Sensor element
The sensor element with a porous protective layer having varying porosity regions addresses thermal shock-induced cracks, enhancing water resistance and measurement accuracy by preventing oxygen reintroduction, ensuring reliable long-term operation.
Patent Information
- Application Number
- JP2023050553
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
- Estimated Expiration
- 2043-03-27
AI Technical Summary
Gas sensors face issues with cracks in their internal structure due to thermal shock when moisture adheres to high-temperature sensor elements, leading to reduced water resistance and measurement accuracy over time.
A sensor element design with a porous protective layer comprising an inner layer and an outer layer, where the porosity of the inner layer is lower in the front region than the main region, effectively reducing thermal shock and maintaining structural integrity and measurement accuracy.
The design enhances water resistance and maintains high measurement accuracy by preventing reintroduction of pumped oxygen, thus ensuring consistent sensor performance during long-term operation.
Smart Images

Figure 2024139556000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a sensor element for detecting a target gas contained in a measurement target gas. [Background technology]
[0002] Gas sensors detect the target gas components (oxygen, O 2 , nitrogen oxides NOx, ammonia NH 3 , Hydrocarbon HC, Carbon dioxide CO 2 These gas sensors are used to detect and measure the concentration of zirconia (ZrO 2 2. Description of the Related Art Gas sensors having a sensor element using an oxygen ion conductive solid electrolyte such as SiO 2 .
[0003] In such a gas sensor, it is known to form a porous protective layer on the surface of the sensor element in order to prevent cracks from occurring in the internal structure of the sensor element due to thermal shock caused by adhesion of moisture to the sensor element (for example, JP 2016-065852 A). That is, a sensor element having an element body and a porous protective layer covering the element body is known. In addition, for example, JP 2014-098590 A and International Publication WO2020 / 203029 A disclose a multi-layer protective layer, which includes an inner layer and an outer layer having a lower porosity than the inner layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2016-065852 A [Patent Document 2] JP 2014-098590 A [Patent Document 3] International Publication No. WO2020 / 203029 Summary of the Invention [Problem to be solved by the invention]
[0005] When a gas sensor measures a target gas, the sensor element becomes hot (for example, about 800°C). If moisture adheres to such a hot sensor element, there is a problem that cracks will occur in the internal structure of the sensor element due to thermal shock.
[0006] In a protective layer including an inner layer and an outer layer having a lower porosity than the inner layer (for example, the above-mentioned JP 2014-098590 A and WO 2020 / 203029 A), increasing the porosity of the inner layer improves the heat insulating performance of the protective layer. As a result, the occurrence of cracks in the internal structure of the sensor element when water is splashed on the sensor element (wetted) can be further suppressed. In other words, the water resistance of the sensor element can be improved. In addition, by providing an outer layer having a lower porosity than the inner layer, the structural strength of the protective layer as a whole can be maintained.
[0007] On the other hand, the gas sensor is required to maintain the measurement accuracy of the concentration of the target gas in the measurement gas even during long-term use.
[0008] SUMMARY OF THE PRESENT EMBODIMENTS Accordingly, an object of the present invention is to provide a sensor element that has high water resistance and can maintain high measurement accuracy. [Means for solving the problem]
[0009] The present inventors have conducted extensive research and have arrived at the present invention.
[0010] (1) An element body including a long plate-like base portion including an oxygen ion conductive solid electrolyte layer and a measurement target gas flow space formed on one end side of the base portion in the longitudinal direction; a porous protective layer formed from the one end of the base portion in the longitudinal direction and covering a predetermined length of the surface of the element body in the longitudinal direction; A sensor element comprising: the element body includes an intra-space electrode disposed in the measurement gas flow space, and an outer-space electrode corresponding to the intra-space electrode and having a predetermined length in the longitudinal direction of the base portion and disposed on one of two main surfaces of the element body at a predetermined distance from the one end, The protective layer is an inner layer covering the element body and an outer layer located outside the inner layer on at least the one main surface on which the outer electrode is present; and a main region including an electrode presence region in which the outer-space electrode is present and a rear region following the electrode presence region, and a front region extending from the one end of the base portion in the longitudinal direction to the electrode presence region, on the one principal surface on which the outer-space electrode is present, a porosity in the front region of the inner layer is less than a porosity in the main region of the inner layer; A sensor element for detecting a gas to be measured in a measurement target gas, wherein the porosity of the outer layer is lower than the porosity of the inner layer in the front region.
[0011] (2) The sensor element according to (1) above, wherein the porosity in the front region of the inner layer is at least 5 vol. % lower than the porosity in the main region of the inner layer.
[0012] (3) The sensor element according to (1) or (2) above, wherein the porosity in the front region of the inner layer is at least 10 volume % lower than the porosity in the main region of the inner layer.
[0013] (4) A sensor element described in any one of (1) to (3) above, wherein the rear region of the protective layer extends in the longitudinal direction of the base portion to a position farther from the one end of the base portion in the longitudinal direction than the measurement gas flow space.
[0014] (5) A sensor element described in any one of (1) to (4) above, wherein, on the one main surface on which the void outer electrode is present, the porosity of the inner layer increases stepwise or continuously in the longitudinal direction of the base portion from the one end of the base portion in the longitudinal direction. Effect of the Invention
[0015] According to the present invention, it is possible to provide a sensor element that has high water resistance and can maintain high measurement accuracy. [Brief description of the drawings]
[0016] [Figure 1] FIG. 2 is a perspective view showing an example of a schematic configuration of a sensor element 101. [Diagram 2] 2 is a schematic vertical sectional view in the longitudinal direction showing an example of a schematic configuration of a gas sensor 100 including a sensor element 101, the schematic sectional view including a sectional view of the sensor element 101 taken along line II-II in FIG. [Diagram 3] 3 is a schematic cross-sectional view of the same cross section as in FIG. 2, showing the configuration of a porous protective layer 90. In FIG. 3, configurations other than the measurement gas flow space 15, the space inner electrode, and the space outer electrode in the element body 102 are omitted from the illustration. [Figure 4] 4 is a schematic cross-sectional view of the sensor element 101 taken along the line IV-IV in Fig. 3. In Fig. 4, configurations other than the measurement gas flow space 15 (buffer space 12) inside the element body 102 are omitted from the illustration. [Diagram 5] 1 is a conceptual diagram showing the principle by which the measurement accuracy of oxygen decreases in a conventional sensor element. [Figure 6] 1 is a conceptual diagram showing how oxygen pumped out from inside a first inner space 20 diffuses in a sensor element 101 according to an embodiment of the present invention. FIG. [Figure 7] 4 is a flowchart showing an example of a method for manufacturing a sensor element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The sensor element of the present invention comprises: an element body including a long plate-like base portion including an oxygen ion conductive solid electrolyte layer and a measurement target gas flow space formed on one end side of the base portion in the longitudinal direction; a porous protective layer formed from the one end of the base portion in the longitudinal direction and covering a predetermined length of the surface of the element body in the longitudinal direction; Includes.
[0018] The element body includes an intra-space electrode disposed in the measurement gas flow space, and an outer-space electrode corresponding to the intra-space electrode and having a predetermined length in the longitudinal direction of the base portion and disposed on one of the two main surfaces of the element body at a predetermined distance from the one end.
[0019] The protective layer is an inner layer covering the element body and an outer layer located outside the inner layer on at least the one main surface on which the outer electrode is present; and a main region including an electrode presence region in which the outer-space electrode is present and a rear region following the electrode presence region, and a front region extending from the one end of the base portion in the longitudinal direction to the electrode presence region, on the one principal surface on which the outer-space electrode is present, a porosity in the front region of the inner layer is less than a porosity in the main region of the inner layer; The porosity of the outer layer is less than the porosity of the inner layer in the front region.
[0020] An embodiment of a gas sensor including a sensor element of the present invention will be described in detail below.
[0021] [Outline of gas sensor configuration] An embodiment of the gas sensor of the present invention will be described below with reference to the drawings. FIG. 1 is a perspective view showing an example of the schematic configuration of a sensor element 101. FIG. 2 is a schematic vertical longitudinal cross-sectional view showing an example of the schematic configuration of a gas sensor 100 including the sensor element 101. In FIG. 2, the cross-sectional view of the sensor element 101 is a schematic cross-sectional view taken along line II-II in FIG. 1. In the following, with reference to FIG. 2, the upper side of FIG. 2 is referred to as the upper side, the lower side as the lower side, the left side of FIG. 2 is referred to as the front end side, and the right side as the rear end side. With reference to FIG. 2, the front side perpendicular to the paper surface is referred to as the right side, and the back side is referred to as the left side.
[0022] In FIG. 2, a gas sensor 100 is an example of a limiting current type NOx sensor that detects NOx in a measurement gas by a sensor element 101 and measures the concentration of NOx.
[0023] The sensor element 101 includes a porous protective layer 90, which will be described in detail later. The porous protective layer 90 corresponds to a protective layer of the present invention. A portion of the sensor element 101 excluding the porous protective layer 90 will be referred to as an element body 102 below. The element body 102 is in the form of a long plate. As shown in FIG. 1, the element body 102 has six faces: two main faces (upper face 102a and lower face 102b), two side faces along the longitudinal direction (left face 102c and right face 102d), and two end faces in the longitudinal direction (front end face 102e and rear end face 102f).
[0024] The element body 102 of the sensor element 101 includes an intra-space electrode disposed in a measurement gas flow space 15 described below, and an outer-space electrode having a predetermined length in the longitudinal direction of the base portion 103 disposed on one of the two main surfaces of the element body 102 in correspondence with the intra-space electrode. The measurement gas flow space 15 also has a predetermined length in the longitudinal direction of the base portion 103. "In correspondence with the intra-space electrode" means that the outer-space electrode is disposed so as to be in contact with the intra-space electrode via a solid electrolyte layer.
[0025] In the sensor element 101 of this embodiment, the electrodes in the void are an inner main pump electrode 22, an auxiliary pump electrode 51, and a measurement electrode 44. As an electrode outside the void, an outer pump electrode 23 is provided on the upper surface 102a at a predetermined distance from the tip of the element body 102.
