Foamable styrene-based resin particle

By integrating a carbon-based radiation heat transfer inhibitor and optimizing the melt flow rate and blowing agent content, the expandable styrenic resin particles achieve high expansion ratios and improved heat resistance in styrenic resin foam molded products, addressing the limitations of existing technologies.

JP2024140138APending Publication Date: 2024-10-10KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051143
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing expandable styrenic resin particles do not incorporate a carbon-based radiation heat transfer inhibitor, leading to reduced heat insulation properties and foaming performance when such inhibitors are added, making it difficult to achieve high expansion ratios in styrenic resin foam molded products.

Method used

Incorporating a styrene resin composition with a carbon-based radiation heat transfer inhibitor, such as graphite, and controlling the melt flow rate and blowing agent content to achieve expandable styrenic resin particles with excellent heat resistance and high expansion ratios, while minimizing the amount of blowing agent to reduce environmental impact and costs.

Benefits of technology

The solution results in styrenic resin foam molded products with high expansion ratios, excellent moldability, and improved heat resistance, along with reduced volatile organic compounds (VOC) emissions and lower production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140138000001
    Figure 2024140138000001
Patent Text Reader

Abstract

To provide a foamable styrene-based resin particle that yields a styrene-based resin foamed molding characterized by superior heat resistance and a high foaming rate.SOLUTION: A foamable styrene-based resin particle according to the present disclosure includes a styrene-based resin composition including a styrene-based resin and a carbon-based radiant heat transfer inhibitor and a foaming agent. The styrene-based resin has a melt flow rate of 7.5-15.5 g / 10 min at 200°C under a 5.0 kg load, and the foaming agent includes isobutane.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to expandable styrene-based resin particles. [Background technology]

[0002] Styrene-based resin foams are well-balanced foams having light weight, heat insulating properties, and cushioning properties, and have been widely used as heat insulating materials for food containers, cooler boxes, cushioning materials, and housing, etc.

[0003] In particular, in recent years, in relation to various problems such as global warming, there has been a trend toward energy saving by improving the thermal insulation of buildings such as houses, and it is expected that the demand for styrene-based resin foamed molded products obtained using expandable styrene-based resin particles will increase. For this reason, various studies have been conducted on the weight reduction and improvement of thermal insulation properties of the styrene-based resin foamed products by increasing the expansion ratio.

[0004] For example, Patent Document 1 discloses expandable styrene-based resin particles used for forming bead foams, which contain a styrene-based resin and a foaming agent, with pentane being contained as the foaming agent, and further contain butane as the foaming agent, the foaming agent being contained in a ratio of 2 parts by mass to 10 parts by mass to 100 parts by mass of the styrene-based resin, the pentane and the butane being contained in a mass ratio of 20:80 to 80:20, and a plurality of bubbles being formed inside so that the expansion ratio is 1.05 times to 1.25 times. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2013-136688 A Summary of the Invention [Problem to be solved by the invention]

[0006] The expandable styrene-based resin particles disclosed in Patent Document 1 were not blended with a carbon-based radiation heat transfer inhibitor. Furthermore, according to the study by the present inventors, it was confirmed that blending a carbon-based radiation heat transfer inhibitor improves heat insulation, but decreases foaming performance, and it was thought that it would be difficult to obtain a foamed molded article with a high expansion ratio if a carbon-based radiation heat transfer inhibitor was applied to expandable styrene-based resin particles that were not blended with a carbon-based radiation heat transfer inhibitor.

[0007] An object of the present inventors is to provide expandable styrene-based resin particles which are excellent in heat resistance and capable of producing styrene-based resin expansion molded articles having a high expansion ratio. [Means for solving the problem]

[0008] An example aspect of this embodiment is described as follows.

[0009] [1] Expandable styrene-based resin particles comprising a styrene-based resin composition containing a styrene-based resin and a carbon-based radiation heat transfer inhibitor, and a blowing agent, The expandable styrene-based resin particles have a melt flow rate of 7.5 to 15.5 g / 10 min at 200° C. under a load of 5.0 kg, and the blowing agent contains isobutane. [2] The apparent density of the expandable styrene-based resin particles is 950 kg / m 3 Super 1200kg / m 3 The expandable styrene-based resin particles according to [1] below. [3] The expandable styrene-based resin particles according to [1] or [2], wherein the styrene-based resin composition contains a flame retardant, and the flame retardant is present in an amount of more than 1.0% by weight and not more than 6.0% by weight in 100% by weight of the styrene-based resin composition. [4] The expandable styrene-based resin particles according to any one of [1] to [3], wherein the carbon-based radiation heat transfer inhibitor is more than 2% by weight and not more than 20% by weight, based on 100% by weight of the styrene-based resin composition. [5] The expandable styrene-based resin particles according to any one of [1] to [4], wherein the carbon-based radiation heat transfer inhibitor is at least one carbon-based radiation heat transfer inhibitor selected from graphite, carbon black, carbon nanotubes, graphene, and activated carbon. [6] The expandable styrene-based resin particles according to any one of [1] to [5], wherein the amount of the blowing agent in the expandable styrene-based resin particles is more than 1.0 part by weight and not more than 8.0 parts by weight per 100 parts by weight of the styrene-based resin composition. [7] The expandable styrene-based resin particles according to any one of [1] to [6], wherein the amount of isobutane is 15 to 90% by weight based on 100% by weight of the blowing agent. [8] The expandable styrene-based resin particles according to any one of [1] to [7], wherein the blowing agent contains a saturated hydrocarbon having 5 to 6 carbon atoms. [9] The expandable styrene-based resin particles according to any one of [1] to [8], wherein the foaming agent contains pentane.

[10] Pre-expanded styrene-based resin particles obtained by expanding the expandable styrene-based resin particles according to any one of [1] to [9].

[11] A foamed molded product of a styrene-based resin obtained by molding the pre-expanded particles of the styrene-based resin according to

[10] . Effect of the Invention

[0010] The expandable styrene-based resin particles of the present disclosure are excellent in heat resistance and can provide styrene-based resin foamed molded articles with a high expansion ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0011] The present invention will be described in detail below. The expandable styrene-based resin particles according to this embodiment are expandable styrene-based resin particles containing a styrene-based resin composition containing a styrene-based resin and a carbon-based radiation heat transfer inhibitor, and a foaming agent, and the styrene-based resin has a melt flow rate of 7.5 to 15.5 g / 10 min at 200° C. and a load of 5.0 kg, and the foaming agent contains isobutane. The expandable styrene-based resin particles of the present disclosure control the melt flow rate (MFR) of the styrene-based resin within the above-mentioned range, and contain isobutane as a foaming agent, thereby making it possible to obtain a styrene-based resin foamed molded product having excellent heat resistance and a high expansion ratio. In addition, the obtained styrene-based resin foamed molded product has excellent moldability. In one aspect of the expandable styrene-based resin particles according to this embodiment, a styrene-based resin foamed molded product having a high expansion ratio can be obtained even when the amount of foaming agent is relatively less than that of the conventional one. Reducing the amount of foaming agent brings about an effect of reducing environmental load such as reducing VOCs (volatile organic compounds) and an effect of reducing costs.

