Slip film for removing fluid contents and coating for forming slip film
A decidua film-forming paint with thermoplastic resin and medium chain fatty acid triglyceride addresses the removability and durability issues of conventional coatings, providing enhanced sliding properties for aqueous emulsions by forming an oil layer on the surface.
Patent Information
- Application Number
- JP2023051467
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional coating films, as described in Patent Documents 1 to 3, do not adequately address the removability of fluid contents, particularly aqueous emulsions such as milky lotions, and there is a need for improved durability and sliding properties.
A decidua film-forming paint is developed, comprising a thermoplastic resin and medium chain fatty acid triglyceride in specific blending ratios, which forms a coating with enhanced sliding properties and durability by creating an oil layer on the surface.
The decidua film exhibits excellent removability and durability for fluid contents, particularly aqueous emulsions, maintaining sliding properties over time due to the presence of medium chain fatty acid triglyceride, which enhances the sliding properties of the coating surface.
Smart Images

Figure 2024140361000017 
Figure 2024140361000018 
Figure 2024140361000019
Abstract
Description
[Technical field]
[0001] The present invention relates to a coating film having excellent removability of fluid contents. [Background technology]
[0002] In a storage container for a fluid content, it is desirable to form a coating film that allows the fluid content to slide down quickly inside a tilted container so that the user can quickly discharge the fluid content or use it up completely without leaving any behind in the container.
[0003] The inventors have previously proposed a coating composition containing an organic solvent-soluble fluororesin having a radically polymerizable reactive group, a one-terminus radically polymerizable polysiloxane, a graft copolymer obtained by copolymerizing a methacrylate monomer, a one-terminus reactive silicone oil, a curing agent, and an organic solvent. They have tested the sliding properties of the coating film produced by this composition against water and oil, and confirmed that the coating film has the required sliding properties (see Patent Document 1). The inventors have also previously proposed a sliding film in which a large amount of oil, such as vegetable oil or silicone oil, is distributed in the resin on the substrate, in which the volume ratio of oil near the surface is greater than the volume ratio of oil in the internal region, and multiple oil aggregates near the surface are exposed, each protruding from the surface, and the inventors have confirmed that the film has a predetermined sliding property (see Patent Document 2). Also, a coating composition for preventing snow adhesion has been disclosed that contains a thermoplastic resin, an acrylic silicone compound, silicone oil, and a solvent (see Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-218462 A [Patent Document 2] JP 2018-184536 A [Patent Document 3] JP 2020-084127 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, even in the conventional coating films of Patent Documents 1 to 3, there is still room for improvement in terms of removability of fluid contents (particularly aqueous emulsions such as milk lotions).
[0006] The present invention has been made in consideration of the above problems, and aims to provide a sliding film and a sliding film-forming paint that are excellent in removability (sliding property) for fluid contents (especially aqueous emulsions such as lotions) and durability. [Means for solving the problem]
[0007] As a result of conducting many experiments on the sliding properties of fluid contents, the inventors discovered that, particularly for aqueous emulsions such as lotions, a sliding film with the desired sliding properties and durability can be obtained by using a paint made of a thermoplastic resin blended with a medium-chain fatty acid triglyceride as a liquid oil at 25°C, leading to the completion of the present invention.
[0008] That is, the sliding film forming paint of the present invention is (A) component: thermoplastic resin, (B) component: medium chain fatty acid triglyceride, A solvent, The compounding ratio ((A) / (B)) of the component (A) to the component (B) is 4 / 96 to 46 / 54.
[0009] The sliding film of the present invention is formed on the surface of a substrate, (A) component: thermoplastic resin, (B) component: medium chain fatty acid triglyceride; The blending ratio ((A) / (B)) of the (A) component and the (B) component is 4 / 96 to 46 / 54, and the weight of the (B) component per area of the sliding membrane is 3.7 to 81 g / m 2It is characterized in that:
[0010] Here, the thickness of the gliding film is preferably 5 to 109 μm. It is also preferred that the object to be slid is a milky liquid, and that the adhesion energy of the slidable film to the base material is greater than the adhesion energy of the milky liquid to the slidable film. Effect of the Invention
[0011] According to the present invention, the sliding film formed on the surface of the substrate contains not only medium-chain fatty acid triglyceride but also a thermoplastic resin, so that the oil layer of the medium-chain fatty acid triglyceride containing the thermoplastic resin can exhibit excellent removability of fluid contents (especially aqueous emulsions such as milky lotions). Furthermore, the removability of fluid contents can be maintained for a long time. [Brief description of the drawings]
[0012] [Figure 1] 1 is an image showing the shapes of the containers (PET containers, WJ-type glass containers, and SV-type glass containers) used in the examples. [Diagram 2] This image can be used as a criterion for determining whether emulsion is slipping out of a PET container. [Diagram 3] This is an image that can be used as a criterion for determining whether lotion is slipping off inside a WJ type glass container. [Figure 4] This is an image that can be used as a criterion for determining whether lotion is slipping off inside an SV type glass container. [Diagram 5] FIG. 1 shows the results of evaluation based on the adhesion energy of a milky liquid to a smeared film on a PET substrate. [Figure 6] FIG. 1 is a diagram showing the evaluation results based on the adhesion energy of a milky liquid to a smeared film on a glass substrate. [Figure 7] FIG. 13 is a graph showing the change in adhesion energy of various emulsions when a sliding film is formed on a PET substrate and when the PET substrate is left as is. [Figure 8]FIG. 1 shows the change in adhesion energy of various emulsions when a sliding film is formed on a glass substrate and when the substrate is left as is. [Figure 9] 1 is a graph showing the relationship between the adhesion energy B of a sliding film to a PET substrate and the adhesion energy A of emulsion 1 to the sliding film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The following describes the embodiments of the present invention, but these are representative examples of the embodiments of the present invention, and the present invention is not limited to these contents as long as it does not deviate from the gist of the present invention. In the following description, "parts" means "parts by mass" and "%" means "% by mass" unless otherwise specified.
[0014] <Structure with slidable membrane> The structure having a sliding membrane of this embodiment is a storage container for an aqueous suspension (e.g., emulsion), which is a fluid content, and can be made of glass or resin depending on the application. Specific applications include storage of various cosmetics, detergents, edible products, etc. A sliding membrane is formed on the inner surface of the container that comes into contact with the aqueous suspension, using a paint containing medium-chain triglyceride (MCT) as a liquid oil at 25°C. Therefore, the oil is exposed on the surface of the sliding membrane, and the sliding membrane exhibits sliding properties for the fluid content.
