Cement composition, mortar composition, and method for repairing concrete structures
A cement composition with calcium carbonate and polycarboxylic acid copolymer addresses the issue of mortar flow into formwork, providing controlled fluidity and viscosity for improved concrete repair adhesion and surface quality.
Patent Information
- Application Number
- JP2023051687
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Existing mortars with high fluidity tend to flow into formwork, leading to air pockets and uneven surfaces, compromising adhesion to concrete bases.
A cement composition comprising calcium carbonate and a polycarboxylic acid copolymer, with specific mass ratios and content, to provide fluidity and viscosity control.
The composition imparts fluidity to mortar, preventing air pockets and ensuring even surfaces, enhancing adhesion and workability in concrete repairs.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a cement composition, a mortar composition, and a method for repairing a concrete structure. [Background technology]
[0002] Concrete structures deteriorate due to various factors such as salt damage, carbonation, etc. Deteriorated concrete structures are repaired, for example, by removing the deteriorated portions and filling them with mortar or concrete.
[0003] When the mortar or concrete is filled by gravity flow or by using a pump or the like, the mortar or concrete needs to have an appropriate fluidity. For this reason, various fluidizing agents (water reducing agents) have been conventionally added to the mortar or concrete. For example, Patent Document 1 describes a high-fluidity non-shrink mortar made of cement, sand, a water reducing agent, an expansive agent, a foaming agent, a defoaming agent, and a separation reducing agent as a filling non-shrink mortar to be filled into gaps between concrete or the like. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2006-248831 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, when the mortar or concrete is filled into the gap between the formwork and the concrete base material, if a highly fluid mortar such as that in Patent Document 1 is used, the mortar will flow quickly into the formwork, causing air pockets at the interface between the concrete base material and the mortar, and there is a risk that adhesion to the concrete base material will not be ensured. In addition, if air pockets remain in the formwork, there is a risk that unevenness will occur on the surface of the hardened product after it is removed from the formwork. Therefore, there is a demand for a mortar that has fluidity and a viscosity that can suppress the occurrence of air pockets.
[0006] The present invention has been made in view of the above-mentioned circumstances, and aims to provide a cement composition and a mortar composition that can impart fluidity and improve viscosity, and also to provide a method for repairing a concrete structure using such a mortar composition. [Means for solving the problem]
[0007] The cement composition according to the present invention comprises a binder containing cement, calcium carbonate, and a water-reducing agent, the water-reducing agent comprising a polycarboxylic acid-based copolymer containing the following structural unit (1) and the following structural unit (2), and the mass ratio of the calcium carbonate to the polycarboxylic acid-based copolymer (calcium carbonate / polycarboxylic acid-based copolymer) is 1.0 or more and 14.0 or less. Structural unit (1): A structural unit formed from one or more monomers selected from those represented by the following formula (1): Structural unit (2): A structural unit formed from one or more selected from (meth)acrylic acid and / or a salt thereof. [ka] (In formula (1), R 1 , R 2 and R 3 are the same or different, each represents a hydrogen atom or a methyl group, R 4 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 22 carbon atoms. p represents an integer of 0 to 5. q represents an integer of 0 or 1. A1 O represents an oxyalkylene group having 2 to 4 carbon atoms. n is A 1 is the average number of moles of O added, and represents a number from 40 to 120.)
[0008] With such a constitution, the cement composition can impart fluidity to mortar or concrete and improve the viscosity.
[0009] In the cement composition according to the present invention, the content of the calcium carbonate may be 2.0% by mass or more and 20.0% by mass or less with respect to the binder.
[0010] With such a constitution, the cement composition can impart fluidity to mortar or concrete and can further improve the viscosity.
[0011] The mortar composition according to the present invention contains the cement composition and fine aggregate.
[0012] With such a constitution, the mortar composition can impart fluidity to mortar or concrete and improve the viscosity.
[0013] In the method for repairing a concrete structure according to the present invention, the mortar composition is used as a grout material.
[0014] The method for repairing a concrete structure is excellent in workability because it uses, as a grout material, a mortar composition that can impart fluidity and improve viscosity. Effect of the Invention
[0015] According to the present invention, it is possible to provide a cement composition and a mortar composition that can impart fluidity and improve viscosity, and also to provide a method for repairing a concrete structure using such a mortar composition. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] <Cement composition> The cement composition according to this embodiment will be described below.
