Direct thermosensitive recording material
The direct thermal recording material addresses scratches and pinholes by incorporating a specific composition of organic silver salt, water-soluble resin, and crosslinking agent, achieving high-quality image formation for printing plates.
Patent Information
- Application Number
- JP2023050938
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Direct thermal recording materials suffer from scratches and pinholes due to contact with thermal heads, which impair their functionality as printing plate materials.
A direct thermal recording material is developed with a heat-sensitive recording layer containing a non-photosensitive organic silver salt, a water-soluble resin, a crosslinking agent, an acidic compound with a pKa of 4.3 or less, and a salt obtained by neutralizing the acidic compound, with a specific mass ratio of water-soluble resin to crosslinking agent in the protective layer ranging from 0.2 to 2.5.
The material effectively suppresses scratches and pinholes, ensuring high-quality image formation suitable for printing plate materials.
Smart Images

Figure 2024139971000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a direct thermal recording material for forming an image by heating with a thermal head, and more particularly to a direct thermal recording material suitable for producing a block copy material. [Background technology]
[0002] As a method for recording high-quality images, a wet-processing image forming method using a silver halide photosensitive material has been generally used for a long time. However, this image forming method requires waste liquid treatment such as a developer and a fixer, and installation of a development processing facility, so a dry-processing image forming method that does not require the wet processing has been desired. As a result, image forming systems such as inkjet printers, electrophotography, and dye thermal transfer systems have been put to practical use at present. However, these dry-processing image forming methods have difficulty in obtaining the high resolution, excellent light shielding properties in image areas, and excellent light transmittance in non-image areas required for a plate material.
[0003] In this context, a direct thermal recording material utilizing the reaction between a non-photosensitive organic silver salt and an organic reducing agent is disclosed, for example, in Patent Document 1. Such a direct thermal recording material is suitable for producing a plate material because it can obtain a high-resolution, high-contrast image by directly recording a thermal image with a thermal printer equipped with a thermal head. In addition, the recording material is non-photosensitive and does not require a darkroom equipped with safelight, and direct thermal type thermal printers have the advantage of being low-cost, highly reliable, and easy to miniaturize, making their introduction easy.
[0004] In the direct thermal recording material used in the direct thermal recording method, a protective layer is generally provided on the thermal recording layer to prevent the thermal head from adhering to the thermal recording layer during printing, i.e., so-called sticking. It is also known that the protective layer contains a crosslinked resin, which is effective in terms of transparency and printability required for the underlay material. For example, Patent Document 1 discloses a direct thermal recording material having a protective layer containing a hydrophilic polymer reacted with a curing agent having an active hydrogen atom, or a polymer crosslinked by ultraviolet light or an electron beam. Patent Document 2 discloses a direct thermal recording material having a protective layer containing a water-soluble resin and a crosslinking agent. Patent Document 3 discloses a reversible thermal recording material having an intermediate layer mainly composed of a heat-resistant resin and a lubricating protective layer mainly composed of a crosslinked cured product of a silicone-modified polyurethane resin and a polyisocyanate on the thermal layer.
[0005] However, in such a direct thermal recording material, the surface of the thermal recording layer may be scratched by contact with a thermal head, causing defects in the image, and when used as a block copy material, the function may be impaired. As a method for suppressing the occurrence of such scratches, a method is known in which fine irregularities are made on the surface by using fine particles to reduce friction with the thermal head, and for example, Patent Document 4 discloses a thermal recording material having a protective layer containing a matting agent. However, in such a thermal recording material, pinholes may occur in the image where the matting agent is present, and improvement was required. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Special Publication No. 9-504752 [Patent Document 2] JP 2007-38633 A [Patent Document 3] Japanese Patent Application Publication No. 05-38881 [Patent Document 4] Special Publication No. 08-503175 Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a direct thermal recording material which is suppressed from being scratched due to contact with a thermal head and which is further suppressed from having pinholes. [Means for solving the problem]
[0008] The above problems are solved by the following invention. A direct thermal recording material comprising at least a thermal recording layer on a light-transmitting support, the thermal recording layer containing a non-photosensitive organic silver salt and a reducing agent, and a protective layer containing, from the side closest to the light-transmitting support, (A) a water-soluble resin, (B) a crosslinking agent for the water-soluble resin, (C) an acidic compound having a pKa of 4.3 or less, and (D) a salt obtained by neutralizing the acidic compound, the mass ratio (B) / (A) of the component (A) to the component (B) in the protective layer being 0.2 to 2.5. Effect of the Invention
[0009] According to the present invention, it is possible to provide a direct thermal recording material which is suppressed from being scratched due to contact with a thermal head and further suppressed from being susceptible to pinholes. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] The present invention will be described in detail below.
