Silane-cross-linked cured product of liquid silane-grafted olefin composition and method for producing the same

The liquid silane-grafted olefin composition addresses the inefficiencies of conventional crosslinkable compositions by enabling a crosslinkable liquid state without heating, resulting in a silane-crosslinked cured product with improved workability and appearance.

JP2024140319AActive Publication Date: 2024-10-10FURUKAWA ELECTRIC CO LTD

Patent Information

Application Number
JP2023051409
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
2043-03-28

AI Technical Summary

Technical Problem

Conventional crosslinkable compositions, whether solid or liquid, require heating processes and special crosslinking devices, leading to poor workability, increased costs, and potential discoloration, which affects the appearance and mechanical properties of molded products.

Method used

A liquid silane-grafted olefin composition is developed by grafting a specific amount of silane coupling agent onto a liquid olefin polymer, allowing for a crosslinkable liquid state without heating during molding and using a silanol condensation catalyst for rapid crosslinking, eliminating the need for special devices and ensuring excellent workability and appearance.

Benefits of technology

The solution provides a silane-crosslinked cured product with excellent appearance and mechanical properties, achieved through a process that maintains a liquid state during molding and final crosslinking, reducing manufacturing costs and improving workability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140319000001
    Figure 2024140319000001
Patent Text Reader

Abstract

To provide: a liquid silane-grafted olefin composition free from discoloration and having excellent workability, which does not require a heating step or a heating device during molding and, while not requiring a cross-linking device such as a cross-linking tube and the like during the final cross-linking reaction, can make the final cross-linking reaction proceed quickly to produce a silane-cross-linked cured product with excellent appearance; and a silane-cross-linked cured product thereof; and methods for producing these.SOLUTION: Provided are: a liquid silane-grafted olefin composition obtained by grafting 3 to 30 pts.mass of a silane coupling agent to 100 pts.mass of a liquid olefin polymer: a silane-cross-linked cured product thereof; and a production method comprising a step of reacting 100 pts.mass of the liquid olefin polymer with 3 to 30 pts.mass of a silane coupling agent in the presence of 0.1 to 2 pts.mass of an organic peroxide at a temperature of 50 to 200°C.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid silane-grafted olefin composition, a silane-crosslinked cured product thereof, and methods for producing them. [Background technology]

[0002] TECHNICAL FIELD Various resin or rubber molded articles are used as covering layers (insulators, sheaths, etc.) provided on wiring materials such as insulated wires, cables, cords, optical fiber cores, and optical fiber cords (optical fiber cables) used in the electric and electronic equipment field and the industrial field, and as various molded articles such as packings and sheets. As a material for forming such a molded body, crosslinkable compositions such as crosslinkable resin compositions and crosslinkable rubber compositions are often used. For example, Patent Document 1 proposes a rubber composition (requirements (a-1) to (a-5) are omitted) that contains "a liquid modified ethylene random copolymer (A) and a rubber component (B), and the liquid modified ethylene random copolymer (A) is a copolymer obtained by graft-copolymerizing an unsaturated silane compound component to an ethylene random copolymer (a0)" and satisfies specific requirements (a-1) to (a-5), and also proposes a "molded body obtained by crosslinking the rubber composition". [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent Publication No. 2021-024912 Summary of the Invention [Problem to be solved by the invention]

[0004] As a material for forming the above-mentioned molded body, a solid crosslinkable composition containing a high molecular weight solid polymer (resin or rubber) as a main component is usually used. For example, the rubber composition described in Patent Document 1 contains a liquid modified ethylene random copolymer (A) as a modifier for the rubber composition, but the main component is a rubber component (B), so the composition as a whole is solid. Such a solid crosslinkable composition is heated to a temperature at which it becomes in a molten state, and then molded to carry out a final crosslinking reaction. As described above, a solid crosslinkable composition requires a heating step for plasticization during molding, and therefore it is poor in workability in that it must be handled in a molten state using manufacturing equipment such as an extrusion molding machine or an injection molding machine. Moreover, this also leads to an increase in manufacturing costs. On the other hand, liquid crosslinkable compositions containing low molecular weight polybutadiene and the like are also known as materials for forming the above-mentioned molded bodies. Although such liquid crosslinkable compositions do not need to be heated to a molten state during molding, the final crosslinking reaction needs to be carried out by external forces such as heat and light. Therefore, even liquid crosslinkable compositions still require special crosslinking equipment (e.g., crosslinking tubes, etc.), which is poor in workability and leads to increased manufacturing costs. In addition, liquid crosslinkable compositions may be easily discolored due to uneven mixing conditions, and if a discolored crosslinkable composition is subjected to a final crosslinking reaction (silanol condensation reaction), the appearance of the resulting crosslinked cured product will be impaired. Furthermore, the unevenness of the mixing condition also causes a problem of reduced mechanical properties of the molded body after the final crosslinking reaction.

[0005] As described above, in conventional crosslinkable compositions as materials for forming molded bodies, whether they are solid compositions or liquid compositions, a heating step and a heating device or a special crosslinking device are required during molding or the final crosslinking reaction, which results in poor workability and in failure to obtain a crosslinked cured product with a good appearance. However, Patent Document 1 does not consider such points of view.

[0006] The present invention aims to provide a liquid silane-grafted olefin composition that does not require a heating step or a heating device during molding, and does not require a crosslinking device such as a crosslinking tube during the final crosslinking reaction, but allows the final crosslinking reaction to proceed quickly, and is excellent in workability and does not discolor, and a silane-crosslinked cured product (silanol condensation cured product) of the liquid silane-grafted olefin composition as a crosslinked molded product with excellent appearance. Another objective of the present invention is to provide a method for producing the liquid silane-grafted olefin composition and the silane-crosslinked cured product. [Means for solving the problem]

[0007] The present inventors have intensively studied materials for forming molded bodies, and have found that when a specific amount of a silane coupling agent is grafted to a liquid olefin polymer, a liquid silane-grafted olefin composition can be prepared while suppressing discoloration and the like, and that by making this liquid silane-grafted olefin composition a silane-crosslinkable composition and then making it a crosslinkable liquid composition that maintains a liquid state as a whole, no heating step or heating device is required during molding, and excellent workability can be achieved. Moreover, it has been found that this crosslinkable liquid composition has excellent workability in the presence of a silanol condensation catalyst, that is, while eliminating the need for a crosslinking device such as a crosslinking tube, the final crosslinking reaction (silanol condensation reaction) proceeds quickly under mild conditions and with simple operations, resulting in a solid silane-crosslinked cured product with excellent appearance. In this way, the present inventors have found that the above-mentioned crosslinkable liquid composition can solve both the problems of conventional solid compositions and liquid compositions at once. Based on this knowledge, the present inventors have further researched and have come up with the present invention.

