fine powder inorganic substance and / or an organic lubricant in the recycled styrene-based resin raw material particle (a) is, for example, a method of kneading a fine powder inorganic substance and / or an organic lubricant during extrusion molding. In this case, it is preferable to mix the pulverized material and the bubble regulator in advance, and then extrusion molding. The method for mixing the pulverized material and the bubble regulator can be any appropriate method within a range that does not impair the effects of the present invention. Examples of such methods include a mixing method using a mixer such as a tumbler, a ribbon blender, a V blender, a Henschel mixer, or a Redigay mixer.

[0046] The recycled styrene-based resin raw material particles (a) are preferably thermally melted for the purpose of adjusting the specific gravity. In this step, the specific gravity of the recycled styrene-based resin raw material particles (a) is preferably adjusted to 0.6 or more, more preferably adjusted to 0.9 or more. If the specific gravity of the recycled styrene-based resin raw material particles (a) is less than 0.6, the dispersion of the recycled styrene-based resin raw material particles (a) is unstable, so that excessively large particles may be generated during the subsequent polymerization step, resulting in a reduced yield. The recycled styrene-based resin raw material particles (a) may be thermally melted by any appropriate method within a range that does not impair the effects of the present invention. Examples of such methods include a method using an extruder or a heat roll. It is preferable that the thermal melting is performed by cooling and solidifying the resin obtained in a state in which no distortion remains in the resin obtained or in a state in which the distortion is small. If distortion remains in the resin particles, the distortion may be relaxed in the subsequent step, causing the particles to shrink in the stretching direction, and the resulting recycled expandable styrene-based resin particles may become flat rather than spherical. Therefore, it is preferable to use an extruder for the thermal melting without stretching. If the thermal melting is performed in a stretched state, there is a risk that distortion will remain in the stretched resin obtained by cooling and solidifying. Even if distortion remains in the resin due to thermal melting, it is possible to alleviate the distortion by curing the resin for a certain period of time at a temperature above the softening point of the resin.

[0047] For the pulverization to obtain the recycled styrene-based resin raw material particles (a), any pulverizer can be used as long as it does not impair the effects of the present invention. As such a pulverizer, for example, a pulverizer for plastics can be used, and a pulverizer for polystyrene is preferable.

[0048] The recycled styrene-based resin raw material particles (a) can be sieved as necessary and subjected to melting again in an extruder or the like.

[0049] The shape of the recycled styrene-based resin raw material particle (a) can be any suitable shape as long as it is particulate, and examples of such shapes include cylindrical, spherical, approximately spherical, elliptical (egg-shaped), etc. In reality, it is difficult to distinguish between spherical and approximately spherical, so in this specification, both are collectively referred to as spherical.

[0050] The average particle diameter of the recycled styrene-based resin raw material particles (a) is preferably 0.2 mm to 3.0 mm, more preferably 0.3 mm to 2.5 mm, further preferably 0.4 mm to 2.0 mm, and particularly preferably 0.5 mm to 1.7 mm. If the average particle diameter of the recycled styrene-based resin raw material particles (a) exceeds 3 mm, the shape of the resulting recycled expandable styrene-based resin particles may be difficult to become spherical. If the average particle diameter of the recycled styrene-based resin raw material particles (a) is less than 0.2 mm, the average particle diameter of the resulting recycled expandable styrene-based resin particles may be too small.

[0051] The L (long side) / D (short side) of the recycled styrene-based resin raw material particle (a) is preferably 1.0 to 6.0, more preferably 1.0 to 5.0, even more preferably 1.0 to 4.0, particularly preferably 1.0 to 3.0, and most preferably 1.0 to 2.5. If the L (long side) / D (short side) of the recycled styrene-based resin raw material particle (a) is out of the above range, the shape of the obtained recycled expandable styrene-based resin particles may be difficult to become spherical.

[0052] The recycled styrene-based resin raw material particles (a) preferably have a content of particles with an average particle size of 200 μm or less of less than 1 mass %. Recycled styrene-based resin raw material particles (a) having a content of particles with an average particle size of 200 μm or less of 1 mass % or more may deteriorate the appearance of the recycled expandable styrene-based resin particles obtained using the recycled styrene-based resin raw material particles (a).

[0053] The mass average molecular weight Mw of the recycled styrene-based resin raw material particles (a) is preferably 100,000 to 510,000, and more preferably 150,000 to 490,000. If the mass average molecular weight Mw of the recycled styrene-based resin raw material particles (a) is less than 100,000, sufficient strength may not be obtained. If the mass average molecular weight Mw of the recycled styrene-based resin raw material particles (a) is more than 510,000, the recycled styrene-based resin raw material particles may not be easily spherical, or the foaming property may decrease, resulting in poor appearance of the molded product.

[0054] Even if the Z-average molecular weight Mz of the recycled styrene-based resin raw material particles (a) used as a raw material of the recycled styrene-based resin foamed molded product according to the embodiment of the present invention is small, the Z-average molecular weight Mz of the finally obtained recycled styrene-based resin foamed molded product can be in the above-mentioned range. When providing the recycled styrene-based resin foamed molded product according to the embodiment of the present invention, the Z-average molecular weight Mz of the recycled styrene-based resin raw material particles (a) may be, for example, 500,000 or less, or 400,000 or less.

[0055] Even if the Z+1 average molecular weight Mz+1 of the recycled styrene-based resin raw material particles (a) used as a raw material of the recycled styrene-based resin foamed molded product according to the embodiment of the present invention is small, the Z+1 average molecular weight Mz+1 of the finally obtained recycled styrene-based resin foamed molded product can be in the above-mentioned range. When providing the recycled styrene-based resin foamed molded product according to the embodiment of the present invention, the Z+1 average molecular weight Mz+1 of the recycled styrene-based resin raw material particles (a) may be, for example, less than 2 million, 1.5 million or less, 1 million or less, or 800,000 or less.

[0056] The styrene-based monomer may be of only one type, or of two or more types.

[0057] The styrene monomer includes styrene or a styrene derivative. Examples of the styrene derivative include α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, and bromostyrene. The styrene monomer may be one type or two or more types. The styrene monomer preferably contains at least styrene. The content ratio of styrene to the total amount of the styrene monomer is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 90% by mass or more, and particularly preferably 95% by mass or more.

[0058] The polyfunctional monomer may be of only one kind, or of two or more kinds.

[0059] The content ratio of the polyfunctional monomer relative to the styrene-based monomer is preferably 0.001 mass% to 0.049 mass%, more preferably 0.003 mass% to 0.045 mass%, further preferably 0.005 mass% to 0.040 mass%, and particularly preferably 0.007 mass% to 0.035 mass%.

[0060] Specific examples of polyfunctional monomers include divinylbenzenes such as o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene; and alkylene glycol di(meth)acrylates such as ethylene glycol di(meth)acrylate and polyethylene glycol di(meth)acrylate. Specific examples of (meth)acrylic acid ester monomers include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, and hexyl (meth)acrylate. Examples of maleic acid ester monomers include dimethyl maleate. Examples of fumaric acid ester monomers include dimethyl fumarate, diethyl fumarate, and ethyl fumarate.

[0061] Among the polyfunctional monomers, divinylbenzene is preferred in that it can more effectively exert the effects of the present invention. Note that divinylbenzene exists as three positional isomers, namely o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene, and in the present invention, any combination of divinylbenzenes of these positional isomers may be used.

[0062] The polyfunctional monomer may be added to the suspension separately from the styrene-based monomer, or may be added together with the styrene-based monomer. When the polyfunctional monomer is added to the suspension together with the styrene-based monomer, typically the polyfunctional monomer is dissolved in the styrene-based monomer and added.

[0063] In the polymerization, the suspension containing the recycled styrene-based resin raw material particles (a) may contain any suitable vinyl monomer other than the styrene-based monomer and the polyfunctional monomer. Such vinyl monomers may be one type only or two or more types. Examples of such vinyl monomers include (meth)acrylic acid ester monomers, maleic acid ester monomers, and fumaric acid ester monomers.

[0064] The vinyl monomer may be added to the suspension separately from the styrenic monomer or together with the styrenic monomer. When the vinyl monomer is added to the suspension together with the styrenic monomer, the vinyl monomer is typically dissolved in the styrenic monomer before addition.

[0065] The ratio of the amount of the recycled styrene-based resin raw material particles (a) to the total amount of the recycled styrene-based resin raw material particles (a) and the styrene-based monomer is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more. The higher the ratio, the higher the recycling rate of the raw material and the higher the environmental contribution.

