Laminate
The laminate with tricyclodecane dimethanol in the polycarbonate resin and acrylic rubber polymer in the acrylic resin enhances interlayer adhesion, addressing separation issues and improving impact and heat resistance.
Patent Information
- Application Number
- JP2023050925
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing laminates with polycarbonate and acrylic resin layers face issues with interlayer adhesion, leading to potential separation, which is a concern in applications requiring strong bonding.
A laminate structure is developed with a polycarbonate resin containing tricyclodecane dimethanol and a specific gel content, combined with an acrylic resin that includes an acrylic rubber polymer, to enhance interlayer adhesion.
The laminate achieves high interlayer adhesion between polycarbonate and acrylic resin layers, providing improved impact resistance and heat resistance while maintaining structural integrity.
Smart Images

Figure 2024139964000001 
Figure 2024139964000002 
Figure 2024139964000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate having excellent interlayer adhesion. [Background technology]
[0002] In industrial fields such as food packaging materials, containers, decorative films, nameplates, plastic windows, and display front panels, there have been efforts to create laminates that combine various functions, such as gas barrier properties, mechanical strength, aroma retention, design, transparency, scratch resistance, and light resistance, by laminating layers each having the respective functions.
[0003] For example, the following Patent Document 1 describes a laminated optical film used as a protective film for a polarizing plate, which has at least one layer mainly made of a polycarbonate resin having excellent impact resistance and at least one layer mainly made of an acrylic resin having excellent optical properties and moist heat resistance. In addition, Patent Document 2 describes a multilayer body having at least one layer each of a polycarbonate resin-containing layer and an acrylic resin-containing layer, which has excellent transparency, chemical resistance, surface hardness, and adhesion. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2017-165086 A [Patent Document 2] JP 2016-7728 A Summary of the Invention [Problem to be solved by the invention]
[0005] By forming the laminates described in Patent Documents 1 and 2, it is possible to provide the laminates with multiple functions. However, there is a concern that the layer containing the polycarbonate resin and the layer containing the acrylic resin may peel off from each other, and in recent years, there has been a demand for further improvement in the interlayer adhesion between the layers.
[0006] The present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a laminate having high interlayer adhesion between a layer containing a polycarbonate resin as a main component and a layer containing an acrylic resin as a main component. [Means for solving the problem]
[0007] The gist of the present invention is as follows. [1] A laminate comprising a layer mainly composed of a polycarbonate resin and a layer mainly composed of an acrylic resin, wherein the polycarbonate resin has a structural unit derived from tricyclodecane dimethanol represented by the following formula (1), and the layer mainly composed of the acrylic resin has a gel content of 20 mass% or more in the total amount of resin constituting the layer mainly composed of the acrylic resin. [ka] [In formula (1), R 1 represents a hydroxymethyl group, and R 2 , R 3 and R 4 One of the groups represents a hydroxymethyl group, and the remaining groups represent hydrogen atoms. [2] The laminate according to claim 1, wherein the polycarbonate resin further has a structural unit derived from a dihydroxy compound represented by the following formula (2): [ka] [3] The laminate according to the above [1] or [2], wherein the content of the structural unit derived from the tricyclodecane dimethanol is 20 to 50 mol % in 100 mol % of the polycarbonate resin. [4] The laminate according to the above [2], wherein the content of the structural unit derived from the dihydroxy compound is 50 to 80 mol % in 100 mol % of the polycarbonate resin. [5] The laminate according to any one of [1] to [4] above, wherein the acrylic resin further contains an acrylic rubber polymer. [6] The laminate according to the above [5], wherein the acrylic rubber polymer is a graft polymer having a polymer having a glass transition temperature of 0°C or lower and a polymer having a glass transition temperature of higher than 20°C. [7] The laminate according to the above [5] or [6], wherein the acrylic rubber polymer has a mass average particle size of 100 to 300 nm. Effect of the Invention
[0008] According to the present invention, it is possible to provide a laminate having high interlayer adhesion between a layer containing a polycarbonate resin as a main component and a layer containing an acrylic resin as a main component. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] Hereinafter, the present invention will be described with reference to embodiments. [Laminate] The laminate of the present invention is a laminate of a layer mainly composed of a polycarbonate resin and a layer mainly composed of an acrylic resin, in which the polycarbonate resin has a structural unit derived from tricyclodecane dimethanol represented by the following formula (1), and the gel content in the total amount of resin constituting the layer mainly composed of the acrylic resin is 20 mass% or more.
[0010] [ka] [In formula (1), R 1 represents a hydroxymethyl group, and R 2 , R 3 and R 4 One of the groups represents a hydroxymethyl group, and the remaining groups represent hydrogen atoms.
[0011] <Layer mainly composed of polycarbonate resin> The laminate of the present invention has a layer mainly composed of polycarbonate resin (hereinafter, also referred to as "polycarbonate resin layer"). Here, the main component means that the polycarbonate resin layer contains preferably 50% by mass or more, more preferably 80% by mass or more, and further preferably 90% by mass or more of the components. The polycarbonate resin may be used alone or in combination of two or more kinds.
[0012] (Polycarbonate resin) The polycarbonate resin used in the present invention is a polycarbonate resin having a structural unit derived from tricyclodecane dimethanol represented by the following formula (1).
[0013] [ka] [In formula (1), R 1 represents a hydroxymethyl group, and R 2 , R 3 and R 4 One of the groups represents a hydroxymethyl group, and the remaining groups represent hydrogen atoms.
[0014] The polycarbonate resin preferably further has a structural unit derived from a dihydroxy compound represented by the following formula (2). [ka]
[0015] The content of the structural unit derived from tricyclodecane dimethanol represented by the above formula (1) in the polycarbonate resin is preferably 20 to 50 mol %, more preferably 25 to 45 mol %, and even more preferably 30 to 40 mol %, based on 100 mol % of the polycarbonate resin.
[0016] Furthermore, the content of the structural unit derived from the dihydroxy compound represented by the above formula (2) in the polycarbonate resin is preferably 50 to 80 mol %, more preferably 55 to 75 mol %, and even more preferably 60 to 70 mol %, based on 100 mol % of the polycarbonate resin.
[0017] By setting the content of the structural unit derived from tricyclodecane dimethanol represented by the above formula (1) and the content of the structural unit derived from the dihydroxy compound represented by the above formula (2) within the above ranges, it is possible to impart practically sufficient impact resistance without impairing the heat resistance of the laminate.
[0018] <Layer containing acrylic resin as main component> The laminate of the present invention has a layer containing an acrylic resin as a main component (hereinafter, also referred to as an "acrylic resin layer"). Here, the main component means that the acrylic resin layer contains preferably 50% by mass or more, more preferably 80% by mass or more, and even more preferably 90% by mass or more of the components. The acrylic resin may be used alone or in combination of two or more kinds.
[0019] In the present invention, the gel content in the total amount of resin constituting the layer mainly composed of an acrylic resin is 20% by mass or more, preferably 20% by mass or more and 80% by mass or less, more preferably 25% by mass or more and 75% by mass or less, and even more preferably 30% by mass or more and 70% by mass or less. By making the gel content 20% by mass or more, it is possible to improve the interlayer adhesion. The gel content can be measured by the method described in the examples below.
[0020] (Acrylic resin) The acrylic resin used in the present invention is a polymer obtained by polymerizing a monomer mainly composed of an alkyl methacrylate ester. Examples of such polymers include thermoplastic polymers, polymer processing aids, and polymer matting agents described in International Publication No. 2014 / 192708. As the polymer matting agent, a polymer having a hydroxyl group described in JP-A-2003-342389 is preferred.
[0021] The acrylic resin of the present invention preferably further contains an acrylic rubber polymer (A1). The acrylic rubber polymer (A1) is obtained by polymerizing a monomer (b) containing an alkyl methacrylate (b1) having an alkyl group having 1 to 4 carbon atoms in the presence of an elastic polymer (A1a) obtained by polymerizing a monomer (a) containing one or more monomers selected from an alkyl acrylate (a1) having an alkyl group having 1 to 8 carbon atoms and an alkyl methacrylate (a2) having an alkyl group having 1 to 4 carbon atoms, and a crosslinkable monomer (a4).
