Decorative sheet and decorative plate
The decorative sheet and board address deformation issues by using a polypropylene-based thermoplastic resin with nano-sized additives and a surface protective layer, achieving low moisture permeability and improved scratch resistance.
Patent Information
- Application Number
- JP2023051498
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Decorative sheets deform due to temperature and humidity differences between indoors and outdoors.
A decorative sheet comprising a base material layer made of polypropylene-based thermoplastic resin with nano-sized additive dispersion, a pattern layer, and a surface protective layer, with moisture permeability of 5 g/m²·24 hours or less, and a decorative board with a substrate and laminated decorative sheet.
The solution suppresses deformation of the decorative sheet by reducing moisture permeability and enhancing scratch resistance, allowing for a durable and designable surface.
Smart Images

Figure 2024140382000001_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a decorative sheet and a decorative board. [Background technology]
[0002] As a decorative sheet technology for protecting a design from surface wear, for example, Patent Document 1 discloses a technology in which a transparent olefin sheet is laminated to a colored olefin sheet to create a multi-layered decorative sheet. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2015-199313 A Summary of the Invention [Problem to be solved by the invention]
[0004] Decorative sheets having conventional configurations, including the technology disclosed in Patent Document 1, have the problem that deformation of the decorative sheet occurs due to temperature and humidity differences between indoors and outdoors. In view of the above-mentioned problems, an object of the present invention is to provide a decorative sheet and a decorative board that are capable of suppressing deformation of the decorative sheet. [Means for solving the problem]
[0005] In order to solve the above-mentioned problems, one aspect of the present invention is a sheet-like material having a base layer, a pattern layer, and a surface protective layer, and having a moisture permeability of 5 g / m 2 A decorative sheet with a shelf life of 24 hours or less. The base layer is made of a polypropylene-based thermoplastic resin, and is a layer to which a dispersion material as a nano-sized additive has been added. The picture pattern layer is a layer laminated on one side of the base layer, and on which a picture is formed. The surface protection layer is a layer laminated on one side of the picture pattern layer. In order to solve the above-mentioned problems, one aspect of the present invention is a decorative board comprising a substrate and a decorative sheet laminated on at least one surface of the substrate. Effect of the Invention
[0006] According to one aspect of the present invention, it is possible to provide a decorative sheet and a decorative board that are capable of suppressing deformation of the decorative sheet. [Brief description of the drawings]
[0007] [Figure 1] FIG. 2 is a cross-sectional view showing a configuration of a decorative board in the first embodiment. [Diagram 2] 1 is a schematic diagram showing the positional relationship between the lines formed by the portion to which the gloss coat is applied and the lines forming the pattern formed in the picture pattern layer. FIG. [Diagram 3] FIG. 4 is a cross-sectional view showing a configuration of a decorative board in a modified example of the first embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] Hereinafter, an embodiment of the present technology will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted with the same or similar reference numerals, and duplicated descriptions are omitted. Each drawing is schematic and may differ from the actual one. The embodiments shown below are examples of devices and methods for embodying the technical idea of the present technology, and the technical idea of the present technology is not limited to the devices and methods exemplified in the following embodiments. The technical idea of the present technology can be modified in various ways within the technical scope described in the claims. In addition, the directions of "left and right" and "up and down" in the following description are merely definitions for the convenience of explanation and do not limit the technical idea of the present invention. Therefore, for example, if the paper is rotated 90 degrees, "left and right" and "up and down" are read interchangeably, and of course, if the paper is rotated 180 degrees, "left" becomes "right" and "right" becomes "left".
[0009] First embodiment Hereinafter, the configuration of a decorative sheet 1 in a first embodiment will be described with reference to FIG. The decorative sheet 1 is used, for example, indoors. Specifically, it is attached to the surfaces of fittings (interior doors, entrance storage) and construction materials (trimmings, moldings, baseboards, window frames, door frames), etc., and is used to match the patterns of fittings and construction materials for each house or room. As shown in FIG. 1, the decorative sheet 1 includes a base layer 2, a colored layer 3, a picture design layer 4, a surface protective layer 5, a moisture-proof layer 6, and a primer layer 7.
[0010] <Base material layer> The base layer 2 is a base layer formed using a polypropylene-based thermoplastic resin, and is a layer that forms the support of the decorative sheet 1. The base layer 2 includes a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c, and is manufactured by extrusion molding, for example. In FIG. 1, the base layer 2 is illustrated as if the first transparent layer 2a, the core layer 2b, and the second transparent layer 2c form separate layers, but in reality, the first transparent layer 2a, the core layer 2b, and the second transparent layer 2c are formed continuously. Therefore, there is no interface between the first transparent layer 2a and the core layer 2b, and no interface between the core layer 2b and the second transparent layer 2c. In the first embodiment, simultaneous extrusion is performed so that the ratio of the thickness of the first transparent layer 2a:the thickness of the core layer 2b:the thickness of the second transparent layer 2c is 0.5:9:0.5, and the thickness of the base layer 2 is 50 μm.
[0011] (first transparent layer) The first transparent layer 2a is formed by adding a dispersant as a nano-sized additive to a transparent polypropylene-based thermoplastic resin. In addition to the dispersant as a nano-sized additive, an inorganic filler is added to the first transparent layer 2a.
[0012] Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, polyarylate, and polycarbonate; and olefin copolymers such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-(meth)acrylic acid (ester) copolymer, and ethylene-unsaturated carboxylic acid copolymer metal neutralized product (ionomer). Examples of the resin that can be used include polyolefin resins such as poly(meth)acrylonitrile, polymethyl(meth)acrylate, polyethyl(meth)acrylate, polybutyl(meth)acrylate, and polyacrylamide; polyamide resins such as 6-nylon, 6,6-nylon, and 6,10-nylon; styrene resins such as polystyrene, AS resin, and ABS resin; vinyl resins such as polyvinyl chloride, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, and polyvinyl butyral; fluorine resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, and ethylene-perfluoroalkyl vinyl ether copolymer; and mixtures, copolymers, composites, and laminates using two or more of the above-mentioned resins.
[0013] In particular, in light of the recent growing social interest in environmental issues, it is not preferable to use thermoplastic resins that contain chlorine (halogen), such as polyvinyl chloride resins, as thermoplastic resins, and it is preferable to use non-halogen thermoplastic resins. In addition, in consideration of various physical properties, processability, versatility, economic efficiency, etc., it is most preferable to use a polyester resin (amorphous or biaxially oriented) or a polyolefin resin, particularly a polyolefin resin, as the non-halogen-based thermoplastic resin. For example, it is preferable to use a polypropylene resin containing 30% by mass or more and 100% by mass or less of a highly crystalline homopolypropylene resin having an isotactic pentad fraction (mmmm fraction) of 95% or more as the polyolefin resin.
[0014] Examples of thermoplastic resins include polyolefin resins such as polyethylene, polypropylene, polymethylpentene, polybutene, ethylene-propylene copolymer, ethylene-α-olefin copolymer, and propylene-α-olefin copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, polytetramethylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-isophthalate copolymer, 1,4-cyclohexanedimethanol copolymerized polyethylene terephthalate, polyarylate, and polycarbonate; and olefin copolymers such as ethylene-vinyl acetate copolymer, ethylene-vinyl alcohol copolymer, ethylene-(meth)acrylic acid (ester) copolymer, and ethylene-unsaturated carboxylic acid copolymer metal neutralized product (ionomer). Examples of the resin that can be used include polyolefin resins such as poly(meth)acrylonitrile, polymethyl(meth)acrylate, polyethyl(meth)acrylate, polybutyl(meth)acrylate, and polyacrylamide; polyamide resins such as 6-nylon, 6,6-nylon, and 6,10-nylon; styrene resins such as polystyrene, AS resin, and ABS resin; vinyl resins such as polyvinyl chloride, polyvinyl acetate, polyvinyl alcohol, polyvinyl acetal, and polyvinyl butyral; fluorine resins such as polyvinyl fluoride, polyvinylidene fluoride, polytetrafluoroethylene, ethylene-tetrafluoroethylene copolymer, and ethylene-perfluoroalkyl vinyl ether copolymer; and mixtures, copolymers, composites, and laminates using two or more of the above-mentioned resins.