[0066] The higher the upper limit value of the ratio of the amount of the recycled styrene resin raw material particles (a) to the total amount of the recycled styrene resin raw material particles (a) and the styrene monomer, the higher the recycling rate of the raw material and the higher the environmental contribution, but if the styrene monomer is not used in a predetermined amount or more, the effect of the present invention may not be realized. Therefore, the upper limit value of the ratio of the amount of the recycled styrene resin raw material particles (a) to the total amount of the recycled styrene resin raw material particles (a) and the styrene monomer is preferably less than 98 mass%, more preferably 95 mass% or less, even more preferably 94 mass% or less, particularly preferably 93 mass% or less, and most preferably 92 mass% or less.

[0067] The recycled styrene-based resin particles (A) are obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing them in the presence of a polymerization initiator. Any appropriate method can be adopted as the polymerization method as long as it does not impair the effects of the present invention. A preferred embodiment of such a polymerization method is a method in which a polymerization initiator, a styrene-based monomer, and a polyfunctional monomer are added to a suspension obtained by dispersing recycled styrene-based resin raw material particles (a) as nuclei in an aqueous medium, and polymerization is carried out.

[0068] When dispersing the recycled styrene-based resin raw material particles (a) as nuclei in an aqueous medium to obtain a suspension, any suitable method can be adopted as a method for dispersing the recycled styrene-based resin raw material particles (a) in an aqueous medium, as long as it does not impair the effects of the present invention. As a method for such dispersion, a preferred method is dispersion using a device equipped with stirring blades. As a method for more fine dispersion, a method using a homomixer can be mentioned.

[0069] When dispersing the recycled styrene-based resin raw material particles (a) as nuclei in an aqueous medium to obtain a suspension, it is preferable to use a dispersant in dispersing the recycled styrene-based resin raw material particles (a) in the aqueous medium. Any suitable dispersant can be used as long as it can be used in suspension polymerization, as long as it does not impair the effects of the present invention. Examples of such dispersants include organic dispersants such as polyvinyl alcohol, polyvinylpyrrolidone, and methylcellulose; and poorly soluble inorganic salts such as magnesium pyrophosphate and calcium triphosphate. Among these, magnesium pyrophosphate is preferred as the dispersant in that it can further express the effects of the present invention.

[0070] The blending ratio of the dispersant per 100 parts by mass of the recycled styrene-based resin particles (A) is preferably 0.1 to 2 parts by mass, more preferably 0.1 to 1.5 parts by mass, and even more preferably 0.1 to 1.0 part by mass.

[0071] When dispersing the recycled styrene-based resin raw material particles (a) as nuclei in an aqueous medium to obtain a suspension, it is preferable to use a surfactant in dispersing the recycled styrene-based resin raw material particles (a) in the aqueous medium. Any appropriate surfactant may be used as long as it can be used in suspension polymerization, as long as it does not impair the effects of the present invention. Examples of such surfactants include sodium dodecylbenzenesulfonate, sodium alkanesulfonate, sodium alkylsulfonate, sodium alkyldiphenyletherdisulfonate, and sodium α-olefinsulfonate. Among these, sodium dodecylbenzenesulfonate is preferable as the surfactant in that it can further express the effects of the present invention.

[0072] The blending ratio of the surfactant per 100 parts by mass of the recycled styrene-based resin particles (A) is preferably 0.005 parts by mass to 0.1 parts by mass, more preferably 0.005 parts by mass to 0.08 parts by mass, and even more preferably 0.005 parts by mass to 0.06 parts by mass.

[0073] The polymerization initiator may be of only one type, or of two or more types.

[0074] The polymerization initiator is preferably added after being dissolved in a styrene monomer or a solvent. Examples of the solvent include aromatic hydrocarbons such as ethylbenzene and toluene; and aliphatic hydrocarbons such as heptane and octane. When a solvent is used, it is usually used in an amount of 10% by mass or less based on the styrene monomer.

[0075] The polymerization initiator preferably contains a peroxyalkyl ester-based peroxide having a 10-hour half-life temperature of 65° C. or higher, in that the effects of the present invention can be more effectively exhibited.

[0076] Examples of peroxyalkyl ester peroxides having a 10-hour half-life temperature of 65° C. or higher include 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (10-hour half-life temperature=65.3° C.), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (10-hour half-life temperature=66.2° C.), t-hexylperoxy-2-ethylhexanoate (10-hour half-life temperature=69.9° C.), t-butylperoxy-2-ethylhexanoate (10-hour half-life temperature=72.1° C.), and t-butylperoxybenzoate (10-hour half-life temperature=104.3° C.).

[0077] Examples of peroxyalkyl ester peroxides having a 10-hour half-life temperature of 65° C. or higher include, in addition to the compounds exemplified above, known compounds described in literature such as NOF Corporation's catalog "Organic Peroxides (10th Edition)."

[0078] The amount of peroxyalkyl ester peroxide having a 10-hour half-life temperature of 65°C or higher used is preferably 0.011 mass% to 1.50 mass%, more preferably 0.055 mass% to 1.00 mass%, even more preferably 0.09 mass% to 0.60 mass%, particularly preferably 0.15 mass% to 0.50 mass%, and most preferably 0.20 mass% to 0.44 mass%, relative to the styrene monomer, in terms of further exhibiting the effects of the present invention.

[0079] The polymerization initiator preferably contains a peroxyalkyl ester peroxide having a 10-hour half-life temperature of 65° C. to 75° C., in order to further exert the effects of the present invention. Examples of peroxyalkyl ester peroxides having a 10-hour half-life temperature of 65° C. to 75° C. include 1,1,3,3-tetramethylbutylperoxy-2-ethylhexanoate (10-hour half-life temperature=65.3° C.), 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane (10-hour half-life temperature=66.2° C.), t-hexylperoxy-2-ethylhexanoate (10-hour half-life temperature=69.9° C.), and t-butylperoxy-2-ethylhexanoate (10-hour half-life temperature=72.1° C.).

[0080] The amount of the peroxyalkyl ester peroxide having a 10-hour half-life temperature of 65°C to 75°C used is preferably 0.01% by mass to 1.00% by mass, more preferably 0.05% by mass to 0.70% by mass, even more preferably 0.08% by mass to 0.40% by mass, particularly preferably 0.10% by mass to 0.35% by mass, and most preferably 0.12% by mass to 0.32% by mass, relative to the styrene monomer.

[0081] As the polymerization initiator, in order to further exert the effects of the present invention, it is preferable to use a peroxyalkyl ester peroxide having a 10-hour half-life temperature of 65° C. to 75° C. in combination with a peroxyalkyl ester peroxide having a 10-hour half-life temperature of 100° C. to 110° C. An example of a peroxyalkyl ester peroxide having a 10-hour half-life temperature of 100° C. to 110° C. is t-butyl peroxybenzoate (10-hour half-life temperature=104.3° C.).

[0082] The amount of the peroxyalkyl ester peroxide having a 10-hour half-life temperature of 100°C to 110°C used is preferably 0.001% by mass to 0.50% by mass, more preferably 0.005% by mass to 0.30% by mass, even more preferably 0.01% by mass to 0.20% by mass, particularly preferably 0.05% by mass to 0.15% by mass, and most preferably 0.08% by mass to 0.12% by mass, based on the styrene monomer.

[0083] When obtaining the recycled styrene-based resin particles (A), the addition temperature when adding the styrene-based monomer to the suspension containing the recycled styrene-based resin raw material particles (a) is preferably 40 ° C. to 119 ° C., more preferably 40 ° C. to 118 ° C., even more preferably 40 ° C. to 117 ° C., particularly preferably 50 ° C. to 117 ° C., and most preferably 60 ° C. to 115 ° C., in order to further demonstrate the effects of the present invention. If the addition temperature when adding the styrene-based monomer to the suspension containing the recycled styrene-based resin raw material particles (a) is adjusted within the above range, the styrene-based monomer can be incorporated while maintaining the recycled styrene-based resin raw material particles (a) at a moderate hardness, so that the recycled styrene-based resin particles (A) can be well spheroidized, and the finally obtained recycled expandable styrene-based resin particles can be well spheroidized and have excellent moldability. If the addition temperature when adding the styrene monomer to the recycled styrene resin raw material particle (a) is too low outside the above range, the recycled styrene resin raw material particle (a) becomes too hard, and when the styrene monomer is incorporated in this state, the recycled styrene resin particle (A) becomes difficult to be spherical, and the finally obtained recycled expandable styrene resin particle may be difficult to be spherical or may have poor moldability. If the addition temperature when adding the styrene monomer to the recycled styrene resin raw material particle (a) is too high outside the above range, the recycled styrene resin raw material particle (a) becomes too soft, and when the styrene monomer is incorporated in this state, the recycled styrene resin particle (A) becomes difficult to be spherical, and the finally obtained recycled expandable styrene resin particle may be difficult to be spherical or may have poor moldability.