[0022] The alkyl acrylate (a1) having an alkyl group having 1 to 8 carbon atoms may be either linear or branched. Specific examples include methyl acrylate, ethyl acrylate, propyl acrylate, butyl acrylate, 2-ethylhexyl acrylate, and n-octyl acrylate. These may be used alone or in combination of two or more.
[0023] The alkyl methacrylate (a2) having an alkyl group having 1 to 4 carbon atoms may be either linear or branched. Specific examples include methyl methacrylate, ethyl methacrylate, propyl methacrylate, and butyl methacrylate. These may be used alone or in combination of two or more.
[0024] The alkyl acrylate (a1) and the alkyl methacrylate (a2) may be used either alone or in combination. The ratio of the alkyl acrylate (a1) in 100% by mass of the monomer (a) used as the raw material of the elastic polymer (A1a) is preferably 35% by mass or more, more preferably 60% by mass or more, even more preferably 90% by mass or more, and particularly preferably 93% by mass or more, since the flexibility of the acrylic resin composition (A) constituting the acrylic resin layer is good.
[0025] As the monomer (a) used as a raw material for the elastic polymer (A1a), other vinyl monomers (a3) other than the alkyl acrylates (a1) and alkyl methacrylates (a2) may be used in combination. Examples of the other vinyl monomers (a3) include acrylate monomers such as alkyl acrylates, alkoxy acrylates, and cyanoethyl acrylates having an alkyl group with 9 or more carbon atoms; acrylamide, acrylic acid, methacrylic acid, styrene, alkyl-substituted styrene, acrylonitrile, and methacrylonitrile.
[0026] The crosslinkable monomer (a4) is a component that forms a crosslinked structure with the alkyl acrylate (a1) and / or alkyl methacrylate (a2) to impart rubber elasticity to the polymer and form a crosslink with the rigid polymer (A1b). Among them, a graft crosslinking agent having a function of generating graft crosslinking is preferable. Examples of agents having such a function include allyl, methallyl, or crotyl esters of copolymerizable α,β-unsaturated carboxylic acids or dicarboxylic acids. In particular, allyl esters of acrylic acid, methacrylic acid, maleic acid, or fumaric acid are preferable. Among them, allyl methacrylate has an excellent effect. In addition, triallyl cyanurate and triallyl isocyanurate are also effective.
[0027] The graft crosslinking agent mainly reacts with the conjugated unsaturated bond of the ester much faster than the allyl group, methallyl group or crotyl group, and chemically bonds. Alternatively, a substantial proportion of the crotyl groups effectively function during the polymerization of the next layer polymer, providing a graft bond between two adjacent layers.
[0028] The crosslinkable monomer (a4) is not limited to a monomer that imparts rubber elasticity to the molded product or that causes graft crosslinking as described above, and may be a crosslinkable monomer for improving heat resistance. Examples of the crosslinkable monomer include alkylene glycol dimethacrylates such as ethylene glycol dimethacrylate, 1,3-butylene glycol dimethacrylate, 1,4-butylene glycol dimethacrylate, and propylene glycol dimethacrylate; and polyvinylbenzenes such as divinylbenzene and trivinylbenzene.
[0029] Of the total of the above monomers (a1) to (a4) being 100% by mass, the total amount of the alkyl acrylate (a1) and the alkyl methacrylate (a2) is preferably 80 to 100% by mass from the viewpoints of weather resistance, etc., and the amount of the monomer (a3) is preferably 0 to 20% by mass.
[0030] The amount of the crosslinkable monomer (a4) is preferably 0.4 to 2.0% by mass, more preferably 0.6 to 1.8% by mass, and even more preferably 1.2 to 1.7% by mass, based on 100% by mass of the total of the monomers (a1) to (a4). If this amount is 0.4% by mass or more, the crosslinking between the elastic polymer (A1a) and the rigid polymer (A1b) becomes stable, and sufficient transparency is exhibited. In addition, the rubber elasticity can be further improved, and the impact resistance of the molded article made of the obtained acrylic resin composition is increased. On the other hand, if the amount is 2.0% by mass or less, the crosslinking can be appropriately controlled, and the flexibility of the molded article made of the obtained acrylic resin composition (A) is suitably exhibited.
[0031] The elastomeric polymer (A1a) may be polymerized in two or more stages. In this case, a mixture of monomers having different compositions may be polymerized.
[0032] When the elastomeric polymer (A1a) is polymerized, for example, in two separate steps, the first elastomeric polymer (A1a-1) and the second elastomeric polymer (A1a-2) preferably have graft bonds between the two layers via a graft crosslinking agent.
[0033] The elastic polymer (A1a) preferably has a graft crosslinking agent unit content of 1.2% by mass or more, more preferably 1.5% by mass or more, based on 100% by mass of the elastic polymer (A1a). If the graft crosslinking agent unit content is 1.2% by mass or more, crosslinking between the layers of the first elastic polymer (A1a-1) and the second elastic polymer (A1a-2), and between the layers of the elastic polymer (A1a) and the rigid polymer (A1b) becomes stable, and interlayer adhesion can be improved.
[0034] The elastic polymer (A1a) can be obtained by a polymerization method such as emulsion polymerization, suspension polymerization, etc. In the case of emulsion polymerization, an emulsifier, a polymerization initiator, and a chain transfer agent can be used.
[0035] As the emulsifier, an anionic, cationic or nonionic surfactant is used, with anionic surfactants being particularly preferred.
[0036] Specific examples of the anionic surfactant include carboxylates such as rosin acid soap, potassium oleate, sodium stearate, sodium myristate, sodium N-lauroyl sarcosinate, and dipotassium alkenyl succinate; sulfates such as sodium lauryl sulfate; sulfonates such as sodium dioctyl sulfosuccinate, sodium dodecylbenzene sulfonate, and sodium alkyl diphenyl ether disulfonate; and phosphates such as sodium polyoxyethylene alkyl phenyl ether phosphate. Among these, alkyl sulfonates are preferred, and dioctyl sodium sulfosuccinate is particularly preferred, because they improve the fluidity of the acrylic rubber polymer (A1).
[0037] Examples of methods for preparing an emulsion include a method of adding a monomer mixture to water and then adding a surfactant, a method of adding a monomer mixture to water and then adding a surfactant, and a method of adding a surfactant to a monomer mixture and then adding water. Among these, the method of adding a monomer mixture to water and then adding a surfactant, and the method of adding a monomer mixture to water and then adding a surfactant are preferred.
[0038] Specific examples of the polymerization initiator include persulfates such as potassium persulfate and sodium persulfate; organic peroxides such as t-butyl hydroperoxide, cumene hydroperoxide, and benzoyl peroxide; azo compounds such as azobisisobutyronitrile; and redox initiators in which these persulfates or organic peroxides are combined with a reducing agent. Among these, redox initiators are preferred, and sulfoxylate initiators in which ferrous sulfate, disodium ethylenediaminetetraacetate, sodium formaldehyde sulfoxylate, and hydroperoxide are combined are more preferred. The polymerization initiator can be added to either or both of the aqueous phase and the monomer phase.
[0039] The amount of the polymerization initiator is preferably 0.05 to 1.0 parts by mass, more preferably 0.1 to 0.6 parts by mass, based on 100 parts by mass of the total of the monomers (a1) to (a4). When the amount of the polymerization initiator is 0.05 parts by mass or more, the mechanical strength of the molded article containing the acrylic rubber polymer (A1) is good. When the amount is 1.0 part by mass or less, the flowability is good, and the moldability when the acrylic resin composition (A) is melt-extruded and molded is good.
[0040] Specific examples of the chain transfer agent include alkyl mercaptans having 2 to 20 carbon atoms, mercapto acids, thiophenol, and carbon tetrachloride. The chain transfer agent is preferably mixed during polymerization of the rigid polymer (A1b), and n-octyl mercaptan is preferred.
[0041] The polymerization temperature varies depending on the type and amount of the polymerization initiator, but is preferably 40 to 120°C, more preferably 60 to 95°C.
[0042] Prior to polymerization of the elastic polymer (A1a), a core having a Tg exceeding 0°C may be polymerized. The core is preferably 0 to 10 mass% of the acrylic rubber polymer (A1) in terms of the stability of polymer particle size generation. The core is preferably obtained by polymerizing monomers (a) (the total of (a1) to (a4) being 100 mass%) including 10 to 50 mass% of an alkyl acrylate (a1) having an alkyl group with 1 to 8 carbon atoms, 20 to 70 mass% of an alkyl methacrylate (a2) having an alkyl group with 1 to 4 carbon atoms, 0 to 10 mass% of other vinyl monomers (a3), and 0.1 to 10 mass% of a crosslinkable monomer (a4).