[0015] In particular, in light of the recent growing social interest in environmental issues, it is not preferable to use thermoplastic resins that contain chlorine (halogen), such as polyvinyl chloride resins, as thermoplastic resins, and it is preferable to use non-halogen thermoplastic resins. In addition, in consideration of various physical properties, processability, versatility, economic efficiency, etc., it is most preferable to use a polyester resin (amorphous or biaxially oriented) or a polyolefin resin, particularly a polyolefin resin, as the non-halogen-based thermoplastic resin. For example, it is preferable to use a polypropylene resin containing 30% by mass or more and 100% by mass or less of a highly crystalline homopolypropylene resin having an isotactic pentad fraction (mmmm fraction) of 95% or more as the polyolefin resin.
[0016] (Nano-sized additives) A nano-sized additive is an additive that has been made into nano-sized particles by a technique for nano-sizing the additive (nanofiber processing). The nano-sized nucleating agent is used by being added to the polypropylene resin in the form of a nucleating agent vesicle, which is encapsulated in a vesicle having a single-layer outer membrane. In addition, the nucleating agent in the resin constituting the first transparent layer 2a may be encapsulated in vesicles with a portion of the nucleating agent exposed. Since the first transparent layer 2a contains a nucleating agent, it is possible to improve the crystallinity and improve the scratch resistance (scratch resistance) of the decorative sheet 1.
[0017] (Particle size of nucleating agent) It is preferable that the average particle size of the nano-sized nucleating agent is less than half the wavelength range of visible light. Specifically, since the wavelength range of visible light is 400 nm or more and 750 nm or less, it is preferable that the average particle size is less than 375 nm. Nano-sized nucleating agents have extremely small particle sizes, so the number of nucleating agents present per unit volume and their surface area increase inversely proportional to the cube of the particle diameter. As a result, the distance between each nucleating agent particle becomes closer, so that when crystal growth occurs from the surface of one nucleating agent particle added to the resin, the end from which the crystal is growing immediately comes into contact with the end of the crystal growing from the surface of another nucleating agent particle adjacent to the one nucleating agent particle, and the ends of the crystals inhibit each other's growth, stopping the growth of each crystal. Therefore, it is possible to reduce the average particle size of the spherulites in the crystalline part of the crystalline resin, for example, to reduce the spherulite size to 1 μm or less.
[0018] As a result, it is possible to produce a resin film with a high degree of crystallinity and high hardness, and since the stress concentration between spherulites that occurs during bending is efficiently dispersed, it is possible to realize a resin film that suppresses cracking and whitening during bending. When a nucleating agent is simply added, the particle size increases due to secondary aggregation of the nucleating agent in the resin. On the other hand, when nucleating agent vesicles are added, the dispersibility in the resin is improved, and the number of crystal nuclei per amount of nucleating agent added is significantly increased compared to when the nucleating agent is simply added. This reduces the average particle size of the spherulites in the crystalline portion of the resin, making it possible to suppress the occurrence of cracks and whitening during bending. Therefore, by adding a vesicle nucleating agent, the degree of crystallization can be increased, making it possible to achieve both improved elastic modulus and processability.
[0019] The first transparent layer 2a is formed, for example, from a resin material to which a nucleating agent has been added in an amount preferably in the range of 0.05 parts by mass or more and 0.5 parts by mass or less, and more preferably 0.1 parts by mass or more and 0.3 parts by mass or less, per 100 parts by mass of a polypropylene-based thermoplastic resin. When nucleating agent vesicles are used, the amount of nucleating agent added to the resin material is the amount converted into the amount of nucleating agent encapsulated in the nucleating agent vesicles.
[0020] If the amount of the nucleating agent added is less than 0.05 parts by mass, the crystallinity of the polypropylene may not be improved sufficiently, and the scratch resistance of the first transparent layer 2a may not be improved sufficiently. Furthermore, if the amount of nucleating agent added exceeds 0.5 parts by mass, the spherulite growth of the polypropylene may be inhibited due to an excess of crystal nuclei, and as a result, the crystallinity of the polypropylene may not be sufficiently improved, and the scratch resistance of the first transparent layer 2a may not be sufficiently improved.
[0021] (Method to nano-size nucleating agents) In addition, the nucleating agent can be nano-sized by using, for example, a solid phase method, a liquid phase method, a gas phase method, or the like. The solid phase method is a method in which additives are mainly mechanically pulverized to obtain nano-sized particles. For the solid phase method, a ball mill, a bead mill, a rod mill, a colloid mill, a conical mill, a disk mill, a hammer mill, a jet mill, etc. can be used. The liquid phase method is a method for synthesizing or crystallizing nano-sized particles in an additive or a solution in which the additive is dissolved, and examples of the liquid phase method that can be used include a crystallization method, a co-precipitation method, a sol-gel method, a liquid phase reduction method, and a hydrothermal synthesis method. The gas phase method is a method for synthesizing or crystallizing nano-sized particles from additives or gas or vapor formed by additives. Examples of the gas phase method that can be used include an electric furnace method, a chemical flame method, a laser method, and a thermal plasma method.
[0022] A more specific method for the nano-processing will be described below. In a specific example of the solid phase method, for example, a mixture of 100 g of isopropyl alcohol and 50 g of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphonate is milled in a bead mill for 60 minutes using 30 μm stabilized zirconia beads to obtain nano-sized nucleating agent particles with an average particle size in the range of 100 nm to 150 nm.
[0023] In a specific example of the crystallization method, for example, a solution obtained by dissolving 50[g] of sodium 2,2'-methylenebis(4,6-di-tert-butylphenyl)phosphonate in a mixed solvent of 96[g] of xylene, 72[g] of isopropyl alcohol, and 24[g] of water is brought into contact with a poor solvent such as ethanol in a microreactor to precipitate nano-sized nucleating agent particles with an average particle size in the range of 1[nm] to 150[nm]. The additive-encapsulating vesicle is a vesicle-like capsule having a membrane structure closed in a spherical shell shape, and particularly, one containing a liquid phase inside is called an additive-encapsulating vesicle. In the present invention, the case where an additive is contained in the liquid phase will be described.
[0024] In addition, the additive-encapsulating vesicles have extremely high dispersibility and do not cause aggregation of particles due to the mutual repulsion of the outer membranes of the vesicles, and the mutual repulsion of the outer membranes of the vesicles makes it possible to uniformly disperse the additive in the resin composition constituting each resin layer. Among the nano-processing methods, methods for obtaining nano-sized additives as additive-encapsulating vesicles (vesicle processing) that can be used include, for example, the Bangham method, extrusion method, hydration method, surfactant dialysis method, reverse phase evaporation method, freeze-thaw method, and supercritical reverse phase evaporation method.
