Rubber electrode for electro-osmotic flow pump and electro-osmotic flow pump
The silicone rubber and carbon black-based rubber electrode addresses bubble generation in electroosmotic flow pumps, ensuring stable liquid delivery by improving adhesion and resistance properties.
Patent Information
- Application Number
- JP2023051320
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing electroosmotic flow pumps experience bubble generation at the interface between the porous dielectric and electrodes during long-term use, leading to instability in liquid delivery.
A rubber electrode composed of silicone rubber and carbon black, with a hardness of 40 to 80 and an elastic recovery rate of 70% or more, is used to suppress bubble generation, ensuring long-term liquid feeding stability.
The rubber electrode effectively prevents bubble formation, maintaining excellent liquid feeding stability over extended periods by enhancing adhesion and reducing resistance changes during deformation.
Smart Images

Figure 2024140263000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a rubber electrode for an electroosmotic flow pump suitable as an electrode for an electroosmotic flow pump capable of pumping liquid by utilizing the electroosmotic flow phenomenon, and to an electroosmotic flow pump. [Background technology]
[0002] Electroosmotic flow is a liquid flow that occurs when a voltage is applied to an electric double layer where a liquid and a solid are in contact. In electroosmotic flow, the solid is fixed, so the bulk liquid moves. An electroosmotic flow pump is a pump that can pump liquid by utilizing this electroosmotic flow phenomenon. An electroosmotic flow pump is capable of pumping minute amounts of liquid on the order of nL without pulsation, and is expected to be used as a medical liquid pump for small infusion devices. An electroosmotic flow pump has a porous dielectric and a pair of electrodes, with the porous dielectric being disposed between the pair of electrodes. For example, Patent Document 1 is known as an electroosmotic flow pump that uses rubber electrodes as electrodes. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] International Publication 2018 / 015779 Summary of the Invention [Problem to be solved by the invention]
[0004] When an electroosmotic pump is used for a long time, air bubbles may be generated at the interface between the porous dielectric and the electrodes, which may reduce the stability of the liquid delivery. For this reason, an improvement is required to suppress the generation of air bubbles in the electroosmotic pump during long-term use.
[0005] An object of the present invention is to provide a rubber electrode for an electroosmotic flow pump that can suppress the generation of air bubbles during long-term use and provide an electroosmotic flow pump that has excellent long-term liquid delivery stability. [Means for solving the problem]
[0006] The rubber electrode for an electroosmotic pump according to the present invention contains silicone rubber and carbon black, and has a hardness of 40 to 80, and an elastic recovery rate of 70% or more.
[0007] The silicone rubber may be a cured product of liquid silicone rubber. The carbon black content may be 7.5 parts by mass or more and 10.5 parts by mass or less per 100 parts by mass of the silicone rubber. The change in volume resistivity between before stretching and when stretched by 15% may be 0% or less.
[0008] The electroosmotic pump according to the present invention comprises a porous dielectric and a pair of electrodes, the porous dielectric being disposed between the pair of electrodes, and each of the pair of electrodes being formed from the above-mentioned rubber electrode for an electroosmotic pump.
[0009] (1) The rubber electrode for an electroosmotic pump according to the present invention contains silicone rubber and carbon black, and has a hardness of 40 to 80, and an elastic recovery rate of 70% or more.
[0010] (2) In the above item (1), the silicone rubber may be a cured product of liquid silicone rubber.
[0011] (3) In the above (1) or (2), the content of the carbon black is preferably 7.5 parts by mass or more and 10.5 parts by mass or less per 100 parts by mass of the silicone rubber.
[0012] (4) In any one of (1) to (3) above, the amount of change in volume resistivity between before and after 15% elongation is preferably 0% or less.
[0013] (5) The electroosmotic pump according to the present invention has a porous dielectric and a pair of electrodes, the porous dielectric being disposed between the pair of electrodes, and each of the pair of electrodes being constituted by any one of the rubber electrodes for electroosmotic pumps described above in (1) to (4). Effect of the Invention
[0014] The rubber electrode for an electroosmotic flow pump according to the present invention contains silicone rubber and carbon black, has a hardness of 40 to 80, and an elastic recovery rate of 70% or more, so that air bubble generation during long-term use is suppressed, and an electroosmotic flow pump with excellent long-term liquid delivery stability can be provided.