[0084] After the styrene monomer is added to the suspension containing the recycled styrene resin raw material particles (a), the polymerization reaction may be continued at any suitable temperature and time, if necessary.

[0085] The suspension containing the recycled styrene-based resin raw material particles (a) may contain a bubble regulator. Examples of such bubble regulators include fatty acid monoamides such as oleic acid amide, stearic acid amide, and hydroxystearic acid amide; fatty acid bisamides such as methylene bisstearic acid amide and ethylene bisstearic acid amide.

[0086] The recycled expandable styrene resin particles are obtained by pressurizing and impregnating the recycled styrene resin particles (A) with a blowing agent.

[0087] A representative method for pressurizing and impregnating the blowing agent is to place the recycled styrene-based resin particles (A) in a reactor such as an autoclave, and pressurize and impregnate the blowing agent.

[0088] The foaming agent may be of only one type, or of two or more types.

[0089] As the foaming agent, any suitable foaming agent can be used as long as it does not impair the effects of the present invention. The foaming agent referred to here is preferably a volatile foaming agent. The foaming agent is preferably an organic compound whose boiling point is equal to or lower than the softening point of the styrene-based resin and is in a gaseous or liquid state at normal pressure. Specific examples include aliphatic hydrocarbons such as propane, n-butane, isobutane, pentane (n-pentane, isopentane, neopentane), and n-hexane; alicyclic hydrocarbons such as cyclopentane and cyclopentadiene; ketones such as acetone and methyl ethyl ketone; alcohols such as methanol, ethanol, and isopropyl alcohol; low-boiling ether compounds such as dimethyl ether, diethyl ether, dipropyl ether, and methyl ethyl ether; halogen-containing hydrocarbons such as trichloromonofluoromethane and dichlorodifluoromethane; and the like. As the foaming agent, inorganic gases such as carbon dioxide, nitrogen, and ammonia may be used. Among these, in terms of further exerting the effects of the present invention, the blowing agent is preferably at least one selected from n-butane, isobutane, n-pentane, isopentane, neopentane, cyclopentane, and cyclopentadiene, and more preferably at least one selected from n-butane, isobutane, n-pentane, and isopentane.

[0090] The content of the blowing agent can be appropriately set according to the purpose as long as it is a sufficient amount to form the recycled pre-expanded styrene-based resin particles and the recycled styrene-based resin foamed molded article. The content of the blowing agent is preferably 2 to 15 parts by mass when the total amount of the recycled styrene-based resin raw material particles (a) and the styrene-based monomer is 100 parts by mass.

[0091] The temperature at which the blowing agent is injected into the recycled styrene-based resin particles (A) is preferably 40°C to 150°C, more preferably 40°C to 140°C, even more preferably 40°C to 130°C, even more preferably 40°C to 123°C, even more preferably 40°C to 110°C, even more preferably 40°C to 105°C, even more preferably 40°C to 95°C, even more preferably 40°C to 89°C, even more preferably 40°C to 88°C, even more preferably 40°C to 87°C, particularly preferably 40°C to 86°C, and most preferably 40°C to 85°C. The temperature at which the blowing agent is injected into the recycled styrene-based resin particles (A) may be changed within the above range. If the injection temperature of the blowing agent into the recycled styrene-based resin particles (A) is within the above range, the blowing agent can be injected at a low temperature, and by injecting the blowing agent at such a low temperature and then raising the temperature, the blowing agent is prevented from being rapidly impregnated into the recycled styrene-based resin particles (A), enabling uniform impregnation, and for example, reducing the number of areas that shrink and melt when molded into a recycled styrene-based resin foamed molded product. If the injection temperature of the blowing agent into the recycled styrene-based resin particles (A) is too low outside the above range, the blowing agent is difficult to impregnate into the recycled styrene-based resin particles (A) when the blowing agent is injected, and the blowing agent is rapidly impregnated when the temperature is raised, so that the blowing agent is not uniformly impregnated into the recycled styrene-based resin particles (A), which is likely to cause bubble variations and surface shrinkage during molding. If the temperature at which the blowing agent is injected into the recycled styrene-based resin particles (A) is too high and falls outside the above range, the blowing agent will be rapidly impregnated into the recycled styrene-based resin particles (A) when the blowing agent is injected, and the blowing agent will not be uniformly impregnated into the recycled styrene-based resin particles (A). This may result in uneven bubble formation and surface shrinkage during molding.

[0092] One embodiment of the impregnation temperature of the blowing agent into the recycled styrene-based resin particles (A) is preferably 40°C to 150°C, more preferably 40°C to 140°C, even more preferably 40°C to 130°C, even more preferably 40°C to 123°C, even more preferably 40°C to 110°C, particularly preferably 40°C to 105°C, and most preferably 40°C to 95°C.

[0093] Another embodiment of the impregnation temperature of the blowing agent into the recycled styrene-based resin particles (A) is preferably a temperature equal to or higher than the pressure-injection temperature of the blowing agent into the recycled styrene-based resin particles (A), preferably 93°C to 130°C, more preferably 94°C to 129°C, even more preferably 95°C to 128°C, particularly preferably 96°C to 127°C, and most preferably 97°C to 126°C.

[0094] The temperature of impregnation of the blowing agent into the recycled styrene-based resin particles (A) may be changed within the above range. If the impregnation temperature of the blowing agent into the recycled styrene-based resin particles (A) is within the above range, in combination with the adjustment of the above-mentioned pressure-in temperature, the blowing agent is prevented from being rapidly impregnated into the recycled styrene-based resin particles (A), enabling uniform impregnation, and for example, reducing the number of areas that shrink and melt when molded into a recycled styrene-based resin foamed molded product. If the impregnation temperature of the blowing agent into the recycled styrene-based resin particles (A) is too low outside the above range, the blowing agent may not be impregnated to the center of the recycled styrene-based resin particles (A), leaving non-foamed areas, and it may not be possible to obtain a good molded product. If the impregnation temperature of the blowing agent into the recycled styrene-based resin particles (A) is too high outside the above range, the blowing agent may be impregnated too much into the recycled styrene-based resin particles (A), causing it to melt during molding.

[0095] The time for impregnating the recycled styrene-based resin particles (A) with the blowing agent can be any appropriate time within the range that does not impair the effects of the present invention, and is preferably 1 hour to 10 hours.

[0096] The recycled expandable styrene-based resin particles may contain any appropriate other components within the scope of not impairing the effects of the present invention. Such other components may be one type only or two or more types.

[0097] The recycled expandable styrene resin particles may contain a flame retardant to enhance flame retardancy. The flame retardant may be of one type or of two or more types.

[0098] As the flame retardant, any suitable flame retardant may be adopted as long as it does not impair the effect of the present invention. As such a flame retardant, a bromine compound compatible with polystyrene is preferable, and examples thereof include tetrabromoethane, tetrabromocyclooctane, hexabromocyclododecane, hexabromocyclohexane, trisdibromopropyl phosphate, tetrabromobisphenol A, tetrabromobisphenol F, tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether), tetrabromobisphenol A-bis(2,3-dibromopropyl ether), tetrabromobisphenol A-diglycidyl ether, 2,2-bis[4'(2'',3''-dibromoalkoxy)-3',5'-dibromophenyl]-propane, tris(tribromophenoxy)triazine, 2,2-bis(4-allyloxy-3,5-dibromo)propane, and hexabromobenzene.

[0099] When a flame retardant is used, a flame retardant assistant may be used in combination. Examples of the flame retardant assistant include cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, 2,3-dimethyl-2,3-diphenylbutane, and 3,4-dimethyl-3,4-diphenylhexane.

[0100] The total amount of the flame retardant and the flame retardant auxiliary may be any appropriate amount within the range that does not impair the effects of the present invention. The total amount is preferably 0.1% to 15% by mass, more preferably 0.2% to 10% by mass, even more preferably 0.2% to 5% by mass, and particularly preferably 0.2% to 3% by mass, based on the recycled styrene-based resin raw material particles (a).