[0008] That is, the object of the present invention has been achieved by the following means. <1> A liquid silane-grafted olefin composition obtained by grafting 100 parts by mass of a liquid olefin polymer with 3 to 30 parts by mass of a silane coupling agent having a site capable of undergoing a grafting reaction with said liquid olefin polymer. <2> Kinematic viscosity at 100°C is 1,000mm 2 / s or less, <1> 2. The liquid silane-grafted olefin composition according to claim 1 . <3> The liquid olefin polymer is reacted with 100 parts by mass of the liquid olefin polymer and 3 to 30 parts by mass of the silane coupling agent in the presence of 0.1 to 2 parts by mass of an organic peroxide at a temperature of 50 to 200° C. <1> or <2> 2. The liquid silane-grafted olefin composition according to claim 1 . <4> The silane coupling agent and the organic peroxide are added to the liquid olefin polymer having a temperature of 50 to 200°C, and the liquid olefin polymer is reacted with the silane coupling agent to obtain a polymerizable composition. <3> 2. The liquid silane-grafted olefin composition according to claim 1 . <5> the above <1> ~ <4> 2. A silane-crosslinked cured product of the liquid silane-grafted olefin composition according to claim 1. <6> 100 parts by mass of a liquid olefin polymer is reacted with 3 to 30 parts by mass of a silane coupling agent having a site capable of undergoing a grafting reaction with the liquid olefin polymer in the presence of 0.1 to 2 parts by mass of an organic peroxide at a temperature of 50 to 200° C.; <1> ~ <4> 13. A method for producing the liquid silane-grafted olefin composition according to claim 12. <7> The silane coupling agent and the organic peroxide are added to the liquid olefin polymer having a temperature of 50 to 200° C. to react the liquid olefin polymer with the silane coupling agent. <6> 2. A method for producing the liquid silane-grafted olefin composition according to claim 1 . <8> The reaction is carried out in a stirred closed reactor. <6> or <7> 2. A method for producing the liquid silane-grafted olefin composition according to claim 1 . <9> the above <6> ~ <8> 1. A method for producing a silane crosslinking curing, comprising contacting the liquid silane-grafted olefin composition obtained by the method for producing a liquid silane-grafted olefin composition according to any one of claims 1 to 7 with water in the presence of a silanol condensation catalyst to produce a silane crosslinking curing of the liquid silane-grafted olefin composition. Effect of the Invention

[0009] The present invention can provide a liquid silane-grafted olefin composition that does not require a heating step or a heating device during molding, and does not require a crosslinking device such as a crosslinking tube during the final crosslinking reaction, but allows the final crosslinking reaction to proceed quickly while producing a silane-crosslinked cured product with excellent appearance, and that is free from discoloration and has excellent workability, as well as a silane-crosslinked cured product of the liquid silane-grafted olefin composition as a crosslinked molded product with excellent appearance.The present invention can also provide a method for producing the liquid silane-grafted olefin composition and the silane-crosslinked cured product thereof. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] In the present invention, when the content, physical properties, etc. of a component are described by showing a numerical range, and when the upper limit and lower limit of the numerical range are described separately, any of the upper limit and lower limit can be appropriately combined to form a specific numerical range. On the other hand, when multiple numerical ranges expressed using "~" are set and described, the upper limit and lower limit forming the numerical range are not limited to the specific combination described before and after "~" as a specific numerical range, and can be a numerical range obtained by appropriately combining the upper limit and lower limit of each numerical range. In addition, in the present invention, a numerical range expressed using "~" means a range including the numerical values ​​described before and after "~" as the upper limit and lower limit.

[0011] [Liquid silane-grafted olefin composition] The liquid silane-grafted olefin composition of the present invention contains a liquid silane-grafted olefin, which will be described later, and the composition as a whole maintains a liquid state. In the present invention, "liquid" means to be liquid at room temperature (25°C) and normal pressure (1 atm), i.e., to be liquid, and specifically means that the (absolute) viscosity measured with a Brookfield viscometer at room temperature and normal pressure is 100 Pa s or less. In the present invention, the viscosity at room temperature and normal pressure is preferably 3 Pa s or less. On the other hand, in the present invention, the term "solid" refers to a state in which the material does not exhibit fluidity at room temperature and normal pressure, and for example, refers to a state in which the (absolute) viscosity measured with a Brookfield viscometer at room temperature and normal pressure is 10,000 Pa s or more.

[0012] The liquid silane-grafted olefin composition is a composition obtained by grafting 3 to 30 parts by mass of a silane coupling agent having a site for grafting reaction to 100 parts by mass of a liquid olefin polymer. The liquid silane-grafted olefin composition is a silane-crosslinkable liquid composition containing a liquid silane-grafted olefin in which a silane coupling agent is grafted to a liquid olefin polymer. The liquid silane-grafted olefin and the liquid silane-grafted olefin composition are preferably prepared by the method for producing the liquid silane-grafted olefin composition of the present invention described below.

[0013] The liquid silane-grafted olefin composition of the present invention has a kinematic viscosity of 1,000 mm at 100°C under normal pressure. 2 / s or less is preferable, and 10 mm 2 When the liquid silane-grafted olefin composition has a kinetic viscosity in the above range, the composition can be easily removed from a vessel after the reaction and the efficiency of purification by separation can be improved.

[0014] The liquid silane-grafted olefin composition of the present invention is liquid under normal temperature and pressure conditions, and as described below, when it is brought into contact with water by a silane crosslinking method, it hardens to become a solid composition (silane-crosslinked cured product). Therefore, this liquid silane-grafted olefin composition utilizes its liquid properties to eliminate the need for a heating step and heating device during molding, and exhibits excellent workability. In addition, the liquid silane-grafted olefin composition of the present invention has high workability in that it is brought into contact with water under mild conditions without the need for an excessive heating step at high temperatures using a crosslinking device such as a crosslinking tube, while the final crosslinking reaction (silanol condensation reaction) proceeds quickly to build a sufficient crosslinked structure, resulting in a crosslinked cured product with excellent appearance.

