Urethane resin composition and polyurethane foam
A specialized urethane resin composition with specific catalysts and flame retardants addresses the inadequacies of existing polyurethane foams by achieving controlled heat generation and enhanced flame retardancy, ensuring fire safety in building applications.
Patent Information
- Application Number
- JP2023050567
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-27
- Publication Date
- 2024-10-09
AI Technical Summary
Existing polyurethane foams do not meet the high flame retardancy demands required for fire safety in buildings, as they are prone to rapid heat generation during a fire, which can spread flames.
A urethane resin composition containing specific catalysts, such as bismuth and tin metal catalysts, imidazole derivatives, and trimerization catalysts, along with a blend of flame retardants like red phosphorus and phosphoric acid esters, is formulated to achieve a polyurethane foam with controlled heat generation rates below 150 BTU/ft²/min, adhering to FM4975 test standards.
The composition results in polyurethane foam with excellent flame retardancy, ensuring controlled heat generation and reduced fire spread, meeting stringent fire safety standards.
Smart Images

Figure 2024139567000001 
Figure 2024139567000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a urethane resin composition and a polyurethane foam. [Background technology]
[0002] Due to its excellent heat insulating properties and adhesive properties, polyurethane foam is used as a heat insulating material for buildings such as apartment complexes, detached houses, various school facilities, commercial buildings, etc. Polyurethane foam can be obtained by mixing a polyol composition and a polyisocyanate composition, foaming the mixture, and spraying the mixture onto objects such as ceilings, walls, and roofs using a spray device or the like.
[0003] Although polyurethane foam has excellent heat insulation properties and is lightweight, it is known to be highly flammable. Therefore, from the viewpoint of preventing the spread of fire in the event of a fire, there is a demand for polyurethane foam that is less likely to burn. In view of this, a urethane resin composition has been proposed which contains a plurality of flame retardants having different decomposition temperatures to improve the flame retardancy of the polyurethane foam formed (see, for example, Patent Document 1). In addition, a urethane resin composition has been proposed that contains red phosphorus as an essential component and also contains at least one of a phosphate-containing flame retardant and a chlorine-containing flame retardant, thereby forming a polyurethane foam that has quasi-nonflammable properties (see, for example, Patent Document 2). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 6776279 [Patent Document 2] Patent No. 6725606 Summary of the Invention [Problem to be solved by the invention]
[0005] However, in recent years, there has been a demand for polyurethane foams with higher flame retardancy, and from this viewpoint, the polyurethane foams of the inventions described in the above-mentioned Patent Documents 1 and 2 are not sufficient. Therefore, an object of the present invention is to provide a urethane resin composition which can give a polyurethane foam having excellent flame retardancy. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted intensive research and have found that the above-mentioned problems can be solved by providing a urethane resin composition for obtaining a polyurethane foam, the composition comprising a polyol, a polyisocyanate, a catalyst, a blowing agent and a flame retardant, and by controlling the heat release rates of the obtained polyurethane foam within 1 minute, 2 minutes and 3 minutes to not more than predetermined values in a test carried out in accordance with the FM4975 test standard, thereby completing the present invention.
[0007] The present invention relates to the following items [1] to [9]. [1] A polyurethane resin composition for obtaining polyurethane foam, comprising a polyol, a polyisocyanate, a catalyst, a blowing agent and a flame retardant, and the polyurethane foam obtained by foaming the polyurethane resin composition has a heat release rate of 150 BTU / ft 3 in 1 minute measured in accordance with the FM4975 test standard. 2 / min or less, heat generation rate in 2 minutes is 140 BTU / ft 2 / min or less, and the heat generation rate in 3 minutes is 130 BTU / ft 2 / min or less. [2] The urethane resin composition according to [1], wherein the catalyst comprises a metal catalyst containing at least one metal selected from the group consisting of bismuth and tin. [3] The urethane resin composition according to [1] or [2], wherein the catalyst contains a quaternary ammonium salt. [4] The urethane resin composition according to any one of [1] to [3], wherein the catalyst contains a potassium salt. [5] The urethane resin composition according to any one of [1] to [4], wherein the catalyst contains an imidazole derivative. [6] The urethane resin composition according to any one of [1] to [5], wherein the flame retardant comprises a red phosphorus-based flame retardant. [7] The urethane resin composition according to any one of [1] to [6], having an isocyanate index of 300 or more. [8] The urethane resin composition according to any one of [1] to [7], which is used for spray applications. [9] A polyurethane foam obtained by foaming the urethane resin composition according to any one of [1] to [7]. Effect of the Invention
[0008] According to the present invention, it is possible to provide a urethane resin composition which can give a polyurethane foam having excellent flame retardancy. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] [Urethane resin composition] The urethane resin composition of the present invention is a composition for obtaining a polyurethane foam, and contains a polyol, a polyisocyanate, a catalyst, a blowing agent, and a flame retardant.
[0010] <Polyol> The polyol is not particularly limited, but examples thereof include polyether polyol, polyester polyol, etc. From the viewpoint of improving the flame retardancy of the polyurethane foam, the polyol preferably includes polyester polyol. Also, from the viewpoint of improving the flame retardancy, it is preferable to use a halogen-containing polyol or a phosphorus-containing polyol. From the viewpoint of improving flame retardancy, out of 100 parts by mass of polyol, it is preferable that the polyester polyol be 20 parts by mass or more, more preferably 50 parts by mass or more, even more preferably 80 parts by mass or more, and particularly preferably 100 parts by mass.
[0011] The average hydroxyl value of the polyol used in the present invention is preferably from 100 to 500 mgKOH / g, more preferably from 150 to 450 mgKOH / g, and even more preferably from 180 to 400 mgKOH / g, from the viewpoint of improving the flame retardancy of the polyurethane foam.
[0012] When one type of polyol is used, the average hydroxyl value means the hydroxyl value of that polyol, and when two or more types of polyols are used, the weighted average value of the hydroxyl groups according to the blending ratio of the two or more types of polyol compounds is taken as the average hydroxyl value. For example, when two types of polyols, polyol (d1) and polyol (d2), are used as polyols, the hydroxyl value of polyol (d1) is X1, the blending ratio is m1, and the hydroxyl value of polyol (d2) is X2, the blending ratio is m2, the average hydroxyl value is represented by the following formula. Note that the blending ratio is based on mass. Average hydroxyl value (mgKOH / g)=X1×(m1 / (m1+m2))+X2×(m2 / (m1+m2)) The hydroxyl value is a value measured in accordance with JIS K1557-1:2007.
[0013] (Polyester polyol) The polyester polyol may be a polyester polyol having an aromatic ring or an aliphatic polyester polyol, but in consideration of the flame retardancy of the resulting polyurethane foam, it is preferable to use a polyester polyol having an aromatic ring. The polyester polyol having an aromatic ring is preferably a condensate of an aromatic dicarboxylic acid such as o-phthalic acid (phthalic acid), m-phthalic acid (isophthalic acid), p-phthalic acid (terephthalic acid), or naphthalenedicarboxylic acid with a glycol. Among them, from the viewpoint of increasing the flame retardancy of the polyurethane foam, it is preferable that the polyol compound contains a phthalic acid-based polyester polyol, which is a condensate of phthalic acid and a glycol, and more preferably contains a p-phthalic acid-based polyester polyol, which is a condensate of p-phthalic acid and a glycol. The glycol is not particularly limited, but it is preferable to use low molecular weight aliphatic glycols known as components of polyester polyols, such as ethylene glycol, propylene glycol, and diethylene glycol.
