Repair sheet for decorative material and repair method for decorative material
The decorative repair sheet with a thermoplastic resin and adhesive layer addresses alignment and construction issues, ensuring excellent workability and adhesion, maintaining design quality and preventing peeling.
Patent Information
- Application Number
- JP2023051984
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional decorative material repair sheets face issues with poor alignment to the adherend, followability to the shape of the adherend, and difficulty in construction, leading to a decline in design quality and adhesive strength.
A decorative repair sheet comprising a thermoplastic resin sheet with a design layer, a transparent resin layer, and an adhesive layer, designed to have an upper yield point load of 25N/10mm to 80N/10mm and adhesive strength of 40N/25mm or less, ensuring excellent workability and adhesion.
The sheet provides improved workability by maintaining design quality and preventing lifting and peeling, with enhanced followability to the shape of the adherend, allowing easy application and repositioning.
Smart Images

Figure 00000023_0000 
Figure 00000023_0001 
Figure 00000023_0002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a repair sheet for a decorative material and a method for repairing a decorative material. [Background technology]
[0002] Exterior decorative materials are durable consumer goods and are usually required to have a certain degree of durability, scratch resistance, and weather resistance. However, the design or function of the exterior decorative material may deteriorate due to long-term use, use in environments beyond the expected range, and other external factors. In response to this problem, repair sheets for decorative materials have been proposed (see, for example, Patent Documents 1 and 2). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2002-127291 A [Patent Document 2] JP 2000-094566 A Summary of the Invention [Problem to be solved by the invention]
[0004] A repair sheet for a decorative material usually comprises a base layer and a design layer provided on one side of the base layer. A form is known in which a pressure-sensitive adhesive layer is laminated in advance on the other side of the base layer to improve ease of application when attaching the repair sheet to an adherend (the decorative material to be repaired).
[0005] Conventional repair sheets for decorative materials have sufficient adhesive strength to prevent lifting and peeling from the adherend, but have problems in terms of workability such as alignment to the adherend, ability to follow the shape of the adherend, and reduced design during application. The object of the present disclosure is to provide a repair sheet for decorative materials with excellent workability. [Means for solving the problem]
[0006] The repair sheet for the decorative material of the present disclosure comprises a decorative sheet and an adhesive layer, the decorative sheet comprising a thermoplastic resin sheet as a base layer, a design layer, and a transparent resin layer, in that order, the adhesive layer being provided on the side of the base layer opposite the side facing the design layer, the repair sheet having an upper yield point load of 25 N / 10 mm or more and 80 N / 10 mm or less, measured in accordance with the test method of JIS K6732:1996, and the repair sheet has an adhesive strength of 40 N / 25 mm or less 24 hours after application to a SUS-BA plate, measured at a peel angle of 180° and a peel speed of 300 mm / min in accordance with Method 1 of the test method of JIS Z0237:2022. Effect of the Invention
[0007] According to the present disclosure, a repair sheet for decorative materials having excellent workability can be provided. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a repair sheet for a decorative material. [Diagram 2] FIG. 2 is a schematic cross-sectional view showing one embodiment of a repair sheet for a decorative material. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing one embodiment of a decorative material to be repaired. [Figure 4] FIG. 4 is a schematic cross-sectional view showing one embodiment of a repaired decorative material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] In this specification, when multiple upper limit candidates and multiple lower limit candidates are given for a certain parameter, the numerical range of the parameter may be configured by combining any one of the upper limit candidates and any one of the lower limit candidates. As an example, the description "parameter B is preferably A1 or more, more preferably A2 or more, even more preferably A3 or more, and also preferably A4 or less, more preferably A5 or less, and even more preferably A6 or less." will be explained. In this example, the numerical range of parameter B may be A1 or more and A4 or less, A1 or more and A5 or less, A1 or more and A6 or less, A2 or more and A4 or less, A2 or more and A5 or less, A2 or more and A6 or less, A3 or more and A4 or less, A3 or more and A5 or less, or A3 or more and A6 or less.
[0010] Hereinafter, the embodiments of the present disclosure will be described in detail. The present disclosure can be implemented in many different forms, and is not to be interpreted as being limited to the description of the embodiments exemplified below. In the drawings, the width, thickness, shape, etc. of each layer may be shown diagrammatically in order to make the explanation clearer, but these are merely examples and do not limit the interpretation of the present disclosure. In this specification and each figure, elements similar to those already explained with respect to the previous figures may be given the same reference numerals, and detailed explanations may be omitted as appropriate.
[0011] Films and sheets may be referred to as films and sheets in the order of relatively thinnest thickness. However, in this specification, unless otherwise specified, sheets include films. In this specification, the terms front and back may be used, but the distinction between front and back has no technical meaning, and when one side of a sheet is the front side, the other side is the back side.
[0012] In the following description, each component (e.g., resin components such as polyolefins, adhesives, UV absorbers, light stabilizers, colorants, and additives) may be used either alone or in combination, unless otherwise specified.
[0013] [Repair sheet for decorative materials] The repair sheet for a decorative material of the present disclosure comprises a decorative sheet and a pressure-sensitive adhesive layer. The decorative sheet comprises a thermoplastic resin sheet as a base layer, a design layer, and a transparent resin layer in this order in the thickness direction (hereinafter referred to as "in this order"). The decorative sheet may comprise a transparent adhesive layer between the design layer and the transparent resin layer. The decorative sheet may comprise a surface protective layer as one surface layer of the sheet. The decorative sheet may comprise a primer layer between the transparent resin layer and the surface protective layer. The decorative sheet may comprise a back primer layer as the other surface layer of the sheet. In one embodiment, the decorative sheet is a highly weather resistant decorative sheet intended for outdoor use.
