Resin composition

The resin composition with specific (meth)acrylic copolymers A and B addresses handling and storage issues of acrylic polymer particles by reducing water absorption and blocking, ensuring stable and efficient molding processes.

JP2024139722APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2024036672
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-11
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing acrylic polymer particles suffer from blocking issues during handling, leading to flow problems and poor mobility, and have inadequate storage stability due to high hygroscopicity and prolonged drying times during molding.

Method used

A resin composition is developed with (meth)acrylic copolymers A and B, where copolymer A has a water absorption rate of 3% or less and a molecular weight between 500,000 and 2,500,000, and copolymer B has a glass transition temperature of 60°C or higher, coated on copolymer A, enhancing storage stability and handling.

Benefits of technology

The resin composition improves storage stability and handling of acrylic polymer particles by preventing water absorption and blocking, allowing for efficient drying and processing without deterioration in mechanical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139722000011
    Figure 2024139722000011
  • Figure 2024139722000001
    Figure 2024139722000001
  • Figure 2024139722000002
    Figure 2024139722000002
Patent Text Reader

Abstract

To provide a resin composition which is excellent in storage stability, and handleability in molding.SOLUTION: There provided a resin composition in which the surface of a (meth)acrylic copolymer A having a water absorption of 5% or more is coated with a (meth)acrylic copolymer B having a water absorption of 3% or less and a weight average molecular weight of 500,000 or more and 2,500,000 or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fat composition having excellent storage stability and moldability. [Background technology]

[0002] When acrylic polymer particles aggregate due to blocking, the flow during handling becomes difficult. The mobility was poor, and it took a long time to dissolve in a solvent, so improvements were needed in terms of handling. For example, Patent Document 1 discloses a method for coating a surface with an acrylic polymer having a specific solubility parameter. Acrylic polymer particles having improved blocking resistance are described. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2019-6896 A Summary of the Invention [Problem to be solved by the invention]

[0004] However, the method described in Patent Document 1 does not provide a storage method for acrylic polymer particles that are highly hygroscopic. The storage stability, drying during molding, and handling properties were not sufficiently improved. The purpose is to solve problems. [Means for solving the problem]

[0005] The present invention has the following aspects. <1> The surface of (meth)acrylic copolymer A, which has a water absorption rate of 5% or more, has a water absorption rate of 3% or less. (Meth)acrylic copolymer having a weight average molecular weight of 500,000 or more and 2,500,000 or less. A resin composition coated with body B. <2> (Meth)acrylic copolymer B is added to 100 parts by mass of the resin composition. , containing 0.01 parts by mass or more and 5 parts by mass or less, <1> The resin composition according to claim 1.

[0006] <3> <1> The particle size of the (meth)acrylic copolymer B is 1 nm or more and 20 μm or less; or <2> The resin composition according to claim 1. <4> The (meth)acrylic copolymer B has a glass transition temperature (Tg) of 60° C. or higher. R <1> ~ <3> 10. The resin composition according to claim 9,

[0007] <5> The (meth)acrylic copolymer A is a (meth)acrylic copolymer A1 and A copolymer including a (meth)acrylic copolymer A2 different from the (meth)acrylic copolymer A1. It is a lock copolymer or a graft copolymer. <1> ~ <4> A resin composition according to any one of thing.

[0008] <6> The (meth)acrylic copolymer A1 contains a monomer unit a represented by the following formula (1): Claims including 1 <5> The resin composition according to claim 1.

[0009] [ka]

[0010] (In the formula, R 3 represents a hydrogen atom or a methyl group, and R 4 represents an alkylene group having 1 to 4 carbon atoms. S, R 5 represents a hydrocarbon group having 1 to 6 carbon atoms, and p is a natural number from 1 to 10. <7> In the case where the total amount of the monomer units contained in the (meth)acrylic copolymer A1 is 100% by mass, The proportion of the monomer unit a1 in the copolymer is 70 mass% or more. <5> or <6> Resin according to composition.

[0011] <8> The monomer unit a1 is methoxymethyl acrylate, methoxyethyl acrylate, acrylate, methoxypropyl acrylate, methoxybutyl acrylate, methoxypolyethylene Polyethylene glycol acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate Methoxypropyl methacrylate, Methoxybutyl methacrylate, Methoxypoly At least one monomer selected from the group consisting of triethylene glycol methacrylate is a monomeric unit derived from the body, <5> ~ <7> 10. The resin composition according to claim 9,

[0012] <9> The (meth)acrylic copolymer A2 has a glass transition point (Tg) of 50 to 150° C. That is, <5> ~ <8> 10. The resin composition according to claim 9, <10> The polymer A2 is composed of a monomer unit a2, and the monomer unit a2 is a hydrocarbon group. A hydrocarbon group-containing (meth)acrylate having 1 to 12 carbon atoms is selected from the group consisting of are monomer units derived from at least one monomer <5> ~ <9> Recorded in one of the The resin composition described above.

[0013] <11> The polymer A2 is composed of a monomer unit a2, and the monomer unit a2 is a methyl methacrylate. Contains monomer units derived from acrylate, <5> ~ <10> A resin composition according to any one of thing. <12> The polymer A2 is a unit derived from a macromonomer d′ represented by the following formula (2): Including, <5> ~ <11> 10. The resin composition according to claim 9,

[0014] [ka]

[0015] (In formula (2), R 0 ~Rn each independently represents a hydrogen atom, an unsubstituted or substituted an alkyl group having an unsubstituted or substituted alicyclic group; an alicyclic group having an unsubstituted or substituted aryl groups having a substituent, unsubstituted or substituted heteroaryl groups, or unsubstituted or or a non-aromatic heterocyclic group having a substituent, 0 ~R n are the same may be different, and X 1 ~X n represents a hydrogen atom or a methyl group, and multiple X 1 ~X n Haso may be the same or different, Z is a terminal group, and n is a natural number from 2 to 10,000. .)

[0016] <13> <1> ~ <12> A molding material comprising the resin composition according to any one of the above. <14> <13> An article molded from the molding material described above. Effect of the Invention

[0017] The resin composition of the present invention improves the storage stability of acrylic polymer particles and ease of handling during molding. Sexuality improves. [Brief description of the drawings]

[0018] [Figure 1] FIG. 1 is a diagram showing an apparatus for preparing a sample for evaluating blocking resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The resin composition of the present invention is characterized in that the surface of a (meth)acrylic copolymer A having a water absorption rate of 5% or more is (Meth) with water absorption rate of 3% or less and weight average molecular weight of 500,000 or more and 2,500,000 or less It is coated with acrylic copolymer B. The water absorption rate of the (meth)acrylic copolymer A is preferably 5.5% or more, more preferably 6% or more. More preferably, the content is 6.5% or more, and particularly preferably 6.5% or more.

[0020] The (meth)acrylic copolymer B has a water absorption rate of 3% or less. In this case, the resin composition can be prevented from absorbing water, and therefore the drying step can be omitted during molding. Since the blocking resistance is excellent, the storage stability is also improved. The water absorption rate of the (meth)acrylic copolymer B is more preferably 2.5% or less, and more preferably 2.0% or less. It is more preferably 1.5% or less, even more preferably 1% or less, and particularly preferably 1% or less.

[0021] In the present invention, the water absorption rate is determined according to JIS K 7209:2000 Plastics-Water Absorption Rate This value is obtained using a measurement method that conforms to the method for determining the above. The weight average molecular weight of the (meth)acrylic copolymer B is 500,000 or more, The mechanical properties of the resin composition are not deteriorated. The molecular weight is preferably 500,000 or more, more preferably 600,000 or more, and more preferably 70,000 or more. It is more preferably 0 or more, and particularly preferably 80,000 or more.

[0022] The (meth)acrylic copolymer (A) has a weight average molecular weight of 2,500,000 or less. If the (meth)acrylic copolymer is used, the processability during molding of the resin composition is not deteriorated. The weight average molecular weight of the polymer (A) is preferably 2,500,000 or less, more preferably 2,250,000 or less. More preferably, it is 2,000,000 or less, even more preferably, it is 1,500,000 or less. stomach. The weight average molecular weight of the copolymer was determined by gel permeation chromatography (GPC). It is calculated as a relative molecular weight using ethyl methacrylate as the standard resin.

[0023] <(Meth)acrylic copolymer A> The (meth)acrylic copolymer A of the present invention comprises (meth)acrylic copolymer A1 and the above The (meth)acrylic copolymer A1 and the (meth)acrylic copolymer A2 different from each other are included in the block copolymer. It is preferred that the copolymer is a block copolymer or a graft copolymer. The block and / or graft structure may be diblock, triblock, multiblock, graft, The structure may be any of raft, ring, star, comb, tree, ladder, etc. Among these structures, the structure that is relatively easy to manufacture is Therefore, it is possible to obtain at least one of the following structures: diblock, triblock, and graft. It is also preferred to include

[0024] The content of the (meth)acrylic copolymer A is 100% by mass of the resin composition of the present invention. %, 99.99% by mass or less is preferable, 99.9% by mass or less is more preferable, The amount is preferably 99.5% by mass or less, and more preferably 99% by mass or less. The content of acrylic copolymer A is 99. When the content is 99% by mass or less, the decrease in blocking properties of the resin composition of the present invention can be further suppressed.

[0025] The content of the (meth)acrylic copolymer A in the resin composition of the present invention is The content is preferably 95% by mass or more, more preferably 96% by mass or more, based on 100% by mass of the total resin composition of the invention. More preferably, the content is 97% by mass or more, even more preferably, 98% by mass or more. It is nice. The (meth)acrylic copolymer A1 contains a monomer unit a1 represented by the following formula (1): It is preferable to do so.

[0026] [ka]

[0027] In formula (1), R 3 represents a hydrogen atom or a methyl group, R 4 is an alkyl group having 1 to 4 carbon atoms. represents a phenyl group, and R 5 represents a hydrocarbon group having 1 to 6 carbon atoms, and p is a natural number of 1 to 10. The monomer unit a1 is a monomer unit derived from the monomer a'1. As the monomer a'1, methoxymethyl acrylate, methoxyethyl acrylate , Methoxypropyl acrylate, Methoxybutyl acrylate, Ethoxymethyl acrylate Acrylate, Ethoxyethyl Acrylate, Ethoxypropyl Acrylate, Ethoxybutyl Acrylate, Propoxymethyl Acrylate, Propoxyethyl Acrylate, Propoxy Propoxypropyl acrylate, Propoxybutyl acrylate, Butoxymethyl acrylate Butoxyethyl acrylate, butoxypropyl acrylate, butoxybutyl acrylate Methacrylate, Methoxymethyl Methacrylate, Methoxyethyl Methacrylate, Methoxypropane propyl methacrylate, methoxybutyl methacrylate, ethoxymethyl methacrylate , ethoxyethyl methacrylate, ethoxypropyl methacrylate, ethoxybutyl methacrylate acrylate, propoxymethyl methacrylate, propoxyethyl methacrylate, Propoxypropyl methacrylate, Propoxybutyl methacrylate, Butoxymethyl methacrylate Butoxyethyl methacrylate, butoxypropyl methacrylate, butoxyethyl methacrylate Methoxybutyl methacrylate, "Blenmer PME-100" (Methoxypoly Ethylene glycol methacrylate (2 ethylene glycol chains), product "Blenmar PME-200" (Methoxy polyethylene glycol manufactured by NOF Corp.) methacrylate (ethylene glycol chains with 4 units), product name) and the like. do.

[0028] As the monomer a'1, from the viewpoint of suppressing protein adhesion, methoxymethyl acrylate is preferably used. , methoxyethyl acrylate, methoxypropyl acrylate, methoxybutyl acrylate acrylate, methoxypolyethylene glycol acrylate, methoxymethyl methacrylate Methoxyethyl methacrylate, Methoxypropyl methacrylate, Methoxybutyl methacrylate, and methoxypolyethylene glycol methacrylate. At least one selected from the group consisting of methoxyethyl acrylate and methoxypropyl acrylate is preferred. acrylate, methoxypolyethylene glycol acrylate, and methoxypolyethylene More preferably, at least one selected from the group consisting of glycol methacrylates. methoxyethyl acrylate and methoxyethyl methacrylate At least one type is more preferred.

[0029] The monomer a'1 can be used alone or in combination of two or more kinds. The polymer A1 may contain a monomer unit other than the monomer unit a1. The constituent units other than the monomer unit a1 are monomers derived from monomers other than the monomer a'1. It is measured by body. The monomer other than the monomer a'1 may be any monomer as long as it has copolymerizability with the monomer a'1. There are no particular limitations and any known monomer can be selected.

[0030] Examples of the monomer other than the monomer a'1 include various radical polymerizable monomers. It can be done. The proportion of the monomer unit a1 in the polymer A1 is not particularly limited. It is preferably 40% by mass or more relative to 100% by mass of the total of the structural units of the entity A1. More preferably, the content is 70% by mass or more, even more preferably, 90% by mass or more, and particularly preferably, 99% by mass or more. It is particularly preferred that the content be 100% by mass.