[0012] (styrene resin) The styrene-based resin may be a styrene homopolymer or a styrene copolymer. As the styrene copolymer, a styrene copolymer obtained by copolymerizing styrene with another monomer copolymerizable with styrene or a derivative thereof can be used. The repeating unit derived from styrene contained in the styrene-based copolymer is preferably 60% by weight or more, more preferably 80% by weight or more, based on 100% by weight of the styrene-based copolymer. As the styrene-based resin, one type may be used alone, or two or more types may be used. However, in the present embodiment, the styrene-based resin usually excludes a brominated styrene-butadiene copolymer described later.

[0013] Examples of other monomers copolymerizable with styrene or derivatives thereof (hereinafter, sometimes referred to as "other monomers or derivatives thereof") include styrene derivatives such as methylstyrene, dimethylstyrene, ethylstyrene, diethylstyrene, isopropylstyrene, bromostyrene, dibromostyrene, tribromostyrene, chlorostyrene, dichlorostyrene, and trichlorostyrene; polyfunctional vinyl compounds such as divinylbenzene; methyl acrylate, methyl methacrylate, ethyl acrylate, ethyl methacrylate, and butyl acrylate. and (meth)acrylic acid ester compounds such as butyl methacrylate; vinyl cyanide compounds such as (meth)acrylonitrile; diene compounds or derivatives thereof such as butadiene; unsaturated carboxylic acid anhydrides such as maleic anhydride and itaconic anhydride; N-alkyl-substituted maleimide compounds such as N-methylmaleimide, N-butylmaleimide, N-cyclohexylmaleimide, N-phenylmaleimide, N-(2-chlorophenyl)maleimide, N-(4-bromophenyl)maleimide, and N-(1-naphthyl)maleimide. The other monomers or derivatives thereof may be used alone or in combination of two or more.

[0014] The styrene-based resin may be blended with a homopolymer or a copolymer of another monomer or a derivative thereof, as long as the effect of the present invention is not impaired.

[0015] From the viewpoint of impact absorption and heat resistance, the styrene resin may be blended with, for example, diene rubber reinforced polystyrene, acrylic rubber reinforced polystyrene, and / or polyphenylene ether resin.

[0016] The styrene-based resin preferably contains at least one selected from a styrene homopolymer, a styrene-acrylonitrile copolymer, and a styrene-butyl acrylate copolymer, and more preferably contains a styrene homopolymer, because the styrene-based resin is relatively inexpensive, can be foam-molded with low-pressure steam or the like without using a special method, and has an excellent balance of heat insulation, flame retardancy, and cushioning properties.

[0017] The styrene resin has a melt flow rate of 7.5 to 15.5 g / 10 min at 200° C. and a load of 5.0 kg, preferably 8.0 to 15.0 g / 10 min, and more preferably 8.5 to 14.5 g / 10 min. The melt flow rate is also referred to as MFR. When the melt flow rate is within the above range, it is possible to obtain expandable resin particles having excellent moldability, and it is possible to obtain a styrene resin foamed molded product having excellent heat resistance and a high expansion ratio. In the present disclosure, when the styrene resin is two or more kinds of resins (polymers), the MFR of the styrene resin does not mean the MFR of each resin, but the MFR of the entire styrene resin. That is, when two or more kinds of resins are used, the resins contained in the styrene resin composition are melt-kneaded in the ratio contained in the styrene resin composition to prepare pellets, and the MFR of the pellets is measured to know the MFR of the styrene resin contained in the styrene resin composition. The MFR in the present invention is a value measured in accordance with JIS K7210. The MFR can be measured by the method described in the Examples below.

[0018] As the styrene-based resin, it is one of the preferred embodiments to use two kinds of styrene-based resins. In one embodiment, two kinds of styrene-based resins are used as the styrene-based resin, and the MFR of at least one of the styrene-based resins is outside the range of 7.5 to 15.5 g / 10 min. In one preferred embodiment, two kinds of styrene-based resins are used as the styrene-based resin, and the MFR of one of the styrene-based resins is less than 7.5 g / 10 min, and the MFR of the other styrene-based resin is more than 15.5 g / 10 min. When two kinds of styrene-based resins are used as the styrene-based resin, it is preferable that one styrene-based resin and the other styrene-based resin are contained in a ratio of 99:1 to 1:99 (weight ratio).

[0019] In a preferred embodiment, the styrene resin is a styrene resin having an MFR of less than 7.5 g / 10 min, preferably 1.0 to 7.4 g / 10 min, more preferably 2.0 to 7.3 g / 10 min, even more preferably 3.0 to 7.2 g / 10 min, particularly preferably 5.5 to 7.1 g / 10 min, and a styrene resin having an MFR of more than 15.5 g / 10 min, preferably 15.6 to 25 g / 10 min, more preferably 16 to 22 g / 10 min. In this case, the ratio of the styrene resin having an MFR of less than 7.5 g / 10 min to the styrene resin having an MFR of more than 15.5 g / 10 min is preferably 20:80 to 90:10 (weight ratio). By using two types of styrene resins, it is easy to adjust the MFR, and it is possible to easily obtain expandable resin particles having excellent moldability.

[0020] In the present invention, the content of the styrene-based resin is not particularly limited, but is preferably 75 to 99.9% by weight, and more preferably 80 to 95% by weight, based on 100% by weight of the styrene-based resin composition.

[0021] In addition, as long as the effect of the present invention is not impaired, other resins may be used in combination with the styrene-based resin as the main component. Examples of the other resins include homopolymers of the above-mentioned other monomers or their derivatives, copolymers thereof, polyolefin-based resins, polyester-based resins, polycarbonate-based resins, acrylic-based resins, etc. The content of the other resins is not particularly limited, but is preferably 20% by weight or less, more preferably 10% by weight or less, based on 100% by weight of the styrene-based resin composition.

[0022] (Carbon-based radiation heat transfer inhibitor) The expandable styrene resin particles are obtained by forming a styrene resin foamed molded article having high thermal insulation properties because the styrene resin composition contains a carbon-based radiation heat transfer inhibitor. Here, the carbon-based radiation heat transfer inhibitor refers to a carbon material having the property of reflecting, scattering, or absorbing light in the near infrared or infrared region (for example, a wavelength region of about 800 to 3000 nm). Examples of the carbon-based radiation heat transfer inhibitor include graphite, graphene, carbon black, expanded graphite, activated carbon, carbon nanotubes, and carbon nanofibers. The carbon-based radiation heat transfer inhibitor can be used alone or in combination of two or more. The carbon-based radiation heat transfer inhibitor is preferably at least one carbon-based radiation heat transfer inhibitor selected from graphite, carbon black, carbon nanotubes, graphene, and activated carbon, from the viewpoints of dispersibility in the styrene resin and cost, and more preferably graphite.

[0023] Examples of graphite include flake graphite, earthen graphite, spherical graphite, and artificial graphite. In this specification, the term "flake" also includes scaly, thin, or plate-like graphite. The graphite may be used alone or in combination of two or more. Among these, flake graphite or a graphite mixture mainly composed of flake graphite is preferred, and flake graphite is more preferred, in terms of its high radiation heat transfer suppression effect.