[0015] When the silicone rubber is a cured liquid silicone rubber, the carbon structure can be dispersed without being destroyed.
[0016] When the content of the carbon black is 7.5 parts by mass or more and 10.5 parts by mass or less with respect to 100 parts by mass of the silicone rubber, low resistance and low hardness can be achieved.
[0017] When the amount of change in volume resistivity between before stretching and when stretched by 15% is 0% or less, the generation of air bubbles during long-term use is easily suppressed. [Brief description of the drawings]
[0018] [Figure 1] 1 is a front view showing an example of an electroosmotic pump including a rubber electrode for an electroosmotic pump according to an embodiment of the present invention. [Diagram 2] 1 is a plan view showing an example of an electroosmotic pump including a rubber electrode for an electroosmotic pump according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view taken along line AA of the electroosmotic pump shown in FIG. 2. [Figure 4] FIG. 1 is a schematic diagram of a rubber electrode for an electroosmotic pump according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0019] A rubber electrode for an electroosmotic flow pump according to the present invention (hereinafter, sometimes simply referred to as a rubber electrode) will be described in detail. Figures 1 and 2 are schematic diagrams showing an example of an electroosmotic flow pump including a rubber electrode for an electroosmotic flow pump according to one embodiment. Figure 3 is a cross-sectional view of the electroosmotic flow pump shown in Figures 1 and 2. Figure 4 is a schematic diagram of a rubber electrode for an electroosmotic flow pump.
[0020] The electroosmotic flow pump 20 has a porous dielectric 12 and a pair of electrodes 10, 10, with the porous dielectric 12 disposed between the pair of electrodes 10, 10. The electroosmotic flow pump 20 is a pump capable of pumping liquid by utilizing the electroosmotic flow phenomenon. An electroosmotic flow is a liquid flow that occurs when a voltage is applied to an electric double layer in which a liquid and a solid are in contact. In an electroosmotic flow, the solid (porous dielectric 12) is fixed, so the bulk liquid moves.
[0021] The porous dielectric 12 may be made of a material that has a suitable strength and allows electroosmotic flow to occur in the porous structure when an external voltage is applied. The porous dielectric 12 may be made of a material with a high dielectric constant. The porous dielectric 12 may be made of a material that has a fine flow path structure for liquid transfer. As such a material, a ceramic porous body may be preferably used.
[0022] Examples of the ceramic include alumina, aluminum nitride, silicon nitride, silicon carbide, silicon oxide, a mixture of two or more of these, etc. The ceramic is preferably a porous sintered body.
[0023] The porous structure of the porous dielectric 12 preferably has an average pore size of 0.1 μm or more from the viewpoint of ensuring an appropriate flow path, etc. Also, from the viewpoint of increasing the amount of electroosmotic flow generated, the average pore size is preferably 5 μm or less, more preferably 1.0 μm or less, and even more preferably 0.5 μm or less.
[0024] Moreover, the porous structure of the porous dielectric 12 preferably has an average porosity of 10% or more from the viewpoints of securing an appropriate flow path, increasing the amount of electroosmotic flow generated, etc., more preferably 25% or more, and further preferably 50% or more. Furthermore, from the viewpoint of strength, etc., the average porosity is preferably 90% or less.
[0025] The shape of the porous dielectric 12 is preferably a shape that does not hinder the movement of the flowing liquid and has a substantially uniform cross-sectional shape perpendicular to the movement direction of the flowing liquid. In order to ensure the flow rate of the flowing liquid and the distance between the electrodes, the shape is preferably a shape that ensures a cross section and member length. Examples of the shape of the porous dielectric 12 include a cylindrical shape, an elliptical cylindrical shape, and a rectangular prism. Examples of the rectangular prism include polygonal prisms such as a triangular prism, a square prism, and a pentagonal prism. Figures 1 to 3 show a cylindrical porous dielectric.
