Resin composition, resin molding and method for manufacturing resin molding

The resin composition, comprising a (meth)acrylic (co)polymer, nanoparticles, and acrylic particles, addresses the issue of reduced bluish tint and increased whiteness in blue-sky lighting by maintaining optical properties and diffusivity, enhancing the lighting experience.

JP2024140269AInactive Publication Date: 2024-10-10MITSUBISHI CHEM CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023051329
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Existing diffusers in blue-sky lighting devices require a large amount of nanoparticles for sufficient diffusivity, leading to reduced bluish tint and increased whiteness when illuminated.

Method used

A resin composition containing a (meth)acrylic (co)polymer, nanoparticles with a specific size range, and acrylic particles with a crosslinked structure, balanced to maintain optical properties and diffusivity.

Benefits of technology

The resin composition achieves excellent bluishness and diffusivity when illuminated, with controlled total light transmittance and haze, suitable for blue-sky lighting applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 00000012_0000
    Figure 00000012_0000
  • Figure 00000012_0001
    Figure 00000012_0001
  • Figure 00000012_0002
    Figure 00000012_0002
Patent Text Reader

Abstract

To provide a resin composition which is excellent in optical characteristics, and bluishness and diffusibility when illumination is turned on.SOLUTION: A resin composition contains a (meth)acrylic (co) polymer (X), nanoparticles (Y), and acrylic particles (Z) having an average particle diameter of 1 μm or more and a crosslinked structure.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a resin composition, a resin molded article, and a method for producing a resin molded article. [Background technology]

[0002] In recent years, indoor lighting devices that mimic the sky have been sold. Such lighting devices are called blue sky lighting, skylight lighting, or skylight lighting, and are often installed on indoor ceilings. The lighting device mimics the sky, reproducing a natural environment, allowing visitors to experience the sky and natural light with a sense of depth even indoors. With such lighting devices, even in closed spaces such as hospital waiting rooms, the pseudo skylight created by the lighting device has the effect of improving the mood of visitors.

[0003] By the way, the sky seen from the ground during the day is blue because sunlight collides with molecules that are sufficiently smaller than the wavelength of the sunlight, and the short-wavelength blue light is scattered more strongly than the long-wavelength red light (Rayleigh scattering). Blue sky lighting utilizes this phenomenon, and generally uses a medium obtained by dispersing nanoparticles capable of generating Rayleigh scattering in a transparent resin. Patent Document 1 proposes a diffuser that can reproduce a natural blue sky and a lighting device using the diffuser. The diffuser described in Patent Document 1 includes a medium and nanoparticles present in the medium, and has specific parameters. Patent Document 2 also proposes a diffuser that reproduces the diffusion of sunlight. The diffuser described in Patent Document 2 includes PMMA (polymethylmethacrylate) and TiO2 or ZnO as nanoparticles having a specific particle size, and has specific parameters. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] International Publication No. 2020 / 240933 [Patent Document 2] International Publication No. 2009 / 156348 Summary of the Invention [Problem to be solved by the invention]

[0005] In the diffusers described in Patent Documents 1 and 2, the medium contains nanoparticles that cause Rayleigh scattering, and the nanoparticles are considered to have both scattering and diffusing functions. However, when nanoparticles are given a diffusing function in addition to a scattering function, a large amount of nanoparticles must be added to obtain sufficient diffusivity. As a result, a lighting device using the diffuser has a problem that the blueness is reduced when the light is turned on, and a whitish color is generated when the light is turned on.

[0006] The present invention has an object to solve the above problems. That is, an object of the present invention is to provide a resin composition and a resin molded article having excellent optical properties, blueness when illuminated, and diffusibility. Another object of the present invention is to provide a method for producing the resin molded article. [Means for solving the problem]

