Papermaking felt and manufacturing method thereof

The papermaking felt with a base fabric, batt layer, and 100% rayon nonwoven fabric layer addresses water squeezing and air permeability issues by ensuring even distribution and gradual fiber loss, maintaining effective moisture transfer and preventing dirt accumulation.

JP2024139568APending Publication Date: 2024-10-09NIPPON FELT CO
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023050568
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-27
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing papermaking felts face issues with water squeezing performance due to strong interfiber bonding in spunbond nonwoven fabrics, leading to decreased air permeability and easy accumulation of dirt, while hydrophilic fibers tend to fall off prematurely, reducing moisture transfer effectiveness.

Method used

A papermaking felt structure incorporating a base fabric, batt layer, and a nonwoven fabric layer made of 100% rayon fibers with a fiber length of 5 to 35 mm, intertwined through needle punching, ensuring even distribution and gradual fiber loss over time, enhancing water transfer and maintaining air permeability.

Benefits of technology

The structure provides excellent water squeezing properties from the initial stage and maintains them without impairing stain resistance, with gradual fiber loss preventing density increase and dirt accumulation, improving moisture transfer efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139568000001_ABST
    Figure 2024139568000001_ABST
Patent Text Reader

Abstract

To provide a papermaking felt that has very good water squeezability from the initial stage of use and can maintain its excellent water squeezability without losing its antifouling property, and a method for manufacturing the same.SOLUTION: A papermaking felt 1 of the invention has: a base fabric 2; a batt layer 3; and a nonwoven fabric layer 4. The nonwoven fabric layer 4 is formed by needlepunching a 100% rayon nonwoven fabric. The rayon fibers in nonwoven fabric layer 4 have a fiber length of 5 to 35 mm. The 100% rayon non-woven fabric preferably has a basis weight of 15-60 g / m2. The non-woven fabric layer 4 is preferably placed directly above or below the base fabric 2 or between the outer surface inner layer 8a and outer surface outer layer 8b of the batt layer 3.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a papermaking felt and a method for producing the same. [Background technology]

[0002] Papermaking felts are used in the press part of papermaking machines to transport wet paper to be squeezed. The papermaking felt carrying the wet paper is pressed by a pair of press rolls, and the water contained in the wet paper is transferred to the papermaking felt, squeezing the water out of the wet paper. Papermaking felts include a base fabric in which warp and weft threads are woven together, and a batt layer that is integrated with the base fabric by needle punching. To improve the water squeezing ability, it has been proposed to add other layers to the papermaking felt or to change the composition of the batt layer.

[0003] For example, Patent Document 1 focuses on the "fineness (thickness)" and "basis weight" of hydrophilic nonwoven fabric, proposing to place a layer of hydrophilic nylon nonwoven fabric in a batt layer on the papermaking surface side (wet paper side) of a base fabric, to make the fibers of the hydrophilic nonwoven fabric thinner than the fibers of the batt layer located on the papermaking surface side of the hydrophilic nonwoven fabric, and to set the basis weight ratio between them to 8:1 to 3:1. The capillary phenomenon causes moisture transfer to the hydrophilic nonwoven fabric, and the transferred moisture is retained, suppressing the rewetting phenomenon in which moisture absorbed in the papermaking felt returns to the wet paper after the pressure of the press roll is released.

[0004] Also, for example, Patent Document 2 focuses on the "elasticity" of the batt layer and proposes using a mixture of "low elasticity" regenerated cellulose fibers such as viscose rayon having an elasticity of less than 25% of that of nylon 6 and polymer fibers such as nylon as the staple fibers that make up the batt layer. In particular, by mixing such "low elasticity" regenerated cellulose fibers as the fibers that make up the batt layer on the wet paper web side surface, the time it takes for the papermaking felt to return to its original thickness from the compressed state after pressure application is increased. This allows the wet paper web to be separated from the papermaking felt more quickly, and rewetting of the wet paper web can be suppressed. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2004-143627 A [Patent Document 2] Special Publication No. 2007-516365 Summary of the Invention [Problem to be solved by the invention]

[0006] When the nonwoven fabric layer is made of a spunbonded nonwoven fabric of synthetic fibers such as nylon, as in the papermaking felt described in Patent Document 1, the synthetic spunbonded nonwoven fabric has strong interfiber adhesion, so it does not collapse when needle punched, and the synthetic fibers that make up the spunbonded nonwoven fabric are difficult to disperse and are distributed as layers. When the nonwoven fibers are distributed as layers, the papermaking felt increases in density because the fibers are difficult to fall off even at the end of use, reducing breathability and making it easier for dirt to accumulate.