[0014] In one embodiment, the decorative sheet comprises, in this order, a back primer layer, a base layer, a design layer, a transparent adhesive layer, a transparent resin layer, a primer layer, and a surface protective layer.
[0015] The upper yield point load of the repair sheet is 25N / 10mm or more and 80N / 10mm or less. The upper yield point load of the repair sheet is preferably 26N / 10mm or more, more preferably 28N / 10mm or more, and even more preferably 30N / 10mm or more. The upper yield point load of the repair sheet is preferably 70N / 10mm or less, more preferably 65N / 10mm or less, and even more preferably 60N / 10mm or less, for example, 50N / 10mm or less, or 40N / 10mm or less. A repair sheet having an upper yield point load of the lower limit or more can suppress a decrease in design (for example, a design in which the design layer and the unevenness of the transparent resin layer are in harmony) because the sheet does not deform too much when the sheet is attached to the shape of the adherend, for example, when the sheet is attached to a corner of the adherend, or when the sheet is reattached. A repair sheet with an upper yield point load equal to or less than the upper limit has excellent conformability to the shape of the adherend, and for example, when the sheet is attached to a corner of an adherend, it has excellent conformability to the corner and can suppress deterioration of the appearance such as wrinkles, lifting, peeling, air bubbles, etc. The upper yield point load can be adjusted, for example, by setting the hardness of the resin constituting each layer of the repair sheet and the thickness of each layer.
[0016] The upper yield point load (N / 10mm) of the repair sheet is defined as the tensile yield point load (N / 10mm) for a 10mm wide test piece measured in accordance with the test method of JIS K6732:1996. The tensile yield point load is measured as follows. (1) Prepare a dumbbell-shaped test piece by punching out the repair sheet into the shape and dimensions shown in "Figure 3" of JIS K6732:1996. If the repair sheet has a release layer, peel off the release layer from the repair sheet or test piece. (2) In accordance with "9.3 Tensile test" of JIS K6732:1996, a tension-compression tester is used to pull the test piece at a temperature of 23°C and a tensile speed of 200 mm / min, a load-elongation curve is created, and the tensile yield load is calculated. The load-elongation curve is a curve in which a tensile load is applied to a test piece held at both ends at a constant speed, the elongation of the test piece is plotted on the horizontal axis and the tensile load on the vertical axis, and the tensile load at each elongation is plotted. The tensile yield load is the first load at which an increase in elongation occurs without an increase in tensile load (however, it may be smaller than the maximum load). The upper yield load is the load at which the test piece yields. (3) In this disclosure, when the longitudinal direction (machine direction, MD) and transverse direction (width direction, TD) of the repair sheet can be distinguished, the tensile yield point load in MD is adopted as the upper yield point load. That is, a dumbbell-shaped test piece is prepared so that the long axis direction of the dumbbell-shaped test piece is aligned with the MD of the repair sheet, and the tensile yield point load is measured. In this disclosure, when the MD and TD of the repair sheet cannot be distinguished, a dumbbell-shaped test piece is prepared so that the long axis direction of the dumbbell-shaped test piece is aligned with each side of the repair sheet, that is, two test pieces are prepared, and the tensile yield point load is measured for each test piece. The average value of the two measured values obtained is adopted as the upper yield point load.
[0017] The repair sheet includes a decorative sheet and an adhesive layer, with the adhesive layer, base layer, design layer, and transparent resin layer in this order. In one embodiment, the repair sheet includes an adhesive layer, a back primer layer, a base layer, a design layer, a transparent adhesive layer, a transparent resin layer, a primer layer, and a surface protective layer in this order. The surface of the decorative sheet in the repair sheet, for example the surface of the surface protective layer in the decorative sheet, is the observation surface.
[0018] The adhesive strength of the repair sheet 24 hours after application to the SUS-BA plate is 40N / 25mm or less, preferably 38N / 25mm or less, more preferably 36N / 25mm or less. The adhesive strength of the repair sheet to the SUS-BA plate is preferably 1N / 25mm or more, more preferably 5N / 25mm or more, even more preferably 10N / 25mm or more, even more preferably 15N / 25mm or more, particularly preferably 20N / 25mm or more, and particularly preferably 25N / 25mm or more. A repair sheet having an adhesive strength of the upper limit or less has good alignment (re-application) with respect to the adherend, and can suppress the deterioration of the design (for example, the design of the design layer and the unevenness of the transparent resin layer) when re-application. Even if the adhesive strength is low, if the upper yield point load is the above-mentioned value or less, the occurrence of lifting and peeling of the sheet from the adherend can be suppressed. A repair sheet with an adhesive strength equal to or greater than the lower limit has better adhesion to the adherend and can better prevent the sheet from lifting or peeling off from the adherend. The adhesive strength can be adjusted, for example, by setting the type, specific gravity, and thickness of the adhesive layer, as well as the hardness of the resin that constitutes the decorative sheet and the thickness of each layer.