[0043] The acrylic rubber polymer (A1) is obtained by polymerizing a monomer (b) containing an alkyl methacrylate (b1) having an alkyl group having 1 to 4 carbon atoms in the presence of the elastic polymer (A1a). The monomer (b) is polymerized to form a rigid polymer (A1b). Specific examples of the alkyl methacrylate (b1) include the same as the specific examples of the alkyl methacrylate (a2). They may be used alone or in combination of two or more.
[0044] As the monomer (b), other monomers (b2) other than the alkyl methacrylate (b1) can also be used in combination. Specific examples of the other monomers (b2) include the same as the specific examples of the alkyl acrylate (a1) and the other vinyl monomers (a3). They may be used alone or in combination of two or more.
[0045] In 100% by mass of the monomer (b), the content of the alkyl methacrylate (b1) is preferably 70% by mass or more, more preferably 85% by mass or more, which allows the Tg of the rigid polymer (A1b) to be appropriately high.
[0046] The monomer (b) may be polymerized in two or more stages. In that case, a mixture of monomers having different compositions may be polymerized. The polymerization reaction of the monomer (b) is preferably carried out by adding the monomer (b) to the polymerization liquid obtained after the polymerization reaction of the elastic polymer (A1a) is completed, as it is. Specific examples of the emulsifier, polymerization initiator, and chain transfer agent in this polymerization are the same as those in the polymerization of the elastic polymer (A1a).
[0047] The amount of the chain transfer agent is preferably 0.1 to 2 parts by mass, more preferably 0.2 to 1 part by mass, based on 100 parts by mass of the monomer (b). When the amount of the chain transfer agent is 0.1 part by mass or more, the flexibility of the molded article is increased. When the amount is 2 parts by mass or less, the mechanical strength of the molded article is increased.
[0048] The Tg of the elastic polymer (A1a) is preferably 0°C or lower, more preferably -30°C or lower, and even more preferably -40°C or lower. If the Tg is 0°C or lower, the molded article made of the acrylic resin composition (A) has a preferable impact resistance. This Tg is a value measured and calculated as follows using a dynamic viscoelasticity measuring device. A test piece is molded into a sheet with a width of 6 mm and a thickness of 1 mm, and the values of the storage modulus (E') and loss modulus (E'') are measured in a tensile mode using a dynamic viscoelasticity measuring device in accordance with ISO6721-4 under the conditions of an initial chuck distance of 2 cm, a measurement frequency of 0.1 Hz, a measurement temperature range of -90 to 150°C, a heating rate of 2°C / min, and a nitrogen gas flow of 200 mL / min, and the value of tanδ (loss tangent) at each temperature is calculated according to the formula tanδ=E'' / E'. Next, when the value of tanδ is plotted against the temperature, two or more peaks appear. The temperature corresponding to the lowest peak among these is taken as the Tg of the elastic polymer (A1a).
[0049] The Tg of the rigid polymer (A1b) is preferably higher than 20°C. If the Tg of the rigid polymer (A1b) is higher than 20°C, the heat resistance and rigidity of the molded article made of the acrylic resin composition (A) are good. The Tg of the rigid polymer (A1b) is more preferably 70 to 120°C, and even more preferably 75 to 110°C. If the Tg of the rigid polymer (A1b) is 120°C or less, the fluidity of the acrylic resin composition (A) is improved and the moldability is good. The Tg of the rigid polymer (A1b) is the temperature corresponding to the peak that appears at the highest temperature in a dynamic viscoelasticity measurement similar to the measurement method of the Tg of the elastic polymer (A1a).
[0050] In addition, after the polymerization reaction of the elastic polymer (A1a) is completed, and before the polymerization of the monomer (b), the intermediate polymer (A1c) can be formed by sequentially polymerizing monomers having a composition in which the proportion of the alkyl acrylate (a1) having an alkyl group with 1 to 8 carbon atoms is gradually decreased and the proportion of the alkyl methacrylate (a2) having an alkyl group with 1 to 4 carbon atoms is gradually increased from the composition of the monomers constituting the elastic polymer (A1a).
[0051] The ratio of the elastic polymer (A1a) in 100% by mass of the acrylic rubber polymer (A1) is preferably 30% by mass or more, more preferably 40 to 70% by mass, and even more preferably 50 to 60% by mass. When the ratio of the elastic polymer (A1a) is 30% by mass or more, the mechanical strength and flexibility of the obtained acrylic resin composition (A) and molded article are improved, and cracks and whitening when folded can be suppressed. In addition, whitening, peeling, and breakage can be suppressed when laminated on a substrate and folded. When the ratio of the elastic polymer (A1a) is 70% by mass or less, the thickness precision is excellent when the obtained acrylic resin composition (A) is molded into a film, and productivity during molding does not decrease.
[0052] The ratio of the rigid polymer (A1b) in 100% by mass of the acrylic rubber polymer (A1) is preferably 70% by mass or less, more preferably 30 to 60% by mass, and even more preferably 40 to 50% by mass. If the ratio of the rigid polymer (A1b) is 30% by mass or more, the fluidity of the resulting acrylic resin composition (A) is improved and the moldability is good. If it is 70% by mass or less, the flexibility is improved and the stress whitening resistance is good.
[0053] When the emulsion polymerization method is used, the acrylic rubber polymer (A1) is recovered as a powder from the latex after the polymerization reaction. As a method for recovering as a powder, for example, the latex is brought into contact with a coagulant to be coagulated or salted out, solid-liquid separated, washed with water in an amount of about 1 to 100 times the mass of the polymer, and made into a wet powder by a dehydration treatment such as filtration, and further this wet powder is dried with a hot air dryer such as a squeeze dehydrator or a fluidized dryer. In addition, the latex may be directly dried by a spray drying method. The drying temperature and drying time of the polymer can be appropriately determined depending on the type of polymer.
[0054] Specific examples of the coagulant include organic salts such as sodium acetate, calcium acetate, potassium formate, and calcium formate; and inorganic salts such as sodium chloride, potassium chloride, calcium chloride, magnesium chloride, and sodium sulfate. Among these, calcium salts such as calcium acetate and calcium chloride are preferred. In particular, calcium acetate is more preferred from the viewpoint of hot water whitening resistance of the molded body and from the viewpoint of reducing the moisture content of the recovered powder. The coagulant may be used alone or in combination of two or more kinds.
[0055] The coagulant is usually used as an aqueous solution. The concentration of the coagulant, preferably calcium acetate, in the aqueous solution is preferably 0.1% by mass or more, more preferably 1% by mass or more, from the viewpoint of stably coagulating and recovering the acrylic resin composition. The concentration of the calcium acetate aqueous solution is preferably 20% by mass or less, more preferably 15% by mass or less, from the viewpoint of reducing the amount of coagulant remaining in the recovered powder and hardly reducing the performance, particularly, resistance to whitening in hot water, colorability, etc. If the concentration of calcium acetate exceeds 20% by mass, calcium acetate may precipitate due to saturation at 10° C. or less.
[0056] The method of contacting the latex with the coagulant includes, for example, a method of continuously adding latex to an aqueous solution of the coagulant while stirring the solution and continuing to stir for a certain period of time, and a method of continuously injecting the aqueous solution of the coagulant and latex at a certain ratio into a container equipped with a stirrer and contacting them, and continuously extracting a mixture containing the coagulated powder and water from the container. The amount of the aqueous solution of the coagulant is preferably 10 to 500 parts by mass per 100 parts by mass of latex. The temperature of the coagulation step is preferably 30 to 100°C from the viewpoint of blocking of the obtained coagulated powder.
[0057] The weight average molecular weight (Mw) of the acetone soluble portion of the acrylic rubber polymer (A1) is preferably 25,000 to 70,000, more preferably 30,000 to 50,000, and even more preferably 35,000 to 40,000. When Mw is 25,000 or more, the mechanical strength is improved and cracking during molding can be suppressed. In addition, breakage and whitening during bending can be suppressed. If the Mw is 70,000 or less, the fluidity of the resulting resin composition is improved, and the processability during melt molding is excellent. In addition, after the resulting film is laminated to a substrate such as a steel plate, whitening does not occur at the bent portion during bending, and the appearance of the resulting various components is good. The Mw is a value measured by the method described below.