[0026] The sensor element 101 is a long plate-like element including a base portion 103 having a structure in which a plurality of oxygen ion conductive solid electrolyte layers are laminated. The long plate-like shape is also referred to as a long plate shape or a strip shape. The base portions 103 are each made of zirconia (ZrO 2 The first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6 are laminated in this order from the bottom as viewed in the drawing. The solid electrolyte forming these six layers is dense and airtight. The six layers may all have the same thickness, or each layer may have a different thickness. The layers are bonded to each other via an adhesive layer made of a solid electrolyte, and the base portion 103 includes the adhesive layer. In FIG. 2, a layer structure consisting of the six layers is illustrated as an example, but the layer structure in the present invention is not limited to this, and any number of layers and layer structure may be used.
[0027] A gas inlet 10 is formed at one end (hereinafter referred to as the tip) in the longitudinal direction of the sensor element 101, between the lower surface of the second solid electrolyte layer 6 and the upper surface of the first solid electrolyte layer 4. The measurement gas flow space 15, i.e., the measurement gas flow section, is formed in such a manner that a first diffusion rate-controlling section 11, a buffer space 12, a second diffusion rate-controlling section 13, a first internal space 20, a third diffusion rate-controlling section 30, a second internal space 40, a fourth diffusion rate-controlling section 60, and a third internal space 61 are adjacently formed in this order in the longitudinal direction from the gas inlet 10 and communicated with each other.
[0028] The gas inlet 10, the buffer space 12, the first internal void 20, the second internal void 40, and the third internal void 61 are spaces inside the sensor element 101, which are defined by an upper portion cut out of the spacer layer 5, the lower portion cut out by the upper surface of the first solid electrolyte layer 4, and the sides cut out by the side surfaces of the spacer layer 5.
[0029] The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, and the third diffusion rate-controlling section 30 are each provided as two horizontally elongated slits (the openings have their longitudinal direction in the direction perpendicular to the plane of the drawing in FIG. 2). The first diffusion rate-controlling section 11, the second diffusion rate-controlling section 13, and the third diffusion rate-controlling section 30 may each have any shape that provides a desired diffusion resistance, and the shape is not limited to the slits.
[0030] The fourth diffusion rate-controlling portion 60 is provided as a single horizontally elongated slit (the opening has its longitudinal direction perpendicular to the plane of the drawing in FIG. 2) between the spacer layer 5 and the second solid electrolyte layer 6. The fourth diffusion rate-controlling portion 60 may have any shape that provides a desired diffusion resistance, and the shape is not limited to the slit.
[0031] Further, at a position farther from the tip side than the measurement gas flow space 15, between the upper surface of the third substrate layer 3 and the lower surface of the spacer layer 5, a reference gas introduction space 43 is provided at a position defined at its side by the side surface of the first solid electrolyte layer 4. The reference gas introduction space 43 has an opening at the other end (hereinafter referred to as the rear end) of the sensor element 101. For example, air is introduced into the reference gas introduction space 43 as a reference gas when measuring the NOx concentration.
[0032] The air introducing layer 48 is a layer made of porous alumina, and a reference gas is introduced into the air introducing layer 48 through the reference gas introducing space 43. In addition, the air introducing layer 48 is formed so as to cover the reference electrode 42.
[0033] The reference electrode 42 is an electrode formed in a manner to be sandwiched between the upper surface of the third substrate layer 3 and the first solid electrolyte layer 4, and as described above, the air introduction layer 48 connected to the reference gas introduction space 43 is provided around it. That is, the reference electrode 42 is disposed so as to be in contact with the reference gas via the porous air introduction layer 48 and the reference gas introduction space 43. As will be described later, the reference electrode 42 can be used to measure the oxygen concentration (oxygen partial pressure) in the first internal space 20, the second internal space 40, and the third internal space 61. The reference electrode 42 is a porous cermet electrode (e.g., Pt and ZrO 2 The electrode is formed as a cermet electrode with a ferrite core.
[0034] In the measurement gas flow space 15 , the gas inlet 10 opens to the outside space, and the measurement gas is introduced into the sensor element 101 from the outside space through the gas inlet 10 .
[0035] In this embodiment, the measurement gas is introduced into the measurement gas flow space 15 through the gas inlet 10 opening at the tip end surface of the sensor element 101, but the present invention is not limited to this. For example, the measurement gas flow space 15 does not need to have a recess for the gas inlet 10. In this case, the first diffusion rate-controlling part 11 essentially serves as the gas inlet.
[0036] Also, for example, the measurement gas flow space 15 may be configured so that the measurement gas is introduced through a porous body.
[0037] The first diffusion rate-controlling portion 11 is a portion that applies a predetermined diffusion resistance to the measurement gas taken in through the gas inlet 10.
[0038] The buffer space 12 is a space provided for guiding the measurement gas introduced from the first diffusion rate-controlling portion 11 to the second diffusion rate-controlling portion 13 .
[0039] The second diffusion rate-controlling portion 13 is a portion that imparts a predetermined diffusion resistance to the measurement gas introduced from the buffer space 12 into the first internal space 20 .
[0040] As a result, it is sufficient that the amount of the measurement gas introduced into the first internal space 20 is within a predetermined range. In other words, it is sufficient that a predetermined diffusion resistance is imparted to the entire area from the tip of the sensor element 101 to the second diffusion rate-controlling section 13. For example, it is also possible to adopt an embodiment in which the first diffusion rate-controlling section 11 directly communicates with the first internal space 20, that is, the buffer space 12 and the second diffusion rate-controlling section 13 do not exist.
[0041] The buffer space 12 is a space provided to reduce the influence of pressure fluctuations on the detection value when the pressure of the gas to be measured fluctuates.
[0042] When the measurement gas is introduced from the outside of the sensor element 101 into the first internal space 20, the measurement gas is suddenly taken into the sensor element 101 from the gas inlet 10 due to pressure fluctuations of the measurement gas in the external space (exhaust pressure pulsations if the measurement gas is automobile exhaust gas), but is not introduced directly into the first internal space 20, but is introduced into the first internal space 20 after the pressure fluctuations of the measurement gas are canceled through the first diffusion rate-controlling section 11, buffer space 12, and second diffusion rate-controlling section 13. As a result, the pressure fluctuations of the measurement gas introduced into the first internal space can be almost ignored.
[0043] The first internal space 20 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the second diffusion rate-controlling part 13. The oxygen partial pressure is adjusted by the operation of the main pump cell 21.
[0044] The main pump cell 21 is an electrochemical pump cell including an inner main pump electrode 22, which is a space inside electrode disposed in the measurement gas flow space 15, and an outer pump electrode 23, which is a space outside electrode disposed so as to be in contact with the inner main pump electrode 22 via a solid electrolyte (second solid electrolyte layer 6 in FIG. 2). The outer pump electrode 23 is disposed on an upper surface 102a of the two main surfaces of the element body 102.
[0045] That is, the main pump cell 21 is an electrochemical pump cell including an inner main pump electrode 22 having a ceiling electrode portion 22a provided on almost the entire lower surface of the second solid electrolyte layer 6 facing the first internal space 20, an outer pump electrode 23 provided in a region corresponding to the ceiling electrode portion 22a on the upper surface of the second solid electrolyte layer 6 so as to be exposed to the external space, and the second solid electrolyte layer 6 sandwiched between these electrodes.
[0046] The inner main pump electrode 22 is disposed facing the first internal space 20. That is, the inner main pump electrode 22 is formed across the upper and lower solid electrolyte layers (the second solid electrolyte layer 6 and the first solid electrolyte layer 4) that partition the first internal space 20, and the spacer layer 5 that provides the side walls. Specifically, a ceiling electrode portion 22a is formed on the lower surface of the second solid electrolyte layer 6 that provides the ceiling surface of the first internal space 20, and a bottom electrode portion 22b is formed on the upper surface of the first solid electrolyte layer 4 that provides the bottom surface. Side electrode portions (not shown) are formed on the side wall surfaces (inner surfaces) of the spacer layer 5 that constitute both side wall portions of the first internal space 20 so as to connect the ceiling electrode portion 22a and the bottom electrode portion 22b, and are disposed in a tunnel-shaped structure at the positions where the side electrode portions are disposed.
[0047] The inner main pump electrode 22 and the outer pump electrode 23 are porous cermet electrodes (e.g., Pt containing 1% Au and ZrO 2 The inner main pump electrode 22 that comes into contact with the measurement gas is formed using a material that has a reduced ability to reduce the NOx component in the measurement gas.
[0048] In the main pump cell 21, by applying a desired pump voltage Vp0 between the inner main pump electrode 22 and the outer pump electrode 23 by a variable power supply 24 and flowing a pump current Ip0 in a positive or negative direction between the inner main pump electrode 22 and the outer pump electrode 23, it is possible to pump oxygen in the first internal space 20 out to the external space, or to pump oxygen from the external space into the first internal space 20.
[0049] In addition, in order to detect the oxygen concentration (oxygen partial pressure) in the atmosphere in the first internal space 20, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 80 for controlling the main pump, is configured by the inner main pump electrode 22, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, and the reference electrode 42.
[0050] The oxygen concentration (oxygen partial pressure) in the first internal space 20 can be determined by measuring the electromotive force V0 in the main pump control oxygen partial pressure detection sensor cell 80. Furthermore, the pump current Ip0 is controlled by feedback controlling the voltage Vp0 of the variable power supply 24 so that the electromotive force V0 is constant. This allows the oxygen concentration in the first internal space 20 to be maintained at a predetermined constant value.
[0051] The third diffusion rate-controlling section 30 is a section that applies a predetermined diffusion resistance to the measurement gas whose oxygen concentration (oxygen partial pressure) has been controlled by the operation of the main pump cell 21 in the first internal space 20, and guides the measurement gas to the second internal space 40.
[0052] The second internal space 40 is provided as a space for adjusting the oxygen partial pressure in the measurement gas introduced through the third diffusion-controlling section 30 with higher accuracy. The oxygen partial pressure is adjusted by the operation of the auxiliary pump cell 50. The second internal space 40 and the auxiliary pump cell 50 may be omitted. From the viewpoint of the accuracy of the adjustment of the oxygen partial pressure, it is more preferable that the second internal space 40 and the auxiliary pump cell 50 are provided.
[0053] In the second internal space 40, the oxygen concentration (oxygen partial pressure) is adjusted in advance in the first internal space 20, and then the oxygen partial pressure of the measurement gas introduced through the third diffusion rate-controlling part is further adjusted by the auxiliary pump cell 50. This makes it possible to keep the oxygen concentration in the second internal space 40 constant with high accuracy, thereby enabling the gas sensor 100 to measure the NOx concentration with high accuracy.