[0019] The adhesive strength is measured as follows. A test piece of the repair sheet with a width of 25 mm and a length of 100 mm is pressed against the adherend (SUS-BA plate) with a 2 kg roller going back and forth once so that the exposed adhesive layer is in contact with the adherend, and left to stand for 24 hours under an environment of a temperature of 23°C and a humidity of 50%RH. After standing, the adhesive strength to the SUS-BA plate is measured by peeling the test piece in the length direction using a tensile tester under the conditions of a width of 25 mm, a peel angle of 180°, and a peel speed of 300 mm / min, in accordance with the test method 1 (temperature 23°C, humidity 50%RH, tape and sheet peeled off at 180° against a stainless steel test plate) of JIS Z0237:2022 (Adhesive tape and adhesive sheet test method). The SUS plate used is a SUS304, surface finish BA, SUS plate with a thickness of 1.5 mm, width 100 mm, and length 150 mm.
[0020] The repair target of the decorative material repair sheet of the present disclosure, i.e., the decorative material (adherend), is not limited to SUS-BA plate; however, when the adhesive strength to SUS-BA plate is within the above-mentioned range, the same tendency will be shown, for example, in terms of alignment ability (repositionability) and lifting / peeling, even for adherends other than SUS-BA plate.
[0021] The decorative material repair sheet of the present disclosure having such physical properties suppresses the deterioration of design during application and the occurrence of lifting and peeling from the adherend after application, while being excellent in repositionability (repositionability) on the adherend and conformability to the shape of the adherend (e.g. conformability to corners). For example, by applying the decorative material repair sheet to the surface or corner of the part of the decorative material to be repaired using fingers, the decorative material can be easily repaired.
[0022] FIG. 1 shows a schematic cross-sectional view of one embodiment of a repair sheet for a decorative material of the present disclosure. The repair sheet 1 includes a decorative sheet 2 and an adhesive layer 3. The decorative sheet 2 includes a base layer 10 including a first surface 11 and a second surface 12 facing the first surface 11, a design layer 20 provided on the first surface 11 of the base layer 10, and a transparent resin layer 30 provided on the design layer 20, in this order. That is, the base layer 10, the design layer 20, and the transparent resin layer 30 are stacked in the thickness direction, which is the vertical direction on the paper surface of FIG. 1. The adhesive layer 3 is provided on the second surface 12 of the base layer 10. A release layer (not shown) may be provided on the surface of the adhesive layer 3 opposite to the surface facing the base layer 10. 2 shows a schematic cross-sectional view of one embodiment of a repair sheet for a decorative material according to the present disclosure. The decorative sheet 2 of the repair sheet 1 includes, in this order, a back primer layer 60, a base layer 10, a design layer 20, a transparent adhesive layer 26, a transparent resin layer 30, a primer layer 40, and a surface protective layer 50. A release layer (not shown) may be provided on the surface of the pressure-sensitive adhesive layer 3 opposite to the surface facing the back primer layer 60.
[0023] The decorative sheet may have unevenness formed by embossing or the like on one surface (for example, the surface protective layer). Such a decorative sheet has excellent designability compared to a design only of a pattern related to the design layer, due to the addition of a visual unevenness or a tactile unevenness. In this case, it is preferable to harmonize the pattern of the design layer with the unevenness caused by the unevenness processing, since this further improves the designability. For example, the sheet can be embossed by heating the sheet to preferably 80°C or higher, more preferably 100°C or higher, even more preferably 120°C or higher, and preferably 260°C or lower, more preferably 220°C or lower, and even more preferably 200°C or lower. The sheet is preferably pressed with an embossing plate, for example, on the surface protective layer of the decorative sheet.
[0024] <Base material layer> The decorative sheet includes a substrate layer. The substrate layer is a layer that serves as the base of the decorative sheet, and is a layer that performs functions such as providing the strength of the decorative sheet and serving as a target for forming the design layer.
[0025] The substrate layer is, for example, a thermoplastic resin sheet. The substrate layer may be a single layer or a multilayer. The substrate layer may be a laminate of thermoplastic resin sheets. Each layer in the laminate may be laminated via a known material such as an adhesive or a heat-sealing resin.
[0026] The thermoplastic resin sheet is a sheet made of a thermoplastic resin. Examples of the thermoplastic resin include polyolefin, polyvinyl chloride, polystyrene, polyester, polyamide, polycarbonate, and acrylic resin. Among these, polyolefin is preferred. Examples of the polyolefin include polyethylene such as high density polyethylene, medium density polyethylene, low density polyethylene, and linear low density polyethylene, polypropylene such as isotactic polypropylene and syndiotactic polypropylene, polybutene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, and olefin-based thermoplastic elastomer. Examples of the polyester include polyethylene terephthalate and polybutylene terephthalate.
[0027] The thermoplastic resin sheet may be colorless and transparent, colored and transparent, colored and semi-transparent, or colored and opaque. The thermoplastic resin sheet may be colored for the purpose of improving the design.
[0028] Among thermoplastic resin sheets, polyolefin sheets are preferred, colored or uncolored polyethylene or polypropylene sheets are more preferred, and polypropylene sheets are even more preferred. From the viewpoint of processability, the content of polyolefin in the polyolefin sheet is preferably 50% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 80% by mass or more, based on the total resin components of the polyolefin sheet.