[0058] The Mw of the acetone soluble portion of the acrylic rubber polymer (A1) can be adjusted by appropriately changing the amount of the chain transfer agent during polymerization. The chain transfer agent is preferably mixed during polymerization of the rigid polymer (A1b).
[0059] The mass average particle diameter of the acrylic rubber polymer (A1) is preferably 100 to 300 nm, more preferably 110 to 250 nm, and even more preferably 120 to 200 nm. If the mass average particle diameter is 100 nm or more, practically sufficient impact resistance is exhibited. If it is 300 nm or less, transparency is excellent. The mass average particle diameter can be measured by the method described in the examples below.
[0060] <Other resins> For the purpose of further improving and adjusting the moldability and various physical properties, the polycarbonate resin or acrylic resin constituting the laminate of the present invention may be blended with other resins to form a polycarbonate resin composition or an acrylic resin composition. Examples of such resins include polyester resins, polyether, polyamide, polyolefin, polymethyl methacrylate, and the like. The blending amount of the resin other than the polycarbonate resin and the acrylic resin is preferably 1% by mass or more and 30% by mass or less, more preferably 3% by mass or more and 20% by mass or less, and even more preferably 5% by mass or more and 10% by mass or less, based on the resin composition constituting each layer of the laminate of the present invention, within a range that does not impair the effects of the present invention.
[0061] <Heat stabilizer> A heat stabilizer can be blended into the resin composition constituting each layer of the laminate of the present invention in order to prevent a decrease in molecular weight or a deterioration in color during molding. Examples of such heat stabilizers include phosphorous acid, phosphoric acid, phosphonous acid, phosphonic acid, and esters thereof. Specific examples of such heat stabilizers include triphenyl phosphite, tris(nonylphenyl)phosphite, tris(2,4-di-tert-butylphenyl)phosphite, tridecyl phosphite, trioctyl phosphite, trioctadecyl phosphite, didecyl monophenyl phosphite, dioctyl monophenyl phosphite, diisopropyl monophenyl phosphite, monobutyl diphenyl phosphite, monodecyl diphenyl phosphite, monooctyl diphenyl phosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, 2,2-methylene bis( Examples of the phosphate phosphate include 4,6-di-tert-butylphenyl)octyl phosphite, bis(nonylphenyl)pentaerythritol diphosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, distearyl pentaerythritol diphosphite, tributyl phosphate, triethyl phosphate, trimethyl phosphate, triphenyl phosphate, diphenyl monoorthoxenyl phosphate, dibutyl phosphate, dioctyl phosphate, diisopropyl phosphate, 4,4'-biphenylenediphosphinic acid tetrakis(2,4-di-tert-butylphenyl), dimethyl benzenephosphonate, diethyl benzenephosphonate, and dipropyl benzenephosphonate. Among them, trisnonylphenyl phosphite, trimethyl phosphate, tris(2,4-di-tert-butylphenyl)phosphite, bis(2,4-di-tert-butylphenyl)pentaerythritol diphosphite, bis(2,6-di-tert-butyl-4-methylphenyl)pentaerythritol diphosphite, and dimethyl benzenephosphonate are preferably used. These heat stabilizers may be used alone or in combination of two or more.The amount of the heat stabilizer is preferably 0.0001% by mass or more and 1% by mass or less, more preferably 0.0005% by mass or more and 0.5% by mass or less, and even more preferably 0.001% by mass or more and 0.2% by mass or less, relative to the resin composition constituting each layer of the laminate of the present invention. By adding the heat stabilizer in such a range, it is possible to prevent a decrease in molecular weight and discoloration of the resin composition constituting the laminate without causing bleeding of the additives, etc.
[0062] <Antioxidants> In addition, the resin composition constituting each layer of the laminate of the present invention may contain a commonly known antioxidant for the purpose of preventing oxidation. Examples of such antioxidants include pentaerythritol tetrakis(3-mercaptopropionate), pentaerythritol tetrakis(3-laurylthiopropionate), glycerol-3-stearylthiopropionate, triethylene glycol-bis[3-(3-tert-butyl-5-methyl-4-hydroxyphenyl)propionate], 1,6-hexanediol-bis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], pentaerythritol-tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate], octadecyl-3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate, 1,3,5-trimethyl -2,4,6-tris(3,5-di-tert-butyl-4-hydroxybenzyl)benzene, N,N-hexamethylenebis(3,5-di-tert-butyl-4-hydroxy-hydrocinnamide), 3,5-di-tert-butyl-4-hydroxy-benzylphosphonate-diethyl ester, tris(3,5-di-tert-butyl-4-hydroxybenzyl)isocyanurate, 4,4'-biphenylenediphosphinic acid tetrakis(2,4-di-tert-butylphenyl), 3,9-bis{1,1-dimethyl-2-[β-(3-tert-butyl-4-hydroxy-5-methylphenyl)propionyloxy]ethyl}-2,4,8,10-tetraoxaspiro(5,5)undecane, and the like. The amount of the antioxidant is preferably 0.0001% by mass or more and 1% by mass or less, more preferably 0.0005% by mass or more and 0.5% by mass or less, and even more preferably 0.001% by mass or more and 0.2% by mass or less, based on the resin composition constituting each layer of the laminate of the present invention. By adding the antioxidant in such a range, it is possible to prevent oxidative deterioration of the resin without causing bleeding of the antioxidant or deterioration of the mechanical properties of the laminate.
[0063] <Lubricant> A lubricant may be blended with the resin composition constituting each layer of the laminate of the present invention to impart surface lubricity. Examples of the lubricant include higher fatty acid esters of monohydric or polyhydric alcohols, higher fatty acids, paraffin wax, beeswax, olefin waxes, olefin waxes containing carboxyl groups and / or carboxylic anhydride groups, silicone oils, and organopolysiloxanes.
[0064] The higher fatty acid ester is preferably a partial or full ester of a monohydric or polyhydric alcohol having 1 to 20 carbon atoms and a saturated fatty acid having 10 to 30 carbon atoms. Examples of such partial or full esters of a monohydric or polyhydric alcohol and a saturated fatty acid include stearic acid monoglyceride, stearic acid diglyceride, stearic acid triglyceride, stearate monosorbitate, stearyl stearate, behenic acid monoglyceride, behenyl behenate, pentaerythritol monostearate, pentaerythritol tetrastearate, pentaerythritol tetrapelargonate, propylene glycol monostearate, stearyl stearate, palmityl palmitate, butyl stearate, methyl laurate, isopropyl palmitate, biphenyl biphenate, sorbitan monostearate, and 2-ethylhexyl stearate. Among them, stearic acid monoglyceride, stearic acid triglyceride, pentaerythritol tetrastearate, and behenyl behenate are preferably used. As the higher fatty acid, saturated fatty acid having 10 to 30 carbon atoms is preferable. As such fatty acid, myristic acid, lauric acid, palmitic acid, stearic acid, behenic acid, etc. may be mentioned. These lubricants may be used alone or in combination of two or more. The amount of the lubricant to be blended is preferably 0.0001% by mass or more and 1% by mass or less, more preferably 0.0005% by mass or more and 0.5% by mass or less, and even more preferably 0.001% by mass or more and 0.2% by mass or less, based on the resin composition constituting each layer of the laminate of the present invention. By blending the lubricant in such a range, it is possible to impart surface lubricity to the laminate without causing bleeding of the lubricant or deterioration of the mechanical properties of various molded products made of the resin composition.