[0007] In addition, the surface of the papermaking felt is easily damaged by showers such as washing in the press part, and is easily damaged by being sucked by a suction box. For this reason, when hydrophilic fibers are arranged on the surface of the papermaking side (wet paper side) of the papermaking felt as in Patent Document 2, the hydrophilic fibers are easily dropped off at the beginning of use. In addition, when hydrophilic fibers such as regenerated cellulose fibers are used as batt fibers (staple fibers constituting the batt layer), even when they are arranged in the batt layer on the surface of the papermaking side or in the batt layer inside, the batt fibers are dispersed throughout the felt, and the hydrophilic fibers are not in close contact with each other, so that the hydration force is not easily exerted and the hydrophilic fibers are not easily contributed to moisture transfer. In addition, since fine hydrophilic fibers of about 1 to 5 dtex are not bonded to each other, the hydrophilic fibers are easily dropped off before the papermaking felt reaches an optimal density for squeezing water, that is, at the beginning of use, and the effect of dewatering performance is reduced from the beginning of use.

[0008] In view of the above background, an object of the present invention is to provide a papermaking felt which has very good water drainage from the initial stage of use and can maintain excellent water drainage without impairing stain resistance, and a method for producing the same. [Means for solving the problem]

[0009] In order to solve the above problems, a papermaking felt (1, 11, 21) according to an embodiment of the present invention comprises a base fabric 2, a batt layer (3) including a back layer (7) arranged on the running surface side of the base fabric and a front layer (8) arranged on the papermaking surface side of the base fabric, and a nonwoven fabric layer (4) arranged between the base fabric and the back layer or the front layer, or within the batt layer, and formed by needle punching a nonwoven fabric consisting of 100% rayon fiber (cellulose), the batt layer and the nonwoven fabric layer are integrated with the base fabric by the needle punching so that the rayon fiber is dispersed inside the batt layer and inside the base fabric, and the rayon fiber constituting the nonwoven fabric has a fiber length of 5 to 35 mm. As shown in FIG. 7, the fibers of the batt layer and the nonwoven fabric layer are intricately intertwined by the needle punching and are also intricately intertwined with the base fabric, so that it is almost impractical to directly specify the batt layer and the nonwoven fabric layer by their structure or properties. For this reason, the batt layer and the nonwoven fabric layer were specified by a method of intertwining fibers called "needle punching."

[0010] According to this embodiment, moisture is easily transferred to the nonwoven fabric layer composed of 100% rayon fibers. In addition, since the fiber length of the 100% rayon nonwoven fabric is 5 to 35 mm, the rayon fibers are appropriately dispersed by needle punching, and although the nonwoven fabric fibers are unlikely to fall off at the beginning of use, they gradually fall off during use, and at the end of use, they have fallen off, so that an increase in density is suppressed and dirt is unlikely to accumulate.

[0011] In the above embodiment, the nonwoven fabric layer (4) may be adjacent to the base fabric (2).

[0012] According to this embodiment, the nonwoven fabric is less likely to be damaged by showers or suction boxes during pressing. Therefore, the nonwoven fabric fibers are less likely to fall off in the early stages of use, and the effect of improving water squeezing is maintained. In addition, by dispersing fine nonwoven fabric fibers even in the base fabric layer, which has many voids, the difference in water pressure between the batt layer and the base fabric layer can be reduced, resulting in an internal structure in which the water pressure between the wet paper, the surface layer, and the base fabric layer changes gradually. Therefore, water can be more easily transferred from the wet paper to the inside of the papermaking felt, improving water squeezing.

[0013] In the above aspect, the rayon fibers may be crimped and randomly arranged in the nonwoven fabric.

[0014] According to this embodiment, the rayon fibers are crimped, which results in a structure of interfiber voids suitable for water absorption and water retention, which increases the water absorption rate and allows the fabric to retain a large amount of water, thereby improving water drainage. Also, the rayon fibers are randomly arranged in the nonwoven fabric, which makes it easier for the rayon fibers to be grasped and carried by needles to the base fabric and batt layer during needle punching. As a result, the nonwoven fabric structure is more easily broken down and the rayon fibers are more easily dispersed into the base fabric and batt layer, which makes it difficult for the density to increase even at the end of use, and makes it difficult for dirt to accumulate.

[0015] In the above embodiment, the nonwoven fabric has a density of 15 to 60 g / m 2 It is advisable to have a weight of

[0016] According to this embodiment, a papermaking felt having a good balance between water drainage and air permeability is obtained.

[0017] In the above aspect, the rayon fibers preferably have a fiber length of 5 to 15 mm.

[0018] According to this embodiment, since the nonwoven fabric is made of 100% rayon fibers having a fiber length of 5 to 15 mm, the nonwoven fabric structure is easily broken down by needle punching, and the density is not easily increased even at the end of use. Therefore, the breathability is not easily decreased, and dirt is not easily accumulated.

[0019] In the above embodiment, the rayon fiber may have a fiber length of 10 to 30 mm.

[0020] According to this embodiment, water decompression is improved.

[0021] In the above aspect, the rayon fibers are preferably finer than the staple fibers that make up the batt layer.

[0022] According to this embodiment, the rayon fibers are easily dispersed in the gaps in the base fabric, so that dirt is less likely to accumulate.

[0023] A method for producing a papermaking felt (1, 11, 21) according to one embodiment of the present invention comprises the steps of overlapping a nonwoven fabric composed of 100% rayon fiber and a staple fiber sheet to be at least a part of the batt layer (3) on a base fabric (2), and needle punching the overlapped product to integrate them, the rayon fiber having a fiber length of 5 to 35 mm.