[0007] The present invention relates to the following. [1] A resin composition comprising: a (meth)acrylic (co)polymer (X); nanoparticles (Y); and acrylic particles (Z) having an average particle size of 1 μm or more and a crosslinked structure. [2] The resin composition according to [1], comprising 0.01 to 0.1 parts by mass of the nanoparticles (Y) per 100 parts by mass of the (meth)acrylic (co)polymer (X). [3] The resin composition according to [1] or [2], comprising 0.01 to 5 parts by mass of the acrylic particles (Z) per 100 parts by mass of the (meth)acrylic (co)polymer (X). [4] The resin composition according to any one of [1] to [3], wherein the average particle size of the acrylic particles (Z) is 1 μm to 50 μm. [5] The resin composition according to any one of [1] to [4], wherein the acrylic particles (Z) are hollow particles. [6] The resin composition according to any one of [1] to [5], wherein the nanoparticles (Y) have a particle diameter of 10 nm to 80 nm. [7] A resin molded product comprising the resin composition according to any one of [1] to [6]. [8] The resin molded article according to [7], having a total light transmittance of 71.7% to 90% as measured in a wavelength range of 380 nm to 780 nm according to JIS K7361-1, and a haze of 20% to 90% as measured in a wavelength range of 380 nm to 780 nm according to JIS K7136. [9] A method for producing a resin molded product, comprising a step of molding the resin composition according to any one of [1] to [6]. Effect of the Invention

[0008] According to the present invention, it is possible to provide a resin composition and a resin molded article that are excellent in optical properties, bluish color when illuminated, and diffusivity. [Brief description of the drawings]

[0009] [Figure 1] FIG. 2 is a diagram showing a black box used for evaluating blueness and diffusion property when the light is turned on in the examples. [Diagram 2] 1 is a diagram showing a state in which an LED light source and a resin molding are installed in the black box. [Diagram 3] 3 is a cross-sectional view of the black box shown in FIG. 2 as viewed from the front side of the paper. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. However, the following description is an example of an embodiment of the present invention, and the present invention is not limited to the following embodiment as long as it does not deviate from the gist of the present invention.

[0011] In the present invention, "(meth)acrylic" means one or both of "acrylic" and "methacrylic". Accordingly, "(meth)acrylic" means one or both of "acrylic" and "methacrylic". In addition, in the present invention, "(co)polymer" means one or both of "polymer" and "copolymer".

[0012] In the present invention, "monomer" means an unpolymerized compound, and "repeating unit" means a unit derived from a monomer formed by polymerization of the monomer. The repeating unit may be a unit formed directly by a polymerization reaction, or may be a unit in which a part of the unit is converted into a different structure by treating a polymer.

[0013] In the present invention, "mass %" indicates the content ratio of a given component contained in a target object (total amount: 100 mass %). In the present invention, unless otherwise specified, a numerical range expressed using "~" means a range including the numerical values ​​before and after "~" as the lower and upper limits, and "A to B" means "A or more and B or less."

[0014] <Resin composition (M)> The resin composition (M) according to the present invention contains at least a (meth)acrylic (co)polymer (X), nanoparticles (Y), and acrylic particles (Z) having an average particle size of 1 μm or more and a crosslinked structure (hereinafter, simply referred to as "acrylic particles (Z)"). By containing the above components in the resin composition (M), the whitishness of the resin composition is suppressed, and as a result, a resin molded product having excellent optical properties, blueness when illuminated, and diffusion can be obtained.

[0015] [(Meth)acrylic (co)polymer (X)] Examples of the (meth)acrylic (co)polymer (X) include a homopolymer of methyl (meth)acrylate and a copolymer of methyl (meth)acrylate and one or more vinyl monomers (hereinafter also referred to as a "methyl (meth)acrylate copolymer"). Specific examples of the methyl (meth)acrylate copolymer include copolymers containing 50% by mass or more of methyl (meth)acrylate units. The (meth)acrylic (co)polymer (X) may be used alone or in combination of two or more.

[0016] Among these (meth)acrylic (co)polymers (X), methyl methacrylate homopolymers or copolymers containing 50% by mass or more of methyl methacrylate units (methyl methacrylate copolymers) are preferred because of their excellent optical properties, mechanical properties, heat resistance, and transparency. As the methyl methacrylate copolymers, copolymers containing 60% by mass or more of methyl methacrylate units are more preferred, and copolymers containing 70% by mass or more of methyl methacrylate units are even more preferred.