[0031] The polymer A1 may further include a monomer unit a4 as a monomer unit. The monomer unit a1 is a monomer unit derived from the monomer a'4. Any known monomer may be selected without particular limitation as long as it is copolymerizable with the compound a'1. Examples of the monomer a'4 include various radical polymerizable monomers. Cut.

[0032] The (meth)acrylic copolymer A2 may be a (meth)acrylic resin such as PMMA; Vinyl halide resins such as polyvinyl chloride, polyolefins, polystyrene, polyamides , polyurethane, polysulfone, polyethersulfone, unsaturated polyester, polyethylene Saturated polyesters such as poly(ethylene terephthalate) and poly(butylene terephthalate), poly(vinyl ether) Ether, polycarbonate, silicone resin, epoxy resin, polyether ether ketone Examples of the polymer A2 include a thermoplastic resin. I wish. The polymer A2 contains, as a monomer unit, a monomer unit a2 represented by the following formula (3): It is preferred.

[0033] [ka]

[0034] In the formula (3), R 1 represents a hydrogen atom or a methyl group, R 2 OR 33 , Halo Gen atom, COR 34 , COOR 35 , C.N., C.O.N. 36 R 37 or R 38 and R 33 ~R 37 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or or an unsubstituted alicyclic group, a substituted or unsubstituted aryl group, a substituted or unsubstituted heterocyclic group, Aryl groups, substituted or unsubstituted non-aromatic heterocyclic groups, substituted or unsubstituted aralkyl groups, an alkyl group, a substituted or unsubstituted alkaryl group, or a substituted or unsubstituted organosilyl group; R represents a cyclic group; 38 is a substituted or unsubstituted aryl group, or a substituted or unsubstituted heterocyclic group. represents an aryl group, and n is a natural number of 2 to 10,000.

[0035] The monomer unit a2 is preferably a structural unit derived from a (meth)acrylic acid ester. Yes. R 1 is preferably a hydrogen atom or a methyl group, and R 2 As COOR 35 is preferred . R 33 ~R 37 The unsubstituted alkyl group may be, for example, a branched or unsubstituted alkyl group having 1 to 22 carbon atoms. Specific examples of the branched or linear alkyl group having 1 to 22 carbon atoms include: The following groups are available: methyl, ethyl, n-propyl, isopropyl, n-butyl, te rt-Butyl group, i-Butyl group, Pentyl group (Amyl group), i-Pentyl group, Hexyl group , heptyl group, 2-ethylhexyl group, octyl group, i-octyl group, nonyl group, i-nonyl group nyl group, decyl group, i-decyl group, undecyl group, dodecyl group (lauryl group), tridecyl group decyl, tetradecyl, pentadecyl, hexadecyl, heptadecyl, octadecyl aryl group (stearyl group), i-octadecyl group, nonadecyl group, icosyl group and docosyl group etc.

[0036] R 33 ~R 37 Examples of the unsubstituted aryl group include aryl groups having 6 to 18 carbon atoms. Specific examples of the aryl group having 6 to 18 carbon atoms include a phenyl group and a naphthyl group. Examples of such groups include R 33 ~R 37 Examples of the unsubstituted heteroaryl group include heteroaryl groups having 4 to 18 carbon atoms. Specific examples of the heteroaryl group having 4 to 18 carbon atoms include pyridyl groups. Examples thereof include a dialkyl group and a carbazolyl group.

[0037] R 33 ~R 37 Examples of the unsubstituted non-aromatic heterocyclic group include a heterocyclic group having 4 to 18 carbon atoms. Specific examples of the heterocyclic group having 4 to 18 carbon atoms include tetrahydrofuran and tetrahydrofuran. Furyl group, tetrahydropyranyl group and other oxygen-containing heterocyclic groups, γ-butyrolactone group Nitrogen-containing groups such as ε-caprolactone, pyrrolidinyl, pyrrolidone, and morpholino groups A heterocyclic group and the like are included.

[0038] R 33 ~R 37 Examples of the unsubstituted aralkyl group include a benzyl group, a phenylethyl group, and the like. groups, etc. R 33 ~R 37 Examples of the unsubstituted organosilyl group include -SiR 17 R 18 R 1 9 (where R 17 ~R 19 each independently represents a substituted or unsubstituted alkyl group, a substituted or an unsubstituted alicyclic group, or a substituted or unsubstituted aryl group. do.

[0039] The RR 17 ~R 19 The substituted or unsubstituted alkyl group in Examples of such groups include a methyl group, an ethyl group, an n-propyl group, an n-butyl ... Mil group, n-hexyl group, n-octyl group, n-dodecyl group, stearyl group, lauryl group , isopropyl group, isobutyl group, s-butyl group, 2-methylisopropyl group, benzyl groups, etc.

[0040] R 17 ~R 19 The substituted or unsubstituted alicyclic group in the formula (I) is the same as that described above. Examples include a cyclohexyl group. R 17 ~R 19 The substituted or unsubstituted aryl group in is the same as that described above. Examples include a phenyl group and a p-methylphenyl group. R 17 ~R 19 may be the same or different.

[0041] R 33 ~R 37 The substituent of is, for example, an alkyl group (where R 33 ~R 37 but (except for alkyl groups having a substituent), aryl groups, -COOR 11 , cyano group , -OR 12 , -NR 13 R 14 , -CONR 15 R 16 , halogen atoms, allyl groups, aryl groups At least one selected from the group consisting of an epoxy group, a siloxy group, and a group exhibiting hydrophilicity or ionicity. At least one species can be named.

[0042] Here, R 11 ~R 16 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl A group, a substituted or unsubstituted alicyclic group, or a substituted or unsubstituted aryl group. The alkyl group and the aryl group in the substituent are the unsubstituted ... The same as unsubstituted aryl groups are exemplified. -COOR in the above substituents 11 R 11 The alkyl group is preferably a hydrogen atom or an unsubstituted alkyl group. The group -COOR is preferred. 11 is a carboxy group or an alkoxycarbonyl group The alkoxycarbonyl group is preferably, for example, a methoxycarbonyl group. can be.

[0043] -OR in the above substituents 12 R 12 The alkyl group is preferably a hydrogen atom or an unsubstituted alkyl group. Preferred. That is, -OR 12 is preferably a hydroxy group or an alkoxy group. Examples of the alkoxy group include alkoxy groups having 1 to 12 carbon atoms. Specific examples include: An example is a methoxy group. In the above substituents, -NR 13 R 14 Examples of the aryl group include an amino group and a monomethylamino group. , dimethylamino group, etc.

[0044] -CONR in the above substituents 15 R 16 Examples of the aryl group include a carbamoyl group (-CO NH2), N-methylcarbamoyl group (-CONHCH3), N,N-dimethylcarbamoyl group Examples include the aryl group (dimethylamide group: -CON(CH3)2). Examples of the halogen atom in the substituent include a fluorine atom, a chlorine atom, and a bromine atom. and an iodine atom. Examples of the hydrophilic or ionic group in the substituent include For example, an alkali salt of a carboxy group or an alkali salt of a sulfo group, polyethyleneoxy poly(alkylene oxide) groups such as tetrafluoroethylene groups, poly(alkylene oxide) groups such as polypropylene oxide groups, and quaternary ammonium Examples of the substituent include cationic substituents such as aryl groups.

[0045] The monomer unit a2 is a monomer unit derived from the monomer a'2. Examples of the monomer include the following: Methyl (meth)acrylate, Ethyl (meth)acrylate, n-Propylene (meth)acrylate (meth)acrylate, isopropyl, n-butyl, (meth)acrylate Isobutyl (meth)acrylate, tert-butyl (meth)acrylate, isoamyl (meth)acrylate (Meth)acrylic acid hexyl, (meth)acrylic acid 2-ethylhexyl, (meth)acrylic acid 2-ethylhexyl Octyl acrylate, isooctyl (meth)acrylate, nonyl (meth)acrylate, p) Isononyl acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate , (meth)acrylate lauryl, (meth)acrylate hexadecyl, (meth)acrylic acid Stearyl, (meth)acrylate isostearyl, (meth)acrylate phenyl, (meth)acrylate ) Benzyl acrylate, (meth)acrylate cyclohexyl, (meth)acrylate tetra Hydrofurfuryl, (meth)acrylic acid isobornyl, (meth)acrylic acid 3,5,5- Trimethylcyclohexyl, (meth)acrylate, dicyclopentanyl, (meth)acrylic acid dicyclopentenyl acrylate, dicyclopentenyloxyethyl (meth)acrylate, terpene Acrylates and their derivatives, hydrogenated rosin acrylates and their derivatives, and (meth) Hydrocarbon group-containing (meth)acrylic acid esters such as docosyl acrylate.

[0046] 2-Hydroxyethyl (meth)acrylate, 2-Hydroxypropyl (meth)acrylate (Meth)acrylate, 2-Hydroxybutyl, (Meth)acrylate, 3-Hydroxybutyl , 4-hydroxybutyl (meth)acrylate, and glycerol (meth)acrylate Hydroxyl group-containing (meth)acrylic acid esters such as those mentioned above. Crotonic acid, fumaric acid, maleic acid, itaconic acid, citraconic acid, monomethyl maleate Monoethyl maleate, Monooctyl maleate, Monomethyl itaconate, Itaconate monoethyl, itaconate monobutyl, itaconate monooctyl, fumarate monomethyl, Monoethyl fumarate, monobutyl fumarate, monooctyl fumarate, and monocitraconate Carboxyl group-containing vinyl monomers such as polyethyl.

[0047] Vinyl monomers containing an acid anhydride group, such as maleic anhydride and itaconic anhydride. Dimethyl maleate, dibutyl maleate, dimethyl fumarate, dibutyl fumarate, di Unsaturated dicarboxilates such as butyl itaconate and diperfluorocyclohexyl fumarate Phosphate diester monomer. Glycidyl (meth)acrylate, α-ethyl glycidyl acrylate. and epoxy group-containing vinyl monomers such as 3,4-epoxybutyl (meth)acrylate Dimethylaminoethyl (meth)acrylate, Diethylaminoethyl (meth)acrylate Vinyl monomers of amino group-containing (meth)acrylic acid esters such as acrylates.

[0048] (Meth)acrylamide, dimethyl (meth)acrylamide, diethyl (meth)acrylamide N-tert-butyl(meth)acrylamide, N-methylol(meth)acrylamide acrylamide, N-isopropylacrylamide, hydroxyethylacrylamide, N- Methoxymethyl (meth)acrylamide, N-butoxymethyl (meth)acrylamide, Amide groups-containing diacetone acrylamide, maleic acid amide, and maleimide A vinyl monomer.

[0049] Styrene, α-methylstyrene, vinyltoluene, (meth)acrylonitrile, vinyl chloride Vinyl monomers such as vinyl, vinyl acetate, and vinyl propionate. Divinylbenzene, ethylene 1,3-Butylene glycol di(meth)acrylate acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate meth)acrylate, diethylene glycol di(meth)acrylate, triethylene glycol Cole di(meth)acrylate, tetraethylene glycol di(meth)acrylate, poly Triethylene glycol di(meth)acrylate, tripropylene glycol di(meth)acrylate Acrylate, polypropylene glycol diallyl ether, and N,N'-methylene bis Multifunctional vinyl monomers such as (meth)acrylamide. (Meth)acryloylmorpholin heterocyclic monomers such as vinyl ether, vinyl pyrrolidone, vinyl pyridine, and vinyl carbazole;

[0050] Acetoxyethyl (meth)acrylate, "Placcel FM" (Daicel Chemical Co., Ltd. Capsule Lactone addition monomer, product name), 3-(meth)acryloxypropyltrimethoxysilane Lan, 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane 3-Acryloxypropyltriethoxysilane, 3-Acryloxypropyltrimethoxysilane, Monomers containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane , trimethylsilyl (meth)acrylate, triethylsilyl (meth)acrylate, Tri-n-propylsilyl (meth)acrylate, Tri-n-butylsilyl (meth)acrylate acrylate, tri-n-amylsilyl (meth)acrylate, tri-n-hexylsilyl ( (meth)acrylate, tri-n-octylsilyl (meth)acrylate, tri-n-dodeca Silsilyl (meth)acrylate, triisopropylsilyl methyl fumarate, triiso Propylsilyl amyl fumarate, tri-n-butylsilyl-n-butyl fumarate, t ert-Butyldiphenylsilyl methyl fumarate, tert-Butyldiphenylsilyl -n-Butyl fumarate, Silaplane FM-0711 (manufactured by JNC Corporation, trade name), Silaplane FM-0721 (product name, manufactured by JNC Corporation), Silaplane FM-07 25 (JNC Corporation, trade name), Silaplane TM-0701 (JNC Corporation, trade name) Product name), Silaplane TM-0701T (JNC Corporation, product name), X-22-17 4ASX (product name, manufactured by Shin-Etsu Chemical Co., Ltd.), X-22-174BX (manufactured by Shin-Etsu Chemical Co., Ltd. ), KF-2012 (Shin-Etsu Chemical Co., Ltd., product name), X-22-242 6 (manufactured by Shin-Etsu Chemical Co., Ltd., trade name), and X-22-2404 (manufactured by Shin-Etsu Chemical Co., Ltd. Organosilyl group-containing monomers other than silane coupling agent-containing monomers, such as .