[0015] Fluid contents are those whose shape can be easily changed by external forces (those that do not exhibit shape retention) and are fluid. Fluid contents are oil-in-water (O / W) emulsions, that is, aqueous suspensions, such as cosmetic liquids such as milky lotions, liquid detergents, water-based pastes, edible sauces and ketchups, etc. The viscosity of fluid contents is within the following range when measured for 300 seconds at the desired rotation speed (1, 12, 30, or 60 rpm) and at a temperature of 25°C using a B-type viscometer with an L4 spindle. Rotational speed (1 rpm): 9,000~24,000 mPa·s Rotational speed (12 rpm): 1,750 to 3,600 mPa·s Rotational speed (30 rpm): 800~ 4,500 mPa s Rotational speed (60 rpm): 700~ 1,200 mPa·s
[0016] <Paint> The paint that forms a sliding film on the inner surface of the container contains (A) a thermoplastic resin, (B) a medium-chain triglyceride (MCT), (C) a solvent, and, if necessary, an appropriate additive (D).
[0017] (A) Thermoplastic resin: The thermoplastic resin is a component that becomes the matrix when a sliding film is formed using the paint of the embodiment. Examples of thermoplastic resins that can be included in the paint include polyolefins such as polyethylene and polypropylene; chlorinated polyolefins; polyvinyl chloride; polyvinylidene chloride; polystyrene; nylon; polyvinyl alcohol; polyvinyl acetate; polymethyl methacrylate; polyurethane; polyurethane acrylate; polyurethane methacrylate; fluororesins such as polytetrafluoroethylene; vinyl chloride-vinyl acetate copolymer resins; ethylene-vinyl acetate copolymer resins; methacrylic styrene copolymer resins; synthetic rubbers such as acrylonitrile butadiene styrene copolymer resins and acrylonitrile-styrene copolymer resins; acrylic resins; polyamides; polyacetals; polycarbonates; polyesters; cellulose acetate; cyclic polyolefins, etc. Although it depends on the use of the article to which the sliding film is applied, for example, the thermoplastic resin suitable as the matrix of the sliding film applied to the container for cosmetics is a hard and transparent resin. As the thermoplastic resin used in the paint of the embodiment, in particular, polyolefin, chlorinated polyolefin, polystyrene, vinyl chloride-vinyl acetate copolymer resin, acrylic resin, polyacetal, polycarbonate, polyurethane, polyurethane acrylate, polyurethane methacrylate, polyester, etc. can be preferably used. As the thermoplastic resin, chlorinated polyolefin, vinyl chloride-vinyl acetate copolymer resin, acrylic resin, etc. are suitable in order to further enhance transparency and adhesion to the substrate. One or a mixture of two or more of these polymer compounds can be selected from these polymer compounds and used as the thermoplastic resin.
[0018] The polyolefin resin is preferably a polypropylene resin or a polyolefin resin obtained by copolymerizing propylene with an α-olefin (e.g., ethylene, butene, 3-methyl-1-butene, 3-methyl-1-heptene), more preferably a propylene-based random copolymer, and even more preferably a polypropylene, an ethylene-propylene copolymer, a propylene-butene copolymer, or an ethylene-propylene-butene copolymer. Chlorinated polyolefin is a polyolefin in which at least a part of hydrogen atoms is replaced with chlorine atoms, and the chlorine content (measurable according to JIS-K7229:1995) is preferably 10 to 40 mass%, more preferably 15 to 30 mass%. By setting the chlorine oil content within the above range, the polarity of the resin component can be adjusted within a certain range, so that compatibility with other components in the coating material becomes good, and sufficient adhesion to the substrate can be obtained. In order to obtain good compatibility and affinity with oil, the weight-average molecular weight of the chlorinated polyolefin is preferably 50,000 to 200,000. If the weight-average molecular weight is 50,000 or more, the cohesive force of the resin component is sufficient, and the adhesion to the substrate is good. If the upper limit of the weight-average molecular weight is 200,000 or less, the compatibility with other components in the coating material is good, and sufficient adhesion to the substrate is obtained.
[0019] The weight average molecular weight can be determined by using a standard polystyrene calibration curve in a gel permeation chromatograph (GPC) device. The GPC measurement conditions are as follows: Equipment: HLC-8320GPC (Tosoh Corporation) Column: TSK-gel G-6000H XL , G-5000H XL , G-4000H XL , G-3000H XL , G-2000H XL (Manufactured by Tosoh Corporation) Eluent:THF Flow rate: 1mL / min Temperature: Pump oven, column oven 40℃ Injection volume: 100μL Standard material: Polystyrene EasiCal PS-1 (Agilent Technology)
[0020] As the chlorinated polyolefin resin, chlorinated polypropylene is preferred. In this embodiment, the chlorinated polyolefin may be a copolymer resin with other monomers. The copolymerizable monomer may be an acrylic monomer, an acidic monomer, a vinyl acetate monomer, a styrene monomer, etc. The acidic monomer may be maleic acid, maleic anhydride, fumaric acid, (meth)acrylic acid, etc.
[0021] Furthermore, as the thermoplastic resin, a vinyl chloride-vinyl acetate-acrylic copolymer resin (also called vinyl chloride acetate acrylic resin) or a vinyl chloride-vinyl acetate copolymer-containing urethane resin (also called vinyl chloride acetate urethane resin) may be used. The vinyl chloride / vinyl acetate resin is formed by copolymerizing 60 to 95% by mass of vinyl chloride monomer, 2 to 15% by mass of vinyl acetate monomer, and 2 to 30% by mass of a hydroxyl group-containing acrylate. Here, by making the vinyl chloride monomer 60-95% by mass, the film is given toughness and high surface hardness. If it is less than 60% by mass, the strength of the film decreases, and if it exceeds 95% by mass, the solubility in the solvent decreases, the viscosity of the paint increases, and the dispersibility decreases. The vinyl acetate monomer is 2 to 15% by mass. If it is less than 2% by mass, the solubility in the solvent decreases, and the viscosity of the paint increases, decreasing dispersibility. If it exceeds 15% by mass, the strength and durability of the coating film decrease. The hydroxyl group-containing acrylate is set to 2 to 30% by mass. If it is less than 2% by mass, the performance in terms of durability and adhesion of the coating film deteriorates, and if it exceeds 30% by mass, the glass transition temperature decreases and blocking occurs. As the hydroxyl group-containing acrylate, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate, polyethylene glycol mono(meth)acrylate, polyethylene glycol polypropylene glycol mono(meth)acrylate, glycerol mono(meth)acrylate, etc. can be suitably used. As the vinyl chloride acetate acrylic resin, for example, a vinyl chloride-vinyl acetate copolymer resin "SOLVINE" (registered trademark) available from Nissin Chemical Industry Co., Ltd. under the trade name TA3 can be used. On the other hand, vinyl chloride-vinyl acetate urethane resin is prepared as a resin solution containing, for example, 3 to 50 mass% of a vinyl chloride-vinyl acetate copolymer resin solution having a hydroxyl group and a solid content of 15%, and 25 to 60 mass% of a polypropylene glycol-containing polyurethane resin solution having a solid content of 30%.