[0015] [Silane-crosslinked cured product of liquid silane-grafted olefin composition] The silane crosslinked cured product of the liquid silane grafted olefin composition of the present invention (hereinafter referred to as the silane crosslinked cured product of the present invention) is a crosslinked cured product (silanol condensation cured product) obtained by crosslinking the silanol condensation reaction sites of the liquid silane grafted olefin composition of the present invention, particularly the silane coupling agent of the liquid silane grafted olefin, of the silanol condensation capable reaction site. This silane crosslinked cured product contains a crosslinked olefin polymer obtained by crosslinking a liquid olefin polymer via a silane coupling agent. The liquid silane grafted olefin composition of the present invention becomes a solid composition (crosslinked cured product) from a liquid composition (liquid composition) by contacting with water in the presence of a silanol condensation catalyst by a silane crosslinking method. The run-crosslinked cured product of the present invention is usually a molded product, but may be in a shapeless (unmolded) bulk state.

[0016] Each component used in the present invention will be described below. Each of the components may be used alone or in combination of two or more.

[0017] <Liquid olefin polymer> The liquid olefin polymer may be any (co)polymer of an olefin compound that is liquid at room temperature and normal pressure, and any known (co)polymer may be used without any particular limitation. In the present invention, the olefin compound refers to a compound having an ethylenically unsaturated group, and includes alkene compounds having one ethylenically unsaturated group in the molecule, such as ethylene and propylene, as well as polyene compounds having two or more ethylenically unsaturated groups in the molecule. Examples of the polyene compound include conjugated diene compounds such as butadiene and isoprene.

[0018] The liquid olefin polymer preferably has a site capable of undergoing graft reaction with a silane coupling agent (described later) in the main chain or at its terminal by radicals generated from an organic peroxide. Examples of the site capable of undergoing graft reaction include an unsaturated bond site in a carbon chain and a carbon atom having a hydrogen atom.

[0019] The liquid olefin polymer is not particularly limited, and examples thereof include ethylene random copolymers, liquid diene polymers, organic mineral oils, and further hydrogenated or modified products thereof. Examples of the liquid diene polymers include liquid butadiene polymers, liquid isoprene polymers, and liquid styrene-butadiene copolymers. Among these, ethylene random copolymers, liquid butadiene polymers, and liquid isoprene polymers are preferred. Examples of the modified products include acid modified products.

[0020] (Ethylene random copolymer) Examples of ethylene-based random copolymers include copolymers having a component derived from ethylene and a component derived from an α-olefin. The α-olefin is not particularly limited, but is preferably an α-olefin having 3 to 20 carbon atoms, more preferably an α-olefin having 3 to 10 carbon atoms, and even more preferably propylene. Examples of the α-olefin include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-decene, 1-undecene, 1-dodecene, 1-tridecene, 1-tetradecene, 1-pentadecene, 1-hexadecene, 1-heptadecene, 1-octadecene, 1-nonadecene, and 1-eicosene. The ethylene random copolymer may have one or more constituent components derived from an α-olefin.

[0021] The ethylene random copolymer may have a constituent derived from at least one other monomer selected from a polar group-containing compound, an aromatic vinyl compound, and a cyclic olefin.

[0022] The polar group-containing compound is not particularly limited, and examples thereof include α,β-unsaturated carboxylic acid compounds such as acrylic acid, methacrylic acid, fumaric acid, maleic anhydride, and metal salt compounds thereof such as sodium salts, α,β-unsaturated carboxylic acid ester compounds such as methyl acrylate, ethyl acrylate, n-propyl acrylate, methyl methacrylate, ethyl methacrylate, n-propyl methacrylate, and other vinyl ester compounds, such as vinyl acetate and vinyl propionate, and unsaturated glycidyl compounds such as glycidyl acrylate and glycidyl methacrylate. The aromatic vinyl compound is not particularly limited, and examples thereof include styrene, o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, methoxystyrene, vinylbenzoic acid, methyl vinylbenzoate, vinylbenzyl acetate, hydroxystyrene, p-chlorostyrene, divinylbenzene, α-methylstyrene, and allylbenzene. The cyclic olefin is not particularly limited, and is preferably a cyclic olefin having 3 to 30 carbon atoms, more preferably a cyclic olefin having 3 to 20 carbon atoms. Examples of the cyclic olefin include cyclopentene, cycloheptene, norbornene, 5-methyl-2-norbornene, and tetracyclododecene.

[0023] The content of components derived from ethylene relative to all components in the ethylene random copolymer (also referred to as ethylene content) is not particularly limited and is appropriately set in consideration of the range in which the crystallinity and liquid state of the ethylene random copolymer can be maintained. The ethylene content is, for example, preferably 30 to 90 mol%, more preferably 30 to 80 mol%, further preferably 40 to 75 mol%, and particularly preferably 40 to 60 mol%. The ethylene content can be determined by the method described in Patent Document 1. The content of the constituent component derived from an α-olefin relative to all the constituent components in the ethylene random copolymer (also referred to as the α-olefin content) is not particularly limited and is appropriately set in consideration of the ethylene content, etc. The content of components derived from other monomers in the ethylene random copolymer is not particularly limited, and can be, for example, 20 parts by mass or less, preferably 10 parts by mass or less, per 100 parts by mass of the total of the components derived from ethylene and the components derived from α-olefins.

[0024] The molecular weight (number average molecular weight, weight average molecular weight, etc.) of the ethylene random copolymer is not particularly limited and may be appropriately set within a range in which the copolymer can be kept liquid. The molecular weight distribution of the ethylene random copolymer is also not particularly limited and may be appropriately set.

[0025] As the ethylene random copolymer, a commercially available product may be used, or it may be appropriately synthesized. An example of a commercially available product is LUCANT (product name, manufactured by Mitsui Chemicals, Inc., ethylene-α-olefin oligomer). When synthesizing an ethylene random copolymer, ethylene and an α-olefin can be polymerized by a known polymerization method. For example, the contents described in Patent Document 1 can be appropriately referred to, and the contents thereof are incorporated as a part of the present specification as they are.