[0051] Vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, chlorotrifluoro Halogenated olefins such as ethylene, 2-isocyanatoethyl (meth)acrylate, 2, 2,2-Trifluoroethyl (meth)acrylate, 2,2,3,3,3-Pentafluoro Perfluorophenyl (meth)acrylate, 2-(perfluorobutyl)ethyl (meth)acrylate acrylate, 3-(perfluorobutyl)-2-hydroxypropyl (meth)acrylate, 2 -(Perfluorohexyl)ethyl (meth)acrylate, 3-perfluorohexyl- 2-Hydroxypropyl (meth)acrylate, 3-(perfluoro-3-methylbutyl )-2-Hydroxypropyl (meth)acrylate, 2,2,3,3-Tetrafluoropropane 1H,1H,5H-Octafluoropentyl (meth)acrylate acrylate, 1H,1H,5H-octafluoropentyl (meth) methacrylate, 1H, 1H,2H,2H-Tridecafluorooctyl(meth)acrylate, 1H-1-(tri Fluorine-containing monomers such as (fluoromethyl)trifluoroethyl (meth)acrylate (excluding halogenated olefins), 1-butoxyethyl (meth)acrylate, 1-(2 -Ethylhexyloxy)ethyl (meth)acrylate, 1-(cyclohexyloxy) Acetals such as ethyl methacrylate and 2-tetrahydropyranyl (meth)acrylate Monomer having the structure, 4-methacryloyloxybenzophenone, and (meth)acrylic acid -2-Isocyanatoethyl.

[0052] The monomer a'2 is a monomer having copolymerizability and a glass transition point (Tg) of the polymer B2. (Meth)acrylic acid esters are preferred, and (meth)acrylic acid esters containing a hydrocarbon group are preferred. More preferred is methyl (meth)acrylate, and even more preferred is methyl methacrylate. The monomer a'2 may be used alone or in combination of two or more. There can be.

[0053] When methyl methacrylate is used as the monomer a'2, which is a raw material of the polymer A2, The content of methyl methacrylate is 50% by mass or less relative to 100% by mass of the total of monomer a'2. Preferably, the content is 80% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more. By containing 50% by mass or more of dimethacrylate, the glass transition point (Tg) of the polymer A2 is This makes it easier to adjust the value to a desired range.

[0054] The (meth)acrylic copolymer A includes, in addition to the polymer A1 and the polymer A2, It may include the combination A3. The polymer A3 contains, as a monomer unit, a monomer unit a3 represented by the following formula (4): It is preferred.

[0055] [ka]

[0056] In the formula (4), R 8 represents a hydrogen atom or a methyl group, R 9 is a hydrogen atom, halogen N atoms, OH, OR 35 , C.N., N.R. 20 R 21 or R 22 and R 20 , R 21 , R 35 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or unsubstituted substituted alicyclic groups, substituted or unsubstituted aryl groups, substituted or unsubstituted heteroaryl groups a substituted or unsubstituted non-aromatic heterocyclic group, a substituted or unsubstituted aralkyl group, A substituted or unsubstituted alkaryl group or a substituted or unsubstituted organosilyl group. S, R 22 is a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group. It represents a aryl group.

[0057] The monomer unit a3 is a monomer unit derived from the monomer a'3. Examples of the monomer a'3 include the following monomers. The same hydrocarbon group-containing (meth)acrylic acid esters as a'2 and hydroxyl group-containing (meth)acrylic acid esters acrylate ester, carboxyl group-containing vinyl monomer, acid anhydride group-containing vinyl monomer, Unsaturated dicarboxylic acid diester monomer, epoxy group-containing vinyl monomer, amino group-containing ( Meth)acrylic acid ester vinyl monomers, and vinyl monomers containing an amide group.

[0058] Ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate Acrylates, 1,4-Butanediol Di(meth)acrylates, 1,6-Hexanediol Diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate Ethylene glycol di(meth)acrylate, Tetraethylene glycol di(meth)acrylate acrylate, polyethylene glycol di(meth)acrylate, tripropylene glycol di( Meth)acrylate, neopentyl glycol di(meth)acrylate, 1,9-nonane Diol di(meth)acrylate, 1,10-decanediol di(meth)acrylate, Trimethylolpropane tri(meth)acrylate, Pentaerythritol tetra(meth)acrylate ) acrylate, dipentaerythritol hexa(meth)acrylate, allyl(meth) Acrylate, triallyl cyanurate, diallyl maleate, polypropylene glycol Multifunctional compounds such as diaryl ether and N,N'-methylenebis(meth)acrylamide A vinyl monomer.

[0059] (Meth)acryloylmorpholine, vinylpyrrolidone, vinylpyridine, and vinylcaprylamide Heterocyclic monomers such as carbazole. (Meth)acrylate, acetoxyethyl, Plaxel F M" (product name of Daicel Chemical Industries, Ltd. caprolactone addition monomer), 3-(meth)acrylonitrile Acryloxypropyltrimethoxysilane, 3-(meth)acryloxypropylmethyldiethion xysilane, 3-(meth)acryloxypropyltriethoxysilane, 3-acryloxy Propyltrimethoxysilane, vinyltrimethoxysilane, vinyltriethoxysilane, etc. Silane coupling agent-containing monomer, trimethylsilyl (meth)acrylate, triethyl n-propylsilyl (meth)acrylate, tri-n-propylsilyl (meth)acrylate, tri -n-Butylsilyl (meth)acrylate, Tri-n-amylsilyl (meth)acrylate , tri-n-hexylsilyl (meth)acrylate, tri-n-octylsilyl (meth)acrylate ) acrylate, tri-n-dodecylsilyl (meth)acrylate, triisopropylsilyl methylsilyl fumarate, triisopropylsilyl amyl fumarate, tri-n-butylsilyl tert-Butyl-n-butyl fumarate, tert-butyldiphenylsilylmethyl fumarate, t ert-Butyldiphenylsilyl-n-butyl fumarate, Silaplane FM-071 1 (JNC Corporation, product name), Silaplane FM-0721 (JNC Corporation, product name) name), Silaplane FM-0725 (manufactured by JNC Corporation, product name), Silaplane TM -0701 (JNC Corporation, product name), Silaplane TM-0701T (JNC Corporation) ), X-22-174ASX (Shin-Etsu Chemical Co., Ltd., product name), X-22 -174BX (product name, manufactured by Shin-Etsu Chemical Co., Ltd.), KF-2012 (manufactured by Shin-Etsu Chemical Co., Ltd. X-22-2426 (manufactured by Shin-Etsu Chemical Co., Ltd., trade name), and X-22- 2404 (Shin-Etsu Chemical Co., Ltd., product name) and other silane coupling agent-containing monomers Other organosilyl group-containing monomers.

[0060] 4-Methacryloyloxybenzophenone and (meth)acrylic acid-2-isocyanate ethyl. As the monomer a'3, from the viewpoint of ease of handling, a group consisting of the following monomers is preferred: At least one selected from the following is preferred.

[0061] Methyl (meth)acrylate, Ethyl (meth)acrylate, n-Propylene (meth)acrylate (meth)acrylate, isopropyl, n-butyl, (meth)acrylate isobutyl acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate , (meth)acrylate 2-ethylhexyl, (meth)acrylate octyl, (meth)acrylate Isooctyl (meth)acrylate, Nonyl (meth)acrylate, Isononyl (meth)acrylate, p) decyl acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, Hexadecyl (meth)acrylate, Stearyl (meth)acrylate, (meth)acrylic acid Isostearyl, (meth)acrylate phenyl, (meth)acrylate benzyl, (meth)acrylate Cyclohexyl acrylate, Tetrahydrofurfuryl (meth)acrylate, (meth)acrylic acid isobornyl acrylate, and terpene acrylates and their derivatives, etc. (Meth)acrylic acid ester.

[0062] 2-Hydroxyethyl (meth)acrylate, 2-Hydroxypropyl (meth)acrylate (Meth)acrylate, 2-Hydroxybutyl, (Meth)acrylate, 3-Hydroxybutyl and hydroxyl group-containing (meth)acrylic acid esters such as 4-hydroxybutyl (meth)acrylate. Steal. Carboxyl group-containing vinyl monomers such as (meth)acrylic acid. (Meth)acrylic acid glycerol Epoxy group-containing vinyl monomers such as glycidyl and α-ethyl acrylate. aminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate, etc. An amino group-containing (meth)acrylic ester vinyl monomer.

[0063] (Meth)acrylamide, N-methyl(meth)acrylamide, N,N'-dimethyl( meth)acrylamide, N-isopropylacrylamide, and N-(hydroxymethyl ) Vinyl monomers containing an amide group such as acrylamide. Ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate Acrylates, 1,4-Butanediol Di(meth)acrylates, 1,6-Hexanediol Diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate Ethylene glycol di(meth)acrylate, Tetraethylene glycol di(meth)acrylate acrylate, pentaerythritol tetra(meth)acrylate, allyl(meth)acrylate and polyfunctional vinyl monomers such as N,N'-methylenebis(meth)acrylamide.

[0064] (Meth)acryloylmorpholine, vinylpyrrolidone, vinylpyridine, and vinylcaprylamide Heterocyclic monomers such as carbazole. 3-(meth)acryloxypropyltrimethoxysilane , 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane Silanes such as 3-propyltriethoxysilane and 3-acryloxypropyltrimethoxysilane Monomer containing silyl coupling agent, trimethylsilyl (meth)acrylate, triethylsilyl (meth)acrylate, tri-n-propylsilyl (meth)acrylate, tri-n- Oligosaccharides other than monomers containing silane coupling agents such as butylsilyl (meth)acrylate A monomer containing a silyl group.

[0065] 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoroethyl Fluorine-containing monomers such as fluoropropyl (meth)acrylate (but not halogenated olefins) ), 1-butoxyethyl (meth)acrylate, 1-(2-ethylhexyloxy ) A monomer having an acetal structure such as ethyl (meth)acrylate. The (meth)acrylic copolymer A further contains a monomer unit d derived from a macromonomer. The macromonomer means a polymer having a polymerizable functional group.

[0066] The monomer unit d can be produced by using a macromonomer d' as a raw material to produce a specific polymer. The above-mentioned component can be introduced into the (meth)acrylic copolymer A. The monomer unit d is contained in any one of the polymer A1, the polymer A2, and the polymer A3. It may be possible. When the macromonomer d' is used as a raw material for the polymer A1, The polymerizable functional group of the monomer d' is copolymerized with the monomer a'2, which is a raw material of the polymer A2. Conversely, it is preferable that the macromonomer d' is used as a raw material for the polymer A2. When the macromonomer d' is used as the polymerizable functional group, the polymerizable functional group of the macromonomer d' is It is preferable that the monomer is copolymerizable with the raw material monomer a'1.

[0067] The monomer units constituting the macromonomer d' are the monomer units a1, The macro unit a2 and the monomer unit a3 can be appropriately selected from the group consisting of the macro unit a1 and the monomer unit a2. The raw material of the monomer d' is the monomer a'1, the monomer a', and the monomer a'3. It can be appropriately selected from the group consisting of: When the macromonomer d' is used as a raw material for the polymer A2, the macromonomer This is preferable because the macromonomer d' can be handled as a solid. By using the monomer unit as the raw material of the polymer A2 and copolymerizing it with the monomer unit that is the raw material of the polymer A1, It is possible to produce a (meth)acrylic copolymer.

[0068] The radical polymerizable group contained in the macromonomer d′ is an ethylenically unsaturated bond. As the group having an ethylenically unsaturated bond, for example, a group having CH2= C(COOR 6 )-CH2-, (meth)acryloyl group, 2-(hydroxymethyl)acryloyl group Examples of the alkyl group include aryl groups, triaryl groups, and vinyl groups. Here, R 6 is a hydrogen atom, an unsubstituted or substituted alkyl group, or substituted alicyclic groups, unsubstituted or substituted aryl groups, unsubstituted or or substituted heteroaryl groups, or unsubstituted or substituted non-aromatic represents a heterocyclic group represented by the formula:

[0069] R 6 As the alkyl group, an unsubstituted alkyl group, an unsubstituted alicyclic group, an unsubstituted aryl group, an unsubstituted Specific examples of the heteroaryl group, the unsubstituted non-aromatic heterocyclic group, and the substituents of each group are as described above. R in formula (1) 2 COOR as 35 R 35 The same as R 6 As is an unsubstituted or substituted alkyl group, or an unsubstituted or substituted alkyl group. Alicyclic groups are preferred, as are unsubstituted alkyl groups or unsubstituted or substituted alkyl groups. Alicyclic groups having a group are more preferred.