[0022] (B) Medium-chain triglycerides (MCT) An oil that is liquid at 25°C is one that exhibits fluidity at room temperature (25°C). Since the purpose is for the oil to seep out onto the surface of the coating film to be formed and further improve the non-adhesiveness of the coating film, it is preferable that the surface tension of the oil itself is low, and it is preferable that the surface tension at 25°C is 30 mN / m or less. To satisfy these conditions, the oil is required to have low intermolecular interactions, and examples of such oils include hydrocarbon oils such as fatty acid esters, polyol esters, polyglycols, polyethers, and polyphenyl ethers.
[0023] The oil in this embodiment contains at least a medium-chain fatty acid triglyceride, which is a fatty acid ester. In addition to using the medium-chain fatty acid triglyceride alone, it can be used by mixing it with the oils listed above that have small intermolecular interactions. The general formula of the medium-chain fatty acid triglyceride is shown in formula (1).
[0024] [ka] R1, R2, and R3 are each a hydrocarbon chain having 5 to 11 carbon atoms, which may contain a carbon double bond.
[0025] The blending ratio ((A) / (B)) of the thermoplastic resin (A) and the medium-chain fatty acid triglyceride (B) is preferably within the range of 4 / 96 to 46 / 54. If the blending amount of oil is small, it may not be possible to ensure good sliding properties on the inner surface of the container. On the other hand, if the blending amount is too large, moldability may be impaired or the container properties may be adversely affected. In the paint of this embodiment, the medium-chain triglyceride is used to impart sliding properties, particularly the ability to remove aqueous suspensions (e.g. emulsions) that are fluid contents. It enhances the property of the aqueous suspensions to slide (roll like balls) on the surface of the sliding film. Since the medium chain fatty acid triglyceride is well compatible with the surface of the polymer structure of the thermoplastic resin, the oil component spreads thinly on the surface of the thermoplastic resin, and a layer of the oil component is easily formed. When the sliding film is applied to the article in this way, more medium chain fatty acid triglyceride is unevenly distributed on the surface of the sliding film, forming a layer of the oil component, and the sliding property of the sliding film surface is improved. Furthermore, the presence of medium-chain fatty acid triglycerides inside the sliding film makes it easier for the surface of the thermoplastic resin to always be wet with oil components, and the sliding properties are maintained for a long time. In this way, an aqueous suspension (O / W emulsion, for example, a milky lotion) that comes into contact with the oil film on the sliding membrane surface slides down the surface due to the difference in surface tension with the oil film. The reason why medium-chain fatty acid triglycerides are suitable is that if the number of carbon atoms in the hydrocarbon chain is greater than this, the compatibility with the surface of the polymer structure of the thermoplastic resin decreases, making it difficult for the oil component to be maintained on the surface for a long time. In addition, the compatibility with other components of the paint (such as thermoplastic resin) becomes poor, and there is a possibility that a cloudy sliding film will result.
[0026] (C) Solvent The purpose of the solvent is not limited as long as it can sufficiently dissolve the solute. Examples of the solvent include ketones such as acetone, methyl ethyl ketone, diethyl ketone, methyl isobutyl ketone, and cyclohexanenone; esters such as methyl acetate, ethyl acetate, ethyl butyrate, and isopentyl acetate; alcohols such as methanol, ethanol, propanol, butanol, hexanol, and propylene glycol monomethyl ether; glycol esters such as ethylene glycol monoethyl ether acetate, butyl carbitol acetate, ethyl carbitol acetate, and propylene glycol monomethyl ether acetate; glycol ethers such as methyl carbitol, ethyl carbitol, butyl carbitol, methyl triglycol, propylene glycol monomethyl ether, 1-methoxy-2-propanol, propylene glycol monobutyl ether, and methyl methoxybutanol; amides such as formamide, acetamide, benzamide, and N,N-dimethylformamide; hydrocarbons such as normal hexane, cyclohexane, ethyl cyclohexane, isooctane, normal decane, and normal pentane; aromatic hydrocarbons such as benzene, toluene, and xylene; and halides thereof. One or more solvents selected from these can be used by mixing them appropriately. In particular, by using methyl ethyl ketone, isopropanol, butyl acetate, etc., which volatilize in air at about room temperature, a coating material capable of easily forming a sliding film can be obtained.
[0027] In order to make the paint of this embodiment suitable for spraying or flow coating, it is preferable to use in the paint an amount of (C) solvent that is 0.1 to 5 times the total mass of (A) thermoplastic resin, (B) medium chain fatty acid triglyceride, and (D) additive. If the amount of solvent is too small, the viscosity of the paint increases, making coating difficult. If the amount of solvent is too large, the viscosity of the paint decreases, and it flows off the surface even when applied, so that an extra process such as recoating is required to further increase the thickness of the sliding film.
[0028] The paint of this embodiment can be produced by mixing (A) thermoplastic resin and (B) medium-chain fatty acid triglyceride, and dissolving the mixture in (C) solvent. In addition to the above-mentioned components, the paint of this embodiment may contain various known additives (D) such as plasticizers, dispersants, antioxidants, UV absorbers, fillers, and leveling agents (to prevent repelling during spray painting) depending on the application of the container, and in applications where transparency is not required, colorants such as pigments and dyes may also be added. In addition, it is also possible to add crystalline additives (inorganic oxides such as titanium oxide and various waxes). If necessary, a curing agent may also be added. However, the amount of such additives to be added should be small enough so that the amount of medium-chain fatty acid triglyceride in the paint is maintained within the range described above, and so that the formability of the coating film is not impaired, and so that the sliding properties of the coating film on the inner surface of the container are not impaired.
[0029] The paint of this embodiment can be applied to the surface of the substrate in the container, and then the solvent can be volatilized by drying through heating or the like to form a sliding film. The weight of medium-chain triglyceride per unit area of the sclerotial membrane is 3.7-81 g / m 2 It is preferable that the thickness of the sliding film is 5 to 109 μm. Although the thickness of the sliding film can be freely changed depending on the application, it is preferable that the thickness of the coating film is 5 to 109 μm. If the thickness of the coating film is less than 5 μm, even if a soft coating film is prepared, the coating film may be scraped off due to its thinness after long-term use. On the other hand, if the thickness is thicker than 109 μm, the coating film may be too thick for the number of years of practical use, which may not be economical. More preferably, the thickness of the coating film is 8 to 109 μm.
[0030] In this embodiment, the conditions are that each component contained in the paint maintains a dispersed state in the solvent and does not separate even after being left to stand for six months or more.
[0031] The substrate to which the coating material of the present embodiment is applied may be glass, resin, etc. As the resin, for example, polyethylene terephthalate resin, acrylic resin, or polycarbonate resin may be used. The coating material of this embodiment can be applied to the surface of the substrate by any conventional coating method such as doctor blade method, bar coating method, dipping method, air spray method, roller brush method, roller coater method, etc. As for the drying method, in addition to drying by heating, the substrate to which the coating material is applied can be left in an atmosphere at about room temperature until the solvent is sufficiently evaporated to form a sliding film. EXAMPLES
[0032] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the contents of these examples.
