Adhesive sheet, adhesive sheet with release film, laminate for image display device, image display device, and adhesive sheet for image display device constituent member

A pressure-sensitive adhesive sheet with tailored elastic and relaxation properties addresses bonding reliability issues at the edges of image display devices, ensuring bubble-free and durable adhesion in narrow frame designs.

JP2024139738APending Publication Date: 2024-10-09MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2024045869
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-03-27
Filing Date
2024-03-22
Publication Date
2024-10-09

AI Technical Summary

Technical Problem

Conventional adhesive sheets for image display devices face challenges in achieving high bonding reliability at the peripheral edges, particularly in designs with curved or bent edges, leading to air bubble formation and adhesive oozing, which are exacerbated by the trend towards narrower frames and frameless designs.

Method used

The development of a pressure-sensitive adhesive sheet with specific elastic modulus, relaxation modulus, and stress relaxation rates, combined with a crosslinking agent and photoinitiator, to ensure effective bonding without bubbles and adhesive oozing, even in narrow frame designs.

Benefits of technology

The adhesive sheet provides reliable bonding at the peripheral edges, reducing air bubbles and adhesive extrusion, suitable for narrow and frameless image display device designs, with improved durability and deformation resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024139738000001
    Figure 2024139738000001
  • Figure 2024139738000002
    Figure 2024139738000002
  • Figure 2024139738000003
    Figure 2024139738000003
Patent Text Reader

Abstract

To provide an adhesive sheet which has an even higher level of sticking reliability than a conventional adhesive sheet.SOLUTION: In an adhesive sheet having an acrylic adhesive layer formed of an adhesive composition containing an acrylic polymer (A), the acrylic adhesive layer has a stress relaxation rate (X0) calculated from an initial elastic modulus (G0'(0)) after a lapse of 0.1 second from application of a strain of 25% at a temperature of 70°C, and a relaxation modulus (G0'(300)) after a lapse of 300 seconds from application of a strain of 25% at a temperature of 70°C according to the formula (I) of 0.20 or less. Stress relaxation rate (X0)=(G0'(300) / G0'(0))...(I)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a pressure-sensitive adhesive sheet, a pressure-sensitive adhesive sheet with a release film, a laminate for an image display device, an image display device, and a pressure-sensitive adhesive sheet for use as a component of an image display device. [Background technology]

[0002] In order to improve the visibility of image display devices, the gap between an image display panel such as a liquid crystal display (LCD), a plasma display (PDP) or an electroluminescence display (ELD) and a protective panel or a touch panel member placed on the front side (viewing side) of the image display panel is filled with a resin such as an adhesive or bonding agent to suppress reflection of incident light and outgoing light from the displayed image at the air layer interface.

[0003] For example, Patent Document 1 discloses a method for manufacturing a component laminate for an image display device having an image display device component laminated on at least one side of a transparent double-sided adhesive sheet, in which an adhesive sheet that has been primarily crosslinked by ultraviolet light is attached to the image display device component, and then the adhesive sheet is irradiated with ultraviolet light through the image display device component for secondary curing.

[0004] Furthermore, Patent Document 2 discloses a pressure-sensitive adhesive sheet containing a (meth)acrylic copolymer having an ultraviolet-crosslinkable site, as an adhesive sheet useful for displays and touch panels. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Patent No. 4971529 [Patent Document 2] Patent No. 6062740 Summary of the Invention [Problem to be solved by the invention]

[0006] As a requirement for image display devices, there is a strong demand to enlarge the effective display area as much as possible without changing the outer dimensions, that is, to narrow the frame. For this reason, there is a demand for adhesive sheets for bonding image display components that can be bonded without air bubbles, even to the peripheral areas near the end faces of the adhesive sheet, which in the past were located directly below the concealing area and therefore could not be seen.

[0007] Furthermore, in recent years, high design quality has been demanded for image display devices, and the shape of the front surface protection panel is changing from flat to curved edges or corners, or to a design in which the entire display unit is curved, etc. In the case of curved members or members with curved edges or corners, air bubbles are more likely to occur in the peripheral area than in flat members.

[0008] The adhesive sheets in Patent Documents 1 and 2 are designed to be laminated structures using conventional components of image display devices, and do not take into consideration the reliability of adhesion near the peripheral edge of the adhesive sheet, which would have been located directly below the concealed portion and therefore not visible in the past. In addition, conventional flexible adhesive sheets have a tendency for the edges to get crushed and the glue (adhesive layer) to spill out. To solve this problem, it is necessary to give the sheet a certain degree of hardness, but if the sheet is made too hard, air bubbles tend to form around the edges. Therefore, for image display devices with increasingly narrower picture frames, there is a demand for pressure-sensitive adhesive sheets that have an appropriate hardness while also providing superior lamination reliability at the peripheral edge, which is a trade-off characteristic.

[0009] Therefore, against this background, the present invention aims to provide an adhesive sheet, an adhesive sheet with a release film, a laminate for an image display device, an image display device, and an adhesive sheet for a component of an image display device, which have a higher level of bonding reliability than conventional ones. [Means for solving the problem]

[0010] That is, the present invention has the following aspects. [1] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), The acrylic pressure-sensitive adhesive layer has an initial elastic modulus (G0'(0)) 0.1 seconds after application of a 25% strain at a temperature of 70°C and a relaxed elastic modulus (G0'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C, calculated by the following formula (I): Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I) [2] A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, the acrylic pressure-sensitive adhesive layer being a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) having an alkyl group with a carbon number of 3 to 30, and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), The acrylic pressure-sensitive adhesive layer has an initial elastic modulus (G0'(0)) 0.1 seconds after application of a 25% strain at a temperature of 70°C and a relaxed elastic modulus (G0'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C, calculated by the following formula (I): Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I) [3] The pressure-sensitive adhesive sheet according to [1] or [2], wherein the relaxation modulus (G0'(0)) is 5 to 100 kPa. [4] The pressure-sensitive adhesive sheet according to any one of [1] to [3], wherein the relaxation modulus (G0'(300)) is 0.1 to 20 kPa. [5] The pressure-sensitive adhesive sheet according to any one of [1] to [4], wherein the pressure-sensitive adhesive sheet has a gel fraction of 30 to 90%. [6] The pressure-sensitive adhesive sheet according to any one of [1] to [5], having a shear storage modulus (G'(25°C)) at a temperature of 25°C, obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, of 100 kPa or more. [7] The pressure-sensitive adhesive sheet according to any one of [1] to [6], which has a glass transition temperature (Tg) of -25°C or higher, defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz. [8] The pressure-sensitive adhesive sheet according to [1], wherein the pressure-sensitive adhesive composition contains a crosslinking agent (B) and a photoinitiator (C). [9] The pressure-sensitive adhesive sheet described in [1], wherein the pressure-sensitive adhesive composition comprises a photoinitiator (C), the photoinitiator (C) comprising a photoinitiator (c1) having within its molecule a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1).

[10] The pressure-sensitive adhesive sheet according to [1], wherein the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3).

[11] The pressure-sensitive adhesive sheet according to any one of [1] to

[10] , which has active energy ray curing properties.

[12] The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The pressure-sensitive adhesive sheet according to

[11] , wherein the acrylic pressure-sensitive adhesive layer has a post-cure stress relaxation rate (X1) of 0.22 or more when irradiated such that the post-cure initial elastic modulus (G1'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C and the post-cure relaxation elastic modulus (G1'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C are used: Stress relaxation rate after curing (X1) = (G1'(300) / G1'(0)) (II)

[13] The pressure-sensitive adhesive sheet for attaching optical members according to

[12] , wherein the difference (X1-X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

[14] The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2 The pressure-sensitive adhesive sheet according to any one of

[11] to

[13] , wherein the acrylic pressure-sensitive adhesive layer has an initial post-curing elastic modulus (G1'(0)) of 1 kPa or more and 100 kPa or less 0.1 seconds after application of a 25% strain at a temperature of 70°C when irradiated so as to satisfy the above condition.

[15] The pressure-sensitive adhesive sheet is exposed to active energy rays having a wavelength of 365 nm with an integrated light amount of 2000 to 4000 mJ / cm 2The pressure-sensitive adhesive sheet according to any one of

[11] to

[14] , wherein the acrylic pressure-sensitive adhesive layer has a post-cure relaxation modulus (G1'(300)) of 0.1 kPa or more and 50 kPa or less 300 seconds after application of a 25% strain at a temperature of 70°C when irradiated so as to give a radiation beam having a curing rate of 100 s.

[16] A pressure-sensitive adhesive sheet with a release film, comprising: the pressure-sensitive adhesive sheet according to any one of [1] to

[15] ; and a release film laminated on the pressure-sensitive adhesive sheet.

[17] A laminate for an image display device comprising two image display device components and an adhesive sheet according to any one of [1] to

[15] interposed between the two image display device components, wherein one of the two image display device components is a surface protection panel and the other is a member consisting of any one or a combination of two or more selected from the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element and a retardation film.

[18] The laminate for an image display device according to

[17] , wherein the surface protection panel has a frame-shaped concealing portion on the periphery, and the frame has a portion having a width of 3 mm or less.

[19] The laminate for an image display device according to

[17] or

[18] , which is fixed in a curved state.

[20] An image display device comprising the laminate for an image display device according to any one of

[17] to

[19] .

[21] An adhesive sheet for use as a component of an image display device, comprising the adhesive sheet according to any one of [1] to

[15] . Effect of the Invention

[0011] The pressure-sensitive adhesive sheet of the present invention can be attached without air bubbles even to the peripheral portion near the end face of the pressure-sensitive adhesive sheet, which was previously located directly below the concealing portion and could not be seen. Therefore, the pressure-sensitive adhesive sheet can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame design or frameless design. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] An example of an embodiment of the present invention will be described in detail below. However, the present invention is not limited to the embodiment described below. In this specification, the term "film" conceptually encompasses a sheet, a film, and a tape. Furthermore, when the term "panel" is used, such as an image display panel or a protective panel, it encompasses a plate, a sheet, and a film.

[0013] In this specification, when it is written "x to y" (x and y are any numbers), unless otherwise specified, it includes the meaning of "greater than x and less than y", as well as "preferably greater than x" or "preferably smaller than y". In addition, when it is stated that the amount is "x or more" (where x is any number), it also means that the amount is "preferably greater than x" unless otherwise specified, and when it is stated that the amount is "y or less" (where y is any number), it also means that the amount is "preferably smaller than y" unless otherwise specified. Furthermore, "x and / or y (x and y are optional configurations)" means at least one of x and y, and means the following three cases: x only, y only, and x and y. In addition, in this specification, "(meth)acrylic" is a comprehensive term that includes acrylic and methacrylic, "(meth)acrylate" is a comprehensive term that includes acrylate and methacrylate, and "(meth)acryloyl" is a comprehensive term that includes acryloyl and methacryloyl. Furthermore, in this specification, the term "main component" refers to a component that has a significant effect on the properties of the material, and the content of the component is usually 50 mass % or more of the entire material, preferably 70 mass % or more, and particularly preferably 90 mass % or more. In addition, for the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range can be arbitrarily combined with the upper limit or lower limit of another numerical range. In addition, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range can be replaced with the value shown in the examples.

[0014] <<Adhesive sheet>> An adhesive sheet according to an example of the first embodiment of the present invention (hereinafter referred to as "the present adhesive sheet 1") is an adhesive sheet having an acrylic adhesive layer formed from an adhesive composition containing an acrylic polymer (A), in which the acrylic adhesive layer has a stress relaxation rate (X0) of 0.20 or less, as calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C and the relaxation elastic modulus (G0'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C. Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I) Furthermore, an adhesive sheet according to an example of the second embodiment of the present invention (hereinafter referred to as "the adhesive sheet 2") is an adhesive sheet having an acrylic adhesive layer, the acrylic adhesive layer being a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) having an alkyl group with 3 or more carbon atoms, and a hydroxyl group-containing (meth)acrylate (a2) and / or a nitrogen-containing monomer (a3), the acrylic adhesive layer having a stress relaxation rate (X0) of 0.20 or less, calculated by the following formula (I) from the initial elastic modulus (G0'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C and the relaxed elastic modulus (G0'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C: Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I) Hereinafter, there will be described the present adhesive sheet 1 and the present adhesive sheet 2. Furthermore, the present adhesive sheet 1 and the present adhesive sheet 2 may collectively be referred to simply as the "present adhesive sheet."

[0015] This pressure-sensitive adhesive sheet satisfies the following requirement (1). Requirement (1) The stress relaxation rate (X0) calculated from the initial elastic modulus (G0'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C to the acrylic pressure-sensitive adhesive layer and the relaxed elastic modulus (G0'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C using the following formula (I) is 0.20 or less. Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0016] The pressure-sensitive adhesive sheets 1 and 2 satisfying the requirement (1) have excellent stress relaxation properties, i.e., are flexible, and therefore have excellent properties for trapping foreign matter and defects that can cause bubbles to form, and also have good properties for diffusing air trapped during lamination of components. As a result, air bubbles remaining at the peripheral edge of the pressure-sensitive adhesive sheet can be reduced or eliminated.

[0017] In laminates requiring precision lamination, such as laminates for image display devices, when members are laminated together, finish lamination is generally performed by a heating and pressurizing treatment using an autoclave. After the autoclave process is completed or after the product is put into use, air bubbles may be generated at the peripheral edge. One of the main causes of the generation of such air bubbles is thought to be that the air present in the autoclave oven during the lamination process penetrates between the lamination member and the pressure-sensitive adhesive sheet due to the high pressure inside the autoclave oven. Conventionally, such bubbles were not visible because the peripheral edges of displays were covered by a concealing layer such as a print or a bezel. However, in recent years, the peripheral edges have become narrower due to the demand for narrower picture frames and frameless designs for displays, and there is a strong demand for improving the foaming resistance of pressure-sensitive adhesive sheets at the peripheral edges.

[0018] From the viewpoint of improving the foaming resistance at the peripheral edge portion of the pressure-sensitive adhesive sheet, the stress relaxation rate (X0) is preferably 0.15 or less, more preferably 0.1 or less, and even more preferably 0.05 or less. On the other hand, from the viewpoint of suppressing the extrusion of the adhesive, the stress relaxation rate (X0) is preferably 0.01 or more, more preferably 0.02 or more, further preferably 0.03 or more, particularly preferably 0.04 or more, and most preferably 0.10 or more. The lower limit and the upper limit of the stress relaxation rate (X0) can be arbitrarily combined.

[0019] The stress relaxation rate (X0) is determined as follows. The initial elastic modulus (G0'(0)) and the relaxation elastic modulus (G0'(300)) are measured by the method described below, and the obtained values ​​are substituted into the following formula (I) to calculate. Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0020] Examples of methods for adjusting the stress relaxation rate (X0) include a method for adjusting the composition or molecular weight of the acrylic polymer (A), the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation, but are not limited to these methods.

[0021] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (2). Requirement (2) The acrylic pressure-sensitive adhesive layer has an initial elastic modulus (G0'(0)) of 5 to 100 kPa 0.1 seconds after a strain of 25% is applied at a temperature of 70°C.

[0022] An adhesive sheet satisfying requirement (2) has an appropriate cohesive strength, and therefore is easy to handle. In addition, the peripheral edges of the adhesive sheet are less likely to be crushed when the sheet is attached to a component, and excess glue at the edges can be reduced or eliminated. From the viewpoint of reducing glue overflow, the initial elastic modulus (G0'(0)) is preferably 10 kPa or more, more preferably 15 kPa or more, and even more preferably 20 kPa or more. In addition, when the adherend has irregularities, from the viewpoint of filling in the surface irregularities during lamination, the initial elastic modulus (G0'(0)) is preferably 60 kPa or less, more preferably 50 kPa or less, and even more preferably 40 kPa or less. The lower limit and upper limit of the initial elastic modulus (G0'(0)) can be arbitrarily combined.