[0070] R 6 is a hydrogen atom, an unsubstituted or substituted alkyl group, an unsubstituted or substituted substituted alicyclic groups, unsubstituted or substituted aryl groups, unsubstituted or A substituted heteroaryl group or an unsubstituted or substituted non-aromatic heteroaryl group. Among the cyclic groups, methyl, ethyl, n-propyl, and isopropyl groups are the most popular due to their availability. propyl group, n-butyl group, tert-butyl group, pentyl group, hexyl group, heptyl group, Octyl, cyclopropyl, cyclobutyl, isobornyl and adamantyl groups Preferred are a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, tert-Butyl, cyclopropyl, cyclobutyl, isobornyl and adamantyl At least one selected from the group consisting of ethyl groups is preferred.

[0071] The macromonomer d' preferably has a monomer unit having a radical polymerizable group. It is preferable that the number of the monomer units having the radical polymerizable group is 2 or more. The macromonomer d' preferably has two or more of the monomer units a2. The macromonomer d' more preferably has a structure represented by the following formula (2).

[0072] [ka]

[0073] In formula (2), R 0 ~R n each independently represents a hydrogen atom, an unsubstituted or substituted an alkyl group having a group, an unsubstituted or substituted alicyclic group, an unsubstituted or substituted substituted aryl groups, unsubstituted or substituted heteroaryl groups, or unsubstituted represents a substituted or substituted non-aromatic heterocyclic group, 0 ~R n are respectively X may be the same or different. 1 ~X n represents a hydrogen atom or a methyl group, and multiple X 1 ~Xn may be the same or different, Z is a terminal group, and n is a natural number from 2 to 10,000. It is.

[0074] Z may be, for example, a hydrogen atom, like the terminal group of a polymer obtained by known radical polymerization. Examples of the radical polymerizable group include an atom, a group derived from a radical polymerization initiator, and a radical polymerizable group. n is 2 to 10,000, and from the viewpoint of moldability, it is preferably 2 to 1,000, and more preferably 5 to 1,000. is more preferable, 10 to 500 is even more preferable, and 20 to 500 is even more preferable. Z is a terminal group of the macromonomer d'. Z may be, for example, a known radical polymerization As with the terminal groups of the polymer obtained in the above, the terminal groups include hydrogen atoms, groups derived from the radical polymerization initiator, and radicals. dialkyl polymerizable groups and the like.

[0075] R in Equation (2) 0 ~R n is a group having an ethylenically unsaturated bond, CH2=C( COOR 6 )-CH2-R 6 is the same as: R in the copolymer 6 From the viewpoint of maintaining hydrophobicity, alkyl groups, alicyclic groups, aryl groups, and heterocyclic groups are used. Preferably, the aromatic group is an aryl group or a non-aromatic heterocyclic group, more preferably an alkyl group or an alicyclic group. It is more preferable that the aryl group is an alkyl group, and it is even more preferable that the aryl group is an alkyl group.

[0076] The number average molecular weight (Mn) of the macromonomer d' is 200 to 100,000. is preferable, 500 to 100,000 is more preferable, and 1,000 to 50,000 is even more preferable. A value of 2,000 to 50,000 is even more preferable. The number average molecular weight of the macromonomer d' is 200 or more and 100,000 or less, The formability is better.

[0077] The number average molecular weight of the macromonomer d' is determined by gel permeation chromatography (GPC). The molecular weight is calculated as a relative molecular weight using polymethyl methacrylate as the standard resin. Constituent monomers relative to 100% by mass of all constituent units constituting the macromonomer d' The proportion of the unit (b2) is preferably 40% by mass or more, more preferably 50% by mass or more, and 00% by mass is even more preferable.

[0078] The macromonomer d' is prepared by a known method described in JP-A-2022-65185. It can be made. The ratio of the monomer unit a1 in the (meth)acrylic copolymer A is ) 10% by mass based on 100% by mass of the total of all structural units constituting acrylic copolymer A It is preferable that the content is 20% by mass or more, more preferably 30% by mass or more. It is more preferable that the content is 40 mass % or more, and even more preferable that the content is 40 mass % or more. The ratio of the monomer unit a1 in the (meth)acrylic copolymer A is 90% by mass or less relative to 100% by mass of the total of all structural units constituting the copolymer A. It is preferable that the content is 80% by mass or less, more preferably 70% by mass or less. It is more preferable that the (meth)acrylic acid content is 60 mass % or less, and even more preferable that the (meth)acrylic acid content is 60 mass % or less. When the proportion of the monomer unit a1 in the copolymer A is 90 mass % or less, the moldability is improved. Better.

[0079] The ratio of the monomer unit a2 in the (meth)acrylic copolymer A is ) 10% by mass based on 100% by mass of the total of all structural units constituting acrylic copolymer A It is preferable that the content is 20% by mass or more, more preferably 30% by mass or more. It is more preferable that the content is 40 mass % or more, and even more preferable that the content is 40 mass % or more. The ratio of the monomer unit a2 in the (meth)acrylic copolymer A is 90% by mass or less relative to 100% by mass of the total of all structural units constituting the copolymer A. It is preferable that the content is 80% by mass or less, more preferably 70% by mass or less. More preferably, the content of the monomer unit a is 60 mass % or less. When the proportion of 2 exceeds 10 mass %, the moldability is superior.

[0080] When the (meth)acrylic copolymer A contains the monomer unit a3, the (meth)acrylic The ratio of the monomer unit a3 in the acrylic copolymer A is The content is 0 to 33% by mass relative to 100% by mass of the total of all constituent units constituting the compound A. It is preferably 0 to 25% by mass, more preferably 0.5 to 20% by mass. More preferably, the monomer in the (meth)acrylic copolymer A may be 0% by mass. The ratio of the monomer unit a3 is 1 / 100 of the total of all the structural units constituting the (meth)acrylic copolymer A. When the content of the polymer A1 is 0 to 33% by mass relative to 00% by mass, the functions of the polymer A1 and the polymer A2 are is not impaired.

[0081] The weight average molecular weight of the (meth)acrylic copolymer A is preferably 75,000 or more, and more preferably 750 00 to 1,000,000 is more preferable, and 80,000 to 500,000 is even more preferable. It is preferable that the weight average molecular weight is 75,000 or more and 1,000,000 or less, since excellent moldability is obtained. The weight average molecular weight of the copolymer was determined by gel permeation chromatography (GPC). It is calculated as a relative molecular weight using methyl methacrylate as the standard resin.

[0082] In the (meth)acrylic copolymer A, the polymer A2 has a low miscibility with other resins C. and compatibility, and (meth)acrylic copolymer A can be handled as a solid. It has the effect of The polymer A2 preferably has a glass transition point (Tg) of 50° C. or higher by itself. It is preferable that the temperature is not lower than 65°C, and more preferably not lower than 80°C. It is more preferable that the Tg is 50° C. or higher. The handleability of the resulting solid is improved. The glass transition point (Tg) of the polymer is preferably 150° C. or lower, and more preferably 130° C. or lower. It is more preferable that the Tg is 110° C. or less, and it is even more preferable that the Tg is 150° C. or less. In this case, the compatibility of the obtained copolymer with other resin C and the resin composition of the present invention can be improved. This improves the miscibility when mixing.

[0083] The (meth)acrylic copolymer A can be produced by a living polymerization method and a macromonomer polymerization method. Examples of the living polymerization method include a living radical polymerization method and Examples of the living radical polymerization method include: Reversible addition-fragmentation chain transfer polymerization (RAFT), atom transfer radical polymerization (ATRP), nitroxyl Cid-mediated polymerization (NMP) and living radical polymerization with organotellurium as a growing end (TER P) and the like. The method using a macromonomer is relatively easy to use. The advantage of this method is that it can produce a vinyl copolymer (B) without the need for a catalyst and This is preferable because it has the advantage that no process for removing residual auxiliary agents or for terminal treatment is required.

[0084] (Method of producing (meth)acrylic copolymer A using macromonomer) A method for producing the (meth)acrylic copolymer A using the macromonomer d' As for the macromonomer d', the polymer A1, the polymer A2, and the polymer As an example, the macromonomer d' may be used as a raw material for the macromonomer A3. The method of using this as a raw material for the polymer A2 will be described.

[0085] For example, a monomer mixture containing monomer b'1 and macromonomer d', which is the raw material of polymer A2, The mixture can be polymerized by bulk polymerization, suspension polymerization, or solution polymerization. Contains 0.001 to 5 parts by mass of a non-metallic chain transfer agent relative to 100 parts by mass of the monomer mixture A method in which the polymerizable composition is subjected to suspension polymerization is preferred. The polymerizable composition preferably contains a dispersant.

[0086] By carrying out suspension polymerization, copolymers with excellent moldability and ease of processing can be obtained. By this method, a copolymer with a narrow molecular weight distribution can be obtained. The copolymer in the form of beads may be recovered from the suspension and used for producing a molded article. The copolymer may be molded into pellets and used to manufacture the molded article. For example, the copolymer may be polymerized in a solution. The polymer solution obtained by the above is dropped into a poor solvent to reprecipitate, or the polymer is extruded by degassing or other methods. The powdered copolymer may be recovered by removing the solvent and used for producing a molded article. The powdered copolymer may be molded into pellets and then used to produce the molded article.

[0087] As a preferred method for producing the copolymer by suspension polymerization, for example, the following method (A) and method (B) are available. ) and method (C). Method (A) is a method of dissolving macromonomer d' in a monomer other than macromonomer d' to obtain a monomer mixture. After preparing the monomer mixture, a radical polymerization initiator and, if necessary, a nonmetallic compound are added to the monomer mixture. A chain transfer agent is added to prepare a polymerizable composition. Thereafter, the polymerizable composition is optionally The polymerizable composition is dispersed in an aqueous solution containing a dispersant to prepare a syrup dispersion of the polymerizable composition. The method is a method of suspension polymerization of a syrup dispersion of the polymerizable composition.

[0088] In method (A), a syrup is prepared in which the macromonomer particles are completely dissolved in the monomer. By this method, it is easy to obtain particles having a uniform composition. The polymer provides a molded article with excellent mechanical strength. In the method (B), the macromonomer d' and, if necessary, a dispersing agent added thereto are first added to water. Monomers other than macromonomer d' are added to the aqueous suspension in which the agent is dispersed to obtain a monomer mixture. A syrup dispersion of the monomer mixture is prepared. A radical polymerization initiator is added to the syrup dispersion of the monomer mixture. and optionally a non-metallic chain transfer agent to prepare a syrup dispersion of the polymerizable composition. Then, the syrup dispersion of the polymerizable composition is subjected to suspension polymerization.

[0089] In method (B), the process for recovering the macromonomer d' can be omitted, thereby shortening the production process. That is, in the method (B), the aqueous suspension is a suspension polymerization The suspension obtained by synthesizing macromonomer d' by the method was used, and monomer was added to the suspension. Since the macromonomer d' can be copolymerized with the amine, the step of recovering the macromonomer d' can be omitted. The macromonomer d' can be synthesized by polymerization using a known method.

[0090] In contrast, in method (A), the macromonomer d' synthesized by suspension polymerization is granulated into particles. It is recovered and used as such. Method (C) is to dissolve macromonomer d' in a monomer other than macromonomer d' to obtain a monomer mixture. After preparing the monomer mixture, a radical polymerization initiator and, if necessary, a nonmetallic compound are added to the monomer mixture. A chain transfer agent is added to prepare a polymerizable composition. The polymerizable composition is then dispersed in water. A syrup dispersion of the polymerizable composition is prepared by adding a dispersant immediately before polymerization. The method is a method of suspension polymerization of a syrup dispersion of the synthetic composition.

[0091] Here, "aqueous suspension" refers to a state in which monomer and / or syrup are dispersed in water. means. In method (C), the monomer dispersion state in the system can be stabilized, so method (A) Particles having a more uniform composition are more likely to be obtained. In any of the above methods (A), (B), or (C), When dissolving macromonomer d' in a monomer other than macromonomer d', it is preferable to heat the mixture. stomach.

[0092] The heating temperature when dissolving macromonomer d' in monomers other than macromonomer d' is 3 The heating temperature is preferably 30° C. or higher, and the macromonomer d' is preferably 0 to 90° C. It tends to improve the solubility of monomers other than d', and the heating temperature is 90°C or higher. The lower limit of the heating temperature is preferably 35°C or higher. The upper limit of the heating temperature is more preferably 75° C. or less. When macromonomer d' is dissolved in a monomer other than macromonomer d', the monomer mixture is Heating to a temperature of 0 to 90°C is preferred, and heating to a temperature of 35 to 75°C is more preferred.