[0033] Physical properties, etc. are measured by the following methods unless otherwise specified. [Mixing ratio of component (A) to component (B) ((A) / (B))] The blending ratio is calculated based on the coating weight after drying (based on non-volatile content). The method of calculating the blending ratio based on non-volatile content will be explained in the case of Production Example 1 described later. The non-volatile content of Resin Example A-1 (chlorinated polyolefin) in Production Example 1 is 21.3%, and the non-volatile content of Oil Example B-1 (medium chain fatty acid triglyceride) is 0%. When Resin Example A-1 and Oil Example B-1 in a solvent-containing state are mixed at 60:40, the blending ratio based on non-volatile content of Resin Example A-1 is 60%×0.213 / (60%×0.213+40%)=0.2421, that is, 24%. In addition, the blending ratio based on non-volatile content of Oil Example B-1 is 40% / (60%×0.213+40%)=0.7579, that is, 76%. Therefore, the blending ratio is 24:76.
[0034] [Oil weight] The oil weight (weight of component (B)) is the weight of oil contained in the coating per coating area, and is a calculated value. First, the amount of coating used after coating and drying (g) was calculated from the difference in the container weight before coating and after coating and drying, and the amount of oil used (g) was obtained from the blending ratio. This was divided by the coating area in the container to obtain the oil weight (g / m2). 2 The oil weight calculated in this way is the coating weight after drying. The details of the coating area in the container will be described later.
[0035] [Film thickness] The film thickness is a calculated value. From the weight and blend ratio of the coating film after coating and drying, (i) the coating amount of only the thermoplastic resin (g / m 2 ), and (ii) the amount of oil applied alone (g / m 2 ) was calculated, and the sum of these values divided by their respective specific gravities was taken as the film thickness (μm). The specific gravity of the thermoplastic resin and oil is the specific gravity of the non-volatile content. The film thickness calculated in this way corresponds to the film thickness after coating and drying.
[0036] (Examples of resins used in paints) The thermoplastic resins chlorinated polyolefin (A-1) and chloro-vinyl acetate resin (A-2) were used. For comparison, the thermosetting resin fluorine acrylic polysiloxane (A-3) was used. For chlorinated polyolefin, we used "CA-PL01" (containing organic solvents) manufactured by Sakuranomiya Chemical Co., Ltd. For the vinyl chloride acrylic resin, we use "KW" (containing organic solvents) manufactured by Sakuranomiya Chemical Co., Ltd. The fluoroacrylic polysiloxanes used were "SW-S51" (for PET substrates) and "SW-S06" (for glass substrates) manufactured by Yamato Can Co., Ltd. (both of which contain organic solvents). Examples of these resins are listed in Table 1.
[0037] [Table 1]
[0038] The surface free energy of the resin in Table 1 is based on the typical Kaelble and Uy theoretical formula. First, a coating of only the resin is formed on a glass slide, and the contact angle of a 10 μL droplet of two reagents (water, diiodomethane, and formamide) on the coating is measured using a contact angle meter Drop Master DMs-401 (Kyowa Interface Science Co., Ltd.). These contact angle measurements are applied to the theoretical formula to calculate the dispersion component and polar component of the surface free energy, and the sum of these is the surface free energy of the resin.
[0039] (Examples of oils to be mixed into paint) As the medium-chain fatty acid triglyceride (B-1), "Actor M-1" manufactured by Riken Vitamin Co., Ltd. was used. Actor M-1 has a surface tension of 27.6 mN / m (25°C), a value measured by the suspension method, a kinematic viscosity (calculated value) of 21 cSt, and an average molecular weight (calculated value from the saponification value, median value) of 501. For comparison, dimethyl silicone oil (B-2) and methylphenyl silicone oil (B-3) were used. For the dimethyl silicone oil, "AK350" manufactured by Wacker Asahi Kasei Silicone Co., Ltd. was used. Dimethyl silicone oil has a surface tension (catalog value) of 21.0 mN / m (25°C) and a kinetic viscosity (catalog value) of 350 cSt. The methylphenyl silicone oil used was "KF-56A" manufactured by Shin-Etsu Chemical Co., Ltd. Methylphenyl silicone oil has a surface tension (catalog value) of 24.4 mN / m (25°C), a kinetic viscosity (catalog value) of 15 cSt, and a volatile content of 15% (105°C x 3 hours). In addition, only oil was applied to a glass slide, the contact angle of a 10 μL droplet of a reagent (water, formamide, diiodomethane) to the oil film was measured, and the surface free energy of the oil was calculated. A list of these oil examples is shown in Table 2.
[0040] [Table 2]
[0041] (Examples of organic solvents) Ketones, esters, alcohols, and hydrocarbons were used according to the resin. If the container was made of resin, a solvent that could prevent the resin (e.g., transparent polyester resin) from becoming cloudy due to crystallization was selected.
[0042] (Paint manufacturing examples 1-14) In Production Example 1, Resin Example (A-1) and Oil Example (B-1) were mixed to a mixing ratio after drying of 24:76, and the mixture was stirred to make it homogenous, thereby obtaining a paint. Similarly, in Production Examples 2 to 11, the above resin examples (A-1) to (A-3) and oil examples (B-1) and (B-3) were combined and mixed in the post-drying compounding ratios shown in Table 3 below, and an organic solvent was added thereto and stirred to homogenize, thereby obtaining a paint. In Production Examples 12 to 14, paints containing only resin or only oil were obtained. The dilution ratio of the organic solvent was adjusted within the range of 0.1 to 5.0 times the weight of the resin and oil. The contact angles of 10 μL droplets of reagents (water, formamide, diiodomethane) on the coating films formed with these paints were measured, and the surface free energy of the coating films was calculated.
[0043] [Table 3]
[0044] The paints of Production Examples 1 to 14 were used to coat the inside of a PET container (referred to as a PET container) or a glass container (referred to as a glass container) to prepare a coating film. PET containers are made of polyethylene terephthalate (PET). The coating area of a PET container is calculated by assuming the inside of the container to be cylindrical (inner diameter 36.72 mm, height 102.5 mm) and calculating the total area of the bottom and sides (1.23 x 10 -2 m 2 ) is used. Two types of glass containers were used: "WJ" type and "SV" type. The coating area of the "WJ" type glass container is cylindrical (inner diameter 45.9 mm, volume 85 cm). 3 ) and the area of the bottom and sides is calculated as a simple sum (0.91 x 10 -2 m 2 The coating area of an "SV" type glass container is calculated by assuming the inside of the container to be cylindrical (inner diameter 36.4 mm, height 75 mm) and adding up the areas of the bottom and sides (0.96 x 10 -2 m 2) is used. A list of these containers is shown in Table 4. The contact angles of 10 μL droplets of reagents (water, diiodomethane) with these containers (substrates) were measured, and the surface free energies of the containers were calculated.
[0045] [Table 4]
[0046] The coating method for the inner surface of the container was "spray" or "flow coating". In both coating methods, drying was performed after coating. The drying temperature and drying time were 100°C and 30 seconds for PET containers, and 100°C and 2 minutes for glass containers. However, if sufficient drying time can be secured, it is possible to form a coating film by drying at room temperature at 25°C. In addition, if the paint flows off before drying, the paint was applied in multiple coats to obtain the specified film thickness. The oil weight and film thickness were calculated based on the above calculation method. The coating film thus created was subjected to a test for durability against slipping off with emulsion (durability of removal performance). The physical properties of the commercially available emulsions used in the tests are shown in Table 5.
