Manufacturing method of adhesive sheet, and adhesive sheet

The manufacturing method for a pressure-sensitive adhesive sheet with a transparent base and grooves filled by a non-adhesive printed resin film with air bubbles, covered by a releasable sheet, addresses the issue of design deterioration by enhancing visibility and functionality while ensuring effective air escape.

JP2024140457APending Publication Date: 2024-10-10TOPPAN HOLDINGS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023051594
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing adhesive sheets with transparent bases suffer from design deterioration due to visible grooves formed to allow air escape, which compromises their aesthetic appeal.

Method used

A method for manufacturing a pressure-sensitive adhesive sheet involving a transparent extensible film base layer with grooves in the adhesive layer, filled by a printed resin film that does not adhere and contains air bubbles, and covered by a releasable sheet, all formed without using antifoaming agents.

Benefits of technology

The method enhances design preservation by minimizing the visibility of grooves, improves workability, and maintains non-flammability while ensuring effective air escape, thus maintaining the adhesive sheet's aesthetic quality and functional integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140457000001_ABST
    Figure 2024140457000001_ABST
Patent Text Reader

Abstract

To provide a manufacturing method of an adhesive sheet capable of suppressing deterioration of designability, and to provide an adhesive sheet.SOLUTION: An adhesive sheet 1 comprises: a substrate layer 11 formed of an extensible film having transparency; an adhesive layer 13 laminated on the one surface of the substrate layer 11, and having a groove part 131 formed on a surface at an opposite side to a surface facing the substrate layer 11; a printed resin coating sheet 14 formed in a shape of burying the groove part 131, and not having adhesiveness; and a releasable sheet 20 laminated on a surface at an opposite side to the surface facing the substrate layer 11 of the adhesive layer 13, and covering the surface facing the substrate layer 11 of the adhesive layer 13, the groove part 131 and the printed resin coating sheet 14. The printed resin coating sheet 14 is formed without using an antifoam agent, and air bubbles are formed inside the printed resin coating sheet 14.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a pressure-sensitive adhesive sheet, and to a pressure-sensitive adhesive sheet. [Background technology]

[0002] Conventionally, adhesive sheets having an adhesive layer on one side of a base layer have been used as building materials, but the adhesive sheet having an adhesive layer is prone to trapping air at the boundary between the adherend and the adhesive sheet, which may reduce the design. For this reason, as disclosed in Patent Document 1, for example, an adhesive sheet has been proposed in which a groove is formed in the adhesive layer of the adhesive sheet to allow air to escape to the surroundings, so that the adhesive sheet can be applied while allowing air to escape when it is applied. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] Patent No. 6856163 Summary of the Invention [Problem to be solved by the invention]

[0004] However, the technology disclosed in Patent Document 1 has a problem in that, for example, when the base material of the adhesive sheet is made transparent so that the pattern applied to the adherend can be seen from the surface of the adhesive sheet, the grooves become visible, thereby reducing the design.

[0005] In view of the above-mentioned problems, an object of the present invention is to provide a method for producing a pressure-sensitive adhesive sheet that can suppress deterioration in design, and a pressure-sensitive adhesive sheet. [Means for solving the problem]

[0006] In order to solve the above problems, one aspect of the present invention is a method for producing a pressure-sensitive adhesive sheet comprising a substrate layer, a pressure-sensitive adhesive layer, a printed resin coating, and a release sheet. The substrate layer is formed of a transparent extensible film. The pressure-sensitive adhesive layer is laminated on one surface of the substrate layer, and has a groove formed on the surface opposite to the surface facing the substrate layer. The printed resin coating is formed in a shape that fills the groove, and does not have adhesiveness. The release sheet is laminated on the surface of the pressure-sensitive adhesive layer opposite to the surface facing the substrate layer, and covers the surface of the pressure-sensitive adhesive layer facing the substrate layer, the groove, and the printed resin coating. The printed resin coating is then formed without using an antifoaming agent.

[0007] In order to solve the above problem, one aspect of the present invention is a pressure-sensitive adhesive sheet comprising a substrate layer, a pressure-sensitive adhesive layer, a printed resin coating, and a release sheet. The substrate layer is formed of a transparent extensible film. The pressure-sensitive adhesive layer is laminated on one surface of the substrate layer, and has a groove formed on the surface opposite to the surface facing the substrate layer. The printed resin coating is formed in a shape that fills the groove, and does not have adhesiveness. The release sheet is laminated on the surface opposite to the surface facing the substrate layer of the pressure-sensitive adhesive layer, and covers the surface facing the substrate layer of the pressure-sensitive adhesive layer, the groove, and the printed resin coating. Air bubbles are formed inside the printed resin coating. Effect of the Invention

[0008] According to one aspect of the present invention, it is possible to provide a method for producing a pressure-sensitive adhesive sheet capable of suppressing deterioration in design, and a pressure-sensitive adhesive sheet. [Brief description of the drawings]

[0009] [Figure 1] 1 is a cross-sectional view illustrating a configuration of a pressure-sensitive adhesive sheet according to a first embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] Hereinafter, an embodiment of the present technology will be described with reference to the drawings. In the description of the drawings, the same or similar parts are denoted with the same or similar reference numerals, and duplicated descriptions are omitted. Each drawing is schematic and may differ from the actual one. The embodiments shown below are examples of devices and methods for embodying the technical idea of ​​the present technology, and the technical idea of ​​the present technology is not limited to the devices and methods exemplified in the following embodiments. The technical idea of ​​the present technology can be modified in various ways within the technical scope described in the claims. In addition, the directions of "left and right" and "up and down" in the following description are merely definitions for the convenience of explanation and do not limit the technical idea of ​​the present invention. Therefore, for example, if the paper is rotated 90 degrees, "left and right" and "up and down" are read interchangeably, and of course, if the paper is rotated 180 degrees, "left" becomes "right" and "right" becomes "left".