[0017] The cement composition according to the present embodiment includes a binder containing cement, calcium carbonate, and a water reducing agent. The binder is a general term for materials that react with water to generate a substance that contributes to the development of strength in concrete, and includes cement. The binder may include other materials besides cement, such as ground granulated blast furnace slag, fly ash, silica fume, cement kiln dust, blast furnace fume, ground granulated converter slag, etc.
[0018] Examples of cement include ordinary Portland cement, high-early-strength Portland cement, ultra-high-early-strength Portland cement, moderate-heat Portland cement, low-heat Portland cement, sulfate-resistant Portland cement, white Portland cement, ultra-high-speed hardening cement, alumina cement, etc. Also usable are various mixed cements obtained by mixing the Portland cement with fly ash, blast furnace slag, etc. One type of cement may be used alone, or two or more types may be used in combination.
[0019] From the viewpoint of stabilizing the strength development, the content of the cement is preferably 80.0% by mass or more and 100.0% by mass or less, and more preferably 90.0% by mass or more and 95.0% by mass or less, based on the total amount of the binder. When two or more kinds of cement are contained, the content is the total content.
[0020] Examples of ground granulated blast furnace slag include ground granulated blast furnace slag 3000, ground granulated blast furnace slag 4000, ground granulated blast furnace slag 6000, ground granulated blast furnace slag 8000, etc., as specified in JIS A 6206: 2013. Note that the ground granulated blast furnace slag may be used alone or in combination of two or more kinds.
[0021] Examples of the fly ash include fly ash type I, fly ash type II, fly ash type III, and fly ash type IV as specified in JIS A 6201: 2015. The fly ash may be used alone or in combination of two or more types.
[0022] From the viewpoint of increasing the separation resistance of the material, the content of the binder is preferably 0.1 mass % or more and 20.0 mass % or less, and more preferably 5.0 mass % or more and 10.0 mass % or less, based on the entire cement composition.
[0023] From the viewpoint of imparting fluidity and increasing the separation resistance of the material, the content of calcium carbonate is preferably 2.0 mass % or more and 20.0 mass % or less, and more preferably 4.0 mass % or more and 15.0 mass % or less, relative to the binder.
[0024] The water reducing agent contains a polycarboxylic acid copolymer containing the following structural unit (1) and the following structural unit (2). Structural unit (1): A structural unit formed from one or more monomers selected from those represented by the following formula (1): Structural unit (2): A structural unit formed from one or more selected from (meth)acrylic acid and / or a salt thereof. [ka]
[0025] In formula (1), R 1 , R 2 and R 3 R represents a hydrogen atom or a methyl group, which may be the same or different. 4 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 22 carbon atoms. p represents an integer of 0 to 5. q represents an integer of 0 or 1. A 1 O represents an oxyalkylene group having 2 to 4 carbon atoms. n is A 1 This is the average number of moles of O added and represents a number from 40 to 120.
[0026] In formula (1), p is an integer of 0 to 5, preferably an integer of 0 to 2, and more preferably an integer of 0 or 1. In addition, q is preferably an integer of 0 or 1.
[0027] In formula (1), A 1 O is an oxyalkylene group having 2 to 4 carbon atoms, and examples thereof include an oxyethylene group, an oxypropylene group, and an oxybutylene group. 1 When O is two or more kinds, it may be in any form of a random adduct, a block adduct, or an alternating adduct. In consideration of the solubility of the copolymer, in order to maintain the water solubility of the copolymer, it is preferable that 50 mol % or more of the total oxyalkylene groups in formula (1) are oxyethylene groups, more preferably 90 mol % or more are oxyethylene groups, and even more preferably 95 mol % or more are oxyethylene groups. In formula (1), n is A 1 It represents the average number of moles of O added and is an integer from 40 to 120, and from the viewpoint of ensuring dispersibility, an integer from 45 to 115 is preferable, and an integer from 50 to 115 is more preferable.