[0047] [Table 5]
[0048] With regard to viscosity, since the viscosity of "mayonnaise" is 8000 mPa s according to literature, the viscosity of "Kewpie Half (registered trademark)" was measured using a B-type viscometer with various settings of the rotation speed to confirm the rotation speed condition under which a viscosity value equivalent to the value in the literature was obtained, and an actual measured value of 7670 mPa s was obtained at 30 rpm. Based on this, the rotation speed condition for measuring the viscosity of the emulsion was set to 30 rpm. To measure the viscosity of the emulsion, a 20 g vial (SV-50A) (manufactured by Nichiden Rika Glass Co., Ltd.) was used, and an L4 spindle (diameter 3.2 mm) was placed at the center of the vial (inner diameter 26.5 mm) with an inner gap of 11.65 mm between the spindle and the inner wall of the vial.
[0049] The method for measuring the surface free energy of the emulsion was the same as the method for measuring the surface free energy of the thermoplastic resin and oil described above. The emulsion was spread on a slide glass to form a film, and the contact angles of 10 μL droplets of two reagents (diiodomethane and hexadecane) to the emulsion film were measured using a contact angle meter Drop Master DMs-401 (Kyowa Interface Science Co., Ltd.), and the surface free energy of the emulsion was calculated using the measured contact angles.
[0050] As shown below, the sliding film of this example has a surface free energy of 27 to 33 mJ / m 2 It exhibits excellent slip resistance against emulsions.
[0051] [Slip-down durability test] Fill the container with the coating with 10 g of commercially available emulsion as the fluid content, and then seal it with the stopper and cap (only the cap if the container does not have an inner stopper). Repeat the inversion of the container upside down and upright as follows, and visually evaluate the sliding properties (removal performance) of the coating against the emulsion after each inversion. 1st time: upright → inverted (record the date and time of inversion: 1st time start date and time) After the first inversion, leave the container in the inverted position until there is no more emulsion adhering to the inside of the container (bottom and sides) and it is determined that the emulsion has slid down to the cap side. When it is visually confirmed that the emulsion has slid down, begin the second inversion. 2nd time: Inverted → Upright (record the date and time when it was upright: start date and time of the 2nd time) Leave the container in the upright position until there is no more emulsion adhering to the inside of the container (shoulder and sides) and it is determined that the emulsion has slid to the bottom. When it is visually confirmed that the emulsion has slid down, begin the third inversion. 3rd time (and every odd number of times thereafter): upright → inverted (same as 1st time) 4th time (and every even number of times thereafter): Inverted → Upright (same as 2nd time)
[0052] The quality of the sliding property of the inner surface of the container (easily or not easily adhered to) is affected not only by the difference in the material of the inner surface of the container, but also by the difference in the shape of the container (e.g., the shape of the shoulder part, the shape of the bottom surface, etc.). For this reason, the shapes of the three types of containers used in the examples (PET container, WJ type glass container, SV type glass container) are shown in Figure 1.
[0053] The criteria for visually checking whether lotion has slid off will be described with reference to the images in Figures 2 to 4. The image on the left in Figure 2 is the appearance of the PET container before the start of the 198th inversion in Example 1-2, and is the image that serves as the criterion for determining whether lotion 2 has slid off. The image on the right in Figure 2 is the appearance of the PET container about one month after the start of the 113th inversion in Comparative Example 5-2 (vertical streaks of lotion 2 are attached to the side wall), and is the image that serves as the criterion for determining whether lotion 2 has not slid off. The image on the left of Fig. 3 is the appearance of the WJ-type glass container before the start of the 74th inversion in Example 42-1, and is the image that serves as the standard for determining whether emulsion 1 has slid down. The image in the center of Fig. 3 is the appearance of the WJ-type glass container (lotion 1 is attached to the bottom and front of the side wall) after 3 months or more have passed since the start of the first inversion in Comparative Example 26-1 (coating film only with oil), and is the image that serves as the standard for determining whether emulsion 1 has not slid down when the coating film is only oil. The image on the right of Fig. 3 is the appearance of the WJ-type glass container (lotion 1 is attached to the bottom and front of the side wall) after 2 months or more have passed since the start of the first inversion in Comparative Example 19-1 (no coating film), and is the image that serves as the standard for determining whether emulsion 1 has not slid down when there is no coating film. The image on the left in Fig. 4 is the appearance of the SV type glass container one day after the start of the 200th inversion in Example 13-2, and is the image that serves as the standard for determining whether lotion 2 has slid down. The image on the right in Fig. 4 is the appearance of the SV type glass container four months or more after the start of the 20th inversion in Comparative Example 9-2 (lotion 2 is attached in the circumferential direction to the center in the height direction of the side wall), and is the image that serves as the standard for determining whether lotion 2 has not slid down.
[0054] "Evaluation method for slip resistance" We will now explain how to evaluate how long a container can maintain the emulsion's ability to slide off (slide durability). First, we will explain how to use a commercially available emulsion (contained in a 60 mL container). Assuming that the amount used each time is about the area of a 100 yen coin (approximately 2.5 mL per use), one commercially available emulsion can be used 24 times. In other words, if the emulsion's ability to slide off is maintained even after the 24th use, the appearance (transparency) of the container will be well maintained, and the emulsion container can be evaluated as having slide durability. The action of using a commercially available lotion once involves lifting the container from the upright position, tilting it (to dispense the lotion), and then returning it to the upright position, which is an "upright → inverted → upright" action. Therefore, repeating the inversion action in the above test up to 48 times is equivalent to the number of uses of one commercially available lotion (24 times). Therefore, by repeating the inversion work up to 100 times, which is more than twice the number of times, and if there is no lotion adhering (residual) to the inner surface of the container by the start of the 100th inversion and the lotion can be visually confirmed to be sliding down, it can be determined that "slide durability (durability of lotion removal) is present." After the 100th inversion, the evaluation of slide durability itself was continued until the start of the 200th inversion, which is twice the number of times, and the evaluation was terminated at the same time as the start of the 200th inversion.
[0055] In the sliding durability test, in order to properly evaluate the sliding durability of lotion and also the sliding speed of lotion, we decided to use the "number of times per 12 hours (including holidays)". In general, it is assumed that commercially available lotions are used twice a day (every 12 hours). Therefore, it is desirable that after the container is inverted, at the longest, 12 hours later, there is almost no lotion remaining on the inner surface of the container and the lotion can be visually confirmed to have slid down. In other words, in the above sliding durability test, if the number of inversions per 12 hours is 1 or more, the evaluation of sliding durability is high. Therefore, we decided to introduce the "number of times per 12 hours" as a numerical value indicating the degree of sliding durability. However, considering that lotion is often left unused on holidays, etc., the criterion for judging whether there is sliding durability is 0.71 times (≒ 1 time x 5 days / 7 days) or more per 12 hours (including holidays). For example, if the reversal operation has reached its 200th time (reversal count: 199 times) and 54 days have passed since then, the number of times per 12 hours (including holidays) is calculated as 199 times / (54 days x 2) = 1.84 times.