[0024] The average particle size of the carbon-based radiation heat transfer inhibitor is preferably 1 to 9 μm, more preferably 1.5 to 8 μm, and even more preferably 2 to 7 μm. The smaller the average particle size of the carbon-based radiation heat transfer inhibitor, the higher the production cost. Carbon-based radiation heat transfer inhibitors with an average particle size of less than 1 μm are very expensive due to high production costs including the cost of pulverization, and the cost of the expandable styrene resin particles tends to be high. On the other hand, when the average particle size exceeds 9 μm, the cell membrane is easily broken when producing pre-expanded particles and styrene resin foam molded bodies from the expandable styrene resin particles, so that it becomes difficult to achieve a high expansion ratio, the ease of molding decreases, and the compressive strength of the styrene resin foam molded body tends to decrease. In the present disclosure, the average particle size of the carbon-based radiation heat transfer inhibitor means the particle size (D50) (volume average particle size by laser diffraction scattering method) when the particle size distribution is measured and analyzed by a laser diffraction scattering method based on the Mie theory in accordance with JIS Z8825-1 and the cumulative volume of the total particle volume becomes 50%.

[0025] Furthermore, if the carbon-based radiation heat transfer inhibitor has an average particle size of 6.0 μm or less, the molded article can have excellent surface appearance and a lower thermal conductivity, that is, a higher thermal insulation property.

[0026] The content of the carbon-based radiation heat transfer inhibitor is not particularly limited, but is preferably more than 2% by weight and not more than 20% by weight, more preferably 3 to 18% by weight, even more preferably 4 to 16% by weight, and particularly preferably 4.5 to 14% by weight, based on 100% by weight of the styrene-based resin composition. Within the above range, it is easy to control the expansion ratio to the desired level, and there is a tendency for the balance of the thermal conductivity reduction effect and the like to be excellent, which is preferable.

[0027] In addition to the carbon-based radiation heat transfer inhibitor, other radiation heat transfer inhibitors may be used as long as the effects of the present invention are not impaired. The other radiation heat transfer inhibitors are not particularly limited as long as they are radiation heat transfer inhibitors other than carbon-based, and examples thereof include aluminum-based compounds, zinc-based compounds, magnesium-based compounds, titanium-based compounds, heat ray reflectors, metal sulfates, antimony-based compounds, metal oxides, heat ray absorbers, metal particles, etc.

[0028] (foaming agent) The expandable styrene-based resin particles of the present disclosure contain a foaming agent. The foaming agent also contains isobutane. By using the specific styrene-based resin described above and containing isobutane as at least a part of the foaming agent, it is possible to obtain a styrene-based resin foamed molded product having excellent heat resistance and a high expansion ratio.

[0029] The blowing agent may contain a blowing agent other than isobutane. The blowing agent other than isobutane is not particularly limited, but from the viewpoint of a good balance between expandability and product life and easy to increase the expansion ratio when actually used, a hydrocarbon having 3 to 6 carbon atoms (excluding isobutane) is preferable, a hydrocarbon having 4 to 6 carbon atoms (excluding isobutane) is more preferable, and a hydrocarbon having 5 to 6 carbon atoms is even more preferable. When the blowing agent has 3 or more carbon atoms, the volatility is low and the blowing agent is less likely to dissipate when made into expandable styrene-based resin particles, so that the blowing agent remains sufficiently in the expansion process when actually used, and it is possible to obtain sufficient expansion power, and it is easy to increase the expansion ratio, which is preferable. In addition, when the carbon number is 6 or less, the boiling point of the blowing agent is not too high, so that it is easy to obtain sufficient expansion power by heating during pre-expansion, and there is a tendency that it is easy to increase the expansion ratio. In addition, it is preferable that the hydrocarbon is a saturated hydrocarbon from the viewpoint of expansion power. The blowing agent is preferably a saturated hydrocarbon having 3 to 6 carbon atoms (excluding isobutane), more preferably a saturated hydrocarbon having 4 to 6 carbon atoms (excluding isobutane), and even more preferably a saturated hydrocarbon having 5 to 6 carbon atoms. Examples of the hydrocarbon having 3 to 6 carbon atoms (excluding isobutane) include hydrocarbons such as propane, normal butane, normal pentane, isopentane, neopentane, cyclopentane, normal hexane, and cyclohexane. These may be used alone or in combination of two or more. In addition, from the perspective of the balance between the ease of increasing the magnification and the product life, it is preferable to use isobutane and a blowing agent other than isobutane as the blowing agent. It is preferable that the blowing agent contains pentane. It is also preferable that the blowing agent contains isobutane and at least one blowing agent selected from the group consisting of normal butane, isopentane, and normal pentane. It is particularly preferable that the blowing agent contains isobutane and at least one blowing agent selected from the group consisting of normal pentane and isopentane, and it is even more preferable that the blowing agent contains isobutane, normal pentane, and isopentane.

[0030] The amount of isobutane in the blowing agent is usually 15 to 90% by weight, preferably 20 to 80% by weight, more preferably 25 to 70% by weight, based on 100% by weight of the blowing agent. In a preferred embodiment, isobutane, normal pentane, and isopentane are used as the blowing agent, and in this embodiment, the weight ratio (isobutane / pentane) of isobutane to pentane (normal pentane and isopentane) is usually 20 / 80 to 90 / 10, preferably 40 / 60 to 70 / 30, more preferably 50 / 50 to 60 / 40. In addition, the weight ratio (normal pentane / isopentane) of normal pentane to isopentane is, for example, 30 / 70 to 90 / 10, preferably 50 / 50 to 85 / 15. Within the above range, the expandable styrene-based resin particles tend to have excellent high expandability.

[0031] The amount of the foaming agent added is preferably more than 1.0 part by weight and not more than 8.0 parts by weight, more preferably 2.0 to 7.0 parts by weight, even more preferably 3.0 to 6.0 parts by weight, and particularly preferably 3.5 to 5.5 parts by weight, based on 100 parts by weight of the styrene-based resin composition. The expandable styrene-based resin particles of the present disclosure control the MFR of the styrene-based resin within the above-mentioned range and contain isobutane as a foaming agent, so that a styrene-based resin foam molded article with a high expansion ratio can be obtained even with a relatively small amount of foaming agent compared to the conventional method. Therefore, it has an effect of reducing environmental load such as VOC reduction, and an effect of reducing costs. In addition, the obtained styrene-based resin foam molded article is excellent in heat resistance in addition to excellent moldability.

[0032] (Flame retardant) The flame retardant is not particularly limited, and any flame retardant conventionally used in styrene resin foam moldings can be used. Among them, bromine-based flame retardants, which have a high flame retardancy-imparting effect, are preferred.

[0033] Examples of the brominated flame retardant include brominated bisphenol compounds such as 2,2-bis[4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl]propane (also known as tetrabromobisphenol A-bis(2,3-dibromo-2-methylpropyl ether)) or 2,2-bis[4-(2,3-dibromopropoxy)-3,5-dibromophenyl]propane (also known as tetrabromobisphenol A-bis(2,3-dibromopropyl ether)), and brominated styrene-butadiene copolymers such as brominated styrene-butadiene block copolymers, brominated random styrene-butadiene copolymers, and brominated styrene-butadiene graft copolymers. Examples of the brominated flame retardant include the heat-stable brominated copolymers disclosed in JP-T-2009-516019. The bromine-based flame retardants may be used alone or in combination of two or more.