[0023] The initial elastic modulus (G0'(0)) is measured, for example, as follows. The adhesive sheets are repeatedly laminated to adjust the thickness to 0.7 to 1.2 mm (for example, about 0.8 mm), and punched out to a diameter of 8 mm. The obtained sample is subjected to a strain of 25% at 70°C using a rheometer, and the elastic modulus is read after 0.1 seconds.

[0024] In measuring the initial elastic modulus (G0'(0)), it is necessary to avoid fluctuations in the measurement results due to the influence of the measuring jig. The initial elastic modulus (G0'(0)) is a value measured after adjusting the thickness to the range of 0.7 to 1.2 mm, and this allows the initial elastic modulus (G0'(0)) to be accurately measured without being influenced by the measuring jig. Incidentally, "adjusted to a thickness of 0.7 to 1.2 mm" means that if the thickness of the pressure-sensitive adhesive sheet as a measurement sample does not fall within this range, the thickness of the measurement sample is adjusted to within this range by stacking several sheets, etc. The same applies when the thickness of the measurement sample is specified in other tests.

[0025] Examples of the method for adjusting the initial elastic modulus (G0'(0)) include a method for adjusting the composition or molecular weight of the acrylic polymer (A), or the type or amount of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation. However, the method is not limited to these methods.

[0026] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (3). Requirement (3) The acrylic pressure-sensitive adhesive layer has a relaxation modulus (G0'(300)) of 0.1 to 20 kPa 300 seconds after a strain of 25% is applied at a temperature of 70°C.

[0027] An adhesive sheet satisfying requirement (3) has an appropriate cohesive strength, and therefore has excellent handleability. In addition, the peripheral edges of the adhesive sheet are less likely to be crushed when the sheet is attached to a component, and there is a tendency for glue overflow at the edges to be reduced or eliminated. From the viewpoint of reducing the overflow of the paste, the relaxation modulus (G0'(300)) is preferably 0.2 kPa or more, more preferably 0.5 kPa or more, and further preferably 1 kPa or more. From the viewpoint of maintaining a suitable flexibility and ensuring wettability to an adherend, the relaxation modulus (G0'(300)) is preferably 15 kPa or less, more preferably 10 kPa or less, and even more preferably 5 kPa or less. The lower limit and upper limit of the relaxation modulus (G0'(300)) can be arbitrarily combined.

[0028] The relaxation modulus (G0'(300)) is measured, for example, as follows. The adhesive sheets are repeatedly laminated to adjust the thickness to 0.7 to 1.2 mm (for example, about 0.8 mm), and punched out to a diameter of 8 mm. The elastic modulus of the obtained sample is read after 300 seconds at 70°C and a strain of 25% is applied using a rheometer.

[0029] Examples of the method for adjusting the relaxation modulus (G0'(300)) include a method for adjusting the composition or molecular weight of the acrylic polymer (A), the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation, although the method is not limited to these methods.

[0030] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (4). Requirement (4) The shear storage modulus (G0'(25°C)) at 25°C, as determined by dynamic viscoelastic measurement in a shear mode at a frequency of 1 Hz, is 100 kPa or more.

[0031] Adhesive sheets that satisfy requirement (4) tend to have excellent handling properties and resistance to adhesive seepage. From this viewpoint, the storage shear modulus at 25°C (G0'(25°C)) is preferably 120 kPa or more, more preferably 150 kPa or more, even more preferably 200 kPa or more, particularly preferably 250 kPa or more, and among these, 300 kPa or more is preferable, and 400 kPa or more is most preferable. On the other hand, from the viewpoint of ensuring the stress relaxation property of the pressure-sensitive adhesive sheet, the shear storage modulus at 25°C (G0'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, even more preferably 750 kPa or less, and particularly preferably 500 kPa or less. The lower limit and upper limit of the storage shear modulus at 25°C (G0'(25°C)) can be arbitrarily combined.

[0032] The shear storage modulus at 25° C. (G0′(25° C.)) is measured, for example, as follows. The adhesive sheet is repeatedly laminated to adjust the thickness to 0.7 to 1.2 mm (for example, 0.8 mm), and then punched out to a diameter of 8 mm. The obtained sample is subjected to dynamic viscoelasticity measurement using a rheometer under the conditions of measurement jig: 8 mm diameter parallel plate, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min, and the shear storage modulus at 25°C (G0'(25°C)) is read.

[0033] Examples of the method for adjusting the shear storage modulus at 25° C. (G0'(25° C.)) to the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A) or the type or content of the crosslinking agent (B) or photoinitiator (C), as well as a method for adjusting the amount of active energy ray irradiation. However, the method is not limited to these methods.

[0034] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (5). Requirement (5) The glass transition temperature (Tg0) defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz is -25°C or higher.

[0035] PSA sheets that satisfy requirement (5) tend to be excellent in handling properties and resistance to adhesive seepage. From this viewpoint, the glass transition temperature (Tg0) is preferably -20°C or higher, more preferably -15°C or higher, even more preferably -10°C or higher, particularly preferably -5°C or higher, and most preferably 0°C or higher. On the other hand, from the viewpoint of obtaining appropriate flexibility and stress relaxation, the upper limit is preferably 60°C or lower, more preferably 50°C or lower, even more preferably 40°C or lower, particularly preferably 20°C or lower, and of these, 5°C or lower is preferable. The lower limit and upper limit of the glass transition temperature (Tg0) can be arbitrarily combined.

[0036] The glass transition temperature (Tg0) can be obtained by reading the temperature at which the loss tangent (Tan δ) is maximized, i.e., the peak temperature, from dynamic viscoelasticity spectrum data in a shear mode obtained by the same measurement method as for the shear storage modulus at 25°C (G0'(25°C)) described above. In the case where a plurality of maximum values ​​exist in the viscoelasticity spectrum, the "peak temperature" is the temperature at which the largest maximum value is obtained.

[0037] Examples of the method for adjusting the glass transition temperature (Tg0) to the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A), the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation, but are not limited to these methods.

[0038] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (6). Requirement (6) The adhesive sheet has a gel fraction of 30 to 90%.

[0039] A PSA sheet satisfying the requirement (6) has an appropriate cohesive strength and tends to be excellent in handleability and shape stability. From the viewpoint of obtaining a suitable cohesive force, the gel fraction is preferably 35% or more, more preferably 40% or more, and even more preferably 45% or more. On the other hand, from the viewpoint of obtaining a stress relaxation property, the gel fraction is preferably 90% or less, more preferably 87% or less, and even more preferably 85% or less. The lower limit and the upper limit of the gel fraction can be arbitrarily combined.

[0040] The gel fraction is measured, for example, as follows. The adhesive sheet, the mass of which has been measured in advance, and a 150-mesh SUS wire mesh are prepared. Next, the adhesive sheet is wrapped in the SUS wire mesh and immersed in ethyl acetate at 23°C for 24 hours. After that, the sheet is dried at 70°C for 4.5 hours, and the mass of the sheet and the SUS wire mesh are measured. The mass of the insoluble adhesive sheet remaining in the wire mesh (mass after immersion) is calculated by subtracting the mass of the SUS wire mesh from the mass of the sheet. The gel fraction (%) is calculated as the percentage of the mass of the insoluble adhesive sheet remaining in the wire mesh (mass after immersion) relative to the mass of the adhesive sheet before immersion in ethyl acetate (mass before immersion).

[0041] Examples of the method for adjusting the gel fraction to the above range include a method for adjusting the composition or molecular weight of the acrylic polymer (A), the type or content of the crosslinking agent (B) or the photoinitiator (C), and a method for adjusting the amount of active energy ray irradiation, but are not limited to these methods.

[0042] It is preferable that the present pressure-sensitive adhesive sheet further satisfies the following requirement (7). Requirement (7) The adhesive strength of the acrylic adhesive layer to soda lime glass at a temperature of 23°C and a peeling speed of 60 mm / min is 2 N / cm or more.

[0043] By having an adhesive strength of 2 N / cm or more, peeling of the adhesive sheet edge surface does not occur, and excellent bonding reliability can be obtained at the peripheral edge. From this viewpoint, the adhesive strength is preferably 4 N / cm or more, more preferably 6 N / cm or more, and even more preferably 12 N / cm or more. The upper limit of the adhesive strength is not particularly limited, but from the viewpoint of reworkability, it is usually 50 N / cm, preferably 30 N / cm.

[0044] The adhesive strength is measured, for example, as follows. A polyethylene terephthalate (PET) film having a thickness of 100 μm is laminated to the acrylic adhesive layer of this adhesive sheet, and the other side is roll-pressed to a soda lime glass to obtain a laminate. The laminate is then autoclaved (temperature 60°C, gauge pressure 0.2 MPa, 20 minutes) to finish and adhere to the sample for measuring adhesive strength. The adhesive strength is determined by the peel strength (N / cm) when the sample is peeled at a peel angle of 180° and a peel speed of 60 mm / min under an environment of temperature 23°C and humidity 50% RH.

[0045] The pressure-sensitive adhesive sheet is preferably active energy ray-curable. Here, the pressure-sensitive adhesive sheet being "active energy ray-curable" means that the pressure-sensitive adhesive sheet has the property of being cured by active energy rays, in other words, that there is room for curing by active energy rays.

[0046] The adhesive sheet 1 may be cured to a state where there is still room for curing by active energy rays (hereinafter also referred to as "primary curing"), or it may be uncured at all (hereinafter referred to as "uncured") and capable of being cured by active energy rays. Moreover, the adhesive sheet 2 is preferably primarily cured. The above-mentioned primarily cured or uncured pressure-sensitive adhesive sheet can be cured (hereinafter also referred to as "secondary curing") by irradiating it with active energy rays after it has been attached to an adherend.

[0047] When the present pressure-sensitive adhesive sheet is curable with active energy rays, it preferably satisfies the following requirements.

[0048] Requirement (8) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When the acrylic pressure-sensitive adhesive layer is irradiated so as to satisfy the above condition, the post-cure stress relaxation rate (X1) is calculated from the initial elastic modulus (G1'(0)) 0.1 second after application of a 25% strain at a temperature of 70°C and the relaxed elastic modulus (G1'(300)) 300 seconds after application of a 25% strain at a temperature of 70°C by the following formula (II), and is 0.22 or more. Stress relaxation rate after curing (X1) = (G1'(300) / G1'(0)) (II)

[0049] A pressure-sensitive adhesive sheet satisfying the requirement (8) has excellent resistance to deformation, and therefore tends to be less susceptible to dents or indentations when made into a laminate for an image display device, and to exhibit excellent durability. From the viewpoint of obtaining excellent durability, the stress relaxation rate after curing (X1) is preferably 0.25 or more, more preferably 0.30 or more, and even more preferably 0.35 or more. On the other hand, from the viewpoint of obtaining stress relaxation property, the stress relaxation rate after curing (X1) is preferably 1.00 or less, more preferably 0.80 or less, and even more preferably 0.70 or less. The lower limit and the upper limit of the stress relaxation rate after curing (X1) can be arbitrarily combined.

[0050] Requirement (9) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the acrylic pressure-sensitive adhesive layer has an initial elastic modulus after curing (G1'(0)) of 10 kPa or more 0.1 seconds after application of a 25% strain at a temperature of 70°C.

[0051] A pressure-sensitive adhesive sheet satisfying the requirement (9) has high cohesive strength, and therefore tends to be able to exhibit excellent durability against dents and indentations when made into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the initial elastic modulus after curing (G1'(0)) is preferably 15 kPa or more, more preferably 20 kPa or more, and even more preferably 25 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the initial elastic modulus after curing (G1'(0)) is preferably 200 kPa or less, more preferably 100 kPa or less, further preferably 70 kPa or less, and particularly preferably 35 kPa or less. The lower limit and upper limit of the initial elastic modulus after curing (G1'(0)) can be arbitrarily combined. The method for measuring the initial elastic modulus after curing (G1'(0)) is the same as that for measuring the initial elastic modulus (G0'(0)).

[0052] Requirement(10) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the acrylic pressure-sensitive adhesive layer has a post-curing relaxation modulus (G1'(300)) of 1 to 200 kPa 300 seconds after application of a 25% strain at a temperature of 70°C.

[0053] A pressure-sensitive adhesive sheet satisfying the requirement (10) has high cohesive strength, and therefore tends to be able to exhibit excellent durability against dents and indentations when made into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the relaxation modulus after curing (G1'(300)) is preferably 2 kPa or more, more preferably 3 kPa or more, further preferably 5 kPa or more, and particularly preferably 8 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the relaxation modulus after curing is preferably 200 kPa or less, more preferably 100 kPa or less, even more preferably 50 kPa or less, particularly preferably 20 kPa or less, and even more preferably 15 kPa or less, and most preferably 10 kPa or less. The lower limit and upper limit of the relaxation modulus after curing (G1'(300)) can be arbitrarily combined. The method for measuring the relaxation modulus after curing (G1'(300)) is the same as that for measuring the relaxation modulus (G0'(300)).

[0054] Requirement (11) The difference (X1-X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

[0055] A pressure-sensitive adhesive sheet satisfying the requirement (11) tends to be able to provide a high level of both resistance to foaming at the peripheral edge and durability against dents and indentations when made into a laminate for image display. From this viewpoint, the value of requirement (11) is preferably 0.02 or greater, more preferably 0.10 or greater, and even more preferably 0.20 or greater.

[0056] Requirement(12) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the shear storage modulus (G1'(25°C)) at 25°C after curing is 100 kPa or more, as determined by dynamic viscoelastic measurement in a shear mode at a frequency of 1 Hz.

[0057] A pressure-sensitive adhesive sheet satisfying the requirement (12) tends to exhibit high cohesive strength after exposure to active energy rays. To obtain high cohesive strength, the shear storage modulus at 25° C. after curing (G1′(25° C.)) is preferably 120 kPa or more, more preferably 150 kPa or more, further preferably 200 kPa or more, and particularly preferably 400 kPa or more. On the other hand, from the viewpoint of obtaining stress relaxation properties, the shear storage modulus at 25°C after curing (G1'(25°C)) is preferably 1000 kPa or less, more preferably 900 kPa or less, even more preferably 800 kPa or less, particularly preferably 750 kPa or less, and most preferably 500 kPa or less. The lower limit and upper limit of the shear storage modulus at 25°C after curing (G1'(25°C)) can be combined in any desired manner. The method for measuring the shear storage modulus at 25° C. after curing (G1′(25° C.)) is the same as that for the shear storage modulus at 25° C. (G1′(25° C.)).

[0058] Requirement (13) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to give the glass transition temperature (Tg) after curing, which is defined as the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz, is -25°C or higher.

[0059] A pressure-sensitive adhesive sheet satisfying the requirement (13) tends to exhibit high cohesive strength after exposure to active energy rays. From the viewpoint of obtaining high cohesive strength, the glass transition temperature (Tg1) after curing is preferably −23° C. or higher, more preferably −20° C. or higher, even more preferably −10° C. or higher, particularly preferably −5° C. or higher, and most preferably 0° C. or higher. On the other hand, from the viewpoint of obtaining stress relaxation properties, the glass transition temperature (Tg1) after curing is preferably 60° C. or less, more preferably 40° C. or less, even more preferably 30° C. or less, and among these, preferably 20° C. or less, particularly preferably 5° C. or less. The lower limit and upper limit of the glass transition temperature (Tg1) can be arbitrarily combined.

[0060] The method for measuring the glass transition temperature (Tg1) after curing is the same as that for the glass transition temperature (Tg0).

[0061] Requirement(14) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to achieve this, the gel fraction of the pressure-sensitive adhesive sheet (gel fraction after curing) is 35 to 95%.