[0011] First embodiment The configuration of the adhesive sheet 1 will now be described with reference to FIG. As shown in FIG. 1, the adhesive sheet 1 includes a base layer 11 , a surface protective layer 12 , an adhesive layer 13 , a printed resin coating 14 , and a release sheet 20 .

[0012] <Base material layer> The base layer 11 is a sheet-like member that serves as the base material of the pressure-sensitive adhesive sheet 1, and is formed of a transparent extensible film. The material for forming the base layer 11 is preferably a resin having excellent mechanical strength, such as polypropylene, polycarbonate, polyethylene, polyethylene terephthalate, or an acrylonitrile-butadiene-styrene copolymer. It is more preferable to use a resin having excellent heat resistance and fire resistance, such as polypropylene, polycarbonate, or an acrylonitrile-butadiene-styrene copolymer, as the material for forming the base layer 11. The transparency of the base material layer 11 may be such that the printed resin coating 14 is visible through the base material layer 11 .

[0013] The thickness of the base material layer 11 may be any thickness that provides sufficient physical properties such as strength as the base material of the adhesive sheet 1, while providing stiffness to facilitate application when applying the adhesive sheet 1. Specifically, the thickness of the base material layer 11 is preferably 50 μm or more. In addition, since an increase in the thickness of the base material layer 11 reduces transparency, and in consideration of various physical properties such as fire resistance, the thickness of the base material layer 11 is preferably 150 μm or less.

[0014] <Surface protective layer> The surface protective layer 12 is a layer for imparting functions such as weather resistance, scratch resistance, stain resistance, and design properties to the pressure-sensitive adhesive sheet 1 and for protecting the base layer 11. The surface protective layer 12 is laminated on the surface of the base layer 11 opposite to the surface on which the pressure-sensitive adhesive layer 13 is laminated (the upper surface of the base layer 11 in FIG. 1). The surface protective layer 12 may be composed of one layer, or two or more layers.

[0015] The surface protective layer 12 is transparent and has sufficient physical properties required for protection, such as strength, stain resistance, weather resistance, etc. The transparency of the surface protective layer 12 may be such that either or both of the design of the article (adherend) to which the pressure-sensitive adhesive sheet 1 is attached and the printed resin coating 14 can be visually recognized.

[0016] The surface protective layer 12 preferably contains at least one type of resin material, such as a thermosetting resin, an electron beam curable resin such as an ultraviolet curable resin, etc. The resin material for forming the surface protective layer 12 may be, for example, an acrylic resin.

[0017] The amount of resin material applied to the surface protective layer 12 is 1.5 g / m 2 ] or more than 7.0[g / m 2 Here, the term "coating amount" refers to the basis weight of the coating agent after it has been dried by a suitable method. The reason why the coating amount of the resin material in the surface protective layer 12 is set within the above-mentioned range is that the coating amount of the resin material in the surface protective layer 12 is set to 1.5 [g / m 2In addition, when the coating amount of the resin material in the surface protective layer 12 is less than 7.0 [g / m 2 ] is preferable from the viewpoints that the production cost increases and the fire resistance decreases.

[0018] The surface protective layer 12 may also contain an antiviral agent. The antiviral agent is preferably a silver-based material. As the antiviral agent, inorganic antibacterial agents such as antibacterial zeolite, antibacterial apatite, and antibacterial zirconia formed by incorporating silver ions, copper ions, or zinc ions into inorganic compounds such as zeolite, apatite, and zirconia can be used. As the antiviral agent, for example, zinc pyridinone 2-(4-thiazolyl)-benzimidazole, 10,10-oxybisphenoxanodine, organic titanium sulfur halogen system, pyridine-2-thiol-oxide, etc., can be used. Among these, silver-based antiviral agents are superior in terms of antiviral effect.

[0019] The amount of the antiviral agent added to the surface protective layer 12 is preferably within the range of 0.2 mass [%] to 20 mass [%]. The reason why the amount of the antiviral agent added to the surface protective layer 12 is set within the above-mentioned range is that when the amount of the antiviral agent added is 0.2 mass [%] or more, the antiviral effect of the surface protective layer 12 is improved. In addition, when the amount of the antiviral agent added is 20 mass [%] or less, the scratch resistance of the surface protective layer 12 is improved.

[0020] The average particle size of the antiviral agent is preferably within the range of 1 μm to 10 μm. The reason for setting the average particle size of the antiviral agent within the above-mentioned range is that when the average particle size of the antiviral agent is within the range of 1 [μm] to 10 [μm], the contact area between surface protective layer 12 and the antiviral agent is improved, resulting in good antiviral properties. It is preferable that the particle size of the antiviral agent has multiple peaks. Specifically, it is more preferable that the particle size of the antiviral agent includes a first peak in the range of 0.5 [μm] or more and less than 5 [μm] and a second peak in the range of 5 [μm] or more and 15 [μm] or less. By dispersing the peaks in the particle size of the antiviral agent, the packing density of the antiviral agent is further improved, and it becomes possible to add a larger amount of the antiviral agent. Therefore, the contact area between the resin material and the antiviral agent is enlarged, and the surface area of ​​the antiviral agent itself is also enlarged, thereby improving the antiviral properties.