[0026] The size of the porous dielectric 12 is not particularly limited, but the appropriate size for a small medical fluid pump such as a small infusion device is a cross-sectional area of 0.2 to 100 mm. 2 , and the member length is 1 to 20 mm.
[0027] A pair of electrodes 10, 10 are each formed of rubber electrodes for an electroosmotic pump according to the present invention. One electrode 10 is disposed at an upstream end of the porous dielectric 12 in the moving direction of the flowing liquid, and the other electrode 10 is disposed at a downstream end of the porous dielectric 12 in the moving direction of the flowing liquid. Each electrode 10, 10 is formed in a rectangular shape. Each electrode 10, 10 has a through hole 10a formed from one surface to the other surface, the through hole 10a having an inner diameter capable of inserting an end of the porous dielectric 12. Since each electrode 10, 10 is formed of a rubber electrode, the end of the porous dielectric 12 inserted into the through hole 10a can be held and fixed by the clamping pressure of the rubber of each electrode 10, 10. In addition, an end of a rubber tube 14 connected to the end of the porous dielectric 12 is inserted into the through hole 10a on the surface opposite to the surface into which the porous dielectric 12 is inserted of each rectangular electrode 10, 10. The upstream rubber tube 14 is connected to an upstream reservoir tank or the like (not shown), and the downstream rubber tube 14 is connected to a drug solution chip or the like (not shown). An enclosing rubber 16 is disposed in an area including the porous dielectric 12 and the pair of electrodes 10, 10 to cover them and maintain the pressure resistance of the entire pump. Examples of the enclosing rubber 16 include silicone rubber. In Figs. 1 and 2, the enclosing rubber 16 is shown transparently by dashed lines to make it easier to see the porous dielectric 12 and the pair of electrodes 10, 10 disposed therein.
[0028] The rubber electrode 10 is formed from a silicone rubber composition containing silicone rubber and carbon black.
[0029] The silicone rubber may be one that is generally known as organopolysiloxane. The silicone rubber may be liquid rubber or millable rubber. The silicone rubber is more preferably liquid rubber. If it is liquid rubber, it can be dispersed without destroying the carbon structure.
[0030] The organopolysiloxane has an organic group. The organic group is a monovalent substituted or unsubstituted hydrocarbon group. Examples of the unsubstituted hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, hexyl, and dodecyl groups, aryl groups such as phenyl groups, and aralkyl groups such as β-phenylethyl and β-phenylpropyl groups. Examples of the substituted hydrocarbon group include chloromethyl and 3,3,3-trifluoropropyl groups. In general, organopolysiloxanes having methyl groups as organic groups are often used because of the ease of synthesis. The organopolysiloxane is preferably linear, but may be branched or cyclic.
[0031] Organopolysiloxanes have a predetermined reactive group (functional group) according to their crosslinking mechanism (curing mechanism). Examples of the reactive group include alkenyl groups (vinyl groups, allyl groups, butenyl groups, pentenyl groups, hexenyl groups, etc.) and silanol groups. Organopolysiloxanes having alkenyl groups are crosslinked by a peroxide crosslinking reaction using an organic peroxide as a crosslinking agent, or an addition reaction using an organopolysiloxane (organohydrogenpolysiloxane) having a hydrosilyl group as a crosslinking agent. A hydrosilylation catalyst can be used in combination for the addition reaction. Organopolysiloxanes having silanol groups are crosslinked by a condensation reaction. A condensation crosslinking agent can be used in combination for the condensation reaction.
[0032] The organopolysiloxane having an alkenyl group preferably has at least two alkenyl groups in one molecule. The organopolysiloxane having a hydrosilyl group preferably has at least two hydrosilyl groups in one molecule. The organopolysiloxane having a silanol group preferably has at least two silanol groups in one molecule.
[0033] Examples of organic peroxides include benzoyl peroxide, 2,4-dichlorobenzoyl peroxide, p-methylbenzoyl peroxide, o-methylbenzoyl peroxide, dicumyl peroxide, cumyl-t-butyl peroxide, 2,5-dimethyl-2,5-di-t-butylperoxyhexane, di-t-butyl peroxide, etc. Among these, dicumyl peroxide, cumyl-t-butyl peroxide, 2,5-dimethyl-2,5-di-t-butylperoxyhexane, and di-t-butyl peroxide are preferred because they provide particularly low compression set.
