Artificial leather and production method thereof

The artificial leather with specified hollow fibers and elastic polymer composition addresses the lack of heat insulation in existing leathers, offering improved thermal retention and flexibility.

JP2024139908AInactive Publication Date: 2024-10-10TORAY INDUSTRIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2023050848
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing artificial leathers lack sufficient heat insulation properties while maintaining flexibility and lightness, as highlighted in Patent Documents 1, 2, and 3.

Method used

The artificial leather is composed of a fibrous structure with hollow fibers having specific diameter and hollow ratio ranges, combined with an elastic polymer, and produced through a method involving sea-island composite fibers and a polymeric elastic material application, followed by removal of island components to create hollow fibers.

Benefits of technology

The resulting artificial leather achieves high heat insulation, flexibility, and lightness, suitable for applications like clothing and automobile interiors.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

To provide an artificial leather having high adiabaticity, flexibility, and lightness.SOLUTION: An artificial leather includes a fiber structure including a nonwoven fabric composed of a hollow fiber having an average single fiber diameter of 40 μm or more and 80 μm or less and an elastomer as components. The hollow fiber has a hollow part having an average diameter of 4 μm or more and 20 μm or less, with a hollowness of 40% or more and 95% or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an artificial leather and a method for producing the same. [Background technology]

[0002] Artificial leathers that combine mechanical properties, light weight, flexibility, and heat insulation are required for applications such as automobile interior materials, furniture, and clothing. As artificial leathers with excellent light weight, artificial leathers that include a fiber structure formed from ultrafine fibers are known.

[0003] This fiber structure can be obtained, for example, by selectively dissolving and removing only the sea component from a fiber structure made of islands-in-sea type composite fibers. As one of the means for obtaining lighter artificial leather, an artificial leather in which ultrafine fibers are hollow fibers has been proposed.

[0004] For example, Patent Document 1 proposes a sheet-like material comprising a nonwoven fabric mainly made of ultrafine hollow fibers and an elastic polymer as constituent components, in which the ultrafine hollow fibers have hollow portions extending in the longitudinal direction of the fibers therein, a specific number of which can be observed when observing a cross section of the ultrafine hollow fibers, and the total area of ​​the hollow portions in the cross section is within a specific range. It is described that this sheet-like material has high mechanical properties similar to those of solid fibers, and is suitable for artificial leather that is flexible, lightweight, and has an excellent texture.

[0005] Patent Document 2 proposes an artificial leather in which a nonwoven fabric is impregnated with an elastic polymer, the nonwoven fabric being made by heat-shrinking a certain amount of a fiber-entangled body containing a specific amount of hollow fibers (A) with a specific shrinkage rate, and the hollow rate of the hollow fibers (A') after shrinkage treatment in the nonwoven fabric, the apparent density of the nonwoven fabric, and the tensile strength converted per unit area and unit weight of the nonwoven fabric are within specific ranges.Then, it is described that the artificial leather is sufficiently light, strong, flexible, and full, and has little tendency to be crushed, and is particularly useful as a material for shoes.

[0006] Furthermore, Patent Document 3 proposes an artificial leather substrate consisting of a nonwoven fabric and a polymeric elastomer in which ultrafine fibers (A) and fibers (B) having a specific number of hollow spaces are three-dimensionally entangled, in which the weight ratio of (A) / (B) is within a specific range and the hollow spaces of the fibers (B) satisfy certain conditions. It also describes that this provides a flexible, lightweight artificial leather substrate that has mechanical properties that can withstand applications such as sports shoes and has excellent flex recovery. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2017-66542 A [Patent Document 2] International Publication No. 2000 / 22217 [Patent Document 3] JP 2002-242077 A Summary of the Invention [Problem to be solved by the invention]

[0008] Although the technology proposed in Patent Document 1 can produce a flexible and lightweight artificial leather, there is still room for improvement in terms of heat insulation, which is not discussed at all in Patent Document 1.