[0026] (Liquid diene polymer) The liquid diene polymer is not particularly limited, but examples thereof include polymers obtained by polymerizing at least a conjugated diene compound, and, if necessary, by copolymerizing both a conjugated diene compound and a vinyl-substituted aromatic compound. The liquid diene polymer may have one or more types of constituents derived from a conjugated diene compound. In addition, the liquid diene polymer may not have a constituent component derived from a vinyl-substituted aromatic compound, and when it has a constituent component derived from a vinyl-substituted aromatic compound, it may have one or more types.

[0027] The conjugated diene compound is not particularly limited as long as it is a polymerizable monomer compound, and is preferably a conjugated diene compound having 4 to 12 carbon atoms, and more preferably a conjugated diene compound having 4 to 8 carbon atoms. Examples of such conjugated diene compounds include 1,3-butadiene, isoprene, 2,3-dimethyl-1,3-butadiene, 1,3-pentadiene, 3-methyl-1,3-pentadiene, 1,3-hexadiene, and 1,3-heptadiene. Among these, 1,3-butadiene and isoprene are preferred from the viewpoint of industrial availability. The vinyl-substituted aromatic compound is not particularly limited as long as it is a monomer that can be copolymerized with conjugated diene compound, and is preferably a monovinyl aromatic compound.As the monovinyl aromatic compound, for example, styrene, p-methylstyrene, α-methylstyrene, vinylethylbenzene, vinylxylene, vinylnaphthalene, diphenylethylene can be mentioned, and from the viewpoint of industrial availability, styrene is preferred.

[0028] As the liquid diene polymer, a homopolymer of 1,3-butadiene, a homopolymer of isoprene, a copolymer of 1,3-butadiene and styrene (SBR), a copolymer of isoprene and styrene, and hydrogenated products thereof are preferable.

[0029] In the homopolymer of 1,3-butadiene and the homopolymer of isoprene, the amount of vinyl groups in the constituent components derived from 1,3-butadiene or isoprene is not particularly limited and may be set appropriately.

[0030] The copolymer of 1,3-butadiene and styrene may be a random copolymer or a block copolymer, with the random copolymer being preferred. In the copolymer of 1,3-butadiene and styrene, the content of the component derived from styrene is not particularly limited, but for example, in 100% by mass of all the components of the copolymer, it is preferably more than 0% by mass and 50% by mass or less, and more preferably more than 0% by mass and 20% by mass or less. In addition, in the copolymer of 1,3-butadiene and styrene, the amount of vinyl groups in the component derived from 1,3-butadiene is not particularly limited and is set appropriately.

[0031] The molecular weight (number average molecular weight, weight average molecular weight, etc.) of the liquid diene polymer is not particularly limited and may be appropriately set within a range in which the liquid state can be maintained. The molecular weight distribution of the liquid diene polymer is also not particularly limited and may be appropriately set.

[0032] As the liquid diene polymer, a commercially available product may be used, or it may be appropriately synthesized. Examples of commercially available products include LBR (product name, manufactured by Kuraray Co., Ltd., liquid butadiene), LIR (product name, manufactured by Kuraray Co., Ltd., liquid isoprene), and LSBR (product name, manufactured by Kuraray Co., Ltd., liquid styrene butadiene). When synthesizing the liquid diene polymer, a conjugated diene compound and an appropriate vinyl-substituted aromatic compound can be polymerized by a known polymerization method.

[0033] Examples of the organic mineral oil include those commonly used in resin compositions, such as paraffin-based oils and various other synthetic oils.

[0034] <Silane coupling agent> The silane coupling agent has a grafting site (a functional group such as a group or an ethylenically unsaturated group) that can undergo a grafting reaction with a grafting site of a liquid olefin polymer in the presence of radicals generated by decomposition of an organic peroxide. The silane coupling agent also has a hydrolyzable silyl group (e.g., an alkoxysilyl group) as a silanol condensable reaction site.

[0035] Silane coupling agent is not particularly limited, and includes silane coupling agents that have been used in the silane crosslinking method.Specifically, includes vinyl alkoxy silanes such as vinyl trimethoxy silane, vinyl triethoxy silane, vinyl tributoxy silane, vinyl dimethoxy ethoxy silane, vinyl dimethoxy butoxy silane, vinyl diethoxy butoxy silane, allyl trimethoxy silane, allyl triethoxy silane, vinyl triacetoxy silane, etc., methacryloxy propyl trimethoxy silane, methacryloxy propyl triethoxy silane, methacryloxy propyl methyl dimethoxy silane, etc. Among them, vinyl trimethoxy silane or vinyl triethoxy silane is particularly preferred. The grafting rate of the silane coupling agent to the liquid olefin polymer (the amount of the silane coupling agent grafted and bonded to the liquid olefin polymer through a grafting reaction with the liquid olefin polymer) is not particularly limited, and is within the range achieved by the grafting reaction according to the production method of the liquid silane-grafted olefin composition of the present invention described below.

[0036] <Organic peroxide> The organic peroxide generates radicals by thermal decomposition, and acts as a catalyst to cause a grafting reaction of the silane coupling agent to the liquid olefin polymer by radical reaction. The organic peroxide is not particularly limited, and any organic peroxide that is used in the conventional silane crosslinking method can be used without any particular limitation. Examples of such organic peroxides include those represented by the general formula: R 1 -O-O-R 2 , R 3 -OO-C(=O)R 4 , R 5 C(=O)-OO(C=O)R 6 Preferred are compounds represented by the formula: 1 ~R 6 Each independently represents an alkyl group, an aryl group, or an acyl group. R 1 ~R 6Among these, those in which all are alkyl groups, or those in which one is an alkyl group and the remaining is an acyl group, are preferred.Specific examples include benzoyl peroxide, dicumyl peroxide (DCP), 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexane, and 2,5-dimethyl-2,5-di-(tert-butylperoxy)hexyne-3.

[0037] <Silanol condensation catalyst> In the present invention, the liquid silane-grafted olefin composition may or may not contain a silanol condensation catalyst. The liquid silane-grafted olefin composition that does not contain a silanol condensation catalyst is contacted with the silanol condensation catalyst together with water during the silanol condensation reaction. The silanol condensation catalyst used in the present invention has the function of promoting a silanol condensation reaction (dehydration condensation reaction) in the presence of moisture at the silanol condensable reactive sites of the silane coupling agent grafted onto the liquid olefin polymer. This condensation reaction crosslinks the liquid olefin polymer via the silane coupling agent. Such a silanol condensation catalyst is not particularly limited, and examples thereof include organotin compounds, metal soaps, platinum compounds, etc., and organotin compounds are preferred. Examples of organotin compounds include dibutyltin dilaurate, dioctyltin dilaurate, dibutyltin dioctiate, dibutyltin diacetate, and other organotin compounds. When the liquid silane-grafted olefin composition contains a silanol condensation catalyst, the content of the silanol condensation catalyst in the liquid silane-grafted olefin composition is not particularly limited and may be appropriately determined. For example, the content is preferably 0.0001 to 0.5 parts by mass, more preferably 0.001 to 0.2 parts by mass, per 100 parts by mass of the liquid olefin polymer.