[0025] The vesicle formation process will now be described. The Bangham method involves putting chloroform or a chloroform / methanol mixed solvent into a flask or other container, then adding and dissolving phospholipids. The solvent is then removed using an evaporator to form a thin film containing lipids, and after adding a dispersion of additives, the mixture is hydrated and dispersed in a vortex mixer to obtain vesicles.
[0026] The extrusion method is a method for obtaining vesicles by preparing a thin film of phospholipid solution and passing it through a filter instead of a mixer used as an external perturbation in the Bangham method. The hydration method is a preparation method similar to the Bangham method, but in this method, vesicles are obtained by dispersing the particles by gentle stirring without using a mixer.
[0027] The reverse phase evaporation method involves dissolving phospholipids in diethyl ether or chloroform, adding a solution containing additives to form a W / O emulsion, removing the organic solvent from the emulsion under reduced pressure, and then adding water to obtain vesicles. The freeze-thaw method uses cooling and heating as an external perturbation, and is a method for obtaining vesicles by repeating cooling and heating. In particular, a method for obtaining an additive-encapsulating vesicle having a unilamellar outer membrane includes supercritical reverse phase evaporation.
[0028] The supercritical reverse phase evaporation method is a method for producing capsules (nano-sized vesicles) encapsulating a target substance using carbon dioxide under temperature or pressure conditions in a supercritical state or above the critical point. Carbon dioxide in a supercritical state refers to carbon dioxide in a supercritical state above the critical temperature (30.98°C) and critical pressure (7.3773±0.0030MPa). Carbon dioxide under temperature or pressure conditions above the critical point means carbon dioxide under conditions where only the critical temperature or only the critical pressure exceeds the critical conditions.
[0029] In the specific vesicle formation process using the supercritical reverse phase evaporation method, an emulsion of supercritical carbon dioxide and aqueous phase is generated by injecting an aqueous phase into a mixed fluid of supercritical carbon dioxide, phospholipids as an outer membrane forming substance, and additives as an encapsulating substance, and stirring the mixture.Then, by reducing the pressure, the carbon dioxide expands and evaporates, causing a phase inversion, and nanocapsules (nanovesicles) are generated in which the phospholipids cover the surface of the nucleating agent particles with a monolayer membrane.
[0030] By using the supercritical reverse phase evaporation method, unlike the conventional encapsulation method in which the dispersant forms multiple layers on the surface of the additive particles, it is possible to easily produce capsules with a single layer, making it possible to prepare capsules with a smaller diameter. The nucleating agent vesicle is prepared, for example, by the Bangham method, the extrusion method, the hydration method, the surfactant dialysis method, the reverse phase evaporation method, the freeze-thaw method, the supercritical reverse phase evaporation method, etc. The nucleating agent vesicle is particularly preferably prepared by the supercritical reverse phase evaporation method.
[0031] If it is desired to make the nanocapsule into a multi-membrane capsule, it is possible to easily produce it by injecting supercritical carbon dioxide into a mixed fluid of phospholipids, additives, and an aqueous phase. Examples of phospholipids used in preparing the additive-encapsulating vesicle include glycerophospholipids such as phosphatidylcholine, phosphatidiethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopine, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin, and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol. Furthermore, the additive-encapsulating vesicle can achieve excellent compatibility with resin materials by being provided with an outer membrane of phospholipids.
[0032] The additive-encapsulating vesicle may also have an outer membrane containing a dispersant, such as a polymeric surfactant, a fatty acid metal salt, a silane coupling agent, a titanate coupling agent, silicone, wax, or a modified resin. Examples of polymer surfactants include aliphatic polyvalent polycarboxylic acids, polycarboxylate alkylamines, polyacrylic acids, polymethacrylic acids, polyoxyethylene alkyl ethers, and sorbitan fatty acid esters.
[0033] Examples of fatty acid metal salts include those in which stearic acid, lauric acid, 12-hydroxystearic acid, montanic acid, behenic acid, ricinoleic acid, myristic acid, or the like is combined with lithium, sodium, potassium, magnesium, calcium, barium, zinc, aluminum, or the like. Examples of the silane coupling agent include 3-methacryloxypropyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyltriethoxysilane, vinyltrimethoxysilane, phenyltrimethoxysilane, 3-isocyanatepropyltriethoxysilane, and 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane.
[0034] Titanate coupling agents include tetrakis[2,2-bis(allyloxymethyl)butoxy]titanium(IV), di-i-propoxytitanium diisostearate, (2-n-butoxycarbonylbenzoyloxy)tributoxytitanium, isopropyl titanium triisostearate, di-n-butoxy bis(triethanolaminato)titanium, tetrakis(2-ethylhexyloxy)titanium, and di-i-propoxy bis(acetylacetonato)titanium.
[0035] Examples of silicones include those obtained by polymerizing olefins or pyrolyzing polyolefins, such as dimethylsilicone oil, methylphenylsilicone oil, methylhydrogensilicone oil, cyclic dimethylsilicone oil, alkyl-modified silicone oil, long-chain alkyl-modified silicone oil, and higher fatty acid-modified silicone oil, and further oxidizing or modifying them with maleic acid, sulfonic acid, carboxylic acid, rosin acid, or the like. Examples of the resin include polyolefins modified with maleic acid, sulfonic acid, carboxylic acid, rosin acid, and the like.
[0036] (The outer membrane that constitutes the nucleating agent vesicle) The outer membrane constituting the nucleating agent vesicle is, for example, composed of a monolayer membrane. Also, the outer membrane constituting the nucleating agent vesicle is, for example, composed of a substance containing a biological lipid such as a phospholipid. In the following description, a nucleating vesicle whose outer membrane is composed of a substance containing a biological lipid such as a phospholipid may be referred to as a nucleating liposome. Examples of phospholipids constituting the outer membrane include glycerophospholipids such as phosphatidylcholine, phosphatidylethanolamine, phosphatidylserine, phosphatidic acid, phosphatidylglycerol, phosphatidylinositol, cardiopin, yolk egg lecithin, hydrogenated yolk egg lecithin, soybean lecithin, and hydrogenated soybean lecithin; and sphingophospholipids such as sphingomyelin, ceramide phosphorylethanolamine, and ceramide phosphorylglycerol.
[0037] (Other substances that form the outer membrane) Other substances that may form the outer membrane of the vesicle include dispersants such as nonionic surfactants and mixtures of nonionic surfactants with cholesterols or triacylglycerols. As the nonionic surfactant, for example, one or more of polyglycerin ether, dialkyl glycerin, polyoxyethylene hydrogenated castor oil, polyoxyethylene alkyl ether, polyoxyethylene sorbitan fatty acid ester, sorbitan fatty acid ester, polyoxyethylene polyoxypropylene copolymer, polybutadiene-polyoxyethylene copolymer, polybutadiene-poly(2-vinylpyridine), polystyrene-polyacrylic acid copolymer, polyethylene oxide-polyethylethylene copolymer, polyoxyethylene-polycaprolactam copolymer, etc. can be used.
[0038] As cholesterols, for example, cholesterol, α-cholestanol, β-cholestanol, cholestane, desmosterol (5,24-cholestadiene-3β-ol), sodium cholate, cholecalciferol, and the like can be used. The outer membrane of the liposome may also be formed from a mixture of phospholipids and a dispersing agent.
[0039] In the first embodiment, it is preferable that the nucleating agent vesicle is a radical scavenger liposome having an outer membrane formed by phospholipids. This is because by forming the outer membrane from phospholipids, it is possible to improve the compatibility between the vesicle and the resin material that is the main component of the decorative sheet 1. Note that the "main component" refers to, for example, a resin material that accounts for 50% or more by mass of the resin material that constitutes the base layer.