[0009] In addition, the technology proposed in Patent Document 2 can produce artificial leather with a certain degree of flexibility, but it does not achieve a level of flexibility suitable for use in clothing, and the insulation properties are also insufficient.

[0010] Although the technology proposed in Patent Document 3 can achieve a certain degree of mechanical properties, flexibility, and weight reduction, there is still room for improvement in terms of heat insulation.

[0011] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide an artificial leather that combines high heat insulation properties, flexibility, and light weight. [Means for solving the problem]

[0012] According to the present invention, the following inventions are provided.

[0013] [1] An artificial leather comprising, as components, a fiber structure including a nonwoven fabric composed of hollow fibers having an average single fiber diameter of 40 μm or more and 80 μm or less, and a polymer elastomer, wherein the hollow fibers have an average diameter of the hollow portion of 4 μm or more and 20 μm or less, and a hollow ratio of 40% or more and 95% or less.

[0014] [2] The artificial leather according to [1], wherein the mass ratio of the polymer elastomer in the artificial leather is 10 mass% or more and 50 mass% or less.

[0015] [3] The artificial leather according to [1] or [2], wherein the polymeric elastomer has a hydrophilic group.

[0016] [4] A step of forming a fiber structure including a nonwoven fabric composed of islands-in-sea type composite fibers having an average single fiber diameter of 40 μm or more and 80 μm or less, the fibers comprising a sea part and an island part; providing a polymeric elastomer to the fiber structure to form a sheet provided with the polymeric elastomer; a step of removing island components from islands-in-sea type composite fibers of a fiber structure contained in the polymer elastomer-imparted sheet to form hollow fibers; The method for producing an artificial leather according to any one of the above [1] to [3], the sea component is polyester, The method for producing an artificial leather, wherein the island components are a copolymerized polyester resin obtained by copolymerizing 5% by mass or more and 15% by mass or less of a polyalkylene glycol having a number average molecular weight of 500 or more and 3,500 or less. Effect of the Invention

[0017] According to the present invention, an artificial leather having heat insulating properties, flexibility, and light weight can be obtained. In particular, the artificial leather of the present invention can be suitably used for clothing having a high heat retaining effect, and also for furniture and automobile interior materials that require heat insulating properties, because of its characteristics. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] The artificial leather of the present invention comprises as its components a fiber structure including a nonwoven fabric composed of hollow fibers having an average single fiber diameter of 40 μm to 80 μm, and a polymer elastomer, the hollow fibers having an average diameter of the hollow portion of 4 μm to 20 μm and a hollow ratio of 40% to 95%. The components are described in detail below, but the present invention is not limited to the scope described below as long as it does not deviate from the gist of the invention, and various modifications are possible without departing from the gist of the invention.

[0019] [Fiber structure] First, the artificial leather of the present invention comprises, as one of its constituent elements, a fiber structure including a nonwoven fabric composed of hollow fibers having an average single fiber diameter of 40 μm or more and 80 μm or less.

[0020] The hollow fibers have an average single fiber diameter of 40 μm to 80 μm, an average diameter of the hollow portion of 4 μm to 20 μm, and a hollow ratio of 40% to 95%. By including a fiber structure containing a nonwoven fabric composed of such hollow fibers as one of its components, an artificial leather that combines heat insulation, flexibility, and light weight can be obtained.

[0021] First, the hollow fibers have an average single fiber diameter of 40 μm or more and 80 μm or less. When the lower limit of the range of the average single fiber diameter is 40 μm or more, preferably 50 μm or more, the artificial leather has high heat insulation. On the other hand, when the upper limit of the range of the average single fiber diameter is 80 μm or less, preferably 70 μm or less, the artificial leather has excellent flexibility.

[0022] Next, the hollow fiber has an average diameter of the hollow portion of 4 μm or more and 20 μm or less. When the lower limit of the range of the average diameter of the hollow portion is 4 μm or more, preferably 5 μm or more, the artificial leather has high heat insulation. On the other hand, when the upper limit of the range of the average diameter of the hollow portion is 20 μm or less, preferably 15 μm or less, the artificial leather has excellent flexibility.