[0011] The direct thermal recording material of the present invention has a light-transmitting support. Examples of such light-transmitting supports include resin films such as polyethylene terephthalate, polyethylene naphthalate, cellulose nitrate, and polycarbonate, and inorganic materials such as glass. In the present invention, the light-transmitting support means a support having a total light transmittance of 60% or more, and more preferably, the total light transmittance of the support is 70% or more. In addition, the haze value of the light-transmitting support is preferably 10% or less. The light-transmitting support may have known layers such as an easy-adhesion layer, a hard coat layer, and an antistatic layer. The thickness of the light-transmitting support in the present invention is not particularly specified, but from the viewpoint of handling, it is preferably 50 μm or more and 300 μm or less.
[0012] The heat-sensitive recording layer of the direct heat-sensitive recording material of the present invention contains a non-photosensitive organic silver salt. The organic silver salt is reduced by heating together with a reducing agent described later to form a silver image. Specifically, silver salts of organic acids such as gallic acid, oxalic acid, behenic acid, stearic acid, palmitic acid, and lauric acid as described in Research Disclosure No. 17029(II) and No. 29963(XVI) related to heat-developable photosensitive materials; silver salts of carboxyalkylthioureas such as 1-(3-carboxypropyl)thiourea and 1-(3-carboxypropyl)-3,3-dimethylthiourea; silver salts of aldehydes such as formaldehyde, acetaldehyde, and butylaldehyde, and aromatic thioureas such as salicylic acid, benzoic acid, 3,5-dihydroxybenzoic acid, and 5,5-thiodisalicylic acid are used. Examples of the silver salt include a complex of a polymer reaction product with a carboxylic acid and silver; a silver salt or complex of thiones such as 3-(2-carboxyethyl)-4-hydroxymethyl-4-thiazoline-2-thione and 3-carboxymethyl-4-methyl-4-thiazoline-2-thione; a silver salt or complex of a nitrogen-containing heterocycle selected from imidazole, pyrazole, urazole, 1,2,4-triazole, 1H-tetrazole, 3-amino-5-benzylthio-1,2,4-triazole and benzotriazole; a silver salt of saccharin, 5-chlorosalicylaldoxime, etc.; and a silver salt of a mercaptide. Among these, a silver salt of a fatty acid having 10 or more carbon atoms is preferred, and silver stearate and silver behenate are more preferred.
[0013] In the present invention, the content of the non-photosensitive organic silver salt contained in the thermosensitive recording layer is preferably 5 to 80 mass %, more preferably 10 to 70 mass %, and even more preferably 20 to 65 mass %, based on the total solid content of the thermosensitive recording layer, from the viewpoints of the sensitivity and storage stability of the thermosensitive recording material.
[0014] The heat-sensitive recording layer of the direct heat-sensitive recording material of the present invention contains a reducing agent. Examples of such reducing agents include polyhydroxybenzene compounds such as hydroquinone, catechol, 4-methylcatechol, 4-tert-butylcatechol, chlorohydroquinone, and pyrogallol, polyhydroxybenzoic acid compounds such as gallic acid, methyl gallate, ethyl gallate, propyl gallate, stearyl gallate, 2,5-dihydroxybenzoic acid, 3,4-dihydroxybenzoic acid, and ethyl 3,4-dihydroxybenzoate, aminophenol compounds such as 2-aminophenol, 3-aminophenol, and 4-aminophenol, 1-phenyl-3-pyrazolidone and its derivatives, hydroxylamines, polyhydroxyindanes described in JP-A-6-317870, and dihydroxybenzoic acid derivatives described in JP-A-2001-328357. Among the above-mentioned reducing agents, polyhydroxybenzene compounds and polyhydroxybenzoic acid compounds are preferred.