[0054] The auxiliary pump cell 50 is an electrochemical pump cell including an auxiliary pump electrode 51, which is an inner-space electrode, disposed in the measurement gas flow space 15 at a position farther from the tip of the base portion 103 than the inner main pump electrode 22 is, and an outer pump electrode 23, which is an outer-space electrode, disposed so as to be in contact with the auxiliary pump electrode 51 via a solid electrolyte (in FIG. 2, the second solid electrolyte layer 6).
[0055] That is, the auxiliary pump cell 50 is an auxiliary electrochemical pump cell constituted by an auxiliary pump electrode 51 having a ceiling electrode portion 51a provided over substantially the entire lower surface of the second solid electrolyte layer 6 facing the second internal space 40, an outer pump electrode 23 (not limited to the outer pump electrode 23, but any suitable electrode located in a position other than within the measurement gas flow space 15, for example, outside the sensor element 101, will suffice), and the second solid electrolyte layer 6.
[0056] The auxiliary pump electrode 51 is disposed in the second internal space 40 in a tunnel-shaped structure similar to that of the inner main pump electrode 22 provided in the first internal space 20. That is, a ceiling electrode portion 51a is formed on the second solid electrolyte layer 6 providing the ceiling surface of the second internal space 40, and a bottom electrode portion 51b is formed on the first solid electrolyte layer 4 providing the bottom surface of the second internal space 40. Furthermore, side electrode portions (not shown) connecting the ceiling electrode portion 51a and the bottom electrode portion 51b are formed on both wall surfaces of the spacer layer 5 providing the side walls of the second internal space 40, forming a tunnel-shaped structure.
[0057] Like the inner main pump electrode 22, the auxiliary pump electrode 51 is also made of a material with a reduced ability to reduce the NOx component in the measurement gas.
[0058] In the auxiliary pump cell 50, by applying a desired voltage Vp1 between the auxiliary pump electrode 51 and the outer pump electrode 23 by a variable power supply 52, it is possible to pump oxygen in the atmosphere within the second internal space 40 out to the external space or pump oxygen from the external space into the second internal space 40.
[0059] In addition, in order to control the oxygen partial pressure in the atmosphere within the second internal space 40, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, is constituted by the auxiliary pump electrode 51, the reference electrode 42, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, and the third substrate layer 3.
[0060] The auxiliary pump cell 50 performs pumping using a variable power supply 52 whose voltage is controlled based on the electromotive force V1 detected by the auxiliary pump control oxygen partial pressure detection sensor cell 81. This allows the oxygen partial pressure in the atmosphere in the second internal space 40 to be controlled to a low partial pressure that does not substantially affect the measurement of NOx.
[0061] In addition, the pump current Ip1 is used to control the electromotive force of the main pump control oxygen partial pressure detection sensor cell 80. Specifically, the pump current Ip1 is input as a control signal to the main pump control oxygen partial pressure detection sensor cell 80, and the electromotive force V0 is controlled so that the gradient of the oxygen partial pressure in the measurement gas introduced from the third diffusion rate-controlling part 30 into the second internal space 40 is always constant. When used as a NOx sensor, the oxygen concentration in the second internal space 40 is kept at a constant value of about 0.001 ppm by the action of the main pump cell 21 and the auxiliary pump cell 50.
[0062] The fourth diffusion rate-controlling section 60 is a section that applies a predetermined diffusion resistance to the measurement gas, the oxygen concentration (oxygen partial pressure) of which has been controlled to be even lower in the second internal space 40 by the operation of the auxiliary pump cell 50, and guides the measurement gas to the third internal space 61.
[0063] The third internal space 61 is provided as a space for measuring the concentration of nitrogen oxides (NOx) in the measurement gas introduced through the fourth diffusion-controlling portion 60. The NOx concentration is measured by the operation of the measuring pump cell 41.
[0064] The measurement pump cell 41 measures the NOx concentration in the measurement gas in the third internal space 61. The measurement pump cell 41 is an electrochemical pump cell including a measurement electrode 44 as an inner-space electrode disposed in the measurement gas flow space 15 at a position farther from the tip of the base portion 103 than the auxiliary pump electrode 51 is, and an outer pump electrode 23 as an outer-space electrode disposed so as to be in contact with the measurement electrode 44 via a solid electrolyte (in FIG. 2, the second solid electrolyte layer 6, the spacer layer 5, and the first solid electrolyte layer 4).
[0065] That is, the measurement pump cell 41 is an electrochemical pump cell constituted by a measurement electrode 44 provided on the upper surface of the first solid electrolyte layer 4 facing the third internal space 61, an outer pump electrode 23 (not limited to the outer pump electrode 23, but a suitable electrode at a position other than within the measurement gas flow space 15, for example, outside the sensor element 101, will suffice), the second solid electrolyte layer 6, the spacer layer 5, and the first solid electrolyte layer 4.
[0066] The measurement electrode 44 is a porous cermet electrode. The measurement electrode 44 also functions as a NOx reduction catalyst that reduces NOx present in the atmosphere in the third internal space 61. The measurement electrode 44 contains, as a metal component, a precious metal having catalytic activity (e.g., at least one of Pt, Rh, Ir, Ru, and Pd).
[0067] In the measurement pump cell 41, oxygen produced by decomposition of nitrogen oxides in the atmosphere surrounding the measurement electrode 44 is pumped out, and the amount of oxygen produced can be detected as a pump current Ip2.
[0068] In order to detect the oxygen partial pressure around the measurement electrode 44, an electrochemical sensor cell, i.e., an oxygen partial pressure detection sensor cell 82 for controlling the measurement pump, is configured by the first solid electrolyte layer 4, the third substrate layer 3, the measurement electrode 44, and the reference electrode 42. The variable power supply 46 is controlled based on the electromotive force V2 detected by the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump.
[0069] The measurement gas introduced into the second internal space 40 reaches the measurement electrode 44 through the fourth diffusion rate-controlling part 60 under conditions in which the oxygen partial pressure is controlled. Nitrogen oxides in the measurement gas around the measurement electrode 44 are reduced (2NO→N 2 +O 2 ) oxygen is generated. The generated oxygen is then pumped by the measurement pump cell 41, and at that time, the voltage Vp2 of the variable power supply 46 is controlled so that the electromotive force V2 detected by the measurement pump control oxygen partial pressure detection sensor cell 82 is kept constant. Since the amount of oxygen generated around the measurement electrode 44 is proportional to the concentration of nitrogen oxides in the measurement gas, the pump current Ip2 in the measurement pump cell 41 is used to calculate the concentration of nitrogen oxides in the measurement gas.
[0070] Furthermore, by combining the measurement electrode 44, the first solid electrolyte layer 4, the third substrate layer 3 and the reference electrode 42 to form an oxygen partial pressure detection means as an electrochemical sensor cell, it is possible to detect an electromotive force corresponding to the difference between the amount of oxygen generated by reduction of the NOx components in the atmosphere around the measurement electrode 44 and the amount of oxygen contained in the reference atmosphere, thereby making it possible to determine the concentration of the NOx components in the measured gas.
[0071] In addition, the second solid electrolyte layer 6, the spacer layer 5, the first solid electrolyte layer 4, the third substrate layer 3, the outer pump electrode 23, and the reference electrode 42 constitute an electrochemical sensor cell 83, and the electromotive force Vref obtained by this sensor cell 83 makes it possible to detect the oxygen partial pressure in the measurement gas outside the sensor.
[0072] In the gas sensor 100 having such a configuration, the main pump cell 21 and the auxiliary pump cell 50 are operated to supply a measurement gas in which the oxygen partial pressure is always kept at a constant low value (a value that has substantially no effect on the measurement of NOx) to the measurement pump cell 41. Therefore, the NOx concentration in the measurement gas can be known based on the pump current Ip2 that flows when oxygen generated by the reduction of NOx is pumped out of the measurement pump cell 41, which is approximately proportional to the NOx concentration in the measurement gas.
[0073] Furthermore, in order to increase the oxygen ion conductivity of the solid electrolyte, the sensor element 101 includes a heater section 70 that adjusts the temperature by heating and keeping the sensor element 101 warm. The heater section 70 includes a heater electrode 71, a heater 72, a heater lead 76, a through hole 73, a heater insulating layer 74, and a pressure relief hole 75.
[0074] The heater electrode 71 is an electrode formed in a manner to contact the lower surface of the first substrate layer 1. By connecting the heater electrode 71 to a heater power supply, which is an external power supply, it is possible to supply power to the heater section 70 from the outside.
[0075] The heater 72 is an electrical resistor sandwiched between the second substrate layer 2 and the third substrate layer 3. The heater 72 is connected to a heater electrode 71 via a heater lead 76 that is connected to the heater 72 and extends to the rear end side of the sensor element 101 in the longitudinal direction, and a through hole 73. The heater 72 generates heat when power is supplied from the outside through the heater electrode 71, and heats and keeps warm the solid electrolyte that forms the sensor element 101.
[0076] The heater 72 is embedded throughout the entire area from the first internal space 20 to the third internal space 61, making it possible to adjust the entire sensor element 101 to a temperature at which the solid electrolyte is activated. The temperature needs to be adjusted so that the main pump cell 21, the auxiliary pump cell 50, and the measurement pump cell 41 can operate. It is not necessary to adjust these entire areas to the same temperature, and the sensor element 101 may have a temperature distribution.
[0077] In the sensor element 101 of this embodiment, the heater 72 is embedded in the base portion 103, but the present invention is not limited to this. The heater 72 may be disposed so as to heat the base portion 103. That is, the heater 72 may be capable of heating the sensor element 101 to an extent that the sensor element 101 exhibits oxygen ion conductivity that allows the above-mentioned main pump cell 21, auxiliary pump cell 50, and measurement pump cell 41 to operate. For example, the heater 72 may be embedded in the base portion 103 as in this embodiment. Alternatively, the heater portion 70 may be formed as a heater substrate separate from the base portion 103 and disposed adjacent to the base portion 103.