[0023] The hollow fiber has a hollow ratio of 40% or more and 95% or less. When the lower limit of the hollow ratio range is 40% or more, preferably 60% or more, the artificial leather has high heat insulation properties. On the other hand, when the upper limit of the hollow ratio range is 95% or less, preferably 80% or less, the artificial leather has excellent flexibility.

[0024] The average single fiber diameter of the hollow fibers, the average diameter of the hollow portion, and the hollow ratio are measured and calculated by the following methods. (i) A cross section of the artificial leather cut in the thickness direction is photographed using a scanning electron microscope (SEM, for example, "VHX-D500 / D510" manufactured by Keyence Corporation). (ii) In the SEM image, 10 hollow fibers whose outer circumference is circular or whose outer circumference is elliptical and has an aspect ratio of 10% or less are randomly selected. (iii) Measure the single fiber diameter for one of the ten fibers. (However, when hollow fibers with an elliptical cross section are used, the cross-sectional area of ​​a single fiber is first measured, and the diameter of the cross section is calculated by assuming it to be a circle (equivalent circle diameter).) (iv) Count the number of hollow spaces in the hollow fibers, measure the diameters (inner diameters) (μm) of all of them, and calculate the arithmetic mean value (μm). (v) Repeat the same measurement and calculation for the remaining 9 hollow fibers, calculate the arithmetic mean (μm) of the single fiber diameter and the diameter of the hollow portion of the obtained 10 hollow fibers, and round off to the first decimal place to obtain the average single fiber diameter (μm) and the average diameter of the hollow portion (μm). (vi) The hollow ratio R (%) is calculated by rounding the value (%) of the following formula to one decimal place. R(%)=(S F -S H ) / S F ×100 Here, S F (μm 2 ), S H (μm 2 ) are the areas calculated using the following formulas: S F (μm 2 ) = π × (average single fiber diameter (μm)) 2 / 4 S H (μm 2 ) = (number of hollows) × π × (average diameter of hollows (μm)) 2 / 4.

[0025] The hollow fiber according to the present invention is preferably made of a thermoplastic resin. Examples of the thermoplastic resin include polyester, polyamide, polyolefin, and polyphenylene sulfide. Polycondensation polymers such as polyester and polyamide have high melting points, and when fibers made of these polycondensation polymers are used to make artificial leather, they exhibit good physical properties such as flexibility, and are therefore preferably used in the present invention.

[0026] Specific examples of polyesters include polyethylene terephthalate, polybutylene terephthalate, and polytrimethylene terephthalate, etc. Specific examples of polyamides include polyamide 6, polyamide 66, and polyamide 12, etc.

[0027] The above thermoplastic resin may contain additives such as particles, flame retardants, and antistatic agents.

[0028] The fiber structure according to the present invention includes a nonwoven fabric composed of the hollow fibers. As the nonwoven fabric, a short fiber nonwoven fabric obtained by forming a laminated web of short fibers using a card or a cross wrapper and then subjecting it to needle punching or water jet punching, a long fiber nonwoven fabric obtained by a spunbonding method or a meltblowing method, or a nonwoven fabric obtained by a papermaking method can be used. Among them, a short fiber nonwoven fabric or a spunbonding nonwoven fabric is preferably used because it can obtain a more uniform thickness.

[0029] The fiber structure according to the present invention preferably further includes a woven fabric or a knitted fabric. This makes the artificial leather stronger. The woven fabric or knitted fabric may be laminated with the nonwoven fabric and entangled by a method such as needle punching, or may be laminated on the back surface of the artificial leather (so-called lining product).

[0030] In particular, when the nonwoven fabric and the woven or knitted fabric are laminated together by needle punching as in the former case, it is more preferable to use a hard twist yarn as the yarn constituting the woven or knitted fabric in order to prevent damage to the fibers constituting the woven or knitted fabric by needle punching. In this case, the twist number of the yarn is preferably 700 T / m to 4500 T / m.