[0034] The amount of organic peroxide added is not particularly limited, but is usually within the range of 0.1 to 10 parts by mass per 100 parts by mass of the organopolysiloxane having an alkenyl group.
[0035] Organopolysiloxanes (organohydrogenpolysiloxanes) having hydrosilyl groups specifically include methylhydrogenpolysiloxanes capped at both ends with trimethylsiloxy groups, dimethylsiloxane-methylhydrogensiloxane copolymers capped at both ends with trimethylsiloxy groups, dimethylpolysiloxanes capped at both ends with dimethylhydrogensiloxane, dimethylsiloxane-methylhydrogensiloxane copolymers capped at both ends with dimethylhydrogensiloxane, methylhydrogensiloxane-diphenylsiloxane copolymers capped at both ends with trimethylsiloxy groups, methylhydrogensiloxane-diphenylsiloxane-dimethylsiloxane copolymers capped at both ends with trimethylsiloxy groups, (CH 3 ) 2 A copolymer consisting of HSiO 1 / 2 units and SiO 4 / 2 units, (CH 3 ) 2 HSiO 1 / 2 units and SiO 4 / 2 units and (C 6 H 5 ) SiO 3 / 2 units and copolymers thereof.
[0036] The amount of the hydrosilyl group-containing organopolysiloxane to be added is not particularly limited, but is usually within the range of 0.1 to 40 parts by mass per 100 parts by mass of the alkenyl group-containing organopolysiloxane.
[0037] Examples of the hydrosilylation catalyst include platinum-based catalysts, such as fine particle platinum, platinum black, platinum-supported activated carbon, platinum-supported silica, chloroplatinic acid, alcohol solutions of chloroplatinic acid, platinum-olefin complexes, and platinum-alkenylsiloxane complexes.
[0038] The amount of hydrosilylation catalyst added is not particularly limited, but is usually in the range of 1 ppm to 1 part by mass, calculated as the amount of platinum-based metal, per 100 parts by mass of the organopolysiloxane having alkenyl groups.
[0039] As the crosslinking agent for condensation, a silane having two or more, preferably three or more, hydrolyzable groups in one molecule, or a partial hydrolysis condensate thereof is used. In this case, the hydrolyzable groups include alkoxy groups such as methoxy, ethoxy, and butoxy groups, ketoxime groups such as dimethylketoxime and methylethylketoxime groups, acyloxy groups such as acetoxy groups, alkenyloxy groups such as isopropenyloxy and isobutenyloxy groups, amino groups such as N-butylamino and N,N-diethylamino groups, and amide groups such as N-methylacetamide groups.
[0040] The amount of the condensation crosslinking agent added is not particularly limited, but is usually within the range of 1 to 50 parts by mass per 100 parts by mass of the organopolysiloxane having a silanol group.
[0041] Carbon black is used for the purpose of imparting electrical conductivity. From the viewpoint of high electrical conductivity, it is preferable that carbon black has a relatively low resistance. From this viewpoint, it is preferable that carbon black has a relatively large specific surface area and a small particle size. Specifically, carbon black has a specific surface area of 100 m 2 / g or more. More preferably, it is 200m 2 / g or more, more preferably 500m 2 The upper limit of the specific surface area of carbon black is not particularly limited, but is preferably 1500 m 2 / g or less. The average particle size is preferably 10 nm or more and 50 nm or less, and more preferably 20 nm or more and 40 nm or less. The specific surface area of carbon black is a value measured by the BET method. The average particle size of carbon black is represented by the arithmetic mean diameter obtained by observing carbon black under an electron microscope.
[0042] The carbon black content is preferably 7.5 parts by mass or more, more preferably 8.0 parts by mass or more, per 100 parts by mass of silicone rubber, from the viewpoint of easily ensuring excellent electrical conductivity, etc. Also, from the viewpoint of being able to reduce hardness while ensuring excellent electrical conductivity, the carbon black content is preferably 10.5 parts by mass or less, more preferably 9.5 parts by mass or less, per 100 parts by mass of silicone rubber.