[0038] <Other ingredients> The liquid silane-grafted olefin composition of the present invention may contain, as optional components, components (other components) other than the above-mentioned components. Examples of other components include various components such as additives that are generally used in resin compositions, such as (co)polymers other than liquid olefin polymers, inorganic fillers, flame retardants, flame retardant assistants, antiaging agents (antioxidants), lubricants, crosslinking agents, crosslinking assistants, etc. The contents of other components in the liquid silane-grafted olefin composition are not particularly limited, and may be appropriately set within a range that does not impair the object of the present invention, particularly within a range that does not impair the liquid state.

[0039] [Method for producing liquid silane-grafted olefin composition] The liquid silane-grafted olefin composition of the present invention can be prepared by any suitable method, for example, it can be produced by mixing or melt-mixing the liquid silane-grafted olefin with other components as appropriate. However, it is preferable to produce it by the method for producing the liquid silane-grafted olefin composition of the present invention described below, since it is possible to produce a silane-crosslinked cured product that exhibits excellent appearance by suppressing the occurrence of discoloration during preparation. The method for producing a liquid silane-grafted olefin composition of the present invention (sometimes simply referred to as the method for producing a liquid composition of the present invention) comprises a step of reacting 100 parts by mass of a liquid olefin polymer with 3 to 30 parts by mass of a silane coupling agent having a site that undergoes a grafting reaction with the liquid olefin polymer in the presence of 0.1 to 2 parts by mass of an organic peroxide at a temperature of 50 to 200°C.

[0040] In the liquid composition production method of the present invention, a stirrable reaction apparatus can be used, for example, an open type reaction apparatus or a closed type reaction apparatus (a sealable reaction apparatus). In the present invention, a closed type reaction apparatus is preferred because it can uniformly proceed with the grafting reaction, suppress the occurrence of discoloration or coloring, and produce a liquid silane-grafted olefin composition with a uniform viscosity, and thus produce a silane-crosslinked cured product with excellent appearance. Examples of the reaction apparatus include a general reaction vessel, an autoclave, an autoclave with a stirrer, etc., and a general closed type reaction vessel or an autoclave with a stirrer is preferred.

[0041] In the liquid composition production method of the present invention, the mixing amount (usage amount) of the silane coupling agent is 3 to 30 parts by mass relative to 100 parts by mass of the liquid olefin polymer. When the mixing amount of the silane coupling agent is within the above range, the grafting reaction proceeds uniformly without discoloration, and the silanol condensation reaction proceeds rapidly under mild conditions, making it possible to prepare a liquid silane-grafted olefin composition capable of constructing a sufficient crosslinked structure. The mixing amount of the silane coupling agent is more preferably 10 to 30 parts by mass, and even more preferably 20 to 25 parts by mass relative to 100 parts by mass of the liquid olefin polymer, in that it is possible to achieve a high level of both suppression of discoloration and the like and rapid progress of the silanol condensation reaction.

[0042] In the liquid composition production method of the present invention, the mixed amount (used amount) of the organic peroxide is 0.1 to 2 parts by mass relative to 100 parts by mass of the liquid olefin polymer. When the mixed amount of the organic peroxide is within the above range, the grafting reaction can be efficiently advanced, and the silanol condensation reaction can be rapidly advanced under mild conditions while suppressing the occurrence of discoloration, etc., to prepare a liquid silane-grafted olefin composition capable of constructing a sufficient crosslinked structure. The mixed amount of the organic peroxide is more preferably 0.5 to 1.5 parts by mass, and even more preferably 1.0 to 1.5 parts by mass relative to 100 parts by mass of the liquid olefin polymer, in that it is possible to achieve a high level of suppression of discoloration, etc., and rapid progression of the silanol condensation reaction.

[0043] In the liquid composition production method of the present invention, the liquid olefin polymer and the silane coupling agent are reacted at a temperature of 50 to 200 ° C. in the above-mentioned mixed amounts. This reaction may be carried out in the presence of an organic peroxide, and is preferably carried out by mixing the liquid olefin polymer, the silane coupling agent, and the organic peroxide in the above-mentioned mixed amounts at a temperature of 50 to 200 ° C. The above reaction is more preferably carried out by injecting (feeding) the liquid olefin polymer into a reactor (preferably a closed reactor) set at 50 to 200 ° C., and injecting (feeding, adding) the silane coupling agent and the organic peroxide together or separately into the reactor to the liquid olefin polymer at 50 to 200 ° C., preferably the liquid olefin polymer heated to 50 to 200 ° C., to mix the liquid olefin polymer, the silane coupling agent, and the organic peroxide. In a more preferred mixing method, the injection time (injection rate) of the silane coupling agent and the organic peroxide cannot be uniquely determined by the apparatus used, and is appropriately set according to the type, performance, etc. of the apparatus. For example, it is preferable that the flow rate is 2 to 10 mL / min per 100 g of the liquid olefin polymer. When the silane coupling agent and the organic peroxide are injected into the reactor together, a mixture of the silane coupling agent and the organic peroxide is prepared. The silane coupling agent and the organic peroxide are mixed using a known mixer or the like, usually under non-heating conditions or low-temperature heating conditions, preferably at 10 to 60°C, more preferably around room temperature (20 to 35°C), for several minutes to several hours, by dry or wet mixing methods and conditions. Preferably, dry mixing (dry blending) is performed under non-heating conditions or low-temperature heating conditions.