[0015] The content of the reducing agent in the thermosensitive recording layer can vary widely depending on the type of reducing agent and the type of organic silver salt, but from the viewpoint of the sensitivity and storage stability of the thermosensitive recording material, it is preferably 0.1 to 3.0 mol per mol of organic silver salt, and more preferably 0.5 to 2.0 mol. For various purposes, two or more of the above-mentioned reducing agents may be used in combination.
[0016] The heat-sensitive recording layer of the direct heat-sensitive recording material of the present invention preferably contains a resin as a binder component that holds the non-photosensitive organic silver salt and the reducing agent. Such resins are not particularly limited, and known resins can be used, such as cellulose derivatives such as hydroxyethyl cellulose and hydroxypropyl cellulose, gelatin, acrylic resins, melamine resins, polyester resins, polyurethane resins, polyvinyl acetal resins such as polyvinyl butyral resins, and polyvinyl alcohol resins. Among them, polyvinyl acetal resins such as polyvinyl butyral resins and polyvinyl alcohol resins are preferred, and polyvinyl acetal resins are more preferred, because they have excellent dispersibility of the non-photosensitive organic silver salts described above. These resins may be used by dissolving them in water or an organic solvent, or may be used as latexes in which hydrophobic polymer solids are dispersed in the form of fine particles, or polymer molecules are dispersed in the form of micelles. In the present invention, the above-mentioned resins are preferably those that form a light-transmitting coating after drying. Furthermore, these resins may be used in combination of two or more mutually compatible resins as necessary.
[0017] In the present invention, the content of the resin contained in the thermosensitive recording layer is preferably 10 to 70% by mass, more preferably 20 to 60% by mass, based on the total solid content of the thermosensitive recording layer, from the viewpoints of the sensitivity and storage stability of the thermosensitive recording material.
[0018] The above-mentioned resin preferably does not substantially contain free halide ions such as chloride ions and bromide ions. The halide ions react with the silver ions of the organic silver salt to form photosensitive silver halide, which causes a decrease in the light resistance of the direct thermal recording material of the present invention. Specifically, the content of the halide ions is preferably 500 ppm or less, more preferably 300 ppm or less, and even more preferably 100 ppm or less relative to the content of the resin.
[0019] The thermosensitive recording layer of the direct thermosensitive recording material of the present invention preferably contains a so-called color toner, which is known in the field of thermography or photothermography. Examples of color toners are known in the above-mentioned Research Disclosure on Photothermographic Materials, items 17029(V) and 29963(XXII), and specifically include imides such as phthalimide, mercapto compounds such as 3-mercapto-1,2,4-triazole, phthalic acid derivatives such as phthalazine, phthalazone, 4-methylphthalic acid, tetrachlorophthalic acid and their anhydrides, and benzoxazine derivatives such as 1,3-benzoxazine-2,4-dione. For various purposes, the above-mentioned color toners may contain two or more kinds.
[0020] In the present invention, the content of the color toning agent contained in the thermosensitive recording layer is preferably 0.10 to 30 mass %, more preferably 0.50 to 20 mass %, and even more preferably 1.0 to 15 mass %, based on the total solid content of the thermosensitive recording layer, from the viewpoints of the sensitivity and storage stability of the thermosensitive recording material.