[0078] The heater insulating layer 74 is an insulating layer made of an insulator such as alumina and formed on the upper and lower surfaces of the heater 72 and the heater lead 76. The heater insulating layer 74 is formed for the purpose of obtaining electrical insulation between the second substrate layer 2 and the heater 72 and the heater lead 76, and between the third substrate layer 3 and the heater 72 and the heater lead 76.
[0079] The pressure relief hole 75 is formed to penetrate the third substrate layer 3 and to communicate between the heater insulating layer 74 and the reference gas introduction space 43. The pressure relief hole 75 can mitigate an increase in internal pressure that accompanies an increase in temperature within the heater insulating layer 74. Note that the pressure relief hole 75 may be omitted.
[0080] (protective layer) The sensor element 101 includes the above-mentioned element body 102, and a porous protective layer 90 formed from one longitudinal end (tip) of the element body 102 (base portion 103) and covering a predetermined length L of the surface of the element body 102 in the longitudinal direction. Here, the one longitudinal end of the element body 102 is the end on the side where the measurement gas flow space 15 is formed, that is, the tip of the element body 102. The element body 102 is in the form of a long plate, and the upper surface 102a and the lower surface 102b of the element body 102 are main surfaces. The left surface 102c and the right surface 102d are sometimes referred to as side surfaces, and the tip surface 102e and the rear end surface 102f are sometimes referred to as end surfaces.
[0081] The porous protective layer 90 includes, at least on the one main surface (upper surface 102a) where the outer space electrode (in this embodiment, the outer pump electrode 23) is present, an inner layer 91 that covers the element body 102, and an outer layer 92 located outside the inner layer 91. Also, on the one main surface (upper surface 102a), in the longitudinal direction of the element body 102 (base portion 103), there is a main region including an electrode presence region where the outer space electrode is present and a rear region continuing to the other end side of the electrode presence region, and a front region from the one longitudinal end of the base portion to the electrode presence region.
[0082] The porous protective layer 90 is made of a porous body. Examples of the material of the porous protective layer 90 include alumina, zirconia, spinel, cordierite, mullite, titania, and magnesia. Any one of these may be used, or two or more may be used. The material of the inner layer 91 and the material of the outer layer 92 may be the same or different from each other. In this embodiment, the porous protective layer 90 (the inner layer 91 and the outer layer 92) is made of an alumina porous body.
[0083] In this embodiment, the porous protective layer 90 covers a predetermined range (a portion indicated by a broken line in FIG. 1) of the element body 102 in the longitudinal direction from the tip of the element body 102. More specifically, the porous protective layer 90 covers the entire region of the upper surface 102a of the element body 102, which has a predetermined length L in the longitudinal direction from the tip of the element body 102. The porous protective layer 90 covers the entire region of the lower surface 102b of the element body 102, which has a length L in the longitudinal direction from the tip of the element body 102. The porous protective layer 90 covers the entire region of the left surface 102c of the element body 102, which has a length L in the longitudinal direction from the tip of the element body 102. The porous protective layer 90 covers the entire region of the right surface 102d of the element body 102, which has a length L in the longitudinal direction from the tip of the element body 102. The porous protective layer 90 covers the entire tip surface 102e of the element body 102.
[0084] The inner layer 91 is formed on the main surface (upper surface 102a) of the element body 102 on which at least the void outer electrode (outer pump electrode 23) is present, so as to cover a predetermined range in the longitudinal direction from the tip of the element body 102. In this embodiment, the inner layer 91 covers the entire region of the surface of the element body 102, which has a predetermined length L in the longitudinal direction from the tip of the element body 102. The outer layer 92 is located outside the inner layer 91. In this embodiment, the outer layer 92 is formed so as to cover the entire surface of the inner layer 91. In other words, the outer layer 92 covers the entire region of the surface of the inner layer 91, which has a predetermined length L in the longitudinal direction from the tip of the element body 102.
[0085] Thus, in this embodiment, the porous protective layer 90 is composed of two layers, an inner layer 91 and an outer layer 92, on each surface (upper surface 102a, lower surface 102b, left surface 102c, right surface 102d, and tip surface 102e) of the element body 102. That is, in this embodiment, the longitudinal length of the inner layer 91 from the tip of the element body 102 is approximately the same as the longitudinal length of the outer layer 92 from the tip of the element body 102. In the following, the upper surface 102a is also referred to as the pump surface 102a. In addition, the main surface (lower surface 102b) facing the pump surface 102a out of the two main surfaces of the element body 102 is also referred to as the heater surface 102b.
[0086] Fig. 3 is a schematic cross-sectional view of the same cross section as Fig. 2, showing the structure of the porous protective layer 90. In Fig. 3, the structure inside the element body 102 is omitted from the illustration, except for the measurement gas flow space 15, the electrode inside the space, and the electrode outside the space. Fig. 4 is a schematic cross-sectional view of the sensor element 101 taken along line IV-IV in Fig. 3, i.e., a schematic cross-sectional view perpendicular to the longitudinal direction of the sensor element 101. In Fig. 4, the structure inside the element body 102 is omitted from the illustration, except for the measurement gas flow space 15 (buffer space 12).
[0087] As shown in FIG. 3, the outer pump electrode 23 is disposed on the pump surface 102a at a predetermined interval from the tip of the element body 102 (base portion 103). The outer pump electrode 23 may be disposed at a position where oxygen can be pumped out from each of the internal spaces 20, 40, 61. The predetermined interval from the tip of the element body 102 is not particularly limited, but the outer pump electrode 23 may be disposed at a position corresponding to the cavity electrodes (at least one of the inner main pump electrode 22, the auxiliary pump electrode 51, and the measurement electrode 44) in the longitudinal direction of the element body 102 (base portion 103). For example, the outer pump electrode 23 may be disposed at a position corresponding to at least one of the internal spaces 20, 40, 61. For example, the outer pump electrode 23 may be disposed at a position corresponding to the first internal space 20. The outer pump electrode 23 may be disposed at a predetermined interval corresponding to the front portion (the portion from the gas inlet 10 to the second diffusion rate-controlling portion 13) for introducing the measurement gas into the first internal space 20.
[0088] As shown in FIG. 3, in the longitudinal direction of the element body 102 (base part 103), the region of the porous protective layer 90 on the pump surface 102a of the element body 102 where the outer pump electrode 23 exists is referred to as the electrode presence region 90E. In addition, the region of the porous protective layer 90 on the pump surface 102a of the element body 102 that continues to the rear of the electrode presence region 90E, that is, the region from the rear end of the electrode presence region 90E to the rear end of the porous protective layer 90 is referred to as the rear region 90P. The rear region 90P is the region from the position farthest from the one end (tip) of the electrode presence region 90E to the position farthest from the one end (tip) of the porous protective layer 90 (the rear end of the porous protective layer 90). The region consisting of the electrode presence region 90E and the rear region 90P is referred to as the main region 90M. The region of the porous protective layer 90 on the pump surface 102a of the element body 102 from the tip of the element body 102 (base portion 103) to the tip of the electrode presence region 90E is referred to as the front region 90A. That is, the front region 90A is a region occupying the predetermined distance from the one end (tip) of the element body 102 in the longitudinal direction to the position of the electrode presence region 90E closest to the one end (tip). That is, the rear end of the front region 90A and the tip of the electrode presence region 90E are in contact with each other, and the rear end of the electrode presence region 90E and the tip of the rear region 90P are in contact with each other. The rear end of the front region 90A and the tip of the main region 90M are in contact with each other.
[0089] In the porous protective layer 90, the porosity of the front region 91A of the inner layer 91 is lower than the porosity of the main region 91M of the inner layer 91. The front region 91A of the inner layer 91 is a region of the inner layer 91 occupying a predetermined longitudinal length (the predetermined interval) from the one longitudinal end (tip) of the element body 102 to the one electrode end (tip) of the outer pump electrode 23 on the side closer to the one longitudinal end. The porosity of the outer layer 92 is lower than the porosity of the front region 91A of the inner layer 91. The porosity of the outer layer 92 is usually lower than the porosity at any position of the inner layer 91. The porosity will be described in detail later.
[0090] As shown in FIG. 3, in the porous protective layer 90 of this embodiment, the inner layer 91 on the tip surface 102e does not have a low porosity region corresponding to the front region 91A, and has a porosity equivalent to that of the main region 91M. Also, as shown in FIG. 4, in the porous protective layer 90 of this embodiment, the inner layers 91b, 91c, and 91d on the surfaces 102b, 102c, and 102d other than the pump surface 102a of the inner layer 91 do not have a low porosity region corresponding to the front region 91A, and have a porosity equivalent to that of the main region 91M over the entire area in the longitudinal direction. Also, in the porous protective layer 90 of this embodiment, each corner shown in FIG. 3 and FIG. 4 does not have a low porosity region corresponding to the front region 91A, and has a porosity equivalent to that of the main region 91M.
[0091] 2 and 3, the porous protective layer 90 also covers the gas inlet 10. However, since the porous protective layer 90 is a porous body, the gas to be measured can flow through the inside of the porous protective layer 90 and reach the gas inlet 10. Therefore, the gas to be measured can be detected and measured without any problems.
[0092] The porous protective layer 90 plays a role in suppressing the occurrence of cracks in the internal structure of the element body 102, for example, when water splashes on the high-temperature sensor element 101 during operation of the gas sensor. Water that reaches the sensor element 101 does not adhere directly to the surface of the element body 102, but adheres to the porous protective layer 90. The surface of the porous protective layer 90 is rapidly cooled by the adhered water, but the thermal shock applied to the element body 102 is reduced due to the insulating effect of the porous protective layer 90. As a result, it is possible to suppress the occurrence of cracks in the internal structure of the element body 102. In other words, the water resistance of the sensor element 101 is improved.
[0093] In the porous protective layer 90, the inner layer 91 mainly plays a role of suppressing heat conduction from the surface of the sensor element 101 (the surface of the porous protective layer 90) to the element body 102. That is, the inner layer 91 has a function of reducing thermal shock applied to the element body 102 due to the heat insulating effect of the inner layer 91. In addition, the outer layer 92, which has a lower porosity than the inner layer 91, mainly has a function of maintaining the structural strength of the porous protective layer 90 as a whole. In addition, the outer layer 92 also has a function of preventing water droplets from penetrating into the inside of the porous protective layer 90 (inside the inner layer 91). This prevents water droplets from evaporating inside the inner layer 91, and reduces thermal shock applied to the element body 102.