[0024] According to this embodiment, a papermaking felt can be produced in which rayon fibers having a fiber length of 5 to 35 mm are appropriately dispersed in the base fabric and the batt layer, so that the papermaking felt has very good water drainage from the beginning of use and can maintain excellent water drainage without impairing the stain resistance. Effect of the Invention

[0025] According to the above-mentioned aspects, it is possible to provide a papermaking felt that has very good water drainage from the beginning of use and can maintain excellent water drainage without impairing the stain resistance, and a method for producing the same. [Brief description of the drawings]

[0026] [Figure 1] Schematic cross-sectional view (warp cross-section) of a papermaking felt according to a first embodiment. [Diagram 2] Schematic cross-sectional views of papermaking felts according to second and third embodiments (warp cross-section, A: second embodiment, B: third embodiment) [Diagram 3] Schematic cross-sectional views of papermaking felts according to examples and comparative examples [Figure 4] An explanatory diagram showing the test method for the water squeezing test [Diagram 5] Graph showing the results of water absorbency evaluation test [Figure 6] Graph showing the results of the water squeezing test [Figure 7] Electron microscope photograph of the embodiment (cross section) DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In the following description, the papermaking side refers to the side (outer side) of the papermaking felt 1 attached to the papermaking machine that supports the wet paper, and the running side refers to the side (inner side) that is supported by the rolls of the papermaking machine. In Figs. 1 to 3, the upper side of the paper surface is the papermaking side, and the lower side of the paper surface is the running side.

[0028] Fig. 1 is a schematic cross-sectional view of a papermaking felt 1 according to a first embodiment. The papermaking felt 1 comprises a base fabric 2, a batt layer 3, and a nonwoven fabric layer 4. Note that Fig. 1 is a schematic view in which each layer is shown separated from the other layers, but in reality, the fibers constituting the batt layer 3 and the nonwoven fabric layer 4 are entangled by needle punching and dispersed in the thickness direction, and are integrated with the base fabric 2 (see Fig. 7, and the same applies to Figs. 2 and 3).

[0029] The base fabric 2 includes warp threads 5 and weft threads 6 woven into the warp threads 5. The material constituting the warp threads 5 and the weft threads 6 is not particularly limited, but for example, polyamide-based resins and polyester-based resins can be used. Examples of polyamide-based resins include nylons such as 66 nylon, 6 nylon, 12 nylon, 11 nylon, 610 nylon, and 612 nylon. The polyester-based resin is not particularly limited to the type as long as it is a polyester made of dicarboxylic acid and glycol, and examples of the polyester-based resin include polyethylene terephthalate (PET), polypropylene terephthalate, polybutylene terephthalate (PBT), and polyethylene naphthalate. These may be used alone or in combination of two or more types. In addition, the warp threads 5 and the weft threads 6 may be made of the same material or different materials. In addition, each thread may be made of a single material, or may be made of two or more different materials. The type of threads of the warp threads 5 and the weft threads 6 is not particularly limited, but may be, for example, a monofilament single thread, a monofilament twisted thread, a multifilament twisted thread, or a combination thereof. In this embodiment, the base fabric 2 is composed of a single plain weave woven fabric, but the base fabric 2 may be woven in a manner other than a plain weave, and may be a double weave (a structure in which one of the warp threads 5 and weft threads 6 is arranged in two layers, one above the other, and the other is arranged in a single layer, and they are woven together) or a triple weave (a structure in which the paper-making surface side and the running surface side are composed of separate warp threads 5 and weft threads 6, respectively, and are joined together into one piece by a bonding thread), or may be a structure in which multiple woven fabrics are layered on top of each other.

[0030] The batt layer 3 includes a back layer 7 arranged on the running surface side of the base fabric 2, and a surface layer 8 arranged on the papermaking surface side of the base fabric. The surface layer 8 includes a surface inner layer 8a arranged on the base fabric 2 side, and a surface outer layer 8b arranged on the papermaking surface side. The batt layer 3 is formed by needle punching a staple fiber sheet on the base fabric 2, and is integrated with the base fabric 2. The material of the staple fibers constituting the batt layer 3 is not particularly limited, but for example, the above-mentioned nylon can be used. The staple fibers constituting the batt layer 3 usually have a thickness of 2 to 150 dtex (the numerical range "x or more and y or less" is expressed as "x to y"), preferably 5 to 120 dtex, more preferably 9 to 100 dtex, and a fiber length of 40 to 100 mm. The thickness and fiber length of the batt layer 3 are appropriately set according to the characteristics required for the papermaking felt 1, such as the surface properties and porosity, and the outer surface layer 8b that comes into contact with the paper uses finer fibers than the inner surface layer 8a.