[0021] The heat-sensitive recording layer of the direct heat-sensitive recording material of the present invention may contain various accelerators, stabilizers and their precursors, together with the organic silver salt described above, for the purpose of suppressing or promoting the formation of image silver by reduction, improving the storage stability before and after printing, etc. Specifically, they may be selected from benzotriazole, 5-methylbenzotriazole, 5-chlorobenzotriazole, 2-mercaptobenzotriazole, 2-mercaptobenzimidazole, 2-mercaptobenzothiazole, 2-mercaptobenzoxazole, 4-hydroxy-6-methyl-1,3,3a,7-tetrazaindene, 1-phenyl-5-mercaptotetrazole, 2-amino-5-mercapto-1,3,4-thiadiazole, 3-mercapto-5-phenyl-1,2,4-triazole, 4-benzamido-3-mercapto-5-phenyl-1,2,4-triazole, etc., which are well known as photographic stabilizers and inhibitors. In addition, two or more of the accelerators and stabilizers described above may be used in combination for various purposes.
[0022] In addition to the above-mentioned components, the heat-sensitive recording layer may contain known additives such as ultraviolet absorbers, antioxidants, pigments, dyes, pH adjusters, surfactants, defoamers, thickeners, softeners, lubricants, crosslinking agents, antistatic agents, and antiblocking agents.
[0023] As a method for forming the above-mentioned thermosensitive recording layer on a light-transmitting support, it is preferable to prepare a thermosensitive recording layer coating liquid containing the above-mentioned non-photosensitive organic silver salt, a reducing agent, a resin, a color toner, and additives that can be contained in the thermosensitive recording layer, and further a known solvent, and then coat the thermosensitive recording layer coating liquid on the above-mentioned light-transmitting support and dry it to form the layer. In addition, the coating amount of the thermosensitive recording layer coating liquid is 2.0 to 30 g / m2 in terms of dry mass in order to obtain a necessary and sufficient UV transmission density as a plate material. 2 is preferable, and 5.0 to 25 g / m 2 More preferably, 8.0 to 20 g / m 2 is more preferred.
[0024] The direct thermal recording material of the present invention has a protective layer on the above-mentioned thermal recording layer. The protective layer contains a water-soluble resin. The water-soluble resin in the present invention refers to a resin that dissolves in water at a ratio of 5.0% by mass or more. Specific examples include cellulose derivatives such as hydroxyethyl cellulose and hydroxypropyl cellulose, polyvinyl acetal resins such as polyvinyl butyral resins, polyvinyl alcohol resins, gelatin, acrylic resins, melamine resins, polyester resins, polyurethane resins, vinyl acetate resins, polyolefin resins, and the like. Among these, acrylic resins, polyvinyl acetal resins, and polyvinyl alcohol resins are preferred, and polyvinyl acetal resins and polyvinyl alcohol resins are more preferred. In addition, the content of the water-soluble resin in the protective layer is preferably 10 to 95% by mass, more preferably 20 to 90% by mass, and even more preferably 30 to 85% by mass of the total solid content of the protective layer in order to obtain sufficient coating strength when handled as a plate material.
[0025] The protective layer in the present invention contains a crosslinking agent together with the above-mentioned resin so as to withstand the application of heat during printing by a thermal head. The crosslinking agent for crosslinking the resin is not particularly limited, but examples thereof include a polyisocyanate compound having two or more isocyanate groups in the molecule, a polyepoxy compound having two or more epoxy groups in the molecule, a polyfunctional (meth)acrylate monomer having two or more acryloyl groups and / or methacryloyl groups in the molecule, boric acid, alkoxysilane, a silicate oligomer which is a partial condensate thereof, titanium alkoxide, zirconium alkoxide, etc., among which polyfunctional (meth)acrylate monomer, polyisocyanate compound, alkoxysilane, and silicate oligomer are preferred, and polyisocyanate compound, alkoxysilane, and silicate oligomer are more preferred. Furthermore, in order to obtain sufficient coating strength when handled as a plate material, the content of the crosslinking agent in the protective layer is preferably 5 to 90 mass %, more preferably 10 to 80 mass %, and even more preferably 20 to 70 mass %, of the total solids content of the protective layer.
