Moisture absorbent

A moisture absorbent using a combination of ionic liquids with phosphate ester/phosphate and carboxylate ions addresses the inefficiencies of existing absorbents by improving water vapor absorption and release, enhancing energy efficiency in dry water electrolysis and air conditioning applications.

JP2024139723APending Publication Date: 2024-10-09NIPPON CHEMICAL IND CO LTD
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2024037113
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-11
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Existing moisture absorbents used in dry water electrolysis gas production and air conditioning equipment face challenges in achieving high water vapor absorption and release efficiency, particularly at low temperatures, and require significant energy for regeneration.

Method used

A moisture absorbent composed of two specific types of ionic liquids, one with a phosphate ester or phosphate ion anion and another with a carboxylate ion having an amino group or nitrogen-containing heterocycle, enhances water vapor absorption and release properties.

Benefits of technology

The absorbent exhibits superior water vapor absorption and release capabilities, reducing energy consumption and enabling efficient operation in dry water electrolysis gas production and air conditioning systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139723000001
    Figure 2024139723000001
  • Figure 2024139723000002
    Figure 2024139723000002
  • Figure 2024139723000003
    Figure 2024139723000003
Patent Text Reader

Abstract

To provide a moisture absorbent that exhibits superior water vapor absorptivity.SOLUTION: A moisture absorbent includes the following ionic liquid (A) and ionic liquid (B). Ionic liquid (A): an ionic liquid where the anion component is a phosphate ion or a phosphoric acid ion. Ionic liquid (B): an ionic liquid where the anion component is a carboxylate ion with an amino group or a carboxylate ion with a nitrogen-containing heterocycle. As the cation components of the ionic liquid (A) and ionic liquid (B), ammonium ions, phosphonium ions and imidazolium ions are preferable, with phosphonium ions being more preferable.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a moisture absorbent, and more particularly to a moisture absorbent used in a dry water electrolysis gas production device, an air conditioning device, or the like. [Background technology]

[0002] Renewable energy sources such as solar and wind power are valuable energy resources. However, suitable locations for sunlight and wind conditions are unevenly distributed, and the locations where these sources can be obtained are often far from consumption areas, and the amount of generated power varies depending on the season and time. For this reason, methods for converting renewable energy sources into hydrogen and using them to adjust the location, amount, and timing are being researched. For example, there are methods for producing hydrogen by electrolyzing water, such as alkaline water electrolysis and solid polymer water electrolysis.

[0003] The electrolytic gas obtained by these water electrolysis processes is hydrogen gas from the anode side and oxygen gas from the cathode side. Unlike the hydrogen gas obtained by steam reforming of hydrocarbons, it does not contain by-products such as carbon dioxide, but it does contain the water vapor that is the raw material. For this reason, depending on the application, it may be necessary to remove this to achieve high purification.

[0004] Common gas dehumidification processes include a process in which a gas mixture containing water vapor is cooled in a chiller to lower the dew point, and a process in which a gas mixture containing water vapor is brought into contact with an adsorbent or absorbent.

[0005] In the dehumidification process in which a mixed gas containing water vapor is brought into contact with an adsorbent or absorbent, there are methods using solid adsorbents and liquid absorbents. When dehumidification is performed using a solid adsorbent such as zeolite, a high temperature (up to 200°C) heat treatment is required to regenerate the solid adsorbent that has absorbed moisture. Therefore, if this dehumidification process is applied to electrolytic gas, which contains a large amount of moisture, a large amount of energy is required. In addition, dehumidification using solid adsorbents is generally performed in batches (two-cylinder or multi-cylinder type). This batch process requires that the entire batch processing unit be heated each time and then cooled. Furthermore, since heat exchange is difficult in this process, a large amount of energy is required.

[0006] As a liquid absorbent, triethylene glycol (TEG) is known as a gas absorbent and air humidity conditioner. However, when trying to use TEG as an absorbent, the absorbent itself has a vapor pressure, which hinders the high purification of hydrogen. In addition, TEG is flammable, which makes it unsuitable for hydrogen gas or oxygen gas, and other issues arise.

[0007] To solve these problems, for example, Patent Document 1 discloses that an ionic liquid is useful as a liquid absorbent, and Patent Document 2 discloses that an absorbing liquid containing an ionic liquid and an inorganic salt is useful.