[0017] The vinyl monomer is not particularly limited as long as it is a monomer copolymerizable with methyl (meth)acrylate and is a monomer other than methyl (meth)acrylate. Examples of vinyl monomers include methyl acrylate, methyl methacrylate, ethyl (meth)acrylate, n-propyl (meth)acrylate, i-propyl (meth)acrylate, t-butyl (meth)acrylate, i-butyl (meth)acrylate, n-butyl (meth)acrylate, cyclohexyl (meth)acrylate, bornyl (meth)acrylate, norbornyl (meth)acrylate, isobornyl (meth)acrylate, adamantyl (meth)acrylate, dimethyladamantyl (meth)acrylate, methylcyclohexyl (meth)acrylate, norbornylmethyl (meth)acrylate, menthyl (meth)acrylate, fenchyl (meth)acrylate, dicyclopentanyl (meth)acrylate, dicyclopentenyloxyethyl (meth)acrylate, cyclodecyl (meth)acrylate, 4-t-butylcyclohexyl (meth)acrylate, trimethylcyclohexyl (meth)acrylate, etc. These may be used alone or in combination of two or more. Although methyl acrylate and methyl methacrylate are exemplified as vinyl monomers, this is intended to mean that the (meth)acrylic (co)polymer (X) may be a copolymer of methyl acrylate and methyl methacrylate.

[0018] [Nanoparticles (Y)] The nanoparticles (Y) are not particularly limited as long as they have a particle diameter sufficiently smaller than the wavelength of sunlight and cause Rayleigh scattering. Examples of such nanoparticles (Y) include TiO2, Al2O3, ZnO2, and SiO2. One type of nanoparticle may be used alone, or two or more types may be used in combination. In general, these nanoparticles are often used in a form dispersed in a solvent in order to ensure dispersibility. In this embodiment, too, from the viewpoint of improving the dispersibility of the nanoparticles (Y) in the resin composition and the resin molded body, it is preferable to add the nanoparticles (Y) as a dispersion liquid dispersed in a solvent, that is, as a nanoparticle dispersion (nanoparticle-containing sol). Examples of nanoparticle dispersions include HTD-710T (trade name, TiO2-IPA dispersion, solid concentration: 40 mass%, particle size: 15 nm to 50 nm) and HTD-711Z (trade name, ZnO2-IPA dispersion, solid concentration: 45 mass%, particle size: 20 nm to 30 nm) manufactured by Teika Corporation; and RTTMIBK20wt%-H36 (trade name, TiO2-MIBK dispersion, solid concentration: 20 mass%, particle size: 36 nm) manufactured by CIK Nanotech Corporation.

[0019] When the difference in refractive index between the nanoparticles (Y) and the (meth)acrylic (co)polymer (X) is large, the resulting resin composition and resin molded product may be whitened depending on the particle size and / or the amount of the nanoparticles (Y). Therefore, from the viewpoints of transparency of the resin composition and the resin molded product, reduction of whiteness, and suppression of aggregation of the nanoparticles, the particle size of the nanoparticles (Y) is preferably 1 nm to 100 nm, more preferably 10 nm to 80 nm. In the present invention, the particle size of the nanoparticles (Y) means the crystallite size calculated by measuring the XRD peak intensity and the half width of the peak using an X-ray diffractometer and applying the Scherrer method.

[0020] The content of the nanoparticles (Y) in the resin composition (M) is preferably 0.01 to 0.1 parts by mass relative to 100 parts by mass of the (meth)acrylic (co)polymer (X). If the content of the nanoparticles (Y) is within the above range, the nanoparticles (Y) can sufficiently cause Rayleigh scattering. The content of the nanoparticles (Y) is more preferably 0.01 to 0.09 parts by mass, and further preferably 0.01 to 0.07 parts by mass.

[0021] [Acrylic particles (Z)] The acrylic particles (Z) have an average particle diameter of 1 μm or more and have a crosslinked structure. The acrylic particles (Z) play a role in imparting diffusibility to the resin composition and the resin molded body. From the viewpoint of transparency and reduction of whiteness of the resin molded body, the acrylic particles (Z) preferably contain a methyl methacrylate unit. Examples of the acrylic particles (Z) include MBX-5 (trade name, refractive index: 1.495, average particle diameter: 5 μm) and SMX-5R (trade name, refractive index: 1.555, average particle diameter: 5 μm) manufactured by Sekisui Chemical Co., Ltd.; MX-300 (trade name, refractive index: 1.49, average particle diameter: 3 μm) and MX-500L (trade name, refractive index: 1.49, average particle diameter: 5 μm) manufactured by Soken Chemical & Engineering Co., Ltd.