[0043] In addition to the silicone rubber and carbon black, the silicone rubber composition may contain general additives that are added to silicone rubber compositions, provided that the additives do not impair the present invention. Examples of additives that can be added include fillers, crosslinking accelerators, crosslinking retarders, crosslinking assistants, scorch inhibitors, antiaging agents, softeners, heat stabilizers, flame retardants, flame retardant assistants, ultraviolet absorbers, and rust inhibitors.
[0044] The hardness of the rubber electrode 10 is 40 or more and 80 or less. The hardness of the rubber electrode 10 can be measured by a durometer type A hardness tester according to JIS K 6253. Since the hardness of the rubber electrode 10 is low, ie, 80 or less, when the end of the porous dielectric 12 is inserted into the through hole of the rubber electrode 10, a gap is unlikely to occur between the end of the porous dielectric 12 and the inner wall of the through hole 10a of the rubber electrode 10, the contact area is large, and the adhesion is excellent. As a result, the dielectric constant is reduced, so that even if the electroosmotic flow pump 20 is used for a long time, the generation of bubbles at the interface between the porous dielectric 12 and the rubber electrode 10 is suppressed, and the liquid transfer stability is excellent. Furthermore, since the hardness of the rubber electrode 10 is low, ie, 80 or less, when the end of the porous dielectric 12 is inserted into the through hole 10a of the rubber electrode 10, the rubber electrode 10 is significantly deformed. When the rubber electrode 10 is greatly deformed, the resistance of the rubber electrode 10 decreases, so that even if the electroosmotic flow pump 20 is used for a long time, the generation of bubbles at the interface between the porous dielectric 12 and the rubber electrode 10 is suppressed, and the liquid transfer stability is excellent. From this viewpoint, the hardness of the rubber electrode 10 is more preferably 75 or less, and even more preferably 70 or less. And, when the hardness of the rubber electrode 10 is 40 or more, it is not too soft, and the generation of bubbles at the interface between the porous dielectric 12 and the rubber electrode 10 is suppressed, and the liquid transfer stability is excellent. From this viewpoint, the hardness of the rubber electrode 10 is more preferably 45 or more, and even more preferably 50 or more. The hardness of the rubber electrode 10 can be adjusted by the properties of the silicone rubber, the content of carbon black, and the like. For example, the hardness of liquid silicone rubber can be made lower than that of Millable. And, the lower the carbon black content, the lower the hardness can be made.
[0045] The elastic recovery rate of the rubber electrode 10 is 70% or more. If the elastic recovery rate of the rubber electrode 10 is low, when the end of the porous dielectric 12 is inserted into the through hole 10a of the rubber electrode 10, a gap is likely to occur between the end of the porous dielectric 12 and the inner wall of the through hole 10a of the rubber electrode 10, and the contact area becomes small, resulting in poor adhesion. If the elastic recovery rate of the rubber electrode 10 is high, 70% or more, adhesion between the end of the porous dielectric 12 and the inner wall of the through hole 10a of the rubber electrode 10 is ensured, and even if the electroosmotic flow pump 20 is used for a long time, the generation of bubbles at the interface between the porous dielectric 12 and the rubber electrode 10 is suppressed, resulting in excellent liquid transfer stability. From this viewpoint, the elastic recovery rate of the rubber electrode 10 is more preferably 75% or more, and even more preferably 80% or more. The elastic recovery rate of the rubber electrode 10 can be measured using a microhardness tester (Fischer Scope H100C manufactured by Fischer) in accordance with ISO14577-1. The elastic recovery rate of the rubber electrode 10 can be adjusted by the properties of the silicone rubber, the carbon black content, and the like.