[0021] The surface protective layer 12 plays an important role in determining the superiority or inferiority of bending workability, weather resistance, scratch resistance, contamination resistance, etc. For this reason, the surface protective layer 12 may contain various additives, such as weather resistance additives, plasticizers, stabilizers, fillers, dispersants, colorants such as dyes and pigments, ultraviolet absorbers, antiblocking agents, catalyst scatterers, light scattering agents, fluorescent agents, luminescent materials, and gloss adjusters, as necessary. In addition to the antiviral agent, agents having various functions can be added to the surface protective layer 12. The functionality can be selected from various options such as antibacterial properties, antiallergenic properties, deodorizing properties, infrared reflection properties, etc., and the surface protective layer 12 may have multiple functions.

[0022] When forming the above-mentioned surface protective layer 12, it is possible to apply the resin material by selecting a coating method suited to the purpose, such as gravure printing, offset printing, flexographic printing, inkjet printing, etc. The surface protective layer 12 is formed by applying the resin material and curing the coating film using a known coating device, heat drying device, ultraviolet ray irradiation device, and electron beam irradiation device according to the type of resin material. For example, the surface protective layer 12 is formed by applying and drying a coating agent containing a solvent such as methyl ethyl ketone, a urethane resin, and an isocyanate curing agent on the surface of the base layer 11 opposite to the surface on which the adhesive layer 13 is provided, and then curing the coating agent by irradiating ultraviolet rays.

[0023] <Adhesive layer> The adhesive layer 13 is a layer for maintaining adhesiveness in the base layer 11, and is laminated on one side of the base layer 11 (the side opposite to the side on which the surface protective layer 12 is formed; in Figure 1, the lower side of the base layer 11). Any material used in general adhesive sheets can be used as the adhesive composition constituting the adhesive layer 13. As an example, it is preferable to use an acrylic pressure-sensitive adhesive whose starting material is acrylic acid or an acrylic acid ester.

[0024] The thickness of the adhesive layer 13 is preferably 20 μm or more, and more preferably 40 μm or more, in order to provide ease of application and sufficient adhesive strength. Note that the "thickness of the adhesive layer 13" refers to the thickness of the thickest part of the adhesive layer 13 at the stage after the adhesive composition is applied and then dried. The pressure-sensitive adhesive layer 13 also has a plurality of grooves 131 formed on the surface opposite to the surface facing the base layer 11 .

[0025] (Groove) The shape of the groove 131 is a recess that matches the shape of the printed resin film 14. Moreover, the grooves 131 may terminate at the outer peripheral portion of the adhesive layer 13, or may be connected to other grooves 131 that terminate at the outer peripheral portion of the adhesive layer 13. This allows air trapped between the adhesive layer 13 and the adherend to flow out to the periphery of the adhesive sheet 1 when the adhesive sheet 1 is attached to the adherend. After the air has flowed out to the periphery, the bottoms of the grooves 131 are brought into close contact with the surface of the adherend, thereby improving the impact resistance and adhesive strength of the adhesive sheet 1. In addition, it is possible to improve the design of the adhesive sheet 1 at the time of final finish after construction.

[0026] The cross-sectional shape of the groove portion 131 may be any shape that allows the air trapped between the adhesive layer 13 and the adherend to flow out to the periphery of the adhesive sheet 1, and can be, for example, V-shaped, U-shaped, rectangular, trapezoidal, linear, etc.

[0027] The depth of groove portion 131 may be any depth as long as it allows air trapped between adhesive layer 13 and the adherend to flow out to the periphery of adhesive sheet 1. As a specific example, the depth is preferably 1 [μm] or more and 1 [μm] or more smaller than the thickness of adhesive layer 13, and more preferably 1 [μm] or more and 10 [μm] or more smaller than the thickness of adhesive layer 13. Therefore, for example, the depth of the groove 131 is preferably within a range of 1 μm to 30 μm. The reason why the depth of the groove portion 131 is set within the above-mentioned range is that when the depth of the groove portion 131 is 1 [μm] or more, a sufficient flow path is secured for the air to flow out to the periphery of the adhesive sheet 1. Also, when the depth of the groove portion 131 is 10 [μm] or more smaller than the thickness of the adhesive layer 13, it is possible to increase the adhesion of the adhesive layer 13 to the base layer 11. Furthermore, when the depth of the groove portion 131 is 30 [μm] or less, it is possible to increase the adhesion of the adhesive layer 13 to the base layer 11 and to easily bring the bottom of the groove portion 131 into close contact with the surface of the adherend after the air has flowed out.

[0028] When forming the grooves 131, for example, an adhesive composition is applied to the back surface of the base layer 11 (the lower surface of the base layer 11 in FIG. 1). Thereafter, it is preferable to form the grooves 131 by attaching the peelable sheet 20 provided with the printed resin coating 14 having the uneven shape of the grooves 131 to the adhesive layer 13, and then drying the adhesive composition. This eliminates the need for a step performed just for forming the grooves 131, and makes it possible to form the grooves 131 by an easy and simple method. Alternatively, the grooves 131 may be formed by, for example, uniformly applying an adhesive composition to the back surface of the base layer 11 and then embossing the adhesive composition using a mold having projections and recesses for forming the grooves 131.