[0034] The flame retardant is preferably more than 1.0% by weight and not more than 6.0% by weight, more preferably 1 to 4% by weight, based on 100% by weight of the styrene-based resin composition, from the viewpoint of easy control of the expansion ratio to the desired value and of the balance of flame retardancy when carbon is added. If the content is more than 1% by weight, the effect of imparting flame retardancy is not reduced, and if it is 6.0% by weight or less, the strength of the obtained styrene-based resin expansion molded article is not likely to decrease.

[0035] (Heat stabilizer) The expandable styrene resin particles may further contain a heat stabilizer. The heat stabilizer is preferably contained in the styrene resin composition. By using the heat stabilizer, it is possible to suppress deterioration of the flame retardancy and deterioration of the expandable styrene resin particles due to decomposition of the flame retardant during the production process.

[0036] The heat stabilizers can be used in appropriate combination depending on the type of styrene-based resin used, the type and content of the carbon-based radiation heat transfer inhibitor, the type and content of the flame retardant, the type and content of the foaming agent, etc.

[0037] The heat stabilizer used in the present invention is preferably a hindered amine compound, a phosphorus-based compound, or an epoxy compound, because it can arbitrarily control the 1% weight loss temperature in thermogravimetric analysis of the styrene-based resin composition. The heat stabilizer can be used alone or in combination of two or more. An example of the hindered amine compound is tetrakis(2,2,6,6-tetramethylpiperidyloxycarbonyl)butane, and an example of the phosphorus-based compound is bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite.

[0038] The heat stabilizer is preferably 0.05 to 3 wt%, more preferably 0.1 to 2.8 wt%, and even more preferably 0.11 to 2.5 wt% in 100 wt% of the styrene-based resin composition, from the viewpoint of easy control of the expansion ratio to the desired value and of the balance of flame retardancy when a carbon-based radiation heat transfer inhibitor is added. If it is 0.05 wt% or more, the flame retardant is unlikely to decompose and the flame retardancy imparting effect is not reduced, and if it is 3 wt% or less, the strength of the obtained styrene-based resin expansion molded article is unlikely to decrease.

[0039] (Other additives) The expandable styrene-based resin particles and the styrene-based resin composition may contain, as necessary, other additives, for example, one or more other additives selected from the group consisting of radical generators, processing aids, light resistance stabilizers, nucleating agents, foaming aids, antistatic agents, and colorants such as pigments, within the scope of not impairing the effects of the present invention.

[0040] Examples of the radical generator include cumene hydroperoxide, dicumyl peroxide, t-butyl hydroperoxide, 2,3-dimethyl-2,3-diphenylbutane, and poly-1,4-isopropylbenzene.

[0041] Examples of the processing aid include sodium stearate, magnesium stearate, calcium stearate, zinc stearate, barium stearate, and liquid paraffin.

[0042] Examples of the light resistance stabilizer include phenol-based antioxidants, nitrogen-based stabilizers, sulfur-based stabilizers, benzotriazoles, etc. Note that the light resistance stabilizer may also act as a heat stabilizer, such as a hindered amine compound, a phosphorus-based compound, a phenol-based stabilizer, or an epoxy compound, but in the present disclosure, those that belong to both light resistance stabilizers and heat stabilizers are considered to be heat stabilizers.

[0043] Examples of the nucleating agent include inorganic compounds such as silica, calcium silicate, wollastonite, kaolin, clay, mica, zinc oxide, calcium carbonate, sodium hydrogen carbonate, and talc; polymer compounds such as methyl methacrylate copolymers and ethylene-vinyl acetate copolymer resins; olefin waxes such as polyethylene wax; and fatty acid bisamides such as methylene bisstearamide, ethylene bisstearamide, hexamethylene bispalmitic amide, and ethylene bisoleic amide.

[0044] As the foaming assistant, a solvent having a boiling point of 200° C. or less under atmospheric pressure can be desirably used. Examples of the foaming assistant include aromatic hydrocarbons such as styrene, toluene, ethylbenzene, and xylene, alicyclic hydrocarbons such as cyclohexane and methylcyclohexane, and acetates such as ethyl acetate and butyl acetate.

[0045] As the antistatic agent and colorant, those used in various resin compositions can be used without any particular limitation.

[0046] These other additives may be used alone or in combination of two or more.

[0047] The expandable styrene-based resin particles of the present invention have an apparent density of 950 kg / m 3 Super 1200kg / m 3 From the viewpoint of foaming property, it is preferable that the viscosity is 950 kg / m or less. 3 More preferably, it is greater than 1000 kg / m 3On the other hand, from the viewpoint of thermal insulation performance, it is more preferable that the thickness is 1170 kg / m 3 It is preferable that the sintering temperature is 1150 kg / m or less. 3 More preferably, it is equal to or less than 1140 kg / m 3 The following is particularly preferred. When the apparent density of the expandable styrene-based resin particles is within the above range, it is considered that the styrene-based resin melt containing the styrene-based resin composition and the foaming agent is suppressed from expanding during extrusion. By obtaining expandable styrene-based resin particles in which expansion during extrusion is suppressed, the closed cell ratio in the pre-expanded particles is increased, and the strength of the cell structure is increased, which is preferable because it is possible to suppress shrinkage immediately after pre-expansion.

[0048] In addition, if the apparent density of the expandable styrene resin particles is low, the pre-expanded particles are easily shrunk, and if the shrinkage immediately after pre-expansion is large, the cells of the pre-expanded particles are buckled, and the expansion ratio cannot be restored even if cured at high temperature, but the expandable styrene resin particles of the present invention are suppressed in shrinkage, so there is no need to cure the pre-expanded particles at high temperature, and the expansion ratio control after curing is easy. Furthermore, by increasing the apparent density of the expandable styrene resin particles, the bulk density of the expandable styrene resin particles is not reduced, making them easier to pack, and therefore the space required for storage can be reduced.

[0049] In the expandable styrene resin particles of the present invention, the bulk ratio of the pre-expanded particles obtained by pre-expanding the expandable styrene resin particles is preferably 70 times or more, more preferably 80 times or more. When the bulk ratio of the pre-expanded particles is 70 times or more, the density of the styrene resin foam molded body obtained by molding the pre-expanded particles is reduced, making it possible to produce a more lightweight styrene resin foam molded body. In addition, increasing the bulk ratio allows the amount of resin used to be reduced, which leads to cost reduction.

[0050] (Method of producing expandable styrene-based resin particles) The expandable styrene-based resin particles can be obtained by a known melt-kneading method. Specifically, the particles can be produced by melt-kneading a styrene-based resin, a carbon-based radiation heat transfer inhibitor, and a foaming agent in an extruder (melt-kneading process), extruding the molten mixture through a die having small holes attached to the tip of the extruder into a chamber filled with pressurized circulating water (extrusion process), cutting the molten mixture immediately after extrusion with a rotating cutter, and cooling and solidifying it with pressurized circulating water (cooling process).