[0014] The hydroxyl value of the polyester polyol is preferably from 100 to 500 mgKOH / g, more preferably from 150 to 450 mgKOH / g, and further preferably from 180 to 400 mgKOH / g.
[0015] (Polyether polyol) Examples of polyether polyols include polyoxyalkylene polyols obtained by ring-opening addition polymerization of alkylene oxide to an initiator having two or more active hydrogen atoms. Specific examples of the initiator include aliphatic polyhydric alcohols (e.g., glycols such as ethylene glycol, propylene glycol, diethylene glycol, dipropylene glycol, 1,4-butanediol, 1,3-butanediol, 1,6-hexanediol, neopentyl glycol, cyclohexylene glycol, and cyclohexanedimethanol, triols such as trimethylolpropane and glycerin, tetrafunctional alcohols such as pentaerythritol, and highly functional alcohols such as sucrose and sorbitol), aliphatic amines (e.g., alkylenediamines such as ethylenediamine, propylenediamine, butylenediamine, hexamethylenediamine, and neopentyldiamine, and alkanolamines such as monoethanolamine and diethanolamine), and aromatic amines (e.g., aniline, tolylenediamine, xylylenediamine, diphenylmethanediamine, and Mannich condensation products). Polyether polyol preferably has aromatic ring.Among the above, the polyether polyol produced by using an initiator having aromatic ring is the polyether polyol having aromatic ring, for example, the polyether polyol produced by using aromatic amine as initiator is the polyether polyol having aromatic ring.Among the polyether polyols having aromatic ring, tolylenediamine-based polyether polyol, Mannich-based polyether polyol, etc. can be preferably used.
[0016] The tolylenediamine-based polyether polyol is a tolylenediamine-based polyether polyol produced using tolylenediamine as an initiator. The Mannich polyether polyol is a polyether polyol obtained by utilizing the Mannich reaction, which is a Mannich condensation product having two or more hydroxyl groups in the molecule, or an alkylene oxide added to such a Mannich condensation product. More specifically, it is a Mannich condensation product obtained by the Mannich reaction of at least one of phenol and its alkyl-substituted derivatives, formaldehyde and alkanolamine, or a polyether polyol obtained by ring-opening addition polymerization of at least one of ethylene oxide and propylene oxide to this compound.
[0017] The hydroxyl value of the polyether polyol is preferably from 200 to 2,000 mgKOH / g, and more preferably from 300 to 1,000 mgKOH / g.
[0018] <Catalyst> The urethane resin composition of the present invention contains a catalyst. The catalyst may contain, for example, one or both of a resinification catalyst and a trimerization catalyst, and preferably contains both.
[0019] (Metal catalyst (resinized metal catalyst)) The resinification catalyst preferably contains a metal catalyst. This metal catalyst is generally called a resinification metal catalyst. In the present invention, the resinification metal catalyst is contained to promote the reaction between the polyol and the polyisocyanate, and in particular to increase the initial reaction rate. In addition, when a certain amount or more of a filler such as a solid flame retardant described later is contained, the reactivity of the polyurethane foam is inhibited and the foamability is likely to decrease, but the resinification metal catalyst is contained, so that the foamability of the polyurethane foam can be easily maintained well. From the viewpoint of foamability, the metal catalyst preferably contains at least one metal selected from the group consisting of bismuth and tin, and more preferably contains bismuth.
[0020] The resinified metal catalyst is preferably a metal salt selected from bismuth salts and tin salts, more preferably a bismuth salt. The metal salt is preferably an organic acid metal salt, more preferably a metal salt of a carboxylic acid having 5 or more carbon atoms. The carboxylic acid has 5 or more carbon atoms, and is stable to a blowing agent, particularly to hydrofluoroolefin. In addition, the number of carbon atoms of the carboxylic acid is preferably 18 or less, more preferably 12 or less, from the viewpoint of catalytic activity. The carboxylic acid is preferably an aliphatic carboxylic acid, more preferably a saturated aliphatic carboxylic acid. The carboxylic acid may be linear or may have a branched structure, but preferably has a branched structure. Specific examples of carboxylic acids include octyl acid, lauric acid, versatic acid, pentanoic acid, and acetic acid, and among these, octyl acid is preferred. That is, the transition metal salt is preferably a metal salt of octyl acid. These carboxylic acids may be linear as described above, but may also have a branched structure. An example of an octyl acid having a branched structure is 2-ethylhexanoic acid. As the metal salt of carboxylic acid, bismuth salt of carboxylic acid and tin salt of carboxylic acid are preferable, and among them, bismuth salt of octylic acid is preferable. In addition, the metal salt of carboxylic acid may be a carboxylate of an alkyl metal. For example, the tin salt of carboxylic acid may be a dialkyltin carboxylate, and preferably is a dioctyltin carboxylate. Specific examples of metal salts of carboxylic acids include bismuth trioctate, dioctyltin versatate, dibutyltin dilaurate, dioctyltin dilaurate, tin dioctylate, etc., and are preferably bismuth trioctate and dioctyltin versatate, and more preferably bismuth trioctate.
[0021] The content of the resinified metal catalyst in the urethane resin composition is not particularly limited, but is preferably 0.1 to 10 parts by mass, more preferably 0.5 to 8 parts by mass, even more preferably 1 to 6 parts by mass, and particularly preferably 1.5 to 4 parts by mass, relative to 100 parts by mass of polyol.
[0022] (imidazole derivatives) The catalyst used in the urethane resin composition of the present invention preferably contains a resinified amine catalyst as a resinification catalyst. The urethane resin composition more preferably contains a resinified amine catalyst in addition to the above-mentioned resinified metal catalyst. Furthermore, the resinified amine catalyst preferably contains an imidazole derivative. The imidazole derivative is less susceptible to the influence of the hydrofluoroolefin, and makes it easier to react the polyol with the polyisocyanate while increasing the stability of the urethane resin composition. Therefore, by containing the imidazole derivative in addition to the above-mentioned metal catalyst, the urethane resin composition has increased reactivity between the polyol and the polyisocyanate, and has further improved foamability. The imidazole derivative is preferably an imidazole substituted at the 1- and 2-positions with an alkyl group having 8 or less carbon atoms, and the alkyl group preferably has 6 or less carbon atoms, more preferably has 4 or less carbon atoms. A specific example of a suitable imidazole derivative is represented by the following general formula (1).
[0023] [ka] (In general formula (1), R 1 and R 2 each independently represents an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms.