[0029] <Printed resin coating> The printed resin coating 14 is disposed on the surface of the peelable sheet 20 opposite to the surface facing the adhesive layer 13, and is formed in a shape (convex portion) that fills the groove portion 131. Therefore, when the adhesive layer 13 is adhered to the adherend and the printed resin coating 14 is not adhered to the adherend, the printed resin coating 14 is disposed on the adherend. The printed resin coating 14 also functions as an air-release groove coating layer that covers the groove portion 131 having the function of an air-release groove that serves as an air flow path. That is, the printed resin coating 14 is formed so as to cover the inner wall surface of the groove portion 131 while leaving a flow path for allowing air to flow out to the periphery of the adhesive sheet 1.

[0030] When the adhesive sheet 1 is applied, if extremely fine air particles remain inside the printed resin coating 14 when the air trapped at the interface between the adhesive sheet 1 and the adherend is released to the surroundings, the adhesive strength between the adhesive sheet 1 and the adherend may decrease. Also, the design of the adhesive sheet 1 may be deteriorated when viewed from the front. Therefore, by giving the printed resin coating 14 a shape that hydrodynamically improves air flow, it is possible to reduce the prominence of the groove portions 131 and improve the design of the final adhesive sheet 1.

[0031] Therefore, in order to improve the air flow, it is preferable that the shape of the printed resin coating 14 is such that, in a cross-sectional view perpendicular to the air flow path, for example, the end of the surface of the printed resin coating 14 facing the adhesive layer 13 has a gradation and the portion of the printed resin coating 14 excluding the end has a curved surface. More specifically, it is preferable that the shape of the portion of the printed resin coating 14 excluding the end has a gently curving shape in a cross-sectional view. In the first embodiment, as an example, a case will be described in which the printed resin coating 14 is formed into a shape in which the cross-sectional shape viewed from a direction perpendicular to the direction in which the pressure-sensitive adhesive layer 13 and the release sheet 20 are laminated has two end portions and a central portion located between the two end portions. In addition, a case will be described in which the end portions are formed into a shape having a surface that slopes toward the release sheet 20 as it moves away from the central portion, and the central portion is formed into a shape in which the surface facing the pressure-sensitive adhesive layer 13 is a curved surface. Note that the shape of the printed resin coating 14 is illustrated in a simplified manner in FIG. 1.

[0032] The resin material forming the printed resin coating 14 is not particularly limited as long as it is a material that has weak adhesion to the release sheet 20. In addition, the material is not particularly limited as long as it allows for a degree of adhesion that prevents the release sheet 20 from peeling off naturally while stored in a rolled state, and allows for printing a pattern having continuous openings on the release sheet 20. In addition, the resin material for forming the printed resin coating 14 is, for example, a material that is capable of maintaining the printed resin coating 14 for a long period of time without being corroded by the solvent such as acrylic or toluene of the adhesive composition constituting the adhesive layer 13.

[0033] Therefore, for example, an acrylic resin mixed with a solvent such as methyl ethyl ketone can be used as the resin material forming the printed resin coating 14. This is because the printability of the printed resin constituting the printed resin coating 14 and the releasability of the printed resin coating 14 from the peelable sheet 20 when peeling the peelable sheet 20 from the adhesive sheet 1 are high. In addition, the resin material forming the printed resin coating 14 preferably contains at least an acrylic resin. By containing an acrylic resin, the solvent resistance of the printed resin coating 14 is improved, so that even if the printed resin coating 14 is stored in contact with the adhesive layer 13, the printed resin coating 14 is less likely to deteriorate, and the drying property of the printed resin is improved, making blocking and traction less likely to occur. In addition, when the printed resin coating 14 is formed, the generation of air bubbles due to the evaporation of residual solvent is suppressed. This improves the design of the adhesive sheet 1.

[0034] In addition, it is preferable to select a resin material for forming the printed resin coating 14 that has a refractive index close to that of the adhesive layer 13, i.e., a refractive index within 0.70 different from that of the adhesive layer 13. It is even more preferable to select a resin material that has a refractive index within 0.30 different from that of the adhesive layer 13. This reduces the refractive index difference at the interface between the printed resin coating 14 and the adhesive layer 13, and reduces the prominence of the grooves 131 when viewed from the surface of the adhesive sheet 1, thereby improving the design of the adhesive sheet 1 when it is finished after application.

[0035] The printed resin coating 14 terminates at the outer periphery of the adhesive layer 13 (or the peelable sheet 20) to match the shape of the groove portion 131, or is connected to another printed resin coating 14 that terminates at the outer periphery of the adhesive layer 13 (or the peelable sheet 20). By terminating the printed resin coating 14 at the outer periphery, it is possible to adhere the adhesive sheet 1 to the adherend without allowing air bubbles to enter the interface. Furthermore, by terminating the printed resin coating 14 at the outer periphery, it is possible to prevent removal marks from remaining when the adhesive sheet 1 is peeled off, even if a long period of time has passed since the adhesive sheet 1 was adhered. Specifically, the edge of at least one of the multiple printed resin coatings 14 is disposed on the outer periphery of the pressure-sensitive adhesive layer 13 or the peelable sheet 20. In addition, the edge of at least one of the multiple printed resin coatings 14 is continuous with an end whose edge is disposed on the outer periphery of the pressure-sensitive adhesive layer 13 or the peelable sheet 20. Note that in Fig. 1, the positional relationship between the printed resin coating 14 and the pressure-sensitive adhesive layer 13 and the peelable sheet 20 is illustrated in a simplified manner.