[0029] The substrate layer may contain additives. Examples of additives include ultraviolet absorbers, light stabilizers, antioxidants, wear resistance improvers, infrared absorbers, antistatic agents, fillers, foaming agents, flame retardants, plasticizers, antisettling agents, lubricants, and colorants. The substrate layer may contain weathering agents such as ultraviolet absorbers, light stabilizers, and antioxidants in order to improve weather resistance. Examples of ultraviolet absorbers include benzotriazole-based ultraviolet absorbers, benzophenone-based ultraviolet absorbers, triazine-based ultraviolet absorbers, and hydroxyphenyltriazine-based ultraviolet absorbers. Examples of light stabilizers include hindered amine-based light stabilizers such as piperidinyl sebacate-based light stabilizers.
[0030] The substrate layer may contain colorants such as dyes and pigments. For example, when the surface hue of the adherend to which the repair sheet is attached varies, in order to conceal the surface hue and improve the stability of the color tone of the design layer, the substrate layer may contain a colorant. Examples of pigments include white pigments such as zinc oxide, white lead, lithopone, titanium dioxide, precipitated barium sulfate, and baryte; black pigments such as carbon black; red pigments such as red lead and red iron oxide; yellow pigments such as yellow lead and zinc yellow (zinc yellow type 1, zinc yellow type 2); and blue pigments such as ultramarine blue and Prussian blue (potassium ferrocyanide). The content of the colorant is preferably 1 part by mass or more, more preferably 3 parts by mass or more, and even more preferably 5 parts by mass or more, and is preferably 50 parts by mass or less, more preferably 40 parts by mass or less, and even more preferably 30 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin contained in the substrate layer.
[0031] From the viewpoint of a balance between design and processability, the thickness of the base layer is preferably 20 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, and even more preferably 50 μm or more, and is preferably 500 μm or less, more preferably 400 μm or less, even more preferably 300 μm or less, and even more preferably 200 μm or less.
[0032] One or both sides of the substrate layer may be subjected to a surface treatment. Examples of the surface treatment include physical surface treatments such as oxidation and roughening, and chemical surface treatments. Examples of the oxidation method include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, and ozone-ultraviolet treatment. Examples of the roughening method include sandblasting and solvent treatment.
[0033] <Design layer> The decorative sheet includes a design layer. The design layer is provided, for example, on a substrate layer. In other words, in this embodiment, the decorative sheet includes a substrate layer and a design layer stacked in the thickness direction. The substrate layer and the design layer may be in contact with each other, or another layer may be present between the substrate layer and the design layer.
[0034] The design layer is provided to display the design expressed by the decorative sheet. The design layer has, for example, a pattern. Examples of patterns include wood grain patterns imitating annual rings or vessel grooves on the surface of a wooden board, stone grain patterns imitating the surface of rocks such as marble and granite, fabric patterns imitating cloth grain or cloth-like patterns, leather grain patterns imitating leather surfaces, pear-skin patterns, tile patterns, brickwork patterns, geometric patterns, and abstract patterns such as letters, figures, symbols, polka dots, and floral patterns. The pattern may be a single solid color (so-called solid image). The pattern may be a composite pattern including two or more of these. The pattern of the design layer may be, for example, the same or similar to the pattern of the decorative material to be repaired, or may be a pattern in the same color tone as the pattern of the decorative material to be repaired. The design layer may have two or more layers. For example, the design layer may have a colored first layer and a second layer provided on the first layer to form a design.
[0035] The design layer can be formed, for example, by a printing method or a coating method. Examples of the printing method include gravure printing, offset printing, silk screen printing, printing by transfer from a transfer sheet, and inkjet printing. Examples of the coating method include gravure coating, gravure reverse coating, gravure offset coating, spinner coating, roll coating, and reverse roll coating. Each layer described below can also be formed, for example, by these methods.
[0036] The design layer contains, for example, a resin component and a colorant. Examples of the resin component include vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-(meth)acrylic copolymer, chlorinated polyethylene, chlorinated polypropylene, urethane-(meth)acrylic copolymer, acrylic resin, acrylic polyol resin, polystyrene, polyurethane, polyester, polyamide, butyral resin, nitrocellulose, and cellulose acetate.
[0037] Examples of colorants include pigments and dyes.Specific examples of colorants include inorganic pigments such as carbon black, iron black, titanium white, antimony white, yellow lead, titanium yellow, red iron oxide, cadmium red, ultramarine blue, and cobalt blue; organic pigments or dyes such as quinacridone red, isoindolinone yellow, phthalocyanine blue, azomethine azo black, and nickel azo complex; metal pigments made of scaly flakes such as aluminum and brass; and pearlescent pigments made of scaly flakes such as titanium dioxide-coated mica and basic lead carbonate.
[0038] The content of colorant in the design layer is preferably 5 parts by mass or more, more preferably 15 parts by mass or more, and even more preferably 30 parts by mass or more, per 100 parts by mass of the resin component contained in the design layer, and is preferably 200 parts by mass or less, more preferably 150 parts by mass or less, and even more preferably 100 parts by mass or less.
[0039] The decorative layer may contain the above-mentioned additives. From the viewpoint of improving weather resistance, the decorative layer may contain weather resistance agents such as ultraviolet absorbers, light stabilizers, and antioxidants.
[0040] The thickness of the design layer is preferably 0.5 μm or more, more preferably 1 μm or more, and even more preferably 1.5 μm or more, and is preferably 20 μm or less, more preferably 15 μm or less, and even more preferably 10 μm or less. A decorative sheet having such a design layer has excellent design properties.