[0008] In addition, in desiccant-type air conditioners, a moisture absorbent (desiccant) that has the property of absorbing water vapor in the air is used. Ionic liquids have been proposed as such moisture absorbents, and are said to have excellent moisture absorption properties and to have no odor or metal solubility. For example, Patent Document 3 discloses a moisture absorbent containing a phosphonium cation and a phosphate ester anion. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2018-51543 A [Patent Document 2] JP 2019-202917 A [Patent Document 3] JP 2020-6349 A Summary of the Invention [Problem to be solved by the invention]

[0010] The ionic liquid disclosed in Patent Document 1 is composed of a cation and an anion, and the cation is not particularly limited, but examples thereof include imidazolium salts, pyrrolidinium salts, piperidinium salts, pyridinium salts, morpholinium salts, ammonium salts, phosphonium salts, and sulfonium salts. Among them, imidazolium salts are preferred. The anion is not particularly limited, but an oxoacid ion is preferred, and examples thereof include carboxylic acid, nitric acid, sulfuric acid, sulfonic acid, phosphoric acid ester, phosphoric acid, phosphonic acid ester, and phosphonic acid.

[0011] Furthermore, Patent Document 2 describes that an absorption liquid containing an ionic liquid and an inorganic salt is useful, and specifically describes that a combination of methyltributylphosphonium dimethylphosphate as the ionic liquid and lithium acetate or calcium acetate, calcium chloride, lithium chloride, calcium nitrate, lithium nitrate, or lithium bromide as the inorganic salt is preferable. However, in order to produce dry electrolytic gas, water is electrolyzed to generate electrolytic gas containing hydrogen and oxygen. However, such electrolytic gas contains water vapor derived from the raw materials, and it is necessary to perform gas-liquid separation of the rich absorbent in which the water vapor has been selectively absorbed into the absorbent. Although the above-mentioned ionic liquids have excellent water absorption capacity, there is a demand for further water absorption capacity. In addition, since it is necessary to separate absorbed water at low temperatures, there is a demand for further separation capacity.

[0012] Patent Document 3 discloses that compounds containing phosphonium cations and phosphate ester anions, particularly tributylmethylphosphonium dimethylphosphonate, are excellent in terms of hygroscopicity, odor, metal solubility, and practical application as ionic liquids. However, although these ionic liquids have excellent hygroscopicity, further water absorption ability is required.

[0013] SUMMARY OF THE PRESENT EMBODIMENT An object of the present invention is to provide a moisture absorbent having excellent water vapor absorbing properties. [Means for solving the problem]

[0014] The present inventors have conducted intensive research in light of the above-mentioned circumstances and have found that a moisture absorbent using two specific types of ionic liquids has excellent water vapor absorption and release properties, thereby completing the present invention.

[0015] The present invention relates to a moisture absorbent containing the following ionic liquid (A) and ionic liquid (B). Ionic liquid (A): An ionic liquid whose anion component is a phosphate ester ion or a phosphate ion. Ionic liquid (B): An ionic liquid in which the anion component is a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle. Effect of the Invention

[0016] According to the present invention, it is possible to provide a moisture absorbent having excellent water vapor absorption properties. Furthermore, it is possible to provide a moisture absorbent that is useful as a moisture absorption and release agent having excellent water vapor release properties in addition to the above properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0017] The moisture absorbent of the present invention contains the following ionic liquid (A) and ionic liquid (B). Ionic liquid (A): An ionic liquid whose anion component is a phosphate ester ion or a phosphate ion. Ionic liquid (B): An ionic liquid in which the anion component is a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle. In the present invention, the ionic liquid refers to a liquid salt composed of a cationic component and an anionic component.

[0018] The cationic components constituting the ionic liquid (A) and the ionic liquid (B) are not particularly limited, and examples thereof include imidazolium ions, pyrrolidinium ions, piperidinium ions, pyridinium ions, morpholinium ions, ammonium ions, phosphonium ions, and sulfonium ions. The cationic components of the ionic liquid (A) and the ionic liquid (B) may be the same or different. The cationic components may contain two or more types of ions.

[0019] Among these, from the viewpoint of hygroscopicity (hereinafter also referred to as water vapor absorbency), ammonium ions, phosphonium ions and imidazolium ions are preferred, phosphonium ions are more preferred, and phosphonium ions represented by the following general formula (I) are particularly preferred.