[0065] <UV absorbers, light stabilizers> In addition, for the purpose of further improving the weather resistance of the resin composition constituting each layer of the laminate of the present invention, an ultraviolet absorber and a light stabilizer can be blended. Examples of such ultraviolet absorbers and light stabilizers include 2-(2'-hydroxy-5'-tert-octylphenyl)benzotriazole, 2-(3-tert-butyl-5-methyl-2-hydroxyphenyl)-5-chlorobenzotriazole, 2-(5-methyl-2-hydroxyphenyl)benzotriazole, 2-[2-hydroxy-3,5-bis(α,α-dimethylbenzyl)phenyl]-2H-benzotriazole, 2,2'-methylenebis(4-cumyl-6-benzotriazolephenyl), and 2,2'-p-phenylenebis(1,3-benzoxazin-4-one). The melting point of the ultraviolet absorber is preferably in the range of 120 to 250°C. When an ultraviolet absorber with a melting point of 120°C or more is used, the clouding caused by gas on the surface of the molded article is reduced and improved. Specifically, benzotriazole-based ultraviolet absorbers such as 2-(2'-hydroxy-5'-methylphenyl)benzotriazole, 2-(2'-hydroxy-3'-tert-butyl-5'-methylphenyl)-5-chlorobenzotriazole, 2-[2'-hydroxy-3'-(3'',4'',5'',6''-tetrahydrophthalimidomethyl)-5'-methylphenyl]benzotriazole, 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)]phenol, and 2-(2-hydroxy-3,5-dicumylphenyl)benzotriazole are used. Among these, 2-(2-hydroxy-3,5-dicumylphenyl)benzotriazole and 2,2-methylenebis[4-(1,1,3,3-tetramethylbutyl)-6-(2H-benzotriazol-2-yl)]phenol are particularly preferred. The molecular weight of the ultraviolet absorbent is preferably 300 or more, more preferably 400 or more. When an ultraviolet absorbent having a molecular weight of 300 or more is used, problems such as the resin adhering to a transfer roll or the like during film production, causing roll stains, can be suppressed. As the type of ultraviolet absorbent, benzotriazole-based or triazine-based ones having a molecular weight of 400 or more are more preferred.Commercially available products of the former include Tinuvin 360 and Tinuvin 234 from BASF Japan Ltd., and ADK STAB LA-31RG from ADEKA Corporation, while commercially available products of the latter include Tinuvin 1577 and Tinuvin 1600 from BASF Japan Ltd., and ADK STAB LA-F70 and ADK STAB LA-46 from ADEKA Corporation (all of the above are product names). In addition, as the light stabilizer, a radical scavenger such as a hindered amine light stabilizer is particularly preferred. Commercially available products of such light stabilizers include Chimassorb 944, Chimassorb 2020, and Tinuvin 770 from BASF Japan Ltd., and Adeka STAB LA-57G and Adeka STAB LA-72 from ADEKA CORPORATION (all trade names). These ultraviolet absorbents and light stabilizers may be used alone or in combination of two or more. The amount of the ultraviolet absorbent and light stabilizer is preferably 0.0001% by mass or more and 1% by mass or less, more preferably 0.0005% by mass or more and 0.5% by mass or less, and even more preferably 0.001% by mass or more and 0.2% by mass or less, based on the resin composition constituting each layer of the laminate of the present invention. By blending the ultraviolet absorbent and light stabilizer in such a range, the weather resistance can be improved without bleeding of the ultraviolet absorbent and light stabilizer to the surface of the laminate or deterioration of the mechanical properties of the laminate.
[0066] <Epoxy compounds> Furthermore, in order to further improve the hydrolysis resistance of the resin composition constituting each layer of the laminate of the present invention, an epoxy-based compound can be blended.Specific examples of the epoxy-based compound include epoxidized soybean oil, epoxidized linseed oil, phenyl glycidyl ether, allyl glycidyl ether, t-butylphenyl glycidyl ether, 3,4-epoxycyclohexylmethyl-3',4'-epoxycyclohexyl carboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-3',4'-epoxy-6'-methylcyclohexyl carboxylate, 2,3-epoxycyclohexylmethyl-3',4'-epoxycyclohexyl carboxylate, 4-(3,4-epoxy-5-methylcyclohexyl)butyl-3',4'-epoxycyclohexylcarboxylate, 3,4-epoxycyclohexylethylene oxide, cyclohexylmethyl-3,4-epoxycyclohexylcarboxylate, 3,4-epoxy-6-methylcyclohexylmethyl-6'-methylcyclohexylcarboxylate, bisphenol A diglycidyl ether, tetrabromobisphenol A glycidyl ether, diglycidyl ester of phthalic acid, diglycidyl ester of hexahydrophthalic acid Glycidyl esters, bis-epoxy dicyclopentadienyl ethers, bis-epoxy ethylene glycols, bis-epoxy cyclohexyl adipates, butadiene diepoxides, tetraphenylethylene epoxides, octyl epoxy thalates, epoxidized polybutadiene, 3,4-dimethyl-1,2-epoxycyclohexane, 3,5-dimethyl-1,2-epoxycyclohexane, 3-methyl-5-t-butyl-1,2-epoxycyclohexane, octadecyl-2,2-dimethyl-3,4-epoxycyclohexane cyclohexyl carboxylate, N-butyl-2,2-dimethyl-3,4-epoxycyclohexyl carboxylate, cyclohexyl-2-methyl-3,4-epoxycyclohexyl carboxylate, N-butyl-2-isopropyl-3,4-epoxy-5-methylcyclohexyl carboxylate, octadecyl-3,4-epoxycyclohexyl carboxylate, 2-ethylhexyl-3',4'-epoxycyclohexyl carboxylate, 4,6-dimethyl-2,3-epoxycyclohexyl-3',Examples of the epoxy compounds include 4'-epoxycyclohexyl carboxylate, 4,5-epoxy tetrahydrophthalic anhydride, 3-t-butyl-4,5-epoxy tetrahydrophthalic anhydride, diethyl-4,5-epoxy-cis-1,2-cyclohexyl dicarboxylate, and di-N-butyl-3-t-butyl-4,5-epoxy-cis-1,2-cyclohexyl dicarboxylate. Bisphenol A diglycidyl ether is preferred from the viewpoint of compatibility. The amount of the epoxy compound is preferably 0.0001% by mass or more and 5% by mass or less, more preferably 0.001% by mass or more and 1% by mass or less, and even more preferably 0.005% by mass or more and 0.5% by mass or less, based on the resin composition constituting each layer of the laminate of the present invention. By adding the epoxy compound in such a range, the hydrolysis resistance can be improved without bleeding of the epoxy compound or deterioration of the mechanical properties of the laminate.
[0067] In addition to the above, additives such as plasticizers, pigments, dyes, and fillers can also be blended into the resin composition constituting each layer of the laminate of the present invention.
[0068] <Applications of laminates> The laminate of the present invention can be used in the form of a film, a sheet, a plate, etc. The laminate can be formed by a known method such as coextrusion, extrusion lamination, heat lamination, dry lamination, etc.
[0069] In the case of co-extrusion, the resins constituting each layer of the laminate and additives are mixed through a feed block or a multi-manifold die using multiple extruders to form a laminate. To further improve the strength and impact resistance of this laminate, the laminate obtained in the above process can be uniaxially or biaxially stretched by a roll method, a tenter method, a tubular method, or the like.
[0070] The laminate of the present invention has a polycarbonate resin layer and an acrylic resin layer. By having the polycarbonate resin layer, it is possible to impart practically sufficient impact resistance. In addition, by having the acrylic resin layer, it is possible to impart excellent surface hardness and heat resistance.
[0071] In the laminate formed by the above method, the thickness ratio of the polycarbonate resin layer to the acrylic resin layer (polycarbonate resin layer / acrylic resin layer) is preferably 5 / 95 or more and 50 / 50 or less, and more preferably 7 / 93 or more and 40 / 60 or less. It is more preferably 10 / 90 or more and 30 / 70 or less. By setting the thickness ratio of the polycarbonate resin layer to the acrylic resin layer in the above range, a laminate having excellent surface hardness and heat resistance as well as excellent impact resistance can be obtained.
[0072] The uses of the laminate of the present invention are not particularly limited, and it can be used, for example, as building materials, interior parts, transparent sheets for display covers, etc., sheets for resin-coated metal plates, sheets for molding (vacuum / pressure molding, hot press molding, etc.), colored plates, transparent plates, shrink films, shrink labels, shrink tubes, automotive interior and exterior materials, home appliance components, office equipment components, etc.
[0073] The laminate of the present invention can be used as a molding sheet and can be subjected to various secondary processing, and can also be made into a thermoformed product by heat molding. The thermoforming method is not particularly limited, and known molding methods such as blister molding, vacuum molding, and pressure molding can be used.