[0094] In addition, the porous protective layer 90 covers the outer pump electrode 23. The porous protective layer 90 also plays a role in suppressing the adhesion of oil components and the like contained in the measured gas to the outer pump electrode 23, thereby suppressing deterioration of the outer pump electrode 23.
[0095] The present inventors have found that in a conventional sensor element having a porous protective layer including an inner layer and an outer layer, when the sensor element is continuously driven for a long period of time, the measurement target gas (e.g., oxygen O 2 It was found that the measurement accuracy of nitrogen oxides (NOx, etc.) may decrease. In particular, it is thought that the measurement accuracy of oxygen may decrease.
[0096] The present inventors have thoroughly investigated the causes of this problem. Fig. 5 is a conceptual diagram showing the principle of the deterioration of the oxygen measurement accuracy in a conventional sensor element. For the sake of convenience, Fig. 5 conceptually shows the gas inlet 10, the first internal space 20, the inner main pump electrode 22, and the outer pump electrode 23 of the element body 102. That is, the configuration of the main pump cell 21 is conceptually shown. In addition, oxygen O 25, the porous protective layer 990 is composed of an inner layer 991 having a uniform porosity and an outer layer 92 having a lower porosity than the inner layer 991. The measurement gas is introduced into the first inner space 20 from the gas inlet 10. Oxygen in the measurement gas is pumped out of the first inner space 20 to the outside of the element body 102 (into the inner layer 991 near the outer pump electrode 23) by applying a voltage between the inner main pump electrode 22 and the outer pump electrode 23. At that time, a pump current corresponding to the oxygen concentration in the gas introduced into the first inner space 20 flows between the inner main pump electrode 22 and the outer pump electrode 23. Therefore, the oxygen concentration in the measurement gas can be measured from the current value of this pump current.
[0097] The inner layer 991 is covered with the outer layer 92 having a low porosity. Therefore, oxygen pumped out from the first internal space 20 to the vicinity of the outer pump electrode 23 mainly diffuses in the inner layer 991 in the longitudinal direction of the element body 102. A small amount of oxygen also diffuses through the outer layer 92 (not shown). Since the porosity of the inner layer 991 is uniform, it is considered that the pumped out oxygen diffuses to the same extent in both the front end direction and the rear end direction of the element body 102 in the longitudinal direction of the inner layer 991.
[0098] The oxygen that has been pumped out of the first internal space 20 and then diffused toward the tip of the element body 102 may be introduced (reintroduced) into the first internal space 20 again through the gas inlet 10 at the tip surface 102e of the element body 102. In this case, in addition to the gas to be measured, the oxygen already pumped out of the first internal space 20 is introduced into the first internal space 20. As a result, there is a concern that the oxygen concentration in the first internal space 20 will be higher than the actual oxygen concentration in the gas to be measured. As described above, the current value of the pump current flowing between the inner main pump electrode 22 and the outer pump electrode 23 is a value corresponding to the oxygen concentration in the gas introduced into the first internal space 20, so it is considered that the oxygen concentration calculated from the current value of this pump current may be higher than the actual oxygen concentration in the gas to be measured. In other words, there is a concern that the measurement accuracy of the oxygen concentration will decrease. In addition, since the oxygen concentration in the first internal space 20 becomes higher than the actual oxygen concentration in the measurement gas, it is considered that the concentration of the measurement target gas other than oxygen (e.g., NOx) in the measurement gas may become relatively lower than the actual measurement target gas concentration in the measurement gas. As a result, the measurement accuracy of the measurement target gas other than oxygen (e.g., NOx) may also decrease.
[0099] When oxygen pumped out of the first internal space 20 is reintroduced into the first internal space 20, it is considered to occur continuously. Therefore, it is considered that the oxygen concentration in the first internal space 20 gradually becomes higher than the actual oxygen concentration in the measurement gas as the driving time of the gas sensor becomes longer. In other words, there is a concern that the measurement accuracy may decrease when the gas sensor is driven continuously for a long period of time.
[0100] On the other hand, the oxygen that has diffused toward the rear end is released from the rear end of the porous protective layer 990 into the external space of the sensor element 101. In this case, the oxygen pumped out from the first internal space 20 is not reintroduced into the first internal space 20 as described above, so the measurement accuracy of the oxygen concentration is maintained.
[0101] As a result of further intensive research, the inventors have found that the occurrence of the above-mentioned reintroduction can be suppressed by making the porosity of the front region 91A of the inner layer 91 of the protective layer (porous protective layer 90) lower than the porosity of the main region 91M following the front region 91A. FIG. 6 is a conceptual diagram showing the diffusion of oxygen pumped out from the first internal space 20 in a sensor element 101 according to one embodiment of the present invention. As in FIG. 5, FIG. 6 conceptually shows the gas inlet 10, the first internal space 20, the inner main pump electrode 22, and the outer pump electrode 23 of the configuration of the element body 102 for ease of explanation. In addition, oxygen O 2 , which is one of the gas components of the measured gas, is not shown in FIG. 6. 2 Only the
[0102] As in the case of the conventional sensor element, the oxygen pumped out from the first internal space 20 mainly diffuses in the inner layer 91 in the longitudinal direction of the element body 102. However, since the porosity of the front region 91A of the inner layer 91 is lower than that of the main region 91M of the inner layer 91, the diffusion toward the front end of the element body 102 (broken arrow) is suppressed, and the diffusion toward the rear end (solid arrow) becomes the main diffusion. The oxygen that diffuses toward the rear end is released from the rear end of the porous protective layer 90 to the external space of the sensor element 101. In this way, in the sensor element 101, the occurrence of reintroduction of the oxygen pumped out from the first internal space 20 into the first internal space 20 can be suppressed, so that the measurement accuracy of the oxygen concentration can be maintained high. By providing a difference in porosity between the front region 91A and the main region 91M, the diffusion toward the rear end can be promoted and the reintroduction can be suppressed, so that the measurement accuracy of the oxygen concentration can be maintained high.
[0103] The porous protective layer 90 (particularly the inner layer 91) may cover a portion of the element body 102 that becomes hot when the gas sensor is operated. The longitudinal length L of the entire porous protective layer 90 and the longitudinal length LA of the inner layer 91 may be appropriately determined within a range longer than the longitudinal length from the tip surface of the element body 102 to the rear end of the electrode outside the void (the outer pump electrode 23) and less than the longitudinal total length of the element body 102, based on the range of the element body 102 exposed to the measured gas in the gas sensor 100, the position of the outer pump electrode 23, the position of the measured gas flow void 15, the temperature distribution of the element body 102, and the like.
[0104] The porous protective layer 90 covers at least the portion of the element body 102 from the tip of the element body 102 to the rear end of the outer pump electrode 23 in the longitudinal direction of the element body 102. Preferably, the porous protective layer 90 covers at least the portion from the tip of the element body 102 to the rear end of the measurement gas flow space 15. That is, the rear region 90P (rear region 91P of the inner layer 91) of the porous protective layer 90 extends in the longitudinal direction of the base portion 103 to a position farther from the one end (tip) in the longitudinal direction of the base portion 103 than the measurement gas flow space 15. When the gas sensor is driven, the position where the measurement gas flow space 15 exists is usually at a high temperature to the extent that the oxygen ion conductivity of the solid electrolyte is expressed. By covering such a range with the porous protective layer 90, the thermal shock applied to the high-temperature portion of the element body 102 can be effectively reduced.
[0105] Also, for example, the porous protective layer 90 may cover almost the entire part of the element body 102 exposed to the measurement gas. For example, the porous protective layer 90 may be formed so as to cover almost the entire part from the tip of the element body 102 to the longitudinal position where the reference electrode 42 is formed. Alternatively, for example, the porous protective layer 90 may be formed so as to cover almost the entire part from the tip of the element body 102 to the longitudinal position of the side of the tip side of the reference gas introduction space 43. Alternatively, the porous protective layer 90 may cover further to the rear. In this embodiment, the longitudinal length L of the porous protective layer 90 is the same on each of the two main surfaces (the pump surface 102a and the heater surface 102b) and the two side surfaces (the left surface 102c and the right surface 102d), but the longitudinal length L of the porous protective layer 90 may be different from each other on the two main surfaces and the two side surfaces.
[0106] The length L of the entire porous protective layer 90 in the longitudinal direction from the tip of the element body 102 varies depending on the configuration of the element body 102, but may be, for example, 7 mm or more, 9 mm or more, or 10 mm or more. The length L may be, for example, 17 mm or less, or 14 mm or less. In this embodiment, the longitudinal length L of the porous protective layer 90 is the same on each of the two main surfaces (the pump surface 102a and the heater surface 102b) and the two side surfaces (the left surface 102c and the right surface 102d), but the longitudinal length L of the porous protective layer 90 may be different from each other on the two main surfaces and the two side surfaces.
[0107] The outer layer 92 may cover the inner layer 91 to an extent that the structural strength of the porous protective layer 90 as a whole can be maintained. As shown in Fig. 3, the longitudinal length of the outer layer 92 from the tip of the element body 102 may be the same as the longitudinal length of the inner layer 91 from the tip of the element body 102. The outer layer 92 may completely cover the inner layer 91 (the longitudinal length of the outer layer 92 from the tip of the element body 102 is longer), or a part of the inner layer 91 including the rear end in the longitudinal direction may be exposed (the longitudinal length of the inner layer 91 from the tip of the element body 102 is longer). In this embodiment, the longitudinal length of the outer layer 92 and the longitudinal length of the inner layer 91 are the same on each of the two main surfaces (pump surface 102a and heater surface 102b) and two side surfaces (left surface 102c and right surface 102d), but the relationship in magnitude between the longitudinal length of the outer layer 92 and the longitudinal length of the inner layer 91 may be different from each other on each surface.
[0108] The thickness of the inner layer 91 may be, for example, 200 μm or more and 800 μm or less. In this embodiment, the thicknesses of the inner layers 91 of the porous protective layers 90 on each surface of the element body 102 are all approximately the same, but the thicknesses of the inner layers 91 may be different on each surface of the element body 102. The thickness of the outer layer 92 may be, for example, 100 μm or more and 400 μm or less. In this embodiment, the thicknesses of the outer layers 92 of the porous protective layers 90 on each surface of the element body 102 are all approximately the same, but the thicknesses of the outer layers 92 may be different on each surface of the element body 102.