[0022] In the present invention, the average particle size of the acrylic particles (Z) is the particle size (D50) at 50% cumulative value in the volume-based particle size distribution determined by a laser diffraction / scattering method. The average particle size of the acrylic particles (Z) is preferably 50 μm or less from the viewpoint of providing the resulting resin composition and resin molded product with excellent smoothness and appearance.

[0023] The acrylic particles (Z) may be hollow particles having a shell formed of a crosslinked polymer and a hollow portion surrounded by the shell. The shell may be composed of one layer or multiple layers. Since hollow particles have a small specific gravity, the number of particles per mass tends to be large, and the resin composition and the resin molded product can be efficiently imparted with diffusibility. An example of such acrylic particles (Z) is MBP-8 (trade name, average particle size: 8 μm) manufactured by Sekisui Chemical Co., Ltd.

[0024] From the viewpoint of obtaining sufficient diffusibility, the content of the acrylic particles (Z) in the resin composition (M) is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, further preferably 0.07 to 3 parts by mass, and particularly preferably 0.1 to 2 parts by mass, relative to 100 parts by mass of the (meth)acrylic (co)polymer (X).

[0025] [Various additives] The resin composition (M) may further contain various additives within a range that does not impair the heat ray shielding property, low colorability, and total light transmittance in the visible light region. Specific examples of the additives include a release agent, a lubricant, a plasticizer, an antioxidant, an antistatic agent, a light stabilizer, an ultraviolet absorber, a flame retardant, a flame retardant assistant, a polymerization inhibitor, a filler, a pigment, a dye, a silane coupling agent, a leveling agent, an antifoaming agent, a fluorescent agent, and a chain transfer agent.

[0026] <Resin molded body> The resin molded article according to the present invention contains the above-mentioned resin composition (M) according to the present invention, and therefore has excellent blueness and diffusibility when illuminated. The resin molded article according to the present invention can be obtained by molding the resin composition according to the present invention.

[0027] In the resin molded body according to one embodiment of the present invention, the total light transmittance measured in the wavelength range of 380 nm to 780 nm according to JIS K7361-1 (Plastics-Test method for total light transmittance of transparent materials-Part 1: Single beam method) is preferably 71.7% to 90%. The total light transmittance is an index representing transparency, and a resin molded body having a total light transmittance of 71.7% or more has excellent transparency and is easy to suppress whiteness when illuminated. Moreover, if the total light transmittance is 90% or less, the resin molded body has excellent blueness when illuminated. The total light transmittance of the resin molded body is more preferably 72.0% or more, and even more preferably 72.5% or more. Moreover, the total light transmittance of the resin molded body is more preferably 89% or less.

[0028] As a method for controlling the total light transmittance of the resin molded product to be within the above range, for example, the refractive index n A and the refractive index n of the acrylic particles (Z) Z The type or amount of the (meth)acrylic (co)polymer (X) and the acrylic particles (Z) may be controlled so that the difference in refractive index between the (X) and the acrylic particles (Z) is 0.2 or less.

[0029] In addition, in the resin molded product according to one embodiment of the present invention, the haze measured in the wavelength range of 380 nm to 780 nm according to JIS K7136 (Method of determining haze of plastic transparent materials) is preferably 20% to 90%. Haze is also called cloudiness or turbidity, and is an index showing the degree of light diffusion. A resin molded product having a haze of 90% or less has excellent transparency and can be suitably used for applications requiring transparency, such as blue sky lighting.

[0030] The haze of the resin molded product can be controlled within the above range by, for example, adjusting the refractive index n A and the refractive index n of the acrylic particles (Z) Z The type or amount of the (meth)acrylic (co)polymer (X) and the acrylic particles (Z) may be controlled so that the difference in refractive index between the (X) and the acrylic particles (Z) is 0.2 or less.