[0093] A radical polymerization initiator is used when polymerizing a monomer mixture containing macromonomer d'. In this case, the timing of adding the radical polymerization initiator is macromonomer d'. It is preferable to add the macromonomer d' after dissolving it in the monomer other than the monomer d'. The monomer mixture is prepared by dissolving the macromonomer d' in a monomer other than the macromonomer d'. It is preferred to add a radical polymerization initiator to the mixture.

[0094] When adding the radical polymerization initiator, the temperature of the monomer mixture should be 0°C or higher. It is preferable that the temperature is equal to or lower than the 10-hour half-life temperature of the polymerization initiator minus 15°C. When adding the radical polymerization initiator, the temperature is 0°C or higher. The solubility of monomers other than d' tends to be good. In addition, the addition of a radical polymerization initiator The temperature at which the polymerization is carried out is equal to or lower than the 10-hour half-life temperature of the radical polymerization initiator minus 15°C. If so, the polymerization tends to be stable.

[0095] As the radical polymerization initiator, known initiators can be used, for example, organic peroxides and aryl groups. Examples of such compounds include zo compounds. The radical polymerization initiators can be used alone or in combination of two or more. Cut. The amount of the radical polymerization initiator to be added is determined based on the amount of the macromonomer d' and the amount of the macromonomer d' in terms of controlling the heat generated by polymerization. 0.0001 parts by mass or more per 100 parts by mass of the total amount of monomers other than chromium monomer d' The amount is preferably 0 parts by mass or less, and more preferably from 0.0005 parts by mass to 5 parts by mass.

[0096] In the above-mentioned method (A) or method (B), the polymerization temperature during suspension polymerization of the polymerizable composition is There is no particular limitation on the temperature, but it is generally preferred that the temperature is 50 to 120°C, and 70 to 100°C is more preferred. The polymerization time is preferably from 1 to 6 hours, more preferably from 1.5 to 4 hours. The stirring conditions are preferably 100 to 800 rpm, and more preferably 150 to 600 rpm. More preferred.

[0097] Examples of dispersants used in suspension polymerization include alkali metal salts of poly(meth)acrylic acid. , a copolymer of an alkali metal salt of (meth)acrylic acid and an ester of (meth)acrylic acid, Copolymerization of alkali metal salts of sulfoalkyl methacrylates with (meth)acrylic esters. Polystyrene sulfonic acid alkali metal salts, styrene sulfonic acid alkali metal salts and Copolymers of (meth)acrylic acid esters, alkali metal salts of (meth)acrylic acid and (meth)acrylic acid ) an alkali metal salt of sulfoalkyl acrylate and an alkali metal salt of styrenesulfonic acid Copolymers of (meth)acrylic acid esters, alkali metal salts of (meth)acrylic acid and (meth)acrylic acid p) Copolymerization of alkali metal salts of sulfoalkyl acrylates with (meth)acrylic esters A combination of an alkali metal salt of (meth)acrylic acid and an alkali metal salt of styrenesulfonic acid and ( Copolymers with meth)acrylic acid esters and alkyl (meth)acrylates Copolymerization of alkali metal salts of styrenesulfonic acid with (meth)acrylic acid esters Polymerization; Polyvinyl alcohol with a saponification degree of 70-100%; Methylcellulose; Starch; Hydroxyapatite is an example of such a material. These materials may be used alone or in combination. Among these, (meth)acrylic acid having good dispersion stability during suspension polymerization is preferred. Copolymers of alkali metal salts of sulfoalkyl acrylates and (meth)acrylic esters are preferred. It is nice.

[0098] The dispersant is preferably used in an amount of 0.005 to 5% by mass, more preferably 0.01 to 5% by mass, based on the total mass of the aqueous suspension. The content of the dispersant in the aqueous suspension is preferably 0.005% by mass or more. The dispersion stability of the suspension polymerization liquid is good, and the washability, dewaterability, drying property and the like of the obtained polymer are excellent. In addition, when the content of the dispersant is 5% by mass or less, the polymerization There is a tendency for the polymerization stability to be good and for foaming to be reduced during polymerization.

[0099] Sodium carbonate, sodium sulfate, and sodium sulfate are used to improve the dispersion stability of aqueous suspensions. An electrolyte such as calcium carbonate may be added to the aqueous suspension. In this case, the proportion of the electrolyte is: In the case of the method (A), the content is 0.01 to 0.5% by mass based on the total mass of the aqueous suspension. In the case of the method (B), the preferred ratio of the electrolyte in the aqueous suspension is The content is preferably 0.01 to 10% by mass.

[0100] A copolymer is obtained by polymerizing a polymerizable composition containing a monomer mixture and a nonmetallic chain transfer agent described later. It is preferable to obtain The nonmetallic chain transfer agent is added to a monomer mixture when a polymer is obtained, and It is preferable to add it when obtaining a polymer by suspension polymerization. By using a nonmetallic chain transfer agent as a chain transfer agent, the unreacted macromonomers contained in the polymer can be easily removed. This can reduce the noise.

[0101] Examples of the nonmetallic chain transfer agent include t-dodecyl mercaptan, n-octyl mercaptan, Sulfur-containing chain transfer agents such as tetrachloromethane, α-methylstyrene dimer, carbon tetrachloride and terpene However, sulfur-containing chain transfer arylsulfides are preferred due to their availability and high chain transfer ability. A kinetic agent is preferred. The content of the nonmetallic chain transfer agent is 0.01 to 100 parts by mass of the total monomer mixture. 0.5 parts by weight is preferred. When the content of the nonmetallic chain transfer agent is 0.01 parts by mass or more, the effect of adding the agent is sufficiently obtained. When the content of the nonmetallic chain transfer agent is 0.5 parts by mass or less, the mechanical strength after curing is excellent. The content is more preferably 0.03 to 0.3 parts by mass, and further preferably 0.05 to 0.2 parts by mass. stomach.

[0102] <(Meth)acrylic copolymer B> The (meth)acrylic copolymer B may have, but is not limited to, a monomer unit represented by the following formula ( It is preferable that the monomer unit b1 represented by the formula (5) is contained.

[0103] [ka]

[0104] In the formula (5), R 10 represents a hydrogen atom or a methyl group, R 11 is a hydrogen atom, halogen atoms, OH, OR 36 , C.N., N.R. 40 R 41 or R 42 and R 40 , R 41 , R 36 each independently represents a hydrogen atom, a substituted or unsubstituted alkyl group, a substituted or Unsubstituted alicyclic groups, substituted or unsubstituted aryl groups, substituted or unsubstituted heteroaryl groups a substituted or unsubstituted non-aromatic heterocyclic group, a substituted or unsubstituted aralkyl group, group, a substituted or unsubstituted alkaryl group, or a substituted or unsubstituted organosilyl group. R 22 is a substituted or unsubstituted aryl group, or a substituted or unsubstituted heteroaryl group. Represents a aryl group.

[0105] Examples of the monomer b1 include the following monomers. The same hydrocarbon group-containing (meth)acrylic acid esters as a'2 and hydroxyl group-containing (meth)acrylic acid esters acrylate ester, carboxyl group-containing vinyl monomer, acid anhydride group-containing vinyl monomer, Unsaturated dicarboxylic acid diester monomer, epoxy group-containing vinyl monomer, amino group-containing ( Meth)acrylic acid ester vinyl monomers, and vinyl monomers containing an amide group.

[0106] From the viewpoint of ease of handling, the monomer b1 is selected from the group consisting of the following monomers: At least one selected from the above is preferred. Methyl (meth)acrylate, Ethyl (meth)acrylate, n-Propylene (meth)acrylate (meth)acrylate, isopropyl, n-butyl, (meth)acrylate isobutyl acrylate, tert-butyl (meth)acrylate, hexyl (meth)acrylate , (meth)acrylate 2-ethylhexyl, (meth)acrylate octyl, (meth)acrylate Isooctyl (meth)acrylate, Nonyl (meth)acrylate, Isononyl (meth)acrylate, p) decyl acrylate, isodecyl (meth)acrylate, lauryl (meth)acrylate, Hexadecyl (meth)acrylate, Stearyl (meth)acrylate, (meth)acrylic acid Isostearyl, (meth)acrylate phenyl, (meth)acrylate benzyl, (meth)acrylate Cyclohexyl acrylate, Tetrahydrofurfuryl (meth)acrylate, (meth)acrylic acid isobornyl acrylate, and terpene acrylates and their derivatives, etc. (Meth)acrylic acid ester.

[0107] 2-Hydroxyethyl (meth)acrylate, 2-Hydroxypropyl (meth)acrylate (Meth)acrylate, 2-Hydroxybutyl, (Meth)acrylate, 3-Hydroxybutyl and hydroxyl group-containing (meth)acrylic acid esters such as 4-hydroxybutyl (meth)acrylate. Steal. Carboxyl group-containing vinyl monomers such as (meth)acrylic acid. (Meth)acrylic acid glycerol Epoxy group-containing vinyl monomers such as glycidyl and α-ethyl acrylate. aminoethyl (meth)acrylate and diethylaminoethyl (meth)acrylate, etc. An amino group-containing (meth)acrylic ester vinyl monomer.

[0108] (Meth)acrylamide, N-methyl(meth)acrylamide, N,N'-dimethyl( meth)acrylamide, N-isopropylacrylamide, and N-(hydroxymethyl ) Vinyl monomers containing an amide group such as acrylamide. Ethylene glycol di(meth)acrylate, 1,3-butylene glycol di(meth)acrylate Acrylates, 1,4-Butanediol Di(meth)acrylates, 1,6-Hexanediol Diethylene glycol di(meth)acrylate, triethylene glycol di(meth)acrylate Ethylene glycol di(meth)acrylate, Tetraethylene glycol di(meth)acrylate acrylate, pentaerythritol tetra(meth)acrylate, allyl(meth)acrylate and polyfunctional vinyl monomers such as N,N'-methylenebis(meth)acrylamide.

[0109] (Meth)acryloylmorpholine, vinylpyrrolidone, vinylpyridine, and vinylcaprylamide Heterocyclic monomers such as carbazole. 3-(meth)acryloxypropyltrimethoxysilane , 3-(meth)acryloxypropylmethyldiethoxysilane, 3-(meth)acryloxypropylmethyldiethoxysilane Silanes such as 3-propyltriethoxysilane and 3-acryloxypropyltrimethoxysilane Monomer containing silyl coupling agent, trimethylsilyl (meth)acrylate, triethylsilyl (meth)acrylate, tri-n-propylsilyl (meth)acrylate, tri-n- Oligosaccharides other than monomers containing silane coupling agents such as butylsilyl (meth)acrylate A monomer containing a silyl group.

[0110] 2,2,2-trifluoroethyl (meth)acrylate, 2,2,3,3-tetrafluoroethyl Fluorine-containing monomers such as fluoropropyl (meth)acrylate (but not halogenated olefins) ), 1-butoxyethyl (meth)acrylate, 1-(2-ethylhexyloxy ) A monomer having an acetal structure such as ethyl (meth)acrylate. The glass transition temperature (Tg) of the (meth)acrylic copolymer B is preferably 60° C. or higher. 65°C or higher is more preferable, 70°C or higher is even more preferable, and 75°C or higher is particularly preferable. When the Tg of the (meth)acrylic copolymer B is 60° C. or higher, the block copolymer of the resin composition It can prevent kings.

[0111] The Tg is determined by the method described in Polymer Handbook, J. Brainard et al. The homopolymer galvanopolymer described in The value is calculated from the glass transition temperature and mass fraction by the Fox formula. The Fox formula is as follows: 1 / (273+Tg)=Σ(Wi / (273+Tgi)) where Wi is the mass fraction of monomer i, Tgi is the glass transition temperature of the homopolymer of monomer i (℃) is shown.

[0112] The glass transition temperature of homopolymers not listed in the "Polymer Handbook" When a monomer is used, the Tg is a value actually measured by a differential scanning calorimeter (DSC). The particle size of the (meth)acrylic copolymer is the mean particle size measured using a particle size distribution meter. The diameter is preferably 20 μm or less, more preferably 10 μm or less, and even more preferably 5 μm or less. The particle size of the (meth)acrylic copolymer B is preferably 1 μm or less, and particularly preferably 1 μm or less. The median diameter measured using a sieve is preferably 1 nm or more, more preferably 10 nm or more. More preferably, the thickness is 50 nm or more, and particularly preferably, the thickness is 100 nm or more. If the particle size of copolymer B is 20 μm or less, (meth)acrylic copolymer B can be efficiently The particle size of (meth)acrylic copolymer B is 1. If the diameter is 1 nm or more, blocking can be prevented. It represents the median value when the values ​​are arranged in order from the minimum to the maximum. The (meth)acrylic copolymer B may be used alone or in combination of two or more. can be done.