[0036] The printed resin coating 14 may be formed from a resin material to which a pigment, dye, pearl, or the like has been added. By coloring the printed resin coating 14, the shape of the printed resin coating 14 becomes visible from the front side of the adhesive sheet 1, which makes it possible to express designs with new textures that could not be expressed with existing adherends. For example, the printed resin coating 14 can realize designs with a three-dimensional effect, designs with a sense of brilliance, and designs where the final finished design can be easily changed or replaced by re-pasting.

[0037] Moreover, the printed resin coating 14 is formed without using an antifoaming agent, and air bubbles are formed inside the printed resin coating 14. Note that the air bubbles formed inside the printed resin coating 14 are not shown in Fig. 1. In addition, the printed resin film 14 is formed without using organic particles such as acrylic beads, urethane beads, etc. Furthermore, the printed resin film 14 is formed without using inorganic particles.

[0038] The reason why the printed resin film 14 is formed without using an antifoaming agent, organic particles, or inorganic particles will be described below. If the printed resin coating 14 is configured to include organic particles such as acrylic beads or urethane beads, the non-flammability will decrease in components that require non-flammability. Also, if inorganic particles are added to the printed resin coating 14, in a transparent adhesive sheet 1, the beads and the printed resin coating 14 to which the beads have been added will be clearly visible from the surface of the adhesive sheet 1, which may significantly impair the design. Therefore, in order to improve non-combustibility while allowing the air remaining at the interface with the adherend to escape to the outside, a method other than adding beads to the printed resin coating 14 is required. Therefore, when forming the printed resin coating 14, a defoaming agent, which is a substance with a defoaming effect, is not used, and the printed resin coating 14 containing fine bubbles is formed. Therefore, the fine bubbles contained in the printed resin coating 14 do not impair the shape stability of the printed resin coating 14, and the non-flammability is not reduced while a passageway for the air remaining at the interface with the adherend is secured. In addition, since the printed resin coating 14 has fine bubbles, the printing suitability such as drying property is improved, and the blocking phenomenon of the printed resin coating 14 is less likely to occur.

[0039] By having the printed resin coating 14, the adhesive sheet 1 can be applied to adherends with a large area or adherends that are not water resistant, while improving the design. In addition, the adhesive sheet 1 can be applied without making holes to allow air trapped at the interface between the adhesive sheet 1 and the adherend to escape to the surroundings when the sheet is attached. This makes it possible to prevent water or contaminants from entering the interface between the adhesive sheet 1 and the adherend through holes formed in the adhesive sheet 1, thereby improving water resistance, contamination resistance, scratch resistance, weather resistance, and the like.

[0040] As a method for forming the printed resin coating 14, for example, a printing method such as gravure printing, flexographic printing, offset printing, screen printing, rotary printing, inkjet printing, etc. Also employable is a method for embossing the printed resin coating 14 using a roller-shaped die, or a method for forming the printed resin coating 14 made of resin on the surface of a plastic film or the like using a roller-shaped die and a fluid resin composition.

[0041] Moreover, the resin material that forms the printed resin film 14 is preferably cured using ultraviolet rays or electron beams. This is because not using a thermosetting resin makes it possible to reduce greenhouse gases that are predicted to be generated by heating and drying, enabling the creation of environmentally friendly products.

[0042] <Removable sheet> The peelable sheet 20 is a sheet-like member that is attached to the adhesive layer 13 in a laminated state on the surface opposite the surface of the adhesive layer 13 facing the base layer 11 (in Figure 1, the underside of the adhesive layer 13). Furthermore, the release sheet 20 is a member for preventing the pressure-sensitive adhesive layer 13 from being exposed before the pressure-sensitive adhesive sheet 1 is used. When the release sheet 20 is attached to the adhesive layer 13, the release sheet 20 covers the surface of the adhesive layer 13 facing the base layer 11, the groove portion 131, and the printed resin coating 14. By covering the adhesive layer 13 with the release sheet 20, it is possible to prevent the adhesive layer 13 from coming into contact with anything other than the adhesive sheet 1 before use of the adhesive sheet 1, and it is also possible to laminate or roll the adhesive sheet 1 without the adhesive layer 13 coming into contact with the surface of the adhesive sheet 1. Furthermore, the release sheet 20 is peeled off from the adhesive layer 13 when the adhesive sheet 1 is used (when the adhesive sheet 1 is attached to an adherend).

[0043] The release sheet 20 may be, for example, a laminate in which a release layer mainly made of silicone resin or the like is laminated on the surface of an appropriate base material such as a plastic film or paper. Alternatively, for example, a polyolefin resin film such as a polyethylene film, or a polyethylene terephthalate resin film may be used. Furthermore, in many cases, the release sheet 20 generally has a coating layer formed on the surface thereof using a silicone coating, a fluorine coating, or the like to improve release properties, but the release sheet 20 having such a coating layer is expensive. For this reason, by using a technique in which an additive such as a release agent is added to the material used for the printed resin coating 14 instead of a coating layer, or by using a release sheet 20 whose surface is not subjected to a surface treatment such as a corona treatment or an ozone treatment, it becomes possible to control the adhesion between the printed resin coating 14 and the release sheet 20 and the adhesion during storage, even if a coating layer is not formed on the surface of the release sheet 20. The peelable sheet 20 is discarded after application as it is no longer necessary. However, the peelable sheet 20 that does not form a coating layer can be used in CO 2This will also contribute to reducing waste in terms of emissions, etc., making it possible to create environmentally friendly products.

[0044] <Method of manufacturing adhesive sheet> A method for producing the adhesive sheet 1 will now be described. When manufacturing the pressure-sensitive adhesive sheet 1, air bubbles are formed inside the printed resin film 14 by forming the printed resin film 14 without using an antifoaming agent. Furthermore, when the printed resin film 14 is formed, the resin material is stirred with a pump that generates minute vibrations.