[0031] <Method for producing resin composition (M) and resin molded product> The method for producing the resin composition (M) according to the present invention includes a method of polymerizing the polymerizable composition (M2) as a raw material. The polymerizable composition (M2) is one embodiment of the raw material for obtaining the resin composition (M) according to the present invention, and is a composition containing at least the raw material composition (M1) described below, a radical polymerization initiator, the nanoparticles (Y), and the acrylic particles (Z). The method for producing the resin molded product according to the present invention includes a step of molding the resin composition (M) according to the present invention.

[0032] [Polymerization method] Examples of the polymerization method for the polymerizable composition (M2) include bulk polymerization, suspension polymerization, emulsion polymerization, and dispersion polymerization. Among these, the bulk polymerization is preferred from the viewpoint of productivity, and among the bulk polymerization methods, the cast polymerization is more preferred.

[0033] Examples of the cast polymerization method include the cell casting method and the continuous casting method described below. When obtaining a resin molded product having a plate-like shape, a space formed by two opposing glass or metal plates (SUS plates) and a gasket such as a soft resin tube disposed on the edge of the two plates is used as a mold. Next, a polymerizable composition (M2) (which may contain a syrup described later) is injected into the mold and heated and polymerized to complete the polymerization, thereby obtaining a resin composition (M). Then, a resin molded product that is a molded product of the resin composition (M) is taken out from the mold (cell casting method). Alternatively, a space formed by two stainless steel endless belts running in the same direction at the same speed and facing each other with a certain distance between them and gaskets such as soft resin tubes arranged on both sides of the endless belts is used as a mold. Next, a polymerizable composition (M2) (which may contain a syrup described later) is continuously injected into the mold from one end of the endless belts, and polymerization is completed by heating and polymerization treatment to obtain a resin composition (M). Then, a resin molded product, which is a molded product of the resin composition (M), is continuously taken out from the other end of the endless belts (continuous casting method). By appropriately adjusting the gap between the mold voids by adjusting the thickness (diameter) of the gasket, a resin molded product having a desired thickness can be obtained. The thickness of the resin molded product is usually set in the range of 0.1 mm to 50 mm.

[0034] [Polymerizable composition (M2)] As described above, the polymerizable composition (M2) in one embodiment of the present invention contains at least the raw material composition (M1), a radical polymerization initiator, the nanoparticles (Y), and the acrylic particles (Z).

[0035] (Raw material composition (M1)) The raw material composition (M1) is a constituent of the polymerizable composition (M2) and is also a raw material component of the (meth)acrylic (co)polymer (X). That is, the raw material composition (M1) is a composition consisting of methyl acrylate alone, a composition consisting of methyl methacrylate alone, or a composition containing methyl (meth)acrylate and one or more vinyl monomers. As the vinyl monomer, the above-mentioned can be used. The content ratio of methyl (meth)acrylate and vinyl monomer in the raw material composition (M1) is not particularly limited. For example, it may be appropriately set so that the finally obtained (meth)acrylic (co)polymer (X) contains 50% by mass or more and 100% by mass or less of methyl (meth)acrylate and 0% by mass or more and 50% by mass or less of the vinyl monomer, with the total mass of the (meth)acrylic (co)polymer (X) being 100% by mass.

[0036] From the viewpoints of optical properties, mechanical properties, heat resistance, and transparency, the raw material composition (M1) is preferably a composition containing 50 mass% or more of methyl methacrylate, more preferably a composition containing 60 mass% or more of methyl methacrylate, and even more preferably a composition containing 70 mass% or more of methyl methacrylate.

[0037] As described above, the raw material composition (M1) is a composition composed of monomers that are raw materials for the (meth)acrylic (co)polymer (X), but may contain a polymer containing methyl methacrylate. Specifically, the raw material composition (M1) may contain a polymer (a) described later in advance. When the raw material composition (M1) contains the polymer (a), the polymerizable composition (M2) becomes a viscous liquid. As a result, it is possible to shorten the polymerization time and improve the productivity. In the present invention, the component of the raw material composition (M1) containing the monomer composition and the polymer (a) is called "syrup". Examples of methods for obtaining the syrup include a method of dissolving the polymer (a) in the raw material composition (M1), or a method of adding a known radical polymerization initiator to the raw material composition (M1) and polymerizing a part of the raw material composition (M1) in advance to obtain the polymer (a).