[0028] Examples of the monomer represented by formula (1) include polyethylene glycol mono(meth)acrylate, (poly)propylene (poly)ethylene glycol mono(meth)acrylate, methoxypolyethylene glycol (meth)acrylate, methoxy(poly)ethylene (poly)propylene glycol mono(meth)acrylate, butoxy(poly)ethylene glycol mono(meth)acrylate, (poly)ethylene glycol (poly)butylene glycol vinyl ether, polyethylene glycol monoallyl ether, (poly)ethylene glycol mono(2-methyl-2-propenyl) ether, polyethylene glycol mono(3-methyl-butenyl) ether, polyethylene(poly)propylene glycol mono(2-methyl-2-propenyl) ether, etc. The monomer represented by formula (1) forming the structural unit (1) may be used alone or in combination.
[0029] The structural unit (2) is a structural unit formed from one or more selected from (meth)acrylic acid and / or a salt thereof. The salt of (meth)acrylic acid forming the structural unit (2) is not particularly limited, and examples thereof include alkali metal salts such as sodium salt and potassium salt, alkaline earth metal salts such as calcium salt and magnesium salt, ammonium salt, and amine salts such as diethanolamine salt and triethanolamine salt.
[0030] From the viewpoint of maintaining dispersibility and fluidity, the polycarboxylic acid copolymer preferably contains 70.0% by mass or more and 86.0% by mass or less of the structural unit (1) in all structural units, more preferably 74.0% by mass or more and 86.0% by mass or less in all structural units, and even more preferably 78.0% by mass or more and 86.0% by mass or less in all structural units. From the viewpoint of maintaining dispersibility and fluidity, the polycarboxylic acid copolymer preferably contains 14.0% by mass or more and 30.0% by mass or less of the structural unit (2) in all structural units, more preferably 14.0% by mass or more and 26.0% by mass or less in all structural units, and even more preferably 14.0% by mass or more and 22.0% by mass or less in all structural units.
[0031] The polycarboxylic acid copolymer preferably contains a structural unit (3) in addition to the structural units (1) and (2). The structural unit (3) is a structural unit formed from one or more selected from (hydroxy)alkyl (meth)acrylates in which the alkyl group has 1 to 4 carbon atoms. Examples of the (hydroxy)alkyl (meth)acrylate include methyl acrylate, hydroxyethyl acrylate, methyl methacrylate, and butyl acrylate. The monomer forming the structural unit (3) may be one or more.
[0032] The polycarboxylic acid copolymer is more preferably composed of the structural unit (1), the structural unit (2), and the structural unit (3). From the viewpoint of maintaining dispersibility and fluidity, the polycarboxylic acid copolymer preferably contains 70.5% by mass or more and 85.0% by mass or less of the structural unit (1) in all structural units, more preferably 74.5% by mass or more and 85.0% by mass or less in all structural units, and even more preferably 78.5% by mass or more and 85.0% by mass or less in all structural units. From the viewpoint of maintaining dispersibility and fluidity, the polycarboxylic acid copolymer preferably contains 14.5% by mass or more and 29.0% by mass or less of the structural unit (2) in all structural units, more preferably 14.5% by mass or more and 25.0% by mass or less in all structural units, and even more preferably 14.5% by mass or more and 21.0% by mass or less in all structural units. From the viewpoint of maintaining dispersibility and fluidity, the polycarboxylic acid copolymer preferably contains the structural unit (3) in an amount of 0.5% by mass or more and 5.0% by mass or less of all structural units, more preferably 0.5% by mass or more and 3.0% by mass or less of all structural units, and even more preferably 0.5% by mass or more and 2.0% by mass or less of all structural units.