[0026] The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent (B) for the water-soluble resin contained in the protective layer in the present invention must be in the range of 0.2 to 2.5. If the amount of crosslinking agent is less than this range, scratch resistance decreases, and if the amount is more than this range, pinholes increase in the printed image. The mass ratio (B) / (A) of the water-soluble resin and the crosslinking agent is preferably 0.3 to 2.0, more preferably 0.4 to 1.5.
[0027] The protective layer in the present invention contains an acidic compound having a pKa of 4.3 or less. The pKa of the acidic compound in the present invention is a value measured by neutralization titration, and the acidic compound having a pKa of 4.3 or less is not particularly limited, but specifically includes inorganic acids such as sulfuric acid (pKa-3.0), nitric acid (pKa-1.3), and phosphoric acid (pKa2.12), and organic acids such as lactic acid (pKa3.84), maleic acid (pKa1.93), fumaric acid (pKa3.03), citric acid (pKa3.09), p-toluenesulfonic acid (pKa-1.34), and methanesulfonic acid (pKa-2.6). Among these, organic acids are preferred, and lactic acid, fumaric acid, p-toluenesulfonic acid, and methanesulfonic acid are more preferred, and lactic acid and p-toluenesulfonic acid are even more preferred. Two or more of these acidic compounds may be used in combination. Furthermore, in order to ensure a sufficient pot life of the protective layer coating solution during production, the content of the acidic compound (when a salt obtained by neutralizing an acidic compound having a pKa of 4.3 or less is contained in the protective layer, as described below, and the acidic compound is neutralized in the protective layer to produce a salt, the amount of free acid remaining after the neutralization) is preferably 0.010 to 5.0 mass %, more preferably 0.030 to 4.0 mass %, and even more preferably 0.050 to 3.0 mass %, relative to the total solids content of the protective layer.
[0028] The protective layer in the present invention contains a salt obtained by neutralizing the above-mentioned acidic compound. In the present invention, the salt obtained by neutralizing the acidic compound is a compound in which the proton of the above-mentioned acidic compound is replaced with another cationic species such as lithium ion, sodium ion, potassium ion, ammonium ion, calcium ion, etc., and in the case of sodium salt, examples thereof include sodium sulfate, sodium nitrate, sodium phosphate, sodium lactate, disodium maleate, monosodium maleate, monosodium fumarate, disodium fumarate, sodium citrate, sodium p-toluenesulfonate, and sodium methanesulfonate. Two or more of these salts may be used in combination. As a method for incorporating the salt of the acidic compound in the protective layer, a basic compound may be incorporated in the protective layer and the above-mentioned acidic compound may be neutralized to generate the salt, or the salt of the acidic compound may be directly added. If the amount of the salt of the acidic compound is too much relative to the acidic compound, pinholes increase, and if the amount of the salt is too little, the prevention of scratches due to contact with a thermal head becomes insufficient. From this viewpoint, the molar ratio of the salt of the acidic compound to the acidic compound is preferably in the range of 0.010 to 10, more preferably in the range of 0.050 to 9.0, and even more preferably in the range of 0.10 to 5.0.
[0029] In the present invention, the protective layer may contain various matting agents for the purpose of improving transportability. When forming the protective layer, it is preferable to use the matting agent by dispersing it in the protective layer. A high-speed stirrer such as a homodisper is suitable for dispersing the matting agent.
[0030] The amount of the matting agent that can be contained in the protective layer is preferably 0.50 to 40 mass %, more preferably 1.0 to 30 mass %, and even more preferably 3.0 to 20 mass %, relative to the content of the resin contained in the protective layer.