[0031] The average single fiber diameter of the yarns constituting the woven or knitted fabric is preferably the same as or smaller than the average single fiber diameter of the hollow fibers.

[0032] [Polymer elastomer] The artificial leather of the present invention comprises the above-mentioned fiber structure and a polymeric elastomer as components. The binder effect of the polymeric elastomer not only prevents the hollow fibers from falling out of the artificial leather, but also provides an appropriate cushioning property.

[0033] In the present invention, polyurethane, polyurea, polyurethane-polyurea elastomer, polyacrylic acid, acrylonitrile-butadiene elastomer, styrene-butadiene elastomer, etc. can be used as the polymer elastomer, but polyurethane is preferably used because it exhibits excellent flexibility and cushioning properties.

[0034] Examples of polyurethanes include polyurethanes and modified products thereof obtained by reacting at least one polymer diol selected from polymer diols such as polyester diols, polyether diols, polycarbonate diols, and polyester polyether diols having a weight average molecular weight of 500 to 3000 with at least one diisocyanate selected from aromatic diisocyanates such as 4,4'-diphenylmethane diisocyanate, alicyclic diisocyanates such as isophorone diisocyanate, and aliphatic diisocyanates such as hexamethylene diisocyanate, in a predetermined molar ratio, and at least one low molecular compound having two or more active hydrogen atoms, such as ethylene glycol, butanediol, ethylenediamine, and 4,4'-diaminodiphenylmethane.

[0035] The weight-average molecular weight of the polyurethane elastomer is preferably 50,000 to 300,000. By making the weight-average molecular weight preferably 50,000 or more, more preferably 100,000 or more, and even more preferably 150,000 or more, the artificial leather has high strength and is less susceptible to hollow fibers falling off. In addition, by making the weight-average molecular weight 300,000 or less, more preferably 250,000 or less, the viscosity of the polyurethane solution can be prevented from increasing, making it easier to impregnate the fiber structure.

[0036] This polymeric elastomer may contain elastomer resins such as polyester, polyamide and polyolefin elastomers, acrylic resins, and ethylene-vinyl acetate resins.

[0037] Furthermore, the polymer elastomer used in the present invention may contain additives such as pigments such as carbon black, dye antioxidants, antioxidants, light resistance agents, antistatic agents, dispersants, softeners, coagulation regulators, flame retardants, antibacterial agents and deodorizers, as necessary.

[0038] In addition, the polymeric elastomer may be either a polymeric elastomer dissolved in an organic solvent or a polymeric elastomer having a hydrophilic group dispersed in water. In particular, from the viewpoint of environmental conservation, it is preferable that the polymeric elastomer has a hydrophilic group. The polymeric elastomer having a hydrophilic group refers to a polymeric elastomer obtained by adding ethylene oxide alone or one or more of alkylene oxides such as ethylene oxide, propylene oxide, and butylene oxide to a relatively low molecular weight polyalkylene glycol such as polyoxyethylene glycol, polyoxyethylene propylene glycol, and polyoxyethylene tetramethylene glycol, a low molecular weight polyhydric alcohol such as ethylene glycol, propylene glycol, 1,4-butanediol, trimethylolpropane, glycerin, pentaerythritol, and sorbitol, and a low molecular weight alkylene polyamine such as ethylenediamine, diethylenetriamine, and triethylenetetramine.

[0039] In the present invention, the mass ratio of the polymer elastomer in the artificial leather is preferably 10% by mass or more and 50% by mass or less. By setting the above mass ratio to preferably 10% by mass or more, more preferably 15% by mass or more, and even more preferably 20% by mass or more, the artificial leather has less hollow fibers falling off. On the other hand, by setting the above mass ratio to preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, the hollow fibers are uniformly dispersed on the sheet surface, resulting in an artificial leather with excellent strength and less hollow fibers falling off.