[0113] <Resin composition> In the resin composition of the present invention, the content of the (meth)acrylic copolymer B is not particularly limited. The content of the (meth)acrylic copolymer B in the resin composition of the present invention is not limited. , preferably 5% by mass or less, more preferably 4% by mass or less, based on 100% by mass of the total of the resin composition of the present invention. More preferably, the content is 3% by mass or less, even more preferably, 2% by mass or less. The content of the (meth)acrylic copolymer B is 100% by mass in total of the resin composition of the present invention. When the (meth)acrylic acid is 5% by mass or less based on the total mass of the resin composition of the present invention, the (meth)acrylic acid can be easily obtained by using the article made of the resin composition of the present invention. In addition, the above (methacrylic copolymer A) in the resin composition of the present invention does not inhibit the performance of the above (methacrylic copolymer B). ) The content of the acrylic copolymer B is, relative to the total 100% by mass of the resin composition of the present invention, 0.01% by mass or more is preferable, 0.05% by mass or more is more preferable, and 0.1% by mass or more is more preferable. More preferably, the content is 0.5 mass % or more, and even more preferably 0.5 mass % or more. The content of the polymer B is 0.01% by mass or more relative to 100% by mass of the total of the resin composition of the present invention. In this case, the decrease in blocking property of the resin composition of the present invention can be further suppressed.

[0114] The resin composition of the present invention is produced by producing a (meth)acrylic copolymer A by a suspension polymerization method. When the beads are recovered, it is preferable to add the (meth)acrylic copolymer B. The form in which the (meth)acrylic copolymer B is added is not particularly limited. It is preferable to add the acrylic copolymer B in the form of a dispersion in water. When the acrylic copolymer B is added in the form of a dispersion, the (meth)acrylic copolymer B can be efficiently added. The (meth)acrylic copolymer A can be coated with the (meth)acrylic copolymer B. The timing of adding the (meth)acrylic copolymer B is determined based on the polymer obtained by suspension polymerization. It may be added in a slurry state, or in the step of dehydrating the polymer slurry or in the step of adding the polymer to the bead after dehydration. It may also be added during the process of recovering the oil.

[0115] <Other resins C> The resin composition of the present invention comprises the (meth)acrylic copolymer A, the (meth)acrylic In addition to the copolymer B, other resins C may be included. Examples of other resins C include There is no limitation to the type of resin, for example, (meth)acrylic resin such as PMMA, halogenated resin such as polyvinyl chloride, etc. Vinyl acrylate resin, polyolefin, polystyrene, polyamide, polyurethane, polysulfone Polyethersulfone, unsaturated polyester, polyethylene terephthalate, poly Saturated polyesters such as butylene terephthalate, polyvinyl ether, polycarbonate , silicone resin, epoxy resin, polyether ether ketone and polyvinylidene fluoride These may be used alone or in combination of two or more. For example, when a polyvinyl chloride resin is used as the resin C, the vinyl chloride polymer C1 and Contains plasticizer C2 and stabilizer C3 as essential ingredients.

[0116] <Vinyl chloride polymer C1> The vinyl chloride polymer C1 is a polymer containing vinyl chloride monomer units. The copolymer C1 is not particularly limited, and may be, for example, a homopolymer of vinyl chloride, Post-chlorinated vinyl chloride polymer, partially crosslinked vinyl chloride polymer, or copolymerized with vinyl chloride and copolymers of vinyl chloride containing other vinyl compounds which can be obtained. The polymer containing vinyl chloride monomer units may be used alone or in combination. You may use it.

[0117] The vinyl chloride polymer C1 is a vinyl chloride polymer having an average chlorine content of 56 to 75% by mass. vinyl chloride polymers, and vinyl chloride copolymers of vinyl chloride polymers and elastic bodies and / or elastomers At least one resin selected from vinyl chloride copolymers is preferred. The vinyl polymer C1 may be used alone or in combination of two or more kinds. In the case of copolymers of vinyl chloride with other vinyl compounds that can be copolymerized with vinyl chloride, the components other than vinyl chloride are Since the mechanical properties decrease as the content of the unit increases, the proportion of the vinyl chloride polymer C1 The proportion of vinyl chloride is preferably 70% by mass or more.

[0118] Monomers that can be copolymerized with vinyl chloride are those that have reactive double bonds in the molecule. For example, α-olefins such as ethylene, propylene, and butylene, vinyl acetate, vinyl esters such as vinyl propionate, butyl vinyl ether, cetyl vinyl Vinyl ethers such as ether; unsaturated carboxylic acids such as acrylic acid and methacrylic acid , methyl acrylate, ethyl methacrylate, phenyl methacrylate, and other acrylic acids; Methacrylic acid esters, aromatic vinyls such as styrene and α-methylstyrene, salts Vinyl halides such as vinylidene chloride and vinyl fluoride, N-phenylmaleimide, N- Examples of the N-substituted maleimides include cyclohexylmaleimide. can be used alone or in combination of two or more.

[0119] The average degree of polymerization of the vinyl chloride polymer C1 is preferably in the range of 300 to 5,000. The average degree of polymerization is preferably 300 or more, and more preferably 500 to 3000. The mechanical properties of the molded product are good. In addition, by setting the average degree of polymerization to 5000 or less, the processability is improved. It will be good. The method for producing the vinyl chloride polymer C1 is not particularly limited, and any method, for example, emulsion polymerization method, can be used. The polymerization can be carried out by a method such as suspension polymerization, solution polymerization, or bulk polymerization.

[0120] The polyvinyl chloride resin contains a plasticizer C2. The plasticizer C2 is polyvinyl chloride. There are no particular limitations on the plasticizer as long as it has good miscibility or compatibility with the vinyl resin, and any known plasticizer may be used. Examples of such plasticizers include phthalic acid compounds, trime Lithium acid compounds, cyclohexanedicarboxylic acid ester compounds, phosphoric acid compounds, Select from dipic acid compounds, citric acid compounds, ether compounds, and polyester compounds. It is preferable to use at least one of the above-mentioned compounds, for example, bis(2-ethylhexyl) phthalate. ) Dioctyl phthalate, diisononyl phthalate, diisodecyl phthalate, and other di-phthalates butyl benzyl phthalate and other alkyl benzyl phthalates; alkyl aryl phthalates Dibenzyl phthalate Diaryl phthalates Cyclohexane-1,2-dicarboxylic acid Cyclohexanedicarboxylic acid esters such as diisononyl acetate; Tris(2- Trialkyl trimellitates such as ethylhexyl; Trialkyl phosphates such as tricresyl phosphate Aryl;Trialkyl phosphates;Alkyl aryl phosphates;Adipates;Acetyl Ethers such as polypropylene glycol; citric acid esters such as tributyl citrate; Compounds: polyester-based compounds. These can be used alone. Alternatively, a combination of a plurality of them may be used.

[0121] Among them, bis(2-ethylhexyl) phthalate and tris(2-ethylhexyl) trimellitate are one or more selected from the group consisting of diisononyl cyclohexane-1,2-dicarboxylate It is preferable to select The content of plasticizer C2 is 10 to 150 parts by mass per 100 parts by mass of polyvinyl chloride resin. parts by mass, and preferably 30 to 150 parts by mass.

[0122] By adding 10 parts by mass or more of the plasticizer C2, the molecular chains of the vinyl chloride resin are prevented from interfacially bonding. The interaction is sufficiently inhibited, and the distance between the molecular chains of the polyvinyl chloride resin is sufficiently increased, resulting in flexibility. It is possible to give the In addition, by limiting the amount to 150 parts by mass or less, deterioration of mechanical properties, flame retardancy, and electrical properties can be prevented. can be done.

[0123] The polyvinyl chloride resin may contain a stabilizer C3. The stabilizer is a polyvinyl chloride resin. Provides thermal and chemical stability to resins during molding and use in articles This refers to an auxiliary agent. Examples of stabilizer C3 include tribasic lead sulfate, dibasic lead phosphite, Lead-based stabilizers such as basic lead sulfite and lead silicate, potassium, magnesium, barium, zinc, Cadmium, lead and other metals and 2-ethylhexanoic acid, lauric acid, myristic acid, palmitic acid Stearic acid, isostearic acid, hydroxystearic acid, oleic acid, ricin acid Metal soap stabilizers derived from fatty acids such as oleic acid, linoleic acid, and behenic acid; Organotin-based stabilizers having alkyl groups, ester groups, fatty acid groups, maleic acid groups, sulfide-containing groups, etc. Agent: Ba-Zn, Ca-Zn, Ba-Ca-Sn, Ca-Mg-Sn, Ca-Z Complex metal soap stabilizers such as n-Sn, Pb-Sn, and Pb-Ba-Ca; barium , zinc and other metal groups and branched fatty acids such as 2-ethylhexanoic acid, isodecanoic acid, and trialkylacetic acid Fatty acids, unsaturated fatty acids such as oleic acid, ricinoleic acid, linoleic acid, etc., alicyclic acids such as naphthenic acid, etc. Organic acids such as aromatic acids, such as phenolic acid, benzoic acid, salicylic acid, and their substituted derivatives. Metal salt stabilizers, usually derived from two or more metal salts; these stabilizers are used in petroleum hydrocarbons, alcohols, and It is dissolved in organic solvents such as glycerin derivatives and phosphite esters, color inhibitors, and permeability inhibitors. Contains stabilizing agents such as clarity improvers, light stabilizers, antioxidants, bleed-out inhibitors, and lubricants In addition to metal-based stabilizers such as metal salt liquid stabilizers, epoxy resins, epoxidized plants, etc. Oils, epoxy compounds such as epoxidized fatty acid alkyl esters, organic phosphites, etc. These can be used alone or in combination of two or more.

[0124] Among them, the composite metal soap-based stabilizer is preferably used because of its excellent effect as a stabilizer. As the complex metal soap-based stabilizer, Ca is preferable because it does not contain harmful heavy metals. The Ca-Zn stabilizer is a fatty acid salt of calcium and a fatty acid salt of zinc. It is a mixture of fatty acid salts. Specific examples of fatty acids include behenic acid, stearic acid, and lauric acid. Acids include oleic acid, palmitic acid, ricinoleic acid, and benzoic acid. It is also possible to use a combination of two or more elements. The ratio of calcium to zinc is The mass ratio of zinc to calcium is preferably 1:2 to 1:3. If the ratio of zinc is too low, the redness characteristic of calcium salts tends to occur, while if the ratio of zinc is too high, calcium salts tend to be too low. If the ratio is more than 3, zinc chloride produced during molding will act as a decomposition catalyst for vinyl chloride resin. This can result in rapid blackening and decomposition known as "zinc burn."

[0125] Among these, the epoxy compounds are preferably used because of their low volatility. Epoxy compounds include epoxidized soybean oil, epoxidized linseed oil, and epoxidized cottonseed oil. , Epoxidized Peanut Oil, Epoxidized Safflower Oil, Epoxidized Grape Seed Oil, Epoxidized Olive Oil Epoxidized vegetable oils include epoxidized soybean oil. Oil is preferred because of its ready availability.

[0126] In addition, the combination of a complex metal soap stabilizer and an epoxy compound has an excellent effect of improving thermal stability. Therefore, it is preferable to use them in combination. The amount of stabilizer to be added is not particularly limited, but it is preferable to use a stabilizer for 100 parts by weight of polyvinyl chloride resin. Relative to the total weight of the polymer, the amount is preferably 1 to 15 parts by mass, and more preferably 1 to 8 parts by mass. By setting the amount to 15 parts by mass or less, it is possible to suppress thermal decomposition during processing. The deterioration of the mechanical properties of the molded body can be prevented.

[0127] Furthermore, the amount of the complex metal soap-based stabilizer to be added is not particularly limited, but polychlorinated The amount is preferably 1 to 14 parts by mass, more preferably 1 to 14 parts by mass, based on 100 parts by mass of the vinyl resin. 7 parts by mass. By making it 1 part by mass or more, it is possible to suppress thermal decomposition during processing, By adjusting the amount to 4 parts by mass or less, it is possible to prevent a decrease in the mechanical properties of the molded body. Furthermore, the amount of the epoxy compound added is not particularly limited, but polyvinyl chloride-based Preferably, the amount is 1 to 14 parts by mass, more preferably 1 to 7 parts by mass, based on 100 parts by mass of the resin. By making it 1 part by mass or more, it is possible to suppress thermal decomposition during processing, and By setting the content to the range below, deterioration of the mechanical properties of the molded body can be prevented.

[0128] The polyvinyl chloride resin may contain other components as necessary. Examples of such additives include release agents, antioxidants, impact resistance improvers, flexibility improvers, weather resistance improvers, adhesion improvers, etc. Coloring agents, inorganic pigments, organic pigments, carbon black, ferrite, conductive agents, UV absorption agent, infrared absorbing material, lubricant, inorganic filler, reinforcing agent, antiplasticizer, neutralizer, crosslinking agent, flame retardant, antibacterial Examples of such materials include preservatives, insect repellents, fragrances, radical scavengers, sound absorbing materials, and core-shell rubber.