[0045] The above-described first embodiment is one example of the present invention, and the present invention is not limited to the above-described first embodiment. Various modifications can be made depending on the design, etc., even in forms other than this embodiment, as long as they do not deviate from the technical idea of ​​the present invention.

[0046] (Effects of the First Embodiment) The method for producing the pressure-sensitive adhesive sheet 1 of the first embodiment makes it possible to achieve the effects described below. (1) A printed resin coating 14 that is formed in a shape that fills the groove portion 131 and does not have adhesiveness is formed without using an antifoaming agent. Therefore, it is possible to form cavities in the printed resin film 14 that are not dependent on particles or the like.

[0047] As a result, the cavities (fine air bubbles contained in the printed resin coating 14) formed in the printed resin coating 14 do not impair the shape stability of the printed resin coating 14, and it is possible to ensure a passageway for any air remaining at the interface with the adherend. As a result, when the adhesive sheet 1 is attached to an adherend, air remaining at the boundary between the adhesive sheet 1 and the adherend can be discharged to the surroundings via the grooves 131 and the printed resin coating 14, making the grooves 131 less visible from the surface of the adhesive sheet 1. It is therefore possible to provide a manufacturing method for the adhesive sheet 1 that can suppress deterioration of the design.

[0048] Furthermore, even if the pressure-sensitive adhesive sheet 1 is transparent, it can be attached to a large area or to an adherend with low water resistance, making it possible to improve workability. Furthermore, since the printed resin film 14 does not contain an antifoaming agent, it is possible to improve non-flammability.

[0049] In addition, it becomes possible to maintain roughness on the surface of the printed resin coating 14, and even when the adhesive sheet 1 is rolled up after the printed resin coating 14 is formed, it becomes possible to suppress the occurrence of blocking and peeling of the printed resin coating 14. Furthermore, it is possible to adjust the size of the cavities formed in the printed resin coating 14 by adjusting the conditions for forming the printed resin coating 14 (printing conditions), regardless of the particles added to the printed resin coating 14.

[0050] (2) The printed resin coating 14 is formed without using organic particles. As a result, the flame retardancy of the pressure-sensitive adhesive sheet 1 can be improved.

[0051] (3) The printed resin coating 14 is formed without using inorganic particles. As a result, it is possible to suppress deterioration in the design of the pressure-sensitive adhesive sheet 1.

[0052] (4) The printed resin coating 14 is formed into a shape having two end portions and a central portion located between the two end portions in a cross section viewed from a direction perpendicular to the lamination direction of the adhesive layer 13 and the release sheet 20. In addition, the end portions are formed into a shape having a surface that slopes toward the release sheet 20 as it moves away from the central portion, and the central portion is formed into a shape in which the surface facing the adhesive layer 13 is a curved surface. This allows the printed resin film 14 to be configured so that the edges have gradation and the center has a curved surface. As a result, air is less likely to remain inside the groove portion 131 whose inner walls are covered with the printed resin coating 14, and the groove portion 131 is less likely to be visible from the surface of the adhesive sheet 1, making it possible to provide a manufacturing method for the adhesive sheet 1 that is capable of suppressing a decrease in design.

[0053] (5) The edge of at least one of the multiple printed resin coatings 14 is disposed on the outer periphery of the pressure-sensitive adhesive layer 13 or the release sheet 20 . For this reason, it is possible to configure the printed resin coating 14 so that it terminates at the outer periphery of the pressure-sensitive adhesive layer 13 or the outer periphery of the release sheet 20 . As a result, when applying the pressure-sensitive adhesive sheet 1, air trapped between the pressure-sensitive adhesive sheet 1 and the adherend can be released to the surroundings.

[0054] (6) At least one of the printed resin coatings 14 has an end that is continuous with an end whose edge is located on the outer periphery of the pressure-sensitive adhesive layer 13 or the release sheet 20 . For this reason, the printed resin film 14 can be configured to be continuous with other printed resin films 14 that terminate at the outer periphery of the pressure-sensitive adhesive layer 13 or the outer periphery of the release sheet 20 . As a result, when applying the pressure-sensitive adhesive sheet 1, air trapped between the pressure-sensitive adhesive sheet 1 and the adherend can be released to the surroundings.

[0055] (7) The printed resin coating 14 is formed using a resin material containing an acrylic resin. As a result, it is possible to improve the printability of the printed resin that forms the printed resin coating 14 and the releasability of the printed resin coating 14, making it easier to leave the printed resin coating 14 formed in the desired shape on the adhesive sheet 1 when the adhesive sheet 1 is used. The adhesive sheet 1 of the first embodiment can achieve the effects described below.

[0056] (8) Air bubbles are formed inside the printed resin coating 14 that is formed in a shape that fills the groove portion 131 and does not have adhesiveness. Therefore, it is possible to form cavities in the printed resin film 14 that are not dependent on particles or the like.

[0057] As a result, the cavities (fine air bubbles contained in the printed resin coating 14) formed in the printed resin coating 14 do not impair the shape stability of the printed resin coating 14, and it is possible to ensure a passageway for any air remaining at the interface with the adherend. As a result, when the adhesive sheet 1 is attached to an adherend, air remaining at the boundary between the adhesive sheet 1 and the adherend can be discharged to the surroundings via the grooves 131 and the printed resin coating 14, making the grooves 131 less visible from the surface of the adhesive sheet 1. Therefore, it is possible to provide an adhesive sheet 1 that can suppress deterioration in design.