[0020] [ka] (In the formula, R 1 , R 2 , R 3 and R 4 each independently represents a linear alkyl group, a branched alkyl group, or a cyclic alkyl group having 1 to 20 carbon atoms.

[0021] R 1 , R 2 , R 3 and R 4Examples of the linear alkyl group having 1 to 20 carbon atoms represented by the formula (I) include a methyl group, an ethyl group, a n-propyl group, a n-butyl group, a n-pentyl group, a n-hexyl group, a n-heptyl group, a n-octyl group, a n-nonyl group, a n-decyl group, a n-undecyl group, a n-tridecyl group, a n-tetradecyl group, a n-pentadecyl group, a n-hexadecyl group, a n-heptadecyl group, a n-octadecyl group, a n-nonadecyl group, and a n-icosyl group.

[0022] R 1 , R 2 , R 3 and R 4 Examples of the branched alkyl group having 1 to 20 carbon atoms represented by the formula (I) include an isopropyl group, an isobutyl group, an s-butyl group, a t-butyl group, an isopentyl group, an s-pentyl group, a t-pentyl group, an isohexyl group, an s-hexyl group, a t-hexyl group, and an ethylhexyl group.

[0023] R 1 , R 2 , R 3 and R 4 Examples of the cyclic alkyl group having 1 to 20 carbon atoms represented by the formula (I) include a cyclopropyl group, a cyclobutyl group, a cyclopentyl group, a cyclohexyl group, a 2-methylcyclopentyl group, a 3-methylcyclopentyl group, a cycloheptyl group, a 2-methylcyclohexyl group, a 3-methylcyclohexyl group, a 4-methylcyclohexyl group, a cyclooctyl group, a 2-methylcycloheptyl group, a 3-methylcycloheptyl group, a 4-methylcycloheptyl group, and a 5-methylcycloheptyl group.

[0024] R 1 , R 2 , R 3 and R 4 From the viewpoint of hygroscopicity, R is preferably a linear or branched alkyl group having 1 to 15 carbon atoms, more preferably a linear alkyl group having 1 to 10 carbon atoms, and particularly preferably a linear alkyl group having 1 to 6 carbon atoms. 1 , R 2 , R 3 and R 4may be the same or different.

[0025] As the phosphonium ion represented by the general formula (I), a methyltributylphosphonium ion and a tetrabutylphosphonium ion are preferred.

[0026] The anion component of the ionic liquid (A) is a phosphate ester ion or a phosphate ion, and the anion component of the ionic liquid (B) is a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle. By containing these two types of ionic liquids, the moisture absorbent has excellent water vapor absorption properties and also has excellent moisture release properties (hereinafter also referred to as water vapor release properties), that is, the moisture absorbent has moisture absorption and release properties.

[0027] The phosphate ester ion or phosphate ion, which is the anion component of the ionic liquid (A), is an ion represented by the following general formula (II).

[0028] [ka] (In the formula, R 5 and R 6 each independently represents a hydrogen atom, or a linear alkyl group, a branched alkyl group, or a cyclic alkyl group having 1 to 20 carbon atoms.

[0029] R 5 and R 6 The linear alkyl group, branched alkyl group and cyclic alkyl group having 1 to 20 carbon atoms represented by the following formula (I) have the same meanings as those in the above formula (I).

[0030] In the general formula (II), R 5 and R 6is a hydrogen atom, the anion component is a phosphate ion, when one is a hydrogen atom and the other is a hydrocarbon group the anion component is a monoalkyl phosphate ion, and when both are hydrocarbon groups the anion component is a dialkyl phosphate ion. In the present invention, the anion component of the ionic liquid (A) is preferably a dialkyl phosphate ion.

[0031] R 5 and R 6 From the viewpoint of moisture absorption and moisture absorption / desorption properties, R is preferably a linear or branched alkyl group having 1 to 10 carbon atoms, more preferably a linear alkyl group having 1 to 5 carbon atoms, and particularly preferably a linear alkyl group having 1 to 3 carbon atoms. 5 and R 6 may be the same or different, but are preferably the same from the viewpoint of synthesis.

[0032] R 5 and R 6 Examples of dialkyl phosphate in which is a linear or branched alkyl group having 1 to 10 carbon atoms include dimethyl phosphate, diethyl phosphate, dibutyl phosphate, bis(2-ethylhexyl) phosphate, etc. In the present invention, dimethyl phosphate is particularly preferred.