[0040] The nucleating agent is not particularly limited as long as it is a substance that serves as a starting point for crystallization when the resin crystallizes. Examples of the nucleating agent include metal phosphate salts, metal benzoate salts, metal pimelate salts, metal rosin salts, benzylidene sorbitol, quinacridone, cyanine blue, talc, and the like. In particular, in order to maximize the effect of the nano-processing, it is preferable to use metal phosphate salts, metal benzoate salts, metal pimelate salts, and metal rosin salts that are non-melting and expected to have good transparency, but if the material itself can be made transparent by the nano-processing, colored quinacridone, cyanine blue, talc, and the like can also be used. In addition, a non-melting nucleating agent may be appropriately mixed with melting benzylidene sorbitol.
[0041] (Core layer 2b) The core layer 2b is laminated on one surface (the upper surface in FIG. 1) of the first transparent layer 2a, and is formed, for example, using a transparent polypropylene-based thermoplastic resin blended with a weathering agent. If necessary, the core layer 2b may contain one or more additives selected from various additives such as a filler, an ultraviolet absorber, a light stabilizer, a heat stabilizer, an antioxidant, an antistatic agent, a lubricant, a flame retardant, an antibacterial agent, an antifungal agent, an antifriction agent, a light scattering agent, and a gloss adjuster.
[0042] (Second transparent layer) The second transparent layer 2c is laminated on one surface (the upper surface in FIG. 1) of the core layer 2b, and is made of a transparent polypropylene-based thermoplastic resin. In addition to a dispersant as a nano-sized additive, an inorganic filler is added to the second transparent layer 2c. Based on the above, in the first embodiment, a configuration of the base material layer 2 is described in which the base material layer 2 is formed of two types of three layers, that is, a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c, stacked in that order.
[0043] (Characteristics of the base layer) The decorative sheet 1 is characterized in that the base layer 2 contains a resin material and a nucleating agent. Furthermore, the decorative sheet 1 is characterized in that a nucleating agent encapsulated in vesicles is added to the resin material to crystallize the resin material when forming the base layer 2. By adding the nucleating agent encapsulated in vesicles to the resin composition, the dispersibility of the nucleating agent in the resin material, i.e., in the base layer 2, is dramatically improved. On the other hand, it may be difficult to directly identify the nucleating agent encapsulated in the vesicle based on the structure and properties of the finished decorative sheet 1, depending on the circumstances, and it may be considered impractical. The reasons for this are as follows.
[0044] The nucleating agent added in the form of a vesicle is dispersed with high dispersibility, and is highly dispersed in the base layer even in the laminate state, which is the precursor of the produced decorative sheet 1. However, in the process of producing the decorative sheet 1, the laminate is usually subjected to various treatments such as compression and hardening, which may cause the outer membrane of the vesicles encapsulating the nucleating agent to break down or cause chemical reactions. Therefore, depending on the processing process of the decorative sheet 1, there is a high possibility that the outer membrane of the nucleating agent in the finished decorative sheet 1 may be broken down, or the state of the chemical reaction may vary, resulting in the nucleating agent not being encapsulated (enveloped) by the outer membrane.
[0045] Furthermore, when the nucleating agent is not encapsulated in the outer membrane, it is difficult to specify the physical properties of the nucleating agent itself within a numerical range, and it is also anticipated that it may be difficult to determine whether the material constituting the crushed outer membrane is the outer membrane of the vesicle or a material added separately from the nucleating agent. Thus, although the present disclosure differs from the prior art in that the nucleating agent is highly dispersed in the decorative sheet 1, it is anticipated that there may be cases in which it is impractical to determine the structure and characteristics of the decorative sheet 1 within a numerical range analyzed based on measurements, whether this is because the nucleating agent is added in the form of vesicles encapsulating the nucleating agent.
[0046] As described above, the base layer 2 contains a dispersion material as a nano-sized additive. The base layer 2 is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to a polypropylene-based thermoplastic resin. Furthermore, the amount of the nucleating agent vesicles added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicles, per 100 parts by mass of the polypropylene-based thermoplastic resin.
[0047] In addition, the first transparent layer 2a and the second transparent layer 2c are formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin. Additionally, nucleating vesicles are nucleating liposomes with an outer membrane formed using phospholipids. Furthermore, the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a monolayer membrane, and then forming the vesicle by supercritical reverse phase evaporation.
[0048] <Colored layer> The colored layer 3 is laminated on one surface of the base layer (the upper surface in FIG. 1), and is formed by using a known printing method (for example, gravure printing). The colored layer 3 is formed to be transparent or semi-transparent.
[0049] <Pattern layer> The picture pattern layer 4 is laminated on one surface (the upper surface in FIG. 1) of the base layer with the colored layer 3 sandwiched therebetween, and is a layer on which a picture is formed to impart design to the decorative sheet 1. In other words, the colored layer 3 is a layer disposed between the base layer 2 and the surface protective layer 5. The picture pattern layer 4 is formed by printing a picture with a urethane resin by, for example, gravure printing. Note that, as a printing method for forming the picture pattern layer 4, various printing methods can be used other than gravure printing, such as offset printing, letterpress printing, flexographic printing, screen printing, inkjet printing, and electrostatic printing.
[0050] The type of pattern formed on the picture pattern layer 4 can be any type depending on the purpose of use, the preferences of the user, etc., and can be a wood grain pattern, a stone pattern, a fabric pattern, an abstract pattern, a geometric pattern, letters, symbols, a solid color, or a combination thereof. The type of pattern can also be, for example, a full-surface solid print. As the printing ink used to form the picture pattern layer 4, in addition to the urethane resin, for example, organic or inorganic dyes, pigments, and other colorants can be used.
[0051] The weight of the picture pattern layer 4 after drying is preferably 0.1 [g / m 2 ] or more than 15[g / m 2 ] or less, more preferably 3 [g / m 2 ] or more than 10[g / m 2 ] or less, more preferably 6 [g / m 2 ] or more than 9 [g / m 2 ] is within the following range. In addition, the picture pattern layer 4 may be configured to have, for example, a solid colored base material layer for concealing the color and pattern of the base to which the decorative sheet 1 is attached, and a picture layer for adding a picture to impart design features.
[0052] The thickness of the picture pattern layer 4 is set within the range of 1 μm to 10 μm, preferably 0.1 μm to 10 μm, more preferably 0.5 μm to 5 μm, and even more preferably 0.7 μm to 3 μm. This is because when the thickness of the picture pattern layer 4 is 1 μm or more, it is possible to make the printing clear. Also, when the thickness of the picture pattern layer 4 is 10 μm or less, it is possible to improve the printing workability when manufacturing the decorative sheet 1 and to suppress the manufacturing cost. In addition, functional additives such as extender pigments, plasticizers, dispersants, surfactants, tackifiers, adhesive aids, drying agents, hardeners, hardening accelerators, and hardening retarders may be added to the picture pattern layer 4 in order to impart various functions.
[0053] <Surface protective layer> The surface protective layer 5 (top coat) is laminated on one surface (the upper surface in FIG. 1) of the picture pattern layer 4 and is formed using a known printing method. The surface protective layer 5 is provided for the purpose of imparting surface properties such as abrasion resistance and water resistance to the decorative sheet 1. The surface protective layer 5 includes an undercoat layer 5a and an overcoat layer 5b.