[0046] The rubber electrode 10 according to the present invention has a characteristic that the volume resistivity is likely to be lower after stretching than before stretching because the silicone rubber, which is the base rubber, is relatively soft and the soft silicone rubber contains carbon black. Therefore, when the end of the porous dielectric 12 is inserted into the through hole 10a of the rubber electrode 10, the resistance is unlikely to increase due to deformation of the rubber, and an appropriate flow rate is maintained, making it easy to ensure stable liquid delivery. In the rubber electrode 10 according to the present invention, the change in the volume resistivity before stretching and the volume resistivity at 15% stretching can be made within a predetermined range by setting the hardness and elastic recovery rate within a desired range. Specifically, the change in the volume resistivity before stretching and the volume resistivity at 15% stretching can be made 0% or less. Moreover, the change in the volume resistivity before stretching and the volume resistivity at 15% stretching is more preferably -10% or less. The volume resistivity of the rubber electrode 10 can be measured in accordance with the parallel terminal electrode method of JIS K6271 (2008). The change in volume resistivity between before and after 15% stretching is expressed as R 0 , volume resistivity at 15% elongation is R 1 Then, {(R0 -R 1 ) / R 0}×100(%).
[0047] The silicone rubber composition can be prepared, for example, as follows. For example, when liquid silicone rubber is used, the liquid silicone rubber, carbon black, and various additives (excluding crosslinking agents and catalysts) added as necessary are mixed using a planetary mixer, Henschel mixer, Ross mixer, Hobart mixer, kneader mixer, etc., and then, as necessary, a crosslinking agent and catalyst are added, and the mixture is kneaded using a planetary mixer, Henschel mixer, Ross mixer, Hobart mixer, kneader mixer, roll, etc., to prepare the composition. In the above preparation method, the crosslinking agent and catalyst may be added during the initial kneading.
[0048] On the other hand, when millable silicone rubber is used, millable silicone rubber, carbon black, and various additives such as catalysts (excluding crosslinking agents) added as necessary are kneaded using a kneader mixer, rolls, etc., and then a crosslinking agent or, if necessary, a retarder such as 1-ethynyl-1-cyclohexanol is added, and the mixture is kneaded using rolls, etc. In the above preparation method, the crosslinking agent may be added during the initial kneading.
[0049] The silicone rubber composition becomes a silicone rubber cured product (molded product) by heat curing. As for the molding method, a predetermined molding method can be selected according to the shape and size of the molded product. Specifically, molding methods such as casting, injection molding, compression molding, calendar molding, extrusion molding, coating, and screen printing can be mentioned.
[0050] The curing conditions are not particularly limited and can be appropriately selected depending on the physical properties of the desired molded product. Generally, the curing is performed at a temperature of 20 to 450° C. for a period of several seconds to about two weeks.
[0051] The obtained silicone rubber molded product is preferably subjected to a secondary cure under specified conditions. This can reduce the compression set of the molded product, reduce the amount of low molecular weight siloxane components remaining in the silicone rubber, and remove decomposition products of organic peroxides. The secondary cure conditions are preferably 200°C or higher, more preferably 200 to 250°C. Also, the cure is preferably at a specified temperature for 1 hour or more, more preferably 1 to 10 hours.
[0052] Rubber electrode 10 having the above configuration contains silicone rubber and carbon black, has a hardness of 40 to 80, and has an elastic recovery rate of 70% or more, thereby suppressing the generation of air bubbles during long-term use, and making it possible to provide electroosmotic flow pump 20 with excellent long-term liquid delivery stability.
[0053] The electroosmotic pump rubber electrode 10 according to the present invention is suitable for use in small medical fluid pumps such as small infusion devices. EXAMPLES
[0054] The present invention will be described in detail below using examples and comparative examples.
[0055] (Examples 1 to 6, 9 to 12, Comparative Examples 2 to 3) Liquid silicone rubber (vinyl-containing dimethylpolysiloxane) <1> ), platinum catalyst, and carbon black were mixed together and mixed for 30 minutes in a planetary mixer. Next, a crosslinking agent (hydrosilyl group-containing dimethylpolysiloxane) and 1-ethynyl-1-cyclohexanol were added and mixed for a further 30 minutes. The mixture was then degassed under reduced pressure to prepare a liquid silicone rubber composition.
[0056] (Examples 7 and 8, Comparative Example 4) Furthermore, calcium carbonate was added to prepare a liquid silicone rubber composition.