[0033] The polycarboxylic acid copolymer may contain, in addition to the structural units (1) and (2), a structural unit (4) derived from a monomer copolymerizable with the monomers forming these structural units. That is, the polycarboxylic acid copolymer may contain the structural units (1), (2) and (4), or the polycarboxylic acid copolymer may contain the structural units (1), (2), (3) and (4). The monomer forming such structural unit (4) is not particularly limited so long as it is copolymerizable with at least one of the monomers forming structural unit (1), structural unit (2), and structural unit (3). Examples of such monomers include unsaturated amides such as (meth)acrylamide and N,N-dimethyl(meth)acrylamide, unsaturated cyanides such as (meth)acrylonitrile, unsaturated dicarboxylic acid esters which form monoesters or diesters of unsaturated dicarboxylic acids such as maleic acid and fumaric acid with (poly)alkylene glycols or alcohols of alkyl or alkenyl groups having 1 to 22 carbon atoms, amide monomers which form monoamides or diamides of unsaturated carboxylic acids or unsaturated dicarboxylic acids with amines having 1 to 22 carbon atoms, amide monomers which form monoamides or diamides of unsaturated carboxylic acids or unsaturated dicarboxylic acids with amines having 1 to 22 carbon atoms, alkyl diamides and alkyl diamides ... Examples of such monomers include reaction products of a condensation product of carboxylic acid and polyethylene polyamine to which ethylene oxide or propylene oxide has been added to a nitrogen atom having active hydrogen, and the resulting product, with (meth)acrylic acid; amide monomers which form monoamides or diamides of unsaturated carboxylic acids or unsaturated dicarboxylic acids and amines having 1 to 22 carbon atoms; polyamide polyamine monomers which are obtained by reacting a condensation product of alkyl dicarboxylic acid and polyethylene polyamine to which ethylene oxide or propylene oxide has been added to a nitrogen atom having active hydrogen, with glycidyl (meth)acrylate; sulfonic acid monomers such as (meth)allylsulfonic acid, vinylsulfonic acid, and salts thereof; and phosphoric acid monomers such as 2-(methacryloyloxy)ethyl phosphate, bis[2-(methacryloyloxy)ethyl] phosphate, and salts thereof.
[0034] From the viewpoint of suppressing an increase in the addition rate, the polycarboxylic acid copolymer preferably has a mass average molecular weight in terms of polyethylene glycol measured by gel permeation chromatography of 20,000 to 100,000, more preferably 25,000 to 45,000. The gel permeation chromatography measurement is carried out under the following conditions.
[0035] (Measurement conditions) Equipment: Showa Denko Co., Ltd. Shodex GPC-101 Column: Showa Denko OHpak SB-G+SB-806M HQ+SB-806M HQ Detector: Differential refractometer (RI) Eluent: 50mM sodium nitrate aqueous solution Flow rate: 0.7mL / min Column temperature: 40℃ Sample concentration: 0.5% by mass in eluent solution Standard material: Polyethylene glycol
[0036] The polycarboxylic acid copolymer can be produced by various methods. For example, radical polymerization using water as a solvent, radical polymerization using an organic solvent as a solvent, and solvent-free radical polymerization can be used. The reaction temperature in the radical polymerization is preferably 0 to 120°C, more preferably 20 to 100°C, and even more preferably 50 to 90°C, from the viewpoint of reaction time and the like. Examples of radical polymerization initiators used in the radical polymerization include peroxides such as hydrogen peroxide, ammonium persulfate, sodium persulfate, and potassium persulfate, and azo compounds such as 2,2-azobis(2-amidinopropane) dihydrochloride and 2,2-azobis(isobutyronitrile), and the type is not particularly limited as long as they decompose at the polymerization reaction temperature and generate radicals. These can also be used as redox initiators in combination with reducing substances such as sulfites and L-ascorbic acid, and further amines. In order to adjust the mass average molecular weight of the resulting polycarboxylic acid copolymer to a desired range, a chain transfer agent such as 2-mercaptoethanol, 2-mercaptopropionic acid, 3-mercaptopropionic acid, thioglycolic acid, thioglycerin, or thiomalic acid may be used. These radical polymerization initiators, reducing substances, and chain transfer agents may be used alone or in combination of two or more. In this embodiment, it is preferable to use the polycarboxylic acid copolymer that has been dried to form a powder.
[0037] In order to maintain fluidity and increase resistance to material separation, the content of the polycarboxylic acid-based copolymer is preferably 0.5% by mass or more and 2.0% by mass or less, and more preferably 1.0% by mass or more and 1.5% by mass or less, relative to the binder.
[0038] The mass ratio of the calcium carbonate to the polycarboxylic acid copolymer (calcium carbonate / polycarboxylic acid copolymer) is 1.0 or more and 14.0 or less, and from the viewpoint of enhancing the stability of fluidity, it is preferably 3.0 or more and 13.0 or less.