[0024] R in general formula (1) 1 and R 2 each independently represents an alkyl group having 1 to 8 carbon atoms or an alkenyl group having 2 to 8 carbon atoms. The alkyl group and the alkenyl group may each be linear or have a branched structure. Specific examples of the alkyl group include a methyl group, an ethyl group, a propyl group, an isopropyl group, a butyl group, an isobutyl group, a sec-butyl group, a pentyl group, a neopentyl group, an isopentyl group, a sec-pentyl group, a hexyl group, a heptyl group, and an octyl group. Specific examples of the alkenyl group include a vinyl group, a 1-propenyl group, an allyl group, an isopropenyl group, a 1-butenyl group, a 2-butenyl group, a pentenyl group, a hexenyl group, a heptenyl group, and an octenyl group. R 1 and R 2 If the number of carbon atoms in the alkyl or alkenyl group of R is equal to or greater than the lower limit, steric hindrance increases and the copolymer is less susceptible to the effects of blowing agents such as hydrofluoroolefins, which is preferable. 1 and R 2 When the number of carbon atoms in the alkyl group is equal to or less than the above upper limit, the steric hindrance is not extremely large, so that the reaction between the polyol and the polyisocyanate can proceed quickly, and the foaming properties are also good. From these perspectives, R 1 and R 2 are each independently preferably an alkyl group having 1 to 6 carbon atoms, more preferably an alkyl group having 1 to 4 carbon atoms, and further preferably a methyl group.
[0025] The imidazole derivative represented by general formula (1) includes 1,2-dimethylimidazole, 1-ethyl-2-methylimidazole, 1-methyl-2-ethylimidazole, 1,2-diethylimidazole, and 1-isobutyl-2-methylimidazole, among which, from the viewpoint of improving the activity of the catalyst in the presence of hydrofluoroolefin and from the viewpoint of rapidly proceeding the reaction, 1,2-dimethylimidazole and 1-isobutyl-2-methylimidazole are preferred.Moreover, from the viewpoint of further increasing stability, 1,2-dimethylimidazole is even more preferred.
[0026] The content of the imidazole derivative in the urethane resin composition is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, further preferably 2 to 15 parts by mass, and particularly preferably 3 to 10 parts by mass, relative to 100 parts by mass of the polyol. If the content of the imidazole derivative is equal to or more than the lower limit, the formation of a urethane bond is likely to occur, the reaction proceeds quickly, and the foamability is good. On the other hand, if the content of the imidazole derivative is equal to or less than the upper limit, the reaction rate is easily controlled, which is preferable.
[0027] (trimerization catalyst) The urethane resin composition of the present invention preferably further contains a trimerization catalyst. The trimerization catalyst is a catalyst that reacts the isocyanate groups contained in the polyisocyanate to trimerize them and promote the formation of isocyanurate rings. By containing the trimerization catalyst, the reaction of unreacted isocyanate groups is completed, resulting in good flame retardancy. Examples of the trimerization catalyst include metal catalysts and ammonium salts. Examples of metal catalysts (trimerization metal catalysts) used as trimerization catalysts include alkali metal salts, and potassium salts are preferred. Potassium salts include potassium octylate such as potassium 2-ethylhexanoate, potassium acetate, potassium propionate, potassium butanoate, potassium benzoate, and other potassium carboxylates having 2 to 8 carbon atoms. A urethane resin composition containing a potassium salt as a trimerization catalyst promotes a crosslinking reaction, improves the flame retardancy of polyurethane foam, and promotes resin curing, and is therefore suitable for use in spray applications. Furthermore, when the composition is sprayed and mixed with polyisocyanate to react with it, it is easy to form a high-quality polyurethane foam. As the ammonium salt, tertiary ammonium salts such as triethylammonium salts and triphenylammonium salts, and quaternary ammonium salts such as tetramethylammonium salts, tetraethylammonium salts and tetraphenylammonium salts can be used, among which quaternary ammonium salts are preferred. The ammonium salt is, for example, an ammonium salt of a carboxylic acid. As the carboxylic acid in the ammonium salt, for example, a saturated fatty acid having 1 to 10 carbon atoms, preferably 2 to 8 carbon atoms, can be mentioned. The saturated fatty acid may have a hydrocarbon group that is linear or branched, but preferably has a branched group. Specific examples of the carboxylic acid include 2-ethylhexanoic acid, 2,2-dimethylpropanoic acid, acetic acid, and formic acid, among which 2,2-dimethylpropanoic acid is preferred. The trimerization catalyst may be used alone or in combination of two or more kinds.
[0028] The content of the trimerization catalyst in the urethane resin composition is preferably 0.5 to 30 parts by mass, more preferably 1 to 25 parts by mass, further preferably 2 to 20 parts by mass, and particularly preferably 3 to 15 parts by mass, relative to 100 parts by mass of the polyol. When the content of the trimerization catalyst is equal to or more than the lower limit, the trimerization proceeds appropriately, improving the flame retardancy. In addition, there is no significant difference in activity between the resinification and the trimerization, and the foaming can be suppressed from becoming two-stage, resulting in good foaming properties. On the other hand, when the content of the trimerization catalyst is equal to or less than the upper limit, the resinification reaction proceeds actively, and the activity of the trimerization can be promoted by the heat of the resinification reaction, resulting in good foaming properties, and a good polyurethane foam can be formed.
[0029] From the above viewpoints, for example, when a quaternary ammonium salt is contained as a trimerization catalyst, the content of the quaternary ammonium salt is preferably 0.3 to 17 parts by mass, more preferably 0.7 to 15 parts by mass, further preferably 1.5 to 12 parts by mass, and particularly preferably 3 to 10 parts by mass, relative to 100 parts by mass of polyol. Also, when a potassium salt is contained as a trimerization catalyst, the content of the potassium salt is preferably 0.2 to 8 parts by mass, more preferably 0.3 to 7 parts by mass, further preferably 0.5 to 6 parts by mass, and particularly preferably 2 to 5 parts by mass, relative to 100 parts by mass of polyol.
[0030] <Foaming agent> The foaming agent promotes foaming of the urethane resin composition. Examples of the foaming agent include organic physical foaming agents such as water, propane, butane, pentane, hexane, heptane, cyclopropane, cyclobutane, cyclopentane, cyclohexane, cycloheptane, and other low-boiling point hydrocarbons, dichloroethane, propyl chloride, isopropyl chloride, butyl chloride, isobutyl chloride, pentyl chloride, isopentyl chloride, and other chlorinated aliphatic hydrocarbon compounds, hydrofluoroolefins (hereinafter sometimes referred to as "HFO"), ether compounds such as diisopropyl ether, and mixtures of these compounds, and inorganic physical foaming agents such as nitrogen gas, oxygen gas, argon gas, and carbon dioxide gas. Among these, it is preferable to use hydrofluoroolefins (HFOs), which have high stability as a blowing agent, are less likely to decrease in catalytic activity, and further have a low environmental impact.