[0101] The flame retardant may be added at any suitable timing within a range that does not impair the effects of the present invention. The flame retardant is preferably added before the blowing agent is injected. By adding the flame retardant before the blowing agent is injected, the flame retardant can be added at a low temperature equivalent to the temperature at which the blowing agent is injected, and therefore the resulting recycled expandable styrene-based resin particles can be well spherical and have excellent moldability.

[0102] The addition temperature when adding the flame retardant is preferably 5°C to 120°C, more preferably 5°C to 118°C, even more preferably 5°C to 115°C, even more preferably 5°C to 113°C, even more preferably 5°C to 110°C, even more preferably 40°C to 89°C, even more preferably 40°C to 87°C, even more preferably 40°C to 85°C, particularly preferably 40°C to 83°C, and most preferably 40°C to 80°C.

[0103] In producing the recycled expandable styrene resin particles, a partial ester of higher fatty acid and alcohol may be used as the cell regulator. That is, the recycled expandable styrene resin particles may contain a partial ester of higher fatty acid and alcohol. The partial ester of higher fatty acid and alcohol may be only one type or two or more types. Examples of the higher fatty acid include fatty acids having 15 or more carbon atoms such as palmitic acid, stearic acid, oleic acid, linoleic acid, linolenic acid, and behenic acid, and monoglycerides and diglycerides thereof can be used. Examples of the partial ester of higher fatty acid and alcohol include monoglyceride stearic acid and diglyceride stearic acid. The content ratio of the partial ester of higher fatty acid and alcohol is preferably 0 to 3.0 parts by mass, more preferably 0.5 to 3.0 parts by mass, relative to 100 parts by mass of the recycled styrene resin particles (A). The partial ester of higher fatty acid and alcohol may be added, for example, together with a foaming agent, or a commonly used method such as a dry blend method, a master batch method, or a melt injection method.

[0104] In producing the recycled expandable styrene-based resin particles, a foaming assistant may be used. That is, the recycled expandable styrene-based resin particles may contain a foaming assistant. The foaming assistant may be only one type, or may be two or more types. Examples of the foaming assistant include diisobutyl adipate, toluene, cyclohexane, ethylbenzene, liquid paraffin, and coconut oil.

[0105] When producing the recycled expandable styrene-based resin particles, a bubble regulator may be used. That is, the recycled expandable styrene-based resin particles may contain a bubble regulator. The bubble regulator may be one type only or two or more types. Examples of the bubble regulator include fatty acid monoamides such as oleic acid amide, stearic acid amide, and hydroxystearic acid amide; fatty acid bisamides such as methylene bisstearic acid amide and ethylene bisstearic acid amide; and the like.

[0106] The amount of the cell regulator may be any appropriate amount within the range that does not impair the effects of the present invention. The amount is preferably 0 to 5.0 parts by mass, more preferably 0.02 to 3.0 parts by mass, even more preferably 0.02 to 2.0 parts by mass, and particularly preferably 0.02 to 1.0 parts by mass, relative to 100 parts by mass of the recycled styrene-based resin particles (A).

[0107] The recycled expandable styrene-based resin particles may contain a bubble regulator such as talc, calcium carbonate, mica, citric acid, sodium bicarbonate, etc. The bubble regulator may be of only one type, or of two or more types.

[0108] In addition to the above, other additives include, for example, pigments, radiative heat transfer suppressing components, crosslinking agents, plasticizers, stabilizers, fillers, lubricants, colorants, antistatic agents, spreading agents, weather resistance agents, antiaging agents, anti-fogging agents, and fragrances.

[0109] The recycled expandable styrene-based resin particles may be surface-treated, preferably with at least one selected from silicone oil, antistatic agents, fatty acid metal salts, and fusion promoters.

[0110] When the recycled expandable styrene resin particles are surface-treated with silicone oil, the amount of silicone oil used relative to 100 parts by mass of recycled expandable styrene resin particles before surface treatment is preferably 0.001 parts by mass to 0.3 parts by mass, more preferably 0.003 parts by mass to 0.28 parts by mass, even more preferably 0.005 parts by mass to 0.25 parts by mass, particularly preferably 0.008 parts by mass to 0.23 parts by mass, and most preferably 0.01 parts by mass to 0.23 parts by mass. If the amount of silicone oil used is too small outside the above range, for example, when an antistatic agent is used, the affinity with the antistatic agent during pre-foaming may be insufficient, and static electricity may be easily generated. If the amount of silicone oil used is too large outside the above range, the surface may melt during molding, resulting in loss of surface properties.

[0111] The silicone oil may be of only one type, or of two or more types.

[0112] As the silicone oil, any suitable silicone oil can be adopted as long as it does not impair the effect of the present invention.In terms of being able to more effectively exhibit the effect of the present invention, the silicone oil can be, for example, straight silicone oil such as dimethylpolysiloxane, methylphenylpolysiloxane, methylhydrogenpolysiloxane, etc., and preferably methylphenylpolysiloxane.

[0113] When the recycled expandable styrene resin particles are surface-treated with an antistatic agent, the amount of the antistatic agent used relative to 100 parts by mass of the recycled expandable styrene resin particles before surface treatment is preferably 0.001 to 0.3 parts by mass, more preferably 0.005 to 0.28 parts by mass, even more preferably 0.01 to 0.27 parts by mass, particularly preferably 0.015 to 0.26 parts by mass, and most preferably 0.02 to 0.25 parts by mass. If the amount of the antistatic agent is too small outside the above range, static electricity may be easily generated during pre-expansion. If the amount of the antistatic agent is too large outside the above range, the surface of the recycled pre-expanded styrene resin particles or the recycled styrene resin foamed molded article may become sticky.

[0114] The antistatic agent may be used alone or in combination of two or more kinds.

[0115] As the antistatic agent, any appropriate antistatic agent may be used as long as it does not impair the effects of the present invention. In terms of being able to more effectively exhibit the effects of the present invention, the antistatic agent may be at least one selected from a nonionic surfactant and a fatty acid glyceride, and preferably a combination of a nonionic surfactant and a fatty acid glyceride.

[0116] The nonionic surfactant may be of only one type, or of two or more types.

[0117] As the nonionic surfactant, any suitable nonionic surfactant may be adopted as long as it does not impair the effects of the present invention. In terms of being able to more effectively express the effects of the present invention, examples of the nonionic surfactant include polyethylene glycol, glycerin, polyoxyethylene alkyl ether, polyoxyethylene alkyl ester, polyhydric alcohol, and 1-amino-2-hydroxy compound. Specific examples of the polyoxyethylene alkyl ether include polyoxyethylene cetyl ether, polyoxyethylene oleyl ether, and polyoxyethylene stearyl ether. Specific examples of the polyoxyethylene alkyl ester include polyoxyethylene laurate, polyoxyethylene palmitate, polyoxyethylene stearate, and polyoxyethylene oleate. Specific examples of the polyhydric alcohol include glycerin and propylene glycol. Specific examples of the 1-amino-2-hydroxy compound include N-hydroxyethyl-N-(2-hydroxyalkyl)amine, N,N-bis(hydroxyethyl)dodecylamine, N,N-bis(hydroxyethyl)tetradecylamine, N,N-bis(hydroxyethyl)hexadecylamine, N,N-bis(hydroxyethyl)octadecylamine, N-hydroxyethyl-N-(2-hydroxytetradecyl)amine, N-hydroxyethyl-N-(2-hydroxyhexadecyl)amine, N-hydroxyethyl-N-(2-hydroxyoctadecyl)amine, N-hydroxypropyl-N Examples of the hydroxyethyl amine include N-(2-hydroxytetradecyl)amine, N-hydroxybutyl-N-(2-hydroxytetradecyl)amine, N-hydroxypentyl-N-(2-hydroxytetradecyl)amine, N-hydroxypentyl-N-(2-hydroxyhexadecyl)amine, N-hydroxypentyl-N-(2-hydroxyoctadecyl)amine, N,N-bis(2-hydroxyethyl)dodecylamine, N,N-bis(2-hydroxyethyl)tetradecylamine, N,N-bis(2-hydroxyethyl)hexadecylamine, N,N-bis(2-hydroxyethyl)octadecylamine, and salts thereof.As the nonionic surfactant, polyethylene glycol is preferred in that the effects of the present invention can be more effectively exhibited.