[0033] Examples of carboxylate ions having an amino group, which are the anion components of the ionic liquid (B), include anions of natural amino acids, and specific examples thereof include anions such as L-asparagine, L-aspartic acid, DL-alanine, β-alanine, D-alanine, L-alanine, L-arginine, L-isoleucine, glycine, L-glutamine, L-glutamic acid, L-cysteine, DL-serine, L-serine, L-tyrosine, L-tryptophan, L-threonine, L-valine, L-histidine, L-phenylalanine, L-proline, L-methionine, L-lysine, and L-leucine.

[0034] Examples of the carboxylate ion having a nitrogen-containing heterocycle include anions of L-proline, L-pyroglutamic acid, α-methylproline, and cis-4-hydroxy-L-proline.

[0035] In the present invention, from the viewpoint of hygroscopicity and moisture absorption / release properties, the anion component of the ionic liquid (B) is preferably an anion of an amino acid selected from DL-alaninate, D-alaninate, L-alaninate, β-alaninate, glycinate, L-prolinate and DL-serinate, and is particularly preferably an anion of an amino acid selected from DL-alaninate, D-alaninate, L-alaninate, β-alaninate and glycinate.

[0036] The ionic liquid (A) and ionic liquid (B) used in the present invention can be produced, for example, by reacting a trialkylphosphine with an alkyl halide under an inert gas atmosphere to obtain a phosphonium salt whose anion is a halogen, followed by neutralization and oxidation treatment as desired, and then dropping and mixing a desired anion component into the obtained phosphonium salt to perform anion exchange.

[0037] In the anion exchange, the ionic liquid (A) used in the present invention can be produced by using an anion component containing a phosphate ester ion or a phosphate ion, and the ionic liquid (B) used in the present invention can be produced by using an anion component containing a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle.

[0038] In addition, in terms of ease of adjusting the mixing molar ratio, it is preferable to separately produce ionic liquid (A) produced using an anion component consisting of a phosphate ester ion or a phosphate ion, and ionic liquid (B) produced using an anion component consisting of a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle, and then mix these to produce the moisture absorbent of the present invention.

[0039] The mixing molar ratio of the ionic liquid (A) to the ionic liquid (B) is preferably from 95:5 to 5:95, more preferably from 92:8 to 28:72, the former:the latter being in the above range, and the resulting moisture absorbent is excellent in moisture absorption and release properties, and is therefore suitable not only as a moisture absorbent but also as a moisture absorbing and releasing agent.

[0040] In addition, the moisture absorbent of the present invention may contain, in addition to the ionic liquid (A) and the ionic liquid (B), an ionic liquid other than the ionic liquid (A) or the ionic liquid (B), another moisture absorbent, or other components used in ordinary moisture absorbents, so long as the effects of the present invention are not adversely affected.

[0041] As shown in the Examples, the moisture absorbent of the present invention has a faster molar moisture absorption rate, calculated by calculating the moisture absorption rate per mole of each moisture absorbent until the relative humidity is reduced by half, compared to a moisture absorbent using ionic liquid (A) or ionic liquid (B) alone, due to the synergistic effect of ionic liquid (A) and ionic liquid (B). Furthermore, compared to moisture absorbents that use the conventional ionic liquid methyltributylphosphonium dimethyl phosphate, the absorbed water vapor can be released at a lower heating temperature, and the moisture release properties are also excellent. Furthermore, the moisture absorbent of the present invention can be reused as a moisture absorbent after releasing all or a part of the absorbed water vapor.

[0042] The moisture absorbent of the present invention can be used in a dry water electrolysis gas production apparatus, etc. For example, these apparatuses are disclosed in JP-A-2018-51543, JP-A-2019-202917, JP-A-2021-7938, etc. The present invention can also be used in devices such as air conditioners and absorption refrigerators. For example, these devices are disclosed in JP-A-2006-142121, JP-A-2018-144029, JP-A-2020-30004, etc. The moisture absorbent of the present invention is preferably used in devices such as dry water electrolysis gas producing devices and air conditioners. EXAMPLES

[0043] The present invention will be described in more detail below by way of examples, but the present invention is not limited thereto.