[0044] In the liquid composition production method of the present invention, the reaction temperature is set to 50 to 200° C. within a temperature range of not less than the 1-hour half-life temperature of the organic peroxide and not more than the 1-minute half-life temperature. The reaction temperature may be the installation temperature of the reaction apparatus, but is preferably the temperature of the liquid olefin polymer, or the normal heating temperature. The reaction time is appropriately set depending on the progress of the grafting reaction, but is preferably 10 minutes or more, more preferably 30 minutes to 2 hours, and even more preferably 45 minutes to 1 hour. The reaction time is defined as the elapsed time from the time (starting point) when the liquid olefin polymer, the silane coupling agent, and the organic peroxide are mixed at a predetermined temperature. Stirring is continued during the reaction, and the stirring speed etc. are appropriately set. In the reaction between the liquid olefin polymer and the silane coupling agent, it is preferable that the silanol condensation catalyst is substantially absent. Here, the term "substantially absent" does not mean excluding the silanol condensation catalyst that is inevitably present, and the silanol condensation catalyst may be present, for example, in an amount of 0.01 parts by mass or less per 100 parts by mass of the liquid olefin polymer.

[0045] In the liquid composition production method of the present invention, when producing a liquid silane-grafted olefin composition containing a silanol condensation catalyst, the liquid silane-grafted olefin composition and the silanol condensation catalyst are mixed, for example, under the conditions for preparing the mixture of the silane coupling agent and the organic peroxide. The amount of the silanol condensation catalyst mixed (used) at this time is not particularly limited and is appropriately set. In terms of being able to rapidly proceed with the silanol condensation reaction under mild conditions, the amount of the silanol condensation catalyst mixed can be set to the same range as the content of the silanol condensation catalyst in the above-mentioned liquid silane-grafted olefin composition.

[0046] In this manner, a liquid silane-grafted olefin composition containing the liquid silane-grafted olefin can be produced.

[0047] [Method of manufacturing silane crosslinked cured product] The silane-crosslinked cured product (silanol condensation cured product) of the present invention can be produced by any suitable method for subjecting silanol condensation-reactive reactive sites of a silane coupling agent in a liquid silane-grafted olefin composition to a silanol condensation reaction, and is preferably produced by the method for producing a silane-crosslinked cured product of the present invention described below, since it is possible to produce a silane-crosslinked cured product having a sufficient crosslinked structure and excellent appearance. The method for producing a silane-crosslinked cured product of the present invention (sometimes simply referred to as the method for producing a cured product of the present invention) comprises a step of contacting the liquid silane-grafted olefin composition obtained by the method for producing a liquid silane-grafted olefin composition of the present invention with water in the presence of a silanol condensation catalyst.

[0048] In this step, the amount of the silanol condensation catalyst used is not particularly limited, and is, for example, preferably 0.0001 to 0.5 parts by mass, more preferably 0.001 to 0.2 parts by mass, per 100 parts by mass of the liquid olefin polymer in the liquid silane-grafted olefin composition. In this step, the method for contacting the liquid silane-grafted olefin composition (including the molded product described later) with water in the presence of a silanol condensation catalyst is not particularly limited, and examples thereof include a method for contacting a liquid silane-grafted olefin composition containing a silanol condensation catalyst with water, and a method for contacting a liquid silane-grafted olefin composition not containing a silanol condensation catalyst with a silanol condensation catalyst and water. The liquid silane-grafted olefin composition can be contacted with water by a method commonly used in the silane crosslinking method. The silanol condensation reaction proceeds under mild conditions, such as leaving the composition at room temperature, for example, at a temperature of about 20 to 25° C., in the presence of moisture, so there is no need to use a special crosslinking device such as a crosslinking tube, and there is no need to actively contact the composition with water. From the viewpoint of promoting the silanol condensation reaction (crosslinking reaction), it is preferable to actively contact the liquid silane-grafted olefin composition with water. Examples of the contact method include methods (conditions) commonly used in the silane crosslinking method, such as contacting the composition with water under mild conditions under normal pressure, and specifically include exposure to a saturated water vapor atmosphere, exposure to a high humidity environment, immersion in room temperature water or hot water (for example, 50 to 90° C.), and insertion into a moist heat bath. In order to increase the efficiency of contact with water, the material may be contacted with water under stirring, and pressure may be applied during contact to allow water to penetrate into the material.

[0049] In the method for producing a cured product of the present invention, the liquid silane-grafted olefin composition can be molded into an appropriate shape before the step of contacting the liquid silane-grafted olefin composition with water. The molding method and molding conditions are selected appropriately according to the shape and form after molding. For example, molding methods include mold molding, coating methods (spray coating, brush coating), and other methods such as impregnating fibers, dipping other molded objects, etc. In addition, in the coating method, a film-shaped or plate-shaped molded object can be molded. The molding conditions are not particularly limited, but since the liquid silane-grafted olefin composition is liquid at room temperature and normal pressure, for example, a heating step and a heating device for heating to a high temperature required to melt a solid crosslinkable composition are not required, and non-heating conditions or low-temperature heating conditions can be used. For example, the molding temperature can be 0 to 60°C, and preferably 5 to 40°C. When the liquid silane-grafted olefin composition is molded under the above molding conditions, the silanol condensation reaction of the silane coupling agent can be effectively suppressed (curing and solidification during molding can be suppressed), and a silane-crosslinked cured product with excellent appearance can be produced.

[0050] In this manner, a solid silane-crosslinked cured product having a sufficient crosslinked structure and excellent appearance can be produced from the liquid silane-grafted olefin composition. This silane-crosslinked cured material is believed to contain a crosslinked polymer crosslinked via the silane coupling agent (siloxane bond), i.e., a crosslinked polymer in which the liquid silane-grafted olefin composition is condensed via a siloxane bond, as a result of hydrolysis of the silanol condensable reactive sites of the silane coupling agent grafted to the liquid olefin polymer and undergoing a silanol condensation reaction with each other.

[0051] <Applications of silane crosslinked cured products> The silane-crosslinked cured product of the present invention can be used in various applications where resin molded products or rubber molded products are usually used, such as insulating coating layers (including sheaths) for wiring materials, molding materials, power plugs, connectors, sleeves, boxes, tape substrates, tubes, sheets, films, packings, gaskets, cushioning materials, and vibration-proofing materials, and other resin molded product substitutes. EXAMPLES

[0052] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these.