[0040] [Artificial leather] The artificial leather of the present invention comprises the above-mentioned fiber structure and the above-mentioned polymeric elastomer as components. The basis weight of the artificial leather is 100 g / m 2 More than 500g / m 2 The lower limit of this range of basis weight is preferably 100 g / m 2 More preferably, 150 g / m 2 By setting the weight per unit area at 500 g / m or more, an artificial leather having sufficient shape stability and dimensional stability can be obtained. On the other hand, the upper limit of the weight per unit area is preferably 500 g / m 2 Less than 300 g / m 2 By satisfying the following conditions, the artificial leather has excellent flexibility.

[0041] The thickness of the artificial leather of the present invention is preferably in the range of 0.1 mm to 10 mm. When the lower limit of the thickness range is preferably 0.1 mm or more, more preferably 0.3 mm or more, the artificial leather has sufficient shape stability and dimensional stability. On the other hand, when the upper limit of the thickness range is preferably 10 mm or less, more preferably 5 mm or less, the artificial leather has excellent flexibility.

[0042] The artificial leather of the present invention is preferably in a form in which at least one side is napped. The thickness of the napped part, which is the distance from the top surface of the base part of the fiber structure to the tip (top) of the napped part when the artificial leather in a dry state is observed with an electron microscope in a cross section cut perpendicularly to the surface direction with the napped part laid down, is preferably 100 μm or more and 400 μm or less, more preferably 150 μm or more and 350 μm or less, and even more preferably 200 μm or more and 300 μm or less. When the thickness of the napped layer is 100 μm or more, the artificial leather has a suede-like soft touch. The exposed part of the polymeric elastomer on the surface is suppressed, and the artificial leather has a good appearance quality. On the other hand, when the thickness of the napped part is 400 μm or less, the artificial leather is suppressed in pilling and shedding of fuzz caused by entanglement of the napped parts on the surface.

[0043] [Manufacturing method of artificial leather] A preferred embodiment of the method for producing the artificial leather of the present invention will now be specifically described.

[0044] (1) Forming a fiber structure First, a fiber structure is formed, which includes a nonwoven fabric made of islands-in-sea type composite fibers having an average single fiber diameter of 40 μm or more and 80 μm or less, and which is composed of a sea part and an island part.

[0045] The sea component of this islands-in-sea type composite fiber is preferably made of the above-mentioned thermoplastic resin, particularly polyester, and the island component is preferably made of a copolymerized polyester resin obtained by copolymerizing 5% by mass or more and 15% by mass or less of polyalkylene glycol having a number average molecular weight of 500 or more and 3,500 or less.

[0046] As a method for obtaining such islands-in-sea type composite fibers, known methods can be used, but the islands-in-sea type composite fibers used in the present invention are preferably imparted with buckling crimp. This is because the buckling crimp improves the entanglement between hollow fibers when a staple fiber nonwoven fabric is formed, enabling high density and high entanglement. In order to impart buckling crimp to islands-in-sea type composite fibers, a normal stuffing box type crimper is preferably used, but in order to obtain a preferred crimp retention coefficient in the present invention, it is a preferred embodiment to appropriately adjust the treatment fineness, crimper temperature, crimper load, pressing pressure, etc.

[0047] The nonwoven fabric according to the present invention can be obtained by a step of forming a composite fiber web and a step of subjecting the composite fiber web to an entanglement treatment.

[0048] This composite fiber web can be formed by any known method, but a method in which the islands-in-the-sea composite fibers obtained above are opened by a card or the like and laminated by a cross wrapper or the like is particularly preferably used.

[0049] Next, as a method for subjecting the composite fiber web to an entanglement treatment, a method for entangling the composite fiber web by needle punching or water jet punching, or a papermaking method can be used. Among these, a method in which the composite fiber web is subjected to treatment such as needle punching or water jet punching in order to form a fiber bundle is preferably used.

[0050] The number of needle barbs (notches) in the needle used in the needle punching process is preferably 1 to 9. By preferably having 1 or more needle barbs, efficient fiber entanglement is possible. On the other hand, by preferably having 9 or less needle barbs, fiber damage can be suppressed.