[0038] Specifically, the polymerizable composition (M2) containing a syrup, which is one embodiment of the polymerizable composition (M2), may be a composition containing the following polymer (a) and the following monomer composition (m). Polymer (a): A polymer containing 50% by mass or more and less than 100% by mass of methyl methacrylate units and more than 0% by mass and 50% by mass or less of the one or more vinyl monomers, relative to the total mass of polymer (a), or a polymer consisting of 100% by mass of methyl methacrylate units. Monomer composition (m): a monomer composition comprising, relative to the total mass of the monomer composition (m), 50 mass% or more and less than 100 mass% of methyl methacrylate and more than 0 mass% and 50 mass% or less of the one or more vinyl monomers, or a monomer composition consisting of 100 mass% methyl methacrylate.

[0039] (Radical polymerization initiator) In the reaction of polymerizing the polymerizable composition (M2) to obtain the resin composition (M), a radical polymerization initiator may be used. Examples of the radical polymerization initiator include known azo compounds such as 2,2'-azobis(isobutyronitrile) and 2,2'-azobis(2,4-dimethylvaleronitrile); and known organic peroxides such as t-hexyl peroxypivalate, benzoyl peroxide, and lauroyl peroxide. These may be used alone or in combination of two or more. If necessary, known polymerization accelerators such as amines and mercaptans may be used in combination with the radical polymerization initiator. The content of the radical polymerization initiator in the polymerizable composition (M2) is not particularly limited, and can be appropriately set by a person skilled in the art according to a well-known technique. The content of the radical polymerization initiator is usually 0.01 parts by mass to 0.5 parts by mass with respect to 100 parts by mass of the raw material composition (M1).

[0040] The polymerization temperature when polymerizing the polymerizable composition (M2) is not particularly limited, and can be appropriately set by a person skilled in the art according to well-known techniques. The polymerization temperature is usually appropriately set in the range of 20°C to 150°C depending on the type of radical polymerization initiator used. In addition, the polymerization of the polymerizable composition (M2) can be carried out under multi-stage temperature conditions as necessary.

[0041] (Nanoparticles (Y)) In the production of the resin composition (M), the content of the nanoparticles (Y) contained in the polymerizable composition (M2) is not particularly limited. However, similar to the content of the nanoparticles (Y) relative to the (meth)acrylic (co)polymer (X), it is preferably 0.01 parts by mass to 0.1 parts by mass relative to 100 parts by mass of the raw material composition (M1). The more preferred range is also similar to the content of the nanoparticles (Y) relative to the (meth)acrylic (co)polymer (X).

[0042] (Acrylic particles (Z)) The content of the acrylic particles (Z) contained in the polymerizable composition (M2) is not particularly limited. However, like the content of the acrylic particles (Z) relative to the (meth)acrylic (co)polymer (X), the content is preferably 0.01 to 5 parts by mass, more preferably 0.05 to 4 parts by mass, further preferably 0.07 to 3 parts by mass, and particularly preferably 0.1 to 2 parts by mass relative to 100 parts by mass of the raw material composition (M1).

[0043] The nanoparticles (Y) and the acrylic particles (Z) may be mixed directly with the raw material composition (M1). Alternatively, the nanoparticles (Y) and the acrylic particles (Z) may be dispersed in a suitable organic solvent in advance to prepare a dispersion, and then the dispersion may be mixed with the raw material composition (M1). EXAMPLES

[0044] The present invention will be described in more detail below with reference to examples. However, the present invention is not limited to the following examples as long as it does not depart from the gist of the present invention.

[0045] [Abbreviations and details of each component] The abbreviations and details of each component used in the examples and comparative examples are as follows. MMA: Methyl methacrylate (Mitsubishi Chemical Corporation) HPP: t-Hexyl peroxypivalate (NOF Corporation) Nanoparticle (Y)-containing sol: HTD-711Z (product name, manufactured by Teika Co., Ltd., IPA dispersion, ZnO2 particle concentration: 45% by mass, particle diameter: 20 to 30 nm) Nanoparticle (Y)-containing sol: HTD-710T (product name, manufactured by Teika Co., Ltd., IPA dispersion, TiO2 particle concentration: 40% by mass, particle diameter: 15 to 50 nm) Acrylic particles (Z): MBX-5 (trade name, manufactured by Sekisui Plastics Co., Ltd., refractive index: 1.495, average particle size: 5 μm) Acrylic particles (Z): MBP-8 (trade name, manufactured by Sekisui Plastics Co., Ltd., hollow particles, average particle size: 8 μm) Silicone particles: Tospearl 120 (product name, manufactured by Momentive Performance Materials Japan, LLC, average particle size: 2 μm) Silicone particles: Tospearl 145 (product name, manufactured by Momentive Performance Materials Japan, LLC, average particle size: 4.5 μm)

[0046] [Evaluation method] The evaluations in the examples and comparative examples were carried out by the following methods.