[0044] [Production Example 1] A 5 cm diameter glass column was filled with 400 ml of ion exchange resin (Organo Corporation, Amberlite IRA400(OH)HG), and 200 ml of pure water was passed through it from above at a rate of SV=1.0 using a tube pump. Next, an aqueous solution of 33.9 g (0.1 mol) of tetrabutylphosphonium bromide (Nihon Kagaku Kogyo, Hishicoline PX-4B) dissolved in 400 ml of pure water was passed through the column from above at a rate of SV=1.0, and then 300 ml of pure water was passed through to obtain 690.5 g of an aqueous solution of tetrabutylphosphonium hydroxide. The concentration was 3.7% (crude yield 92.4%) when neutralized with 0.1 N hydrochloric acid. The residual bromide concentration was 540 ppm when titrated with 0.1 N silver nitrate. The ion exchange resin was regenerated by pumping 400 ml of 0.1 mol / L sodium hydroxide solution from above at a rate of SV=1.0 using a tube pump, followed by 300 ml of pure water. Similarly, 33.9 g (0.1 mol) of tetrabutylphosphonium bromide (Nihon Kagaku Kogyo, Hishicolin PX-4B) dissolved in 400 ml of pure water was pumped from above the column at a rate of SV=1.0, followed by 300 ml of pure water. This operation was repeated 10 times in total to obtain 7150 g (93.1% crude yield) of tetrabutylphosphonium hydroxide solution with an average concentration of 3.6%. The residual bromide concentration was 500 ppm by titration with 0.1 N silver nitrate.

[0045] The resulting aqueous solution of tetrabutylphosphonium hydroxide (614 g, 0.08 mol) and an aqueous solution of β-alanine (7.1 g, 0.08 mol) dissolved in 100 ml of pure water were mixed at room temperature under stirring. The resulting mixed aqueous solution was concentrated under reduced pressure using an evaporator, and the concentrated solution was mixed with methanol to form a methanol solution, which was dehydrated overnight using anhydrous magnesium sulfate. The dehydrated methanol solution was concentrated under reduced pressure using an evaporator to obtain 27.5 g (crude yield 99.0%) of a colorless, transparent, viscous liquid, compound 2. The water content measured by the Karl Fischer method was 5702 ppm. The NMR identification data of the obtained compound 1 are as follows: (Identification data) 31 P-NMR: 33.10 ppm 1 H-NMR; 0.98 ppm (t, 12H, -CH 3 ), 1.51~1.58ppm(m,16H,-CH 2 -), 2.29 ppm (t, 2H, -C(=O)-CH 2 -), 2.39~2.44(m,8H,P-CH 2 -), 2.87(t,2H,-CH 2 -NH 2 ), 3.35(s,2H,-NH 2 ) As a result, compound 1 was confirmed to be tetrabutylphosphonium β-alaninate.

[0046] [Production Example 2] 614g (0.08 mol) of the aqueous solution of tetrabutylphosphonium hydroxide obtained in the same manner as in Preparation Example 1 and an aqueous solution in which 6.0g (0.08 mol) of glycine was dissolved in 100ml of pure water were mixed at room temperature with stirring. The resulting mixed aqueous solution was concentrated under reduced pressure using an evaporator, and the concentrated solution was mixed with methanol to form a methanol solution, which was dehydrated overnight with anhydrous magnesium sulfate, and the dehydrated methanol solution was concentrated under reduced pressure using an evaporator to obtain 26.5g (crude yield 99.0%) of compound 3, a colorless, transparent, viscous liquid. The water content measured by the Karl Fischer method was 5092ppm. The NMR identification data of the obtained compound 2 are as follows. (Identification data) 31 P-NMR: 33.37 ppm 1 H-NMR; 0.98 ppm (t, 12H, -CH 3 ), 1.51~1.58ppm(m,16H,-CH 2 -), 2.36~2.42ppm(m,8H,P-CH 2 -), 3.12 ppm (s, 2H, -CH 2 -NH 2 ), 3.35 ppm (s, 2H, -NH 2 ) As a result, compound 2 was identified as tetrabutylphosphonium glycinate.