[0051] The manufacturing method of expandable styrene resin particles includes, for example, a manufacturing method of expandable styrene resin particles, which comprises preparing a styrene resin composition containing a styrene resin and a carbon-based radiation heat transfer inhibitor by melt kneading, adding a blowing agent to the molten styrene resin composition, further kneading, extruding the melt containing the styrene resin composition and the blowing agent from a die having a plurality of small holes into pressurized circulating water, and cutting it with a rotary cutter to form particles. The type and amount of the styrene resin, the type and amount of the carbon-based radiation heat transfer inhibitor, the type and amount of the blowing agent, and other additives can be appropriately set based on the above description.

[0052] In the above-mentioned production method, from the viewpoint of dispersibility between the styrene-based resin and various components, a preferred embodiment is to previously use a kneading device equipped with a twin-screw agitator (e.g., a Banbury mixer) to knead a part of the styrene-based resin with various components under load to prepare a kneaded product such as a master batch, and then to feed the resulting kneaded product together with new styrene-based resin and other components into an extruder to melt-knead and subsequently cut into particles.

[0053] In one preferred embodiment of the above-mentioned production method, a styrene-based resin and a carbon-based radiation heat transfer inhibitor are kneaded with a kneading device equipped with a two-shaft agitator such as a Banbury mixer to prepare a master batch, the prepared master batch, new styrene-based resin, and other components such as a flame retardant as necessary are melt-kneaded in an extruder, a foaming agent is then added, and the resulting resin melt is extruded through a die having small holes attached to the tip of the extruder into a cutter chamber filled with pressurized circulating water, and immediately after extrusion, the resin is cut with a rotating cutter and cooled and solidified with the pressurized circulating water.

[0054] In another preferred embodiment of the above-mentioned manufacturing method, a styrene-based resin and a carbon-based radiation heat transfer inhibitor are kneaded with a kneading device equipped with a twin-shaft agitator such as a Banbury mixer to prepare a master batch, and a styrene-based resin, a flame retardant, and a heat stabilizer are further kneaded with a kneading device equipped with a twin-shaft agitator such as a Banbury mixer to prepare another master batch. The two master batches prepared, a new styrene-based resin, and other components as necessary are melt-kneaded in an extruder, a foaming agent is then added, and the resulting resin melt is extruded through a die having small holes attached to the tip of the extruder into a cutter chamber filled with pressurized circulating water, and immediately after extrusion, the resin is cut with a rotary cutter and cooled and solidified with the pressurized circulating water.

[0055] In the above-mentioned production method, the melt kneading in the extruder may be performed using a single extruder, a plurality of extruders connected together, or an extruder in combination with a second kneading device such as a static mixer or a stirrer without a screw, and may be appropriately selected.

[0056] When two or more kinds of blowing agents are used in combination, the method of addition is not particularly limited as long as each blowing agent is added, and the agents may be added simultaneously or in two or more portions.

[0057] (Pre-expanded particles and styrene-based resin foamed molded products) A styrene-based resin foamed molded article can be obtained by using the expandable styrene-based resin particles. In order to obtain a styrene-based resin foamed molded article, the expandable styrene-based resin particles may be pre-expanded and then foamed in a mold. The pre-expanded particles are also referred to as pre-expanded particles. That is, the present disclosure includes pre-expanded particles of a styrene-based resin obtained by expanding the expandable styrene-based resin particles described above, and a foamed molded article of a styrene-based resin obtained by molding the pre-expanded particles of a styrene-based resin.

[0058] The expandable styrene resin particles can be used for molding after being expanded 10 to 110 times by a conventionally known pre-expanding process, for example, by heated steam to obtain pre-expanded particles, and then cured for a certain period of time as necessary. The expansion ratio is preferably 50 times or more, more preferably 70 times or more. The obtained pre-expanded particles are molded (for example, molded in a mold) by steam using a conventionally known molding machine to produce a styrene resin foamed molded article. Depending on the shape of the mold used, a molded article with a complex shape or a block-shaped molded article can be obtained.

[0059] The expandable styrene resin particles can be molded into a styrene resin foamed molded article having a high expansion ratio. The expansion ratio of the foamed molded article is preferably 40 times or more, more preferably 60 times or more, even more preferably 70 times or more, and particularly preferably 80 times or more. The expandable styrene resin particles can achieve high expansion of the foamed molded article even when the amount of foaming agent is less than that of the conventional method.

[0060] For heat insulating materials, since they are used for a long period of time, maintaining the heat insulating performance after a long period of time is an important issue. For the styrene resin foam molded product molded with the styrene resin composition and expandable styrene resin particles according to the present invention, a sample for measuring thermal conductivity is cut out from the styrene resin foam molded product, and the sample is annealed at 70°C for 35 days, and even after being left to stand for 24 hours under 23°C, a low thermal conductivity can be achieved. By annealing at 70°C for 35 days, the content of the hydrocarbon foaming agent such as butane or pentane contained in the styrene resin foam molded product is 1.0% or less, and the effect of the foaming agent on the thermal conductivity is negligible, and the thermal conductivity can be evaluated as the thermal conductivity when the styrene resin foam molded product is used for a long period of time at room temperature.

[0061] When the expandable styrene-based resin particles are used to produce an expanded molded product with an expansion ratio of 80 times, the 80-fold expanded molded product is left at 70°C for 35 days and then left at 23°C for 24 hours. The thermal conductivity at 23°C measured according to JIS A9511:2006R is preferably 0.034 W / mK or less. That is, if the thermal conductivity is 0.034 W / mK or less, it can be said that a very low thermal conductivity and therefore high thermal insulation can be maintained for a long period of time. More preferably, the thermal conductivity is 0.033 W / mK or less, and even more preferably, the thermal conductivity is 0.032 W / mK or less.

[0062] In this specification, the expansion ratio is expressed as "times" or "cm 3 / g", but these have the same meaning.

[0063] The pre-expanded particles and the styrene-based resin foamed molded article thereof preferably have an average cell diameter of 70 to 300 μm, more preferably 90 to 250 μm, and even more preferably 100 to 200 μm. By having the average cell diameter within the above range, the styrene-based resin foamed molded article has higher heat insulating properties. When the average cell diameter is 70 μm or more, there is a tendency that the expansion ratio can be easily increased, and when the average cell diameter is 300 μm or less, an increase in thermal conductivity, i.e., a deterioration in heat insulating performance, can be avoided.

[0064] (Applications of foamed molded products) The foamed molded article made by using the expandable styrene-based resin particles has excellent surface beauty, a high expansion ratio, a high closed cell ratio, low thermal conductivity, a significant suppression of the increase in thermal conductivity over time, and high long-term heat insulation, and is therefore suitable for various applications such as building insulation materials, food container boxes, cold storage boxes, cushioning materials, agricultural and fishery boxes, bathroom insulation materials, and hot water tank insulation materials.