[0047] (1) Total light transmittance The total light transmittance (the ratio of the total transmitted light flux to the equilibrium incident light flux), which is an index of transparency, was measured as follows using an integrating sphere light transmittance measuring device (model name: NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.). In accordance with JIS K7361-1, parallel light was incident on a test piece of a resin molded body (length: 50 mm x width: 50 mm, thickness: 5 mm), and the total light transmittance (Tt) was measured in the wavelength range of 380 nm to 780 nm. Three test pieces were used, and one measurement was performed for each test piece, and the average value was taken as the total light transmittance (%).

[0048] (2) Haze Haze (the ratio of diffuse transmitted light flux to equilibrium incident light flux), which is an index of diffusivity, was measured as follows using an integrating sphere light transmittance measuring device (model name: NDH4000, manufactured by Nippon Denshoku Industries Co., Ltd.). In accordance with JIS K7136, parallel light was incident on a test piece of a resin molded body (length: 50 mm x width: 50 mm, thickness: 5 mm), and the haze was measured in the wavelength range of 380 nm to 780 nm. Three test pieces were used, and one measurement was performed for each test piece, and the average value was taken as the haze (%).

[0049] (3) Blueness and diffusion A black box as shown in FIG. 1 was prepared. As shown in FIG. 2, 15 LED light sources A were installed on one side of the bottom of the black box, and a test piece of resin molded body B (length: 300 mm × width: 600 mm, thickness: 5 mm) was installed on one side of the upper part of the black box. FIG. 3 is a cross-sectional view of the black box shown in FIG. 2 when observed from the front side of the paper. As shown in FIG. 3, the transparency of the light source at the measurement point X where the angle between the LED light source A and the test piece of the resin molded body B is 30° was visually evaluated and used as an index of diffusivity. In addition, the blueness of the resin molded body at the measurement point X when the LED light source A was turned on was visually evaluated. The measurement point X exists in a line in the depth direction of the paper of the black box shown in FIG. 2 (direction D in FIG. 1), and the blueness and diffusivity were evaluated on the line where the measurement point X exists. The blueness and diffusivity were evaluated according to the following criteria (ranks). (Evaluation Criteria) AA: Excellent blueness or diffusion A: Excellent blueness or diffusion B: Lack of blueness or diffusion

[0050] [Example 1] (1) Syrup production 100 parts by mass of MMA as a monomer composition (m) was supplied to a reactor (polymerization kettle) equipped with a cooling tube, a thermometer, and a stirrer, and after stirring for 15 minutes while bubbling nitrogen gas, the temperature of the reactor was raised with stirring until the internal temperature of the reactor reached 60°C. Next, 0.1 parts by mass of 2,2'-azobis(2,4-dimethylvaleronitrile) was added to the reactor as a radical polymerization initiator, and the mixture was heated to 100°C while stirring, and then maintained for 13 minutes. Next, the reactor was cooled until the internal temperature reached room temperature to obtain a syrup. The content of polymer (a) in the syrup was 20% by mass.

[0051] (2) Casting polymerization To 94 parts by mass of the above syrup, 6 parts by mass of methyl methacrylate, 0.1 part by mass of HTD-711Z as a sol containing nanoparticles (Y) (ZnO2: 0.045 parts by mass), 0.5 parts by mass of MBX-5 as an acrylic particle (Z), and 0.4 parts by mass of HPP as a radical polymerization initiator were added and dissolved with stirring to obtain a polymerizable composition (M2). A soft resin gasket was placed on the ends of two SUS plates arranged opposite each other so that the gap between the two SUS plates was constant, and a mold was prepared. Next, the polymerizable composition (M2) was poured into the mold, sealed with a soft resin gasket, heated to 80°C, and held for 40 minutes. The temperature was further raised to 130°C and held for 30 minutes to polymerize the polymerizable composition (M2), thereby obtaining a resin composition (M). After that, the mold was cooled to room temperature, and the SUS plate was removed to obtain a plate-shaped resin molded body having a thickness of 5 mm. The obtained resin molded body was subjected to measurement of total light transmittance, measurement of haze, and evaluation of blueness and diffusion. The evaluation results are shown in Table 1.