[0031] The nonwoven fabric layer 4 is disposed between the base fabric 2 and the surface layer 8, directly on the base fabric 2, i.e., adjacent to the paper-making surface of the base fabric 2. The nonwoven fabric layer 4 is formed by needle punching a nonwoven fabric composed of 100% rayon fiber. The rayon fiber of the nonwoven fabric layer 4 has a fiber length of 5 to 35 mm, preferably 5 to 15 mm. The nonwoven fabric for forming the nonwoven fabric layer 4 has a fiber length of 15 to 100 g / m 2 , preferably 15 to 60 g / m 2 The rayon fibers of the nonwoven fabric layer 4 are thinner than the staple fibers constituting the batt layer 3, and have a thickness of 1 to 5 dtex. The nonwoven fabric for the nonwoven fabric layer 4 is a nonwoven fabric in which the fibers are self-fused to each other to form a sheet without using a binder (adhesive), and the rayon fibers are randomly arranged without being aligned in a specific direction such as the machine direction or cross machine direction, and the crimp number is preferably 20 to 30 per 2.54 cm (per inch), and may have heat-fused portions.

[0032] A method for manufacturing the papermaking felt 1 will be described. An operator manufactures the papermaking felt 1 according to the following procedure. First, the base fabric 2 is woven. Next, a nonwoven fabric composed of 100% rayon fiber to become the nonwoven fabric layer 4 is laid on the papermaking surface side of the base fabric 2, and a staple fiber sheet (short fiber sheet) to become the portion 8c of the front inner layer 8a on the papermaking surface side of the nonwoven fabric is laid on the papermaking surface side of the nonwoven fabric, and these are integrated by needle punching to create a first work-in-progress. Next, a staple fiber sheet to become the portion 8d of the front inner layer 8a on the papermaking surface side of the first work-in-progress is laid on the papermaking surface side of the first work-in-progress, and these are integrated by needle punching to create a second work-in-progress. Next, a staple fiber sheet to become the front outer layer 8b is laid on the papermaking surface side of the second work-in-progress, and these are integrated by needle punching to create a third work-in-progress. Next, a staple fiber sheet to become the back layer 7 is placed on the running surface side of the third work-in-progress, and these are integrated by needle punching to create a fourth work-in-progress. Next, the fourth work-in-progress is subjected to a finishing process including chemical treatment and special processing to finish it to a set size, and cleaning and resin processing to improve performance, to complete the papermaking felt 1. The needle punching of the staple fiber sheet to become the back layer 7 may be performed before the needle punching of the nonwoven fabric composed of 100% rayon fiber, between the needle punching of the nonwoven fabric composed of 100% rayon fiber and the needle punching of the portion 8d on the papermaking surface side of the front inner layer 8a, or between the needle punching of the portion 8d on the papermaking surface side of the front inner layer 8a and the needle punching of the front outer layer 8b.

[0033] The effects of the papermaking felt 1 will be described. A nonwoven fabric made of 100% rayon fiber is a nonwoven fabric made only of rayon fiber, and has higher water absorption than a nonwoven fabric made of synthetic fiber or a rayon nonwoven fabric mixed with resin, so water is easily transferred to the nonwoven fabric layer 4. This improves the water squeezing ability of the papermaking felt 1. In addition, a nonwoven fabric made of 100% rayon fiber does not use resin, heat-sealing fiber, or adhesive, and the fibers are bonded together with a moderate bonding force. Therefore, especially when the fiber length of the nonwoven fabric is 5 to 35 mm, the nonwoven fabric structure collapses during needle punching, and a portion where the layer shape is maintained and a portion where the fibers are dispersed around the nonwoven fabric insertion position are formed. In other words, the papermaking felt 1 has a base fabric 2 and a batt layer 3 arranged at least on the paper surface side of the base fabric 2, and rayon fibers with a fiber length of 5 to 35 mm are not exposed on the surface of the papermaking felt 1 but are dispersed inside the batt layer 3 and inside the base fabric 2. By using a rayon nonwoven fabric containing such short rayon fibers, many rayon fibers penetrate into the base fabric 2 by needle punching during the manufacture of the papermaking felt 1, and moisture can be transferred to the inside of the papermaking felt 1 quickly from the start of use. In addition, since the rayon fibers have crimps, the rayon fibers are not too dispersed and are moderately entangled with each other by needle punching during the manufacture of the papermaking felt 1, so that the rayon fibers can be prevented from falling off quickly during use. In addition, by using a rayon nonwoven fabric containing such short rayon fibers, the voids in the base fabric 2, which has relatively more voids compared to the batt layer 3, can be appropriately filled, the water pressure difference between the wet paper and the base fabric 2 is reduced, and moisture transfer between the wet paper and the inside of the papermaking felt 1 becomes smoother, thereby improving water drainage. In addition, in the papermaking felt 1 in which the nonwoven fabric layer 4 of such a shape is arranged, the rayon fibers are unlikely to fall off at the beginning of use, but they gradually fall off during use, and at the end of use, they have fallen off, so that an increase in density is suppressed. As a result, a constant air permeability value is maintained, so dirt is unlikely to accumulate. Also, because the thickness of the rayon fibers is thinner than the thickness of the fibers in the batt layer 3, the dispersion of the rayon fibers in the base fabric 2 and the batt layer 3 is improved, and the stain resistance is enhanced.