[0109] The thickness is obtained as follows using an image (SEM image) obtained by observation with a scanning electron microscope (SEM). The sensor element 101 is cut in the longitudinal direction of the sensor element 101 in a region where the element body 102 exists (for example, near the center in the width direction of the sensor element 101). The cut surface is filled with resin and polished to obtain an observation sample. The magnification of the SEM is set to 80 times, and the observation surface of the observation sample is photographed to obtain an SEM image of the cross section of the porous protective layer 90. The direction perpendicular to the surface of the element body 102 is defined as the thickness direction, and the distance from the surface of the outer layer 92 (the surface of the porous protective layer 90) to the boundary surface with the inner layer 91 is derived, and this distance is defined as the thickness of the outer layer 92. In addition, the distance from the surface of the inner layer 91 to the boundary surface with the element body 102 is derived, and this distance is defined as the thickness of the inner layer 91. In addition, the distance from the surface of the outer layer 92 (the surface of the porous protective layer 90) ... porous protective layer 90. The thickness of the porous protective layer 90 may be determined by calculating the sum of the thicknesses of the outer layer 92 and the inner layer 91 thus derived.
[0110] 3, in the vicinity of the rear end in the longitudinal direction of the porous protective layer 90, the thickness of the inner layer 91 usually becomes thinner toward the rear end. Also, the corners of the front end in the longitudinal direction of the porous protective layer 90 are often rounded. The above thickness is derived in a region where the porous protective layer 90 has a uniform thickness (a region other than the front end and rear end portions).
[0111] Next, the porosity of the inner layer 91 of the porous protective layer 90 will be described with reference to FIG.
[0112] As described above, in the inner layer 91, the porosity ρA in the front region 91A of the inner layer 91 is lower than the porosity ρM in the main region 91M of the inner layer 91 (ρA<ρM). That is, the porosity difference Δρ (=ρA-ρM) between the porosity ρA in the front region 91A and the porosity ρM in the main region 91M is negative (Δρ<0). As shown in Fig. 3, this embodiment shows an example in which the front region 91A and the main region 91M each have a uniform porosity.
[0113] Preferably, the porosity ρA in the front region 91A of the inner layer 91 may be lower than the porosity ρM in the main region 91M of the inner layer 91 by 5% or more. That is, the porosity difference Δρ (=ρA-ρM) between the porosity ρA in the front region 91A and the porosity ρM in the main region 91M may be -5% or less (Δρ≦-5%). In this range, the oxygen pumped to the vicinity of the outer pump electrode 23 by the main pump cell 21, the auxiliary pump cell 50, and the measurement pump cell 41 can be more effectively prevented from diffusing toward the front end of the element body 102. Therefore, the pumped oxygen can be more effectively prevented from being reintroduced from the gas inlet 10 into the measurement gas flow space 15. The pumped oxygen mainly diffuses toward the rear end of the element body 102 and is released from the rear end of the porous protective layer 90 to the outside of the sensor element 101. More preferably, the porosity difference Δρ (=ρA−ρM) may be −10% or less (Δρ≦−10%).
[0114] The porosity in the front region 91A of the inner layer 91 may be, for example, 30 volume % or more and 50 volume % or less. Here, the porosity in the front region 91A may be the average porosity in the front region 91A. The porosity in the front region 91A of the inner layer 91 may be, for example, 30 volume % or more and 45 volume % or less, or 30 volume % or more and 40 volume % or less.
[0115] The porosity in the main region 91M of the inner layer 91 may be, for example, 40 volume % or more and 80 volume % or less, provided that the porosity is higher than the porosity in the front region 91A of the inner layer 91. Here, the porosity in the main region 91M may be the average porosity of the main region 91M. The porosity in the main region 91M of the inner layer 91 may be, for example, 40 volume % or more and 70 volume % or less, or 40 volume % or more and 60 volume % or less.
[0116] The porosity of the inner layer 91 on each surface (heater surface 102b, left surface 102c, right surface 102d, and tip surface 102e) other than the pump surface 102a of the element body 102 is not particularly limited, and may be, for example, 30 volume % or more and 80 volume % or less. The porosity of the inner layer 91 on each surface other than the top surface 102a may be approximately the same as the porosity in the main region 91M on the pump surface 102a.
[0117] The porosity is determined as follows using an image (SEM image) obtained by observation with a scanning electron microscope (SEM). An observation sample is prepared in the same manner as in the case of the thickness described above, and the magnification of the SEM is set to 100 times to obtain an SEM image of the cross section of the inner layer 91 of the porous protective layer 90. In detail, a plurality of SEM images are obtained over the entire front region 91A of the inner layer 91. Each SEM image is binarized using "Otsu's binarization" (also called discriminant analysis method). In the binarized image, alumina is represented in white and pores are represented in black. The area of the alumina part (white) and the area of the pore part (black) of the binarized image are obtained. For each SEM image, the ratio of the area of the pore part to the total area (the sum of the area of the alumina part and the area of the pore part) is calculated, and the average value (average porosity) of the calculated areas may be used as the porosity of the inner layer 91 in the front region 91A.
[0118] In addition, a plurality of SEM images are obtained over the entire area of the main region 91M of the inner layer 91. As in the case of the front region 91A described above, for each of the obtained SEM images, the ratio of the area of the pores to the total area (the sum of the area of the alumina portion and the area of the pores) is calculated, and the average value thereof (average porosity) may be used as the porosity of the main region 91M of the inner layer 91.
[0119] As the porosity in the front region 91A of the inner layer 91, the porosity at a predetermined position in the longitudinal direction of the front region 91A may be used instead of the average porosity. For example, the porosity at a central position of the front region 91A may be used. Furthermore, as the porosity in the main region 91M of the inner layer 91, the porosity at a predetermined position in the longitudinal direction of the main region 91M may be used instead of the average porosity. For example, the porosity at the central position of the main region 91M may be used. Alternatively, the porosity at the position of the rear electrode end of the outer pump electrode 23 in the main region 91M (the rear end of the electrode presence region 91E) may be used.
[0120] As described above, the porosity of the outer layer 92 is lower than the porosity at any position of the inner layer 91. The porosity of the outer layer 92 may be, for example, about 10 volume % or more and 35 volume % or less. However, the porosity must be lower than the porosity at any position of the front region 91A and the main region 91M of the inner layer 91. The porosity of the outer layer 92 can also be calculated using the above-mentioned porosity calculation method. It is considered that the outer layer 92 has substantially the same porosity regardless of the observation position. Therefore, the porosity value calculated using one cross-sectional image may be used as the porosity value of the outer layer 92.
[0121] The sensor element 101 for detecting the NOx concentration in a measurement gas and the gas sensor 100 including the sensor element 101 have been described above as examples of embodiments of the present invention, but the present invention is not limited to this embodiment. The present invention may include sensor elements of various forms as long as they achieve the object of the present invention, which is to maintain high measurement accuracy even during long-term continuous operation while maintaining high water resistance.
[0122] In the gas sensor 100 according to the embodiment described above, the front region 91A and the main region 91M of the inner layer 91 of the porous protective layer 90 each have a uniform porosity as shown in Fig. 3, but the present invention is not limited to this. As long as the porosity ρA in the front region 91A of the inner layer 91 is lower than the porosity ρM in the main region 91M, the inner layer 91 may have various structures.
[0123] For example, in the front region 91A of the inner layer 91, the porosity may vary in the longitudinal direction of the element body 102. For example, in the front region 91A, the porosity may be higher in the longitudinal direction from the tip of the element body 102. Alternatively, for example, the porosity may be lower in the longitudinal direction from the tip.
[0124] Also, for example, in the main region 91M of the inner layer 91, the porosity may increase in the longitudinal direction from the tip side of the element body 102. Alternatively, for example, in the longitudinal direction of the element body 102, the porosity may be different between an electrode presence region 91E where the outer pump electrode 23 is present and a rear region 91P following the electrode presence region 91E. The porosity in the electrode presence region 91E may be higher or lower than the porosity in the rear region 91P.
[0125] In the gas sensor 100 of the embodiment described above, the porosity of the inner layer 91 of the porous protective layer 90 on each surface other than the pump surface 102a is set to be approximately the same as the porosity of the main region 91M on the pump surface 102a, but is not limited to this. On at least one of the surfaces (heater surface 102b, left surface 102c, right surface 102d, tip surface 102e) other than the pump surface 102a of the element body 102, the inner layer 91 may further have a region with low porosity corresponding to the front region 91A.
[0126] In the cross section of Fig. 4, at least one of the inner layers 91b, 91c, and 91d on the surfaces of the inner layer 91 other than the pump surface 102a may further include a low-porosity region corresponding to the front region 91A on the pump surface 102a. For example, in the cross section of Fig. 4, the entire inner layer 91 may be a low-porosity region corresponding to the front region 91A on the pump surface 102a. That is, in the longitudinal direction of the element body 102, the entire circumference of the region from the element body 102 to the tip of the outer pump electrode 23 (the pump surface 102a, the heater surface 102b, the left surface 102c, and the right surface 102d) may be a low-porosity region corresponding to the front region 91A on the pump surface 102a.
[0127] Also, for example, the inner layers 91c, 91d on both side surfaces of the inner layer 91 may be low-porosity regions corresponding to the front region 91A on the pump surface 102a. Also, for example, the inner layers 91cu, 91du on both side surfaces in the range from the upper end to the lower surface of the measurement target gas flow space 15 (buffer space 12) may be low-porosity regions corresponding to the front region 91A on the pump surface 102a. Since the diffusion of oxygen toward the tip can be further suppressed through the inner layers 91c, 91d on the side surfaces, it is possible to maintain a higher measurement accuracy.
[0128] The porosity of the inner layer 91 may increase stepwise or continuously from the one end (tip) in the longitudinal direction of the element body 102 (base part 103) of the element body 102. In the inner layer 91 in the above-mentioned embodiment, the porosity increases in two steps, but the porosity may decrease stepwise (almost stepwise) in three or more steps. Furthermore, the porosity may decrease continuously (almost continuously).
[0129] In the gas sensor 100 according to the embodiment described above, the porous protective layer 90 is composed of the inner layer 91 and the outer layer 92, but is not limited to this. One or more intermediate layers may be present between the inner layer 91 and the outer layer 92.