[0052] [Examples 2 to 8] A resin composition (M) and a resin molded product were produced in the same manner as in Example 1, except that the composition of the polymerizable composition (M2) was changed as shown in Table 1. The total light transmittance and haze of the obtained resin molded product were measured, and the blueness and diffusibility were evaluated. The evaluation results are shown in Table 1.

[0053] [Comparative Examples 1 to 2] Except for not using the acrylic particles (Z), a resin composition (M) and a resin molded product were produced in the same manner as in Example 1 or 4, and the total light transmittance and haze of the resulting resin molded product were measured, and the blueness and diffusivity were evaluated. The evaluation results are shown in Table 1.

[0054] [Comparative Examples 3 to 4] A resin composition (M) and a resin molded product were produced in the same manner as in Example 1, except that, as particles having an average particle size of 1 μm or more and a crosslinked structure, silicone particles, Tospearl 120 or 145, were used in place of the acrylic particles (Z) in the compositions shown in Table 1. The total light transmittance and haze of the obtained resin molded product were measured, and the blueness and diffusivity were evaluated. The evaluation results are shown in Table 1.

[0055] [Table 1]

[0056] From Table 1, we can see the following: The resin moldings according to Examples 1 to 8 contained the (meth)acrylic (co)polymer (X), nanoparticles (Y), and the acrylic particles (Z) having an average particle diameter of 1 μm or more and a crosslinked structure, and therefore exhibited excellent blueness and diffusibility when illuminated. On the other hand, the resin molded products according to Comparative Examples 1 and 2, which do not contain acrylic particles (Z), had low haze or insufficient transparency and poor diffusibility. The resin molded products according to Comparative Examples 3 and 4, which contain silicone particles as particles having an average particle size of 1 μm or more and have a crosslinked structure, had insufficient transparency and were poor in blueness when illuminated. The resin molded product according to Comparative Example 4 also had poor diffusibility. [Industrial Applicability]

[0057] INDUSTRIAL APPLICABILITY The resin molded article according to the present invention is excellent in optical properties, blueness when illuminated, and diffusion property, and can be suitably used for blue sky illumination. [Explanation of symbols]

[0058] A LED light source B Resin molded body X Measurement point

Claims

1. A (meth)acrylic (co)polymer (X); Nanoparticles (Y), acrylic particles (Z) having an average particle size of 1 μm or more and a crosslinked structure; A resin composition comprising:

2. The resin composition according to claim 1, comprising 0.01 to 0.1 parts by mass of the nanoparticles (Y) relative to 100 parts by mass of the (meth)acrylic (co)polymer (X).

3. The resin composition according to claim 1, comprising 0.01 to 5 parts by mass of the acrylic particles (Z) relative to 100 parts by mass of the (meth)acrylic (co)polymer (X).

4. The resin composition according to claim 1, wherein the average particle size of the acrylic particles (Z) is 1 μm to 50 μm.

5. The resin composition according to claim 1 , wherein the acrylic particles (Z) are hollow particles.

6. The resin composition according to claim 1, wherein the nanoparticles (Y) have a particle diameter of 10 nm to 80 nm.

7. A resin molded product comprising the resin composition according to any one of claims 1 to 6.

8. The resin molded article according to claim 7, having a total light transmittance of 71.7% to 90% as measured in a wavelength range of 380 nm to 780 nm according to JIS K7361-1, and a haze of 20% to 90% as measured in a wavelength range of 380 nm to 780 nm according to JIS K7136.

9. A method for producing a resin molded product, comprising a step of molding the resin composition according to any one of claims 1 to 6.

Citation Information

Patent Citations

  • Optical sky-sun diffuser

    WO2009156348A1

  • Diffusion body and illumination device

    WO2020240933A1