[0058] Furthermore, even if the pressure-sensitive adhesive sheet 1 is transparent, it can be attached to a large area or to an adherend with low water resistance, making it possible to improve workability. Furthermore, since the printed resin film 14 does not contain an antifoaming agent, it is possible to improve non-flammability.

[0059] In addition, it becomes possible to maintain roughness on the surface of the printed resin coating 14, and even when the adhesive sheet 1 is rolled up after the printed resin coating 14 is formed, it becomes possible to suppress the occurrence of blocking and peeling of the printed resin coating 14. Furthermore, it is possible to adjust the size of the cavities formed in the printed resin coating 14 by adjusting the conditions for forming the printed resin coating 14 (printing conditions), regardless of the particles added to the printed resin coating 14.

[0060] (Modification of the first embodiment) (1) In the first embodiment, a configuration in which the surface protective layer 12 is laminated on the base layer 11 has been described, but the present invention is not limited to this, and a configuration in which another layer is disposed between the base layer 11 and the surface protective layer 12 may also be used. In this case, for example, a configuration in which a picture pattern layer is disposed between the base layer 11 and the surface protective layer 12 may also be used. This makes it possible to impart a desired design to the pressure-sensitive adhesive sheet 1.

[0061] (2) In the first embodiment, the base layer 11 has a single-layer structure. However, the present invention is not limited to this. The base layer 11 may have a structure of two or more layers.

[0062] (3) In the first embodiment, an example of a structure in which the surface (upper surface) of the pressure-sensitive adhesive sheet 1 is flat is shown, but the present invention is not limited thereto. That is, for example, unevenness may be formed by embossing only on the surface protective layer 12, or on both the base layer 11 and the surface protective layer 12. This makes it possible to impart a three-dimensional design to the pressure-sensitive adhesive sheet 1.

[0063] (4) In the first embodiment, a configuration example in which the surface protective layer 12 has a single-layer structure is shown, but this is not limited to this, and the surface protective layer 12 may be configured to be formed of multiple layers. EXAMPLES

[0064] With reference to the first embodiment, the pressure-sensitive adhesive sheet of Example 1 and the pressure-sensitive adhesive sheets of Comparative Examples 1 to 6 will be described below.

[0065] Example 1 As a release sheet, a 70 μm-thick polypropylene (PP) laminated paper with no coating film such as silicone coating or fluorine coating on the surface was used. Furthermore, without using an antifoaming agent, an acrylic resin (manufactured by DIC Corporation) was printed on a release sheet by gravure printing, and then dried and cured to form a plurality of printed resin coatings. In this manner, the adhesive sheet of Example 1 was formed.

[0066] Comparative Example 1 An adhesive sheet of Comparative Example 1 was formed in the same manner as in Example 1, except that the printed resin coating was formed by adding transparent beads (organic particles). Comparative Example 2 A pressure-sensitive adhesive sheet of Comparative Example 2 was formed in the same manner as in Example 1, except that the printed resin coating was formed using an antifoaming agent. Comparative Example 3 An adhesive sheet of Comparative Example 3 was formed in the same manner as in Example 1, except that the printed resin coating was formed by adding a urethane-based mixed resin. Comparative Example 4 The adhesive sheet of Comparative Example 4 was formed in the same manner as in Example 1, except that the printed resin coating was formed by adding transparent beads (organic particles) to a urethane resin instead of using an acrylic resin. Comparative Example 5 An adhesive sheet of Comparative Example 5 was formed in the same manner as in Example 1, except that the printed resin coating was formed using a urethane resin instead of an acrylic resin. Comparative Example 6 An adhesive sheet of Comparative Example 6 was formed in the same manner as in Example 1, except that the printed resin coating was formed by adding inorganic beads (inorganic particles).

[0067] (Performance evaluation, evaluation results) The adhesive sheet of Example 1 and the adhesive sheets of Comparative Examples 1 to 6 were each evaluated for printability, releasability, solvent resistance, drying conditions, low visibility of the printed resin coating, air venting effect, and non-flammability.

[0068] <Printability> The printing resin coating was printed by gravure printing on printing base paper and PVC base roll, and printability was evaluated by visually checking whether printing was performed according to the plate design. Printing suitability was evaluated as "good" when the printing resin coating was printed on the printing base paper and PVC base roll according to the plate design, evaluated as "good" when there were gaps or chips in the areas that should have been printed according to the plate design, and evaluated as "bad" when printing was not possible at all.

[0069] <Mold releasability> Polypropylene laminated paper was used as the release sheet, and each base agent was gravure printed and cured. Then, Cellotape (registered trademark) was attached and pressed onto the sheet, and the tape was peeled off. The release property was evaluated by visually checking whether the printed resin coating peeled off completely from the release sheet. The release properties were evaluated as "good" when all the printed resin coating peeled off cleanly to the cellophane tape side, as "good" when the printed resin coating did not peel off completely in one try but peeled off after several tries, and as "poor" when no peeling at all was observed.

[0070] <Solvent resistance> Polypropylene laminated paper was used as the release sheet, and the gravure-printed printed resin coating was lightly rubbed with a cloth soaked in ethanol or methyl ethyl ketone. The solvent resistance was evaluated by visually checking whether the printed resin coating had peeled off, changed in gloss, or dissolved. The solvent resistance was evaluated as "good" when no significant change occurred in the printed resin coating in any of the various solvents, evaluated as "good" when only a slight change in gloss occurred in the printed resin coating in either of the solvents, and evaluated as "bad" when the printed resin coating peeled off in both solvents.