[0130] In the gas sensor 100 of the above embodiment, the porous protective layer 90 is configured of two layers, the inner layer 91 and the outer layer 92, on each surface of the element body 102, but is not limited to this. The porous protective layer 90 may be configured of a single layer on at least one of the surfaces (the heater surface 102b, the left surface 102c, the right surface 102d, and the tip surface 102e) of the element body 102 other than the pump surface 102a.
[0131] In the gas sensor 100 of the above embodiment, the outer pump electrode 23 is located on the surface of the element body 102, and the inner layer 91 of the porous protective layer 90 is formed in contact with the outer pump electrode 23 on the surface of the element body 102, but this is not limited thereto. For example, the element body 102 may have a main surface protective layer on two main surfaces (the pump surface 102a and the heater surface 102b). The main surface protective layer is provided for the purpose of preventing foreign matter or poisonous substances from adhering to the main surfaces (the pump surface 102a and the heater surface 102b) of the element body 102 and the outer pump electrode 23 on the pump surface 102a. The main surface protective layer is a porous layer made of ceramics such as alumina. The porosity of the main surface protective layer may be, for example, about 20 volume % or more and 40 volume % or less. The thickness of the main surface protective layer may be, for example, about 5 μm to 30 μm.
[0132] Also, for example, the element body 102 may further be provided with an underlayer when the inner layer 91 is formed. The underlayer is provided to further improve the adhesion between the element body 102 and the inner layer 91. When the underlayer is provided, it is preferable to provide it on at least two main surfaces (the pump surface 102a and the heater surface 102b) of the element body 102. The underlayer is, for example, a porous layer made of ceramics such as alumina. The porosity of the underlayer may be about 40% by volume or more. For example, it may be about 40% by volume or more and 60% by volume or less. Also, the thickness of the underlayer may be, for example, about 20 μm to 60 μm.
[0133] In the above embodiment, the gas sensor 100 detects the NOx concentration in the measurement gas, but the measurement target gas is not limited to NOx. The sensor element of the gas sensor 100 may be configured using a solid electrolyte with oxygen ion conductivity. The measurement target gas may be, for example, oxygen O 2 Or other oxide gases other than NOx (e.g., carbon dioxide CO 2 , water H 2 Alternatively, ammonia NH 3 The gas may be a non-oxide gas such as
[0134] In the gas sensor 100 according to the embodiment described above, as shown in FIG. 2, the sensor element 101 has three internal cavities, the first internal cavities 20, the second internal cavities 40, and the third internal cavities 61, and the inner main pump electrode 22, the auxiliary pump electrode 51, and the measurement electrode 44 are disposed in each internal cavities, but the structure is not limited to this. For example, the sensor element 101 may have two internal cavities, the first internal cavities 20 and the second internal cavities 40, and the inner main pump electrode 22 is disposed in the first internal cavities 20, and the auxiliary pump electrode 51 and the measurement electrode 44 are disposed in the second internal cavities 40. In this case, for example, a porous protective layer covering the measurement electrode 44 may be formed as a diffusion rate-controlling part between the auxiliary pump electrode 51 and the measurement electrode 44. For example, the number of internal cavities may be one or four or more.
[0135] In the gas sensor 100 according to the above embodiment, the outer pump electrode 23 functions as three electrodes: the outer main pump electrode in the main pump cell 21, the outer auxiliary pump electrode in the auxiliary pump cell 50, and the outer measurement electrode in the measurement pump cell 41. However, the present invention is not limited to this. For example, the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode may be formed as separate electrodes. For example, any one or more of the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode may be provided on the outer surface of the base portion 103 separately from the outer pump electrode 23 so as to be in contact with the measurement gas. In this case, the front region means a region from the tip of the element body 102 to the tip of the electrode disposed at the most tip side among the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode in the longitudinal direction of the element body 102. In addition, the reference electrode 42 may also function as one or two of the outer main pump electrode, the outer auxiliary pump electrode, and the outer measurement electrode.
[0136] In addition to the above configuration, the components of the element body 102, such as the measurement gas flow space 15 and the electrodes, may take various forms depending on the type of gas to be measured, the purpose and environment of use of the gas sensor, etc.
[0137] [Sensor element manufacturing method] Next, an example of a method for manufacturing the above-mentioned sensor element will be described. In the method for manufacturing the sensor element 101, first, the element body 102 is manufactured, and then the porous protective layer 90 is formed on the element body 102 to manufacture the sensor element 101.
[0138] In the following, an example will be described in which the sensor element 101 made up of six layers as shown in Fig. 2 is manufactured. Fig. 7 is a flow chart showing an example of a method for manufacturing a sensor element.
[0139] (Manufacturing of the element body) First, a method for manufacturing the element body 102 will be described. First, six blank sheets are prepared (step S1). The blank sheets are made of zirconia (ZrO 2 The green sheets contain oxygen ion conductive solid electrolytes such as SiO 2 , etc., as ceramic components. A known forming method can be used to prepare the green sheets. Each of the six green sheets is previously formed with holes or the like for use in positioning during printing or lamination, using a known method such as punching with a punching device. These are called blank sheets. In addition, in the blank sheets used for the spacer layer 5, through-holes such as internal voids are also formed in the same manner. Necessary through-holes are also formed in the other layers. All six blank sheets may be of the same thickness, or the thickness may differ depending on the layer being formed.
[0140] Various patterns required for each layer are printed and dried on blank sheets to be used for six layers, namely, the first substrate layer 1, the second substrate layer 2, the third substrate layer 3, the first solid electrolyte layer 4, the spacer layer 5, and the second solid electrolyte layer 6 (step S2). A known screen printing technique can be used for printing the patterns. A known drying means can also be used for the drying process.
[0141] After repeating these steps and printing and drying various patterns on each of the six blank sheets, the six printed blank sheets are stacked in a predetermined order while being positioned using sheet holes, etc., and are then pressed under predetermined temperature and pressure conditions to form a laminate (step S3). The pressing process is performed by applying heat and pressure using a laminator such as a known hydraulic press. The temperature, pressure, and time for heating and pressing depend on the laminator used, but can be determined appropriately so as to achieve good lamination.
[0142] The obtained laminate contains a plurality of element bodies 102. The laminate is cut into units of element bodies 102 (step S4). The cut laminate is fired at a predetermined firing temperature to obtain element bodies 102 (step S5). The firing temperature may be any temperature at which the solid electrolyte constituting the base portion 103 of the sensor element 101 is sintered to form a dense body and at which the electrodes and the like maintain a desired porosity. For example, firing is performed at a firing temperature of about 1300 to 1500°C.
[0143] (Protective Layer Production) Next, there will be described a method for forming the porous protective layer 90 (the inner layer 91 and the outer layer 92) on the element body 102. In this embodiment, the porous protective layer 90 is formed by plasma spraying.
[0144] First, a sprayed film to become the inner layer 91 is formed. That is, a powder for forming the inner layer prepared in advance is sprayed onto a predetermined region of the element body 102 (step S6). Next, a powder for forming the outer layer prepared in advance is sprayed onto the sprayed film to become the inner layer 91 of the element body 102 (step S7). Thereafter, degreasing is performed (step S8) to form the porous protective layer 90 (the inner layer 91 and the outer layer 92).
[0145] The powder for forming the inner layer includes a raw material powder (alumina powder in this embodiment) made of the material of the inner layer 91 and having a predetermined particle size distribution, and a pore former. Examples of the pore former include xanthine derivatives such as theobromine, organic resin materials such as acrylic resin, and inorganic materials such as carbon. The powder for forming the inner layer includes alumina powder and an organic pore former in a ratio according to the porosity of the inner layer 91 to be formed. In this embodiment, a first powder for forming the inner layer corresponding to the porosity of the front region 91A of the inner layer 91 on the pump surface 102a and a second powder for forming the inner layer corresponding to the porosity of the main region 91M of the inner layer 91 on the pump surface 102a are prepared.
[0146] The powder for forming the inner layer is sprayed onto the area of the surface of the element body 102 where the inner layer 91 is to be formed, to form a sprayed film (step S6). A known plasma spraying technique can be used for the spraying. Specifically, the powder for forming the first inner layer is sprayed onto the area where the front region 91A is to be formed among the areas where the inner layer 91 is to be formed, to form a sprayed film. For example, the area of the element body 102 other than the area where the front region 91A is to be formed may be covered (masked) with a baffle plate, and the powder for forming the first inner layer may be sprayed onto the area where the front region 91A is to be formed. Also, the powder for forming the second inner layer is sprayed onto the area where the main region 91M is to be formed among the areas where the inner layer 91 is to be formed, to form a sprayed film. In this embodiment, the porosity of the inner layer 91 on each surface other than the pump surface 102a is the same as the porosity of the main region 91M, so that the powder for forming the second inner layer is sprayed to form a sprayed film on the region on each surface other than the pump surface 102a where the inner layer 91 is to be formed. For example, the sprayed film to be the front region 91A and the region of the element body 102 where the inner layer 91 is not to be formed may be covered (masked) with a baffle plate, and the powder for forming the second inner layer may be sprayed on the unmasked region. The order of forming these sprayed films may be determined appropriately. Also, a plurality of regions may be formed simultaneously.
[0147] Next, the outer layer 92 is formed. A powder for forming the outer layer, which has been prepared in advance, is sprayed onto a predetermined region on the sprayed film that is to become the inner layer 91 of the element body 102 (step S7), to form the outer layer 92.
[0148] The powder for forming the outer layer contains a raw material powder (alumina powder in this embodiment) made of the material of the outer layer 92 and having a predetermined particle size distribution. Unlike the powder for forming the inner layer, the powder for forming the outer layer does not usually contain a pore-forming material.
[0149] A powder for forming an outer layer is sprayed onto an area where an outer layer 92 is to be formed on the surface of the sprayed film that is to become the inner layer 91 formed on the element body 102, to form a sprayed film (i.e., outer layer 92) (step S7). A known plasma spraying technique can be used for the spraying.