[0118] When a nonionic surfactant is used as at least a part of the antistatic agent, the amount of the nonionic surfactant used relative to 100 parts by mass of recycled expandable styrene-based resin particles before surface treatment is preferably 0.001 parts by mass to 2.0 parts by mass, more preferably 0.001 parts by mass to 1.5 parts by mass, even more preferably 0.001 parts by mass to 1.0 parts by mass, even more preferably 0.001 parts by mass to 0.5 parts by mass, even more preferably 0.001 parts by mass to 0.3 parts by mass, even more preferably 0.005 parts by mass to 0.28 parts by mass, even more preferably 0.01 parts by mass to 0.27 parts by mass, particularly preferably 0.015 parts by mass to 0.26 parts by mass, and most preferably 0.02 parts by mass to 0.25 parts by mass. If the amount of the nonionic surfactant is too small outside the above range, static electricity may be easily generated during pre-expansion. If the amount of the nonionic surfactant is too large and deviates from the above range, the surfaces of the recycled pre-expanded styrene-based resin particles and the recycled styrene-based resin foamed molded article may become sticky.

[0119] The fatty acid glyceride may be of only one type, or of two or more types.

[0120] As the fatty acid glyceride, any suitable fatty acid glyceride can be adopted as long as it does not impair the effects of the present invention.Specific examples of the fatty acid glyceride that can further demonstrate the effects of the present invention include stearic acid monoglyceride and linoleic acid monoglyceride.As the fatty acid glyceride, stearic acid monoglyceride is preferred in terms of further demonstrating the effects of the present invention.

[0121] When fatty acid glyceride is used as at least a part of the antistatic agent, the amount of the fatty acid glyceride relative to 100 parts by mass of the recycled expandable styrene-based resin particles before surface treatment is preferably 0.001 parts by mass to 0.3 parts by mass, more preferably 0.005 parts by mass to 0.28 parts by mass, even more preferably 0.01 parts by mass to 0.27 parts by mass, particularly preferably 0.015 parts by mass to 0.26 parts by mass, and most preferably 0.02 parts by mass to 0.25 parts by mass. If the amount of fatty acid glyceride is too small outside the above range, static electricity may be easily generated during pre-expansion. If the amount of fatty acid glyceride is too large outside the above range, the surface of the recycled pre-expanded styrene-based resin particles or the recycled styrene-based resin foamed molded article may become sticky.

[0122] When the recycled expandable styrene resin particles are surface-treated with a fatty acid metal salt, the amount of fatty acid metal salt used relative to 100 parts by mass of recycled expandable styrene resin particles before surface treatment is preferably 0.005 parts by mass to 0.5 parts by mass, more preferably 0.007 parts by mass to 0.45 parts by mass, even more preferably 0.01 parts by mass to 0.4 parts by mass, particularly preferably 0.015 parts by mass to 0.35 parts by mass, and most preferably 0.02 parts by mass to 0.3 parts by mass. If the amount of fatty acid metal salt is too small outside the above range, blocking may occur frequently during pre-expansion, and a good styrene resin foam molded article may not be obtained. If the amount of fatty acid metal salt is too large outside the above range, a large amount of metal salt is present during pre-expansion, which makes it easy to be charged, which makes it easy to generate static electricity, and the fusion of the molded article may be poor.

[0123] The fatty acid metal salt may be of one type only, or of two or more types.

[0124] As the fatty acid metal salt, any suitable fatty acid metal salt may be adopted as long as it does not impair the effects of the present invention. In terms of being able to more effectively express the effects of the present invention, examples of the fatty acid metal salt include metal stearates and metal laurates. Specific examples of the metal stearates include magnesium stearate, calcium stearate, zinc stearate, barium stearate, aluminum stearate, and lithium stearate. Specific examples of the metal laurate include zinc laurate and barium laurate. In terms of being able to more effectively express the effects of the present invention, magnesium stearate and zinc stearate are preferred as fatty acid metal salts.

[0125] When the recycled expandable styrene resin particles are surface-treated with a fusion promoter, the amount of the fusion promoter used relative to 100 parts by mass of the recycled expandable styrene resin particles before surface treatment is preferably 0.01 parts by mass to 0.8 parts by mass, more preferably 0.01 parts by mass to 0.7 parts by mass, even more preferably 0.01 parts by mass to 0.6 parts by mass, particularly preferably 0.01 parts by mass to 0.55 parts by mass, and most preferably 0.013 parts by mass to 0.5 parts by mass. If the amount of the fusion promoter is too small outside the above range, the fusion property may decrease during molding, and a good recycled styrene resin foam molded article may not be obtained. If the amount of the fusion promoter is too large outside the above range, blocking may occur during pre-expansion.

[0126] The fusion promoter may be of only one type, or of two or more types.

[0127] As the fusion promoter, any suitable fusion promoter may be adopted as long as it does not impair the effects of the present invention. In terms of being able to further demonstrate the effects of the present invention, examples of the fusion promoter include fatty acid triglyceride, fatty acid diglyceride, fatty acid monoglyceride, and vegetable oil. Specific examples of fatty acid triglyceride include lauric acid triglyceride, stearic acid triglyceride, linoleic acid triglyceride, and hydroxystearic acid triglyceride. Specific examples of fatty acid diglyceride include lauric acid diglyceride, stearic acid diglyceride, and linoleic acid diglyceride. Specific examples of fatty acid monoglyceride include lauric acid monoglyceride. Specific examples of vegetable oil include hydrogenated castor oil. In terms of being able to further demonstrate the effects of the present invention, stearic acid triglyceride and hydroxystearic acid triglyceride are preferred as the fusion promoter.

[0128] <<B. Recycled expandable styrene resin particles>> The recycled expandable styrene resin particles according to the embodiment of the present invention have a particle shape as a whole. The average particle diameter of the recycled expandable styrene resin particles is preferably 0.40 mm to 2.0 mm, more preferably 0.6 mm to 1.8 mm. The average particle diameter can be measured in accordance with JIS Z 8815. Specifically, the average particle diameter is the value measured as a particle diameter of 50% of the cumulative value from the particle size distribution by the sieving test of JIS Z 8815.

[0129] The shape of the recycled expandable styrene resin particles according to the embodiment of the present invention can be any suitable shape as long as it does not impair the effects of the present invention. Specific examples of such shapes include, for example, spherical, approximately spherical, and elliptical (egg-shaped). The shape of the recycled expandable styrene resin particles according to the embodiment of the present invention is preferably spherical or approximately spherical, and more preferably spherical, in terms of achieving the effects of the present invention. However, in reality, it is difficult to distinguish between spherical and approximately spherical, so in this specification, both are collectively referred to as spherical.

[0130] The mass average molecular weight of the recycled expandable styrene-based resin particles according to the embodiment of the present invention can be any appropriate mass average molecular weight within a range that does not impair the effects of the present invention. Such a mass average molecular weight is preferably 100,000 to 600,000, more preferably 110,000 to 500,000, even more preferably 120,000 to 470,000, and particularly preferably 130,000 to 450,000.

[0131] The recycled expandable styrene-based resin particles according to an embodiment of the present invention are formed from recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles, and the recycled styrene-based resin foamed molding has a Z-average molecular weight Mz of 370,000 to 5,000,000 and a Z+1 average molecular weight Mz+1 of 2,000,000 to 15,000,000.

[0132] The Z-average molecular weight Mz of the recycled styrene-based resin foamed molding molded from the recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles is preferably 370,000 to 5,000,000, and more preferably 370,000 to 4,000,000.

[0133] The Z+1 average molecular weight Mz+1 of the recycled styrene-based resin foamed molding molded from the recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles is preferably 2 million to 15 million, and more preferably 2 million to 12 million.

[0134] The recycled pre-expanded styrene-based resin particles according to an embodiment of the present invention are formed from recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles, and the Z-average molecular weight Mz and Z+1-average molecular weight Mz+1 of the recycled styrene-based resin foamed molded product are adjusted to fall within the above-mentioned ranges. This allows the recycled styrene-based resin foamed molded product obtained using the recycled expandable styrene-based resin particles as a raw material to exhibit high strength at the same level as that of a styrene-based resin foamed molded product produced without using recycled raw materials.

[0135] The recycled expandable styrene-based resin particles according to an embodiment of the present invention are obtained by injecting and impregnating a blowing agent into recycled styrene-based resin particles (A), which are obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing the mixture in the presence of a polymerization initiator.

[0136] For an explanation of how to obtain recycled expandable styrene-based resin particles, such as the recycled styrene-based resin raw material particles (a), styrene-based monomers, polyfunctional monomers, details regarding polymerization such as polymerization method and polymerization conditions, recycled styrene-based resin particles (A), and injection / impregnation of a blowing agent, the explanation in the above section ``A. Recycled styrene-based resin foamed moldings'' may be used.