[0034] The rayon fibers for the nonwoven fabric layer 4 preferably have a fiber length of 5 to 15 mm. A nonwoven fabric formed from fibers of such a length is more likely to collapse in structure by needle punching, and is less likely to increase in density even at the end of its life. Therefore, the breathability is less likely to decrease, and dirt is less likely to accumulate.

[0035] In the nonwoven fabric for nonwoven fabric layer 4, the rayon fibers are preferably arranged randomly, without being aligned in a specific direction such as the machine direction or cross machine direction. When the rayon fibers of nonwoven fabric layer 4 are arranged in this manner, the rayon fibers are more easily grasped and carried by needles to the base fabric 2 and batt layer 3 during needle punching, so that the nonwoven fabric structure is more easily broken down and the rayon fibers are more easily dispersed into the base fabric 2 and batt layer 3. Therefore, as with the above, the density is less likely to increase even at the end of use, and dirt is less likely to accumulate.

[0036] In addition, the rayon fiber for nonwoven fabric layer 4 preferably has a crimp number of 20 to 30 per inch (2.54 cm). When the crimp number of the rayon fiber for nonwoven fabric layer 4 is within this range, the fiber void structure becomes more suitable for water absorption and water retention, resulting in a faster water absorption rate and the ability to retain a large amount of water, thereby improving water drainage.

[0037] On the other hand, when the fiber length of the nonwoven fabric is longer than 35 mm, even if the fibers are bonded with an appropriate bonding force, the nonwoven fabric structure is not easily broken down by needle punching, and the fibers of the nonwoven fabric layer 4 are hardly dispersed into the base fabric 2 or batt layer 3. As a result, the fibers of the nonwoven fabric layer 4 are not easily shed until the end of use, the density increases, the breathability decreases, and dirt is easily accumulated in the nonwoven fabric layer 4. Also, when the fiber length is 5 mm or less, the fibers are dispersed throughout the papermaking felt by needle punching, and the fibers are easily shed in the early stages of use. As a result, the effect of improving water squeezing is lost in a short period of time.

[0038] By arranging the nonwoven fabric layer 4 directly above the base fabric 2 (adjacent to the paper-making surface side of the base fabric 2) rather than in the surface layer 8 close to the surface of the papermaking felt 1, it is less susceptible to damage from showers and suction boxes 36 (see Figure 4) during pressing. This makes it less likely for the nonwoven fabric fibers to fall off in the early stages of use, and the effect of improving water squeezing is maintained. In addition, by dispersing fine nonwoven fabric fibers even in the layer of the base fabric 2, which has many voids, the difference in water pressure between the batt layer 3 and the layer of the base fabric 2 can be reduced, resulting in an internal structure in which the water pressure between the wet paper, the surface layer 8, and the layer of the base fabric 2 changes gradually. This makes it easier for moisture to move smoothly from the wet paper to the inside of the papermaking felt 1, improving water squeezing.

[0039] The larger the basis weight of the nonwoven fabric for the nonwoven fabric layer 4, the better the water drainage, but the lower the air permeability. If the air permeability is low, dirt tends to accumulate, especially at the end of use. For this reason, the basis weight of the nonwoven fabric for the nonwoven fabric layer 4 is set to 15 to 100 g / m 2 , preferably 15 to 60 g / m 2 It is better to say:

[0040] The second and third embodiments of the present invention will be described with reference to Fig. 2. Fig. 2(A) is a schematic cross-sectional view of a papermaking felt 11 according to the second embodiment, and Fig. 2(B) is a schematic cross-sectional view of a papermaking felt 21 according to the third embodiment. In describing the second and third embodiments, the description of the components common to the first embodiment will be omitted and the same reference numerals will be used.

[0041] The configuration of the papermaking felt 11 according to the second embodiment differs from that of the first embodiment only in that the nonwoven fabric layer 4 is disposed between the base fabric 2 and the back layer 7, directly below the base fabric 2, i.e., adjacent to the running surface of the base fabric 2. By disposing the nonwoven fabric layer 4 directly below the base fabric 2 in this way, the nonwoven fabric layer 4 is separated from the papermaking surface compared to when it is disposed directly above, so that marks on the surface of the wet paper due to the joints of the nonwoven fabric layer 4 are less likely to occur. For this reason, the papermaking felt 11 is particularly suitable for use in a papermaking machine that manufactures paper in which surface properties are important. In other respects, the papermaking felt 11 according to the second embodiment in which the nonwoven fabric layer 4 is disposed directly below the base fabric 2 has the same effects as the first embodiment in which the nonwoven fabric layer 4 is disposed directly above the base fabric 2 (see FIG. 1).