[0065] In addition, the production conditions of the expandable styrene-based resin particles of the present disclosure and the method for measuring the physical properties of the obtained product can be carried out by appropriately referring to JP 2019-65073 A in addition to the disclosure in this specification. EXAMPLES

[0066] The present embodiment will be described below with reference to examples, but the present disclosure is not limited to these examples.

[0067] The methods for measuring and evaluating the various physical properties in the following Examples and Comparative Examples are as follows.

[0068] (Method of measuring the melt flow rate (MFR) of styrene resin) The melt flow rate of the styrene resin was measured in accordance with the method described in JIS K7210 "Determination of melt mass flow rate (MFR) and melt volume flow rate (MVR) of plastics-thermoplastics" Method B. More specifically, the melt flow rate of the styrene resin (styrene resin pellets) was measured using a "semi-automatic melt flow index tester" manufactured by Yasuda Seiki Seisakusho under the measurement conditions of a test temperature of 200°C and a load of 5.0 kg.

[0069] (Method for measuring apparent density of expandable styrene resin particles) A measurement sample of W (kg) of expandable styrene resin particles was taken, and this measurement sample was allowed to fall naturally into a measuring cylinder containing ethanol, and its mass (kg) and volume (m 3 ) was measured, and the apparent density was calculated based on the following formula: Apparent density (kg / m 3 ) = weight of sample (W) / volume of sample (V)

[0070] (Method for measuring bulk magnification of pre-expanded particles) A sample of pre-expanded particles was taken in an amount of W (g) as a measurement sample, and this measurement sample was allowed to fall naturally into a measuring cylinder. The measuring cylinder was then struck to determine the apparent volume V (cm 3 ) is constant, and its mass (g) and volume (cm 3 ) was measured, and the bulk magnification was calculated based on the following formula. Bulk magnification (cm 3 / g) = volume of measurement sample (V) / weight of measurement sample (W)

[0071] (Expansion ratio of styrene-based resin foam molding) The styrene-based resin foam molded product was removed from the mold and dried at 30°C for 24 hours, after which the weight (g) of the foam molded product was measured, and the length, width, and thickness were measured using a caliper. The volume (cm3) of the styrene-based resin foam molded product was calculated from each measured dimension. 3 ) was calculated, and the expansion ratio was calculated according to the following formula. Expansion ratio (cm 3 / g) = test piece volume (cm 3 ) / test piece weight (g) The expansion ratio of styrene-based resin foamed moldings is conventionally expressed as "cm 3 It is also expressed as " / g".

[0072] (Method for measuring thermal conductivity of styrene-based resin foam molded products) It is generally known that the higher the average temperature at which thermal conductivity is measured, the higher the thermal conductivity value, and it is necessary to determine the average temperature at which it is measured in order to compare thermal insulation. In this specification, the standard temperature of 23°C, as specified in JIS A9511:2006R, which is the standard for foamed plastic insulation materials, was adopted. The thermal conductivity was measured after leaving the styrene resin foam molded body at 70°C for 35 days, cutting out a sample for measuring thermal conductivity, and leaving it at 23°C for another 24 hours.

[0073] More specifically, the styrene-based resin foam molded product was left to stand at 70°C for 35 days, and then a sample of 300 mm length x 300 mm width x 25 mm was cut out. The sample was then left to stand at 23°C for 24 hours, and the thermal conductivity was measured at an average temperature of 23°C and a temperature difference of 20°C by the heat flow meter method using a thermal conductivity measuring device (HC-074, manufactured by Eiko Seiki Co., Ltd.) in accordance with JIS A1412-2:1999.

[0074] (Surface property evaluation of styrene-based resin foam molded products) The surface properties of the obtained styrene-based resin foam molded articles were visually observed in a field of 300 mm×300 mm and evaluated according to the following criteria. AA: The number of foam particles with depressions on the surface of the molded article is 100 or less. BB: More than 100 foam particles have depressions on the surface of the molded article.

[0075] (Evaluation of dimensional change rate of styrene-based resin foam molded bodies at high temperatures) The dimensional change rate at high temperature in this specification is a value measured in accordance with the B method of dimensional stability at high temperature defined in JIS K6767. More specifically, a sample of 150 mm length x 150 mm width x 25 mm length was cut out, and the sample was left at 23°C for 24 hours, and then three straight lines were drawn on the sample in parallel in the vertical and horizontal directions at 50 mm intervals. The lengths of the three lines in the vertical and horizontal directions were measured, and the average value was taken as the initial dimension (L1). The sample was heated at 80°C for 22 hours, removed, and left at 23°C for 1 hour, and then the lengths of the three lines in the vertical and horizontal directions were measured, and the average value was taken as the dimension after heating (L2). The dimensional change rate was calculated according to the following formula. Dimensional change rate (%) = (L2 (mm) - L1 (mm)) / (L1 (mm)) x 100

[0076] (Evaluation of heat resistance of styrene-based resin foam molded bodies) From the above-mentioned evaluation of the dimensional change rate at high temperatures, the heat resistance performance of the styrene-based resin foam molded article was evaluated based on the following criteria. AA: Dimensional change rate is greater than -3.0% and less than +3.0% BB: Dimensional change rate is -3.0% or less or +3.0% or more

[0077] The raw materials used in the examples and comparative examples are shown below.

[0078] (styrene resin) (A1) Styrene homopolymer [PS Japan Co., Ltd., 680] (MFR: 7.0 g / 10 min) (A2) Styrene homopolymer [PS Japan Co., Ltd., 679] (MFR: 18.0 g / 10 min) (Carbon-based radiation heat transfer inhibitor) (B) Graphite [Flake graphite SGP-40B, manufactured by Marutoyo Foundry Co., Ltd.]

[0079] (Brominated flame retardants) (C) 2,2-bis[4-(2,3-dibromo-2-methylpropoxy)-3,5-dibromophenyl]propane [manufactured by Daiichi Kogyo Seiyaku Co., Ltd., SR-130, bromine content = 66% by weight] (Heat stabilizer) (D1) Tetrakis(2,2,6,6-tetramethylpiperidyloxycarbonyl)butane [ADEKA Corporation LA-57] (D2) Bis(2,6-di-t-butyl-4-methylphenyl)pentaerythritol diphosphite [ADEKA Corporation, PEP-36]

[0080] (foaming agent) (E1) Normal pentane [Fujifilm Wako Pure Chemical Industries, Ltd., reagent product] (E2) Isopentane [Fujifilm Wako Pure Chemical Industries, Ltd., reagent product] (E3) Isobutane [Mitsui Chemicals, Inc.] (Other additives) (F) Ethylene bis stearic acid amide [NOF Corporation, Alflow H-50S]

[0081] (Production Example 1) (Graphite Masterbatch (G)) The raw materials were fed into a Banbury mixer so that the total weight (A1+B+F) of 49% by weight of styrene resin (A1), 50% by weight of graphite (B), and 1% by weight of ethylene bisstearic acid amide (F) was 100% by weight, and the mixture was mixed at 5 kgf / cm 2 The mixture was kneaded for 20 minutes without heating or cooling under a load of 1000 g for 20 minutes. The resin temperature was measured and found to be 180°C. The strand-shaped resin was fed to a ruder and extruded at 250 kg / hr through a die with small holes attached to the tip. It was cooled and solidified in a water bath at 30°C, and then cut to obtain master batch (G). The graphite content in master batch (G) was 50% by weight.