[0054] The undercoat layer 5a is formed on one surface of the picture pattern layer 4, and is formed by applying an acrylic two-component curing resin (acrylic urethane resin manufactured by DIC Graphics Inc.) to a thickness of, for example, 6 μm. The topcoat layer 5b is laminated on one surface of the undercoat layer 5a (the upper surface in FIG. 1) and is formed by applying the same resin as the undercoat layer 5a but with a lower gloss. That is, the topcoat layer 5b has a lower gloss than the undercoat layer 5a. The topcoat layer 5b is formed by printing a pattern that is in harmony with the pattern formed on the picture pattern layer 4.
[0055] Specifically, the topcoat layer 5b of the surface protection layer 5 is provided with a gloss coat and a matte coat. At least one of the lines formed by the gloss coated portions and the lines formed by the matte coated portions of the topcoat layer 5b and the lines forming the pattern formed in the picture pattern layer 4 at least partially overlap each other when viewed from the direction in which the base material layer 2, the picture pattern layer 4, and the surface protection layer 5 are stacked. In addition, the lines formed by the parts that are coated with a gloss coat, the lines formed by the parts that are coated with a matte coat, and the lines forming the pattern formed in the pattern layer 4 are lines that form vessels when the pattern is, for example, a wood grain pattern.
[0056] 2, the lines GL formed by the gloss coated portion and the lines KL forming the pattern formed in the picture pattern layer 4 at least partially overlap each other when viewed from the direction in which the base material layer 2, the picture pattern layer 4, and the surface protective layer 5 are laminated. As a result, the surface protective layer 5 is formed by printing a pattern that is in harmony with the pattern formed in the picture pattern layer 4.
[0057] Although not shown in the drawings, the lines formed by the matte coated portions and the lines KL forming the pattern formed in the picture pattern layer 4 may at least partially overlap each other when viewed from the direction in which the base layer 2, the picture pattern layer 4, and the surface protective layer 5 are stacked. Also, although not shown in the drawings, the lines GL formed by the gloss coated portions, the lines formed by the matte coated portions, and the lines KL forming the pattern formed in the picture pattern layer 4 may at least partially overlap each other when viewed from the direction in which the base layer 2, the picture pattern layer 4, and the surface protective layer 5 are stacked.
[0058] Furthermore, the surface protective layer 5 is subjected to an antiviral treatment by adding an antiviral agent. As the antiviral agent, for example, a silver-based inorganic additive carrying silver ions (Biocide TB-B100, manufactured by Taisho Technos Co., Ltd.) can be used. Since the surface protective layer 5 includes the undercoat layer 5a and the topcoat layer 5b, the antiviral agent may be added to both the undercoat layer 5a and the topcoat layer 5b. In addition, the antiviral agent may be applied only to the topcoat layer 5b located on the surface side of the surface protective layer 5, for example. Although an antiviral agent is added to the surface protective layer 5, the present invention is not limited to this, and an antiviral agent may be applied to the surface side of the surface protective layer 5, i.e., at least the surface of the topcoat layer 5b.
[0059] The weight of the surface protective layer 5 after drying is preferably 0.1 [g / m 2 ] or more than 15[g / m 2 ] or less, more preferably 3 [g / m 2 ] or more than 10[g / m 2 ] or less, more preferably 6 [g / m 2 ] or more than 9 [g / m 2 ] is within the following range. The thickness of the surface protection layer 5 is preferably in the range of 0.1 μm to 10 μm, more preferably in the range of 3 μm to 10 μm, and even more preferably in the range of 6 μm to 9 μm.
[0060] In addition, the surface protective layer 5 may contain various additives, such as weathering agents, plasticizers, stabilizers, fillers, dispersants, colorants such as dyes and pigments, solvents, ultraviolet absorbers, heat stabilizers, light stabilizers, antiblocking agents, catalyst scatterers, colorants, light scattering agents, and gloss adjusters, as necessary. Furthermore, the surface protective layer 5 may contain functional additives such as antibacterial agents and antifungal agents, if necessary.
[0061] <Moisture-proof layer> The moisture-proof layer 6 is formed on the other surface (the lower surface in FIG. 1) of the base layer 2, and is formed by laminating, for example, an anchor coat layer, a deposition layer, and an overcoat layer (not shown). Note that in FIG. 1, the moisture-proof layer 6 is illustrated as a single layer. The anchor coat layer is a layer containing a first polyolefin having at least one material selected from the group consisting of a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester. The vapor-deposited layer is disposed between the anchor coat layer and the overcoat layer, and is a layer formed by vapor-depositing a metal or an inorganic compound. The overcoat layer is a layer containing a second polyolefin having at least one material selected from the group consisting of a carboxyl group, a salt of a carboxyl group, a carboxylic anhydride group, and a carboxylic ester.
[0062] <Primer layer> The primer layer 7 is formed on the other surface of the base layer 2 (the lower surface in FIG. 1) by applying a primer (undercoat agent) to the other surface of the base layer 2. The function of the primer layer 7 is mainly to improve adhesion, and further includes surface stabilization after surface treatment, corrosion prevention of metal surfaces, imparting adhesion, and preventing deterioration of adhesives.
[0063] The primer layer 7 is formed by, for example, a gravure printing method so that the solid content is 1 [g / m 2 ] is formed by coating a urethane resin. For example, urethane-based, acrylic-based, ethylene-vinyl acetate copolymer, vinyl chloride-vinyl acetate copolymer, polyester-based, etc. can be used for the primer layer 7. In particular, a two-component curing urethane-based primer agent made by blending polyester polyol and polyisocyanate is preferable. In addition, if inorganic powder such as silica, barium sulfate, calcium carbonate, etc. is added to the material for the primer layer 7 to form the primer layer 7, it is effective in improving the adhesive strength by the anchoring effect.
[0064] (Hardness of decorative sheet) The decorative sheet 1 is formed so that the hardness is B or higher in the pencil hardness test specified in JIS K 5600, i.e., B or harder than B. Therefore, each layer constituting the decorative sheet 1 is formed so that the hardness of the decorative sheet 1 in the pencil hardness test is B or higher. Methods for adjusting the hardness of the decorative sheet 1 include, for example, a method for adjusting the thickness of the base layer 2, a method for adding a dispersant as a nano-sized additive to the base layer 2, or the like. The hardness of the decorative sheet 1 refers to the hardness of the entire decorative sheet 1. The pencil hardness test is a test on the surface protective layer 5.
[0065] (Moisture permeability of decorative sheets) The moisture permeability of the decorative sheet 1 is 5 [g / m 2 -24hr or less. In the first embodiment, as an example, from the viewpoint of suppressing warping of the decorative board, the moisture permeability of the decorative sheet 1 is set to 3 [g / m 2 This section explains the case where the time is set to 24 hours or less.
[0066] (Method of manufacturing decorative sheets) The manufacturing method for producing the decorative sheet 1 is an in-line method for producing the decorative sheet 1, and includes a first step, a second step, and a third step. Here, "in-line" means that there is no lamination process for laminating films together, and printing, which is usually performed in multiple steps, can be processed in one line. In other words, in the method for producing the decorative sheet 1, the production process from printing to providing the surface protective layer 5 can be performed in a single in-line process.
[0067] (1) First step The first step is a step of manufacturing a base layer 2 formed by extrusion molding a core layer 2b made of a transparent polypropylene-based thermoplastic resin, and a first transparent layer 2a and a second transparent layer 2c made of a thermoplastic resin to which a dispersant as a nano-sized additive has been added.