[0042] A method for manufacturing the papermaking felt 11 will be described. An operator manufactures the papermaking felt 11 according to the following procedure. First, the base fabric 2 is woven. Next, a nonwoven fabric made of 100% rayon fiber to become the nonwoven fabric layer 4 is laid on the running surface side of the base fabric 2, and a staple fiber sheet to become the portion 7a of the back layer 7 on the base fabric 2 side is laid on the running surface side of the nonwoven fabric, and a first work-in-progress is created by integrating these by needle punching. Next, a staple fiber sheet to become the portion 7b of the back layer 7 on the running surface side is laid on the running surface side of the first work-in-progress, and a second work-in-progress is created by integrating these by needle punching. Next, a staple fiber sheet to become the front inner layer 8a is laid on the papermaking surface side of the second work-in-progress, and a third work-in-progress is created by integrating these by needle punching. Next, a staple fiber sheet to become the outer surface layer 8b is placed on the papermaking surface side of the third work-in-progress, and these are integrated by needle punching to create a fourth work-in-progress. Next, the fourth work-in-progress is subjected to the above-mentioned finishing process to complete the papermaking felt 11. Note that the needle punching of the staple fiber sheet to become the inner surface layer 8a may be performed before the needle punching of the nonwoven fabric composed of 100% rayon fiber.

[0043] The papermaking felt 21 according to the third embodiment differs from the first embodiment only in that the nonwoven fabric layer 4 is disposed between the inner surface layer 8a and the outer surface layer 8b. In the papermaking felt 21 according to the third embodiment, the nonwoven fabric layer 4 is farther away from the base fabric 2 than in the first and second embodiments, making it difficult for the nonwoven fabric fibers to disperse within the layer of the base fabric 2. For this reason, the third embodiment is considered to have a lower effect than the first embodiment, due to the nonwoven fabric fibers dispersing within the layer of the base fabric 2, but has the same effects as the first embodiment in other respects.

[0044] A method for manufacturing the papermaking felt 21 will be described. An operator manufactures the papermaking felt 21 according to the following procedure. First, the base fabric 2 is woven. Next, a staple fiber sheet to be the outer inner layer 8a is laid on the papermaking surface side of the base fabric 2, and the first work-in-progress is created by integrating them by needle punching. Next, a nonwoven fabric made of 100% rayon fiber to be the nonwoven fabric layer 4 is laid on the papermaking surface side of the first work-in-progress, and a staple fiber sheet to be the portion 8e of the outer outer layer 8b on the base fabric 2 side is laid on the papermaking surface side of the nonwoven fabric, and the second work-in-progress is created by integrating them by needle punching. Next, a staple fiber sheet to be the portion 8f of the outer outer layer 8b on the papermaking surface side is laid on the papermaking surface side of the second work-in-progress, and the third work-in-progress is created by integrating them by needle punching. Next, a staple fiber sheet to become the back layer 7 is placed on the running surface side of the third work-in-progress, and these are integrated by needle punching to create a fourth work-in-progress. Next, the fourth work-in-progress is subjected to the above-mentioned finishing process to complete the papermaking felt 21. Note that the needle punching of the staple fiber sheet to become the back layer 7 may be performed before the needle punching of the front inner layer 8a, between the needle punching of the front inner layer 8a and the needle punching of the nonwoven fabric composed of 100% rayon fiber, or between the needle punching of the nonwoven fabric composed of 100% rayon fiber and the needle punching of the papermaking surface side portion 8f of the front outer layer 8b. EXAMPLES

[0045] A water squeezing test was carried out on the felt samples having the configurations shown in Table 1 and FIG. 3, and a water absorbency evaluation test was carried out on the nonwoven fabric of the nonwoven fabric layers 4, 4' used in each felt sample.

[0046] [Table 1]

[0047] <Water absorbency evaluation test> The water absorbency evaluation test was conducted based on the water absorbency evaluation test (Byreck method) listed in JIS L 1907. Ten rectangular test pieces measuring 25 mm x 200 mm (five each with the machine direction as the longitudinal direction and the cross machine direction as the longitudinal direction) were taken from the nonwoven fabric sample, the ends of the test pieces were immersed in water, and the height (mm) of the water that rose above the water surface due to capillary action was measured after 10 minutes.

[0048] <Water squeezing test> The workers carried out the water squeezing test by carrying out the following tasks.

[0049] <Felt sample production> The base fabric 2 had two layers. The upper base fabric layer arranged on the paper-making side was woven in a single weave using twisted yarns of 6 nylon monofilament with a diameter of 0.2 mm as the warp yarn 5 and single yarns of 6 nylon monofilament with a diameter of 0.25 mm as the weft yarn 6, and had a weight of 275 g / m 2 The lower base fabric layer arranged on the running side was woven in a double weave using 0.4 mm diameter 6 nylon monofilament single yarn as the warp yarn 5 and 0.4 mm diameter 6·10 nylon monofilament single yarn as the weft yarn 6, and had a weight of 581 g / m 2 The upper fabric layer was overlaid on the lower fabric layer to form the fabric 2 layer.