[0057] Comparative Example 1 Millable silicone rubber (vinyl group-containing dimethylpolysiloxane) is used to obtain the composition shown in the table. <2> ), platinum catalyst, and carbon black were kneaded in a kneader for 15 minutes, and then 1-ethynyl-1-cyclohexanol and a crosslinking agent (hydrosilyl group-containing dimethylpolysiloxane) were kneaded in using a two-roll mill to prepare a millable silicone rubber composition.
[0058] (Sheet molding) Each silicone rubber composition was press molded at 170°C for 10 minutes, and then secondary cured at 200°C for 4 hours to produce a sheet with a thickness of 3.0 mm.
[0059] Details of the materials used in the examples and comparative examples are as follows. <Liquid silicone rubber> ·Vinyl group-containing dimethylpolysiloxane <1> (Gelest "DMS-V35") <Millable Silicone Rubber> ·Vinyl group-containing dimethylpolysiloxane <2> (KCC "SF3900C") <Crosslinking agent> Hydrosilyl-containing dimethylpolysiloxane (Gelest "HMS-151") <Retarder> 1-Ethynyl-1-cyclohexanol (Tokyo Chemical Industry Co., Ltd., reagent) <Catalyst> Platinum catalyst (Gelest "SIP6831.2") <Carbon black> Ketjenblack ("EC300J" manufactured by Lion Specialty Chemicals), BET specific surface area 800m 2 / g, primary particle size 39.5nm Acetylene black (Denka Black HS-100 manufactured by Denki Kagaku Kogyo Co., Ltd.), hydrochloric acid absorption capacity 10.4ml / 5g, bulk density 0.15g / ml <Calcium carbonate> "Softon 3200" manufactured by Shiraishi Calcium Co., Ltd.
[0060] The hardness, elastic recovery rate, and volume resistivity of each rubber sheet were measured. In addition, the change in volume resistivity between before and after 15% elongation was measured for each rubber sheet. Furthermore, the liquid transfer stability when a certain voltage was applied was evaluated.
[0061] (hardness) The hardness of each rubber sheet was measured using a durometer type A hardness tester in accordance with JIS K 6253.
[0062] (Elastic recovery rate) In accordance with ISO14577-1, the surface of the rubber sheet was measured under the following measurement conditions using a microhardness tester (Fischer Scope H100C, manufactured by Fischer), and ηIT [%] was calculated. That is, when a microhardness tester is used to press an indenter into the material surface with a constant test load, only a small portion of the total mechanical work Wtotal of the indentation shown during the indentation work is consumed as the plastic deformation work Wplast of the indentation. When the test load is released, the remaining portion is released as the elastic return deformation work Welast of the indentation. If this mechanical work is defined as W=∫Fdh, the relationship is as follows: ηIT[%]=Welast / Wtotal However, Wtotal = Welast + Wplast <Measurement conditions> Indenter: Square vertical diamond indenter with facing angle of 136° Initial load: 0mN Maximum pressing load: 20mN (constant load) Time to reach maximum load: 0.25~10sec Maximum load holding time: 5sec Unloading time: 0.25~10sec Measurement temperature: 25℃
[0063] (Volume resistivity) First, the volume resistivity of the rubber sheet in its natural state (initial state) before stretching was measured. The volume resistivity was measured according to the parallel terminal electrode method of JIS K6271 (2008). In the measurement of the volume resistivity, a commercially available rubber sheet (Sumitomo 3M's "VHB (registered trademark) 4910") was used as an insulating resin support for supporting the rubber sheet. Next, the rubber sheet was stretched together with the support in a uniaxial direction at an elongation rate of 15%, and the volume resistivity was measured. Next, the change (%) between the volume resistivity before stretching and the volume resistivity at 15% elongation was calculated. The elongation rate is a value calculated by the following formula (i). The change is a value calculated by the following formula (ii). Stretching rate (%)=(ΔL0 / L0)×100...(i) [L0: Gauge length of the test piece, ΔL0: Increase due to elongation of the gauge length of the test piece] Change (%) = {(R 0 -R 1 ) / R 0}×100...(ii) [R 0 : Volume resistivity before stretching, R 1 : Volume resistivity at 15% elongation
[0064] (liquid transfer stability) As shown in Figure 1, a porous dielectric (ceramics) was placed between a pair of rubber electrodes formed using the prepared liquid silicone rubber composition, terminals were connected to the rubber electrodes, a specified voltage was applied, and it was confirmed that pure water flowed (pure water flows from the positive electrode to the negative electrode). Next, it was connected to a Surpass Industrial flow rate measuring device (NDFD-1.6S-0.35) and monitored. It was determined that the flow had stopped when the flow rate dropped to zero. If the time during which the flow rate was stable was 3500 seconds or more, it was marked as "good", if it was 2000 seconds or more but less than 3500 seconds, it was marked as "good", and if it was less than 2000 seconds, it was marked as "bad".