[0137] The recycled expandable styrene-based resin particles according to an embodiment of the present invention can be used as is for producing a recycled styrene-based resin foamed molded article according to an embodiment of the present invention.

[0138] <<C. Recycled pre-expanded styrene resin particles>> The recycled pre-expanded styrene-based resin particles according to an embodiment of the present invention are obtained by pre-expanding the recycled expandable styrene-based resin particles according to an embodiment of the present invention.

[0139] The average bubble diameter of the recycled pre-expanded styrene resin particles is preferably 0.01 mm to 1.10 mm, more preferably 0.01 mm to 1.00 mm, even more preferably 0.01 to 0.90 mm, particularly preferably 0.01 mm to 0.80 mm, and most preferably 0.01 mm to 0.70 mm. If the average bubble diameter of the recycled pre-expanded styrene resin particles is within the above range, it is possible to provide recycled pre-expanded styrene resin particles that can prevent blocking during expansion and molding, and can further suppress electrostatic charge during expansion and molding while exhibiting better fusion properties and surface properties, thereby enabling the molding of a recycled styrene resin foamed molded article with less static electricity. If the average bubble diameter of the recycled pre-expanded styrene resin particles is smaller than 0.01 mm, there is a risk that the surface will melt and shrink during molding.

[0140] Pre-expansion includes expanding the recycled expandable styrene-based resin particles according to the embodiment of the present invention to a desired bulk expansion ratio (bulk density) using steam or the like. The bulk expansion ratio of the recycled pre-expanded styrene-based resin particles is preferably 2 to 150 times, more preferably 2 to less than 100 times, more preferably 5 to 90 times, even more preferably 10 to 85 times, and particularly preferably 15 to 83 times. The bulk density is the reciprocal of the bulk expansion ratio. By having the bulk expansion ratio of the recycled pre-expanded styrene-based resin particles within the above range, blocking during expansion and molding can be more effectively prevented, and further, electrostatic charge during expansion and molding can be suppressed while exhibiting better fusion properties and surface properties, and a recycled styrene-based resin foam molded article with less static electricity can be molded.

[0141] In one representative embodiment, the recycled pre-expanded styrene-based resin particles according to the embodiment of the present invention can be used to mold a recycled styrene-based resin foamed molded article. In another embodiment, the recycled pre-expanded styrene-based resin particles according to the embodiment of the present invention can be used as it is as a cushioning material, a heat insulating material, a concrete aggregate, etc. When the recycled pre-expanded styrene-based resin particles according to the embodiment of the present invention are used as they are, the recycled pre-expanded styrene-based resin particles according to the embodiment of the present invention can be preferably used as a filler in which a large number of recycled pre-expanded styrene-based resin particles are filled in a bag. Such recycled pre-expanded styrene-based resin particles are suitable, for example, for the core material of a cushion (foam particles filled inside the cushion).

[0142] The recycled pre-expanded styrene-based resin particles according to an embodiment of the present invention can be used as is for producing a recycled styrene-based resin foamed molded article according to an embodiment of the present invention. EXAMPLES

[0143] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. The methods for measuring and evaluating each property are as follows.

[0144] <Measurement of mass average molecular weight Mw> In this specification, the mass average molecular weight Mw means the polystyrene (PS) equivalent mass average molecular weight measured using gel permeation chromatography (GPC). Specifically, the mass average molecular weight was measured as follows. 3 mg of sample was dissolved in 10 mL of THF (tetrahydrofuran) (immersion time: 24 h±1 hr (complete dissolution)) to obtain a sample solution. The sample solution was filtered through a non-aqueous 0.45 μm syringe filter manufactured by Shimadzu GLC Co., Ltd. to obtain a filtrate. The obtained filtrate was measured using a chromatograph under the following measurement conditions. The mass average molecular weight Mw was determined from a previously prepared standard polystyrene calibration curve. Equipment used: Tosoh Corporation's "HLC-8320GPC EcoSEC" gel permeation chromatograph (with built-in RI and UV detectors) GPC measurement conditions: Sample column: guard column (Tosoh Corporation, TSK guardcolumn SuperMP(HZ)-H (4.6mmI.D.×2cm)×1), measurement column (Tosoh Corporation, TSKgel SuperMultiporeHZ-H (4.6mmI.D.×15cm)×2 in series) Reference column: Tosoh Corporation, TSKgel Super HZ1000 (6.0 mm I.D. x 15 cm) x 1 Column temperature = 40℃ ·Mobile phase=THF Mobile phase flow rate (sample pump = 0.2mL / min, reference pump = 0.2mL / min) Detector = RI detector Sample concentration = 0.1% by mass ·Injection volume=20μL Measurement time = 26 min -Sampling pitch = 200msec The standard polystyrene samples used for the calibration curve were "STANDARD SM-105" and "STANDARD SH-75" manufactured by Showa Denko K.K., with mass average molecular weights of 5,620,000, 3,120,000, 1,250,000, 442,000, 151,000, 53,500, 17,000, 7,660, 2,900, and 1,320. The above-mentioned standard polystyrene for the calibration curve was grouped into A (5,620,000, 1,250,000, 151,000, 17,000, 2,900) and B (3,120,000, 442,000, 53,500, 7,660, 1,320), and then A (2 mg, 3 mg, 4 mg, 4 mg, 4 mg) was weighed and dissolved in 30 mL of THF, and B (3 mg, 4 mg, 4 mg, 4 mg, 4 mg) was also weighed and dissolved in 30 mL of THF. The standard polystyrene calibration curve was obtained by injecting 20 μL of the prepared A solution and B solution and creating a calibration curve (linear equation) from the retention time obtained after measurement. The mass average molecular weight Mw, Z average molecular weight Mz, and Z+1 average molecular weight Mz+1 were calculated using the calibration curve.

[0145] <Measurement of average maximum bending strength> The average maximum bending strength of the foam molded article was measured in accordance with the method described in JIS A9511. Specifically, the average maximum bending strength of the foam molded article was measured in accordance with the method described in JIS A9511:1999 "Foamed plastic heat-insulating material". More specifically, the average maximum bending strength of the foam molded article was measured in accordance with the method described in JIS A9511:1999 "Foamed plastic heat-insulating material". 3 (0.0167g / cm 3 Five rectangular parallelepiped test pieces measuring 75 mm long x 300 mm wide x 30 mm thick were cut out from the foam of 100 mm x 100 mm x 100 mm in diameter, and the maximum bending strength of each of the five test pieces was measured using a bending strength measuring device (manufactured by Orientec Co., Ltd., product name "UCT-10T") under the conditions of a compression speed of 10 mm / min, a distance between supports of 200 mm, a pressure wedge of 10R, and a support stand of 10R. The arithmetic mean of the five measurement results was taken as the average maximum bending strength. The conditions for measuring the maximum bending strength were a start load of 0.0 fs%, an end load of 20.0 fs%, and a pitch load of 0.2 fs%. The evaluation was based on the following criteria. ○: Average maximum bending strength is 0.33 MPa or more. ×: Average maximum bending strength is less than 0.33 MPa.

[0146] <Appearance evaluation> The appearance of the foamed molded article was evaluated according to the following criteria. ◯: When the surface of the foam is visually inspected, there are no gaps between the surface particles, and the foam is not shrinking. ×: When the surface of the foam is visually inspected, there are many gaps between the surface particles, or the foam has shrunk.

[0147] <Measurement of bulk density and bulk expansion ratio of recycled pre-expanded styrene resin particles> The bulk density and bulk expansion ratio of the recycled pre-expanded styrene-based resin particles were measured as follows. (Method of measuring bulk density) The recycled pre-expanded styrene resin particles were allowed to fall naturally into a measuring cylinder as a sample, and the bottom of the measuring cylinder was struck to make the sample volume constant. The volume and mass were then measured and calculated according to the following formula. Bulk density (g / mL) = sample mass (g) / sample volume in measuring cylinder (mL) (Method of measuring bulk expansion ratio) The recycled pre-expanded styrene resin particles were allowed to fall naturally into a measuring cylinder as a sample, and the bottom of the measuring cylinder was struck to make the sample volume constant. The volume and mass were measured and calculated using the following formula. The resin specific gravity was set to 1.0 for styrene resin. Bulk expansion ratio (times) = sample volume in measuring cylinder (mL) / sample mass (g) x resin specific gravity The bulk expansion ratio may be calculated as the reciprocal of the bulk density.