[0050] To form the back layer 7, a fabric having an average fineness of 39 dtex and a basis weight of 150 g / m is placed under the base fabric 2 (on the running surface side). 2To form the inner surface layer 8a, a 66 nylon staple fiber sheet having an average fineness of 39 dtex and a basis weight of 450 g / m was placed on the top (paper-making surface) of the base fabric 2. 2 To form the outer surface layer 8b, a 66 nylon staple fiber sheet having an average fineness of 22 dtex and a basis weight of 200 g / m was placed on the staple fiber sheet for the inner surface layer 8a. 2 In addition, nonwoven fabrics for forming nonwoven fabric layers 4, 4' (the nonwoven fabric layer of the comparative example is designated by the reference symbol "4'") were inserted at the positions shown in Table 1 and FIG. 3. 2 The nonwoven fabric has a basis weight of 50g / m 2 When forming the nonwoven fabric layer 4, multiple sheets of nonwoven fabric were arranged in layers. The laminate of the base fabric 2, staple fiber sheet and nonwoven fabric was needle punched to form the batt layer 3 and the nonwoven fabric layers 4, 4', and the base fabric 2, batt layer 3 and the nonwoven fabric layers 4, 4' were entangled and integrated. The needle punch density was 606 times / cm 2 Further pressing was carried out to produce felt samples.

[0051] As shown in Fig. 3, in Examples 1 to 4 and 9 and Comparative Examples 1 to 4, a nonwoven fabric was placed between the base fabric 2 and the front inner layer 8a as in the first embodiment, and the nonwoven fabric was needle-punched from the front (paper-making side) simultaneously with the staple fiber sheet forming the front inner layer 8a. In Examples 5 and 6, a nonwoven fabric was placed between the base fabric 2 and the back layer 7 as in the second embodiment, and the nonwoven fabric was needle-punched from the back (running side) simultaneously with the staple fiber sheet forming the back layer 7. In Examples 7 and 8, a nonwoven fabric was placed between the front inner layer 8a and the front outer layer 8b as in the third embodiment, and the nonwoven fabric was needle-punched from the front (paper-making side) simultaneously with the staple fiber sheet forming the front outer layer 8b.

[0052] <Water squeezing test> Advance preparation Figure 4 shows a schematic diagram of the testing machine. (1) Each felt sample was cut into a size of 42 x 20 cm, sewn into an endless belt to form a felt specimen F, and attached to a press roll tester 31. The press roll tester 31 is equipped with a roll 32 that supports the felt specimen F, a top roll 33 and a bottom roll 34 that cooperate with each other to compress the wet paper (filter paper S containing moisture) placed on the felt specimen F, a shower device 35 that sprays water on the part of the felt specimen F from which the filter paper S has been removed after passing through the top roll 33 and the bottom roll 34, and a suction box 36 that sucks moisture from the part of the felt specimen F that has passed through the shower device 35. This press roll tester 31 is structured to press (compress) the felt specimen F and the filter paper S with the top roll 33 and the bottom roll 34 once per revolution during the test. The felt runs in such a way that the surface of the felt is bent both outward and inward by each of the attached rolls 32.

[0053] (2) In order to minimize changes in thickness of felt specimen F during the water squeezing test, the running speed was set to 250 m / min and the press line pressure to 60 kN / m, and felt specimen F was run while being showered from the surface side until the number of presses reached 9,000.

[0054] ·Filter paper S Filter paper S (Whatman No.3 φ150mm (grammage approx. 185g / m 2 )) was soaked in water for 24 hours or more, and then the moisture content was adjusted to 65% before pressing, and used as a substitute for wet paper.

[0055] Testing Procedure (1) A felt specimen F attached to a press roll testing machine 31 was run at a running speed of 40 m / min, a press line pressure of 50 kN / m by the top roll 33 and the bottom roll 34, and a shower flow rate of 4 L / min from the shower device 35 while moisture was sucked from the surface side by a suction box 36.

[0056] (2) The filter paper S, whose moisture content had been adjusted to 65%, was placed on top of the felt test specimen F (at the press entrance) during continuous operation together with an aluminum plate, and passed through the press made by the top roll 33 and the bottom roll 34. After passing through, the filter paper S was removed from the felt test specimen F, and the weight of the filter paper S before and after pressing was recorded.

[0057] (3) The filter paper S was pre-dried in a dryer (at 60°C for about 1 hour), and the bone dry weight was measured using an infrared moisture meter (thermobalance) to determine the moisture content of the filter paper S before and after pressing. For each of Examples 1 to 9 and Comparative Examples 1 to 4, a test was performed with 10 sheets of filter paper S on one felt specimen F, and the average value was calculated.

[0058] Air permeability measurement The air permeability was measured at five points for each felt specimen F, and the average value was calculated.