[0039] The cement composition according to the present embodiment may further contain other admixtures other than the polycarboxylic acid copolymer. Examples of other admixtures include AE agents, AE water reducing agents, high performance water reducing agents, fluidizing agents, separation reducing agents, setting retarders (e.g., tartaric acid, etc.), setting accelerators (e.g., aluminum sulfate, etc.), quick-setting agents, shrinkage reducing agents, thickeners, foaming agents, foaming agents, waterproofing agents, and defoamers. The admixtures may be used alone or in combination of two or more.
[0040] The content of the other admixtures may be, for example, 2.0% by mass or more and 30.0% by mass or less, or 5.0% by mass or more and 20.0% by mass or less, relative to the binder.
[0041] The cement composition according to the present embodiment may further contain an admixture. Examples of the admixture include inorganic fine powders such as anhydrous gypsum, hemihydrate gypsum, dihydrate gypsum, expanding material, quicklime fine powder, and dolomite fine powder, sodium bentonite, calcium bentonite, attapulgite, sepiolite, activated clay, acid clay, allophane, imogolite, shirasu (volcanic ash), shirasu balloon, kaolinite, metakaolin (calcined clay), synthetic zeolite, artificial zeolite, artificial zeolite, mordenite, and clinoptilolite. The admixture may be used alone or in combination of two or more kinds.
[0042] The content of the admixture may be, for example, 1.0% by mass or more and 20.0% by mass or less, or 5.0% by mass or more and 10.0% by mass or less, relative to the binder.
[0043] The cement composition according to this embodiment comprises a binder containing cement, calcium carbonate, and a water-reducing agent, the water-reducing agent comprising a polycarboxylic acid-based copolymer containing the structural unit (1) and the structural unit (2), and the mass ratio of the calcium carbonate to the polycarboxylic acid-based copolymer (calcium carbonate / polycarboxylic acid-based copolymer) is 1.0 or more and 14.0 or less, thereby making it possible to impart fluidity to mortar or concrete and improve its viscosity.
[0044] In the cement composition according to the present embodiment, the content of the calcium carbonate is 2.0 mass % or more and 20.0 mass % or less relative to the binder, thereby imparting fluidity to mortar or concrete and further improving viscosity.
[0045] <Mortar composition> The mortar composition according to the present embodiment will be described below. The mortar composition according to the present embodiment contains the above-mentioned cement composition and fine aggregate.
[0046] Fine aggregate refers to aggregate that passes entirely through a 10 mm mesh sieve and 85% or more by mass through a 5 mm mesh sieve (JIS A 0203:2014). Examples of fine aggregate include naturally occurring sand such as mountain sand, river sand, land sand, sea sand, crushed sand, and limestone crushed sand, as specified in JIS A 5308 Appendix A Aggregates for Ready Mixed Concrete, and sand derived from slag such as blast furnace slag, electric furnace oxidized slag, and ferro-nickel slag. These fine aggregates may be used alone or in combination of two or more types.
[0047] From the viewpoint of improving the filling property, the range of the particle size of the fine aggregate is preferably 0.053 mm or more and less than 10 mm, and more preferably 0.053 mm or more and less than 5.6 mm. The particle size of the fine aggregate is a value measured in accordance with JIS A 1102:2014.
[0048] From the viewpoint of improving resistance to shrinkage and strength development, the content of the fine aggregate is preferably 50.0% by mass or more and 80.0% by mass or less, and more preferably 60.0% by mass or more and 75.0% by mass or less, based on the entire mortar composition. When two or more types of fine aggregate are contained, the above content is the total content.
[0049] From the viewpoint of improving resistance to shrinkage and strength development, the content of the binder in the mortar composition according to this embodiment is preferably 20.0 mass % or more and 50.0 mass % or less, and more preferably 25.0 mass % or more and 40.0 mass % or less, based on the entire mortar composition.
[0050] The mortar composition according to the present embodiment can be suitably used as a repair material for concrete structures by adding water to the mortar composition. The water is not particularly limited, and for example, tap water, industrial water, recycled water, groundwater, river water, rainwater, etc. can be used. The amount of water added can be, for example, 5.0 parts by mass or more and 20.0 parts by mass or less with respect to 100 parts by mass of the mortar composition.