[0041] The design layer may have a metal thin film. Examples of metals constituting the metal thin film include tin, indium, chromium, aluminum, nickel, iron, cobalt, copper, silver, gold, platinum, and zinc, as well as alloys containing at least one selected from these metals. Examples of alloys include brass, bronze, and stainless steel. Examples of methods for forming the metal thin film include vacuum deposition, sputtering, and ion plating. The thickness of the metal thin film is, for example, 0.1 μm or more and 1 μm or less.
[0042] <Transparent adhesive layer> The decorative sheet may have a transparent adhesive layer between the design layer and the transparent resin layer in order to improve the adhesion between the two layers. The transparent adhesive layer may be transparent enough to allow the substrate layer side to be visually recognized through the transparent adhesive layer, and may be colorless and transparent, colored, transparent, or translucent.
[0043] The transparent adhesive layer is, for example, composed of a transparent adhesive. Examples of adhesives include urethane resin adhesives, acrylic resin adhesives, epoxy resin adhesives, and rubber adhesives. Among these, urethane resin adhesives are preferred from the viewpoint of adhesive strength. Examples of urethane resin adhesives include two-liquid curing urethane resin adhesives, and specifically, adhesives using two-liquid curing urethane resins containing various polyol compounds such as polyether polyols, polyester polyols, and (meth)acrylic polyols, and curing agents such as various isocyanate compounds such as tolylene diisocyanate and hexamethylene diisocyanate. The transparent adhesive layer may contain the above-mentioned additives.
[0044] The thickness of the transparent adhesive layer is preferably 0.1 μm or more, more preferably 1 μm or more, even more preferably 1.5 μm or more, and is preferably 20 μm or less, more preferably 15 μm or less, even more preferably 10 μm or less.
[0045] <Transparent resin layer> The decorative sheet includes a transparent resin layer. By providing the transparent resin layer, for example, the upper yield point load of the repair sheet can be increased. The transparent resin layer is, for example, located between the design layer and the surface protective layer.
[0046] The transparent resin layer contains, for example, a transparent thermoplastic resin. Examples of the thermoplastic resin include polyolefin, polyvinyl chloride, polystyrene, polyester, polyamide, polycarbonate, and acrylic resin. Examples of the polyolefin include polyethylene such as high density polyethylene, medium density polyethylene, low density polyethylene, and linear low density polyethylene, polypropylene such as isotactic polypropylene and syndiotactic polypropylene, polybutene, ethylene-propylene copolymer, ethylene-propylene-butene copolymer, and olefin-based thermoplastic elastomer. Examples of the polyester include polyethylene terephthalate and polybutylene terephthalate. Among these, polyolefin and polyvinyl chloride are preferred, polyethylene, polypropylene, and polyvinyl chloride are more preferred, and polypropylene and polyvinyl chloride are even more preferred, from the viewpoint of easily adjusting the upper yield point load to the above-mentioned range. In one embodiment, the polyolefin contained in the transparent resin layer and the polyolefin contained in the base layer may be the same or different. From the viewpoint of processability, the content of polyolefin or polyvinyl chloride in the transparent resin layer is preferably 50 mass% or more, more preferably 60 mass% or more, even more preferably 70 mass% or more, and particularly preferably 80 mass% or more, based on the total resin components of the transparent resin layer.
[0047] The transparent resin layer may contain the above-mentioned additives. The transparent resin layer may contain weathering agents such as ultraviolet absorbers, light stabilizers and antioxidants to improve the weather resistance of the decorative sheet. In one embodiment, the content of the ultraviolet absorber in the transparent resin layer is preferably 0.05 parts by mass or more, more preferably 0.10 parts by mass or more, and preferably 10 parts by mass or less, more preferably 5 parts by mass or less, relative to 100 parts by mass of the polyolefin contained in the transparent resin layer. In one embodiment, the content of the light stabilizer in the transparent resin layer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, relative to 100 parts by mass of the polyolefin contained in the transparent resin layer.
[0048] The transparent resin layer may be transparent to such an extent that the substrate layer side can be visually confirmed through the transparent resin layer, and may be colorless transparent, colored transparent or translucent.
[0049] The transparent resin layer may have irregularities that are in harmony with the design layer. This can impart a three-dimensional feel to the decorative sheet. When the design layer pattern and the irregularities of the transparent resin layer are in harmony or in harmony with each other, it is possible to express, for example, a sense of luxury. For example, when the design layer has a wood grain pattern and the transparent resin layer has irregularities in a shape that is in harmony with the wood grain pattern, the design of the wood grain becomes more natural and three-dimensional. The irregularities can be formed, for example, by applying embossing pressure to the surface of the transparent resin layer.
[0050] The thickness of the transparent resin layer is preferably 20 μm or more, more preferably 30 μm or more, even more preferably 40 μm or more, even more preferably 50 μm or more, and is preferably 400 μm or less, more preferably 300 μm or less, even more preferably 200 μm or less, and even more preferably 150 μm or less, from the viewpoint of balance between scratch resistance, processing suitability, and weather resistance. By increasing the thickness of the transparent resin layer, for example, the upper yield point load of the repair sheet can be increased. The thickness of the transparent resin layer is preferably larger than the thickness of the substrate layer from the viewpoint of protecting the design layer and obtaining excellent scratch resistance.
[0051] <Primer layer> The decorative sheet may have a primer layer between the transparent resin layer and the surface protective layer. The primer layer is provided as necessary for the purpose of improving the adhesion between the transparent resin layer and the surface protective layer.