[0059] The results of the water absorbency evaluation test are shown in Table 2 and FIG. 5. As shown in Table 2 and FIG. 5, the 100% rayon nonwoven fabric had higher water absorbency than nonwoven fabrics made of other materials, regardless of whether the fiber length was 10 mm or 30 mm. In the rayon nonwoven fabric of Example 9, the water absorption rate in the machine direction was obviously higher than that in the cross-machine direction. On the other hand, in the rayon nonwoven fabrics used in Examples 1 to 8, the water absorption rates in the machine direction and the cross-machine direction were approximately the same. The reason for this difference is thought to be that, as shown in the "fiber orientation" column in Table 1, the fibers in the rayon nonwoven fabrics used in Examples 1 to 8 were randomly oriented, whereas the fibers in the rayon nonwoven fabric of Example 9 were basically oriented only in the warp direction. [Table 2]

[0060] Table 3 and FIG. 6 show the results of the water squeezing evaluation test. As shown in Table 3 and FIG. 6(A), the filter paper S transported by the felt specimen F (Examples 1 and 9) having a nonwoven fabric layer 4 of 100% rayon had a larger moisture difference before and after pressing and a higher water squeezing ability than the felt specimen F (Comparative Examples 1 to 4) having the other nonwoven fabric layer 4' and the felt specimen F (Comparative Example 5) not having the nonwoven fabric layers 4, 4'. As shown in Table 3 and FIG. 6(B), the felt specimen F (Examples 1 to 4) in which the nonwoven fabric layer 4 is arranged directly above the base fabric 2 and the felt specimen F (Examples 7 and 8) in which the nonwoven fabric layer 4 is arranged between the surface inner layer 8a and the surface outer layer 8b had a larger moisture difference before and after pressing and a higher water squeezing ability than the felt specimen F (Examples 5 and 6) in which the nonwoven fabric layer 4 is arranged directly below the base fabric 2. In addition, as the basis weight increases, the moisture difference before and after pressing becomes larger and the water squeezing ability becomes higher. [Table 3]

[0061] Table 4 shows the results of the air permeability measurement of felt specimen F. The unit of air permeability is cm 3 / cm 2 As shown in Table 4, the air permeability decreased as the basis weight increased, provided that the type and position of the nonwoven fabric was the same. Judging from the results of Examples 1 to 4, when the nonwoven fabric layer 4 was disposed directly on the base fabric 2 and was formed from a nonwoven fabric having a fiber length of 10 mm and made of 100% rayon, the air permeability decreased as the basis weight increased. 2 If so, about 20 cm 3 / cm 2 It was estimated that the air permeability of 75 g / m2 / s could be obtained. 2 Example 3 and 100 g / m 2 In Example 4, the air permeability of the felt specimen F is 20 cm 3 / cm 2 / s, dirt easily accumulates, especially towards the end of use. Therefore, the basis weight of the nonwoven fabric is 60 g / m 2 The following is preferred: [Table 4]

[0062] 7(A) and (B) are electron microscope photographs of the weft cross sections of Examples 1 and 9, and Figs. 7(C) and (D) are enlarged photographs of Figs. 7(A) and (B). From Figs. 7(A) to (D), it can be seen that in Examples 1 and 9, the fibers of the 100% rayon nonwoven fabric are also dispersed in the gaps of the base fabric 2. Also, from Figs. 7(C) and (D), it can be seen that the crimp of the rayon fibers is large in Example 1, and that the crimp of the rayon fibers is small in Example 9, in which the nonwoven fabric was produced by a manufacturing method different from that of Example 1. Note that the nonwoven fabrics of Examples 2 to 8 were produced by the same manufacturing method as Example 1, so it can be said that the rayon fibers of Examples 2 to 8 also have a large crimp similar to that of Example 1.

[0063] Although the specific embodiment has been described above, the present invention is not limited to the above embodiment and its modified examples, and can be modified in a wide range of ways. [Explanation of symbols]

[0064] 1, 11, 21: Papermaking felt 2: Base fabric 3: Batt layer 4: Non-woven layer 5: Warp threads 6: Weft 7: Lining 8: Surface layer 8a: Surface and inner layer 8b: Outer layer

Claims

1. A base fabric; a batt layer including a back layer disposed on the running surface side of the base fabric and a front layer disposed on the papermaking surface side of the base fabric; a nonwoven fabric layer formed by needle punching a nonwoven fabric made of 100% rayon fiber, the nonwoven fabric layer being disposed between the base fabric and the back layer or the front layer, or within the batt layer; the batt layer and the nonwoven fabric layer are integrated with the base fabric by the needle punching so that the rayon fibers are dispersed inside the batt layer and inside the base fabric; The rayon fibers have a fiber length of 5 to 35 mm.

2. The papermaking felt of claim 1 , wherein the nonwoven layer is adjacent to the backing.

3. 2. The papermaking felt of claim 1, wherein the rayon fibers are crimped and randomly oriented in the nonwoven fabric.

4. The nonwoven fabric has a density of 15 to 60 g / m 2 2. The papermaking felt according to claim 1, having a basis weight of

5. 2. The papermaking felt according to claim 1, wherein the rayon fibers have a fiber length of 5 to 15 mm.

6. 2. The papermaking felt of claim 1, wherein said rayon fibers are finer than the staple fibers that make up said batt layer.

7. The method includes a step of stacking a nonwoven fabric made of 100% rayon fiber and a staple fiber sheet to be at least a part of the batt layer on a base fabric, and needle punching the stacked product to integrate them; The method for producing papermaking felt, wherein the rayon fibers have a fiber length of 5 to 35 mm.

Citation Information

Patent Citations

  • Press felt for papermaking and press unit for paper machine

    JP2004143627A

  • Improved paper web dewatering in the press section of papermaking machines and press felts therefor