[0031] Examples of HFOs that are suitable blowing agents include fluoroalkenes having about 3 to 6 carbon atoms. In addition, the HFO may be a hydrochlorofluoroolefin having a chlorine atom, and therefore may be a chlorofluoroalkene having about 3 to 6 carbon atoms. Examples of HFOs include trifluoropropene, tetrafluoropropenes such as HFO-1234, pentafluoropropenes such as HFO-1225, chlorodifluoropropenes, chlorotrifluoropropenes such as HFO-1233, and chlorotetrafluoropropene. More specifically, 3,3,3-trifluoropropene (HFO-1243zf), trans-1,3,3,3-tetrafluoropropene (HFO-1234ze(E)), cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z)), 2,3,3,3-tetrafluoropropene (HFO-1234yf), 1,1,3,3-tetrafluoropropene, cis-1,3,3,3-tetrafluoropropene (HFO-1234ze(Z)), trans-1,2,3,3,3-pentafluoropropene (HFO-1234ze(Z)), Examples of the fluoropropene include fluoropropene (HFO-1225ye(E)), cis-1,2,3,3,3-pentafluoropropene (HFO-1225ye(Z)), 1,1,3,3,3-pentafluoropropene (HFO-1225zc), 1,1,2,3,3-pentafluoropropene (HFO-1225yc), trans-1-chloro-3,3,3-trifluoropropene (HFO-1233zd(E)), and 1,1,1,4,4,4-hexafluorobut-2-ene (HFO-1336mzz). Among these, HFO-1233zd(E) is preferred.
[0032] The content of the blowing agent is preferably 20 to 80 parts by mass, more preferably 30 to 70 parts by mass, and even more preferably 35 to 60 parts by mass, based on 100 parts by mass of the polyol. When the content of the blowing agent is equal to or more than the lower limit, foaming is promoted, the foamability is improved, and the density of the polyurethane foam can be reduced. On the other hand, when the content of the blowing agent is equal to or less than the upper limit, excessive foaming can be suppressed.
[0033] The above-mentioned blowing agents can be used alone or in combination. In the urethane resin composition of the present invention, it is preferable to use the above-mentioned HFO in combination with another blowing agent, for example, HFO may be used in combination with water, oxygen gas, or carbon dioxide gas, which is easy to handle. In particular, water is preferable from the viewpoint of adjusting the isocyanate index and from the viewpoint of ease of handling.
[0034] The content of HFO is preferably 19 to 75 parts by mass, more preferably 29 to 67 parts by mass, and even more preferably 34 to 58 parts by mass, based on 100 parts by mass of polyol. When the content of the blowing agent is equal to or more than the lower limit, foaming is promoted, the foaming property is improved, and the density of the polyurethane foam can be reduced. On the other hand, when the content of the blowing agent is equal to or less than the upper limit, excessive foaming can be suppressed.
[0035] The content of water is preferably 0.1 to 5 parts by mass, more preferably 0.3 to 3 parts by mass, and even more preferably 0.5 to 2 parts by mass, based on 100 parts by mass of polyol. When the content of the blowing agent is equal to or more than the lower limit, foaming is promoted, the foamability is improved, and the density of the polyurethane foam can be reduced. On the other hand, when the content of the blowing agent is equal to or less than the upper limit, excessive foaming can be suppressed.
[0036] <Flame retardants> The urethane resin composition of the present invention contains a flame retardant. By containing a flame retardant, it becomes easier to impart excellent flame retardancy to the polyurethane foam. Examples of the flame retardant include phosphorus-based flame retardants, phosphorus-based solid flame retardants, bromine-containing flame retardants, boron-containing flame retardants, antimony-containing flame retardants, chlorine-containing flame retardants, and metal hydroxides. In addition, it is preferable that the flame retardant contains a phosphorus-based flame retardant from the viewpoint of effectively imparting flame retardancy. In the case where a phosphorus-based flame retardant is contained, it is preferable that at least one selected from a phosphorus-based liquid flame retardant and a phosphorus-based solid flame retardant is contained.
[0037] (Phosphorus-based liquid flame retardant) As the phosphorus-based liquid flame retardant, a phosphate ester-based flame retardant is preferable. Examples of the phosphate ester-based flame retardant include monophosphate ester and condensed phosphate ester. The liquid flame retardant is a flame retardant that becomes liquid at room temperature (23°C) and normal pressure (1 atm). The monophosphate ester is a phosphoric acid ester having one phosphorus atom in the molecule. The monophosphate ester is not particularly limited, but examples thereof include trialkyl phosphates such as trimethyl phosphate, triethyl phosphate, tributyl phosphate, and tri(2-ethylhexyl)phosphate, halogen-containing phosphates such as tris(β-chloropropyl)phosphate, trialkoxy phosphates such as tributoxyethyl phosphate, aromatic ring-containing phosphates such as tricresyl phosphate, trixylenyl phosphate, tris(isopropylphenyl)phosphate, cresyl diphenyl phosphate, and diphenyl(2-ethylhexyl)phosphate, and acidic phosphates such as monoisodecyl phosphate and diisodecyl phosphate. Examples of the condensed phosphate ester include aromatic condensed phosphate esters such as trialkyl polyphosphate, resorcinol polyphenyl phosphate, bisphenol A polycresyl phosphate, and bisphenol A polyphenyl phosphate. Commercially available condensed phosphate esters include, for example, "CR-733S", "CR-741", and "CR747" manufactured by Daihachi Chemical Industry Co., Ltd., and "ADEKA STAB PFR" and "FP-600" manufactured by ADEKA Corporation.
[0038] The phosphoric acid ester may be used alone or in combination of two or more of the above-mentioned phosphoric acid esters. Among these, from the viewpoint of easily adjusting the viscosity of the polyol to an appropriate value and from the viewpoint of improving the flame retardancy of the polyurethane foam, monophosphate esters are preferred, and halogen-containing phosphoric acid esters such as tris(β-chloropropyl)phosphate are more preferred.
[0039] When the urethane resin composition contains a phosphorus-based liquid flame retardant, the content of the phosphorus ester is preferably 5 to 100 parts by mass, more preferably 10 to 80 parts by mass, further preferably 20 to 70 parts by mass, and particularly preferably 35 to 65 parts by mass, relative to 100 parts by mass of the polyol. When the content of the phosphorus ester is equal to or more than the above lower limit, the effect of containing the phosphorus ester is easily exerted, and the flame retardancy is improved. In addition, when the content of the phosphorus ester is equal to or less than the above upper limit, the foaming of the polyurethane foam is not inhibited by the phosphorus ester.
[0040] (Phosphorus-based solid flame retardant) Examples of phosphorus-based solid flame retardants include red phosphorus-based flame retardants, phosphates, etc. Note that a solid flame retardant is a flame retardant that becomes solid at room temperature (23° C.) and normal pressure (1 atm).
[0041] The red phosphorus-based flame retardant may be made of red phosphorus alone, may be red phosphorus coated with a resin, a metal hydroxide, a metal oxide, or may be a mixture of red phosphorus and a resin, a metal hydroxide, a metal oxide, or the like. The resin that coats the red phosphorus or is mixed with the red phosphorus is not particularly limited, but examples of the resin include thermosetting resins such as phenol resin, epoxy resin, unsaturated polyester resin, melamine resin, urea resin, aniline resin, and silicone resin. From the viewpoint of flame retardancy, metal hydroxides are preferred as the compound to be coated or mixed. The metal hydroxide to be used may be appropriately selected from those described below.