[0052] In one embodiment, the primer layer contains a resin component. Examples of the resin component include vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-(meth)acrylic copolymer, chlorinated polyethylene, chlorinated polypropylene, urethane-(meth)acrylic copolymer, acrylic resin, acrylic polyol resin, polystyrene, polyurethane, polyester, polyamide, butyral resin, nitrocellulose, and cellulose acetate. The resin component may be a crosslinked cured product of these resins using a curing agent. The resin component may be, for example, a cured product of a two-component curing type urethane resin described later.
[0053] The primer layer may contain the above-mentioned additives. The primer layer may contain weathering agents such as ultraviolet absorbers, light stabilizers, and antioxidants from the viewpoint of improving weather resistance. When the primer layer contains an ultraviolet absorber, the content of the ultraviolet absorber in the primer layer is preferably 1 part by mass or more, more preferably 5 parts by mass or more, and preferably 40 parts by mass or less, more preferably 30 parts by mass or less, relative to 100 parts by mass of the resin component contained in the primer layer. When the primer layer contains a light stabilizer, the content of the light stabilizer in the primer layer is preferably 0.1 parts by mass or more, more preferably 0.5 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, relative to 100 parts by mass of the resin component contained in the primer layer.
[0054] The thickness of the primer layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 1 μm or more, and is preferably 10 μm or less, more preferably 8 μm or less, and even more preferably 6 μm or less.
[0055] <Surface protective layer> The decorative sheet may include a surface protective layer. The surface protective layer is provided, for example, on the transparent resin layer. In other words, the surface protective layer is superposed on the transparent resin layer in the thickness direction. In one embodiment, the surface protective layer is provided on the entire surface of the transparent resin layer. In one embodiment, the surface protective layer constitutes one of the surface layers of the decorative sheet. A decorative sheet including a surface protective layer has excellent heat resistance, scratch resistance, abrasion resistance, and contamination resistance.
[0056] In order to allow the design of the design layer to be clearly visible from the observation surface (surface protective layer) side of the repair sheet, the surface protective layer is preferably colorless and transparent. However, the present invention is not limited thereto, and the surface protective layer may be colored and transparent or translucent.
[0057] The surface protective layer contains a cured resin. The cured resin functions as, for example, a binder in the surface protective layer. Examples of the cured resin include a cured product of a curable compound. Examples of the cured product of a curable compound include a cured product of an ionizing radiation curable compound and a cured product of a thermosetting resin. The surface protective layer may contain two or more of these cured resins.
[0058] Examples of the thermosetting resin include unsaturated group-containing (meth)acrylic resins, unsaturated polyesters, urethane resins, epoxy resins, phenolic resins, aminoalkyd resins, urea resins, melamine resins, melamine-urea co-condensation resins, guanamine resins, diallyl phthalate resins, and silicone resins.
[0059] A curing agent is used together with the thermosetting resin as necessary. In the case of unsaturated group-containing (meth)acrylic resin and unsaturated polyester, for example, a peroxide such as methyl ethyl ketone peroxide or a radical initiator such as azoisobutylnitrile is used. In the case of urethane resin, for example, an isocyanate-based curing agent is used. In the case of epoxy resin, for example, an organic amine-based curing agent is used.
[0060] Examples of the thermosetting resin include two-liquid curing urethane resins that use polyol as a base and an isocyanate compound as a curing agent. Examples of the polyol include (meth)acrylic polyol, polyether polyol, polyester polyol, polyethylene glycol, and polypropylene glycol. The isocyanate compound is a polyvalent isocyanate having two or more isocyanate groups, and examples of the isocyanate compound include aromatic isocyanates such as 4,4-diphenylmethane diisocyanate; and aliphatic (or alicyclic) isocyanates such as hexamethylene diisocyanate, isophorone diisocyanate, hydrogenated tolylene diisocyanate, and hydrogenated diphenylmethane diisocyanate.
[0061] In one embodiment, the surface protective layer contains a cured product of a thermosetting resin as a cured resin, for example, a crosslinked cured product of a (meth)acrylic polyol with an isocyanate-based curing agent.
[0062] The ionizing radiation curable compound means a compound that crosslinks and cures by irradiation with ionizing radiation, and has an ionizing radiation curable functional group. The ionizing radiation curable functional group is a group that crosslinks by irradiation with ionizing radiation, and examples thereof include functional groups (ethylenically unsaturated groups) having an ethylenic double bond, such as (meth)acryloyl group, vinyl group, and allyl group. The ionizing radiation means electromagnetic waves or charged particle beams that have an energy quantum capable of polymerizing or crosslinking molecules. Examples of the ionizing radiation include electron beams (EB) and ultraviolet rays (UV), and also include electromagnetic waves such as X-rays and gamma rays; and charged particle beams such as alpha rays and ion beams. From the viewpoint of incorporating an ultraviolet absorbing agent into the surface protective layer, the ionizing radiation is preferably an electron beam.
[0063] Examples of the ionizing radiation curable compound include polymerizable monomers and polymerizable oligomers that have been conventionally used as ionizing radiation curable compounds. The polymerizable monomer is preferably a (meth)acrylate monomer having a (meth)acryloyl group in the molecule, more preferably a polyfunctional (meth)acrylate monomer having two or more (meth)acryloyl groups in the molecule. The number of (meth)acryloyl groups in the polyfunctional (meth)acrylate monomer is 2 or more, preferably 8 or less, more preferably 6 or less.