[0056] After inversion, the container was left alone until it was determined that the lotion had slid off, so if the lotion continued to adhere indefinitely, the evaluation was terminated after a certain period of time had passed. In this case, the number of inversions per 12 hours was calculated from the number of inversions at the last inversion and the number of days that had passed. For example, if the number of inversions at the last inversion was 37 and the number of days that had passed was 28, the number of inversions per 12 hours (including holidays) would be calculated as 37 times / (28 days x 2) = 0.66 times.
[0057] The degree of slip resistance was evaluated according to the following criteria: If the number of inversions per 12 hours (including holidays) was 0.71 or more (ratings A to C), there was no practical problem. A: 1.5 or more times per 12 hours (including holidays) B: Number of times per 12 hours (including holidays) is 1.0 or more and less than 1.5 C: Number of times per 12 hours (including holidays) is 0.71 or more and less than 1.0 D: Number of times per 12 hours (including holidays) is less than 0.71 Furthermore, since the amount used per application and the method of use vary depending on the type of lotion and the user, the evaluation criteria here are set merely as a guideline. The evaluation results using PET containers are shown in Tables 6 to 8.
[0058] [Table 6]
[0059] <Evaluation using lotion 1> As shown in Table 6, the number of times per 12 hours for Comparative Example 1-1 (PET substrate only) is used as the standard. The slippage resistance of the PET substrate was observed only for Emulsion 1. Comparative Example 30-1 did not use a resin, and only medium-chain fatty acid triglyceride (B-1) was applied, so the oil weight was 12 g / m 2Even if the oil is mixed with the medium chain triglyceride (B-1), the slip resistance is not obtained. Comparative Example 31-1 also does not have slip resistance because only the dimethyl silicone oil (B-2) is applied. In addition, in the case of a coating film containing only the medium chain triglyceride (B-1), the thickness of the entire coating film is substantially the thickness of the oil. In contrast, Examples 1-1 to 3-1 use a paint containing chlorinated polyolefin (A-1) and medium chain fatty acid triglyceride (B-1) in a blending ratio of 24:76, and the oil weight falls within a specified range, so all of them show sufficient slip resistance for practical use. In particular, it is possible to increase the oil weight and film thickness by changing the amount of application, and in Examples 1-1 and 2-1, the oil weight and the overall film thickness of the coating are relatively large. Example 1-1, which has large values for these values, shows excellent slip resistance, and Example 2-1, which has the next largest values, shows good slip resistance. In the table, when the "Number of times" column indicates 199, this indicates that the evaluation ended at the same time as the start of the next 200th time.
[0060] [Table 7]
[0061] <Test using lotion 2> Example 1-2 in Table 7 is the same coating as Example 1-1, and shows excellent slip resistance to emulsion 2. Example 30-2 has half the oil weight of Example 1-2, but maintains good slip resistance even after 143 repeated operations. For those still undergoing evaluation, such as Example 30-2, "ongoing" is indicated in the remarks column. Example 31-2 has a relatively small oil weight, but shows sufficient slip resistance for practical use. In Example 17-2, a paint containing vinyl chloride / vinyl acetate (A-2) and medium-chain fatty acid triglyceride (B-1) in a mixing ratio of 4:96 was used, and the oil weight was within the specified range, thereby showing excellent slip resistance against emulsion 2. In Comparative Example 5-2 in Table 7, since the oil is methylphenyl silicone oil (B-3), even if the blending ratio and oil weight are within the specified range, no slip-down durability is obtained. The remarks column indicates that the evaluation was terminated because the emulsion remained on the side wall of the container in the form of vertical stripes even after a certain period of time had passed after the 113th repeated operation. In Comparative Examples 2-2 and 3-2, since the resin is fluoroacrylic polysiloxane (A-3) and the blending ratio ((A) / (B)) is outside the specified range, neither of them can obtain a practically sufficient slip-down durability. In Comparative Example 30-2, as in Comparative Example 30-1, since no resin is used and only medium-chain fatty acid triglyceride (B-1) is applied, there is a limit to the increase in oil weight even if the amount applied is adjusted. However, for emulsion 2, a practically sufficient slip-down durability is obtained. Note that Comparative Example 1-2 is the case of only a PET substrate, and in Comparative Example 1-2, the slip-down durability of the PET substrate for emulsion 2 cannot be obtained.
[0062] [Table 8]
[0063] <Tests using emulsion 3, emulsion 7, emulsion 10, and emulsion 12> Comparative Examples 1-3, 1-7, 1-10, and 1-12 in Table 8 are for the PET substrate only, and the slippage durability of the PET substrate is evaluated for each emulsion. As a result, the slippage durability of the PET substrate is not obtained for any emulsion. In contrast, in Examples 1-3, 1-7, 30-10, and 30-12, a coating film was formed on a PET substrate using the same paint as in Example 1-1 (a paint containing (A-1) and (B-1) in a mixing ratio of 24:76), and the slide-off durability of each emulsion was evaluated. Although there was variation in the oil weight of each emulsion, it was within the specified range, and therefore sufficient slide-off durability was obtained for each emulsion. In addition, in Examples 17-3 and 17-10 in Table 8, a coating film was formed on a PET substrate using the same paint as in Example 17-2 (a paint containing (A-2) and (B-1) in a mixing ratio of 4:96), and the slide-off durability was evaluated for emulsion 3 and emulsion 10. As a result, both emulsion 3 and emulsion 10 showed excellent slide-off durability.
[0064] Next, the evaluation results using glass containers are shown in Tables 9 to 11.
[0065] [Table 9]
[0066] <Test using lotion 1> As shown in Table 9, in Examples 40-1, 41-1, 16-1, and 42-1, the same paint as in Example 1-1 was used on the glass substrate to form a coating film at the same blending ratio, and the oil weight of the coating film was within a specified range, so all of them showed sufficient slip-off durability for practical use with respect to emulsion 1. In particular, it was possible to increase the oil weight and the overall coating film thickness by changing the coating amount, and the oil weight and the overall coating film thickness were relatively large in Examples 40-1, 41-1, and 16-1. Example 40-1, which has a large value for these values, showed excellent slip-off durability, and Examples 41-1 and 16-1, which have the next largest values, showed good slip-off durability. In contrast, in Comparative Example 26-1 in Table 9, no resin was used and only the medium-chain fatty acid triglyceride (B-1) was applied, so the oil weight was 11 g / m 2 However, the slip resistance to emulsion 1 is not obtained. Comparative Example 19-1 is the case of only a glass substrate (WJ type glass container), and does not provide the sliding durability of the glass substrate for emulsion 1. Furthermore, Comparative Example 40-1 is the case of only a glass substrate (SV type glass container), and does not provide the sliding durability of the glass substrate for emulsion 1. Thus, for emulsion 1, neither of the two types of glass substrates (glass containers) provided the sliding durability.