[0062] A pressure-sensitive adhesive sheet satisfying the requirement (14) has high cohesive strength and can exhibit excellent durability when made into a laminate for an image display device. From the viewpoint of obtaining excellent durability, the gel fraction after curing is preferably 40% or more, more preferably 45% or more, and even more preferably 50% or more. On the other hand, from the viewpoint of obtaining an appropriate stress relaxation property, the gel fraction after curing is preferably 95% or less, and more preferably 90% or less. The lower limit and the upper limit of the gel fraction after curing can be combined arbitrarily.

[0063] The method for measuring the gel fraction after curing is the same as that for the gel fraction described above.

[0064] Requirement(15) The adhesive sheet is exposed to active energy rays with a wavelength of 365 nm, with an integrated light intensity of 2000 to 4000 mJ / cm 2 When irradiated so as to satisfy the above condition, the post-curing adhesive strength of the acrylic adhesive layer to soda lime glass at a temperature of 23° C. and a peeling speed of 60 mm / min is 2 N / cm or more.

[0065] A pressure-sensitive adhesive sheet satisfying the requirement (15) tends to exhibit excellent reliability without peeling even when used as a laminate for an image display device. From this viewpoint, the adhesive strength after curing is preferably 3 N / cm or more, more preferably 8 N / cm or more, and even more preferably 12 N / cm or more. The upper limit of the adhesive strength after curing is not particularly limited, but is usually 50 N / cm, preferably 30 N / cm, from the viewpoint of reworkability.

[0066] The post-curing adhesive strength is measured, for example, as follows. A 100 μm thick polyethylene terephthalate (PET) film as a backing film is laminated to the acrylic adhesive layer of this adhesive sheet, and the other side is roll-pressed onto soda lime glass, and then autoclaved (temperature 60°C, gauge pressure 0.2 MPa, 20 minutes) for finishing and pasting. After that, the integrated light intensity at a wavelength of 365 nm is 2000 to 4000 mJ / cm. 2 The adhesive sheet is irradiated with active energy rays through the backing film so as to cure the adhesive sheet, thereby preparing a sample for measuring adhesive strength. The peel strength (N / cm) obtained when this sample is peeled off at a peel angle of 180° and a peel speed of 60 mm / min in an environment of 23° C. and 50% RH is defined as the adhesive strength after curing.

[0067] <Adhesive sheet 1> The present pressure-sensitive adhesive sheet 1 has an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A). The pressure-sensitive adhesive composition preferably further contains a crosslinking agent (B) and a photoinitiator (C). Furthermore, the pressure-sensitive adhesive composition may further contain other components in addition to the acrylic polymer (A), the crosslinking agent (B) and the photoinitiator (C). When the pressure-sensitive adhesive composition is active energy ray-curable, the pressure-sensitive adhesive sheet 1 is typically obtained by curing a pressure-sensitive adhesive composition containing an acrylic polymer (A). Each component contained in the pressure-sensitive adhesive composition will be described in detail below.

[0068] [Acrylic polymer (A)] Examples of the acrylic polymer (A) include homopolymers of alkyl (meth)acrylates, as well as copolymers obtained by polymerizing monomer components copolymerizable therewith. In particular, it is preferred that the acrylic polymer (A) contains two or more copolymerization components, and at least one of the copolymerization components is an alkyl(meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms (hereinafter sometimes referred to as "alkyl(meth)acrylate (a1)").

[0069] A more specific example of the acrylic polymer (A) is a copolymer of a copolymerization component containing an alkyl(meth)acrylate (a1) and at least one copolymerizable monomer selected from the group consisting of an alkyl(meth)acrylate (a1) and a copolymerizable monomer (a2), a nitrogen-containing monomer (a3), a carboxyl group-containing monomer (a4), an epoxy group-containing monomer (a5), a vinyl monomer (a6), an alkyl(meth)acrylate monomer (a7) having an alkyl group with 1 or 2 carbon atoms, an alicyclic monomer (a8), a macromonomer (a9), and other copolymerizable monomers (a10) (hereinafter, sometimes referred to as "copolymerizable monomers (a2) to (a10)"). Among them, it is preferable to contain a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3) ​​as a copolymerization component, since it is possible to provide both corrosion resistance, adhesion, and resistance to wet heat whitening when the adherend contains a corrosive component such as metal, and it is particularly preferable to contain a hydroxyl group-containing monomer (a2) and a nitrogen-containing monomer (a3) ​​in order to further enhance cohesion. Also, when the adherend contains a corrosive component such as metal, it is preferable from the viewpoint of corrosion resistance that the copolymerization component does not contain a carboxyl group-containing monomer (a4). Such an acrylic polymer (A) usually has structural units derived from the alkyl (meth)acrylate (a1), as well as structural units derived from the copolymerizable monomers (a2) to (a10) contained in the copolymerization components.

[0070] [Alkyl (meth)acrylate (a1)] The alkyl (meth)acrylate (a1) is a linear or branched alkyl (meth)acrylate having an alkyl group with 3 to 30 carbon atoms, and is represented by the following formula (Chemical Formula 1). CH2=C(R 1 )-COO(R 2 )...(Case 1) (In Chemical 1, R 1 represents a hydrogen atom or a methyl group, R 2 represents a linear or branched alkyl group having 3 to 30 carbon atoms.

[0071] Examples of the alkyl (meth)acrylate represented by the formula (Chemical Formula 1) include linear alkyl (meth)acrylates such as n-propyl (meth)acrylate, i-propyl (meth)acrylate, n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-heptyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, n-decyl (meth)acrylate, undecyl (meth)acrylate, lauryl (meth)acrylate, n-tridecyl (meth)acrylate, n-tetradecyl (meth)acrylate, cetyl (meth)acrylate, stearyl (meth)acrylate, icosyl (meth)acrylate, henicosyl (meth)acrylate, and behenyl (meth)acrylate; sec-butyl (meth)acrylate, Branched chain alkyl (meth)acrylates such as isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, isobornyl (meth)acrylate, isostearyl (meth)acrylate, isoicosyl (meth)acrylate, butyloctyl (meth)acrylate, isomyristyl (meth)acrylate, isocetyl (meth)acrylate, hexyldecyl (meth)acrylate, isostearyl (meth)acrylate, octyldecyl (meth)acrylate, octyldodecyl (meth)acrylate, and isobehenyl (meth)acrylate can be mentioned. These may be used alone or in combination of two or more.

[0072] Among these, from the viewpoint of obtaining flexibility, linear alkyl (meth)acrylates are preferred. From the viewpoint of balancing adhesion and flexibility, linear alkyl (meth)acrylates having 3 to 20 carbon atoms in the alkyl group, further 5 to 18 carbon atoms, particularly 6 to 16 carbon atoms, and especially 7 to 14 carbon atoms are preferred, such as n-butyl (meth)acrylate, n-pentyl (meth)acrylate, n-hexyl (meth)acrylate, n-octyl (meth)acrylate, n-nonyl (meth)acrylate, decyl (meth)acrylate, and lauryl (meth)acrylate.

[0073] Among these, a branched alkyl (meth)acrylate, i.e., an alkyl (meth)acrylate containing a tertiary carbon atom in the alkyl group, is preferred because a hydrogen abstraction reaction described later is likely to occur during irradiation with active energy rays, and as a result, a crosslinked structure can be efficiently formed. Among these, a branched alkyl (meth)acrylate having an alkyl group with 3 to 20 carbon atoms, more preferably 5 to 18, particularly preferably 6 to 16, and especially preferably 7 to 14 carbon atoms is preferred, and for example, sec-butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, isopentyl (meth)acrylate, neopentyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isooctyl (meth)acrylate, isononyl (meth)acrylate, isodecyl (meth)acrylate, and isobornyl (meth)acrylate are particularly preferred.

[0074] The ratio of the alkyl (meth)acrylate (a1)-derived structural unit to the acrylic polymer (A) is usually 5 to 95% by mass, preferably 10 to 90% by mass, more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass. If the ratio of the alkyl (meth)acrylate (a1)-derived structural unit is equal to or greater than the lower limit, the flexibility tends to be excellent, and the conformability to unevenness tends to be excellent when the adherend has unevenness. If the ratio is equal to or less than the upper limit, the effect of the copolymerizable monomer described below is easily obtained, and the adhesive strength and cohesive strength tend to be excellent.

[0075] [Hydroxyl group-containing monomer (a2)] Examples of the hydroxyl group-containing monomer (a2) include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 5-hydroxypentyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 8-hydroxyoctyl (meth)acrylate; caprolactone-modified hydroxy (meth)acrylates such as caprolactone-modified 2-hydroxyethyl (meth)acrylate; diethylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, polytetramethylene glycol (meth)acrylate, and polyoxyethylene poly(meth)acrylate. Examples of the hydroxyl group-containing (meth)acrylate include (meth)acrylates having an oxyalkylene structure such as oxypropylene glycol (meth)acrylate, primary hydroxyl group-containing (meth)acrylates such as 2-acryloyloxyethyl-2-hydroxyethyl phthalate, secondary hydroxyl group-containing (meth)acrylates such as 2-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, tertiary hydroxyl group-containing (meth)acrylates such as 2,2-dimethyl 2-hydroxyethyl (meth)acrylate, and vinyl ethers such as 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, and 4-hydroxybutyl vinyl ether. These may be used alone or in combination of two or more. The hydroxyl group-containing monomer (a2) improves the adhesive strength of the pressure-sensitive adhesive sheet and suppresses whitening under wet heat. In addition, when the pressure-sensitive adhesive composition contains a thermal crosslinking agent described below, the monomer (a2) serves as a crosslinking reaction site.

[0076] Among the hydroxyl group-containing monomers (a2), hydroxyl group-containing monomers having a hydroxyalkyl group having 1 to 10 carbon atoms, further 1 to 6, especially 2 to 4 carbon atoms, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 2-hydroxyethyl vinyl ether, diethylene glycol monovinyl ether, 4-hydroxybutyl vinyl ether, etc. are preferred, and primary hydroxyl group-containing (meth)acrylates, such as 2-hydroxyethyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate are particularly preferred.

[0077] When the acrylic polymer (A) has a structural unit derived from a hydroxyl group-containing monomer (a2), the content thereof is usually 3 to 30% by mass, preferably 5 to 25% by mass, and particularly preferably 7 to 20% by mass, based on the acrylic polymer (A) from the viewpoint of imparting adhesive strength and resistance to wet heat whitening.

[0078] [Nitrogen-containing monomer (a3)] Examples of the nitrogen-containing monomer (a3) ​​include amino group-containing monomers, amide group-containing monomers, isocyanate group-containing monomers, and (meth)acrylonitrile. These may be used alone or in combination of two or more. The nitrogen-containing monomer (a3) ​​improves the cohesive strength of the pressure-sensitive adhesive sheet and can suppress wet heat whitening. In addition, when a hydrogen abstraction type photoinitiator described below is used, the acrylic polymer (A) preferably has a structural unit derived from the nitrogen-containing monomer (a3). When a hydrogen abstraction type photoinitiator described below is used, the nitrogen-containing monomer (a3) ​​has the effect of promoting the hydrogen abstraction reaction.

[0079] Examples of the amino group-containing monomer include primary amino group-containing (meth)acrylates such as aminomethyl (meth)acrylate and aminoethyl (meth)acrylate; secondary amino group-containing (meth)acrylates such as t-butylaminoethyl (meth)acrylate and t-butylaminopropyl (meth)acrylate; tertiary amino group-containing (meth)acrylates such as ethylaminoethyl (meth)acrylate, dimethylaminoethyl (meth)acrylate, diethylaminoethyl (meth)acrylate, dimethylaminopropyl (meth)acrylate, diethylaminopropyl (meth)acrylate, and dimethylaminopropylacrylamide; and monomers such as N-vinylpyrrolidone, methylvinylpyrrolidone, vinylpyridine, vinylpiperidone, vinylpyrimidine, vinylpiperazine, vinylpyrazine, vinylpyrrole, vinylimidazole, vinyloxazole, vinylmorpholine, (meth)acryloylmorpholine, N-vinylacetamides, and N-vinylcaprolactam.

[0080] Examples of the amide group-containing monomer include (meth)acrylamide; N-alkyl (meth)acrylamides such as N-methyl (meth)acrylamide, N-ethyl (meth)acrylamide, N-propyl (meth)acrylamide, Nn-butyl (meth)acrylamide, diacetone (meth)acrylamide, and N,N'-methylene bis (meth)acrylamide; N,N-dialkyl (meth)acrylamides such as N,N-dimethyl (meth)acrylamide, N,N-diethyl (meth)acrylamide, N,N-dipropyl (meth)acrylamide, N,N-ethyl methyl acrylamide, and N,N-diallyl (meth)acrylamide; hydroxyalkyl (meth)acrylamides such as N-hydroxymethyl (meth)acrylamide and N-hydroxyethyl (meth)acrylamide; alkoxyalkyl (meth)acrylamides such as N-methoxymethyl (meth)acrylamide and N-(n-butoxymethyl) (meth)acrylamide; maleimide or its derivatives. Among them, (meth)acrylamide is preferred.

[0081] Examples of the isocyanate group-containing monomer include 2-(meth)acryloyloxyethyl isocyanate and its alkylene oxide adducts, etc. The isocyanate group may be protected with a blocking agent such as methyl ethyl ketone oxime, 3,5-dimethylpyrazole, 1,2,4-triazole, diethyl malonate, etc.

[0082] Among these, those having a tertiary nitrogen atom are preferred, since they have a sensitizing effect on the hydrogen abstraction reaction by the hydrogen abstraction photoinitiator described later, and as a result, can efficiently form a crosslinked structure. Tertiary amino group-containing (meth)acrylates, N,N-dialkyl(meth)acrylamides, N-vinylpyrrolidone, acryloylmorpholine, and the like are particularly preferred.

[0083] When the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3), the content thereof is usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, based on the acrylic polymer (A), from the viewpoint of imparting cohesive strength and resistance to wet heat whitening.

[0084] [Carboxy group-containing monomer (a4)] Examples of the carboxyl group-containing monomer (a4) include (meth)acrylic acid, 2-(meth)acryloyloxyethylhexahydrophthalic acid, 2-(meth)acryloyloxypropylhexahydrophthalic acid, 2-(meth)acryloyloxyethylphthalic acid, 2-(meth)acryloyloxypropylphthalic acid, 2-(meth)acryloyloxyethylmaleic acid, 2-(meth)acryloyloxypropylmaleic acid, 2-(meth)acryloyloxyethylsuccinic acid, 2-(meth)acryloyloxypropylsuccinic acid, crotonic acid, fumaric acid, maleic acid, itaconic acid, etc. These may be used alone or in combination of two or more.

[0085] When the acrylic polymer (A) has a structural unit derived from a carboxy group-containing monomer (a4), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0086] [Epoxy group-containing monomer (a5)] Examples of the epoxy group-containing monomer (a5) include glycidyl (meth)acrylate, methyl glycidyl (meth)acrylate, 3,4-epoxycyclohexylmethyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate glycidyl ether. These may be used alone or in combination of two or more.

[0087] When the acrylic polymer (A) has a structural unit derived from an epoxy group-containing monomer (a5), the content thereof is usually 0.1 to 15 mass%, preferably 0.3 to 13 mass%, more preferably 0.5 to 10 mass%, and particularly preferably 1 to 6 mass%, based on the acrylic polymer (A).

[0088] [Vinyl monomers (a6)] The vinyl monomer (a6) may be a compound having a vinyl group in the molecule. Examples of such a compound include vinyl ester monomers such as vinyl acetate, vinyl propionate, vinyl laurate, and vinyl stearate, and aromatic vinyl monomers such as styrene, chlorostyrene, chloromethylstyrene, α-methylstyrene, and other substituted styrenes. These may be used alone or in combination of two or more.