[0031] The matting agent may be either organic or inorganic. Examples of organic matting agents include silicone, polytetrafluoroethylene, polymethyl methacrylate, polyacrylate, etc., and examples of inorganic matting agents include silica, alumina, talc, mica, etc. Examples of commercially available products include talc such as Microace (registered trademark) series, Nanoace (registered trademark) series, SG-95, and SG-2000 manufactured by Nippon Talc Co., Ltd., and HC-08L and HC-1L manufactured by Hyogo Clay Co., Ltd., silicone resin matting agents such as Tospearl (registered trademark) 120, 130, 145, and 2000B sold by Momentive Performance Materials Japan LLC, and silica matting agents such as Sunsphere (registered trademark) H-31, H-51, and NP-30 sold by AGC Si-Tech Co., Ltd., and among these, silicone resin matting agents are suitable from the viewpoint of head matching with a thermal head. Although these are single particles, the matting agent may be in the form of either a single particle or a particle aggregate in which particles are aggregated.
[0032] The protective layer in the invention may contain known additives such as ultraviolet absorbers, antioxidants, pigments, dyes, surfactants, dispersants, defoamers, thickeners, softeners, antistatic agents, and antiblocking agents in addition to the above-mentioned components.
[0033] The method for forming the protective layer is preferably to prepare a protective layer coating solution containing the above-mentioned water-soluble resin, a crosslinking agent for the water-soluble resin, an acidic compound having a pKa of 4.3 or less, a salt obtained by neutralizing the acidic compound, additives that can be contained in the protective layer, and further a known solvent, and to coat the protective layer coating solution on the above-mentioned thermosensitive recording layer, dry the solution, and, if necessary, harden the solution using heat or radiation such as ultraviolet light or electron beams. The coating amount of the protective layer coating solution is 0.5 to 10 g / m2 in terms of dry mass. 2 is preferable, and 1.0 to 9.0 g / m 2 More preferably, 1.5 to 8.0 g / m 2If the coating amount exceeds the upper limit, the light transmittance decreases and the function as a plate material decreases, whereas if it is below the lower limit, scratches and the like tend to occur during handling.
[0034] In the present invention, the coating method for the above-mentioned heat-sensitive recording layer and protective layer is not particularly limited, and can be selected from various coating methods such as those described in ED Cohen, EB Gutoff, "Modern Coating and Drying Technology", Wiley-VCH, Inc. New York, 1992. Furthermore, it is particularly preferable to coat a plurality of layers simultaneously in terms of improving productivity.
[0035] In addition to the heat-sensitive recording layer and protective layer, the direct heat-sensitive recording material of the present invention may further have, if necessary, an easy-adhesion layer, a heat-insulating layer, etc. between the light-transmitting support and the heat-sensitive recording layer, and a functional layer such as an antistatic layer on the side of the light-transmitting support opposite the heat-sensitive recording layer and the protective layer.
[0036] According to the present invention, an image can be obtained by using the above-mentioned direct thermal recording material, bringing a thermal head into contact with the protective layer of the direct thermal recording material, conveying the direct thermal recording material under the thermal head and heating it according to an image. The direct thermal recording material can be heated to various temperatures up to 400°C by changing the number of heat pulses applied by the thermal head, and the UV transmission density of the image area can be changed by changing the number of heat pulses. EXAMPLES
[0037] The present invention will be described below using examples, but the present invention is not limited to these examples. In the description, "%" is based on mass.
[0038] <Example 1>
[0039] <Preparation of Silver Behenate Dispersion> 20 g of silver behenate crystals and 20 g of Butvar (registered trademark) B-79 (polyvinyl butyral manufactured by Eastman Chemical Japan, Ltd.) were added to 180 g of 2-butanone, and dispersed using a beads mill to obtain a silver behenate dispersion.
[0040] <Preparation and Coating of Thermal Recording Layer Coating Solution> 0.5 g of Butvar B-79, 10 g of the above silver behenate dispersion, 0.3 g of ethyl 3,4-dihydroxybenzoate, 0.1 g of tetrachlorophthalic anhydride, and 0.2 g of phthalazone were added to 10 g of 2-butanone and mixed to prepare a thermal recording layer coating solution. A 100 μm thick polyethylene terephthalate film (total light transmittance 92%, haze value 4%, 500 mm × 400 mm) was prepared as a light-transmitting support, and the thermal recording layer coating solution was applied to one side of the film so that the dry mass was 13.0 g / m 2 The mixture was then dried at 80° C. for 3 minutes to form a heat-sensitive recording layer.