[0129] Examples of the lubricant include liquid paraffin, natural paraffin, microwax, and synthetic paraffin. Fins, low molecular weight polyethylene and other pure hydrocarbon lubricants, halogenated hydrocarbon lubricants, high-grade Fatty acid lubricants such as fatty acids and oxyfatty acids, fatty acid amides, bisfatty acid amides, etc. Mido-based lubricants, lower alcohol esters of fatty acids, polyhydric alcohols of fatty acids such as glycerides Esters, polyglycol esters of fatty acids, fatty alcohol esters of fatty acids (Ester In addition to ester-based lubricants such as lubricants for wax, metal soaps, fatty alcohols, polyhydric alcohols , polyglycols, polyglycerols, partial esters of fatty acids and polyhydric alcohols, fatty acids and polyglycols, partial esters of polyglycerol, silicone oils, etc. These can be used alone or in combination of two or more.

[0130] Among these, the use of the lubricant is preferred since it has an excellent effect of improving moldability. As for lubricants, pure hydrocarbon lubricants, fatty acid amide lubricants, and silicone lubricants are available in terms of ease of availability. Corn oil is preferred. There are no particular restrictions on the amount of lubricant added, but it is recommended that the amount be less than 100 parts by mass of polyvinyl chloride resin. The amount is preferably 0.1 to 15 parts by mass, and more preferably 0.1 to 5 parts by mass. By using 15 parts by mass or more, adhesion of the resin composition to the molding machine can be reduced. By setting the temperature below 100° C., it is possible to prevent deterioration in processability.

[0131] A method of mixing the polyvinyl chloride resin with other components which are added as required. The method is not particularly limited, and a generally known method can be used. For example, Mix using a shell mixer, Banbury mixer, V-type mixer, ribbon blender, etc. This can be obtained by: The average polymerization degree of the resin C is preferably in the range of 300 to 5,000, and more preferably in the range of 500 to 30 By making the average degree of polymerization 300 or more, the mechanical properties of the molded product are improved. In addition, by setting the average degree of polymerization to 5000 or less, the processability becomes good.

[0132] The method for producing the resin C is not particularly limited, and any method, for example, emulsion polymerization, suspension polymerization, solution polymerization, etc., may be used. The polymerization can be carried out by a liquid polymerization method, a bulk polymerization method, or the like. Resin C may contain other components as necessary. Examples of other components include , plasticizer, stabilizer, release agent, antioxidant, impact modifier, flexibility enhancer, weather resistance improver , colorants, inorganic pigments, organic pigments, carbon black, ferrite, conductive agents, ultraviolet rays Absorbents, infrared absorbing materials, lubricants, inorganic fillers, reinforcing agents, antiplasticizers, neutralizing agents, crosslinking agents, flame retardants , preservatives, insect repellents, fragrances, radical scavengers, sound absorbing materials, core-shell rubber, etc. .

[0133] <Molding material> The resin composition of the present invention can be used as a molding material. In addition to extrusion molding using a kneading extruder such as an extruder or a twin screw extruder, a conventional molding method, for example It can also be applied to injection molding, blow molding, roll processing, etc. to obtain various desired molded products. .

[0134] There is no particular restriction on the shape of the molding material, but it is possible to melt-mold a molded body using the molding material. In this case, the copolymer, other polymers, and other polymers to be mixed as necessary are preliminarily used. It is preferable that the components are melt-kneaded and processed into pellets or beads. The molding material of the present invention can be used by appropriately selecting a general method. The production of the material and the production of the molded body described later may be carried out in separate steps or may be carried out continuously. .

[0135] The molding material of the present invention can be produced using a Henschel mixer, a Banbury mixer, or a V Type mixer, ribbon blender, planetary mixer, super mixer, tumbler , single screw extruder, twin screw extruder, multi-screw extruder, co-kneader, planetary gear extruder, plastic The manufacturing process for molding materials is assembled by combining manufacturing equipment such as stictors and roll mixers. It is possible to do so.

[0136] The molding material is made of various materials to prevent the inclusion or adsorption of foreign matter, or the absorption of unnecessary gases. For example, various clean packaging methods can be used to prevent contamination by foreign objects. By applying various coatings to packaging materials to impart gas barrier properties, This can be done.

[0137] <Molded body> The shape of the article (molded body) may be, for example, a sheet, a film, a tube, or a three-dimensional shape. Furthermore, the surface of the molded product may be a mirror surface, or may have a surface irregularity such as a grained or matte surface. The convex processing may be applied to both sides or one side. Also, a protective film or a ceramic may be applied to the surface of the molded product. In addition, various powders can be used to prevent blocking. It can be attached to a surface.

[0138] <Method of manufacturing molded body> The method for producing an article (molded body) by molding the molding material is preferably a melt molding method, e.g. For example, injection molding, compression molding, blow molding, extrusion molding, rotational molding, casting and solvent Among these, injection molding and extrusion molding are preferred from the viewpoint of productivity. There are no particular restrictions on the mold, resin temperature, molding conditions, etc., used when molding using a molding machine. isn't it.

[0139] When manufacturing the molded body, the moisture content of the molding material must be adjusted to the appropriate level, just as when manufacturing the molding material described above. In order to achieve this range, it is preferable to pre-dry the molding material at an appropriate temperature and time. If the temperature is low or the time is short, the molding material containing volatile components is melted and molded. Conversely, if the pre-drying temperature is too high, problems such as foaming and / or poor appearance may occur. If the time is too long, the molding material may deteriorate due to heat, resulting in a decrease in the physical properties of the molded product and / or discoloration. It may be the cause.

[0140] <Processing using molded bodies> Molded products can be bonded or welded to other parts, or sheets, films, or tubes can be bonded to each other. By using the resin composition of the present invention, various products can be manufactured. As the welding method of the molded body, ultrasonic welding, vibration welding, high-frequency welding, hot plate welding, laser welding, spin welding, etc. can be mentioned. As the bonding method of the molded body, epoxy resin-based, acetic vinyl-based, acrylic resin-based, phenolic resin-based, chloroprene rubber-based, nitrile rubber-based , silicone rubber-based, styrene-butadiene rubber-based, cyanoacrylate-based and other various adhesives can be appropriately selected and used. Solvent bonding can also be applied. Furthermore, tape adhesion such as tape attachment or double-sided tape can be performed. When bonding different materials, a plurality of bonding methods can be further combined according to the material to be bonded.

Example

[0141] Hereinafter, the present invention will be described in more detail with reference to examples and comparative examples, but the present invention is not limited to these examples

[0142] <GPC measurement> Mw and Mn were determined using gel permeation chromatography (GPC). The measurement conditions are shown below. Apparatus: HLC-8220 (manufactured by Tosoh Corporation) Column: TSK GUARDCOLUMN SUPER H-H (4.6×35 mm, manufactured by Tosoh Corporation) and two TSK-GEL SUPER HM-H (6.0×150 mm, manufactured by Tosoh Corporation) connected in series Eluent: Tetrahydrofuran Measurement temperature: 40°C Flow rate: 0.6 mL / min

[0143] Mw (weight average molecular weight) and Mn (number average molecular weight) were determined by Polymer Labora Polymethyl methacrylate (Mp (peak molecular weight) = 141,500) manufactured by Tories Calculation was performed using a calibration curve prepared using four types of 55600, 11100, and 1590. The molecular weight distribution was calculated according to the formula "Molecular weight distribution = (mass average molecular weight) / (number average molecular weight)". I put it out.

[0144] <Blocking resistance> Figure 1 shows the equipment used to prepare samples for evaluating blocking resistance. The sample is placed in a cylindrical case 2 having a casing 1, and a top cover 3 is placed on top of the sample. A weight stand 4 is placed on top of the top cover 3. A 5 kg weight 5 was placed on the sample through the wire and the load of the weight 5 (pressure: 20 kPa / cm 2 ) or The sample preparation tool was placed in a gear oven at 50°C for 6 hours, and the block was After the sample was prepared, it was cooled to room temperature and shaken with a shaker. The sample was placed on a sieve (1.4 mm mesh) and shaken at a constant rate. By doing this, the sample block is broken down, and the time and the amount of broken blocks (received) are recorded. The amount of powder in the test piece was measured at regular intervals. The time it took for 35% of the blocks (7g) to break was 35%. The time required for 50% of the blocks (10g) to break was defined as the 50% time required for the blocks to break. The kingliness was evaluated. If 50% of the blocks do not crumble after 20 minutes, the 50% crushing time cannot be measured. Therefore, blocking resistance is judged to be insufficient.

[0145] <Water absorption rate> The mixture was pressed in a press at 180°C and 18 MPa for 5 minutes to produce a 1 mm thick molded body. The water absorption of the obtained molded product was measured in accordance with JISK 7209:2000. The amount of water absorption of each sample was measured by first drying each sample at 50°C for 24 hours and then measuring the weight (W 1) was measured, and then the dried sample was soaked in ion-exchanged water at 100°C for 30 minutes. After immersion, the weight (W2) of the sample was measured again, and the weight change (W2-W1) was calculated. Ta. <Checking the coating condition> The surface of the resin composition is observed with an optical microscope (×100 to ×300), and a part of the surface is If it was covered with particles, it was considered to be coated.

[0146] <Production Example 1: Synthesis of Dispersant (1)> In a reaction vessel equipped with a stirrer, a condenser and a thermometer, 6 ml of a 17% by mass aqueous solution of potassium hydroxide was added. 1.6 parts of ethyl acetate, 19.1 parts of methyl methacrylate, and 19.3 parts of deionized water were then charged. The liquid in the reactor was stirred at room temperature, and after the exothermic peak was confirmed, the liquid was stirred for 4 hours. Thereafter, the reaction solution in the reactor was cooled to room temperature to obtain an aqueous solution of potassium methacrylate.

[0147] Next, 900 parts of deionized water, 42 % by weight of 2-sulfoethyl sodium methacrylate aqueous solution (manufactured by Mitsubishi Chemical Corporation, product name: A 70 parts of Cryester SEM-Na, 16 parts of the above potassium methacrylate aqueous solution and 10 parts of methacrylate. Add 7 parts of ethyl methacrylate and stir. While replacing the inside of the polymerization apparatus with nitrogen, The temperature was raised to 50°C. V-50 (FUJIFILM Wako Pure Chemical Industries, Ltd.) was added as a polymerization initiator to the polymerization apparatus. 2,2'-azobis(2-methylpropionamidine) dihydrochloride (trade name, manufactured by Epson Corporation) 0.0 53 parts of the polymerization initiator was added, and the temperature of the liquid in the reactor was raised to 60°C. After the polymerization initiator was added, Add 1.4 parts of ethyl methacrylate in 5 separate additions (total amount of methyl methacrylate: 7 parts) After that, the liquid in the polymerization apparatus was stirred and kept at 60°C for 6 hours, and then cooled to room temperature. Thus, a dispersant (1) was obtained as a transparent aqueous solution having a solid content of 8 mass %.

[0148] <Production Example 2: Synthesis of Chain Transfer Agent (1)> In a synthesis apparatus equipped with a stirrer, cobalt(II) acetate tetrahydrate (rich 2.00 g (8.03 mmol) of 1,2-diphenyl glycine (Wako Pure Chemical Industries, Ltd., special grade) and 3.86 g (16.1 mmol) of oxime (Tokyo Chemical Industry Co., Ltd., EP grade) and nitrogen 100 ml of diethyl ether that had been deoxygenated by stirring was added, and the mixture was stirred at room temperature for 2 hours. Next, 20 ml of boron trifluoride diethyl ether complex (Tokyo Chemical Industry Co., Ltd., EP grade) The mixture was then stirred for another 6 hours. The obtained mixture was filtered, and the solid was washed with diethyl ether. , 100MPa or less, dried at 20℃ for 12 hours, brown solid chain transfer agent (1) The product was obtained in an amount of 5.02 g (7.93 mmol, 99% yield).

[0149] <Production Example 3: Synthesis of Macromonomer (d'-1)> In a polymerization apparatus equipped with a stirrer, a condenser, and a thermometer, 135 parts of deionized water, 10 parts of sodium sulfate, 0.1 parts of Na2SO4 and the dispersant (1) (solid content 10% by mass) produced in Production Example 1 0.26 parts by mass of methyl methacrylate was added and stirred to obtain a uniform aqueous solution. 5 parts by mass of methyl acrylate, 5 parts by mass of the chain transfer agent (1) produced in Production Example 2 As a polymerization initiator, Perocta O (NOF Corp., 1,1,3,3-tetramethylbutane) was used. 0.1 parts by mass of ethylperoxy-2-ethylhexanoate (trade name) was added to the aqueous dispersion. It was decided.

[0150] Next, the inside of the polymerization apparatus was thoroughly replaced with nitrogen, the aqueous dispersion was heated to 80°C, and then kept for 3 hours. After that, the reaction mixture was cooled to 40°C and cooled to 90°C for 2 hours. The aqueous suspension was filtered through a filter cloth, and the filtrate was poured into deionized water. The mixture was washed with water and dried at 40°C for 16 hours to obtain macromonomer (d'-1). The Mw of mer (d'-1) was 36,000 and the Mn was 15,000.