[0089] When the acrylic polymer (A) has a constituent portion derived from a vinyl monomer (a3), the content thereof is, from the viewpoint of imparting cohesive strength to the pressure-sensitive adhesive sheet, usually 1 to 40 mass %, preferably 5 to 35 mass %, more preferably 8 to 30 mass %, and particularly preferably 10 to 25 mass %, relative to the acrylic polymer (A).

[0090] [Alkyl (meth)acrylate monomer (a7) having an alkyl group with 1 or 2 carbon atoms] Examples of the alkyl (meth)acrylate monomer (a7) in which the alkyl group has 1 or 2 carbon atoms include methyl (meth)acrylate and ethyl (meth)acrylate. These may be used alone or in combination of two or more.

[0091] When the acrylic polymer (A) has a structural unit derived from an alkyl (meth)acrylate monomer (a7), the content thereof is, from the viewpoint of imparting cohesive strength to the pressure-sensitive adhesive sheet, usually 1 to 60 mass %, preferably 5 to 55 mass %, particularly preferably 10 to 50 mass %, and especially preferably 15 to 45 mass %, relative to the acrylic polymer (A).

[0092] [Alicyclic monomer (a8)] Examples of the alicyclic monomer (a8) include cyclohexyl (meth)acrylate, 3,3,5-trimethylcyclohexyl (meth)acrylate, isobornyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, t-butylcyclohexyl (meth)acrylate, adamantyl (meth)acrylate, etc. These may be used alone or in combination of two or more.

[0093] When the acrylic polymer (A) has a structural unit derived from an alicyclic monomer (a8), the content thereof is, from the viewpoint of imparting cohesive strength to the pressure-sensitive adhesive sheet, usually 0.1 to 15 mass %, preferably 0.5 to 13 mass %, particularly preferably 1 to 10 mass %, and especially preferably 2 to 7 mass %, based on the acrylic polymer (A).

[0094] [Macromonomer (a9)] The macromonomer (a9) is a monomer that, when polymerized into the acrylic polymer (A), can easily increase the number of carbon atoms in the side chain of the acrylic polymer (A), for example, to 20 or more. By using the macromonomer (a9) as a copolymerization component, the acrylic polymer (A) can be made into a graft copolymer having a constituent part (segment) derived from the macromonomer (a9). In addition, by changing the blending ratio of the macromonomer (a9) to other monomers, the properties of the main chain and side chain of the graft copolymer can be changed.

[0095] The macromonomer (a9) has a radically polymerizable functional group, or a functional group such as a hydroxyl group, an isocyanate group, an epoxy group, a carboxyl group, an amino group, an amide group, a thiol group, etc. The macromonomer (a9) may have these functional groups alone or in combination of two or more kinds. Among them, the macromonomer (a9) is preferably one having a radically polymerizable functional group capable of copolymerizing with other monomers, and may contain one or more radically polymerizable functional groups, with one being particularly preferred. Furthermore, when the macromonomer (a9) has a functional group, it may contain one or more functional groups, but it is particularly preferred that the macromonomer (a9) contains one functional group.

[0096] The macromonomer (a9) preferably has a skeleton component composed of an acrylic polymer or a vinyl polymer. Examples of the backbone component of the macromonomer (a9) include the alkyl(meth)acrylate (a1) having 3 to 30 carbon atoms in the alkyl group, the vinyl monomer (a6), the alkyl(meth)acrylate monomer (a7) having 1 or 2 carbon atoms in the alkyl group, and the alicyclic monomer (a8). These may be used alone or in combination of two or more kinds. Among these, it is preferable to use, as the backbone component, an alkyl (meth)acrylate having an alkyl group with 1 to 8 carbon atoms, an alicyclic monomer, or an aromatic monomer such as styrene, since this allows the pressure-sensitive adhesive sheet to have excellent cohesive strength. On the other hand, the use of an alkyl (meth)acrylate having 9 to 30 carbon atoms is preferable in that it allows the production of a pressure-sensitive adhesive sheet with excellent flexibility.

[0097] The number average molecular weight of the macromonomer (a9) is preferably 1,000 or more and 40,000 or less, more preferably 1,500 or more and 20,000 or less, and even more preferably 2,000 or more and 15,000 or less. The number average molecular weight of the macromonomer (a9) is a value calculated as standard polystyrene as measured by gel permeation chromatography (GPC).

[0098] As the macromonomer (a9), a generally produced macromonomer (for example, a macromonomer manufactured by Toagosei Co., Ltd.) can be appropriately used.

[0099] When the acrylic polymer (A) has a structural unit derived from the macromonomer (a9), the content thereof is usually 1 to 30% by mass, preferably 3 to 20% by mass, and more preferably 5 to 18% by mass, based on the acrylic polymer (A). If it is equal to or greater than the lower limit, the phase separation force between the segment containing the structural unit derived from the macromonomer (a9) and the segment formed by the other structural units becomes stronger, and the cohesive force of the pressure-sensitive adhesive sheet tends to be better. If it is equal to or less than the upper limit, the phase separation structure is more likely to collapse during lamination, and the unevenness-following ability tends to be better.

[0100] [Other copolymerizable monomers (a10)] Examples of the other copolymerizable monomers (a10) include (meth)acrylates having an alkoxyalkylene glycol skeleton, such as methoxydiethylene glycol (meth)acrylate, methoxypolyethylene glycol (meth)acrylate, butoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, butoxypolypropylene glycol (meth)acrylate, methoxypolytetramethylene glycol (meth)acrylate, butoxypolytetramethylene glycol (meth)acrylate, methoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate, and butoxypolyoxyethylene polyoxypropylene glycol (meth)acrylate; phenyl (meth)acrylate, benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenyldiethylene glycol (meth)acrylate, phenoxypolyethylene glycol (meth)acrylate, and phenoxypolyethylene glycol-polypropylene glycol-(meth)acrylate. Aromatic (meth)acrylates such as acrylates and nonylphenol ethylene oxide adduct (meth)acrylates, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxybenzophenone, 4- ... Examples of the benzophenone structure-containing (meth)acrylates include methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, and mixtures thereof, heterocyclic ring-containing (meth)acrylates such as tetrahydrofurfuryl (meth)acrylate, and macromonomers. These may be used alone or in combination of two or more.

[0101] When the acrylic polymer (A) has a structural unit derived from another copolymerizable monomer (a10), the content thereof is usually 1 to 30 mass %, preferably 3 to 20 mass %, and more preferably 5 to 15 mass %, based on the acrylic polymer (A).

[0102] The method for producing the acrylic polymer (A) is not particularly limited, and may be, for example, by polymerizing a copolymerization component including an alkyl (meth)acrylate (a1) and, if necessary, at least one selected from the group consisting of copolymerizable monomers (a2) to (a10).

[0103] Examples of the polymerization method include conventionally known methods such as solution polymerization, suspension polymerization, bulk polymerization, and emulsion polymerization. Among these, solution polymerization is preferred in that it can safely and stably produce an acrylic resin with any monomer composition. Thus, the acrylic polymer (A) can be obtained.

[0104] The acrylic polymer (A) may have a photoactive site, such as a polymerizable carbon-carbon double bond group, introduced into its side chain, which can increase the crosslinking efficiency of the pressure-sensitive adhesive composition and crosslink the pressure-sensitive adhesive composition in a shorter time, thereby increasing productivity.

[0105] Examples of a method for introducing a polymerizable carbon-carbon double bond group into a side chain of the acrylic polymer (A) include a method in which a copolymer containing a functional group-containing ethylenically unsaturated monomer such as the above-mentioned hydroxyl group-containing monomer (a2), nitrogen atom-containing monomer (a3), carboxy group-containing monomer (a4), or epoxy group-containing monomer (a5) is prepared, and then a compound having a functional group reactive with the functional group and a polymerizable carbon-carbon double bond group is subjected to a condensation or addition reaction while maintaining the activity of the polymerizable carbon-carbon double bond group.

[0106] Examples of combinations of these functional groups include epoxy groups (glycidyl groups) and carboxy groups, amino groups and carboxy groups, amino groups and isocyanate groups, epoxy groups (glycidyl groups) and amino groups, hydroxyl groups and epoxy groups, and hydroxyl groups and isocyanate groups. Among these combinations of functional groups, the combination of hydroxyl groups and isocyanate groups is preferred because of the ease of reaction control. Among these, the combination in which the copolymer has a hydroxyl group and the compound has an isocyanate group is preferred.

[0107] Examples of the isocyanate compound having a polymerizable carbon-carbon double bond group include the above-mentioned 2-(meth)acryloyloxyethyl isocyanate and its alkylene oxide adducts.

[0108] The content of the compound having a functional group reactive with the functional group and a polymerizable carbon-carbon double bond group is preferably 10 parts by mass or less, more preferably 5 parts by mass or less, even more preferably 1 part by mass or less, and particularly preferably 0.1 parts by mass or less, based on 100 parts by mass of the acrylic polymer (A) from the viewpoint of improving adhesion and stress relaxation properties. The lower limit is usually 0 parts by mass.

[0109] The weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 200,000 or more, more preferably 300,000 or more, and even more preferably 400,000 or more, from the viewpoint of obtaining a pressure-sensitive adhesive composition with high cohesive strength. In addition, the upper limit of the weight average molecular weight (Mw) of the acrylic polymer (A) is preferably 1.5 million or less, more preferably 1.2 million or less, even more preferably 1.1 million or less, and particularly preferably 1 million or less, from the viewpoints of handleability and uniform stirring. The lower limit and the upper limit of the weight average molecular weight of the acrylic polymer (A) can be combined in any desired manner. The weight average molecular weight of the acrylic polymer (A) is a value calculated as standard polystyrene as measured by gel permeation chromatography (GPC).

[0110] The acrylic polymer (A) is preferably a main component of the pressure-sensitive adhesive composition, where the term "main component" refers to the component that is contained in the largest proportion among the components constituting the pressure-sensitive adhesive composition. Specifically, the content of the acrylic polymer (A) is preferably 50% by mass or more, more preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total mass of the pressure-sensitive adhesive composition. The upper limit is 100% by mass, but is usually preferably 99% by mass or less, more preferably 98% by mass or less, and even more preferably 97% by mass or less.

[0111] [Crosslinking agent (B)] The pressure-sensitive adhesive composition preferably contains a crosslinking agent (B) from the viewpoint of promoting the crosslinking reaction. This allows the pressure-sensitive adhesive composition to efficiently form a crosslinked structure. In addition, when a crosslinked structure is formed in a pressure-sensitive adhesive sheet using the pressure-sensitive adhesive composition, it is possible to prevent the adhesive from spilling out during storage or application, and to obtain good adhesion and cohesion. However, in the case where the acrylic polymer (A) undergoes a hydrogen abstraction reaction due to the action of a photoinitiator (C) or the like described below, and a sufficient crosslinked structure can be formed within the acrylic polymer (A) and / or between the acrylic polymers (A), it is not necessarily necessary to contain the crosslinking agent (B).

[0112] Examples of the crosslinking agent (B) include acrylic crosslinking agents, isocyanate crosslinking agents, epoxy crosslinking agents, aziridine crosslinking agents, melamine crosslinking agents, aldehyde crosslinking agents, amine crosslinking agents, and metal chelate crosslinking agents. Among these, it is preferable to use an isocyanate crosslinking agent because of its excellent reactivity with the acrylic polymer (A). On the other hand, from the viewpoint of ease of reaction control and active energy ray curability, it is preferable to use an acrylic crosslinking agent, and it is particularly preferable to use a polyfunctional (meth)acrylate.

[0113] Examples of the polyfunctional (meth)acrylate include polyfunctional (meth)acrylic monomers and polyfunctional (meth)acrylic oligomers having two or more (meth)acryloyl groups, which may be used alone or in combination of two or more.

[0114] Examples of the polyfunctional (meth)acrylic monomer include pentanediol di(meth)acrylate, hexadiol di(meth)acrylate, heptanediol di(meth)acrylate, octanediol di(meth)acrylate, nonanediol di(meth)acrylate, decanediol di(meth)acrylate, undecanediol di(meth)acrylate, dodecanediol di(meth)acrylate, 1,4-Butanediol di(meth)acrylate, glycerin di(meth)acrylate, neopentyl glycol di(meth)acrylate, glycerin glycidyl ether di(meth)acrylate, tricyclodecane dimethacrylate, tricyclodecane dimethanol di(meth)acrylate, bisphenol A polyethoxy di(meth)acrylate, bisphenol A polypropoxy di(meth)acrylate, bisphenol F polyethoxy di(meth)acrylate, ethylene glycol di(meth)acrylate (meth)acrylate, neopentyl glycol di(meth)acrylate, trimethylolpropane trioxyethyl (meth)acrylate, ε-caprolactone modified tris(2-hydroxyethyl) isocyanurate tri(meth)acrylate, pentaerythritol tri(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate, ethoxylated pentaerythritol tri(meth)acrylate, pentaerythritol tetra(meth)acrylate, propoxylated pentaerythritol tri(meth)acrylate Taerythritol tetra(meth)acrylate, ethoxylated pentaerythritol tetra(meth)acrylate, dipentaerythritol hexa(meth)acrylate, polyethylene glycol di(meth)acrylate, polypropylene glycol di(meth)acrylate, polytetramethylene glycol di(meth)acrylate, tris(acryloxyethyl)isocyanurate, dipentaerythritol hexa(meth)acrylate, dipentaerythritol penta(meth)acrylate , tripentaerythritol hexa(meth)acrylate, tripentaerythritol penta(meth)acrylate, hydroxypivalic acid neopentyl glycol di(meth)acrylate, di(meth)acrylate of hydroxypivalic acid neopentyl glycol adduct of ε-caprolactone, trimethylolpropane tri(meth)acrylate, trimethylolpropane polyethoxy tri(meth)acrylate, ditrimethylolpropane tetra(meth)acrylate, etc.

[0115] Examples of the polyfunctional (meth)acrylic oligomer include polyfunctional (meth)acrylic oligomers such as polyester (meth)acrylate oligomers, epoxy (meth)acrylate oligomers, urethane (meth)acrylate oligomers, and polyether (meth)acrylate oligomers.

[0116] Among these crosslinking agents (B), polyfunctional (meth)acrylate monomers and oligomers having a glycol structure are preferred from the viewpoint of imparting appropriate flexibility to the cured product, and acrylic acid adducts of pentaerythritol and dipentaerythritol, and alkoxylated products thereof are preferred from the viewpoint of imparting cohesive strength.

[0117] When the pressure-sensitive adhesive composition contains a crosslinking agent (B), the content thereof is usually 0.1 parts by mass or more, preferably 0.5 parts by mass or more, and more preferably 1 part by mass or more, based on 100 parts by mass of the acrylic polymer (A), from the viewpoint of imparting shape stability to the pressure-sensitive adhesive sheet and durability when made into a laminate for an image display device. The upper limit is usually 25 parts by mass or less, preferably 22 parts by mass or less, more preferably 20 parts by mass or less, and particularly preferably 18 parts by mass or less, from the viewpoint of maintaining the flexibility of the pressure-sensitive adhesive sheet. The lower limit and the upper limit of the content of the crosslinking agent (B) can be combined in any desired manner.