[0041] <Preparation and Application of Protective Layer Coating Solution> 20.8 g of S-LEC (registered trademark) KW-10 (manufactured by Sekisui Chemical Co., Ltd.; polyvinyl butyral resin, solid content 24%) was dissolved in 29.2 g of water and 20.0 g of isopropanol, and 2.6 g of Duranate (registered trademark) WB40-80D (manufactured by Asahi Kasei Corporation; polyisocyanate, solid content 80%), 0.071 g of p-toluenesulfonic acid (pKa-1.34), 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added thereto, and the mixture was stirred at 300 rpm with a three-one motor for 1 hour to obtain a protective layer coating solution. The protective layer coating solution was applied onto the above-mentioned thermal recording layer so that the dry mass was 5.0 g / m. 2 The coating was applied using a wire bar so that the coating became as follows: the coating was dried at 90° C. for 3 minutes to form a protective layer, and then the coating was heated at 40° C. for 24 hours to obtain a direct thermal recording material of Example 1. The mass ratio (B) / (A) of the water-soluble resin (A) to the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.42.
[0042] <Example 2> A direct thermal recording material of Example 2 was obtained in the same manner as in Example 1, except that 0.037 g of lactic acid (pKa 3.84) was added instead of 0.071 g of p-toluenesulfonic acid to obtain a protective layer coating solution.
[0043] <Example 3> A direct thermal recording material of Example 3 was obtained in the same manner as in Example 1, except that 0.026 g of nitric acid (pKa-1.3) was added instead of 0.071 g of p-toluenesulfonic acid to obtain a protective layer coating solution.
[0044] <Example 4> A direct thermal recording material of Example 4 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 (polyvinyl alcohol resin, manufactured by Kuraray Co., Ltd.) was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g of tetramethyl orthosilicate (2.17 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0045] <Example 5> A direct thermal recording material of Example 5 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g of tetramethyl orthosilicate (2.17 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.00120 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0046] <Example 6> A direct thermal recording material of Example 6 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g of tetramethyl orthosilicate (2.17 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0130 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0047] <Example 7> A direct thermal recording material of Example 7 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g of tetramethyl orthosilicate (2.17 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0148 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0048] <Example 8> A direct thermal recording material of Example 8 was obtained in the same manner as in Example 1, except that 5.5 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 4.19 g of tetramethyl orthosilicate (1.65 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.30.
[0049] <Example 9> A direct thermal recording material of Example 9 was obtained in the same manner as in Example 1, except that 3.6 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 9.13 g of tetramethyl orthosilicate (3.60 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. Note that the mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 1.00.
[0050] <Example 10> A direct thermal recording material of Example 10 was obtained in the same manner as in Example 1, except that 3.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 10.6 g of tetramethyl orthosilicate (4.18 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 1.39.
[0051] <Example 11> A direct thermal recording material of Example 11 was obtained in the same manner as in Example 1, except that 2.4 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 12.1 g of tetramethyl orthosilicate (4.77 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 1.99.
[0052] <Comparative Example 1> A direct thermal recording material of Comparative Example 1 was obtained in the same manner as in Example 1, except that 0.025 g of acetic acid (pKa 4.76) was added instead of 0.071 g of p-toluenesulfonic acid to obtain a protective layer coating solution.
[0053] <Comparative Example 2> A direct thermal recording material of Comparative Example 2 was obtained in the same manner as in Example 1, except that 0.063 g of p-nitrophenol (pKa 7.14) was added instead of 0.071 g of p-toluenesulfonic acid to obtain a protective layer coating solution.
[0054] <Comparative Example 3> A direct heat-sensitive recording material of Comparative Example 3 was obtained in the same manner as in Example 1, except that a protective layer coating solution was obtained without adding sodium hydroxide.