[0082] (Production Example 2) (Masterbatch (H) of a mixture of brominated flame retardant and heat stabilizer) A styrene-based resin (A1) was fed into a twin-screw extruder and melt-kneaded, and then a mixture of a brominated flame retardant (C), a heat stabilizer (D1) and (D2) was fed into the extruder midway and further melt-kneaded. The weight ratio of each material was (A1):(C):(D1):(D2)=70:28.5:0.6:0.9, (A1)+(C)+(D1)+(D2)=100% by weight. A strand-shaped resin extruded at 300 kg / hr through a die with small holes attached to the tip of the extruder was cooled and solidified in a water bath at 20°C, and then cut to obtain a master batch (H) of a mixture of a brominated flame retardant and a heat stabilizer. The extruder was set at a temperature of 170°C.

[0083] Example 1 [Preparation of styrene-based resin pellets] The styrene resin (A1) and the styrene resin (A2) were uniformly blended in a mixer, melt-kneaded in a 26 mm diameter twin-screw extruder, and formed into strands through a die attached to the tip of the extruder. The strands were cooled and solidified in a water bath, and then cut with a strand cutter to obtain styrene resin pellets. The weight ratio of (A1):(A2) was 80:20, and the total supply amount was 5 kg / h. The MFR of the obtained styrene resin pellets was 9.2 (g / 10 min).

[0084] [Preparation of expandable styrene resin particles] A mixture of styrene-based resin (A1) and styrene-based resin (A2) uniformly blended in a mixer, graphite master batch (G), and master batch (H) of a mixture of bromine-based flame retardant and heat stabilizer were fed to a tandem-type two-stage extruder in which a 40 mm diameter twin-screw extruder (first extruder) and a 90 mm diameter single-screw extruder (second extruder) were connected in series, and melt-kneaded at a set temperature of 190°C and a rotation speed of 167 rpm for the 40 mm diameter extruder. The weight ratio of (A1):(A2):(G):(H) was 54.2:17.5:20:8.3, and the total feed amount was 55.7 kg / h. From the middle of the 40 mm diameter extruder (first extruder), mixed pentane [mixture of 80% by weight of normal pentane (E1) and 20% by weight of isopentane (E2)] was injected at a ratio of 1.8 parts by weight per 100 parts by weight of the melt of the resin mixture (resin composition), and 2.4 parts by weight of isobutane (E3) was injected per 100 parts by weight of the resin composition, adding a total of 4.2 parts by weight of a foaming agent. Then, the mixture was supplied to a 90 mm diameter extruder (second extruder) through a continuation pipe set at 200°C.

[0085] The molten resin was cooled to a resin temperature of 170°C using a 90mm diameter extruder (second extruder), and then extruded from a die having 40 small holes with a diameter of 0.75mm and a land length of 5.0mm attached to the tip of the second extruder set at 260°C into pressurized circulating water at a temperature of 70°C and a pressure of 1.3MPa. The extruded molten resin was cut and pelletized using a rotary cutter with six blades that contacted the die, and transferred to a centrifugal dehydrator to obtain expandable styrene resin particles. At this time, the residence time in the first extruder was 2 minutes, and the residence time in the second extruder was 5 minutes.

[0086] The weight ratio of (A1):(A2) in the resin composition is 54.2+20×0.49+8.3×0.7:17.5≒80:20, taking into account the styrene-based resin (A1) contained in the master batches (G) and (H). Therefore, the MFR of the styrene-based resin pellets can be considered to be the same as the MFR of the styrene-based resin in the resin composition. Similarly, the MFR of the styrene-based resin pellets in the other examples and comparative examples can be considered to be the same as the MFR of the styrene-based resin in each resin composition.

[0087] [Preparation of pre-expanded particles] The obtained expandable styrene resin particles were stored at 15°C for one week or more, and then 0.04 parts by weight of zinc stearate and 0.1 parts by weight of hydroxystearic acid triglyceride, which are external additives, were dry-blended with the expandable styrene resin particles. 270g of the expandable styrene resin particles containing the external additives were put into a pre-expander [batch-type pre-expander manufactured by Daikai Kogyo Co., Ltd.], the pressure inside the can was set to 0.015MPa to 0.025MPa, and steam at 0.12MPa was introduced into the pre-expander to expand to a bulk ratio of 80 times, thereby obtaining pre-expanded particles. The expansion ratio of the obtained pre-expanded particles was 82 times.

[0088] [Preparation of styrene-based resin foam molded products] The obtained pre-expanded particles were cured at 30°C for 24 hours, and then filled into a mold for in-mold molding (length 400mm x width 400mm x thickness 25mm) attached to a polystyrene foam molding machine [KR-57, manufactured by Daisen Kogyo Co., Ltd.], and 0.05 MPa of water vapor was introduced to cause in-mold foaming, and then water was sprayed onto the mold to cool it. The styrene-based resin foam molded body was held in the mold until the pressure of the styrene-based resin foam molded body pressing the mold reached 0.01 MPa (gauge pressure), and then the styrene-based resin foam molded body was taken out to obtain a styrene-based resin foam molded body. The expansion ratio of the obtained styrene-based resin foam molded body was 82 times, and the thermal conductivity of the styrene-based resin foam molded body was measured by the above-mentioned measurement method and found to be 0.02980 W / mK.

[0089] The various properties of the resulting expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0090] Example 2 In [Preparation of styrene-based resin pellets], except that the weight ratio of (A1):(A2) was changed from 80:20 to 60:40, styrene-based resin pellets were prepared by the same process as in Example 1. The MFR of the obtained styrene-based resin pellets was 11.4 (g / 10 min).

[0091] In [Preparation of expandable styrene-based resin particles], expandable styrene-based resin particles were prepared by the same process as in Example 1, except that the weight ratio of (A1):(A2):(G):(H) was changed from 54.2:17.5:20:8.3 to 36.7:35:20:8.3. Using the prepared expandable styrene-based resin particles, pre-expanded particles and styrene-based resin foamed molded products were obtained by the same method as in Example 1.

[0092] The various properties of the resulting expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0093] Example 3 In [Preparation of styrene-based resin pellets], except that the weight ratio of (A1):(A2) was changed from 80:20 to 40:60, styrene-based resin pellets were prepared by the same process as in Example 1. The MFR of the obtained styrene-based resin pellets was 13.6 (g / 10 min).

[0094] In [Preparation of expandable styrene-based resin particles], expandable styrene-based resin particles were prepared by the same process as in Example 1, except that the weight ratio of (A1):(A2):(G):(H) was changed from 54.2:17.5:20:8.3 to 19.2:52.5:20:8.3.

[0095] In [Preparation of pre-expanded particles], except that the pressure setting in the can was changed from 0.015 MPa to 0.025 MPa to 0.005 MPa to 0.015 MPa, pre-expanded particles were prepared in the same manner as in Example 1. Using the prepared pre-expanded particles, a styrene-based resin foamed molded article was obtained in the same manner as in Example 1.