[0074] The applications of the thermoformed article are not particularly limited, but for example, applications requiring printability, weather resistance, and heat resistance include simulated cans (so-called dummy cans) used in vending machines, backlit advertisement display boards, etc. Applications requiring deep drawing suitability include food packaging materials such as egg packs, and press-through packs (PTPs) for pharmaceuticals.
[0075] In addition, a molten resin may be further injected onto the thermoformed article to form a backing layer, thereby producing an in-mold molded article having excellent design. In this case, a printed layer may be provided on one side of the thermoformed article, and the printed layer may be protected by injection molding on the printed side. In addition to the case where the molten resin is injection molded after being subjected to secondary processing by thermoforming once, thermoforming and injection molding may be performed simultaneously in a mold, and an in-mold molded article can be obtained in one step using a sheet-like laminate. The in-mold molded article can be suitably used for automobile interior and exterior materials, home appliance parts, office automation equipment parts, etc. EXAMPLES
[0076] The present invention will be described in more detail below using examples and comparative examples, but the present invention is not limited to the following examples and comparative examples as long as it does not deviate from the gist of the present invention. In addition, "parts" means "parts by mass".
[0077] <Measurement and evaluation methods> The produced laminates and laminate molded articles were evaluated by the following methods. (Gel Content of Rubber-Containing Multistage Polymer and Acrylic Resin Composition) The acetone solution in which 0.5 g of rubber-containing multi-stage polymer was dissolved in 50 mL of acetone as the pre-extraction mass M was refluxed at 65° C. for 4 hours. The obtained extract was centrifuged at 14,000 rpm for 30 minutes at 4° C. using a high-speed cooling centrifuge (manufactured by Hitachi Koki Co., Ltd., product name: CR21G). The solution was removed by decantation to obtain "supernatant 1" and the remaining solid. The reflux, centrifugation, and decantation were repeated again for this solid, and it was separated into "supernatant 2" and the solid. The mass of the acetone insoluble matter obtained by drying the obtained solid at 50° C. for 24 hours was measured as the post-extraction mass m. The gel content G (%) of the rubber-containing multi-stage polymer was calculated from the pre-extraction mass M and the post-extraction mass m according to the following formula. The gel content G (%) of the acrylic resin composition was calculated in the same manner. Gel content G (%) = (mass after extraction m (g) / mass before extraction M (g)) x 100
[0078] (Adhesion) At room temperature, 100 squares were cut into the board at 1 mm intervals with a cutter knife, and peelability was checked with cellophane tape (manufactured by Nichiban Co., Ltd.). When no squares peeled off (100 / 100), the board was rated as "○", when 1 to 5 squares peeled off (99-95 / 100), the board was rated as "△", and when 6 or more squares peeled off (94-0 / 100), the board was rated as "×".
[0079] (Thickness) The thickness of each layer was determined by observing the cross section using an optical microscope (model: KH-8700, manufactured by Hirox Japan Co., Ltd.).
[0080] (Mass average molecular weight (Mw)) Acetone was evaporated from the "supernatant 1" obtained in the measurement of the gel content of the rubber-containing multistage polymer described above, and the resulting solution was dissolved in tetrahydrofuran (THF) to obtain a sample, which was then measured at 40°C using gel permeation chromatography (model name: "HLC-8200", Tosoh Corporation), columns (trade name: "TSK-GEL SUPER MULTIPORE HZ-H", Tosoh Corporation, inner diameter 4.6 mm x length 15 cm x 2 columns), and eluent (THF). Mw was determined from a calibration curve using standard polystyrene.
[0081] (Mass average particle size of rubber-containing multi-stage polymer) The mass average particle size of the rubber-containing multistage polymer was determined by dynamic light scattering using a light scattering photometer (DLS-700, manufactured by Otsuka Electronics Co., Ltd.).
[0082] The abbreviations used in the following description are as follows: MMA: Methyl methacrylate MA: Methyl acrylate n-BA: n-butyl acrylate 1,3-BD: butylene glycol dimethacrylate St: Styrene AMA: Allyl methacrylate CHP: Cumene hydroperoxide t-BH: t-butyl hydroperoxide n-OM: n-octyl mercaptan EDTA: disodium ethylenediaminetetraacetate SFS: Sodium formaldehyde sulfoxylate (Rongalite) RS610NA: Sodium polyoxyethylene alkyl ether phosphate (manufactured by Toho Chemical Industry Co., Ltd., trade name: Phosphanol RS610NA)
[0083] <Acrylic rubber polymer> [Production Example 1] Production of rubber-containing multistage polymer (I) After 10.8 parts of deionized water was charged into a vessel equipped with a stirrer, monomer components (ia-1) consisting of 0.3 parts of MMA, 4.5 parts of n-BA, 0.2 parts of 1,3-BD, 0.05 parts of AMA, and 0.025 parts of CHP were added and mixed by stirring at room temperature. Next, 1.3 parts of RS610NA was added to the vessel while stirring, and stirring was continued for 20 minutes to prepare "emulsion 1".
[0084] Next, 156.0 parts of deionized water was added to a polymerization vessel equipped with a reflux condenser, and the temperature was raised to 74°C. Furthermore, a mixture was prepared by adding 0.20 parts of SFS, 0.0001 parts of ferrous sulfate, and 0.0003 parts of EDTA to 4.5 parts of deionized water, and this mixture was added to the polymerization vessel. Next, while stirring under a nitrogen atmosphere, the emulsion 1 was dropped into the polymerization vessel over 9 minutes, and the reaction was continued for 15 minutes to complete the polymerization of the first elastic polymer (I-a1).
[0085] Then, MMA 9.6 parts, n-BA 14.4 parts, 1,3-BD 1 part, AMA 0.25 parts and CHP 0.016 parts of monomer component (ia-2) were dropped into the polymerization vessel over 90 minutes, and the reaction was continued for 60 minutes to produce a second elastomer (I-a2). In this way, an elastomer (IA) containing a first elastomer (I-a1) and a second elastomer (I-a2) was obtained.
[0086] Next, a monomer component (ic) consisting of 6 parts of MMA, 4 parts of MA, 0.075 parts of AMA and 0.013 parts of CHP was added dropwise to the polymerization vessel over 45 minutes, and the reaction was continued for 60 minutes to form an intermediate polymer (IC).
[0087] Then, monomer components (ib) consisting of 57 parts of MMA, 3 parts of MA, 0.075 parts of t-BH and 0.264 parts of n-OM were dropped into the polymerization vessel over 140 minutes, and the reaction was continued for 60 minutes to form a hard polymer (IB) and obtain a polymer latex of rubber-containing multi-stage polymer (I). The average particle size of the resulting latex-like rubber-containing multi-stage polymer (I) was 0.11 μm.
[0088] The polymer latex of the rubber-containing multi-stage polymer (I) obtained is filtered using a vibration filter with a SUS mesh (average mesh size: 54 μm) attached to the filter medium, then salted out in an aqueous solution containing 3.5 parts of calcium acetate, washed with water, recovered, and then dried to obtain a powdered rubber-containing multi-stage polymer (I).The gel content of the rubber-containing multi-stage polymer (I) is 70%, and Mw is 58,000.
[0089] [Production Example 2] Production of rubber-containing multi-stage polymer (II) In a nitrogen atmosphere, 153 parts of deionized water was placed in a reaction vessel equipped with a reflux condenser and heated to 80°C. 0.4 parts of SFS, 0.00004 parts of ferrous sulfate, and 0.00012 parts of EDTA were added, and while stirring, 50.9 parts of n-BA, 11.6 parts of St, 0.56 parts of AMA, 0.19 parts of t-BH, and 1.0 part of RS610NA were added. The mixture was then held for 1 hour to polymerize, yielding an elastic polymer (II-A).
[0090] Next, 0.1 parts of SFS was added to the vessel. After 15 minutes, 35.6 parts of MMA, 1.9 parts of MA, 0.056 parts of t-BH, 0.16 parts of n-OM, and 0.25 parts of RS610NA were added while stirring at 80°C under a nitrogen atmosphere. After that, the vessel was held for 1 hour to polymerize, forming a hard polymer (II-B), and a latex of a rubber-containing multi-stage polymer (II) was obtained. The average particle size of the rubber-containing multi-stage polymer (II) was 0.12 μm.
[0091] The latex of the rubber-containing multi-stage polymer (II) was filtered through a filter with a mesh size of 50 μm. It was then coagulated with calcium acetate, filtered, washed with water, and dried to obtain the rubber-containing multi-stage polymer (II). The gel content of the rubber-containing multi-stage polymer (II) was 84%, and Mw was 61,000.