[0055] <Comparative Example 4> A direct thermal recording material of Comparative Example 4 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g (2.17 g in terms of solid content), 0.025 g of acetic acid (pKa 4.76), 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0056] <Comparative Example 5> A direct thermal recording material of Comparative Example 5 was obtained in the same manner as in Example 1, except that 5.0 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 5.5 g of tetramethyl orthosilicate (2.17 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, and 0.35 g of Tospearl 145 were added, and the mixture was stirred for 1 hour at 300 rpm with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.43.
[0057] <Comparative Example 6> A direct thermal recording material of Comparative Example 6 was obtained in the same manner as in Example 1, except that 6.5 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 1.65 g of tetramethyl orthosilicate (0.652 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred for 1 hour at 300 rpm with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 0.10.
[0058] <Comparative Example 7> A direct thermal recording material of Comparative Example 7 was obtained in the same manner as in Example 1, except that 1.8 g of Kuraray Poval 3-80 was dissolved in 45 g of water and 20 g of isopropanol, 13.6 g of tetramethyl orthosilicate (5.38 g in terms of solid content), 0.071 g of p-toluenesulfonic acid, 0.0100 g of sodium hydroxide, and 0.35 g of Tospearl 145 were added, and the mixture was stirred at 300 rpm for 1 hour with a three-one motor to obtain a protective layer coating solution. The mass ratio (B) / (A) of the water-soluble resin (A) and the crosslinking agent for the water-soluble resin (B) in the protective layer was 2.99.
[0059] The direct thermal recording materials of Examples 1 to 11 and Comparative Examples 1 to 7 thus obtained were cut to a width of 360 mm, and a solid image with an image size of 350 mm (width) x 450 mm (length) was printed on the cut sheets using a thermal digital printer (TDP-459 manufactured by Mitsubishi Paper Mills, Ltd.: 1200 dpi / 120 lpi, line head) at a printing speed of 1 msec / line.
[0060] <Scratch resistance evaluation> As described above, in the direct thermal recording materials on which the solid image was printed, the scratches that occurred in the image area were evaluated on a three-point scale, and the results are shown in Table 1. Specifically, ◯ indicates that there were almost no scratches, △ indicates that there were scratches but no loss in the image and there is no practical problem as a plate material, and × indicates that there were scratches that caused loss in the image and there is a practical problem as a plate material, and materials rated ◯ and △ were deemed to be direct thermal recording materials in which the occurrence of scratches due to printing was suppressed.
[0061] <Pinhole evaluation> In the direct thermal recording material on which a fill-in image was printed as described above, the number of pinholes generated in the fill-in image (image size 350 mm (width) × 450 mm (length)) was measured using a 50x loupe and rated on a three-level scale, with the results shown in Table 1. Specifically, a pinhole count of 0-10 was rated as ◯, 11-20 as △, and 21 or more as ×, and materials rated as ◯ and △ were deemed to be direct thermal recording materials in which pinhole generation was suppressed.
[0062] [Table 1]
[0063] As is clear from the results in Table 1, it is understood that the present invention makes it possible to obtain a direct thermal recording material in which the occurrence of scratches due to contact with a thermal head is suppressed and further the occurrence of pinholes is suppressed.
Claims
[Claim 1] A direct thermal recording material comprising at least a thermal recording layer on a light-transmitting support, the thermal recording layer containing a non-photosensitive organic silver salt and a reducing agent, and a protective layer containing, from the side closer to the light-transmitting support, (A) a water-soluble resin, (B) a crosslinking agent for the water-soluble resin, (C) an acidic compound having a pKa of 4.3 or less, and (D) a salt obtained by neutralizing the acidic compound, the mass ratio (B) / (A) of the component (A) to the component (B) in the protective layer being 0.2 to 2.5.
Citation Information
Patent Citations
Reversible heat-sensitive recording material
JP1993038881A
Direct thermal imaging materials
JP1996503175A
Direct thermal imaging method using protective heat-sensitive recording material
JP1997504752A
Thermosensitive recording material and thermosensitive recording method
JP2007038633A