[0051] The mortar composition according to the present embodiment may be used as a repair material for concrete structures by adding the water and coarse aggregate to the mortar composition. The coarse aggregate is not particularly limited, and examples thereof include natural aggregates such as river gravel, mountain gravel, and sea gravel, artificial aggregates such as crushed stone such as sandstone, hard limestone, basalt, andesite, and recycled aggregates. The coarse aggregate may be used alone or in combination of two or more kinds.
[0052] The mortar composition according to the present embodiment contains the cement composition and fine aggregate, and thus can impart fluidity and improve viscosity to mortar or concrete.
[0053] <Method of repairing concrete structures> The concrete structure repair method according to this embodiment will be described below.
[0054] In the method for repairing a concrete structure according to the present embodiment, the mortar composition is used as a grout material. More specifically, the method for repairing a concrete structure includes, for example, arranging a formwork so as to surround a portion of the concrete structure from which a deteriorated portion has been removed, and filling the gap between the formwork and the concrete structure with the grout material, thereby repairing the concrete structure. In addition, the method for repairing a concrete structure includes, for example, applying the grout material to the portion from which the deteriorated portion has been removed, thereby repairing the concrete structure.
[0055] The method for producing the grout material is not particularly limited, and may be, for example, a method in which water or the like is added on-site to a powdered mortar composition (i.e., a premix) in which the components constituting the mortar composition are mixed in advance, and then kneaded, or a method in which the components constituting the mortar composition are mixed on-site, and then water or the like is added to the obtained powdered mixture, and then kneaded.
[0056] The method for repairing a concrete structure according to the present embodiment is excellent in workability by using a mortar composition as a grout material that can impart fluidity and improve viscosity. Specifically, the method is excellent in filling property, and when the grout material is filled into the gap between a formwork and a concrete structure, the occurrence of air pockets can be suppressed.
[0057] The present invention includes the following aspects. [1] A concrete structure comprising a binder containing cement, calcium carbonate, and a water-reducing agent; The water reducing agent contains a polycarboxylic acid copolymer containing the following structural unit (1) and the following structural unit (2), A cement composition, wherein a mass ratio of the calcium carbonate to the polycarboxylic acid copolymer (calcium carbonate / polycarboxylic acid copolymer) is 1.0 or more and 14.0 or less. Structural unit (1): A structural unit formed from one or more monomers selected from those represented by the following formula (1): Structural unit (2): A structural unit formed from one or more selected from (meth)acrylic acid and / or a salt thereof. [ka] (In formula (1), R 1 , R 2 and R 3 are the same or different, each represents a hydrogen atom or a methyl group, R 4 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 22 carbon atoms. p represents an integer of 0 to 5. q represents an integer of 0 or 1. A 1 O represents an oxyalkylene group having 2 to 4 carbon atoms. n is A 1 is the average number of moles of O added, and represents a number from 40 to 120.) [2] The cement composition according to [1], wherein the content of the calcium carbonate is 2.0% by mass or more and 20.0% by mass or less relative to the binder. [3] A mortar composition comprising the cement composition according to [1] or [2] and fine aggregate. [4] A method for repairing a concrete structure, comprising using the mortar composition according to [3] as a grout material. EXAMPLES
[0058] Examples of the present invention will be described below, but the present invention is not limited to the following examples.
[0059] Mortar compositions of each Example and Comparative Example were prepared by mixing the materials shown in Table 1 in the ratio shown in Table 1. 100 parts by mass of each prepared mortar composition was mixed with 9 parts by mass of water and kneaded for 180 seconds to prepare mortars of each Example and Comparative Example.
[0060] Details of each component shown in Table 1 are given below. Binder: Contains cement as the main component (85% by mass or more), as well as ground granulated blast furnace slag and fly ash Calcium carbonate (CaCO3): Manufactured by Omi Mining Co., Ltd. Fine aggregate: Mixed sand with a grain size range of 0.053 mm or more and less than 5.6 mm Water reducing agent (polycarboxylic acid type): Polycarboxylic acid copolymer (Takemoto Oil Co., Ltd.) Water reducing agent (naphthalene type): Paul Fine 510-AN, manufactured by Takemoto Oil Co., Ltd.