[0092] <Polycarbonate> [Production Example 3] Production of polycarbonate (A-1) Polycarbonate (A-1) was obtained by a method according to JP 2008-024919 A, in which the molar ratio of monomer units derived from isosorbide, a dihydroxy compound, and monomer units derived from tricyclodecane dimethanol was isosorbide / tricyclodecane dimethanol=70 / 30 mol %. The glass transition temperature was 130°C.
[0093] [Production Example 4] Production of polycarbonate (A-2) By a method according to JP 2022-106010 A, a polycarbonate (A-2) was obtained in which the molar ratio of monomer units derived from isosorbide, a dihydroxy compound, and monomer units derived from 1,4-cyclohexanedimethanol was isosorbide / 1,4-cyclohexanedimethanol = 70 / 30 mol%. The glass transition temperature was 124 ° C.
[0094] [Production Example 5] Production of film (F-1) of polycarbonate (A-1) The polycarbonate (A-1) pellets obtained in Production Example 3 were dried overnight at 80° C. in a dehumidifying dryer. The dried pellets were extruded into a film using a 25 mmφ (diameter) non-vented screw extruder (L / D=20) equipped with a 150 mm wide T-die at a cylinder temperature of 210°C to 250°C, a T-die temperature of 250°C, and a cooling roll temperature of 80°C to obtain a 100 μm thick film (F-1).
[0095] [Production Example 6] Production of polycarbonate (A-2) film (F-2) A film (F-2) having a thickness of 100 μm was obtained in the same manner as in Production Example 5, except that the pellets of the polycarbonate (A-2) obtained in Production Example 4 were used.
[0096] [Production Example 7] Production of acrylic resin composition (I-1) 75 parts of the rubber-containing multistage polymer (I) obtained in Production Example 1, 15 parts of an alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET VH), and 0.1 parts of a hindered phenol-based antioxidant (manufactured by BASF Japan Ltd.; product name: Irganox1076) as an additive were mixed using a Henschel mixer. Thereafter, the mixture was extruded into a strand shape using a twin-screw extruder (manufactured by Toshiba Machine Co., Ltd.; product name: TEM-35B, the same applies below) under conditions of a cylinder temperature of 200 to 240°C and a die head temperature of 240°C while removing impurities with a filter, and was cut after passing through a water tank to obtain pellets of a transparent acrylic resin composition (I-1). The gel content was 48%.
[0097] [Production Example 8] Production of acrylic resin composition (II-1) Pellets of a transparent acrylic resin composition (II-1) were obtained in the same manner as in Production Example 7, except that the rubber-containing multistage polymer (II) obtained in Production Example 2 was changed to 50 parts, and the alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET VH) was changed to 50 parts. The gel content was 41%.
[0098] [Production Example 9] Production of acrylic resin composition (II-2) Pellets of a transparent acrylic resin composition (II-2) were obtained in the same manner as in Production Example 7, except that the amount of the rubber-containing multistage polymer (II) obtained in Production Example 2 was changed to 20 parts, and the amount of the alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET VH) was changed to 80 parts. The gel content was 16%.
[0099] [Production Example 10] Production of acrylic resin composition (I-2) Pellets of a transparent acrylic resin composition (I-2) were obtained in the same manner as in Production Example 7, except that 1.1 parts of a benzotriazole-based ultraviolet absorber (manufactured by ADEKA Corporation; product name: Adeka STAB LA-31G) and 0.2 parts of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd.; product name: Chimassorb 2020FDL) were added as additives to the formulation of Production Example 7. The gel content was 49%.
[0100] [Example 1] Production of a laminate (TI) of a polycarbonate film (F-1) and an acrylic resin composition (I-1) The pellets of the acrylic resin composition (I-1) obtained in Production Example 7 were hot pressed at 220° C. to prepare a sheet of the acrylic resin composition having a thickness of 500 μm. Next, the obtained sheet of acrylic resin composition and the polycarbonate film obtained in Production Example 5 were sandwiched between mirror-finished SUS plates, and heat-pressed under conditions of 140°C, 4.9 MPa, and 5 minutes, and then cooled to room temperature while applying a pressure of 5.0 MPa to obtain a polycarbonate and acrylic resin composition laminate (TI). An adhesion evaluation was performed on the polycarbonate film side of the obtained laminate. The results of the adhesion evaluation are shown in Table 1.
[0101] [Example 2] Production of a laminate (T-II) of a polycarbonate film (F-1) and an acrylic resin composition (II-1) A laminate (T-II) was obtained in the same manner as in Example 1, except that the pellets obtained in Production Example 8 were used as the acrylic resin composition. The adhesion of the obtained laminate was evaluated on the polycarbonate film side. The results of the adhesion evaluation are shown in Table 1.
[0102] Comparative Example 1: Production of a laminate (T-III) of a polycarbonate film (F-1) and an acrylic resin composition (II-2) A laminate (T-III) was obtained in the same manner as in Example 1, except that the pellets obtained in Production Example 9 were used as the acrylic resin composition. The adhesion of the obtained laminate was evaluated on the polycarbonate film side. The results of the adhesion evaluation are shown in Table 1.
[0103] [Comparative Example 2] Production of a laminate (T-IV) of a polycarbonate film (F-1) and an acrylic resin composition A laminate (T-IV) was obtained in the same manner as in Example 1, except that pellets of an alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET VH) were used as the acrylic resin composition. An adhesion evaluation was carried out on the polycarbonate film side of the obtained laminate. The results of the adhesion evaluation are shown in Table 1. The gel content of ACRYPET VH was 0%.
[0104] [Comparative Example 3] Production of a laminate (TV) of a polycarbonate film (F-2) and an acrylic resin composition (I-1) A laminate (TV) was obtained in the same manner as in Example 1, except that the film (F-2) obtained in Production Example 6 was used as the polycarbonate film. The adhesion evaluation was performed on the polycarbonate film side of the obtained laminate. The results of the adhesion evaluation are shown in Table 1.
[0105] Comparative Example 4: Production of a laminate (T-VI) of a polycarbonate film (F-2) and an acrylic resin composition (II-1) A laminate (T-VI) was obtained in the same manner as in Comparative Example 3, except that the pellets obtained in Production Example 8 were used as the acrylic resin composition. The adhesion of the obtained laminate was evaluated on the polycarbonate film side. The results of the adhesion evaluation are shown in Table 1.
[0106] Comparative Example 5: Production of a laminate (T-VII) of a polycarbonate film (F-2) and an acrylic resin composition (II-2) A laminate (T-VII) was obtained in the same manner as in Comparative Example 3, except that the pellets obtained in Production Example 9 were used as the acrylic resin composition. The adhesion of the obtained laminate was evaluated on the polycarbonate film side. The results of the adhesion evaluation are shown in Table 1.
[0107] [Comparative Example 6] Production of a laminate (T-VIII) of a polycarbonate film (F-2) and an acrylic resin composition A laminate (T-VIII) was obtained in the same manner as in Comparative Example 3, except that pellets of an alkyl methacrylate-alkyl acrylate copolymer (manufactured by Mitsubishi Chemical Corporation; product name: ACRYPET VH) were used as the acrylic resin composition. An adhesion evaluation was carried out on the polycarbonate film side of the obtained laminate. The results of the adhesion evaluation are shown in Table 1.
[0108] [Production Example 11] Production of polycarbonate resin composition (A-1A) 100 parts of the polycarbonate (A-1) obtained in Production Example 3, 0.8 parts of a hindered phenol-based antioxidant (manufactured by ADEKA Corporation, product name: Adeka STAB AO-60) and 0.34 parts of a hindered amine-based light stabilizer (manufactured by BASF Japan Ltd., product name: Chimassorb2020FDL) were added as additives, and then mixed using a Henschel mixer. Thereafter, the mixture was extruded into a strand shape using a twin-screw extruder under conditions of a cylinder temperature of 180 to 200 ° C. and a die head temperature of 250 ° C. while removing impurities with a filter, and then cut after passing through a water tank to obtain pellets of a transparent polycarbonate resin composition (A-1A).