[0065] [Table 1]
[0066] [Table 2]
[0067] [Table 3]
[0068] The rubber electrode of Comparative Example 1 uses millable rubber as the silicone rubber. Therefore, the dispersibility of carbon black is poor, and in order to reduce the resistance to the desired value, it is necessary to increase the amount of carbon black, which deteriorates the elastic recovery rate. As a result, air bubbles are generated and the liquid transfer stability is deteriorated when the electrode is used for less than 2000 seconds. The rubber electrode of Comparative Example 2 uses liquid rubber as the silicone rubber, but has low hardness. Therefore, air bubbles are generated and the liquid transfer stability is deteriorated when the electrode is used for less than 2000 seconds. The rubber electrode of Comparative Example 3 uses liquid rubber as the silicone rubber, but has high hardness, and the gap between the end of the porous dielectric and the inner wall of the through hole of the rubber electrode is large, and the contact area is reduced. Therefore, air bubbles are generated and the liquid transfer stability is deteriorated when the electrode is used for less than 2000 seconds. The rubber electrode of Comparative Example 4 uses liquid rubber as the silicone rubber, but has poor elastic recovery rate. Thus, air bubbles are generated and the liquid transfer stability is deteriorated when the electrode is used for less than 2000 seconds.
[0069] On the other hand, the rubber electrodes of the Examples contain silicone rubber and carbon black, and have a hardness of 40 to 80 and an elastic recovery rate of 70% or more. The Examples show that the generation of air bubbles is suppressed and the liquid transfer stability is excellent when used for 2000 seconds or more. Examples 1 to 6 show that when the hardness of the rubber electrode is 65 to 75, the liquid transfer stability is particularly excellent.
[0070] Although the embodiments and examples of the present invention have been described above, the present invention is not limited to the above-mentioned embodiments and examples, and various modifications are possible without departing from the spirit and scope of the present invention. [Explanation of symbols]
[0071] 10 Rubber Electrode 10a through hole 12 Porous Dielectrics 14 Rubber tube 16 Comprehensive Rubber 20 Electroosmotic Pump
Claims
1. A rubber electrode for an electroosmotic pump, comprising: Contains silicone rubber and carbon black, A rubber electrode for an electroosmotic pump, having a hardness of 40 or more and 80 or less, and an elastic recovery rate of 70% or more.
2. 2. The rubber electrode for an electroosmotic pump according to claim 1, wherein the silicone rubber is a cured product of liquid silicone rubber.
3. 3. The rubber electrode for an electroosmotic pump according to claim 1, wherein the content of the carbon black is 7.5 parts by mass or more and 10.5 parts by mass or less based on 100 parts by mass of the silicone rubber.
4. 3. The rubber electrode for an electroosmotic pump according to claim 1, wherein the change in volume resistivity between before and after 15% stretching is 0% or less.
5. 3. An electroosmotic flow pump comprising: a porous dielectric; and a pair of electrodes, the porous dielectric being disposed between the pair of electrodes, each of the pair of electrodes being formed from a rubber electrode for an electroosmotic flow pump according to claim 1 or 2.
Citation Information
Patent Citations
Multi-criteria adaptive scheduling for a market-oriented hybrid cloud infrastructure
WO2018015779A1