[0150] Finally, the sprayed film that is to become the inner layer 91 is degreased by heat treatment (step S8). The pore-forming material in the sprayed film is removed by degreasing, and the inner layer 91 made of a porous body is formed. The degreasing process is performed at a predetermined degreasing temperature. The degreasing temperature may be any temperature at which all of the pore-forming material components in the film of the inner layer 91 are removed and the porous structure of the inner layer 91 is maintained. The degreasing temperature may be lower than the firing temperature of the element body 102. For example, degreasing is performed at a degreasing temperature of about 400 to 900° C. In the degreasing process, the sprayed film of the outer layer 92 that does not contain the pore-forming material is also heat treated at the same time.
[0151] In the above manufacturing method, the steps of thermal spraying of the powder for forming the inner layer (step S6), thermal spraying of the powder for forming the outer layer (step S7), and degreasing (step S8) are performed in that order, but it is also possible to perform thermal spraying of the powder for forming the inner layer (step S6) and degreasing (step S8) first, and then thermal spraying of the powder for forming the outer layer (step S7).
[0152] In the above manufacturing method, the inner layer 91 and the outer layer 92 are formed by plasma spraying, but the method is not limited to this. The inner layer 91 and the outer layer 92 may be formed by other methods such as screen printing, dipping, gel casting, etc. Also, the inner layer 91 and the outer layer 92 may be formed by different methods.
[0153] The obtained sensor element 101 is accommodated in a predetermined housing and assembled into the gas sensor 100 such that the front end of the sensor element 101 contacts the gas to be measured and the rear end of the sensor element 101 contacts the reference gas. EXAMPLES
[0154] Examples in which a sensor element was specifically produced and tested will be described below as examples, although the present invention is not limited to the following examples.
[0155] [1. Preparation of Examples 1-2 and Comparative Examples 1-2] According to the above-mentioned manufacturing method of the sensor element 101, the sensor elements of Examples 1 and 2 and Comparative Examples 1 and 2 were manufactured. Specifically, first, an element body 102 was manufactured having a length in the front-rear direction of 67.5 mm, a width in the left-right direction of 4.25 mm, and a thickness in the up-down direction of 1.45 mm. Then, the porous protective layer 90 (inner layer 91 and outer layer 92) was formed by plasma spraying to manufacture the sensor element.
[0156] The sensor elements of Examples 1 and 2 and Comparative Examples 1 and 2 were designed so that the porosity difference Δρ (=ρA-ρM) between the porosity ρA in the front region 91A and the porosity ρM in the main region 91M was the value shown below. The porosity ρA in the front region 91A of the inner layer 91 and the porosity ρM in the main region 91M were each determined using the above-mentioned method for deriving porosity.
[0157] In the sensor element of Example 1, the porosity difference Δρ was −5%. The porosity ρA in the front region 91A was about 50%, and the porosity ρM in the main region 91M was about 55%.
[0158] In the sensor element of Example 2, the porosity difference Δρ was −10%. The porosity ρA in the front region 91A was about 45%, and the porosity ρM in the main region 91M was about 55%.
[0159] In the sensor element of Comparative Example 1, the porosity difference Δρ was set to 0%. The porosity ρA in the front region 91A was about 50%, and the porosity ρM in the main region 91M was about 50%.
[0160] In the sensor element of Comparative Example 2, the porosity difference Δρ was set to 5%. The porosity ρA in the front region 91A was about 55%, and the porosity ρM in the main region 91M was about 50%.
[0161] In each of the sensor elements of Examples 1 and 2 and Comparative Examples 1 and 2, the length of the inner layer 91 in the longitudinal direction from the tip of the element body 102 was 10 mm, and the thickness of the inner layer 91 was 500 μm. In each case, the porosity on each surface of the inner layer 91 other than the pump surface 102a was set to be the same as the porosity ρM in the main region 91M.
[0162] In each of the sensor elements of Examples 1 and 2 and Comparative Examples 1 and 2, the length of the outer layer 92 in the longitudinal direction from the tip of the element body 102 was 10 mm, and the thickness of the outer layer 92 was 200 μm. The porosity of the outer layer 92 was 25%.
[0163] [2. Evaluation of measurement accuracy] The measurement accuracy was evaluated for the sensor elements of Examples 1 and 2 and Comparative Examples 1 and 2. 2 The measurement accuracy during continuous operation was evaluated using the pump current Ip0 that flows according to the concentration. Specifically, first, the heater 72 was energized to heat the sensor element to a temperature of 800°C. In this state, pump control during normal operation was performed in the air atmosphere. That is, as described above, the main pump cell 21, the auxiliary pump cell 50, the measurement pump cell 41, the oxygen partial pressure detection sensor cell 80 for controlling the main pump, the oxygen partial pressure detection sensor cell 81 for controlling the auxiliary pump, and the oxygen partial pressure detection sensor cell 82 for controlling the measurement pump were operated. The oxygen concentration in the first internal space 20 was controlled to be kept at a predetermined constant value, and a pump current Ip0 corresponding to the oxygen concentration in the measured gas (here, the air) was passed through the main pump cell 21. In this state, the device was continuously operated for 100 hours.
[0164] Pump current Ip0 at the start of normal operation (Ip0 0H ) and the pump current Ip0 after 100 hours of continuous operation (Ip0 100H ) were obtained. Here, the start of normal driving means the point at which the temperature of the sensor element is stable and the current value of the pump current Ip0 is stable. The rate of change (O 2 The signal change rate (PSD) was calculated.
[0165] O 2 Signal change rate (%) = (Ip0 100H / Ip0 0H -1) x 100
[0166] Calculated O 2 Based on the signal change rate, the following criteria are used: 2 Accuracy of concentration measurement (O 2 The results are shown in Table 1.
[0167] A:O 2 Signal change rate is within ±5% B:O 2 Signal change rate is greater than ±5% and within ±10% C:O 2 Signal change rate is greater than ±10%
[0168] [Table 1]
[0169] As shown in Table 1, in all of Examples 1 and 2, compared with Comparative Examples 1 and 2, even after 100 hours of continuous operation, O 2 It was confirmed that the signal accuracy was maintained at a high level. In addition, when the porosity difference is large, that is, when the porosity ρA in the front region 91A is lower than the porosity ρM in the main region 91M, O 2 It was found that signal accuracy could be maintained at a higher level.
[0170] As described above, according to the present invention, the front region 91A of the inner layer 91 can prevent oxygen pumped out from the measurement gas flow space 15 from flowing through the inner layer 91 again into the measurement gas flow space 15 from the gas inlet 10, so that high measurement accuracy can be maintained even during continuous operation. Therefore, the heat insulating effect of the electrode presence region 91b can be maintained high while maintaining high adhesion strength between the element body 102 and the inner layer 91. Therefore, a sensor element that has high water resistance and can maintain high measurement accuracy can be provided. [Explanation of symbols]
[0171] 1 First board layer 2 Second board layer 3 Third board layer 4 First solid electrolyte layer 5 Spacer layer 6 Second solid electrolyte layer 10 Gas inlet 11 First diffusion-controlled section 12 Buffer space 13 Second diffusion-controlled section 15 Measurement gas flow space 20 1st internal void 21 Main pump cell 22 Inner main pump electrode 22a (Inner main pump electrode) ceiling electrode part 22b Bottom electrode part (of the inner main pump electrode) 23 Outer pump electrode 24 Variable power supply (for main pump cell) 30 Third diffusion-controlled section 40 Second internal void 41 Measuring pump cell 42 Reference electrode 43 Reference gas introduction space 44 Measuring electrode 46 Variable power supply (for measuring pump cell) 48 Atmospheric introduction layer 50 Auxiliary pump cell 51 Auxiliary pump electrode 51a (auxiliary pump electrode) ceiling electrode part 51b (auxiliary pump electrode) bottom electrode part 52 Variable power supply (for auxiliary pump cell) 60 4th diffusion-controlled section 61 3rd internal void 70 Heater section 71 Heater electrode 72 Heater 73 Through Hole 74 Heater insulation layer 75 Pressure relief hole 76 Heater lead 80 Oxygen partial pressure detection sensor cell for main pump control 81 Oxygen partial pressure detection sensor cell for controlling auxiliary pump 82 Oxygen partial pressure detection sensor cell for measuring pump control 83 Sensor cell 90, 990 porous protective layer 91, 991 Inner layer 92 Outer layer 100 Gas Sensor 101 Sensor element 102 Element body 103 Base
Claims
1. an element body including a long plate-like base portion including an oxygen ion conductive solid electrolyte layer and a measurement target gas flow space formed on one end side of the base portion in the longitudinal direction; a porous protective layer formed from the one end of the base portion in the longitudinal direction and covering a predetermined length of the surface of the element body in the longitudinal direction; A sensor element comprising: the element body includes an intra-space electrode disposed in the measurement gas flow space, and an outer-space electrode corresponding to the intra-space electrode, the outer-space electrode having a predetermined length in the longitudinal direction of the base portion and disposed on one of two main surfaces of the element body at a predetermined distance from the one end, The protective layer is an inner layer covering the element body and an outer layer located outside the inner layer on at least the one main surface on which the outer electrode is present; and a main region including an electrode presence region in which the outer-space electrode is present and a rear region following the electrode presence region, and a front region extending from the one end of the base portion in the longitudinal direction to the electrode presence region, on the one principal surface on which the outer-space electrode is present, a porosity in the front region of the inner layer is less than a porosity in the main region of the inner layer; A sensor element for detecting a gas to be measured in a measurement target gas, wherein the porosity of the outer layer is lower than the porosity of the inner layer in the front region.
2. 2. The sensor element of claim 1, wherein the porosity of the inner layer in the front region is at least 5% by volume lower than the porosity of the inner layer in the main region.
3. 2. The sensor element of claim 1, wherein the porosity of the inner layer in the front region is at least 10% by volume lower than the porosity of the inner layer in the main region.
4. 2. The sensor element according to claim 1, wherein the rear region of the protective layer extends in the longitudinal direction of the base portion to a position farther from the one longitudinal end of the base portion than the measurement target gas flow space.
5. 2. The sensor element according to claim 1, wherein, on the one main surface on which the void outer electrode is present, the porosity of the inner layer increases stepwise or continuously in the longitudinal direction of the base portion from the one end in the longitudinal direction of the base portion.
Citation Information
Patent Citations
Sensor element and gas sensor
JP2021148612A
Gas sensor
JP2022155844A
Gas sensor element and gas sensor
WO2022196233A1
Gas sensor element and gas sensor
JP2014098590A
Gas sensor production method
JP2016065852A