[0109] [Production Example 12] Production of polycarbonate resin composition (A-1B) Pellets of a transparent polycarbonate resin composition (A-1B) were obtained in the same manner as in Production Example 11, except that 0.34 parts of the hindered amine-based light stabilizer in Production Example 11 was changed to 0.3 parts of a hindered amine-based light stabilizer (manufactured by ADEKA CORPORATION; product name: Adeka STAB LA-57G).
[0110] [Production Example 13] Production of polycarbonate resin composition (A-1C) Pellets of a transparent polycarbonate resin composition (A-1C) were obtained in the same manner as in Production Example 11, except that 2.1 parts of a benzotriazole-based ultraviolet absorber (manufactured by ADEKA Corporation; product name: Adeka STAB LA-31G) was added to the formulation of Production Example 12.
[0111] [Example 3] Laminate (T-IX) of polycarbonate (A-1) and acrylic resin composition (I-2) Pellets of polycarbonate (A-1) obtained in Production Example 3 as the polycarbonate resin layer and pellets of acrylic resin composition (I-2) obtained in Production Example 10 as the acrylic resin layer were dehumidified and dried at 85 ° C. for one day. Using a 30 mm φ non-vent screw type extruder, polycarbonate (A-1) was plasticized under the condition of a cylinder temperature of 200 to 240 ° C., while using a 40 mm φ non-vent screw type extruder, acrylic resin composition (I-2) was plasticized under the condition of a cylinder temperature of 220 to 240 ° C., and then, using a 500 mm wide two-kind two-layer multi-manifold T die set at 245 ° C., a laminate film with a polycarbonate resin layer thickness of 10 μm and an acrylic resin layer thickness of 65 μm was produced as a laminate (T-IX) with the acrylic resin layer side in contact with a mirror-cooled roll.
[0112] Next, a vacuum pump was installed at the bottom of the mold on the cavity side, 3 cm horizontally from the central gate, and 1 cm 2 Using a mold with a 1 mm deep recess, in-mold molding was performed using an in-mold molding device that combined a J85ELII injection molding machine (manufactured by Japan Steel Works, Ltd., product name) and a hot pack system (manufactured by Nissha Printing Co., Ltd., product name) so that a polycarbonate resin layer was placed on the inner wall surface of the mold. The detailed shape of the laminate is a box shape with dimensions of 150mm length x 120mm width x 2mm thickness and 10mm depth, and the gate positions of the mold are three in total, one in the center of the laminate and one each 40mm above and below the central gate (vertical direction of the laminate), and the gate shape is a pinpoint gate with a diameter of 1mm. Also, the corner radius of the corner connecting the bottom and side of the cavity side of the mold is approximately 3. In other words, the corner radius of the laminate on the side where the laminate film is laminated is approximately 3. The corner radius was measured using a FUJI TOOL RADIUS GAGE.
[0113] The vacuum forming of the laminated film was performed under the conditions of a heater temperature of about 330° C., a heating time of 6 seconds, and a distance of 15 mm between the heater and the film, with the polycarbonate resin layer side in contact with the mold. In the subsequent injection molding carried out in the same mold, the substrate (Y) resin was injected from the opposite side of the polycarbonate resin layer under the conditions of a cylinder temperature of 250°C, an injection speed of 30%, an injection pressure of 43%, and a mold temperature of 60°C. A heat-resistant ABS resin (manufactured by Techno UMG Co., Ltd., product name "Bulksam TM25B") was used as the substrate (Y) resin. After injection molding, a laminated molded product was obtained in which the polycarbonate resin layer side was arranged on the surface. The adhesion of the polycarbonate resin layer side of the obtained laminated molded product was evaluated, and the results are shown in Table 2.
[0114] [Example 4] Laminate (TX) of polycarbonate resin composition (A-1A) and acrylic resin composition (I-2) Except for using the polycarbonate resin composition (A-1A) obtained in Production Example 11 as the polycarbonate resin layer, a laminate film and a laminate molded product were obtained as the laminate (TX) in the same manner as in Example 3. The results of the adhesion evaluation of the polycarbonate resin layer side of the obtained laminate molded product are shown in Table 2.
[0115] [Example 5] Laminate (T-XI) of polycarbonate resin composition (A-1B) and acrylic resin composition (I-2) Except for using the polycarbonate resin composition (A-1B) obtained in Production Example 12 as the polycarbonate resin layer, a laminate film and a laminate molded article were obtained as a laminate (T-XI) in the same manner as in Example 3. The results of the adhesion evaluation of the polycarbonate resin layer side of the obtained laminate molded article are shown in Table 2.
[0116] [Example 6] Laminate (T-XII) of polycarbonate resin composition (A-1C) and acrylic resin composition (I-2) Except for using the polycarbonate resin composition (A-1C) obtained in Production Example 13 as the polycarbonate resin layer, a laminate film and a laminate molding were obtained as a laminate (T-XII) in the same manner as in Example 3. The results of the adhesion evaluation of the polycarbonate resin layer side of the obtained laminate molding are shown in Table 2.
[0117] [Comparative Example 7] Laminate (T-XIII) of polycarbonate (A-2) and acrylic resin composition (I-2) Except for using the polycarbonate (A-2) obtained in Production Example 4 as the polycarbonate resin layer, a laminate film and a laminate molded product were obtained as a laminate (T-XIII) in the same manner as in Example 3. The results of the adhesion evaluation are shown in Table 2.
[0118] [Table 1]
[0119] [Table 2]
[0120] The laminates of Examples 1 to 6 have good adhesion because the polycarbonate resin has a structural unit derived from tricyclodecane dimethanol and the layer containing an acrylic resin has a gel content of 20% by mass or more. On the other hand, the laminates of Comparative Examples 1 and 2 have poor adhesion because the layer containing an acrylic resin does not have a gel content of 20% by mass or more. Moreover, the laminates of Comparative Examples 3, 4, and 7 have poor adhesion even though the polycarbonate resin does not have a structural unit derived from tricyclodecane dimethanol and the layer containing an acrylic resin has a gel content of 20% by mass or more. Furthermore, the laminates of Comparative Examples 5 and 6 have poor adhesion because the polycarbonate resin does not have a structural unit derived from tricyclodecane dimethanol and the layer containing an acrylic resin does not have a gel content of 20% by mass or more. [Industrial Applicability]
[0121] The laminate of the present invention can be used as a transparent sheet for building materials, interior parts, display covers, etc., a sheet for resin-coated metal plates, a sheet for molding (vacuum / pressure molding, hot press molding, etc.), a colored plate, a transparent plate, a shrink film, a shrink label, a shrink tube, an automobile interior material, a home appliance component, an office equipment component, etc.
Claims
1. A laminate including a layer mainly made of a polycarbonate resin and a layer mainly made of an acrylic resin, The polycarbonate resin has a structural unit derived from tricyclodecane dimethanol represented by the following formula (1), The layer containing the acrylic resin as a main component has a gel content of 20 mass % or more in a total amount of resin constituting the layer. 【Chemistry 1】 [In formula (1), R 1 represents a hydroxymethyl group, R 2 , R 3 and R 4 one of the groups represents a hydroxymethyl group, and the remaining groups represent a hydrogen atom.
2. The laminate according to claim 1 , wherein the polycarbonate resin further has a structural unit derived from a dihydroxy compound represented by the following formula (2): 【Chemistry 2】
3. 3. The laminate according to claim 1, wherein the content of the structural unit derived from tricyclodecane dimethanol is 20 to 50 mol % in 100 mol % of the polycarbonate resin.
4. 3. The laminate according to claim 2, wherein the content of the structural unit derived from the dihydroxy compound is 50 to 80 mol % in 100 mol % of the polycarbonate resin.
5. The laminate according to claim 1 or 2, wherein the acrylic resin further contains an acrylic rubber polymer.
6. 6. The laminate according to claim 5, wherein the acrylic rubber polymer is a graft polymer having a polymer having a glass transition temperature of 0°C or lower and a polymer having a glass transition temperature of 20°C or higher.
7. The laminate according to claim 5, wherein the acrylic rubber polymer has a mass average particle size of 100 to 300 nm.
Citation Information
Patent Citations
Polycarbonate resin molding having hard coat layer
JP2005179504A
Polycarbonate resin molded product
JP2008150548A
Scratch-resistant resin plate, display protective plate using the same, and display window protective plate of portable data terminal
JP2011148130A
Laminated optical film, and polarizing plate