[0118] [Photoinitiator (C)] The pressure-sensitive adhesive composition preferably contains a photoinitiator (C). The photoinitiator (C) is a compound that generates radicals when exposed to active energy rays. The photoinitiator (C) is roughly classified into two types according to the radical generating mechanism. More specifically, it is roughly classified into a cleavage type photoinitiator capable of generating radicals by cleaving and decomposing the single bond of the photoinitiator itself, and a hydrogen abstraction type photoinitiator capable of generating radicals by an excited initiator abstracting hydrogen from a hydrogen donor in the system. These may be used alone or in combination of two or more kinds. The cleavage-type photoinitiator is preferred in that it has high photosensitivity. On the other hand, hydrogen abstraction type photoinitiators are preferred because they do not produce photodecomposition products and can incorporate the acrylic polymer (A) into a crosslinked structure by a hydrogen abstraction reaction.

[0119] Examples of the hydrogen abstraction type photoinitiator include benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, 2-methylbenzoylbenzoate, 4-[(4-methylphenyl)thio]benzophenone, 4-acryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, 4-acryloyloxy-4'-bromobenzophenone, 4-acryloyloxyethoxy-4'-bromobenzophenone, 4-methacryloyloxyethoxy-4'-bromobenzophenone, Examples of the photoinitiator include intermolecular hydrogen abstraction photoinitiators such as acryloyloxybenzophenone, 4-methacryloyloxyethoxybenzophenone, 4-methacryloyloxy-4'-methoxybenzophenone, 4-methacryloyloxyethoxy-4'-methoxybenzophenone, 4-methacryloyloxy-4'-bromobenzophenone, and 4-methacryloyloxyethoxy-4'-bromobenzophenone; and intramolecular hydrogen abstraction photoinitiators such as methylbenzoylformate, methyl benzoylformate, oxyphenylacetic acid-2-(2-oxo-2-phenyl-acetoxy-ethoxy)ethyl ester, and oxyphenylacetic acid-2-(2-hydroxy-ethoxy)ethyl ester. These may be used alone or in combination of two or more kinds.

[0120] Among the intermolecular hydrogen abstraction type photoinitiators, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, and photoinitiators (c1) having a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals in the molecule, such as 4-acryloyloxybenzophenone, 4-methacryloyloxybenzophenone, 4-acryloyloxyethoxybenzophenone, 4-acryloyloxy-4'-methoxybenzophenone, 4-acryloyloxyethoxy-4'-methoxybenzophenone, and 4-methacryloyloxybenzophenone, are preferred, and 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-methacryloyloxybenzophenone, and 4-methacryloyloxybenzophenone are more preferred. The photoinitiator (c1), which has a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals within its molecule, tends to be able to suppress bleed-out of the photoinitiator and improve the cohesive strength of the adhesive sheet by being incorporated into the polymerization structure after photoreaction. Furthermore, intramolecular hydrogen abstraction photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as the starting point for radical generation themselves, and methylbenzoyl formate is more preferred.

[0121] Examples of the cleavage-type photoinitiator include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)benzyl]phenyl}-2-methyl-propan-1-one, oligo(2-hydroxy-2-methyl-1-(4-(1-methylvinyl)phenyl)propanone), 2-benzyl-2-dimethylamino-1-(4-morpholinyl)phenyl)propanone, and the like. Examples of suitable phosphine oxides include bis(2,4,6-trimethylbenzoyl)phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide, bis(2,6-dimethoxybenzoyl)2,4,4-trimethylpentylphosphine oxide, and derivatives thereof.

[0122] In the present invention, it is preferable for the photoinitiator (C) to contain an intermolecular hydrogen abstraction type photoinitiator and an intramolecular hydrogen abstraction type photoinitiator, from the viewpoint of increasing the cohesive strength of the pressure-sensitive adhesive sheet.

[0123] Furthermore, in the present invention, the photoinitiator (C) preferably comprises a photoinitiator (c1) having, in the molecule, a radical-polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1). By using these photoinitiators (C) in combination, the cohesive strength of the adhesive sheet can be increased, and if the adhesive sheet is curable with active energy rays, it can be made into an adhesive sheet with excellent secondary curing properties after being attached to an adherend. The hydrogen abstraction type photoinitiator (c2) refers to a hydrogen abstraction type photoinitiator other than the photoinitiator (c1) having, in the molecule, a radical polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, among the above-mentioned hydrogen abstraction type photoinitiators. Among the hydrogen abstraction type photoinitiators (c2), intramolecular hydrogen abstraction type photoinitiators are preferred because they can act not only as hydrogen donors in the system but also as the starting point for radical generation, and methylbenzoyl formate is more preferred.

[0124] When the pressure-sensitive adhesive composition contains a photoinitiator (C), the content is usually 10 parts by mass or less, preferably 5 parts by mass or less, more preferably 4 parts by mass or less, and particularly preferably 3 parts by mass or less, based on 100 parts by mass of the acrylic polymer (A). The lower limit is usually 0.1 parts by mass. When two or more kinds of photoinitiators (C) are used in combination, the above content is the total amount of the photoinitiators (C) used.

[0125] When the photoinitiator (C) contains a photoinitiator (c1) having, in its molecule, a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates a radical, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1), the mass ratio (c2 / c1) of the photoinitiator (c2) to the photoinitiator (c1) is preferably 0.5 to 10, more preferably 1 to 8, and even more preferably 2 to 6.

[0126] [Monofunctional (meth)acrylate] The pressure-sensitive adhesive composition may further contain a monofunctional (meth)acrylate having one (meth)acryloyl group, if necessary. By containing a monofunctional (meth)acrylate having one (meth)acryloyl group, the molecular weight between crosslinking points of the cured product can be increased, so that the degree of freedom of movement of the molecular chain is increased, and it is easy to obtain a cured product with excellent stress relaxation properties, which is preferable.

[0127] Examples of the monofunctional (meth)acrylate include ethyl (meth)acrylate, propyl (meth)acrylate, isopropyl (meth)acrylate, butyl (meth)acrylate, isobutyl (meth)acrylate, t-butyl (meth)acrylate, amyl (meth)acrylate, isoamyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, decyl (meth)acrylate, isodecyl (meth)acrylate, dodecyl (meth)acrylate, and the like. (meth)acrylate, isododecyl (meth)acrylate, tetradecyl (meth)acrylate, stearyl (meth)acrylate, isostearyl (meth)acrylate, behenyl (meth)acrylate, cyclopropyl (meth)acrylate, cyclobutyl (meth)acrylate, cyclopentyl (meth)acrylate, cyclohexyl (meth)acrylate, cycloheptyl (meth)acrylate, cyclooctyl (meth)acrylate, cyclononyl (meth)acrylate, cyclodecyl (meth)acrylate, isobornyl (meth)acrylate acrylate, norbornyl (meth)acrylate, adamantyl (meth)acrylate, tricyclodecane dimethanol acrylate, ethoxylated-o-phenylphenol acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, methoxypolyethylene glycol (meth)acrylate, methoxypolypropylene glycol (meth)acrylate, polyethylene glycol (meth)acrylate, polypropylene glycol (meth)acrylate, phenoxyethylene glycol (meth)acrylate, phenoxydiethylene glycol Chole (meth)acrylate, phenoxy polyethylene glycol (meth)acrylate, 2-hydroxy-o-phenylphenol propyl acrylate, 2-(meth)acryloyloxyethyl succinate, 2-(meth)acryloyloxyethyl tetrahydrophthalate, 2-(meth)acryloyloxyethyl hexahydrophthalate, 2-(meth)acryloyloxypropyl phthalate, 2-(meth)acryloyloxypropyl hydrophthalate, 2-(meth)acryloyloxypropyl hexahydrophthalate, etc. benzyl (meth)acrylate,Benzyl (meth)acrylate, phenoxyethyl (meth)acrylate, phenoxyethylene glycol (meth)acrylate, 2-naphthyl (meth)acrylate, 9-anthracenyl (meth)acrylate, 1-pyrenylmethyl (meth)acrylate, benzyl (meth)acrylate, tricyclodecane dimethanol monoacrylate monocarboxylic acid, dicyclopentanyl acrylate, 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxybutyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, trimethylolpropane mono(meth)acrylate, glycerin mono(meth)acrylate, pentaerythritol mono(meth)acrylate, diglycerin mono(meth)acrylate, ditrimethylolpropane mono(meth)acrylate, di Examples of the acrylate include pentaerythritol mono(meth)acrylate, ethoxylated trimethylolpropane mono(meth)acrylate, propoxylated trimethylolpropane mono(meth)acrylate, ethoxylated glycerin mono(meth)acrylate, propoxylated glycerin mono(meth)acrylate, ethoxylated pentaerythritol mono(meth)acrylate, propoxylated pentaerythritol mono(meth)acrylate, ethoxylated ditrimethylolpropane mono(meth)acrylate, propoxylated ditrimethylolpropane mono(meth)acrylate, alkylene oxide-modified diglycerin mono(meth)acrylate, and alkylene oxide-modified dipentaerythritol mono(meth)acrylate, as well as monofunctional oligomers such as monofunctional urethane (meth)acrylate, monofunctional epoxy (meth)acrylate, and monofunctional polyester (meth)acrylate. These may be used alone or in combination of two or more.

[0128] When the monofunctional (meth)acrylate component is contained, the content thereof is preferably 2 parts by mass or more, more preferably 4 parts by mass or more, and particularly preferably 6 parts by mass or more, based on 100 parts by mass of the acrylic polymer (A), from the viewpoint of adjusting the crosslinking density and imparting appropriate flexibility to the cured product. The upper limit is preferably 20 parts by mass or less, more preferably 18 parts by mass or less, and particularly preferably 15 parts by mass or less.

[0129] [Other ingredients] The pressure-sensitive adhesive composition may contain various additives such as silane coupling agents, ultraviolet absorbers, plasticizers, tackifiers, antioxidants, light stabilizers, metal deactivators, anti-aging agents, moisture absorbents, rust inhibitors, and inorganic particles as "other components" as necessary, as long as the effects of the present invention are not impaired. In addition, the pressure-sensitive adhesive composition may contain reaction catalysts such as tertiary amine compounds, quaternary ammonium compounds, and tin laurate compounds as necessary. These may be used alone or in combination of two or more. These may be used alone or in combination of two or more. Among them, the pressure-sensitive adhesive composition preferably contains a silane coupling agent.

[0130] [Silane coupling agents] The silane coupling agent is an organosilicon compound containing one or more reactive functional groups and one or more alkoxy groups bonded to silicon atoms in the structure. Examples of the reactive functional groups include epoxy groups, (meth)acryloyl groups, mercapto groups, hydroxyl groups, carboxy groups, amino groups, amide groups, and isocyanate groups. Among these, epoxy groups and mercapto groups are preferred from the viewpoint of durability balance.

[0131] The alkoxy group bonded to the silicon atom preferably contains an alkoxy group having 1 to 8 carbon atoms from the viewpoint of durability and storage stability, and is particularly preferably a methoxy group or an ethoxy group. The silane coupling agent may have an organic substituent other than the reactive functional group and the alkoxy group bonded to the silicon atom, such as an alkyl group or a phenyl group.

[0132] Examples of the silane coupling agent include monomeric epoxy group-containing silane coupling agents which are silane compounds such as 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltriethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane; and silane coupling agents in which a part of the silane compound is hydrolyzed and condensed, or in which the silane compound and methyltriethoxysilane, ethyltriethoxysilane, methyltrimethoxysilane, Oligomeric epoxy group-containing silane coupling agents which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as ethyltrimethoxysilane; monomeric mercapto group-containing silane coupling agents which are silane compounds such as 3-mercaptopropyltrimethoxysilane, 3-mercaptopropyltriethoxysilane, γ-mercaptopropyldimethoxymethylsilane, 3-mercaptopropylmethyldimethoxysilane, and the like, and silane coupling agents in which a part of the silane compounds is hydrolyzed and condensed, or in which the silane compounds are hydrolyzed and condensed, or the like, and methyltriethoxysilane, ethyltriethoxysilane, methyl ... oligomeric mercapto group-containing silane coupling agents, which are silane compounds obtained by co-condensation of alkyl group-containing silane compounds such as aryltrimethoxysilane and ethyltrimethoxysilane; (meth)acryloyl group-containing silane coupling agents such as 3-acryloxypropyltrimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane, and 3-acryloxypropyltrimethoxysilane; N-2-(aminoethyl)-3-aminopropylmethyldimethoxysilane; Examples of the silane coupling agents include amino group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, 3-triethoxysilyl-N-(1,3-dimethyl-butylidene)propylamine, and N-phenyl-3-aminopropyltrimethoxysilane; isocyanate group-containing silane coupling agents such as 3-isocyanatepropyltriethoxysilane; and vinyl group-containing silane coupling agents such as vinyltrimethoxysilane and vinyltriethoxysilane. These may be used alone or in combination of two or more kinds.

[0133] Among these, from the viewpoint of excellent durability, epoxy group-containing silane coupling agents and mercapto group-containing silane coupling agents are preferably used, and among these, epoxy group-containing silane coupling agents are particularly preferred.

[0134] When the pressure-sensitive adhesive composition contains a silane coupling agent, the content thereof is usually 0.005 to 10 parts by mass, preferably 0.01 to 5 parts by mass, and particularly preferably 0.05 to 1 part by mass, based on 100 parts by mass of the acrylic polymer (A). When the content is within the above range, the adhesive strength and durability tend to be improved.

[0135] [Plasticizer] The plasticizer may be at least one selected from the group consisting of, but is not limited to, polyisobutylene, polyisoprene, polybutadiene, amorphous polyolefins and their copolymers, silicones, polyacrylates, oligomeric polyurethanes, ethylene propylene copolymers, and the like, and any combination or mixture thereof. Of these, polyisobutylene is preferred. The polyisobutylene plasticizer may be, for example, one selected from the OPPANOL B series, which is commercially available from BASF under the trade name OPPANOL.

[0136] When the pressure-sensitive adhesive composition contains a plasticizer, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, per 100 parts by mass of the acrylic polymer (A).

[0137] [Tackifier] The pressure-sensitive adhesive composition may contain a tackifier to improve the adhesive strength of the pressure-sensitive adhesive sheet. Examples of the tackifier include terpene resins such as polyterpene (e.g., α-pinene resins, β-pinene resins, and limonene resins) and aromatic modified polyterpene resins (e.g., phenol modified polyterpene resins); coumaran-indene resins; petroleum resins such as C5 hydrocarbon resins, C9 hydrocarbon resins, C5 / C9 hydrocarbon resins, and dicyclopentadiene resins; and rosins such as modified rosin, hydrogenated rosin, polymerized rosin, and rosin esters.

[0138] When the pressure-sensitive adhesive composition contains a tackifier, the content thereof is not particularly limited and is usually 0.1 to 20 parts by mass, preferably 0.5 to 15 parts by mass, based on 100 parts by mass of the acrylic polymer (A).

[0139] [Rust inhibitor] The pressure-sensitive adhesive composition may contain a rust inhibitor to prevent corrosion when the adherend contains a corrosive portion such as a metal wiring. Examples of the rust inhibitor include triazoles and benzotriazoles.

[0140] When the pressure-sensitive adhesive composition contains a rust inhibitor, the content thereof is usually 0.01 to 5 parts by mass, and preferably 0.1 to 3 parts by mass or less, based on 100 parts by mass of the acrylic polymer (A).

[0141] <Method of manufacturing the present pressure-sensitive adhesive sheet 1> Next, a method for producing the present pressure-sensitive adhesive sheet 1 will be described. However, the following explanation is merely one example of a method for producing the present pressure-sensitive adhesive sheet 1, and the present pressure-sensitive adhesive sheet 1 is not limited to those produced by this production method.

[0142] The adhesive sheet 1 can be produced by preparing an adhesive composition containing an acrylic polymer (A), preferably a crosslinking agent (B), a photoinitiator (C), and other components as necessary, forming the adhesive composition into a sheet, curing it by crosslinking, i.e., polymerization reaction, and then appropriately processing the sheet as necessary.