[0053] Details of each compound used in the examples and comparative examples are given below. <Liquid olefin polymer> LUCANT LX004 (product name): copolymer of ethylene and α-olefin, viscosity 0.82 Pa·s, manufactured by Mitsui Chemicals Lucant LX200 (product name): copolymer of ethylene and α-olefin, viscosity 52 Pa·s, manufactured by Mitsui Chemicals LBR-302 (product name): Liquid butadiene, viscosity 0.6 Pa·s, manufactured by Kuraray Co., Ltd. <Silane coupling agent> KBM-1003 (trade name, trimethoxyvinylsilane, manufactured by Shin-Etsu Silicones) <Organic peroxide> Perhexa 25B (trade name, 2,5-dimethyl-2,5-di-tert-butylperoxyhexane, 1-hour half-life temperature 138.1°C, 1-minute half-life temperature 179.8°C, manufactured by NOF Corporation) <Silanol condensation catalyst> Adeka STAB OT-1 (product name, dioctyltin dilaurate, manufactured by ADEKA Corporation)

[0054] [Examples 1 to 8 and Comparative Examples 1 to 2] Examples 1 to 8 and Comparative Examples 1 and 2 were each carried out using the components shown in Table 1. Specifically, liquid silane-grafted olefin compositions having the compositions shown in Table 1 were prepared by the following production method, and these were brought into contact with a silanol condensation catalyst and water to produce silane-crosslinked cured materials. In Table 1, the numerical values ​​relating to the mixed amount (content) of each example are in parts by mass unless otherwise specified. Furthermore, a blank for each component means that the mixed amount of the corresponding component is 0 parts by mass.

[0055] <Example 1> First, a silane coupling agent and an organic peroxide were mixed in the mass ratio shown in Table 1 and stirred at room temperature (25° C.) for 1 minute to obtain a mixture. Next, 100 g of liquid olefin polymer (Lucant LX004) was introduced into a sealed reaction vessel equipped with a stirrer (autoclave with a stirrer having a capacity of 1 L), and heating was started while stirring at a rotation speed of 200 rpm. After the temperature of the liquid olefin polymer in the sealed reaction vessel reached the set temperature of 160°C, a mixture of the silane coupling agent and the organic peroxide was injected into the sealed reaction vessel at an injection rate of 5 mL / min. After the entire amount of the mixture was injected, stirring was continued for 1 hour at the set temperature. In this way, the liquid olefin polymer and the silane coupling agent were reacted in the presence of the organic peroxide to prepare the liquid silane-grafted olefin composition of Example 1.

[0056] <Example 2> A liquid silane-grafted olefin composition of Example 2 was prepared in the same manner as in Example 1, except that the mixture of the silane coupling agent and the organic peroxide was injected before the start of heating the liquid olefin polymer.

[0057] <Examples 3 to 6, 8 and Comparative Examples 1 and 2> In Example 2, the type and amount of the liquid olefin polymer, the amount of the silane coupling agent, and the amount of the organic peroxide were changed to those shown in Table 1. The liquid silane-grafted olefin compositions of Examples 3 to 6 and 8 and Comparative Examples 1 and 2 were prepared in the same manner as in Example 2.

[0058] <Example 7> A liquid silane-grafted olefin composition of Example 7 was prepared in the same manner as in Example 2, except that a stirring device (magnetic stirrer) and an open-type reaction vessel (a beaker with a capacity of 1 L) were used instead of the closed-type reaction vessel (an autoclave with a capacity of 1 L) equipped with a stirring device in Example 2.

[0059] Each of the liquid silane-grafted olefin compositions produced in Examples 1 to 8 and Comparative Examples 1 and 2 was in a liquid state at room temperature and normal pressure. The following tests were carried out on each of the produced liquid silane-grafted olefin compositions, and the results are shown in Table 1.

[0060] <Evaluation 1: Dynamic viscosity measurement at 100℃> For the liquid silane-grafted olefin compositions produced in each of the Examples and Comparative Examples, the kinetic viscosity at normal pressure and 100° C. was measured using a Brookfield viscometer (model number: RVDV2T, manufactured by Brookfield Corporation). This test is a reference test to evaluate the workability of the reaction product at the highest temperature within the range in which it can be handled. Viscosity at 100°C is 1,000mm 2 / s or less is considered "OK" (passed), and 2 If the test result exceeded 100 / s, it was marked as "X" (fail).

[0061] <Evaluation 2: Workability test> In each of the Examples and Comparative Examples, after reacting the liquid olefin polymer with the silane coupling agent in the presence of an organic peroxide, when the temperature of the liquid silane-grafted olefin composition in the reaction vessel dropped to 50°C, the reaction vessel was tilted 90° from the vertical (turned over). One minute after the reaction vessel was turned over on its side, it was confirmed whether any liquid silane-grafted olefin composition was attached (remained) on the inner surface of the vessel located above the turned over reaction vessel. This test is a test to evaluate whether the prepared liquid silane-grafted olefin composition maintains its liquid state. If the composition passes this test, it becomes possible to mold the composition without the need for a high-temperature heating process or heating device during molding, thereby realizing high workability (ease of handling). The workability test was evaluated as follows: if no liquid silane-grafted olefin composition was found to be attached (remaining) on ​​the inner surface of the vessel above the overturned reaction vessel within one minute of the reaction vessel being turned on its side, it was evaluated as "○" (pass); if the liquid silane-grafted olefin composition was found to be attached (remaining) on ​​the inner surface of the vessel above the overturned reaction vessel even after one minute had passed since the reaction vessel was turned on its side, it was evaluated as "△" (pass); and if the shape did not change at all and the vessel did not flow out, it was evaluated as "×" (fail).

[0062] <Evaluation 3: Discoloration test> The liquid silane-grafted olefin compositions produced in each of the Examples and Comparative Examples were visually inspected to evaluate the presence or absence of discoloration (usually yellowing). This test is a test for evaluating the grafting reaction and the uniformity of the mixed state during the preparation of a liquid silane-grafted olefin composition. If this test is passed, a silane-crosslinked cured product with excellent appearance can be produced. The discoloration test was evaluated as follows: when no discoloration was observed in the produced liquid silane-grafted olefin composition, it was rated as "◯" (pass); when discoloration was observed, it was rated as "×" (fail).