[0151] <Production Example 4 Polymer B-1> In a reaction vessel equipped with a stirrer, a condenser and a thermometer, 280 parts of deionized water, 1 part of alkenyl chloride, Dipotassium chloride 1 part, potassium persulfate 0.12 parts, methyl methacrylate 40 parts, butyrate A mixture of 2 parts of ethyl acrylate and 0.0057 parts of n-octyl mercaptan was charged. After replacing the inside of the vessel with nitrogen, the reaction vessel was heated to 65° C. with stirring and heated and stirred for 2 hours. Then, 44 parts of methyl methacrylate and 44 parts of butyl acrylate were added to the reaction vessel. A mixture of 14 parts of ethyl acetate was added over a period of 1 hour, and after the addition was completed, stirring was continued for 2 hours. The polymerization was then completed to obtain a latex of polymer B. The Mw of the obtained polymer B was 1,500,000. The median diameter was 100 nm and the water absorption rate was 2.5%.

[0152] <Production Example 5 Polymer B-2> After replacing the inside of a reaction vessel equipped with a stirrer and a reflux condenser with nitrogen, add 230 parts of ion-exchanged water. , Sodium dioctyl sulfosuccinate 1.0 parts, Potassium persulfate 0.15 parts, Methacrylate 85 parts of methyl acrylate, 15 parts of n-butyl acrylate and 0.0 parts of n-octyl mercaptan 175 parts of the mixture was charged, the atmosphere in the vessel was replaced with nitrogen again, and the reaction vessel was heated to 600° C. with stirring. The temperature is raised to 5°C and the mixture is stirred for 2 hours to complete the polymerization reaction. The mixture is then cooled to obtain a latex of polymer (B-2). A part of the obtained latex was added to an aqueous solution of aluminum chloride to cause salting out and coagulation. After that, the polymer was washed and dried to obtain a polymer (B-2). The Mw was 1,600,000, the median diameter was 76 μm, and the water absorption was 2.7%.

[0153] <Production Example 6 Polymer B-3> A reaction vessel equipped with a stirrer and a reflux condenser is charged with 150 parts of ion-exchanged water, and sodium carbonate anhydride is added thereto. Add 0.1 parts of thorium, 80 parts of methyl methacrylate, and 20 parts of n-butyl methacrylate. The atmosphere in the container was replaced with nitrogen. Then, 1.1 parts of sodium dodecyl sulfate was added and stirred. The reaction vessel was heated to 43°C under the above conditions, and 0.15 parts of potassium persulfate was added to initiate the polymerization reaction. After that, the mixture was heated and stirred for 2 hours to complete the polymerization, and polymer B-3 was obtained. The Mw of the obtained polymer was 3,000,000, the median diameter was 195 μm, and the water absorption was 2.4%.

[0154] <Production Example 7 Polymer B-4> 5 liter, 4-neck flask equipped with a thermometer, nitrogen gas inlet, stirring rod, dropping funnel and cooling tube Put 952g of pure water into a flask, and pass nitrogen gas through it for 60 minutes to measure the dissolved oxygen in the pure water. After stopping the nitrogen gas flow, 45.6 g of methyl methacrylate and n-butyl ether were added. 34.9 g of dimethacrylate was added, and the temperature was raised to 80° C. while stirring at 180 rpm. When the temperature reaches 80°C, add 0.28g of potassium persulfate dissolved in 35g of pure water at once. The mixture was stirred at 80°C for 60 minutes and the seed solution was added. A particle dispersion was obtained. Next, sodium dialkyl sulfosuccinate (Kao Add 0.70 g of PELEX O-TP (manufactured by PELEX Co., Ltd.) and 49 g of pure water, and mix. In addition, a monomer emulsion (methyl methacrylate 555.5 g, n-butyl methacrylate Rate 425.5g, glycidyl methacrylate 7.0g, AIBN (FUJIFILM Wako Junyaku Co., Ltd., 2,2'-azobis(isobutyronitrile) 0.42 g, PELLEX OT P9.80g and 490.0g of pure water were mixed and stirred to form an emulsion, and the mixture was added dropwise over a period of 3 hours. The mixture was then stirred at 80° C. for 1 hour to obtain a first polymer dispersion. To this first dripped polymer dispersion, 2.80 g of potassium persulfate was added, and the monomer emulsion was further Solution (methyl methacrylate 383.4g, methacrylic acid 36.6g, thioglycolic acid 36.6g) 1.12g of octyl (manufactured by Yodo Chemical Co., Ltd., trade name: OTG), sodium dialkyl sulfosuccinate 8.2 g of sodium (Kao Corporation, product name: Pelex O-TP) and 350.0 g of pure water were Mix and stir to emulsify) and add dropwise over 1.5 hours, then stir at 80°C for 1 hour. The above was continued to obtain a second polymer dispersion. The obtained second polymer dispersion was cooled to room temperature and then sprayed with a spray dryer (Okawahara Chemical The inlet temperature was 150°C, the outlet temperature was 65°C, and the atomizer The mixture was spray-dried at a rotation speed of 20,000 rpm to obtain a powdered polymer B-4. The Mw was 2,000,000, the median diameter was 52 μm, and the water absorption was 3.4%.

[0155] <Example 1> In a reaction vessel equipped with a stirrer, a condenser and a thermometer, 145 parts of deionized water, 10 parts of sodium sulfate, 0.36 parts of dispersant (1) produced in Production Example 1, 1.25 parts of dispersant (1) produced in Production Example 3, 40 parts of monomer (d'-1), methoxyethyl acrylate (Osaka Organic Chemical Industry Co., Ltd.) 60 parts of n-octyl mercaptan (trade name, manufactured by Kanto Chemical Co., Ltd.) and 0.2 parts of n-octyl mercaptan were charged and stirred. The composition was then cooled to 40°C or lower. After that, V601 (Dimethyl 2,2'-azobis( 2-Methylpropionate (trade name) 0.12 parts was dissolved and polymerized in a syrup dispersion state. A sexual composition was obtained.

[0156] Next, the syrup dispersion was heated to 75°C and held for 2 hours. After that, the temperature was raised to 85°C. The suspension was cooled to 40° C. or lower, and polymer A in a syrup-dispersed state was obtained. The obtained syrup was filtered, the filtrate was washed with deionized water, and dried at 50°C for 12 hours. The bead-shaped (meth)acrylic copolymer obtained had an Mn of 56,000 and an Mw of 30. 0000 and the water absorption rate was 6.2%.

[0157] To the polymer A, 7.6 parts of the polymer B obtained in Production Example 4 was added with stirring, and the mixture was heated to 75° C. The temperature was raised to 40°C and held for 30 minutes. After that, the mixture was cooled to 40°C or lower, filtered, and the filtrate was poured into deionized water. The resin composition (AB) was obtained by washing with water and drying at 50°C for 12 hours. It was confirmed that the surface of composition (AB) was coated. The obtained resin composition (AB) was used to evaluate blocking properties. The results are shown in Table 1. showed.

[0158] <Comparative Example 1> The (meth)acrylic copolymer A in the syrup dispersion state of the above example was filtered, and the filtrate was Wash with deionized water and dry at 50°C for 12 hours to obtain beads of (meth)acrylic copolymer. The blocking agent (Mn is 56,000, Mw is 300,000, and water absorption is 6.2%) A property evaluation was carried out, and the results are shown in Table 1.

[0159] <Example 2> 98 parts of the bead-shaped (meth)acrylic copolymer A of Comparative Example 1, The polymer (B-2) (2 parts) was fed to a Henschel mixer and mixed uniformly to obtain a resin composition ( An optical microscope revealed that the surface of the resin composition (AB-2) was coated. The obtained resin composition (AB-2) was used to evaluate the blocking property. The results are shown in Table 1.

[0160] <Comparative Example 2> Instead of the polymer (B-2) obtained in the above-mentioned Production Example 5, the polymer (B-3) obtained in the above-mentioned Production Example 6 A resin composition (AB-3) was obtained in the same manner as in Example 2, except that (B-3) was used. It was confirmed by an optical microscope that the surface of the resin composition (AB-3) was coated. The resin composition (AB-3) was used to evaluate blocking properties, and the results are shown in Table 1. Ta.

[0161] <Comparative Example 3> Instead of the polymer (B-2) obtained in the above Production Example 5, the polymer (B-3) obtained in the above Production Example 7 A resin composition (AB-4) was obtained in the same manner as in Example 2, except that (B-4) was used. The obtained resin composition (AB-4) was used to evaluate blocking properties. The results are shown in Table 1. As shown in.

[0162] [Table 1]

[0163] Comparative Example 1 in which polymer B was not used, and polymer B-3 having a weight average molecular weight of 3,000,000 In Comparative Example 2, where the water absorption rate of the polymer B-4 was 3.4%, and in Comparative Example 3, where the water absorption rate of the polymer B-4 was 3.4%, the blocking resistance was insufficient. It was minutes. [Industrial Applicability]

[0164] The resin composition of the present invention is easy to handle during storage and molding, and is easy to dry during molding. It is possible to reduce the amount. [Explanation of symbols]

[0165] 1 Bottom lid 2 Cases 3 Top lid 4. Weight stand 5. Weight

Claims

1. The surface of the (meth)acrylic copolymer A having a water absorption rate of 5% or more is A (meth)acrylic copolymer B having an average molecular weight of 500,000 or more and 2,500,000 or less. A coated resin composition.

2. The (meth)acrylic copolymer B was added in an amount of 0. The resin composition according to claim 1, comprising 0.1 part by mass or more and 5 parts by mass or less of the polyvinyl chloride.

3. 2. The (meth)acrylic copolymer B has a particle size of 1 nm or more and 20 μm or less.

3. The resin composition according to claim 2.

4. The (meth)acrylic copolymer B has a glass transition temperature (Tg) of 60° C. or higher. Item 3. The resin composition according to item 1 or 2.

5. The (meth)acrylic copolymer A is a (meth)acrylic copolymer A1 and the ( Block containing (meth)acrylic copolymer A2 different from (meth)acrylic copolymer A1 3. The resin composition according to claim 1, which is a copolymer or a graft copolymer.

6. The (meth)acrylic copolymer A1 contains a monomer unit a1 represented by the following formula (1): The resin composition according to claim 5 . 【Chemistry 1】 (In the formula, R 3 represents a hydrogen atom or a methyl group, R 4 represents an alkylene group having 1 to 4 carbon atoms. S, R 5 represents a hydrocarbon group having 1 to 6 carbon atoms, and p is a natural number from 1 to 10.

7. The (meth)acrylic copolymer A1 contains, in a total of 100% by mass of the monomer units, The resin composition according to claim 6, wherein the proportion of the monomer unit a1 is 70 mass % or more.

8. The monomer unit a1 is methoxymethyl acrylate, methoxyethyl acrylate, Methoxypropyl acrylate, Methoxybutyl acrylate, Methoxypolyethylene Licorice acrylate, methoxymethyl methacrylate, methoxyethyl methacrylate , methoxypropyl methacrylate, methoxybutyl methacrylate, methoxypolyethylene The compound is derived from at least one monomer selected from the group consisting of ethylene glycol methacrylate. The resin composition according to claim 6, wherein the monomer unit is a monomer unit derived from the above-mentioned monomer unit.

9. The (meth)acrylic copolymer A2 has a glass transition point (Tg) of 50 to 150° C. The resin composition according to claim 5 .

10. The polymer A2 is composed of monomer units a2, The monomer unit a2 is a hydrocarbon group-containing (meth)a monomer having a hydrocarbon group having 1 to 12 carbon atoms. A monomer unit derived from at least one monomer selected from the group consisting of acrylates. The resin composition according to claim 5 .

11. The polymer A2 is composed of monomer units a2, The monomer unit a2 includes a monomer unit derived from methyl methacrylate. The resin composition described above.

12. The polymer A2 contains a unit derived from a macromonomer d′ represented by the following formula (2): The resin composition according to claim 5. 【Chemistry 2】 (In formula (2), R 0 ~R n each independently represents a hydrogen atom, an unsubstituted or substituted an alkyl group having an unsubstituted or substituted alicyclic group; an alicyclic group having an unsubstituted or substituted aryl groups having a substituent, unsubstituted or substituted heteroaryl groups, or unsubstituted or or a non-aromatic heterocyclic group having a substituent, 0 ~R n are the same may also be different, X 1 ~X n represents a hydrogen atom or a methyl group, and a plurality of X 1 ~X n Haso may be the same or different, Z is a terminal group, and n is a natural number from 2 to 10,000. 。)

13. A molding material comprising the resin composition according to claim 1 or 2.

14. An article molded from the molding material according to claim 13.

Citation Information

Patent Citations

  • Polymer powder

    JP2019006896A