[0143] The pressure-sensitive adhesive composition may be prepared by kneading the raw materials using a temperature-controllable kneader (for example, a single-screw extruder, a twin-screw extruder, a planetary mixer, a twin-screw mixer, a pressure kneader, or the like). When various raw materials are kneaded, various additives such as silane coupling agents and antioxidants may be blended together with the resin in advance and then fed to the kneader, or all of the materials may be melt-mixed in advance and then fed, or a master batch in which only the additives are concentrated in the resin may be prepared and then fed.

[0144] The method for forming the pressure-sensitive adhesive composition into a sheet may be a known method, such as a wet lamination method, a dry lamination method, an extrusion casting method using a T-die, an extrusion lamination method, a calendar method, an inflation method, an injection curing method, etc. Among them, when producing a sheet, the wet lamination method, the extrusion casting method, and the extrusion lamination method are preferable.

[0145] The pressure-sensitive adhesive composition can be cured by irradiating it with active energy rays, and the pressure-sensitive adhesive composition molded body, for example, a sheet body, can be irradiated with active energy rays to produce the pressure-sensitive adhesive sheet 1. In addition to irradiating it with active energy rays, the composition can also be further cured by heating.

[0146] Furthermore, the irradiation energy, irradiation time, irradiation method, etc. of the active energy ray are not particularly limited as long as they can activate the photoinitiator (C) and polymerize the photoreactive component such as the (meth)acrylic acid ester compound. When a hydrogen abstraction type photoinitiator is used as the photoinitiator (C), a hydrogen abstraction reaction also occurs from the acrylic polymer (A), and the acrylic polymer (A) is incorporated into the crosslinked structure, thereby forming a crosslinked structure having many crosslinking points. Therefore, the present pressure-sensitive adhesive sheet 1 is preferably cured using a hydrogen abstraction type photoinitiator.

[0147] Examples of the active energy ray in the active energy ray irradiation include light rays such as far ultraviolet rays, ultraviolet rays, near ultraviolet rays, infrared rays, and visible light rays, and ionizing radiation such as X-rays, α rays, β rays, γ rays, electron beams, proton beams, and neutron beams. Among them, ultraviolet rays are preferable from the viewpoint of suppressing damage to optical device components and controlling reactions. In addition, ultraviolet rays are preferable from the viewpoint of curing speed, ease of availability of irradiation equipment, price, and the like.

[0148] Examples of light sources for ultraviolet irradiation include high-pressure mercury lamps, ultra-high-pressure mercury lamps, low-pressure mercury lamps, carbon arc lamps, metal halide lamps, xenon lamps, chemical lamps, electrodeless discharge lamps, LED lamps, etc. that emit light in the 150 to 450 nm wavelength range. Of these, it is preferable to use high-pressure mercury lamps, metal halide lamps, and LED lamps.

[0149] The amount of active energy ray irradiation (accumulated light amount) is 100 to 10,000 mJ / cm from the viewpoint of curing. 2 is preferable, and more preferably 200 to 5000 mJ / cm 2 , and more preferably 300 to 4000 mJ / cm 2 , especially 400~3000mJ / cm 2 , and even more so, 500~2000mJ / cm 2 It is preferable to carry out the reaction under the conditions of

[0150] The pressure-sensitive adhesive sheet 1 is preferably pre-cured (primary cured) by irradiation with active energy rays so that it has latent active energy ray curability, in other words, so that it retains active energy ray reactivity. When the primary curing is performed by irradiation with active energy rays, it is possible to adjust the degree of active energy ray crosslinking (gel fraction) by controlling the amount of active energy ray irradiation, but it is also possible to adjust the degree of active energy ray crosslinking (gel fraction) by using a filter or the like to partially block the active energy rays.

[0151] The adhesive sheet 1 can also be provided as an adhesive sheet with a release film having a configuration in which a release film is laminated on one or both sides of the adhesive sheet 1. From the viewpoint of preventing blocking and adhesion of foreign matter, it is preferable to cover both sides of the adhesive sheet 1 with a release film.

[0152] When release films are provided on both sides of the present pressure-sensitive adhesive sheet 1, it is preferable to use a laminate configuration in which a light release film with a relatively low release strength and a heavy release film with a relatively high release strength are laminated together. When using an adhesive sheet with release films on both sides, first one release film (light release film) is peeled off to expose one side of the adhesive sheet and then the adhesive sheet is bonded to an image display device component (referred to as the first component), and the other release film (heavy release film) is peeled off to expose the other side of the adhesive sheet, to which an image display device component (referred to as the second component) can then be bonded.

[0153] As such a release film, any known release film can be appropriately used. As the base material for the release film, for example, a film such as a polyester film, a polyolefin film, a polycarbonate film, a polystyrene film, an acrylic film, a triacetyl cellulose film, or a fluororesin film that has been subjected to a release treatment by coating with a release agent such as a silicone resin, or release paper, etc. can be appropriately selected and used. Of these, polyester films are preferred, polyethylene terephthalate (PET) films are more preferred, and biaxially oriented PET films are particularly preferred because of their excellent transparency, mechanical strength, heat resistance, flexibility, and the like. A release film can be used in which a release layer formed by curing a curable silicone-based release agent containing silicone resin as a main component is provided on the substrate.

[0154] The thickness of the release film is not particularly limited, but from the viewpoints of processability and handling, the thickness is preferably from 10 to 250 μm, more preferably from 25 to 200 μm, and particularly preferably from 35 to 190 μm.

[0155] As another embodiment of the method for producing the pressure-sensitive adhesive sheet 1, the pressure-sensitive adhesive composition can be dissolved in an appropriate solvent and various coating methods can be used. When a coating method is used, in addition to the above-mentioned curing by irradiation with active energy rays, it is also possible to obtain the present pressure-sensitive adhesive sheet 1 by thermal curing. Furthermore, when a coating method is used, the thickness of the present pressure-sensitive adhesive sheet 1 can be adjusted by the coating thickness and the solids concentration of the coating liquid.

[0156] The coating method may be a commonly used method such as roll coating, die coating, gravure coating, comma coating, screen printing, or bar coating.

[0157] To manufacture the present adhesive sheet 1 using the coating method, for example, the adhesive composition is dissolved in a solvent, and then coated on the release film, dried, and cured by active energy ray irradiation to form the present adhesive sheet 1. Furthermore, a release film may be laminated as necessary. In this case, the adhesive composition may be coated on a release film, dried, cured by active energy ray irradiation, and a release film may be laminated thereon, or the adhesive sheet 1 may be coated on a release film, dried, and a release film may be laminated thereon, and then cured by active energy ray irradiation to form the present adhesive sheet 1.

[0158] The solvent is not particularly limited as long as it dissolves the pressure-sensitive adhesive composition, and examples thereof include ester-based solvents such as methyl acetate, ethyl acetate, butyl acetate, methyl acetoacetate, and ethyl acetoacetate, ketone-based solvents such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, aromatic solvents such as toluene and xylene, and alcohol-based solvents such as methanol, ethanol, and propyl alcohol. These can be used alone or in combination of two or more. Among them, ethyl acetate, acetone, methyl ethyl ketone, and toluene are preferred from the viewpoints of solubility, drying property, and price, and ethyl acetate is particularly preferred.

[0159] The content of the solvent is preferably 600 parts by mass or less, more preferably 500 parts by mass or less, even more preferably 400 parts by mass or less, and particularly preferably 300 parts by mass or less, based on 100 parts by mass of the acrylic polymer (A) in terms of drying property, while it is preferably 1 part by mass or more, more preferably 50 parts by mass or more, even more preferably 100 parts by mass or more, and particularly preferably 150 parts by mass or more.

[0160] The solvent content in the pressure-sensitive adhesive composition after drying is preferably 1% by mass or less, more preferably 0.5% by mass or less, particularly preferably 0.1% by mass or less, and most preferably 0% by mass.

[0161] The drying temperature is usually 40 to 150° C., more preferably 45 to 140° C., further preferably 50 to 130° C., and particularly preferably 55 to 120° C. When the temperature is within the above range, the solvent can be removed efficiently and relatively safely while suppressing thermal deformation of the release film.

[0162] The drying time is usually 1 to 30 minutes, more preferably 3 to 25 minutes, and further preferably 5 to 20 minutes. When the drying time is within the above range, the solvent can be removed efficiently and sufficiently.

[0163] Examples of drying methods include drying with a dryer, drying with a heated roll, drying by blowing hot air onto the film, etc. Among these, the use of a dryer is preferred because it allows for uniform and easy drying. These methods can be used alone or in combination of two or more.

[0164] As yet another embodiment of the method for producing the present pressure-sensitive adhesive sheet 1, a pressure-sensitive adhesive composition may be prepared, coated onto a component of an image display device described below, and cured to produce the present pressure-sensitive adhesive sheet 1. However, the method is not limited to this.

[0165] In addition, the adhesive sheet 1 may be a single-layer adhesive sheet consisting of only an acrylic adhesive layer formed from an adhesive composition, or may be a multi-layer adhesive sheet in which other acrylic adhesive layers or other adhesive layers are laminated. In particular, the layer structure of the adhesive sheet 1 is preferably at least two layers, more preferably at least three layers, the outermost layer, the innermost layer, and the middle layer, and particularly preferably at least three layers, the outermost layer and the innermost layer being acrylic adhesive layers. By adopting such a layer structure, it tends to be possible to obtain an adhesive sheet that is less likely to be indented or dented even when local pressure is applied.

[0166] When the pressure-sensitive adhesive sheet 1 has at least three layers, namely, a top layer, a bottom layer, and an intermediate layer, the top layer and the bottom layer (hereinafter also referred to as "top and bottom layers") and the intermediate layer (layer sandwiched between the top layer and the bottom layer) are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) with different compositions, particularly containing acrylic polymers (A) with different compositions as main components. Such a layer structure is advantageous in that trade-off properties such as stress relaxation and shape retention can be functionally separated for each layer. The outermost layer and the innermost layer may be formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) having different compositions, particularly containing acrylic polymers (A) having different compositions as the main component, but are preferably formed from a pressure-sensitive adhesive composition containing acrylic polymers (A) having the same composition.

[0167] When the present pressure-sensitive adhesive sheet 1 has at least three layers (top layer / middle layer / bottom layer) with the top layer and bottom layer being acrylic pressure-sensitive adhesive layers, the top layer and bottom layer (surfaces to be attached to components of an image display device) are preferably high Tg layers. Also, the middle layer sandwiched between the top layer and bottom layer is preferably a low Tg layer. Furthermore, the high Tg layers used for the top layer and bottom layer may have different glass transition temperatures (Tg), but it is preferable that the top layer and bottom layer have the same glass transition temperature, and it is particularly preferable that the top layer and bottom layer are acrylic pressure-sensitive adhesive layers formed from the same pressure-sensitive adhesive composition.

[0168] The high Tg layer refers to a layer in which the maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode is usually −25° C. or higher, preferably −10° C. or higher, and particularly preferably 0° C. or higher. The upper limit of the glass transition temperature of the high Tg layer is usually 60° C. or lower, preferably 40° C. or lower, more preferably 30° C. or lower, and even more preferably 20° C. or lower. The low Tg layer is a layer having a maximum value (glass transition temperature) of loss tangent (Tan δ) obtained by dynamic viscoelasticity measurement in the shear mode described above that is lower than the glass transition temperature of the high Tg layer, and the glass transition temperature is usually 20° C. or lower, preferably 15° C. or lower, more preferably 10° C. or lower, even more preferably 8° C. or lower, particularly preferably 5° C. or lower, and most preferably 0° C. or lower. The lower limit of the glass transition temperature of the low Tg layer is usually −80° C., preferably −60° C. or higher, more preferably −50° C. or higher, and even more preferably −40° C. or higher.

[0169] Furthermore, when the present pressure-sensitive adhesive sheet 1 has at least three layers, the outermost layer and the innermost layer being acrylic pressure-sensitive adhesive layers, the ratio of the total thickness of the outermost layer and the innermost layer to the total thickness is preferably 5 to 70%, more preferably 10 to 60%, and particularly preferably 20 to 45%. By setting the thicknesses of the outermost layer and the innermost layer within the above ranges, a pressure-sensitive adhesive sheet can be obtained that has excellent adhesion suitability and durability, such as resistance to foaming at the peripheral edge, resistance to glue extrusion, and level difference absorbency.

[0170] The pressure-sensitive adhesive sheet 1 thus obtained is an optically transparent pressure-sensitive adhesive sheet. Here, "optically transparent" means that the total light transmittance is 80% or more, preferably 85% or more, and more preferably 90% or more. The haze value of the pressure-sensitive adhesive sheet is preferably 10% or less, more preferably 5% or less, and particularly preferably 3% or less.

[0171] The thickness of the present pressure-sensitive adhesive sheet is preferably from 50 to 1000 μm, more preferably from 60 to 500 μm, and particularly preferably from 75 to 300 μm.

[0172] The pressure-sensitive adhesive sheet may be embossed or processed to have various irregularities (such as a cone, pyramid, or hemisphere) if necessary. In order to improve adhesion to various members, the surface may be subjected to various surface treatments such as corona treatment, plasma treatment, and primer treatment.

[0173] <Adhesive sheet 2> As described above, the adhesive sheet 2 has an acrylic adhesive layer, and the acrylic adhesive layer is a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3). Each component contained in the acrylic pressure-sensitive adhesive layer (syrup composition) will be described in detail below.

[0174] [Alkyl (meth)acrylate (a1)] The alkyl (meth)acrylate (a1) may be the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1, and the types of preferred monomers are also the same as those of the alkyl (meth)acrylate (a1) described in the present adhesive sheet 1.

[0175] The content of the structural unit derived from the alkyl (meth)acrylate (a1) is preferably 5 to 95% by mass relative to the acrylic pressure-sensitive adhesive layer (syrup composition) in terms of obtaining flexibility, more preferably 10 to 90% by mass, even more preferably 15 to 85% by mass, and particularly preferably 20 to 80% by mass. When the content of the structural unit derived from the alkyl (meth)acrylate (a1) is equal to or more than the lower limit, the peripheral end portion is excellent in anti-foaming property during lamination, and when it is equal to or less than the upper limit, it is preferable in terms of compatibility with other physical properties such as adhesion.

[0176] [Hydroxyl-containing monomer (a2)] The hydroxyl group-containing monomer (a2) may be the hydroxyl group-containing monomer (a2) described in the present adhesive sheet 1, and the preferred types of monomers are also the same as those of the hydroxyl group-containing monomer (a2) described in the present adhesive sheet 1.

[0177] When the acrylic pressure-sensitive adhesive layer (syrup composition) contains a structural unit derived from a hydroxyl group-containing monomer (a2), the content thereof is usually 3 to 30% by mass, preferably 5 to 25% by mass, and particularly preferably 7 to 20% by mass, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is too low, the adhesive strength and moist heat resistance when used as an adhesive tend to decrease, whereas if the content is too high, the adhesive layer is more likely to undergo a self-crosslinking reaction, and the heat resistance tends to decrease.

[0178] [Nitrogen-containing monomer (a3)] The nitrogen-containing monomer (a3) ​​may be the nitrogen-containing monomer (a3) ​​described in the present adhesive sheet 1, and the preferred types of monomers are also the same as those of the nitrogen-containing monomer (a3) ​​described in the present adhesive sheet 1.

[0179] When the acrylic pressure-sensitive adhesive layer (syrup composition) contains a structural unit derived from a nitrogen-containing monomer (a3), the content thereof is usually 0.1 to 15 mass%, preferably 0.5 to 13 mass%, particularly preferably 1 to 10 mass%, and especially preferably 2 to 7 mass%, relative to the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is too low, the adhesive strength and moist heat resistance when used as an adhesive tend to decrease, whereas if the content is too high, the adhesive layer is more likely to undergo a self-crosslinking reaction, and the heat resistance tends to decrease.