[0063] <Evaluation 4: Curability test> The liquid silane-grafted olefin compositions produced in each of the Examples and Comparative Examples were left in contact with water for 24 hours in an environment of 60°C and a relative humidity of 80% in the presence of 0.1 parts by mass of a silanol condensation catalyst per 100 parts by mass of the liquid olefin polymer used in the production of each liquid silane-grafted olefin composition. The method of contacting with water in the presence of a silanol condensation catalyst involved adding a predetermined amount of silanol condensation catalyst to each liquid silane-grafted olefin composition under normal temperature and humidity (25°C, 50RH%), stirring at 100 rpm for 1 minute to prepare a mixture, and leaving it in the above-mentioned environment. This test evaluates whether a silane-crosslinked cured product (solid composition) of a liquid silane-grafted olefin composition can be produced by inducing and progressing a silanol condensation reaction under mild conditions without the need for an excessively high-temperature heating process or crosslinking equipment such as a crosslinking tube. The curing test was evaluated as follows: if the liquid silane-grafted olefin composition produced underwent a silanol condensation reaction (losing its liquid state) and changed into a solid-state composition (silane-crosslinked cured product), it was evaluated as "good" (pass); if it did not lose its liquid state and remained a liquid composition, it was evaluated as "bad" (fail).

[0064] <Evaluation 5: Uniformity test> Five 10 mL test liquid samples were taken from any location of the liquid silane-grafted olefin composition produced in each Example and Comparative Example, and the viscosity of each test sample was measured using a Brookfield viscometer (model number: RVDV2T, manufactured by Brookfield Corporation). This test is one of the reference tests for evaluating whether a liquid silane-grafted olefin composition maintains a uniform liquid state. If this test is passed, the final crosslinking reaction will proceed uniformly, resulting in a silane-crosslinked cured product with almost constant appearance and properties. The uniformity test was evaluated by the average viscosity (ρ AV ) and the viscosity of each sample (ρ M ) and the absolute value of the difference (|ρ AV -ρ M |), the absolute values ​​of all five samples (|ρ AV -ρM |) is the average value (ρ AV ) was judged as "◎" (passed), and the absolute values ​​of all five samples (|ρ AV -ρ M If the absolute value (|ρ AV -ρ M If the difference between the two was more than 10%, it was marked as "×" (fail).

[0065] [Table 1]

[0066] In Table 1, in the "Reaction vessel" column, "sealed" indicates that a sealed reaction vessel (autoclave) was used, and "open" indicates that an open reaction vessel (beaker) was used. In the "Injection" column, "during" indicates that the mixture was injected after the liquid olefin polymer reached the set temperature, and "at the beginning" indicates that the mixture was injected before the liquid olefin polymer was heated.

[0067] The results shown in Table 1 reveal the following: That is, the liquid silane-grafted olefin composition of Comparative Example 1, in which the amount of silane coupling agent grafted to the liquid olefin polymer is too large, discolors the liquid silane-grafted olefin composition itself, and a silane crosslinked cured product with excellent appearance cannot be produced. On the other hand, the liquid silane-grafted olefin composition of Comparative Example 2, in which the amount of silane coupling agent grafted to the liquid olefin polymer is too small, does not produce a silane crosslinked cured product with a sufficient crosslinked structure. In contrast, the liquid silane-grafted olefin compositions of Examples 1 to 8, in which the amount of silane coupling agent to be grafted to the liquid olefin polymer is set to a predetermined amount, are all liquid at room temperature and normal pressure, making it unnecessary to perform a heating process and a heating device during molding, and no discoloration occurs. Moreover, without using a special crosslinking device such as a crosslinking tube, the silanol condensation reaction, which is the final crosslinking reaction, proceeds under mild conditions to produce a silane-crosslinked cured product having a sufficient crosslinked structure. In particular, the liquid silane-grafted olefin compositions of Examples 1 to 6 and 8, which were prepared using a closed reaction vessel, are all in a uniform liquid state, and can produce a silane-crosslinked cured product with almost constant appearance and properties.

Claims

1. A liquid silane-grafted olefin composition obtained by grafting 100 parts by mass of a liquid olefin polymer with 3 to 30 parts by mass of a silane coupling agent having a site capable of undergoing a grafting reaction with said liquid olefin polymer.

2. Kinematic viscosity at 100°C is 1,000 mm 2 2. The liquid silane-grafted olefin composition of claim 1, wherein the olefin moiety is 0.01 to 0.15 wt.

3. The liquid silane-grafted olefin composition according to claim 1, obtained by reacting 100 parts by mass of the liquid olefin polymer with 3 to 30 parts by mass of the silane coupling agent in the presence of 0.1 to 2 parts by mass of an organic peroxide at a temperature of 50 to 200°C.

4. The liquid silane-grafted olefin composition according to claim 3, which is obtained by adding the silane coupling agent and the organic peroxide to the liquid olefin polymer at a temperature of 50 to 200°C, and reacting the liquid olefin polymer with the silane coupling agent.

5. A silane-crosslinked cured product of the liquid silane-grafted olefin composition according to any one of claims 1 to 4.

6. The method for producing the liquid silane-grafted olefin composition according to claim 1, comprising reacting 100 parts by mass of a liquid olefin polymer with 3 to 30 parts by mass of a silane coupling agent having a site capable of grafting reaction with the liquid olefin polymer in the presence of 0.1 to 2 parts by mass of an organic peroxide at a temperature of 50 to 200°C.

7. The method for producing the liquid silane-grafted olefin composition according to claim 6, wherein the silane coupling agent and the organic peroxide are added to the liquid olefin polymer at a temperature of 50 to 200°C to react the liquid olefin polymer with the silane coupling agent.

8. 7. The method for producing a liquid silane-grafted olefin composition according to claim 6, wherein the reaction is carried out in a stirred closed reactor.

9. A method for producing a silane-crosslinked cured product, comprising contacting the liquid silane-grafted olefin composition obtained by the method for producing a liquid silane-grafted olefin composition according to any one of claims 6 to 8 with water in the presence of a silanol condensation catalyst to produce a silane-crosslinked cured product of the liquid silane-grafted olefin composition.

Citation Information

Patent Citations

  • Reactive plasticizer

    JP1986200136A

  • Liquid modified ethylene random copolymer

    JP1986246215A

  • Production of polyolefin containing hydrolyzable silicon

    JP1997059317A

  • Hydrolyzable silyl-containing ethylene.alpha- olefin.nonconjugated polyene random copolymer rubber and its production

    JP2001031719A

  • Silane-grafted materials for solid and foam applications

    JP2001503813A

Cited By

  • Liquid silane graft polyol composition and silane crosslinked cured product thereof, and methods for producing the same.

    JP2026161975A