[0068] (2)Second process The second step is a step of forming a colored layer 3, a picture pattern layer 4, and a surface protective layer 5 on one surface of the base layer 2 produced in the first step. The layers formed in the second step are not limited to three layers, namely, the colored layer 3, the picture pattern layer 4, and the surface protective layer 5, but may be, for example, one layer, two layers, or four or more layers.
[0069] (3) Third step The third step is a step of forming a primer layer 7 on the other surface (the lower surface in Figure 1) of the base layer 2 produced in the first step, either after the second step or prior to the second step. Therefore, the method for producing the decorative sheet 1 is carried out in one of two orders: the first step, the second step, and the third step, or the first step, the third step, and the second step.
[0070] <Decorative board> The configuration of the decorative board 10 will be described with reference to FIG. As shown in FIG. 1, the decorative board 10 is formed, for example, in a plate shape, and includes a decorative sheet 1, a substrate 8, and a moisture-proof film 9.
[0071] <Substrate> The substrate 8 is disposed on the decorative sheet 1 on the other surface of the primer layer 7 (the lower surface in FIG. 1). The material of the substrate 8 may be any type, such as wood, steel, or resin. For example, a non-combustible steel plate or a non-combustible material as specified by Notification No. 1400 of the Ministry of Construction may be used. Furthermore, the substrate 8 has a folded structure or a three-dimensional structure. When the decorative sheet 1 is laminated onto the substrate 8, it may be laminated via an appropriately selected adhesive as necessary, or it may be laminated without an adhesive or the like.
[0072] The decorative sheet 1 can be laminated and bonded to the substrate 8 by a method of contacting a metal plate and pressing it with a flat pressure, or a continuous lamination method using a circular pressure system. In particular, the continuous lamination method using an endless metal belt makes it possible to continuously produce a high-quality decorative board 10 at high speed that is free of surface warping or waviness, has good interlayer adhesion, and is densely cured and integrated.
[0073] <Moisture-proof film> The moisture-proof film 9 is laminated, for example, via an adhesive or the like, on the surface of the substrate 8 opposite the surface facing the decorative sheet 1 (the lower surface in FIG. 1). The moisture-proof film 9 is formed, for example, by using a polypropylene moisture-proof film laminated with a gas barrier layer formed of a composition of a (meth)acrylic acid polymer and an ethylene-vinyl alcohol copolymer.The moisture-proof film 9 is formed, for example, by using a transparent polypropylene film stretched in the transverse direction, coated with a gas barrier layer formed of a (meth)acrylic acid polymer and an ethylene-vinyl alcohol copolymer on a laminated sheet obtained by co-extrusion of polypropylene and modified polypropylene polymer.
[0074] The above-described first embodiment is one example of the present invention, and the present invention is not limited to the above-described first embodiment. Various modifications can be made depending on the design, etc., even if the modifications are in a form other than the first embodiment, as long as they do not deviate from the technical idea of the present invention.
[0075] (Effects of the First Embodiment) The decorative sheet 1 of the first embodiment can achieve the effects described below. (1) The decorative sheet 1 is provided with a base layer 2 formed using a polypropylene-based thermoplastic resin, a picture pattern layer 4 laminated on one side of the base layer 2 and having a picture formed thereon, and a surface protective layer 5 laminated on one side of the picture pattern layer 4. The base layer 2 is added with a dispersion material as a nano-sized additive. In addition, the moisture permeability of the decorative sheet 1 is 5 [g / m 2 -24hr or less. As a result, the moisture permeability was increased to 5 [g / m 2 By setting the shelf life to be [.048 hr] or less, it is possible to suppress warping and the like that occurs due to moisture absorption and release of the decorative sheet 1, and it is possible to provide a decorative sheet 1 that is capable of suppressing deformation of the decorative sheet 1.
[0076] In addition, since no lamination step with other sheets is required during production, the number of production steps can be reduced, and further, the production steps can be performed in a single in-line process. Furthermore, because it is a single layer, it can be easily made into a thin film, and by using nano-sized additives, it is possible to improve the hardness of the decorative sheet 1 even when it is a thin film, thereby imparting excellent moisture resistance.
[0077] (2) Moisture permeability is 3 [g / m 2 -24hr or less. As a result, the moisture permeability was 3 [g / m 2 In comparison with the case where the drying time exceeds [1.4 hr.·24 hr], it is possible to further suppress warping and the like caused by moisture absorption and release of the decorative sheet 1, and it is possible to suppress deformation of the decorative sheet 1.
[0078] (3) In the pencil hardness test specified in JIS K 5600, the hardness is B or higher. As a result, by forming the decorative sheet 1 so that the hardness is B or more in the pencil hardness test specified by JIS K 5600, it is possible to obtain a decorative sheet 1 with low moisture permeability without using a polysand sheet or a moisture-proof film. This makes it possible to suppress the occurrence of warping and dimensional changes when the decorative sheet 1 is attached to a wood substrate. In addition, it is possible to easily obtain a decorative sheet 1 with low moisture permeability without increasing the number of manufacturing steps. Furthermore, since it is possible to obtain a decorative sheet 1 with low moisture permeability and a single layer, it is possible to obtain a decorative sheet 1 with low moisture permeability without using a dedicated machine or the like for reducing the moisture permeability. In addition, since it is possible to form a configuration without using a polysand sheet or a moisture-proof film, it is possible to make the decorative sheet 1 a mono-material, which makes it easy to recycle.
[0079] (4) The base layer 2 includes a first transparent layer 2a, a core layer 2b laminated on one surface of the first transparent layer 2a, and a second transparent layer 2c laminated on one surface of the core layer 2b. As a result, it is possible for the decorative sheet 1 to be configured without including the colored layer 3. (5) The optical fiber further includes a colored layer 3 disposed between the base layer 2 and the picture pattern layer 4, and the colored layer 3 is transparent or translucent. As a result, it becomes possible to impart hiding properties to the decorative sheet 1. (6) A primer layer 7 is further provided on the other surface of the base layer 2 . As a result, for example, the interlayer adhesion between the decorative sheet 1 and the substrate 8 can be improved. (7) The moisture-proof layer 6 is further provided between the substrate layer 2 and the primer layer 7 . As a result, the moisture resistance of the decorative sheet 1 can be improved.
[0080] (8) The base layer 2 is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to a polypropylene-based thermoplastic resin. As a result, it is possible to improve the scratch resistance and abrasion resistance of the decorative sheet 1. In addition, because the crystallinity of the resin material that constitutes the base layer 2 is sufficiently improved, it is possible to provide a decorative sheet 1 that has sufficient scratch resistance and abrasion resistance.
[0081] (9) The amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based thermoplastic resin. As a result, it is possible to improve the crystallinity of the resin material constituting the base layer 2 compared to a configuration in which the amount of nucleating agent vesicles added is outside the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicles, per 100 parts by mass of polypropylene-based thermoplastic resin.
[0082] (10) Nucleating vesicles are nucleating liposomes with an outer membrane formed using phospholipids. As a result, it is possible to improve the compatibility between the vesicles and the polypropylene-based thermoplastic resin, which is the main component of the base layer 2. (11) The nucleating agent vesicle is formed by encapsulating a nucleating agent in a vesicle with a monolayer membrane and then converting it into a vesicle by supercritical reverse phase evaporation. As a result, it becomes possible to easily produce unilamellar vesicles encapsulating a nucleating agent, and to prepare smaller vesicles (capsules) encapsulating a nucleating agent.