[0051] The number of composite fibers caught by the barb is determined by the shape of the barb and the diameter of the composite fiber, so the barb shape of the needle used in the needle punching process preferably has a kick-up of 0 μm to 50 μm, an undercut angle of 0° to 40°, a throat depth of 100 μm to 200 μm, and a throat length of 0.5 mm to 1.0 mm.

[0052] The number of punches is 100 per cm. 2 ~800 pieces / cm 2 The number of punches is preferably 100 / cm. 2 By setting the number of punches at 800 / cm or more, denseness can be obtained and a highly accurate finish can be obtained. 2 By setting the content to the range below, it is possible to prevent deterioration of processability, fiber damage, and reduction in strength.

[0053] In addition, when woven or knitted fabrics are laminated together with nonwoven fabric, the barb direction of the needle punch needle is preferably set at 90°±25° perpendicular to the traveling direction of the woven or knitted fabric and nonwoven fabric, thereby making it less likely that the weft yarn, which is easily damaged, will get caught.

[0054] In addition, when performing water jet punching, it is preferable to perform the treatment with water in the form of a columnar flow. Specifically, it is preferable to eject water from a nozzle having a diameter of 0.05 mm to 1.0 mm at a pressure of 1 MPa to 60 MPa.

[0055] From the viewpoint of densification, it is preferable that the fiber structure made of the composite fiber thus obtained is shrunk by dry heat or wet heat or both to further increase the density.

[0056] (2) Step of forming a polymeric elastomer-imparted sheet In this step, a polymeric elastomer is applied to the fiber structure to form a sheet with the polymeric elastomer applied. The polymeric elastomer may be applied before or after the step of forming the hollow fibers.

[0057] As a solvent used when providing polyurethane as a polymeric elastomer, N,N'-dimethylformamide, dimethyl sulfoxide, etc. are preferably used, but polyurethane can also be used as a water-dispersed polyurethane liquid in which the polyurethane is dispersed in water as an emulsion.

[0058] The polymeric elastomer is applied to the fiber structure by, for example, immersing the fiber structure in a solution of the polymeric elastomer, and then drying the fiber structure to substantially coagulate and solidify the polymeric elastomer. In the case of a solvent-based polyurethane solution, the polymeric elastomer can be coagulated by immersing the fiber structure in a non-soluble solvent, and in the case of a water-dispersed polyurethane liquid having gelling properties, the polymeric elastomer can be coagulated by, for example, a dry coagulation method in which the polyurethane liquid is gelled and then dried. When drying, the polymeric elastomer is preferably heated at a temperature that does not impair the performance of the fiber structure and the polymeric elastomer.

[0059] (3) Forming the hollow fibers Furthermore, in this process, the island components of the islands-in-the-sea type composite fibers of the fiber structure contained in the polymer elastomer-imparted sheet are removed to form hollow fibers. As a solvent for dissolving the island components from the composite fibers, an aqueous alkali solution of sodium hydroxide or the like can be used if the island components are polylactic acid or copolymer polyester.

[0060] The hollow fiber can be formed by immersing a fiber structure made of composite fibers in a solvent and squeezing the solvent, using known machines such as a continuous dyeing machine, a vibro washer type seaweed remover, a liquid jet dyeing machine, a winch dyeing machine, and a jigger dyeing machine.

[0061] The step of forming the hollow fibers can be carried out either before or after the nap raising treatment described below.

[0062] (4) Other processes In the method for producing an artificial leather of the present invention, the product obtained through the step of forming the hollow fibers may be used as the artificial leather as it is, but it is also preferable to use the product obtained through various further steps as the artificial leather.

[0063] First, the artificial leather of the present invention may be subjected to a step of nap-raising treatment to impart nap to at least one surface thereof.

[0064] The nap raising treatment can be performed by grinding the surface with sandpaper or a roll sander. Before the nap raising treatment, a lubricant such as a silicone emulsion may be applied to the artificial leather. In particular, the use of sandpaper can result in uniform and dense nap raising.