[0042] Specific examples of phosphates include monophosphates, polyphosphates, etc. The phosphates mentioned here are not limited to orthophosphates, but also include phosphites, phosphinates, etc. The same applies to polyphosphates. Examples of monophosphates include ammonium salts such as ammonium phosphate, ammonium dihydrogen phosphate, and diammonium hydrogen phosphate; sodium salts such as monosodium phosphate, disodium phosphate, trisodium phosphate, monosodium phosphite, and disodium phosphite; potassium salts such as monopotassium phosphate, dipotassium phosphate, tripotassium phosphate, monopotassium phosphite, and dipotassium phosphite; lithium salts such as monolithium phosphate, dilithium phosphate, trilithium phosphate, monolithium phosphite, and dilithium phosphite; barium salts such as barium dihydrogen phosphate, barium hydrogen phosphate, and tribarium phosphate; magnesium salts such as monohydrogen magnesium phosphate, magnesium hydrogen phosphate, and trimagnesium phosphate; calcium salts such as calcium dihydrogen phosphate, calcium hydrogen phosphate, and tricalcium phosphate; zinc salts such as zinc phosphate and zinc phosphite; and aluminum salts such as monoaluminum phosphate, dialuminum phosphate, trialuminum phosphate, and aluminum phosphite. Among these, ammonium phosphate and aluminum phosphite are preferred, and ammonium phosphate is more preferred. Examples of polyphosphates include ammonium polyphosphate, piperazine polyphosphate, melamine polyphosphate, ammonium amide polyphosphate, aluminum polyphosphate, and the like. Among these, ammonium polyphosphate is preferred.
[0043] Phosphinic acid salts include metal phosphinic acid salts, such as sodium phosphinic acid, calcium phosphinic acid, aluminum phosphinic acid, zinc phosphinic acid, calcium dimethylphosphinic acid, aluminum dimethylphosphinic acid, zinc dimethylphosphinic acid, calcium ethylmethylphosphinic acid, aluminum ethylmethylphosphinic acid, zinc ethylmethylphosphinic acid, calcium diethylphosphinic acid, aluminum diethylphosphinic acid, zinc diethylphosphinic acid, aluminum tris(diethylphosphinic acid), aluminum tris(methylethylphosphinic acid), ... Examples of such titanium dioxide include aluminum tris(dibutylphosphinate), aluminum tris(butylethylphosphinate), aluminum tris(diphenylphosphinate), zinc bis(diethylphosphinate), zinc bis(methylethylphosphinate), zinc bis(diphenylphosphinate), titanyl bis(diethylphosphinate), titanyl tetrakis(diethylphosphinate), titanyl bis(methylethylphosphinate), titanyl tetrakis(methylethylphosphinate), titanyl bis(diphenylphosphinate), and titanyl tetrakis(diphenylphosphinate). The metal phosphinate used in the present invention preferably contains at least one selected from sodium phosphinate and aluminum phosphinate among the above.
[0044] When the urethane resin composition of the present invention contains a phosphorus-based solid flame retardant, it is preferable to contain any one selected from red phosphorus-based flame retardants, polyphosphates, and metal phosphinates, and it is more preferable to contain any one selected from red phosphorus-based flame retardants, ammonium polyphosphate, sodium phosphinate, and aluminum phosphinate. When the composition contains these phosphorus-based solid flame retardants, it is easy to impart excellent flame retardancy to the polyurethane foam while suppressing the shrinkage of the polyurethane foam. In addition, it is preferable that the flame retardant contains a red phosphorus-based flame retardant in particular.
[0045] The content of the phosphorus-based solid flame retardant in the urethane resin composition is preferably 25 to 90 parts by mass, more preferably 30 to 85 parts by mass, and even more preferably 35 to 80 parts by mass, based on 100 parts by mass of the polyol. When the content of these phosphorus-based solid flame retardants is equal to or greater than the above lower limit, it is possible to impart good flame retardancy to the polyurethane foam. In addition, it is easy to form a polyurethane foam with a strong resin structure, and it is easy to suppress the shrinkage of the polyurethane foam. On the other hand, when the content of these phosphorus-based solid flame retardants is equal to or less than the above upper limit, the handling property and foaming property when mixing the polyol with the polyisocyanate are good.
[0046] (Bromine-containing flame retardants) The bromine-containing flame retardant is not particularly limited as long as it contains bromine in its molecular structure and is a solid at room temperature (23°C) and normal pressure (1 atm), and examples thereof include brominated aromatic ring-containing aromatic compounds. Examples of the brominated aromatic ring-containing aromatic compound include monomeric organic bromine compounds such as hexabromobenzene, pentabromotoluene, hexabromobiphenyl, decabromobiphenyl, decabromodiphenyl ether, octabromodiphenyl ether, hexabromodiphenyl ether, bis(pentabromophenoxy)ethane, ethylene bis(pentabromophenyl), ethylene bis(tetrabromophthalimide), and tetrabromobisphenol A.
[0047] In addition, the brominated aromatic ring-containing aromatic compound may be a bromine compound polymer.Specific examples include brominated polycarbonates such as polycarbonate oligomers produced from brominated bisphenol A as a raw material, copolymers of this polycarbonate oligomer and bisphenol A, and diepoxy compounds produced by the reaction of brominated bisphenol A and epichlorohydrin.Furthermore, examples include brominated epoxy compounds such as monoepoxy compounds obtained by the reaction of brominated phenols and epichlorohydrin, brominated phenol condensates of brominated polyphenylene ether, brominated bisphenol A and cyanuric chloride, and uncrosslinked or crosslinked brominated polystyrene. In addition, compounds other than brominated aromatic ring-containing aromatic compounds such as hexabromocyclododecane may be used. These bromine-containing flame retardants may be used alone or in combination of two or more.
[0048] The content of the bromine-containing flame retardant in the urethane resin composition is preferably 5 to 50 parts by mass, more preferably 10 to 45 parts by mass, and even more preferably 15 to 40 parts by mass, based on 100 parts by mass of the polyol. When the content of these bromine-containing flame retardants is equal to or greater than the above lower limit, it is possible to impart good flame retardancy to the polyurethane foam. In addition, it is easy to form a polyurethane foam with a strong resin structure, and it is easy to suppress the shrinkage of the polyurethane foam. On the other hand, when the content of these bromine-containing flame retardants is equal to or less than the above upper limit, the handling property and foaming property when mixing the polyol with the polyisocyanate are good.
[0049] (Boron-containing flame retardants) Examples of boron-containing flame retardants include borax, boron oxide, boric acid, borates, etc. Examples of boron oxide include diboron trioxide, boron trioxide, diboron dioxide, tetraboron trioxide, and tetraboron pentoxide. Examples of borates include borates of alkali metals, alkaline earth metals, elements of Groups 4, 12, and 13 of the periodic table, and ammonium. Specific examples include alkali metal borates such as lithium borate, sodium borate, potassium borate, and cesium borate, alkaline earth metal borates such as magnesium borate, calcium borate, and barium borate, zirconium borate, zinc borate, aluminum borate, and ammonium borate. The boron-containing flame retardants may be used alone or in combination of two or more kinds. The boron-containing flame retardant used in the present invention is preferably a borate, more preferably zinc borate.