[0061] Details of the polycarboxylic acid copolymer used as a water reducing agent are shown in Table 2 and below. M-1: α-methacryloyl-ω-hydroxy-poly(n=43)oxyethylenepoly(m=2)oxypropylene (in M-1, R 1 and R 3 is a hydrogen atom, and R 2 is a methyl group, and R 4 is a hydrogen atom. p is 0 and q is 1. A 1 O is an oxyethylene group and an oxypropylene group. M-2: α-(3-methyl-3-butenyl)-ω-hydroxy-poly(n=50)oxyethylene (M-2, R 1 and R 3 is a hydrogen atom, and R 2 is a methyl group, and R 4 is a hydrogen atom. p is 1 and q is 0. A 1 O is an oxyethylene group. M-3: α-methacryloyl-ω-methoxy-poly(n=68)oxyethylene (M-3, R 1 and R 2 is a hydrogen atom, and R 3 is a methyl group, and R 4 is a methyl group. p is 0 and q is 1. A 1 O is an oxyethylene group. M-4: α-methacryloyl-ω-methoxy-poly(n=113)oxyethylene (in M-4, R 1 and R 3 is a hydrogen atom, and R 2 is a methyl group, and R 4 is a methyl group. p is 0 and q is 1. A 1 O is an oxyethylene group. M-5: α-methacryloyl-ω-methoxy-poly(n=150)oxyethylene (M-5, R 1 and R 3 is a hydrogen atom, and R 2 is a methyl group, and R 4 is a methyl group. p is 0 and q is 1. A 1 O is an oxyethylene group. C-1: Acrylic acid C-2: Methacrylic acid E-1: Hydroxyethyl acrylate E-2: Methyl acrylate
[0062] [Table 1]
[0063] [Table 2]
[0064] [Table 3]
[0065] <Slump flow measurement> For the mortars of each Example and Comparative Example, the slump flow was measured immediately after mixing (0 hr in Table 3) and one hour after mixing (1 hr in Table 3) based on JIS A 1150: 2020. The measured values are shown in Table 3.
[0066] <Measurement of 50cm flow arrival time> For the mortars of each Example and Comparative Example, the 50 cm flow time was measured immediately after mixing based on JIS A 1150: 2020. The measured values are shown in Table 3.
[0067] As can be seen from the results in Table 3, the mortars of the Examples satisfying all the constituent requirements of the present invention have a slump flow value of 720 to 830 mm immediately after mixing and a 50 cm flow time of 3.8 to 9.5 seconds, and are therefore superior in fluidity and viscosity compared to the mortars of the Comparative Examples. Thus, the cement compositions and mortar compositions of the Examples satisfying all the constituent requirements of the present invention can impart fluidity to mortar or concrete and improve its viscosity.
[0068] Moreover, the mortars of the examples which satisfy all of the constituent requirements of the present invention also had slump flow values of 670 to 800 mm one hour after mixing, which suggests that they are able to maintain their fluidity and viscosity.
Claims
1. The concrete comprises a binder containing cement, calcium carbonate, and a water reducing agent, The water reducing agent contains a polycarboxylic acid copolymer containing the following structural unit (1) and the following structural unit (2), A cement composition, wherein a mass ratio of the calcium carbonate to the polycarboxylic acid copolymer (calcium carbonate / polycarboxylic acid copolymer) is 1.0 or more and 14.0 or less. Structural unit (1): A structural unit formed from one or more monomers selected from those represented by the following formula (1): Structural unit (2): A structural unit formed from one or more selected from (meth)acrylic acid and / or a salt thereof. 【Chemistry 1】 (In formula (1), R 1 , R 2 and R 3 R represents a hydrogen atom or a methyl group, which may be the same or different. 4 are the same or different and represent a hydrogen atom or a hydrocarbon group having 1 to 22 carbon atoms. p represents an integer of 0 to 5. q represents an integer of 0 or 1. A 1 O represents an oxyalkylene group having 2 to 4 carbon atoms. n represents A 1 is the average number of moles of O added, and represents a number from 40 to 120.)
2. The cement composition according to claim 1, wherein the content of the calcium carbonate is 2.0 mass% or more and 20.0 mass% or less relative to the binder.
3. A mortar composition comprising the cement composition according to claim 1 or 2 and fine aggregate.
4. A method for repairing a concrete structure, comprising using the mortar composition according to claim 3 as a grout material.