[0064] Examples of the polymerizable monomer include bifunctional (meth)acrylates such as ethylene glycol di(meth)acrylate, propylene glycol di(meth)acrylate, 1,4-butanediol di(meth)acrylate, 1,6-hexanediol di(meth)acrylate, bisphenol A tetraethoxy di(meth)acrylate, and bisphenol A tetrapropoxy di(meth)acrylate; trimethylolpropane tri(meth)acrylate, pentaerythritol tri(meth)acrylate, pentaerythritol tri(meth)acrylate, tri- or higher functional (meth)acrylates such as dipentaerythritol tetra(meth)acrylate, dipentaerythritol tri(meth)acrylate, dipentaerythritol tetra(meth)acrylate, dipentaerythritol penta(meth)acrylate, and dipentaerythritol hexa(meth)acrylate; and ethylene oxide-modified, propylene oxide-modified, caprolactone-modified, isocyanuric acid-modified, or propionic acid-modified products of these (meth)acrylates.
[0065] Examples of the polymerizable oligomer include (meth)acrylate oligomers having two or more (meth)acryloyl groups in the molecule. Examples of the (meth)acrylate oligomer include urethane (meth)acrylate, epoxy (meth)acrylate, polyester (meth)acrylate, polyether (meth)acrylate, polycarbonate (meth)acrylate, polycaprolactone urethane (meth)acrylate, polycaprolactone diol urethane (meth)acrylate, and acrylic (meth)acrylate. The number of (meth)acryloyl groups in the polymerizable oligomer is 2 or more, preferably 8 or less, more preferably 6 or less.
[0066] Other examples of the polymerizable oligomer include highly hydrophobic polybutadiene (meth)acrylate oligomers having (meth)acryloyl groups in the side chains of polybutadiene oligomers, and silicone (meth)acrylate oligomers having polysiloxane bonds in the main chains.
[0067] The weight average molecular weight of the polymerizable oligomer is preferably 500 or more, more preferably 1,000 or more, and even more preferably 2,000 or more, and is preferably 10,000 or less, more preferably 8,000 or less, and even more preferably 6,000 or less. The weight average molecular weight is an average molecular weight measured by gel permeation chromatography (GPC) analysis and converted into standard polystyrene.
[0068] As the ionizing radiation curable compound, a monofunctional (meth)acrylate may be appropriately used in combination with the polyfunctional (meth)acrylate for the purpose of reducing the viscosity of the curable composition during coating, etc. Examples of the monofunctional (meth)acrylate include methyl (meth)acrylate, ethyl (meth)acrylate, propyl (meth)acrylate, butyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, cyclohexyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, lauryl (meth)acrylate, stearyl (meth)acrylate, and isobornyl (meth)acrylate.
[0069] When the ionizing radiation curable compound is an ultraviolet ray curable compound, it is preferable to use at least one selected from a photopolymerization initiator and a photopolymerization accelerator together with the ultraviolet ray curable compound.
[0070] From the viewpoint of excellent heat resistance, scratch resistance, and contamination resistance, the surface protective layer preferably contains a cured product of a curable compound, and more preferably contains a cured product of an ionizing radiation curable compound. Among ionizing radiation curable compounds, electron beam curable compounds are preferred as components for forming the surface protective layer, since they can be made solvent-free, do not require a photopolymerization initiator, and provide stable curing properties. Among ionizing radiation curable compounds, polymerizable oligomers are preferred, (meth)acrylate oligomers having two or more (meth)acryloyl groups in the molecule are more preferred, and urethane (meth)acrylates are even more preferred. It is even more preferred that the surface protective layer contains a cured product of a urethane (meth)acrylate-based electron beam curable compound.
[0071] The content of the cured resin relative to all resin components contained in the surface protective layer is preferably 50% by mass or more, more preferably 70% by mass or more, further preferably 80% by mass or more, and particularly preferably 90% by mass or more.
[0072] The surface protective layer may contain a thermoplastic resin within a range that does not inhibit the curing of the ionizing radiation curable resin by irradiation with ionizing radiation. Examples of the thermoplastic resin include acrylic resin, polyester resin, vinyl chloride resin, urethane resin, polyolefin resin, and styrene resin.
[0073] The surface protective layer may contain additives, such as weathering agents such as ultraviolet absorbers, light stabilizers, and antioxidants, wear resistance improvers, infrared absorbers, antistatic agents, leveling agents, thixotropy agents, coupling agents, defoamers, flame retardants, plasticizers, particles, and antiblocking agents. From the viewpoint of weather resistance, the surface protective layer may contain weathering agents such as ultraviolet absorbers, light stabilizers, and antioxidants.
[0074] From the viewpoint of weather resistance, the surface protective layer may contain an ultraviolet absorbing agent. Examples of ultraviolet absorbers include triazine-based ultraviolet absorbers, benzotriazole-based ultraviolet absorbers, and benzophenone-based ultraviolet absorbers. Triazine-based ultraviolet absorbers are preferred because they have excellent weather resistance. Among triazine-based ultraviolet absorbers, hydroxyphenyltriazine-based ultraviolet absorbers are preferred from the viewpoint of weather resistance. Among triazine-based ultraviolet absorbers, hydroxyphenyltriazine-based ultraviolet absorbers in which at least one organic group selected from hydroxyphenyl groups, alkoxyphenyl groups, and organic groups containing these groups are linked to a triazine ring are more preferred. Hydroxyphenyltriazine-based ultraviolet absorbers have a branched structure, so they are expected to be less likely to bleed out from the surface protective layer, and excellent weather resistance can be obtained over a longer period of time. In addition, ultraviolet absorbers having an ethylenic double bond such as a (meth)acryloyl group, a vinyl group, or an allyl group are preferred because they are easy to suppress bleed out.