[0050] The content of the boron-containing flame retardant in the urethane resin composition is preferably 5 to 60 parts by mass, more preferably 10 to 55 parts by mass, and even more preferably 15 to 50 parts by mass, based on 100 parts by mass of the polyol. When the content of these boron-containing flame retardants is equal to or greater than the above lower limit, it is possible to impart good flame retardancy to the polyurethane foam. In addition, it is easy to form a polyurethane foam with a strong resin structure, and it is easy to suppress the shrinkage of the polyurethane foam. On the other hand, when the content of these boron-containing flame retardants is equal to or less than the above upper limit, the handling property and foaming property when mixing the polyol with the polyisocyanate are good.
[0051] (Antimony-containing flame retardants) Examples of antimony-containing flame retardants include antimony oxide, antimony salts, and pyroantimony salts. Examples of antimony oxide include antimony trioxide and antimony pentoxide. Examples of antimony salts include sodium antimonate and potassium antimonate. Examples of pyroantimonate include sodium pyroantimonate and potassium pyroantimonate. The antimony-containing flame retardants may be used alone or in combination of two or more. The antimony-containing flame retardant used in the present invention is preferably antimony oxide.
[0052] (Chlorine-containing flame retardants) Chlorine-containing flame retardants include those commonly used in polyurethane foams, such as polychlorinated naphthalenes, chlorendic acid, and dodecachlorododecahydrodimethanodibenzocyclooctene, sold under the trade name "Dechlorane Plus."
[0053] (metal hydroxide) Examples of metal hydroxides include magnesium hydroxide, calcium hydroxide, aluminum hydroxide, iron hydroxide, nickel hydroxide, zirconium hydroxide, titanium hydroxide, zinc hydroxide, copper hydroxide, vanadium hydroxide, tin hydroxide, etc. The metal hydroxides may be used alone or in combination of two or more kinds.
[0054] The flame retardant may be contained in combination of two or more kinds. For example, the combination of flame retardants is preferably a combination of a phosphorus-based liquid flame retardant, a phosphorus-based solid flame retardant, and one selected from a bromine-containing flame retardant, a boron-containing flame retardant, an antimony-containing flame retardant, a chlorine-containing flame retardant, and a metal hydroxide, and more preferably a combination of a phosphorus-based liquid flame retardant, a phosphorus-based solid flame retardant, and one or both of a bromine-containing flame retardant and a boron-containing flame retardant. In this case, the phosphorus-based solid flame retardant is preferably a red phosphorus-based flame retardant.
[0055] The total content of the flame retardant in the urethane resin composition is preferably from 90 to 200 parts by mass, more preferably from 100 to 190 parts by mass, and even more preferably from 110 to 180 parts by mass, relative to 100 parts by mass of the polyol.
[0056] <Inorganic fillers> The urethane resin composition may contain an inorganic filler other than the solid flame retardant. As the inorganic filler, needle-shaped filler, alumina, titanium oxide, calcium oxide, magnesium oxide, iron oxide, tin oxide, ferrites, basic magnesium carbonate, calcium carbonate, magnesium carbonate, zinc carbonate, barium carbonate, dawsonite, hydrotalcite, calcium sulfate, barium sulfate, calcium silicate, talc, mica, montmorillonite, bentonite, activated clay, imogolite, sericite, glass beads, aluminum nitride, boron nitride, silicon nitride, various metal powders, magnesium sulfate, lead zirconate titanate, molybdenum sulfide, silicon carbide, various magnetic powders, fly ash, etc. may be appropriately used. These inorganic fillers may be used alone or in combination of two or more. The inorganic filler used in the present invention is not particularly limited, but from the viewpoint of imparting good mechanical properties to the polyurethane foam, it is preferable to contain a needle-shaped filler among the above-mentioned ones.
[0057] (Needle filler) Examples of needle-like fillers include potassium titanate whiskers, aluminum borate whiskers, magnesium-containing whiskers, silicon-containing whiskers, wollastonite, sepiolite, zonolite, elestadite, boehmite, rod-shaped hydroxyapatite, glass fibers, carbon fibers, graphite fibers, metal fibers, slag fibers, gypsum fibers, silica fibers, alumina fibers, silica alumina fibers, zirconia fibers, boron nitride fibers, boron fibers, and stainless steel fibers. These needle-like fillers can be used alone or in combination of two or more. The aspect ratio (length / diameter) of the needle-like filler used in the present invention is preferably in the range of 5 to 50, and more preferably in the range of 10 to 40. The aspect ratio can be determined by observing the needle-like filler with a scanning electron microscope and measuring its length and width.
[0058] <Foam stabilizer> The urethane resin composition may contain a foam stabilizer. The foam stabilizer can improve the foaming properties of the polyurethane foam, and can promote foaming when reacting with polyisocyanate during spraying, for example. The foam stabilizer may be specifically a surfactant, more specifically a nonionic surfactant, a cationic surfactant, an anionic surfactant, etc. Specific examples of nonionic surfactants include polyoxyalkylene foam stabilizers such as polyoxyalkylene alkyl ethers, silicone foam stabilizers such as organopolysiloxanes, etc. The foam stabilizer used in the present invention is not particularly limited, but silicone foam stabilizers are preferred from the viewpoint of foaming properties. The foam stabilizer may be used alone or in combination of two or more kinds.
[0059] <Polyisocyanate> Examples of the polyisocyanate in the present invention include aromatic polyisocyanates, alicyclic polyisocyanates, and aliphatic polyisocyanates. Examples of aromatic polyisocyanates include phenylene diisocyanate, tolylene diisocyanate, xylylene diisocyanate, diphenylmethane diisocyanate, dimethyldiphenylmethane diisocyanate, triphenylmethane triisocyanate, naphthalene diisocyanate, and polymethylene polyphenyl polyisocyanate (polymeric MDI).
[0060] Examples of the alicyclic polyisocyanate include cyclohexylene diisocyanate, methylcyclohexylene diisocyanate, isophorone diisocyanate, dicyclohexylmethane diisocyanate, and dimethyldicyclohexylmethane diisocyanate.
[0061] Examples of the aliphatic polyisocyanate include methylene diisocyanate, ethylene diisocyanate, propylene diisocyanate, tetramethylene diisocyanate, and hexamethylene diisocyanate.
[0062] Among these, from the viewpoints of ease of use and availability, aromatic polyisocyanates are preferred, diphenylmethane diisocyanate, polymeric MDI, or a mixture thereof is more preferred, and among these, diphenylmethane diisocyanate is even more preferred, and 4,4'-diphenylmethane diisocyanate is particularly preferred. The polyisocyanates may be used alone or in combination of two or more. Furthermore, the polyisocyanate may be appropriately mixed with known additives to be mixed with the polyisocyanate before being mixed with the polyol composition containing the polyol.