[0083] (12) The first transparent layer 2a is formed by adding a nucleating agent vesicle having a single-layer outer membrane and a nano-sized nucleating agent encapsulated therein to a polypropylene-based thermoplastic resin, and the second transparent layer 2c is formed by adding a nucleating agent vesicle having a single-layer outer membrane and a nano-sized nucleating agent encapsulated therein to a polypropylene-based thermoplastic resin. As a result, the crystallinity of the resin material constituting the first transparent layer 2a and the second transparent layer 2c is sufficiently improved, making it possible to provide a decorative sheet 1 that has sufficient scratch resistance and abrasion resistance. (13) The surface protective layer 5 is provided with at least one of a gloss coat and a matte coat. As a result, the design of the decorative sheet 1 can be improved.
[0084] (14) At least one of the lines formed by the portions to which the gloss coating is applied and the lines formed by the portions to which the matte coating is applied and the lines KL forming the pattern formed in the pattern layer 4 at least partially overlap each other when viewed from the direction in which the base layer 2, the pattern layer 4, and the surface protection layer 5 are stacked. As a result, it becomes possible to harmonize the pattern formed on the surface protective layer 5 with the pattern formed on the picture pattern layer 4, thereby improving the design of the decorative sheet 1.
[0085] Moreover, the decorative board 10 in the first embodiment can achieve the effects described below. (15) The device comprises a substrate 8 and a decorative sheet 1 laminated on at least one surface of the substrate 8. As a result, it is possible to prevent warping and the like caused by moisture absorption and release in the decorative sheet 1, and it is possible to provide a decorative board 10 in which deformation of the decorative sheet 1 can be prevented. (16) The substrate 8 further includes a moisture-proof film 9 laminated on the surface opposite to the surface facing the decorative sheet 1. As a result, the moisture resistance of the decorative board 10 can be improved.
[0086] <Modification of the first embodiment> (1) In the first embodiment, the base layer 2 is configured to be formed of two types of three layers, including a first transparent layer 2a, a core layer 2b, and a second transparent layer 2c. However, this is not limited to this. For example, as shown in FIG. 3, the base layer 2 may be configured to be a single layer. (2) In the first embodiment, the moisture-proof layer 6 is disposed between the base layer 2 and the primer layer 7, but this is not limited to the above. In other words, the decorative sheet 1 may be configured without the primer layer 7, and the moisture-proof layer 6 may be laminated on the other surface of the base layer 2. Even in this case, it is possible to improve the moisture-proof property of the decorative sheet 1. EXAMPLES
[0087] With reference to the first embodiment, the decorative sheets of Examples 1 to 4 and the decorative sheets of Comparative Examples 1 and 2 will be described below. Example 1 The base layer was formed by adding a weathering agent and a dispersion material as a nano-sized additive to a transparent polypropylene thermoplastic resin and extruding the resin to a thickness of 70 μm. That is, in Example 1, the base layer was made of only one layer. The colored layer was formed from a two-component urethane resin. The design layer was formed by printing a design with a urethane resin by gravure printing.
[0088] The surface protection layer was first formed by applying a low-gloss acrylic two-component curing resin (DIC Graphics: acrylic urethane resin) to a thickness of 6 μm to form an undercoat layer. Then, a pattern that matched the pattern formed in the picture pattern layer was printed on the undercoat layer using an acrylic two-component curing resin (DIC Graphics: acrylic urethane resin) with a higher gloss than the undercoat layer to form a topcoat layer, forming the surface protection layer. The primer layer was applied by gravure printing with a solid content of 1 g / m 2 A urethane resin was applied so that the shape of the surface was as follows: The hardness is B in the pencil hardness test specified in JIS K 5600, and the moisture permeability is 5 [g / m 2 -24hr]. In this manner, the decorative sheet of Example 1 was formed.
[0089] Example 2 A decorative sheet of Example 2 was formed in the same manner as in Example 1, except that the thickness of the substrate layer was 100 μm. Example 3 The decorative sheet of Example 3 was formed in the same manner as in Example 1, except that the base layer was formed of two types of three layers, including a first transparent layer, a core layer, and a second transparent layer, and the thickness of the base layer was 80 μm. Example 4 A decorative sheet of Example 4 was formed in the same manner as in Example 3, except that the thickness of the substrate layer was 100 μm.
[0090] Comparative Example 1 The base layer is configured without the addition of a dispersion material as a nano-sized additive, the hardness is 3B in the pencil hardness test specified in JIS K 5600, and the moisture permeability is 6 [g / m 2 A decorative sheet of Comparative Example 1 was formed in the same manner as in Example 1, except that the drying time was changed to [.times.24 hr]. Comparative Example 2 A decorative sheet of Comparative Example 2 was formed in the same manner as in Comparative Example 1, except that the thickness of the substrate layer was 100 μm.
[0091] (Performance evaluation) Performance evaluations were carried out on the decorative sheets of Examples 1 to 4 and Comparative Examples 1 and 2. Evaluation methods used were a scratch test, a scratch hardness test (pencil hardness), and a moisture permeability test. Scratch tests and scratch hardness tests were performed using decorative sheets from the examples and comparative examples, which were formed by applying a water-based urethane adhesive to a 3 mm thick piece of MDF (medium density fiberboard), bonding the substrate to the sheet, and compressing the sheet using a press set at a temperature between 30°C and 50°C to form decorative panels. The moisture permeability test was carried out in the form of a decorative sheet.
[0092] (Scratch test) The scratch test was performed by subjecting the decorative board to a coin scratch test and measuring the load at which no continuous scratches were produced on the surface (surface protection layer) of the decorative board. In the scratch test, a 10 yen coin was placed on the surface of the decorative sheet, and the test was started with a load of 1 [Kg], and the load was then increased by 1 [Kg] until a load of 4 [Kg] was applied. (Scratch hardness test) The scratch hardness test was performed on the decorative panel using the scratch hardness test (pencil hardness test) specified in JIS K5600-5-4:1999 to measure the hardness (pencil hardness) of the hardest pencil that did not leave a scratch on the surface (surface protection layer) of the decorative panel.
[0093] (Moisture permeability test) The moisture permeability test was carried out according to the method for measuring moisture permeability of building materials (cup method) specified in JIS A 1324. Specifically, first, a moisture absorbent was placed in the bottom of a cup that is impermeable to water vapor, and the sample decorative sheets were attached to the four cups and sealed with aluminum tape. The samples were then placed inside a thermo-hygrostat set at a temperature of 23°C and a relative humidity of 50%, and after 120 hours had passed, the samples were removed. The increase in the mass of the cup was then measured, and the amount of moisture transmitted through the sample was calculated to obtain the moisture permeability.
[0094] (Evaluation Criteria) In the scratch test, a load of 1 [Kg] or more was rated as pass ("◯"), and a load of less than 1 [Kg] was rated as fail ("×"). In the scratch hardness test, a pencil hardness of 2B or more was rated as pass (◯), and a pencil hardness of less than 2B was rated as fail (×). The moisture permeability test was conducted to determine whether the moisture permeability was 5 [g / m 2 If the moisture permeability is less than 5 [g / m 2 -24hr] was deemed a failure ("X").
[0095] (Evaluation Results) The evaluation results are shown in Table 1. [Table 1]
[0096] (Evaluation Results) As shown in Table 1, the decorative sheets of Examples 1 to 4 had a scratch hardness of 2B or more, and passed both the scratch test and the moisture permeability test. 2 It was confirmed that it was possible to obtain a moisture permeability of less than 24 hours. On the other hand, as shown in Comparative Examples 1 and 2, in the case of decorative sheets having a scratch hardness of less than 2B, the moisture permeability is [g / m 2 It was confirmed that the time required for the 24-hour incubation period exceeded 10 hours. From the above, the decorative sheets of Examples 1 to 4 were able to show excellent performance in all the evaluation tests. On the other hand, the decorative sheets of Comparative Examples 1 and 2 were unable to show excellent performance in all the evaluation tests.