[0047] [Production Example 3] 614g (0.08 mol) of the aqueous solution of tetrabutylphosphonium hydroxide obtained in the same manner as in Preparation Example 1 and an aqueous solution in which 7.1g (0.08 mol) of DL-alanine was dissolved in 100ml of pure water were mixed at room temperature with stirring. The resulting mixed aqueous solution was concentrated under reduced pressure using an evaporator, and the concentrated solution was mixed with methanol to form a methanol solution, which was dehydrated overnight with anhydrous magnesium sulfate, and the dehydrated methanol solution was concentrated under reduced pressure using an evaporator to obtain 27.2g (crude yield 98.0%) of colorless, transparent, viscous liquid compound 1. The water content measured by the Karl Fischer method was 4947ppm. The NMR identification data of the obtained compound 3 are as follows. (Identification data) 31 P-NMR: 33.37 ppm 1 H-NMR; 0.98 ppm (t, 12H, -CH 3 ), 1.51~1.58ppm(m,16H,-CH 2 -), 1.29 ppm (d, 3H, -CH 3 ), 2.39~2.40(m,8H,P-CH 2 -), 3.25(q, 1H, -CH-NH 2 ), 3.35(s,2H,-NH 2 ) As a result, compound 3 was identified as tetrabutylphosphonium DL-alaninate.

[0048] [Examples 1-1 to 1-3] Compound 1 (tetrabutylphosphonium β-alaninate) obtained in Production Example 1 and methyltributylphosphonium dimethylphosphate (PX-4MP: manufactured by Nippon Chemical Industry Co., Ltd.) were mixed to obtain the composition shown in Table 1 to obtain a moisture absorbent. The obtained moisture absorbent was subjected to a moisture absorption test and a moisture release test according to the procedures described below. The results are shown in Tables 2 and 4. The moisture absorbent of Example 1-2 was subjected to a moisture re-absorption test according to the procedure described below. The results are shown in Table 3.

[0049] [Comparative Example 1-1] Using methyltributylphosphonium dimethylphosphate, moisture absorption and desorption tests were carried out in the same manner as in Examples 1-1 to 1-3. The results are shown in Tables 2 and 4.

[0050] [Comparative Example 1-2] Using Compound 1, a moisture absorption test and a moisture desorption test were carried out in the same manner as in Examples 1-1 to 1-3. The results are shown in Tables 2 and 4.

[0051] <Moisture absorption test> A stainless steel cage measuring 170 mm in length, 220 mm in width, and 80 mm in height was placed in a polyethylene bag with a zipper and placed in an acrylic test box with a relative humidity adjusted to about 50%. Approximately 1 g of moisture absorbent was placed in a 70 mm diameter glass petri dish and weighed accurately to the nearest 0.1 mg. The petri dish and a thermo-hygrometer (a T&D data logger TR72nw) were placed in the cage, the bag was sealed, and the change in relative humidity inside the bag over time was measured. The time required for the initial relative humidity to be reduced by half was defined as the humidity half-life, and the moisture absorption rate per mole of each moisture absorbent until the relative humidity was reduced by half was calculated as the molar moisture absorption rate, and the moisture absorption performance of each moisture absorbent was compared. The molar moisture absorption rate (% / mol min) was calculated using the following formula: (1 / 2 of the initial humidity) / [(sample weight / molecular weight) x (time to reach 1 / 2 of the initial humidity)]

[0052] <Re-moisture absorption test> For the moisture absorbent of Example 1-2, the above moisture absorption test was carried out until the relative humidity in the bag was 10% or less, and then the relative humidity in the bag was adjusted to about 50% again, and the change in the relative humidity over time in the bag was measured in the same manner as in the above moisture absorption test. The half-life and molar moisture absorption rate are shown in Table 3.

[0053] <Moisture release test> Approximately 3 g of moisture absorbent, which had been adjusted to a moisture content of approximately 2% by adding ion-exchanged water, was placed in a 75 mm diameter glass petri dish and weighed accurately to the nearest 0.1 mg. The petri dish was placed in an incubator heated to a specified temperature in air. After 30 minutes, the petri dish was removed and the moisture content of each moisture absorbent was measured using a Karl Fischer moisture meter to determine the reduction rate (%) from the initial moisture content, and the moisture release performance of each moisture absorbent was compared. The appearance after heating was also observed. The heating temperature, moisture reduction rate, and appearance after heating are shown in Table 4.

[0054] [Table 1]

[0055] [Table 2]

[0056] [Table 3]

[0057] [Table 4]

[0058] The results shown in Table 3 show that although the moisture absorption rate was slow, the moisture absorption capacity was still sufficient.