[0063] <Other ingredients> The urethane resin composition may contain, as necessary, one or more selected from additives such as phenol-based, amine-based, and sulfur-based antioxidants, heat stabilizers, metal damage inhibitors (metal deactivators), antistatic agents, stabilizers, crosslinking agents, lubricants, softeners, plasticizers, and tackifier resins, and tackifiers such as polybutene and petroleum resins, within the scope of the present invention.
[0064] The urethane resin composition of the present invention is cured by the reaction of polyol and polyisocyanate. Therefore, before using the urethane resin composition, the foamable urethane resin composition is divided into two or more parts to prevent the urethane resin composition from reacting and curing. When using the urethane resin composition, it is preferable to combine the two or more parts of the urethane resin composition into one.
[0065] When the urethane resin composition of the present invention is divided into two or more components, each of the two or more divided components does not start curing by itself, but the curing reaction starts after the respective components of the composition are mixed. Usually, a two-component type in which the composition is divided into a polyol composition containing a polyol and a polyisocyanate composition containing a polyisocyanate is preferred.
[0066] The above-mentioned catalyst, blowing agent, and flame retardant, as well as other components contained as necessary, may be contained in the polyol composition, may be contained in the polyisocyanate composition, or may be provided separately from the polyol composition and the polyisocyanate composition, but are preferably contained in the polyol composition. The polyisocyanate composition may be composed of a simple polyisocyanate.
[0067] The polyol composition and the polyisocyanate composition to be mixed with the polyol composition preferably have substantially the same volume. Specifically, the volume ratio of the polyisocyanate composition to the polyol composition is preferably 0.8 to 1.2, more preferably 0.9 to 1.1, and further preferably 0.95 to 1.05.
[0068] <Heat generation rate> In the present invention, the polyurethane foam obtained by foaming the urethane resin composition has a heat release rate of 150 BTU / ft 4 in 1 minute measured in accordance with the FM4975 test standard. 2 / min or less, heat generation rate in 2 minutes is 140 BTU / ft 2 / min or less, and the heat generation rate in 3 minutes is 130 BTU / ft 2 / min or less. If the heat release rate per hour does not satisfy the above requirements, the polyurethane foam will have insufficient flame retardancy, making it difficult to prevent the spread of fire. From the standpoint of improving the flame retardancy and making it possible to prevent the spread of fire, the heat release rate per minute must be 145 BTU / ft 2 / min or less, and 140 BTU / ft 2 / min or less is more preferable, and 145 BTU / ft 2 From the same viewpoint, the heat release rate in 2 minutes is preferably 135 BTU / ft 2 / min or less, and 130 BTU / ft 2 / min or less is more preferable, and 125 BTU / ft 2From the same viewpoint, it is more preferable that the heat generation rate in 3 minutes is 125 BTU / ft 2 / min or less, and 120 BTU / ft 2 / min or less is more preferable, and 115 BTU / ft 2 It is more preferable that the rate is equal to or less than 1 / min. In the present invention, the measurement of the FM4975 test standard was performed by preparing two types of substrates (1.3 m long, 1.5 m wide, 1 / 2 inch high) of Douglas fir plywood and cellulose fiberboard (1.3 m long, 1.5 m wide, 5 / 8 inch high), and foaming the urethane resin composition on each of the two substrates to prepare two types of polyurethane foams with a thickness of 15 mm. When preparing the polyurethane foam, the urethane resin composition may be foamed using a spraying device, as described below. In the present invention, it is sufficient that the heat generation rates for one of the two samples over 1, 2, and 3 minutes are all equal to or less than the upper limit values described above, but it is preferable that the heat generation rates for both samples over 1, 2, and 3 minutes are all equal to or less than the upper limit values described above.
[0069] <Isocyanate Index> The isocyanate index of the urethane resin composition of the present invention is not particularly limited, but is preferably 300 or more. If the isocyanate index is equal to or more than the lower limit, the amount of polyisocyanate relative to the polyol becomes excessive, and isocyanurate bonds due to the trimer of polyisocyanate are easily formed, resulting in improved flame retardancy of the polyurethane foam. Furthermore, if the isocyanate index is equal to or more than the lower limit, combined with the use of the various catalysts described above, it is easy to produce a polyurethane foam having sufficient isocyanurate bonds, that is, a polyurethane foam having both high levels of flame retardancy and heat insulation. From these viewpoints, the isocyanate index is more preferably 350 or more, and even more preferably 400 or more. The isocyanate index is preferably not more than 1,000, more preferably not more than 800, and even more preferably not more than 600. When the isocyanate index is not more than the above upper limit, flame retardancy that is sufficiently commensurate with the production costs can be obtained.
[0070] The isocyanate index can be calculated by the following method. Isocyanate Index = equivalents of polyisocyanate ÷ (equivalents of polyol + equivalents of water) × 100 Here, each equivalent number can be calculated as follows: Equivalent number of polyisocyanate = Amount of polyisocyanate used (g) × NCO content (mass%) / Molecular weight of NCO (mol) × 100 Equivalent weight of polyol = OHV × amount of polyol used (g) ÷ molecular weight of KOH (mmol) OHV is the hydroxyl value of the polyol (mg KOH / g). Equivalents of water = amount of water used (g) / molecular weight of water (mol) × number of OH groups in water In the above formulas, the molecular weight of NCO is 42 (mol), the molecular weight of KOH is 56,100 (mmol), the molecular weight of water is 18 (mol), and the number of OH groups in water is 2.
[0071] <Application> The urethane composition of the present invention can be preferably used for spraying. Therefore, the urethane composition and polyurethane foam of the present invention are excellent in flame retardancy and heat insulation, and can be suitably used for buildings such as walls, ceilings, roofs, and floors of buildings, and the polyurethane foam may be molded by spraying the walls, ceilings, roofs, floors, etc.
[0072] <Method of manufacturing polyurethane foam> As described above, the method for producing a polyurethane foam of the present invention involves obtaining a urethane resin composition and foaming the obtained urethane resin composition to produce a polyurethane foam. As described above, the urethane resin composition can be obtained by mixing the polyol composition and the polyisocyanate composition. However, it is preferable to prepare a polyol composition containing at least a polyol, a catalyst, a foaming agent, and a flame retardant, and then mix the polyol composition with the polyisocyanate composition to obtain the urethane resin composition.
[0073] The polyurethane foam is preferably produced using, for example, a foaming machine. For example, the polyurethane foam may be produced by mixing the polyol composition with the polyisocyanate composition in a foaming machine or the like, and foaming the resulting mixed liquid (urethane resin composition). As the foaming machine, a spray device having a spray gun or the like may be used. The polyol composition is preferably fed to a foaming machine and mixed by collision inside the foaming machine with a polyisocyanate composition fed from another container, etc. Then, the mixed liquid (urethane composition) is preferably discharged from a discharge port of a spray gun, etc., and a polyurethane foam is formed from the discharged urethane resin composition.
[0074] The present production method is preferably applicable to spray applications, and therefore the mixed liquid discharged from the foaming machine may be sprayed onto a target surface at a certain discharge pressure to cause foaming, thereby forming a polyurethane foam on the target surface. EXAMPLES
[0075] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.