[0097] The present technology can be configured as follows. (1) A base layer formed using a polypropylene-based thermoplastic resin; A pattern layer laminated on one surface of the base layer and having a pattern formed thereon; A surface protective layer is laminated on one surface of the picture pattern layer, The base layer is added with a dispersion material as a nano-sized additive, Moisture permeability is 5g / m 2 Decorative sheets that are 24 hours or less. (2) The moisture permeability is 3g / m 2 The decorative sheet described in (1) above, which has a shelf life of 24 hours or less. (3) A decorative sheet according to (1) or (2) above, which has a hardness of B or higher in a pencil hardness test specified in JIS K 5600. (4) The decorative sheet according to any one of (1) to (3), wherein the base layer comprises a first transparent layer, a core layer laminated on one side of the first transparent layer, and a second transparent layer laminated on one side of the core layer. (5) The substrate further includes a color layer disposed between the substrate layer and the pattern layer, The decorative sheet according to any one of (1) to (4) above, wherein the colored layer is transparent or translucent. (6) The decorative sheet according to any one of (1) to (5) above, further comprising a primer layer laminated on the other surface of the base layer. (7) The decorative sheet according to any one of (1) to (6) above, further comprising a moisture-proof layer disposed between the substrate layer and the primer layer. (8) The decorative sheet according to any one of (1) to (6) above, further comprising a moisture-proof layer laminated on the other surface of the base layer. (9) The decorative sheet according to any one of (1) to (8), wherein the base layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin. (10) A decorative sheet as described in (9) above, wherein the amount of the nucleating agent vesicle added is within the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based thermoplastic resin. (11) A decorative sheet according to (9) or (10) above, wherein the nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid. (12) The decorative sheet according to any one of (9) to (11), wherein the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a single-layer membrane, and then forming the vesicle by a supercritical reverse phase evaporation method. (13) The first transparent layer is formed by adding a nucleating agent vesicle having a single-layer outer membrane and a nano-sized nucleating agent encapsulated therein to the polypropylene-based thermoplastic resin, The decorative sheet according to any one of (1) to (8), wherein the second transparent layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin. (14) The decorative sheet according to (13) above, wherein the nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid. (15) The decorative sheet according to (13) or (14) above, wherein the nucleating agent vesicle is formed by encapsulating the nucleating agent in a vesicle having a single-layer membrane, and then forming the vesicle by a supercritical reverse phase evaporation method. (16) The decorative sheet according to any one of (1) to (15) above, wherein the surface protective layer is coated with at least one of a gloss coat and a matte coat. (17) A decorative sheet as described in (16) above, in which at least one of the lines formed by the portions to which the gloss coat is applied and the lines formed by the portions to which the matte coat is applied and the lines forming the pattern formed in the pattern layer at least partially overlap each other when viewed from the direction in which the base layer, the pattern layer, and the surface protective layer are laminated. (18) A substrate; A decorative board comprising: a decorative sheet according to any one of (1) to (17) above, laminated on at least one surface of the substrate. (19) The decorative board according to (18) above, further comprising a moisture-proof film laminated on the surface of the substrate opposite to the surface facing the decorative sheet. [Explanation of symbols]
[0098] 1...decorative sheet, 2...base material layer, 2a...first transparent layer, 2b...core layer, 2c...second transparent layer, 3...colored layer, 4...picture pattern layer, 5...surface protection layer, 5a...undercoat layer, 5b...topcoat layer, 6...moisture-proof layer, 7...primer layer, 8...substrate, 9...moisture-proof film, 10...decorative board, GL...line formed by portion to which gloss coat is applied, KL...line forming pattern formed in picture pattern layer
Claims
1. A base layer formed using a polypropylene-based thermoplastic resin; A pattern layer laminated on one surface of the base layer and having a pattern formed thereon; A surface protective layer is laminated on one surface of the picture pattern layer, The base layer is added with a dispersion material as a nano-sized additive, Moisture permeability is 5g / m 2 - Decorative sheet lasting less than 24 hours.
2. The moisture permeability is 3g / m 2 The decorative sheet according to claim 1, wherein the retention time is 24 hours or less.
3. 2. The decorative sheet according to claim 1, which has a hardness of B or more in the pencil hardness test specified in JIS K 5600.
4. The decorative sheet according to claim 1 , wherein the base layer comprises a first transparent layer, a core layer laminated on one side of the first transparent layer, and a second transparent layer laminated on one side of the core layer.
5. The substrate further includes a color layer disposed between the substrate layer and the pattern layer, 2. The decorative sheet according to claim 1, wherein said colored layer is transparent or translucent.
6. 2. The decorative sheet according to claim 1, further comprising a primer layer laminated on the other surface of said base layer.
7. 7. The decorative sheet according to claim 6, further comprising a moisture-proof layer disposed between said substrate layer and said primer layer.
8. 2. The decorative sheet according to claim 1, further comprising a moisture-proof layer laminated on the other surface of said base layer.
9. The decorative sheet according to claim 1, wherein the base layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin.
10. The decorative sheet according to claim 9, wherein the amount of the nucleating agent vesicle added is in the range of 0.05 parts by mass or more and 0.5 parts by mass or less, calculated as the nucleating agent encapsulated in the nucleating agent vesicle, per 100 parts by mass of the polypropylene-based thermoplastic resin.
11. 10. The decorative sheet according to claim 9, wherein said nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid.
12. 10. The decorative sheet according to claim 9, wherein said nucleating agent vesicle is formed by encapsulating said nucleating agent in a vesicle having a monolayer membrane, and further forming the vesicle by a supercritical reverse phase evaporation method.
13. The first transparent layer is formed by adding a nucleating agent vesicle having a single-layer outer membrane and a nano-sized nucleating agent encapsulated therein to the polypropylene-based thermoplastic resin, The decorative sheet according to claim 4, wherein the second transparent layer is formed by adding nucleating agent vesicles, in which a nano-sized nucleating agent is encapsulated in a vesicle having a single-layer outer membrane, to the polypropylene-based thermoplastic resin.
14. 14. The decorative sheet according to claim 13, wherein said nucleating agent vesicle is a nucleating agent liposome having an outer membrane formed using a phospholipid.
15. 14. The decorative sheet according to claim 13, wherein said nucleating agent vesicle is formed by encapsulating said nucleating agent in a vesicle having a monolayer membrane, and further forming the vesicle by a supercritical reverse phase evaporation method.
16. 2. The decorative sheet according to claim 1, wherein said surface protective layer is provided with at least one of a gloss coat and a matte coat.
17. The decorative sheet of claim 16, wherein at least one of the lines formed by the portions to which the gloss coating is applied and the lines formed by the portions to which the matte coating is applied and the lines forming the pattern formed in the pattern layer at least partially overlap each other when viewed from the direction in which the base layer, the pattern layer, and the surface protective layer are stacked.
18. A substrate; A decorative board comprising: a decorative sheet according to any one of claims 1 to 17 laminated on at least one surface of the substrate.
19. 20. The decorative board according to claim 18, further comprising a moisture-proof film laminated on a surface of said substrate opposite to the surface facing said decorative sheet.
Citation Information
Patent Citations
Front / back-synchronized gloss mat decorative sheet
JP2015199313A