[0180] The syrup composition may also contain the copolymerizable monomers (a4) to (a10) described above in connection with the present pressure-sensitive adhesive sheet 1. The preferred types of these monomers are the same as those described above in connection with the present pressure-sensitive adhesive sheet 1. The preferred content of the structural units derived from these copolymerizable monomers (a4) to (a10), i.e., the mass ratio relative to the acrylic pressure-sensitive adhesive layer (syrup composition), is the same as the mass ratio relative to all structural units of the acrylic polymer (A) described above in connection with the present pressure-sensitive adhesive sheet 1.

[0181] Furthermore, the acrylic adhesive layer preferably contains the crosslinking agent (B) and photoinitiator (C) described above in the present adhesive sheet 1, and may also contain other components such as a silane coupling agent, described above in the present adhesive sheet 1.

[0182] [Crosslinking agent (B)] When the crosslinking agent (B) is used, the preferred compound and physical properties are the same as those of the crosslinking agent (B) described in the present pressure-sensitive adhesive sheet 1. The preferred content of the crosslinking agent (B) is usually 0.1 to 20 mass%, preferably 0.5 to 15 mass%, and particularly preferably 1 to 10 mass% relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is equal to or more than the lower limit, there is a tendency for poor curing to be prevented, and when the content is equal to or less than the upper limit, there is a tendency for moderate flexibility and excellent stress relaxation properties to be obtained.

[0183] [Photoinitiator (C)] The photoinitiator is not particularly limited as long as it is the photoinitiator (C) described above in the present adhesive sheet 1, but from the viewpoint of efficiently progressing the polymerization reaction, it is preferable for it to contain a cleavage-type photoinitiator, and among the above-mentioned cleavage-type photoinitiators, 2,2-dimethoxy-1,2-diphenylethan-1-one, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, bis(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, and (2,4,6-trimethylbenzoyl)ethoxyphenylphosphine oxide are particularly preferred. From the viewpoint of efficiently forming a crosslinked structure, it is preferable to contain a hydrogen abstraction type photoinitiator, and benzophenone, 4-methylbenzophenone, 2,4,6-trimethylbenzophenone, 4-phenylbenzophenone, 3,3'-dimethyl-4-methoxybenzophenone, and 4-(meth)acryloyloxybenzophenone are particularly preferable. The photoinitiator (C) can include one or more selected from the group consisting of cleavage type photoinitiators and / or hydrogen abstraction type photoinitiators.

[0184] When the photoinitiator (C) is used, its content is usually 0.1 to 10% by mass, preferably 0.5 to 6% by mass, and more preferably 1 to 4% by mass, based on the acrylic pressure-sensitive adhesive layer (syrup composition). If the content is equal to or more than the lower limit, curing failure tends to be prevented, while if the content is equal to or less than the upper limit, deterioration in stability such as precipitation from the pressure-sensitive adhesive sheet tends to be easily suppressed, and problems such as embrittlement and coloration tend to be easily suppressed.

[0185] [Monofunctional (meth)acrylate] When a monofunctional (meth)acrylate is used, the preferred compounds and physical properties are the same as those explained for the present pressure-sensitive adhesive sheet 1 above.

[0186] [Other ingredients] As other components, the same ones as explained in the present pressure-sensitive adhesive sheet 1 can be used. In particular, when a silane coupling agent is used, its content is usually 0.005 to 5 mass %, preferably 0.01 to 3 mass %, and more preferably 0.05 to 1 mass % relative to the acrylic pressure-sensitive adhesive layer (syrup composition). When the content is within the above range, adhesive strength and durability tend to be improved.

[0187] The syrup component constituting the syrup composition in the pressure-sensitive adhesive sheet 2 may be composed of an acrylic polymer (A) and a monomer component. In one example, such a syrup component may be formed by partial polymerization of the so-called monomer component, or may be prepared by adding the monomer component to a polymer in which the monomer component constituting the acrylic polymer (A) is completely or partially polymerized. That is, when a specific copolymerization component is partially polymerized, some of the monomers are polymerized to form oligomers or polymers, and some of the monomers remain, which can form a syrup component. In another example, a syrup-like form can be formed by adding a monomer component to a partially or completely polymerized polymer. Therefore, in this specification, the monomer unit constituting the acrylic pressure-sensitive adhesive layer may mean a monomer present in the form of an oligomer or polymer in the acrylic polymer component, or a monomer contained in the syrup component before polymerization.

[0188] <Method of manufacturing the present pressure-sensitive adhesive sheet 2> Next, a method for producing the pressure-sensitive adhesive sheet 2 will be described. However, the following explanation is merely one example of a method for producing the present pressure-sensitive adhesive sheet 2, and the present pressure-sensitive adhesive sheet 2 is not limited to those produced by this production method.

[0189] In producing the present pressure-sensitive adhesive sheet 2, a syrup composition is prepared by mixing an alkyl (meth)acrylate (a1) having an alkyl group with 3 to 30 carbon atoms, a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), and, if necessary, copolymerizable monomers (a4) to (a10), a photoinitiator (C), and the like. Next, this syrup composition is irradiated with active energy rays to carry out prepolymerization. Thereafter, the syrup composition to which, if necessary, additional photoinitiator (C), crosslinking agent (B), and other components have been added is coated on a release film or the like using various coating methods, and the pressure-sensitive adhesive sheet 2 can be obtained by curing the syrup composition by irradiating active energy rays or heating. The crosslinking agent and other components may be added to the syrup composition from the beginning, or may be added to the syrup composition after the prepolymerization is completed. Furthermore, the prepolymerization and curing may be carried out in one step.

[0190] In another embodiment of the manufacturing method of the present adhesive sheet 2, the syrup composition is dissolved in a solvent, then coated onto a release film and dried, and prepolymerized and cured by irradiation with active energy rays to form the present adhesive sheet 2.

[0191] In the method for producing the present adhesive sheet 2, the release film, active energy rays, solvent, etc., mixing method, coating method, drying conditions, etc. may follow the explanation for the present adhesive sheet 1 above.

[0192] The adhesive sheet 2 thus obtained may be a single layer sheet having only an acrylic adhesive layer, or a multilayer sheet having a plurality of acrylic adhesive layers and other adhesive layers laminated thereon. The preferred layer structure and thickness are the same as those of the adhesive sheet 1. The adhesive sheet 2 may also be provided as an adhesive sheet with a release film having a structure in which a release film is laminated on one or both sides of an adhesive layer (the adhesive sheet) made of an adhesive composition.

[0193] <Preferred uses of this adhesive sheet> The pressure-sensitive adhesive sheets 1 and 2 are preferably used for bonding optical members. Specifically, they are preferably used for bonding members constituting a display, particularly members used for producing a display, and are preferably used as pressure-sensitive adhesive sheets for bonding an image display panel and image display device components such as a protective panel or touch panel disposed on the front side (viewing side) of the image display panel, or components constituting the image display device components. Incidentally, the image display device components may be the same as those described below.

[0194] <<Laminate for image display device>> A laminate for an image display device according to an embodiment of the present invention (hereinafter, sometimes referred to as "the laminate for the image display device") is a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween. The laminate for the image display device is preferably a laminate for an image display device having a configuration in which two components of the image display device are laminated with the present pressure-sensitive adhesive sheet interposed therebetween.

[0195] Of the components of the laminate for an image display device, the pressure-sensitive adhesive sheet is as described above, and the components other than the pressure-sensitive adhesive sheet will be described below.

[0196] <Image display device components> Examples of image display device components constituting the present laminate for image display devices include flat panel image display device components, image display device components having a curved portion, and flexible image display device components. Examples of such image display device components include image display panels such as liquid crystal displays and organic electroluminescence (EL) displays, surface protection panels (surface protection films), polarizing plates, polarizing elements, retardation films, color filters, barrier films, viewing angle compensation films, brightness improvement films, contrast improvement films, diffusion films, semi-transmissive reflective films, electrode films, transparent conductive films, metal mesh films, and touch sensor films. Any one of these or two of them may be used in combination. For example, a surface protection panel may be combined with other image display device components, or may be combined with other image display device components.

[0197] Of the two image display device components, one is preferably a surface protection panel, and the other is preferably a member consisting of one or a combination of two or more of the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element, and a retardation film, and it is more preferable that the surface protection panel has a frame-shaped concealing portion on the periphery, and has a portion with a frame width of 3 mm or less. With this configuration, the effects of the present invention can be particularly enjoyed. From this perspective, it is particularly preferable that the frame has a portion with a width of 2 mm or less, and particularly preferably that the frame has a portion with a width of 1.5 mm or less.

[0198] The present laminate for an image display device is preferably fixed in a curved shape. Since the present pressure-sensitive adhesive sheet has excellent bonding reliability to curved parts, the above-mentioned configuration can particularly provide the effects of the present invention.

[0199] <Method of manufacturing the laminate for the image display device> The method for producing the present laminate for an image display device is not particularly limited, and as described above, for example, the adhesive composition may be applied onto a component of the image display device to form an adhesive sheet, or an adhesive sheet with a release film may be formed in advance and then laminated to the component of the image display device.

[0200] <<Image display devices>> An image display device according to an embodiment of the present invention (hereinafter, sometimes referred to as "the image display device") is an image display device incorporating a laminate for an image display device having a configuration in which two components of the image display device are bonded together via the pressure-sensitive adhesive sheet. For example, there can be mentioned an image display device having a structure in which a laminate for an image display device having a configuration in which two components of the image display device are bonded together via the pressure-sensitive adhesive sheet is combined with another component of the image display device. In this case, examples of "other image display device components" include FPC cables, reflective sheets, light guide plates and light sources, diffusion films, prism sheets, liquid crystal panels, organic EL panels, anti-reflection films, color filters, polarizing plates, retardation plates, glass substrates, surface protection films, and integrated composites of these components. Specific examples of the present image display device include liquid crystal displays, organic EL displays, inorganic EL displays, electronic paper, plasma displays, and microelectromechanical system (MEMS) displays used in personal computers, mobile terminals, game consoles, televisions (TVs), car navigation systems, touch panels, pen tablets, etc. EXAMPLES

[0201] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0202] Prior to the examples, the following raw materials were prepared.

[0203] [Acrylic polymer (A)] Acrylic polymers (A-1) to (A-4) having copolymer component compositions and weight average molecular weights (Mw) as shown in Table 1 below were prepared.

[0204] [Table 1]

[0205] [Crosslinking agent (B)] (B-1): Polypropylene glycol #400 diacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester APG-400") (B-2): Propoxylated pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester ATM-4PL") (B-3): Pentaerythritol tri- and tetraacrylate (manufactured by Shin-Nakamura Chemical Co., Ltd., "NK Ester ATMM-3L")

[0206] [Photoinitiator (C)] (C-1): Methyl benzoyl formate (IGM "Omnirad MBF") (C-2): 4-Methallyloyloxybenzophenone ("MBP" manufactured by Shinryo Corporation) (C-3): A mixture of 2,4,6-trimethylbenzophenone and 4-methylbenzophenone (IGM "Esacure TZT"

[0207] 〔others〕 Silane coupling agent: 3-glycidyloxypropyltrimethoxysilane ("KBM403" manufactured by Shin-Etsu Chemical Co., Ltd.)

[0208] <Example 1> A pressure-sensitive adhesive composition was prepared by uniformly mixing 100 parts by mass of an acrylic polymer (A-1), 1.5 parts by mass of a crosslinking agent (B-1), 2.45 parts by mass of a photoinitiator (C-1), 1.05 parts by mass of a photoinitiator (C-2), and 0.2 parts by mass of a silane coupling agent.

[0209] Next, the pressure-sensitive adhesive composition was spread in a sheet shape on a 100 μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment so that the thickness of the pressure-sensitive adhesive composition was 150 μm. In addition, a 75 μm-thick release film (PET film manufactured by Mitsubishi Chemical Corporation) that had been subjected to a silicone release treatment was laminated on the sheet-shaped pressure-sensitive adhesive composition. Then, using a high-pressure mercury lamp, the integrated light intensity of 365 nm was 440 mJ / cm 2 Both surfaces of the sheet-like pressure-sensitive adhesive composition were irradiated with active energy rays through the release film so as to obtain a pressure-sensitive adhesive sheet with release films consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 1 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0210] <Examples 2 to 5> A pressure-sensitive adhesive sheet with a release film was prepared in the same manner as in Example 1, except that the composition, thickness and integrated light amount were changed as shown in Table 2. The pressure-sensitive adhesive sheets of Examples 2 to 5 were pressure-sensitive adhesive sheets having active energy ray curability, that is, they were cured by irradiation with active energy rays.

[0211] <Example 6> 100 parts by mass of acrylic polymer (A-1), 1.5 parts by mass of crosslinking agent (B-1), 2.45 parts by mass of photoinitiator (C-1), 1.05 parts by mass of photoinitiator (C-2), and 0.2 parts by mass of silane coupling agent were prepared and mixed uniformly to form a pressure-sensitive adhesive composition for the front and back layers. On the other hand, 100 parts by mass of the acrylic polymer (A-4), 15 parts by mass of the crosslinking agent (B-3), and 2.0 parts by mass of the photoinitiator (C-3) were prepared and mixed uniformly to form a pressure-sensitive adhesive composition for the intermediate layer. The adhesive composition for the front and back layers and the adhesive composition for the intermediate layer were each supplied to two extruders, and co-extruded in a layer structure of two types and three layers (outermost layer / middle layer / outermost layer, thickness ratio 1:2:1) to be hot melt molded into a sheet having a thickness of 150 μm.

[0212] Next, the sheet-like adhesive composition was sandwiched between two polyethylene terephthalate films (PET film manufactured by Mitsubishi Chemical Corporation, thickness 100 μm, and PET film manufactured by Mitsubishi Chemical Corporation, thickness 75 μm) whose surfaces had been treated with a silicone release agent, i.e., two release films, to obtain a laminate consisting of release film / adhesive composition / release film. Then, using a high-pressure mercury lamp, the integrated light intensity of 365 nm was 500 mJ / cm 2 Both surfaces of the sheet-like pressure-sensitive adhesive composition were irradiated with active energy rays through the release film so as to obtain a pressure-sensitive adhesive sheet with release films consisting of release film / pressure-sensitive adhesive sheet / release film. The pressure-sensitive adhesive sheet of Example 6 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0213] <Example 7> A pressure-sensitive adhesive sheet with a release film was prepared in the same manner as in Example 6, except that the formulation, thickness, layer composition ratio and integrated light amount were changed to those shown in Table 2 below. The pressure-sensitive adhesive sheet of Example 7 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0214] <Comparative Example 1> A pressure-sensitive adhesive sheet with a release film was prepared in the same manner as in Example 1, except that the composition, thickness and integrated light amount were changed to those shown in Table 2 below. The pressure-sensitive adhesive sheet of Comparative Example 1 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0215] <Comparative Example 2> A pressure-sensitive adhesive sheet with a release film was prepared in the same manner as in Example 6, except that the formulation, thickness, layer composition ratio and integrated light amount were changed to those shown in Table 2 below. The pressure-sensitive adhesive sheet of Comparative Example 2 was an active energy ray-curable pressure-sensitive adhesive sheet that was cured by irradiation with active energy rays.

[0216] [Table 2]

[0217] [Physical property measurement and evaluation] The pressure-sensitive adhesive sheets produced in the above Examples and Comparative Examples were subjected to the following various measurements and evaluations. The evaluation results are summarized in Table 3 below.