[0065] Furthermore, in order to form uniform nap on the surface of the artificial leather, it is preferable to reduce the grinding load. In order to reduce the grinding load, for example, it is more preferable to use multi-stage buffing with three or more buff stages and use sandpaper with a grit size in the range of JIS No. 120 to JIS No. 600 for each stage.

[0066] Furthermore, the method for producing the artificial leather of the present invention may include a step of incorporating functional agents such as dyes, pigments, softeners, anti-pilling agents, antibacterial agents, deodorants, water repellents, light resistance agents, and weather resistance agents.

[0067] In particular, it is preferable to dye the artificial leather of the present invention. As a dyeing means, a liquid jet dyeing machine is preferably used because the artificial leather can be dyed and kneaded at the same time to soften it. The dyeing temperature is preferably 70°C to 140°C. When the hollow fiber is made of a thermoplastic resin and the thermoplastic resin is polyester, a disperse dye is preferably used as the dye. In addition, reduction washing can be performed after dyeing.

[0068] When carrying out this dyeing, it is preferable to use a dyeing assistant during dyeing in order to improve the uniformity of the dyeing. Furthermore, finishing treatments such as softeners such as silicone, antistatic agents, water repellents, flame retardants, and light fasteners can be carried out. The finishing treatments can be carried out after dyeing or in the same bath as dyeing.

[0069] In addition, the method for producing the artificial leather of the present invention may include a step of forming a coating layer (silver-coated layer) made of a resin. Examples of the resin components forming the coating layer include resin liquids such as emulsions, suspensions, dispersions, or solutions of elastomers such as polyurethane, polyolefin-based elastomers, polyamide-based elastomers, acrylic-based elastomers, silicone-based elastomers, diene-based elastomers, nitrile-based elastomers, fluorine-based elastomers, polystyrene-based elastomers, and halogen-based elastomers. These may be used alone or in combination of two or more kinds. Among them, polyurethane is preferred because of its excellent abrasion resistance and mechanical properties.

[0070] Furthermore, the resin of this coating layer may contain, as necessary, a colorant, an ultraviolet absorbing agent, a surfactant, a flame retardant, an antioxidant, etc. The thickness of the silver-coated layer is preferably in the range of 0.03 to 3.00 mm, and more preferably in the range of 0.05 to 0.50 mm.

Claims

1. An artificial leather comprising, as components, a fiber structure including a nonwoven fabric composed of hollow fibers having an average single fiber diameter of 40 μm or more and 80 μm or less, and a polymer elastomer, wherein the hollow fibers have an average diameter of hollow portions of 4 μm or more and 20 μm or less, and a hollow ratio of 40% or more and 95% or less.

2. 2. The artificial leather according to claim 1, wherein the mass ratio of the polymer elastomer in the artificial leather is 10 mass % or more and 50 mass % or less.

3. 3. The artificial leather according to claim 1, wherein the polymeric elastomer has a hydrophilic group.

4. forming a fiber structure including a nonwoven fabric composed of islands-in-sea type composite fibers having an average single fiber diameter of 40 μm or more and 80 μm or less, the fiber structure being composed of a sea part and an island part; providing a polymeric elastomer to the fiber structure to form a sheet provided with the polymeric elastomer; a step of removing island components from islands-in-sea type composite fibers of a fiber structure contained in the polymer elastomer-imparted sheet to form hollow fibers; The method for producing an artificial leather according to claim 1 or 2, the sea component is polyester, The method for producing an artificial leather, wherein the island component is a copolymerized polyester resin obtained by copolymerizing 5% by mass or more and 15% by mass or less of a polyalkylene glycol having a number average molecular weight of 500 or more and 3,500 or less.

Citation Information

Patent Citations

  • Artificial leather substrate and method for producing the same

    JP2002242077A

  • Sheet like material and production method thereof

    JP2017066542A

  • Nonwoven fabric and artificial leather using the same

    WO2000022217A1