[0071] <Drying conditions> When a resin film was printed using a gravure printing machine, the drying conditions were evaluated by visually checking whether the print was dried to a degree that did not cause blocking and whether there was any resin traction on the rolls of the printing machine. The drying conditions were evaluated as "good" when neither blocking nor roll error occurred, "good" when there was some uncured state and there was a tendency for blocking, and "bad" when drying was clearly insufficient and significant blocking was observed.

[0072] <Low visibility of printed resin coating> The low visibility of the printed resin coating was evaluated by attaching a transparent adhesive sheet having a base layer with various printed resin coatings to a black board and visually checking whether the shape, etc. of the printed resin coating was clearly visible. Low visibility was evaluated as "good" when some parts were only slightly visible, but not so unnatural that it detracted from the design. It was evaluated as "good" when the shape of the printed resin coating was visible only if one looked closely. It was evaluated as "good" when the shape of the printed resin coating was clearly visible.

[0073] <Air removal effect> The air release effect was evaluated by checking whether the air remaining between the adhesive sheet and the adherend could be released by pressing the adhesive sheet against the adherend when the adhesive sheet was peeled off from the release sheet and attached to the adherend. The air release effect was evaluated as "Good" when the remaining air could be released when the material was pressed, and "Good" when the remaining air could be released when the material was pressed but there were some areas where it was difficult to release air or when there was fine air remaining. Furthermore, the air release effect was evaluated as "Poor" when the remaining air could not be released at all even when the material was pressed.

[0074] <Nonflammable> In a heat generation test using a cone calorimeter tester conforming to ISO5660-1, non-combustibility was evaluated by checking whether requirements 1 to 3 were met. Note that gypsum board was used as the non-combustible substrate. Requirement 1: Total heat output is 8 [MJ / m 2 ]below. Requirement 2: The maximum heat generation rate is 200 [kW / m for 10 seconds or more. 2 ]. Requirement 3: There must be no cracks or holes that are harmful to fire resistance and penetrate to the back surface. For non-flammability, a material was rated as "Good" if it met all of the requirements 1 to 3, "Average" if it did not meet one or two of the requirements 1 to 3, and "Poor" if it did not meet all of the requirements 1 to 3.

[0075] [Table 1]

[0076] As a result of evaluating various performances using the above-mentioned methods, the pressure-sensitive adhesive sheet of Example 1 exhibited excellent performance in all evaluation tests, whereas the pressure-sensitive adhesive sheets of Comparative Examples 1 to 6 were unable to exhibit excellent performance in all evaluation tests. [Explanation of symbols]

[0077] 1...adhesive sheet, 11...base material layer, 12...surface protection layer, 13...adhesive layer, 131...groove portion, 14...printed resin coating, 20...peelable sheet

Claims

1. A base layer formed of a transparent extensible film; a pressure-sensitive adhesive layer laminated on one surface of the base layer and having a groove formed on a surface opposite to a surface facing the base layer; a printed resin coating formed in a shape that fills the groove portion and that does not have adhesiveness; a peelable sheet laminated on a surface of the pressure-sensitive adhesive layer opposite to a surface facing the base layer, the peelable sheet covering the surface of the pressure-sensitive adhesive layer facing the base layer, the groove portion, and the printed resin coating, The method for producing a pressure-sensitive adhesive sheet, wherein the printed resin film is formed without using a defoaming agent.

2. The method for producing a pressure-sensitive adhesive sheet according to claim 1 , wherein the printed resin film is formed without using organic particles.

3. The method for producing a pressure-sensitive adhesive sheet according to claim 1 or 2, wherein the printed resin film is formed without using inorganic particles.

4. The printed resin coating is formed into a shape having two end portions and a central portion disposed between the two end portions in a cross section viewed from a direction perpendicular to a direction in which the pressure-sensitive adhesive layer and the release sheet are laminated; The end portion is formed into a shape having a surface that is inclined so as to approach the release sheet as it moves away from the central portion, The method for producing a pressure-sensitive adhesive sheet according to claim 1 , wherein the central portion is formed so that the surface facing the pressure-sensitive adhesive layer is curved.

5. forming a plurality of the printed resin coatings; The method for producing a pressure-sensitive adhesive sheet according to claim 4 , wherein an edge of an end portion of at least one of the plurality of printed resin coatings is disposed on an outer periphery of the pressure-sensitive adhesive layer or the release sheet.

6. A method for manufacturing an adhesive sheet as described in claim 5, wherein the end portion of at least one of the multiple printed resin coatings is continuous with the end portion where the edge is located on the outer periphery of the adhesive layer or the release sheet.

7. The method for producing a pressure-sensitive adhesive sheet according to claim 1 , wherein the printed resin film is formed using a resin material containing an acrylic resin.

8. A base layer formed of a transparent extensible film; a pressure-sensitive adhesive layer laminated on one surface of the base layer and having a groove formed on a surface opposite to a surface facing the base layer; a printed resin coating formed in a shape that fills the groove portion and that does not have adhesiveness; a peelable sheet laminated on a surface of the pressure-sensitive adhesive layer opposite to a surface facing the base layer, the peelable sheet covering the surface of the pressure-sensitive adhesive layer facing the base layer, the groove portion, and the printed resin coating, An adhesive sheet having air bubbles formed inside the printed resin coating.

Citation Information

Patent Citations

  • Adhesive sheet and method for manufacturing same

    JP6856163B1