[0059] [Examples 2-1 to 2-4] Compound 2 (tetrabutylphosphonium glycinate) obtained in Production Example 2 and methyltributylphosphonium dimethylphosphate (PX-4MP: Nippon Chemical Industry Co., Ltd.) were mixed to obtain the composition shown in Table 5 to obtain a moisture absorbent. The moisture absorbents obtained in Examples 2-1, 2-3, and 2-4 were used to carry out moisture absorption tests in the same manner as in Examples 1-1 to 1-3. The results are shown in Table 6. Further, for the moisture absorbent of Example 2-2, a moisture release test was carried out in the same manner as in Examples 1-1 to 1-3. The results are shown in Table 7.

[0060] [Comparative Example 2-1] Using Compound 2, a moisture absorption test and a moisture desorption test were carried out in the same manner as in Examples 1-1 to 1-3. The results are shown in Tables 6 and 7.

[0061] [Table 5]

[0062] [Table 6]

[0063] [Table 7]

[0064] [Examples 3-1 to 3-3] Compound 3 (tetrabutylphosphonium DL-alaninate) obtained in Production Example 3 and methyltributylphosphonium dimethylphosphate (PX-4MP: manufactured by Nippon Chemical Industry Co., Ltd.) were mixed so as to obtain the composition shown in Table 8, thereby obtaining a moisture absorbent. Using the obtained moisture absorbent, a moisture absorption test was carried out in the same manner as in Examples 1-1 to 1-3. The results are shown in Table 7.

[0065] [Comparative Example 3-1] A moisture absorption test was carried out in the same manner as in Examples 1-1 to 1-3 using Compound 3. The results are shown in Table 9.

[0066] [Table 8]

[0067] [Table 9]

[0068] The results shown in Tables 2, 6 and 9 show that the inclusion of two specific types of ionic liquids results in a moisture absorbent with superior moisture absorption properties compared to the inclusion of only one type of ionic liquid. Furthermore, the results shown in Tables 4 and 7 show that the inclusion of two specific types of ionic liquids enables the absorbed moisture to be released at the same or lower heating temperature as when only one type of ionic liquid is included, resulting in a moisture absorbent with excellent moisture absorption and release properties.

Claims

1. A moisture absorbent comprising the following ionic liquid (A) and ionic liquid (B). Ionic liquid (A): An ionic liquid in which the anion component is a phosphate ester ion or a phosphate ion. Ionic liquid (B): An ionic liquid in which the anion component is a carboxylate ion having an amino group or a carboxylate ion having a nitrogen-containing heterocycle.

2. 2. The moisture absorbent according to claim 1, wherein the cationic components of the ionic liquid (A) and the ionic liquid (B) are ammonium ions, phosphonium ions, or imidazolium ions.

3. The moisture absorbent according to claim 2 , wherein the cationic component is a phosphonium ion represented by the following general formula (I): 【Chemistry 1】 (In the formula, R 1 , R 2 , R 3 and R 4 each independently represents a linear alkyl group, a branched alkyl group, or a cyclic alkyl group having 1 to 20 carbon atoms.

4. the anion component of the ionic liquid (A) is a dialkyl phosphate ion, The moisture absorbent according to claim 1, wherein the anion component of the ionic liquid (B) is an anion of an amino acid selected from L-asparagine, L-aspartic acid, DL-alanine, β-alanine, D-alanine, L-alanine, L-arginine, L-isoleucine, glycine, L-glutamine, L-glutamic acid, L-cysteine, DL-serine, L-serine, L-tyrosine, L-tryptophan, L-threonine, L-valine, L-histidine, L-phenylalanine, L-proline, L-methionine, L-lysine and L-leucine.

5. 2. The moisture absorbent according to claim 1, wherein a mixing molar ratio of the ionic liquid (A) to the ionic liquid (B) is 95:5 to 5:

95.

6. The moisture absorbent according to claim 1, which has moisture absorbing and releasing properties.

7. A device using the moisture absorbent according to any one of claims 1 to 6.

8. The apparatus according to claim 7, wherein the apparatus is a dry water electrolysis gas production apparatus, an air conditioner, or an absorption chiller.

Citation Information

Patent Citations

  • Manufacturing method of dried water electrolysis gas and device thereof

    JP2018051543A

  • Production method of dry hydrogen gas derived from water electrolysis, and absorbent solution

    JP2019202917A

  • Hygroscopic material

    JP2020006349A