[0096] The various properties of the resulting expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0097] Comparative Example 1 In the [Preparation of styrene-based resin pellets], except that the weight ratio of (A1):(A2) was changed from 80:20 to 100:0, styrene-based resin pellets were prepared by the same process as in Example 1. The MFR of the obtained styrene-based resin pellets was 7.0 (g / 10 min).

[0098] In [Preparation of expandable styrene-based resin particles], expandable styrene-based resin particles were prepared by the same process as in Example 1, except that the weight ratio of (A1):(A2):(G):(H) was changed from 54.2:17.5:20:8.3 to 71.7:0:20:8.3. Using the prepared expandable styrene-based resin particles, pre-expanded particles and a styrene-based resin expansion molded product were obtained by the same method as in Example 1.

[0099] The obtained styrene resin foamed molded article had some recessed foam particles on the surface of the molded article, and it was impossible to measure the dimensions, so it was impossible to measure the molded article magnification and evaluate the dimensional change rate at high temperatures. Regarding the molded article magnification, the dimensional change rate at high temperatures, and the heat resistance performance, various properties of the obtained expandable styrene resin particles, pre-expanded particles, and styrene resin foamed molded article were measured and evaluated by the above-mentioned measurement and evaluation methods.

[0100] Comparative Example 2 In the [Preparation of styrene-based resin pellets], except that the weight ratio of (A1):(A2) was changed from 80:20 to 100:0, styrene-based resin pellets were prepared by the same process as in Example 1. The MFR of the obtained styrene-based resin pellets was 7.0 (g / 10 min).

[0101] In [Preparation of expandable styrene-based resin particles], the weight ratio of (A1):(A2):(G):(H) was changed from 54.2:17.5:20:8.3 to 71.7:0:20:8.3, the amount of mixed pentane was changed from 1.8 parts by weight to 4.2 parts by weight, and the amount of isobutane (E3) was changed from 2.4 parts by weight to 0 parts by weight. Except for this, expandable styrene-based resin particles were prepared by the same process as in Example 1.

[0102] In [Preparation of pre-expanded particles], the same treatment as in Example 1 was carried out to prepare pre-expanded particles, but the expansion ratio of the obtained expanded particles was 60 times, and it was impossible to expand the particles up to 80 times. Using the prepared pre-expanded particles, a styrene-based resin foamed molded article was obtained by the same method as in Example 1.

[0103] The various properties of the resulting expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0104] Comparative Example 3 In [Preparation of styrene-based resin pellets], except that the weight ratio of (A1):(A2) was changed from 80:20 to 18:82, styrene-based resin pellets were prepared by the same process as in Example 1. The MFR of the obtained styrene-based resin pellets was 16.0 (g / 10 min).

[0105] In [Preparation of expandable styrene-based resin particles], expandable styrene-based resin particles were prepared by the same process as in Example 1, except that the weight ratio of (A1):(A2):(G):(H) was changed from 54.2:17.5:20:8.3 to 0:71.7:20:8.3.

[0106] In [Preparation of pre-expanded particles], except that the pressure setting in the can was changed from 0.015 MPa to 0.025 MPa to 0.005 MPa to 0.015 MPa, pre-expanded particles were prepared in the same manner as in Example 1. Using the prepared pre-expanded particles, a styrene-based resin foamed molded article was obtained in the same manner as in Example 1.

[0107] The various properties of the resulting expandable styrene resin particles, pre-expanded particles and styrene resin foamed molded articles were measured and evaluated by the above-mentioned measuring and evaluating methods.

[0108] For each of the Examples and Comparative Examples, the composition of the styrene-based resin pellets, MFR, the amount of each component in the styrene-based resin composition, the amount of each blowing agent, the apparent density of the expandable styrene-based resin particles, the bulk expansion ratio of the pre-expanded particles, the expansion ratio (molded product expansion ratio) of the styrene-based resin foamed molded product, the surface properties of the molded product, the dimensional change rate at high temperatures, and the heat resistance performance are shown in Table 1.

[0109] [Table 1]

[0110] As can be seen from Table 1, by using the expandable styrene-based resin particles of the present disclosure, it is possible to obtain a styrene-based resin foamed molded article having excellent heat resistance and a high expansion ratio.

[0111] The upper and / or lower limit values ​​of the numerical ranges described in this specification can be arbitrarily combined to define a preferred range. For example, the upper and lower limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range, the upper limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range, and the lower limit values ​​of the numerical ranges can be arbitrarily combined to define a preferred range. In addition, in this application, a numerical range expressed using the symbol "~" includes the numerical values ​​described before and after the symbol "~" as the lower and upper limits, respectively.

[0112] Although the present embodiment has been described in detail above, the specific configuration is not limited to this embodiment, and even if there are design changes within the scope that does not deviate from the gist of this disclosure, they are included in this disclosure.

Claims

1. A styrene-based resin composition containing a styrene-based resin and a carbon-based radiation heat transfer inhibitor, and an expandable styrene-based resin particle containing a blowing agent, The expandable styrene-based resin particles have a melt flow rate of 7.5 to 15.5 g / 10 min at 200° C. under a load of 5.0 kg, and the foaming agent contains isobutane.

2. The expandable styrene-based resin particles have an apparent density of 950 kg / m 3 Super 1200kg / m 3 The expandable styrene-based resin particles according to claim 1, wherein:

3. The expandable styrene-based resin particles according to claim 1 , wherein the styrene-based resin composition contains a flame retardant, and the flame retardant is contained in an amount of more than 1.0% by weight and not more than 6.0% by weight based on 100% by weight of the styrene-based resin composition.

4. 2. The expandable styrene-based resin particles according to claim 1, wherein the carbon-based radiation heat transfer inhibitor is more than 2% by weight and not more than 20% by weight based on 100% by weight of the styrene-based resin composition.

5. The expandable styrene-based resin particles according to claim 1 , wherein the carbon-based radiation heat transfer inhibitor is at least one carbon-based radiation heat transfer inhibitor selected from the group consisting of graphite, carbon black, carbon nanotubes, graphene, and activated carbon.

6. The expandable styrene-based resin particles according to claim 1, wherein the amount of the blowing agent in the expandable styrene-based resin particles is more than 1.0 part by weight and not more than 8.0 parts by weight per 100 parts by weight of the styrene-based resin composition.

7. 2. The expandable styrene-based resin particles according to claim 1, wherein the amount of isobutane is 15 to 90% by weight based on 100% by weight of the blowing agent.

8. 2. The expandable styrene-based resin particles according to claim 1, wherein the foaming agent contains a saturated hydrocarbon having 5 to 6 carbon atoms.

9. 2. The expandable styrene-based resin particles according to claim 1, wherein the blowing agent comprises pentane.

10. 2. A pre-expanded styrene resin bead obtained by expanding the expandable styrene resin bead according to claim 1.

11. A foamed molded article of a styrene-based resin obtained by molding the pre-expanded particles of the styrene-based resin according to claim 10.

Citation Information

Patent Citations

  • Foamable polystyrene-based resin particle and method for producing foamable polystyrene-based resin particle

    JP2013136688A