[0218] [Shear storage modulus at 25℃ (G0')] The release film on one side of the pressure-sensitive adhesive sheets with release film produced in the Examples and Comparative Examples was removed, and the sheets were repeatedly laminated with a hand roller to adjust the thickness to about 0.8 mm, and punched out into a circle with a diameter of 8 mm to prepare a sample. The obtained sample was placed in a rheometer ("DHR-2" manufactured by TA Instruments) and subjected to dynamic viscoelasticity measurement under the conditions of measurement jig: 8 mm diameter parallel plate, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min, and the shear storage modulus at 25°C (G0'(25°C)) was read.

[0219] In addition, the adhesive sheets with release films prepared in the examples and comparative examples were irradiated with active energy rays having a wavelength of 365 nm through the release film using a metal halide lamp so that the accumulated light amount was as shown in Table 3 below, thereby curing the adhesive sheets. Using the cured pressure-sensitive adhesive sheet, the shear storage modulus at 25° C. after curing (G1′(25° C.)) was measured in the same manner as the shear storage modulus before light irradiation (G0′(25° C.)).

[0220] [Glass transition temperature] The release film on one side was removed from the pressure-sensitive adhesive sheet with release film produced in the Examples and Comparative Examples, and the sheet was repeatedly laminated with a hand roller to adjust the thickness to about 0.8 mm, and a circular sample with a diameter of 8 mm was punched out. The obtained sample was placed in a rheometer (TA Instruments' "DHR-2"), and dynamic viscoelasticity measurement was performed under the following conditions: measurement tool: 8 mm diameter parallel plate, frequency: 1 Hz, measurement temperature: -50 to 150°C, and heating rate: 5°C / min. Then, the glass transition temperature (Tg0) defined by the maximum value of Tan δ obtained by dynamic viscoelasticity measurement in shear mode at a frequency of 1 Hz was obtained. In Example 5, two maximum values ​​were observed in the dynamic viscoelasticity measurement, and the temperature at which the larger maximum value was observed is recorded in the table as the glass transition temperature (Tg0).

[0221] In addition, the adhesive sheets with release films prepared in the examples and comparative examples were irradiated with active energy rays having a wavelength of 365 nm through the release film using a metal halide lamp so that the accumulated light amount was as shown in Table 3 below, thereby curing the adhesive sheets. Using the cured pressure-sensitive adhesive sheet, the glass transition temperature after curing (Tg1) was determined in the same manner as for the glass transition temperature before light irradiation.

[0222] [Stress relaxation rate] The release film on one side of the adhesive sheets with release film produced in the Examples and Comparative Examples was removed, and the sheets were repeatedly laminated with a hand roller to adjust the thickness to approximately 0.8 mm, and then punched out into a circle with a diameter of 25 mm to prepare a sample. A viscoelasticity measuring device (TA Instruments, "DHR2") was used to apply a 25% strain at 70°C to the obtained sample, and the storage modulus after 0.1 seconds was read as the initial modulus (G0'(0)). In addition, a 25% strain was applied at 70°C, and the storage modulus after 300 seconds was read as the relaxation modulus (G0'(300)). The values ​​of the initial modulus (G0'(0)) and the relaxation modulus (G0'(300)) were substituted into the following formula (I) to calculate the stress relaxation rate (X0). Stress relaxation rate (X0) = (G0'(300) / G0'(0)) (I)

[0223] In addition, the adhesive sheets with release films prepared in the examples and comparative examples were irradiated with active energy rays having a wavelength of 365 nm through the release film using a metal halide lamp so that the accumulated light amount was as shown in Table 3 below, thereby curing the adhesive sheets. Using the cured pressure-sensitive adhesive sheet, the initial elastic modulus (G1'(0)) and relaxation elastic modulus (G1'(300)) after curing were measured in the same manner as in the measurement of the stress relaxation rate before light irradiation. The initial elastic modulus (G1'(0)) and relaxation elastic modulus (G1'(300)) after curing were substituted into the following formula (II) to calculate the stress relaxation rate after curing (X1). Stress relaxation rate (X1) = (G1'(300) / G1'(0)) (II)

[0224] Further, the difference (X1-X0) between the stress relaxation rate before and after curing was calculated from the stress relaxation rate (X0) and the stress relaxation rate after curing (X1).

[0225] [Gel fraction] For the adhesive sheets with release film prepared in the Examples and Comparative Examples, about 0.1 g of adhesive sheet pieces were collected from the adhesive sheets from which the release film was peeled off. The collected adhesive sheet pieces were wrapped in a SUS mesh (#150) with a mass (X) that had been previously made into a bag shape, and the mouth of the bag was closed to prepare a sample, and the mass (Y) of the sample was measured. The sample was immersed in ethyl acetate and stored in a dark place at 23°C for 24 hours, and then the sample was taken out and heated at 70°C for 4.5 hours to evaporate the ethyl acetate, and the mass (Z) of the dried sample was measured. The gel fraction before light irradiation was calculated from each measured mass according to the following formula. Gel fraction (%) = [(ZX) / (YX)] x 100

[0226] In addition, the adhesive sheets with release films prepared in the examples and comparative examples were irradiated with active energy rays having a wavelength of 365 nm through the release film using a high-pressure mercury lamp so that the accumulated light amount was as shown in Table 3, thereby curing the adhesive sheets. Using the cured pressure-sensitive adhesive sheet, the gel fraction after curing was calculated in the same manner as the gel fraction before light irradiation.

[0227] [Adhesive strength] The release film on one side was removed from the adhesive sheet with release film prepared in the Examples and Comparative Examples, and a PET film (Toyobo Co., Ltd., Cosmoshine A4300, thickness 100 μm) was attached as a backing film with a hand roller. This was cut into a strip of width 10 mm x length 150 mm, and the remaining release film was peeled off to expose the adhesive sheet surface, which was attached to the surface of soda lime glass with a hand roller. The obtained laminate was subjected to autoclave treatment (60°C, gauge pressure 0.2 MPa, 20 minutes) for finish attachment to prepare an adhesive strength measurement sample. The obtained adhesive strength measurement sample was pulled at an angle of 180° at a peeling speed of 60 mm / min under conditions of 23°C and 50% RH, and the adhesive sheet together with the backing film was peeled off from the soda-lime glass, and the tensile strength (N / cm) was measured with a load cell to determine the adhesive strength.

[0228] [Adhesive strength after curing] The release film on one side was removed from the adhesive sheet with release film prepared in the Examples and Comparative Examples, and a PET film (Toyobo Co., Ltd., Cosmoshine A4300, thickness 100 μm) was attached as a backing film with a hand roller. This was cut into a strip of width 10 mm x length 150 mm, and the remaining release film was peeled off to expose the adhesive sheet surface, which was attached to the surface of soda lime glass with a hand roller. The obtained laminate was subjected to autoclave treatment (60 ° C, gauge pressure 0.2 MPa, 20 minutes) for finishing and attachment. Thereafter, the adhesive sheet was irradiated with light through the backing film using a high-pressure mercury lamp so that the active energy rays with a wavelength of 365 nm were the accumulated light amount shown in Table 3, and the adhesive sheet was cured to obtain an adhesive strength measurement sample. The obtained adhesive strength measurement sample was pulled at an angle of 180° at a peeling speed of 60 mm / min under conditions of 23°C and 50% RH, and the adhesive sheet together with the backing film was peeled off from the soda-lime glass, and the tensile strength (N / cm) was measured with a load cell to obtain the adhesive strength after curing.

[0229] [Bubble resistance (edge ​​bubble)] The adhesive sheets with release film prepared in the Examples and Comparative Examples were cut to 45 mm × 45 mm. The release film on one side of the cut adhesive sheet was removed, and the exposed adhesive surface was roll-pressed onto a soda-lime glass (54 mm × 82 mm × thickness 0.6 mm). The remaining release film was then peeled off, and a polarizing plate (54 mm x 82 mm x 0.1 mm thick) was roll-laminated, after which it was autoclaved (temperature 60°C, gauge pressure 0.8 MPa, 8 minutes) to finish lamination, producing a glass / adhesive sheet / polarizing plate laminate. The obtained laminate was irradiated from the soda lime glass side with an integrated light intensity of 3000 mJ / cm at a wavelength of 365 nm. 2 The sample was irradiated with active energy rays using a metal halide lamp so that the edge bubble resistance was evaluated. Eight evaluation samples were prepared for each example. The number of bubbles that had occurred within 1 mm from the edge of the adhesive sheet was counted, and the average number of bubbles at the edge per sample was calculated. A sample with an average number of bubbles of 10 or less was rated as "○ (good)", and a sample with an average number of bubbles of more than 10 was rated as "× (poor)".

[0230] [Anti-glue spillage] The release film on one side of the adhesive sheets with release film produced in the Examples and Comparative Examples was peeled off and the sheets were cut in half to 10 mm x 10 mm. The exposed adhesive surface was placed opposite a piece of soda lime glass with a thickness of 0.6 mm, and the adhesive sheet and the glass were pressure-bonded using a vacuum laminator at a temperature of 23°C, a gauge pressure of 0.4 MPa, and a pressure application time of 60 seconds. The adhesive overflow distance from the half-cut mark at the center of each side of the adhesive sheet was measured, and the average value of the four sides was taken as the adhesive overflow distance (μm). Adhesive overflow distances of 100 μm or less were judged as "◎ (excellent)", those of 200 μm or less were judged as "○ (good)", and those of more than 200 μm were judged as "× (poor)".

[0231] [Table 3]

[0232] The pressure-sensitive adhesive sheets of the examples had a stress relaxation rate (X0) of 0.20 or less, and had excellent resistance to foaming at the end faces. This is thought to be because the excellent stress relaxation properties allowed the gas trapped during lamination to escape easily, and even if bubbles were generated, they would disappear easily over time. Furthermore, the pressure-sensitive adhesive sheets of the examples had a predetermined initial elastic modulus (G0'(0)) value, and therefore were also excellent in resistance to adhesive extrusion. On the other hand, the pressure-sensitive adhesive sheets of Comparative Examples 1 and 2 had a high stress relaxation rate (X0) and poor end face foaming resistance. Moreover, the pressure-sensitive adhesive sheet of Comparative Example 2 had a low storage shear modulus at 25° C. (G'(25° C.)) and was poor in resistance to adhesive extrusion. [Industrial Applicability]

[0233] The pressure-sensitive adhesive sheet of the present invention has excellent adhesion and can be adhered without air bubbles even to the peripheral portion near the end face of the pressure-sensitive adhesive sheet. Therefore, the pressure-sensitive adhesive sheet can be suitably used as a pressure-sensitive adhesive sheet for image display devices, particularly image display devices with narrow frame design or frameless design.

Claims

1. A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer formed from a pressure-sensitive adhesive composition containing an acrylic polymer (A), The initial elastic modulus (G 0 '(0)) and the relaxation modulus (G 0 The pressure-sensitive adhesive sheet has a stress relaxation rate (X0) of 0.20 or less, as calculated from the following formula (I) of Stress relaxation rate (X0) = (G 0 '(300) / G 0 '(0))...(I)

2. A pressure-sensitive adhesive sheet having an acrylic pressure-sensitive adhesive layer, the acrylic pressure-sensitive adhesive layer being a cured reaction product formed from a syrup composition containing an alkyl (meth)acrylate (a1) having an alkyl group with a carbon number of 3 to 30, and a hydroxyl group-containing monomer (a2) and / or a nitrogen-containing monomer (a3), The initial elastic modulus (G 0 '(0)) and the relaxation modulus (G 0 The pressure-sensitive adhesive sheet has a stress relaxation rate (X0) of 0.20 or less, as calculated from the following formula (I) of Stress relaxation rate (X0) = (G 0 '(300) / G 0 '(0))...(I)

3. The relaxation modulus (G 0 The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein (0)′ is 5 to 100 kPa.

4. The relaxation modulus (G 0 The pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the elastic modulus (300) is 0.1 to 20 kPa.

5. 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the pressure-sensitive adhesive sheet has a gel fraction of 30 to 90%.

6. The shear storage modulus (G) at a temperature of 25° C. obtained by dynamic viscoelasticity measurement in a shear mode at a frequency of 1 Hz 0 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the compressive strength (MPa) (25° C.) is 100 kPa or more.

7. The glass transition temperature (Tg 0 3. The pressure-sensitive adhesive sheet according to claim 1, wherein the temperature is -25° C. or higher.

8. The pressure-sensitive adhesive sheet according to claim 1 , wherein the pressure-sensitive adhesive composition comprises a crosslinking agent (B) and a photoinitiator (C).

9. The pressure-sensitive adhesive composition comprises a photoinitiator (C), the photoinitiator (C) comprising a photoinitiator (c1) having in its molecule a radically polymerizable functional group having a carbon-carbon double bond and a structure that generates radicals, and a hydrogen abstraction type photoinitiator (c2) other than the photoinitiator (c1).

10. The pressure-sensitive adhesive sheet according to claim 1 , wherein the acrylic polymer (A) has a structural unit derived from a nitrogen-containing monomer (a3).

11. The pressure-sensitive adhesive sheet according to claim 1 or 2, which has active energy ray curability.

12. The pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm in an integrated amount of 2000 to 4000 mJ / cm 2 The initial elastic modulus after curing (G 1 '(0)) and the post-curing relaxation modulus (G 1 The pressure-sensitive adhesive sheet according to claim 11, wherein the post-cure stress relaxation rate (X1) calculated from the above formula (II) (300) is 0.22 or more: Stress relaxation rate after curing (X1) = (G 1 '(300) / G 1 '(0))...(II)

13. The pressure-sensitive adhesive sheet for attaching optical members according to claim 12, wherein the difference (X1-X0) between the post-cure stress relaxation rate (X1) and the stress relaxation rate (X0) is 0.01 or more.

14. The pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm in an integrated amount of 2000 to 4000 mJ / cm 2 The initial elastic modulus after curing (G 1 The pressure-sensitive adhesive sheet according to claim 11, wherein (0)′ is 1 kPa or more and 100 kPa or less.

15. The pressure-sensitive adhesive sheet is irradiated with active energy rays having a wavelength of 365 nm in an integrated amount of 2000 to 4000 mJ / cm 2 The post-curing relaxation elastic modulus (G 1 The pressure-sensitive adhesive sheet according to claim 11, wherein the elastic modulus (300) is 0.1 kPa or more and 50 kPa or less.

16. 3. A pressure-sensitive adhesive sheet with a release film, comprising: the pressure-sensitive adhesive sheet according to claim 1 or 2; and a release film laminated on the pressure-sensitive adhesive sheet.

17. A laminate for an image display device comprising two image display device components and the adhesive sheet according to claim 1 or 2 interposed between the two image display device components, wherein one of the two image display device components is a surface protection panel and the other is a member consisting of any one or a combination of two or more of the group consisting of a touch sensor film, an image display panel, a color filter, a polarizing element and a retardation film.

18. 18. The laminate for an image display device according to claim 17, wherein the surface protection panel has a frame-shaped concealing portion on its periphery, and has a portion where the frame width is 3 mm or less.

19. 18. The laminate for an image display device according to claim 17, which is fixed in a curved state.

20. An image display comprising the laminate for an image display device according to claim 17.

21. 3. A pressure-sensitive adhesive sheet for use as a component of an image display device, comprising the pressure-sensitive adhesive sheet according to claim 1 or 2.

Citation Information

Patent Citations

  • JP1974071529A

  • Split broadcast system

    JP1985062740A

Cited By

  • Double-sided adhesive sheet, double-sided adhesive sheet with release film, laminate for image display device using the same, and image display device

    WO2025205558A1

  • Pressure-sensitive adhesive sheet, pressure-sensitive adhesive sheet equipped with release film, laminate for image display device, flexible image display device, and pressure-sensitive adhesive sheet for constituent member of flexible image display device

    WO2026204833A1