[0076] [Materials used] <Polyisocyanate> 4,4'-Diphenylmethane diisocyanate (4,4'-MDI) (manufactured by Manka Chemical Japan Co., Ltd., product name: PM200)
[0077] <Polyol Composition> (Polyol) Polyester polyol (Hitachi Chemical Co., Ltd., product name: SV-208, hydroxyl value = 235 mg KOH / g) · Polyether polyol (manufactured by AGC, product name: Excenol 750ED, hydroxyl value = 750 mgKOH / g)
[0078] (Flame retardant) · Phosphorus-based liquid flame retardant (phosphate ester, tris(β-chloropropyl) phosphate, manufactured by Daihachi Chemical Industry Co., Ltd., product name: TMCPP) · Phosphorus-based solid flame retardant (red phosphorus, manufactured by Phosphorus Chemical Industry Co., Ltd., product name: Nova Excel 140) · Boron-containing flame retardant (zinc borate, manufactured by Hayakawa Trading Co., Ltd., product name: Firebrake ZB) · Bromine-containing flame retardant (hexabromobenzene, manufactured by Manac Co., Ltd., product name: HBB-b)
[0079] (Catalyst) · Ammonium salt (trimerization catalyst), tetramethylammonium 2,2-dimethylpropanoate (manufactured by Air Products, product name: DABCO® TMR7) concentration 45 - 55 mass% · Metal catalyst (trimerization catalyst), potassium 2-ethylhexanoate (manufactured by Air Products, product name: DABCO® K-15) concentration 70 - 80 mass% · Resinified metal catalyst, bismuth trioctoate (manufactured by Nitto Kasei Co., Ltd., product name: Neostan U-600) concentration 55 - 58 mass% · Resinified amine catalyst, 1,2-dimethylimidazole (manufactured by Tosoh Corporation, product name: TOYOCAT DM70) concentration 65 - 75 mass%
[0080] (Blowing agent) · Hydrofluoroolefin (HFO), trans-1-chloro-3,3,3-trifluoropropene (manufactured by Honeywell, product name: Solstice LBA) · Water
[0081] [Evaluation method for polyurethane foam] <FM4975 test standard (heat release rate)> Two types of substrates were prepared: Douglas fir plywood (1.3 m long, 1.5 m wide, 1 / 2 inch high) and cellulose fiberboard (1.3 m long, 1.5 m wide, 5 / 8 inch high). Spray foaming was performed on each of the two substrates to produce two types of polyurethane foam samples with a thickness of 15 mm. The heat release rate of the two samples was measured for any one, two, or three minute period in accordance with the FM4975 test standard. The evaluation criteria for the heat release rate for one, two, and three minutes are as follows: 《Conditions for ○》 150 BTU / ft for 1 minute at the specified test time 2 / min or less 140 BTU / ft for a 2-minute period during the test 2 / min or less 130 BTU / ft for a 3-minute period during the test 2 / min or less "Condition x" ·Does not meet any of the conditions
[0082] [Examples 1-2, Comparative Example 1] A polyol composition was prepared by mixing each component according to the formulation shown in Table 1. Under the following conditions, the polyol composition and polyisocyanate were mixed to obtain a urethane resin composition, and two types of samples were produced by preparing polyurethane foam on two types of substrates prepared, and evaluated based on the evaluation method described above. The results are shown in Table 1. <Manufacturing conditions> Spray machine: Graco HVR spray machine Settings (Heater settings) Isocyanate heater: 38℃ Premix heater (for heating polyol composition): 38℃ Hose heater (for heating polyisocyanate and polyol compositions before mixing): 38°C Pressure: Adjust so that the mist becomes a wide circular shape. · Substrate temperature (temperature of the surface to be sprayed): 20℃±1℃
[0083] [Table 1] *The catalyst content is the content in the product. *The heat release rate of the sample made of Douglas fir plywood in Example 1 was measured for 1, 2, and 3 minutes in accordance with the FM4975 test standard, and the results were 107, 97, and 103 BTU / ft 2 In addition, the heat generation rate of the sample using the cellulose fiber board of Example 1 was measured for any one, two, or three minute period in accordance with the FM4975 test standard, and the results were 83, 77, and 79 BTU / ft 2 / min. *The heat release rate of the sample made of Douglas fir plywood in Example 2 was measured in accordance with the FM4975 test standard for 1, 2, and 3 minutes, and the results were 76, 73, and 74 BTU / ft 2 In addition, the heat generation rate of the sample using the cellulose fiber board of Example 2 was measured for any one, two, or three minute period in accordance with the FM4975 test standard, and the results were 110, 106, and 109 BTU / ft 2 / min.
[0084] As is clear from the results of the above Examples and Comparative Examples, the polyurethane foams formed using the urethane resin compositions of the Examples had heat release rates below the prescribed values for 1 minute, 2 minutes, and 3 minutes in both samples, satisfying the criteria of the FM4975 test standard and therefore exhibiting good flame retardancy. In contrast, for the polyurethane foams formed using the urethane resin composition of the comparative example, the heat release rates at 1 minute, 2 minutes, and 3 minutes were all greater than the prescribed values in both samples, and did not meet the criteria of the FM4975 test standard, resulting in poor flame retardancy.
Claims
1. A urethane resin composition for obtaining a polyurethane foam, comprising: Contains polyol, polyisocyanate, catalyst, blowing agent and flame retardant, The polyurethane foam obtained by foaming the urethane resin composition has a heat generation rate of 150 BTU / ft in one minute measured in accordance with the FM4975 test standard. 2 / min or less, heat generation rate in 2 minutes is 140 BTU / ft 2 / min or less, and the heat generation rate in 3 minutes is 130 BTU / ft 2 / min or less.
2. The urethane resin composition according to claim 1 , wherein the catalyst comprises a metal catalyst containing at least one metal selected from the group consisting of bismuth and tin.
3. The urethane resin composition according to claim 1 , wherein the catalyst comprises a quaternary ammonium salt.
4. The urethane resin composition of claim 1 , wherein the catalyst comprises a potassium salt.
5. The urethane resin composition according to claim 1 , wherein the catalyst comprises an imidazole derivative.
6. The urethane resin composition according to claim 1 , wherein the flame retardant comprises a red phosphorus-based flame retardant.
7. The urethane resin composition according to claim 1, having an isocyanate index of 300 or more.
8. The urethane resin composition according to any one of claims 1 to 7, which is used for spray applications.
9. A polyurethane foam obtained by foaming the urethane resin composition according to any one of claims 1 to 7.
Citation Information
Patent Citations
Non-combustible panel and its manufacturing process
JP2004050495A
Active hydrogen-containing composition for production of resin and method for producing foam
JP2016124912A
Mixed liquid agent, polyurethane composition, polyurethane foam, spray can, and mixing system
US20220002582A1
Polyurethane composition raw material liquid, polyurethane composition, and mixed discharge system
US20220049113A1
Flame-retardant urethane resin composition
WO2014112394A1
Cited By
Preparation method of polyurethane foam and combined polyether used for preparing polyurethane foam
CN118027336A
Process for the preparation of polyurethane foams and combined polyethers used for the preparation of the polyurethane foams
CN118027336B