[0148] <Measurement of density and expansion ratio of recycled styrene-based resin foamed moldings> (Method of measuring density) The density of the recycled styrene-based resin foam molded body was calculated by measuring the dimensions and mass of the test piece to three or more significant figures and using the following formula. Density (g / cm 3 ) = mass of test piece (g) / volume of test piece (cm3 ) (Method of measuring foaming ratio) The expansion ratio of the recycled styrene-based resin foam molded product was calculated by the following formula, measuring the dimensions and mass of the test piece to three or more significant figures. The resin specific gravity was set to 1.0 for styrene-based resin. Expansion ratio (times) = test piece volume (cm 3 ) / test piece mass (g) × resin specific gravity

[0149] [Example 1] After crushing the expanded polystyrene containers used as fish boxes, they were fed into a φ30mm twin-screw extruder, melted and kneaded at 230°C, and extruded into strands from a die with 8 holes and a hole diameter of 0.6mm. After cooling in a water cooling bath at 25°C, they were cut into pieces with an average diameter of 0.8mm and a length of 1.0mm to obtain cylindrical recycled styrene resin raw material particles (a). The mass average molecular weight Mw, calculated in styrene equivalent, of the obtained recycled styrene resin raw material particles (a) was 190,000, Mz was 370,000, and Mz+1 was 630,000. Next, 2000 parts by mass of water, 1600 parts by mass of recycled styrene-based resin raw material particles (a), 6 parts by mass of magnesium pyrophosphate, and 0.3 parts by mass of calcium dodecylbenzenesulfonate were supplied to a pressure-resistant polymerization vessel equipped with a stirrer, and heated to 70°C with stirring to prepare a dispersion. Next, 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene were dissolved in 400 parts by mass of styrene monomer, and all of this styrene monomer solution was fed into the above dispersion liquid while stirring. After 30 minutes had passed since the feeding, the temperature was raised to 90°C and polymerization was carried out for 3 hours, and then the temperature was further raised to 125°C and maintained for 2 hours to carry out polymerization, thereby obtaining recycled styrene-based resin particles (A1). Next, 160 parts by mass of butane was pressed into the container while keeping it at 90°C again and maintained for 6 hours, and the recycled styrene resin particles (A1) were impregnated with butane, and then cooled to 30°C to obtain recycled expandable styrene resin particles. After polyethylene glycol was applied to the surface of the obtained recycled expandable styrene resin particles as an antistatic agent, zinc stearate and hydroxystearic acid triglyceride were applied to the surface of the recycled expandable styrene resin particles. The zinc stearate and hydroxystearic acid triglyceride were each adjusted to be 0.05% by mass in the recycled expandable styrene resin particles. Thereafter, the recycled expandable styrene resin particles were left for 5 days in a thermostatic chamber at 13°C. The butane content in the recycled expandable styrene resin particles (1) after leaving it was measured by gas chromatography and found to be 5.1% by mass. Thereafter, the recycled expandable styrene resin particles (1) are placed in a cylindrical batch type pressure expansion machine and heated with steam for 2 minutes to a bulk density of 0.0167 g / cm 3 The recycled pre-expanded styrene-based resin particles (1) were then aged at 20° C. for 24 hours. Next, the obtained recycled pre-expanded styrene resin particles (1) were left in a room temperature atmosphere for 24 hours, and then, using a molding machine having a mold with a cavity size of 300 mm wide, 400 mm long, and 30 mm thick, the recycled pre-expanded styrene resin particles (1) were filled into the cavity of the mold, heated at a vapor pressure of 0.08 MPa (gauge pressure) for 30 seconds, and then cooled until the pressure inside the mold became 0.03 MPa, and then released from the mold to obtain a plate-shaped recycled styrene resin foam molded product (1) corresponding to the mold. The obtained recycled styrene resin foam molded product (1) had an Mw of 260,000, an Mz of 520,000, and an Mz+1 of 3.9 million. The recycled styrene resin foam molded product (1) was aged for 6 hours in a drying chamber at 50°C, and the density was measured, which was 0.0167 g / cm. 3 The recycled styrene-based resin foam molded product (1) had no shrinkage and its appearance was good. The average maximum bending strength of the recycled styrene-based resin foam molded product (1) was 0.35 MPa. The results are shown in Table 1.

[0150] [Example 2] Instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 1.0 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene were dissolved in 400 parts by mass of styrene monomer, and the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (2), recycled pre-expanded styrene-based resin particles (2), and recycled styrene-based resin foam molded body (2). The Mw of the recycled styrene-based resin foam molded body (2) was 280,000, the Mz was 570,000, and the Mz+1 was 4.7 million. The recycled styrene-based resin foam molded body (2) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded body (2) was 0.36 MPa. The results are shown in Table 1.

[0151] [Example 3] Instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.8 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.12 parts by mass of divinylbenzene were dissolved in 400 parts by mass of styrene monomer, and the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (3), recycled pre-expanded styrene-based resin particles (3), and recycled styrene-based resin foam molded body (3). The Mw of the recycled styrene-based resin foam molded body (3) was 280,000, the Mz was 590,000, and the Mz+1 was 6.5 million. The recycled styrene-based resin foam molded body (3) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded body (3) was 0.37 MPa. The results are shown in Table 1.

[0152] [Example 4] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1000 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 3.0 parts by mass of t-butylperoxy-2-ethylhexanoate, 1.0 parts by mass of t-butylperoxybenzoate, and 0.15 parts by mass of divinylbenzene were dissolved in 1000 parts by mass of styrene monomer. The same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (4), recycled pre-expanded styrene-based resin particles (4), and recycled styrene-based resin foam molded body (4). The Mw of the recycled styrene-based resin foam molded body (4) was 280,000, the Mz was 670,000, and the Mz+1 was 7.3 million. The recycled styrene-based resin foam molded body (4) had no shrinkage and had an appearance of 0. The average maximum bending strength of the recycled styrene-based resin foam molded product (4) was 0.37 MPa. The results are shown in Table 1.

[0153] [Example 5] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1000 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 3.0 parts by mass of t-butylperoxy-2-ethylhexanoate, 1.0 parts by mass of t-butylperoxybenzoate, and 0.3 parts by mass of divinylbenzene were dissolved in 1000 parts by mass of styrene monomer. The same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (5), recycled pre-expanded styrene-based resin particles (5), and recycled styrene-based resin foam molded body (5). The Mw of the recycled styrene-based resin foam molded body (5) was 290,000, the Mz was 700,000, and the Mz+1 was 8.9 million. The recycled styrene-based resin foam molded body (5) had no shrinkage and had an appearance of 0. The average maximum bending strength of the recycled styrene-based resin foam molded product (5) was 0.37 MPa. The results are shown in Table 1.

[0154] [Example 6] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1800 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.3 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.2 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene were dissolved in 200 parts by mass of styrene monomer, the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (6), recycled pre-expanded styrene-based resin particles (6), and recycled styrene-based resin foam molded body (6). The Mw of the recycled styrene-based resin foam molded body (6) was 200,000, the Mz was 480,000, and the Mz+1 was 2.85 million. The recycled styrene-based resin foam molded body (6) had no shrinkage and had an appearance of 0. The average maximum bending strength of the recycled styrene-based resin foam molded product (5) was 0.35 MPa. The results are shown in Table 1.

[0155] [Example 7] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1900 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.15 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.1 parts by mass of t-butylperoxybenzoate, and 0.03 parts by mass of divinylbenzene were dissolved in 100 parts by mass of styrene monomer, in the same manner as in Example 1, to obtain recycled expandable styrene-based resin particles (7), recycled pre-expanded styrene-based resin particles (7), and recycled styrene-based resin foam molded body (7). The Mw of the recycled styrene-based resin foam molded body (7) was 200,000, the Mz was 420,000, and the Mz+1 was 2,050,000. The recycled styrene-based resin foam molded body (7) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded product (7) was 0.34 MPa. The results are shown in Table 1.

[0156] [Example 8] Except for using 1.2 parts by mass of t-hexylperoxy-2-ethylhexanoate instead of 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (8), recycled pre-expanded styrene-based resin particles (8), and recycled styrene-based resin foam molded body (8). The Mw of the recycled styrene-based resin foam molded body (8) was 220,000, the Mz was 590,000, and the Mz+1 was 5,050,000. The recycled styrene-based resin foam molded body (8) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded body (8) was 0.37 MPa. The results are shown in Table 1.