[0067] [Table 10]
[0068] <Test using lotion 2> In Example 40-2, Example 14-2, Example 13-2, Example 15-2, and Example 16-2 in Table 10, a coating film was formed on a glass substrate using the same paint as in Example 1-1 (a paint containing (A-1) and (B-1) in a mixing ratio of 24:76), and the sliding resistance to emulsion 2 was evaluated. Although there was variation in the oil weight of each, it was within the specified range. As a result, all of the coating films showed good sliding resistance to emulsion 2. Furthermore, when comparing the three Examples with similar oil weights while focusing on the difference in the shape of the glass container (WJ type or SV type), Example 14-2 (WJ type, 24 g / m 2 , 1.03 times per 12 hours), Example 13-2 (SV type, 33 g / m 2 , 2.62 times per 12 hours), Example 15-2 (WJ type, 41 g / m 2 , 1.33 times per 12 hours), The difference in the shape of the glass container is as follows: Shoulder shape (WJ type: square shoulders, SV type: sloping shoulders), Shape of the bottom (WJ type: dome-shaped with a convex inner surface, SV type: flat), Sidewall shape (WJ type: non-uniform thickness, with steps; SV type: uniform thickness, flat) This is thought to be the reason for the difference in resistance to sliding, with the SV type showing superior resistance to sliding compared to the WJ type. Example 12-2 is a case where the ratio of (A-1) is increased within a prescribed range of the compounding ratio of (A-1) and (B-1), and shows sufficient slippage resistance for practical use with respect to emulsion 2. In Comparative Example 9-2 in Table 10, the same paint as in Example 12-2 was used, but the oil weight was smaller than the prescribed range, so no slippage durability was obtained. In Comparative Examples 41-2, 42-2, 43-2, 44-2, 45-2, and 46-2 in Table 10, the resin is fluoroacrylic polysiloxane (A-3), and the compounding ratio ((A) / (B)) is changed in various ways within the range of 10 / 90 to 100 / 0, but none of them have sufficient slip resistance for practical use. Note that Comparative Example 46-2 is a coating film made only of fluoroacrylic polysiloxane (A-3) without using oil. Comparative Example 19-2 was the case of only a WJ type glass container, and Comparative Example 6-2 was the case of only an SV type glass container. For emulsion 2, neither of the two types of glass substrates (glass containers) exhibited resistance to slipping.
[0069] [Table 11]
[0070] <Test using emulsion 3 and 11> Comparative Examples 19-3 and 19-11 in Table 11 are the cases where only the glass substrate is used, and the slide-down durability of the glass substrate is evaluated for each emulsion. As a result, no slide-down durability of the glass substrate is obtained for any of the emulsions. In contrast, in Examples 16-3 and 16-11, a coating film was formed on a glass substrate using the same paint as in Example 1-1 (a paint containing (A-1) and (B-1) in a mixing ratio of 24:76), and the slide-off durability of each emulsion was evaluated. Since the oil weights of each were within the specified range, emulsion 3 and emulsion 11 had sufficient slide-off durability for practical use.
[0071] <Evaluation of the sliding durability of sliding films based on the adhesive energy of emulsion> Since the durability to slipping off differs depending on the type of emulsion, the inventors attempted to evaluate the durability to slipping off based on the adhesion energy of the emulsion to the coating film (referred to as adhesion energy A).
[0072] "How to calculate adhesion energy" In general, the interfacial free energy (γLS) between a coating film and an emulsion is expressed by equation (2). γLS=γL+γS-2√(γLd·γSd) ···(2) where γL is the surface free energy of the emulsion, (Hereafter, unless otherwise specified, it refers to the sum of the variance component and the polarity component.) γS: Surface free energy of the coating film, γLd: surface free energy of emulsion (dispersion component), γSd: Surface free energy of the coating film (dispersion component). is based on the theoretical formula of Fowkes. Fowkes hypothesized that only dispersion forces act between nonpolar molecules and between nonpolar and polar molecules, and that the interaction is expressed as the geometric mean of the surface tensions of each, and proposed the theoretical formula (2) for the interfacial tension between solids and liquids in 1964. On the other hand, the adhesion energy (WSL) is expressed by the Young's equation "γSV=γLVcosθ+γSL" and the Dupre's equation "γSV+γLV=WSL+γSL", as shown in formula (3). WSL = γSV + γLV - γSL (3) Using the symbols in equation (2), equation (3) can be expressed as equation (4). WSL = γL + γS - γLS (4) In this way, the adhesion energy A of the emulsion to the coating film is expressed as "γL + γS - γLS." In other words, the surface free energies γL, γS, γLd, and γSd in equation (2) are calculated using the theoretical equation of surface free energy, Kaelble and Uy, and the contact angle of a 10 μL droplet of the reagent is measured using a contact angle meter, as described in the explanation of the surface free energy in Table 1. Then, γLS can be obtained from equation (2), and the adhesion energy A, expressed as WSL, can be obtained from equation (4).
[0073] Here, the adhesion energy of the emulsion to the coating (adhesion energy A) was calculated for each emulsion. For comparison, the adhesion energy of the emulsion to the substrate and the adhesion energy of the emulsion to the coating (oil only) were also calculated. Furthermore, the inventors similarly calculated the adhesion energy of the coating to the substrate (called adhesion energy B) using the above theory. This is based on the prediction that if the adhesion energy B of the coating film is greater than the adhesion energy A of the emulsion, good resistance to sliding off against the emulsion will be obtained.
[0074] These adhesion energies can be calculated using the measured surface free energy values shown in Tables 2 to 5.
[0075] FIG. 5 shows the evaluation results based on the adhesion energy A of emulsion 1 when the sliding film of representative Manufacturing Example 1 (A-1:B-1=24:76) was formed on a PET substrate. In Comparative Example 1-1, the adhesion energy A of emulsion 1 to the PET substrate is relatively large. In Comparative Example 30-1, a coating film (medium-chain fatty acid triglyceride only) is formed, and the adhesion energy A of emulsion 1 to the coating film is reduced. However, the test result of sliding durability is poor (D). In contrast, when a coating film (chlorinated polyolefin + medium-chain fatty acid triglyceride) was formed in Example 3-1, the adhesion energies A and B were equivalent to those of Comparative Example 30-1, but a specified slip resistance was obtained even with a smaller oil weight. Furthermore, in Example 2-1 and Example 1-1, the coating contains chlorinated polyolefin, so that a sliding film with a large oil weight is formed. Also, the adhesion energy B of the coating is larger than the adhesion energy A of the emulsion. These are considered to be one of the reasons why excellent sliding durability was obtained.