[0157] [Example 9] Except for using 1.2 parts by mass of 2,5-dimethyl-2,5-di(2-ethylhexanoylperoxy)hexane instead of 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, the procedure was carried out in the same manner as in Example 1 to obtain recycled expandable styrene resin particles (9), recycled pre-expanded styrene resin particles (9), and recycled styrene resin foam molded body (9). The Mw of the recycled styrene resin foam molded body (9) was 220,000, the Mz was 540,000, and the Mz+1 was 3.55 million. The recycled styrene resin foam molded body (9) had no shrinkage and had an appearance of 0. The average maximum bending strength of the recycled styrene resin foam molded body (9) was 0.37 MPa. The results are shown in Table 1.

[0158] [Example 10] Instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.4 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.12 parts by mass of divinylbenzene were dissolved in 400 parts by mass of styrene monomer, and the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (10), recycled pre-expanded styrene-based resin particles (10), and recycled styrene-based resin foam molded body (10). The Mw of the recycled styrene-based resin foam molded body (10) was 520,000, the Mz was 3,940,000, and the Mz+1 was 10,650,000. The recycled styrene-based resin foam molded body (10) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded body (10) was 0.36 MPa.

[0159] [Example 11] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1400 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.9 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.6 parts by mass of t-butylperoxybenzoate, and 0.18 parts by mass of divinylbenzene were dissolved in 600 parts by mass of styrene monomer. The same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (11), recycled pre-expanded styrene-based resin particles (11), and recycled styrene-based resin foam molded body (11). The Mw of the recycled styrene-based resin foam molded body (11) was 700,000, the Mz was 2.99 million, and the Mz+1 was 6.1 million. The recycled styrene-based resin foam molded body (11) had no shrinkage and had an appearance of 0. The average maximum bending strength of the recycled styrene-based resin foam molded product (11) was 0.36 MPa.

[0160] [Comparative Example 1] Instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 1.2 parts by mass of benzoyl peroxide, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene were dissolved in 400 parts by mass of styrene monomer, and the same procedure as in Example 1 was carried out to obtain recycled expandable styrene-based resin particles (C1), recycled pre-expanded styrene-based resin particles (C1), and recycled styrene-based resin foam molded body (C1). The Mw of the recycled styrene-based resin foam molded body (C1) was 220,000, the Mz was 450,000, and the Mz+1 was 1,050,000. The recycled styrene-based resin foam molded body (C1) had no shrinkage and had a good appearance. The average maximum bending strength of the recycled styrene-based resin foam molded body (C1) was 0.31 MPa. The results are shown in Table 1.

[0161] [Comparative Example 2] Except for not using divinylbenzene, the same procedure as in Example 1 was carried out to obtain recycled expandable styrene resin particles (C2), recycled pre-expanded styrene resin particles (C2), and recycled styrene resin foam molded body (C2). The Mw of the recycled styrene resin foam molded body (C2) was 210,000, the Mz was 420,000, and the Mz+1 was 810,000. The recycled styrene resin foam molded body (C2) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene resin foam molded body (C2) was 0.30 MPa. The results are shown in Table 1.

[0162] [Comparative Example 3] The same procedure as in Example 1 was carried out except that the amount of divinylbenzene was changed to 0.2 parts by mass, and recycled expandable styrene-based resin particles (C3) were obtained. However, the expandability was low, and the appearance of the obtained foamed molded article was poor. The results are shown in Table 1.

[0163] [Comparative Example 4] The amount of the recycled styrene-based resin raw material particles (a) was changed to 1960 parts by mass, and further, instead of dissolving 1.2 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.4 parts by mass of t-butylperoxybenzoate, and 0.06 parts by mass of divinylbenzene in 400 parts by mass of styrene monomer, 0.12 parts by mass of t-butylperoxy-2-ethylhexanoate, 0.04 parts by mass of t-butylperoxybenzoate, and 0.012 parts by mass of divinylbenzene were dissolved in 40 parts by mass of styrene monomer, in the same manner as in Example 1, to obtain recycled expandable styrene-based resin particles (C4), recycled pre-expanded styrene-based resin particles (C4), and recycled styrene-based resin foam molded body (C4). The Mw of the recycled styrene-based resin foam molded body (C4) was 190,000, the Mz was 350,000, and the Mz+1 was 720,000. The recycled styrene-based resin foam molded body (C4) had no shrinkage and had an appearance of ◯. The average maximum bending strength of the recycled styrene-based resin foam molded product (C4) was 0.30 MPa. The results are shown in Table 1.

[0164] [Table 1] [Industrial Applicability]

[0165] The recycled styrene-based resin foam molded article according to the embodiment of the present invention is preferably used as an insulating material for houses and automobiles, an insulating material for building materials, a packaging material for transport such as fish boxes and food containers, a cushioning material, etc. More specifically, the recycled styrene-based resin foam molded article according to the embodiment of the present invention is preferably used as an insulating material for walls, an insulating material for floors, an insulating material for roofs, an insulating material for automobiles, an insulating material for hot water tanks, an insulating material for piping, an insulating material for solar systems, an insulating material for water heaters, a container for food and industrial products (e.g., food containers such as fish boxes, and commuting boxes), a cushioning material, a float, a block, a packaging material for fish and agricultural products, an embankment material (embankment blocks, etc.), a core material for tatami mats, a core material for cushions, an aggregate for concrete, etc.

Claims

1. A recycled styrene-based resin foamed molded article formed from recycled pre-expanded styrene-based resin particles obtained by pre-expanding recycled expandable styrene-based resin particles, A recycled styrene-based resin foam molded article having a Z-average molecular weight Mz of 370,000 to 5,000,000 and a Z+1-average molecular weight Mz+1 of 2,000,000 to 15,000,000.

2. The recycled styrene-based resin foam molded article according to claim 1, having an average maximum bending strength of 0.33 MPa or more.

3. The recycled styrene-based resin foamed molded article according to claim 1, wherein the recycled expandable styrene-based resin particles are obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing the mixture in the presence of a polymerization initiator to obtain recycled styrene-based resin particles (A), and then pressurizing and impregnating the particles with a blowing agent.

4. The recycled styrene-based resin foamed molded article according to claim 3, wherein the ratio of the amount of the recycled styrene-based resin raw material particles (a) to the total amount of the recycled styrene-based resin raw material particles (a) and the styrene-based monomer is 50 mass% or more.

5. The recycled styrene-based resin foam molded article according to claim 3, wherein the polymerization initiator comprises a peroxyalkyl ester-based peroxide having a 10-hour half-life temperature of 65°C or higher.

6. The recycled styrene-based resin foam molded article according to claim 3, wherein the content ratio of the polyfunctional monomer relative to 100 parts by mass of the styrene-based monomer is 0.001 parts by mass to 0.049 parts by mass.

7. A recycled expandable styrene-based resin particle is obtained by adding a styrene-based monomer and a polyfunctional monomer to a suspension containing recycled styrene-based resin raw material particles (a) and polymerizing the mixture in the presence of a polymerization initiator to obtain recycled styrene-based resin particles (A), and then injecting a blowing agent into the recycled styrene-based resin particles (A), The recycled styrene-based resin foamed molding obtained by pre-expanding the recycled expandable styrene-based resin particles has a Z-average molecular weight Mz of 370,000 to 5,000,000 and a Z+1-average molecular weight Mz+1 of 2,000,000 to 15,000,000. Recycled expandable styrene resin particles.

8. The recycled expandable styrene-based resin particles according to claim 7, wherein the polymerization initiator contains a peroxyalkyl ester-based peroxide having a 10-hour half-life temperature of 65°C or higher.

9. The recycled expandable styrene-based resin particles according to claim 7, wherein the content ratio of the polyfunctional monomer to 100 parts by mass of the styrene-based monomer is 0.001 parts by mass to 0.049 parts by mass.

10. 10. Recycled pre-expanded styrene-based resin particles obtained by pre-expanding the recycled expandable styrene-based resin particles according to any one of claims 7 to 9.

Citation Information

Patent Citations

  • JP1974012567A

  • Reikyakuhoreiyomatsuto

    JP1976028246A

  • Reclaimed foamable sytrenic resin particle, method for producing the same, reclaimed styrenic foamed bead and reclaimed foamed styrenic resin molded article

    JP2006160905A

  • Recycling process for collected styrenic resin

    JP2007211230A

  • Method for producing spherical recycled expandable styrene resin particles

    JP3044942B2