[0076] Figure 5 also shows the evaluation results based on the adhesion energy A of emulsion 2. In Comparative Example 1-2, the adhesion energy A of emulsion 2 to the PET substrate is relatively large, and the test result for slip resistance is poor. In Comparative Example 30-2, by forming a coating film (medium-chain fatty acid triglyceride only), the adhesion energy A of emulsion 1 to the coating film is reduced, and the test result for slip resistance is slightly improved. In contrast, in Example 31-2, a coating film (chlorinated polyolefin + medium-chain fatty acid triglyceride) was formed, and while the adhesion energies A and B were equivalent to those of Comparative Example 30-2, a certain level of slip resistance was achieved even with a smaller amount of oil. Furthermore, in Example 30-2 and Example 1-2, the coating contains chlorinated polyolefin, so a sliding film with a large oil weight is formed. Also, the adhesion energy B of the coating is greater than the adhesion energy A of the emulsion. Thus, the results were similar to those of emulsion 1.
[0077] In addition, Fig. 6 shows the evaluation results based on the adhesion energy A of emulsion 2 when the sliding films of Production Example 1 and Production Example 2 (A-1:B-1 = 46:54) were formed on a glass substrate. Fig. 6 shows that the sliding film of this embodiment can achieve the same effect on a glass substrate.
[0078] In addition, the adhesion energy of the emulsion to the PET substrate on which the sliding film of Production Example 1 was formed and to the PET substrate as is is shown in Figure 7. According to this, for each emulsion, the adhesion energy B of the coating to the PET substrate (measured value: 55.30 mJ / m) was greater than the adhesion energy A of the emulsion to the sliding film. 2 For convenience, the scale of the horizontal axis in Fig. 7 is different between the left and right halves. In addition, the results of FIG. 7 show that the adhesion energy of various emulsions is 20 mJ / m2 when the PET substrate has the sliding film of this embodiment compared to the case of the PET substrate alone. 2 For example, the decrease is 20-25 mJ / m 2 It was revealed that the emulsion was easily able to slide off due to the sliding membrane of this example.
[0079] Similarly, the adhesion energy of the emulsion to a glass substrate (WJ type) on which the sliding film of Production Example 1 was formed and to a glass substrate (WJ type) as is was calculated, and the results are shown in Figure 8. In addition, the results of FIG. 8 show that the adhesion energy of various emulsions is 4 mJ / m2 when the glass substrate has the sliding film of this embodiment, compared to the case of the glass substrate alone. 2 For example, the decrease is 4 to 5 mJ / m 2It was revealed that the emulsion was easily able to slide off due to the sliding membrane of this example.
[0080] The calculated adhesion energy A of the emulsion for each of the Examples and Comparative Examples is shown below in Table 12 (PET substrate) and Table 13 (glass substrate) together with the test results of slippage durability.
[0081] [Table 12]
[0082] [Table 13]
[0083] Table 14 shows the calculated adhesion energy B of the coating to the substrate.
[0084] [Table 14]
[0085] Here, in order to further examine the relationship between the adhesion energy A of the emulsion and the adhesion energy B of the coating film to the substrate, Comparative Examples 50-1 to 50-5 were added to Example 2-1, and the evaluation results are shown in Table 15. For slip resistance, the target value for the number of times per 12 hours (including holidays) is 0.71, and the target value for the number of repetitions is 199. Example 2-1 and Comparative Example 50-4 (oil only) are the only two that achieved both target values.
[0086] [Table 15]
[0087] The ratio (B / A) of the adhesion energy B of the sliding film of this embodiment to the PET substrate and the adhesion energy A of emulsion 1 to the sliding film is 1.265 because the emulsion and the substrate are the same. That is, the results in Table 15 are plotted on a function of B / A=1.265 in a graph with adhesion energy B on the vertical axis and adhesion energy A on the horizontal axis (see FIG. 9).
[0088] In Figure 9, the smaller the adhesion energy A on the horizontal axis, the more difficult it is for the emulsion to adhere, and the greater the adhesion energy B on the vertical axis, the better the adhesion of the sliding film to the substrate. Those that have reached the target value are indicated with a "black circle," and those that have not reached the target value are indicated with a "white circle." As mentioned above, since the ratio (B / A) is constant, it can be said that reducing the adhesion energy A is important in improving the emulsion removal performance. As shown in Figure 9, the smaller the adhesion energy A, the greater the number of times per 12 hours, so it is advisable to lower the adhesion energy A depending on the sliding film conditions. In the case of emulsion 1, the boundary between those that meet the target value and those that do not is when the adhesion energy A is 43.72 to 46.36 mJ / m 2 It is estimated to be in the range.
[0089] The ratio of adhesion energies (B / A) is theoretically expressed as follows: B / A=√(dispersion component of base material / dispersion component of emulsion) It is expressed by and is determined by the dispersion component of the surface free energy of the substrate and the dispersion component of the surface free energy of the emulsion. Therefore, in order to make the adhesion energy ratio (B / A) 1 or more, as shown in Table 4, a PET substrate with a relatively large dispersion component is advantageous. In the case of a glass substrate, depending on the characteristics of the emulsion, it may be difficult to make the adhesion energy ratio (B / A) 1 or more. However, as shown in the examples (Examples 40-1, 41-1, 16-1, and 42-1 of emulsion 1, and Example 16-11 of emulsion 11, etc.), there are some that show good slip-off durability even under conditions where the ratio (B / A) is not 1 or more. In these examples, it is difficult to make the adhesion energy ratio (B / A) 1 or more, but good slip-off durability is ensured by reducing the adhesion energy A of the emulsion to the coating film.
[0090] When the adhesion energy ratio (B / A) is the same and the adhesion energy A is also the same (for example, Examples 1-1, 2-1, 3-1, etc. of emulsion 1 in FIG. 5), the number of times per 12 hours increases with the oil weight. From the results of this example, the oil weight is 3.7 to 81 g / m 2 It is recommended that the thickness is 3.7g / m 2 If the above is true, sufficient slip resistance for practical use is obtained.
Claims
1. (A) component: a thermoplastic resin; (B) component: medium chain fatty acid triglyceride, A solvent, A sliding film forming paint, characterized in that the blending ratio ((A) / (B)) of the component (A) to the component (B) is 4 / 96 to 46 / 54.
2. A slip film formed on the surface of a substrate, (A) component: a thermoplastic resin; (B) component: medium chain fatty acid triglyceride; The blending ratio ((A) / (B)) of the (A) component and the (B) component is 4 / 96 to 46 / 54, and the weight of the (B) component per area of the slip membrane is 3.7 to 81 g / m 2 A decidua characterized by:
3. The slip membrane according to claim 2, characterized in that the membrane has a thickness of 5 to 109 μm.
4. The object to be slid down is emulsion, 4. The sliding film according to claim 2 or 3, characterized in that the adhesion energy of the sliding film to the substrate is greater than the adhesion energy of the emulsion to the sliding film.
Citation Information
Patent Citations
Falling film
JP2018184536A
Sliding-down agent and article coated with coating thereof
JP2019218462A
Coating agent, coating film and article using the same, and snow accretion prevention method of article surface
JP2020084127A