[0075] In the surface protective layer, the content of the ultraviolet absorber relative to 100 parts by mass of the cured resin is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 2 parts by mass or more, and preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less. When the content of the ultraviolet absorber is equal to or more than the lower limit, the weather resistance of the decorative sheet tends to be improved. When the content of the ultraviolet absorber is equal to or less than the upper limit, the bleeding out of the ultraviolet absorber tends to be suppressed.
[0076] From the viewpoint of weather resistance, the surface protective layer may contain a light stabilizer. Examples of the light stabilizer include aromatic light stabilizers, amine light stabilizers, organic acid light stabilizers, catechin light stabilizers, and hindered amine light stabilizers, and among these, hindered amine light stabilizers are preferred. The hindered amine light stabilizer is, for example, a compound having a structure containing a 2,2,6,6-tetramethylpiperidine skeleton in the molecule.
[0077] Examples of the light stabilizer include a reactive light stabilizer having an ethylenic double bond that can be polymerized with a curable compound that can form the cured resin of the surface protective layer, and a non-reactive light stabilizer that does not have an ethylenic double bond that can be polymerized with the curable compound.The ethylenic double bond is, for example, possessed by a functional group such as a (meth)acryloyl group, a vinyl group, and an allyl group.The surface protective layer may contain at least one selected from a reactive light stabilizer and a non-reactive light stabilizer, and may contain a reactive light stabilizer and a non-reactive light stabilizer.
[0078] Reactive light stabilizers are usually incorporated and fixed in the cured resin system when the surface protective layer is formed, so they can exert a long-term effect. Non-reactive light stabilizers can move within the surface protective layer, so they can exert an immediate effect. The number of ethylenic double bonds in the reactive light stabilizer may be one or two or more.
[0079] In the surface protective layer, the content of the light stabilizer relative to 100 parts by mass of the cured resin is preferably 0.5 parts by mass or more, more preferably 1 part by mass or more, even more preferably 1.5 parts by mass or more, and is preferably 10 parts by mass or less, more preferably 8 parts by mass or less, even more preferably 6 parts by mass or less.
[0080] The surface protective layer preferably contains the reactive light stabilizer and the non-reactive light stabilizer. The blending ratio of the reactive light stabilizer and the non-reactive light stabilizer in the surface protective layer (reactive light stabilizer:non-reactive light stabilizer) based on mass is preferably 8:2 to 0:10.
[0081] In one embodiment, the surface protective layer can be formed by preparing a curable composition, applying the composition to a transparent resin layer or a primer layer or the like to form an uncured resin layer, and crosslinking and curing the uncured resin layer. The crosslinking and curing can be performed, for example, by curing through a heat treatment when a thermosetting resin is used, or by curing through irradiation with ionizing radiation such as an electron beam or ultraviolet light when an ionizing radiation curable compound is used.
[0082] When an electron beam is used as the ionizing radiation, the exposure dose is preferably 5 kGy or more (0.5 Mrad or more), more preferably 10 kGy or more (1 Mrad or more), and preferably 300 kGy or less (30 Mrad or less), more preferably 100 kGy or less (10 Mrad or less).When an ultraviolet ray is used as the ionizing radiation, a light beam containing an ultraviolet ray having a wavelength of 190 nm or more and 380 nm or less may be emitted.
[0083] From the viewpoint of a balance between processability, scratch resistance, and weather resistance, the thickness of the surface protective layer is preferably 1 μm or more, more preferably 1.5 μm or more, even more preferably 2 μm or more, and is preferably 30 μm or less, more preferably 20 μm or less, even more preferably 15 μm or less, and particularly preferably 10 μm or less.
[0084] <Back primer layer> The decorative sheet may have a back primer layer on the surface of the base layer opposite to the surface on which the design layer is provided. The back primer layer is provided as necessary for the purpose of increasing the adhesion between the base layer and the pressure-sensitive adhesive layer.
[0085] The back primer layer is composed of, for example, an adhesive. Examples of adhesives include acrylic resins, acrylic-modified polyolefins, chlorinated polyolefins, vinyl chloride resins, vinyl acetate resins, vinyl chloride-vinyl acetate copolymers, styrene-(meth)acrylic copolymers, polyesters, polyurethanes, and polyamides. Two-part curing polyurethane adhesives or polyester adhesives using an isocyanate compound or the like as a curing agent may also be used. Examples of adhesives include acrylic, urethane, silicone, or rubber pressure-sensitive adhesives.
[0086] From the viewpoint of obtaining excellent adhesion, the thickness of the back primer layer is preferably 0.1 μm or more, more preferably 0.5 μm or more, even more preferably 1 μm or more, and is preferably 10 μm or less, more preferably 6 μm or less, even more preferably 4 μm or less.
[0087] <Adhesive layer> The repair sheet for a decorative material has an adhesive layer on the surface of the base layer or the back primer layer of the decorative sheet. The adhesive layer is a layer that adheres and fixes the repair sheet to the decorative material, which is the adherend, when the repair sheet is applied.
[0088] The adhesive layer is composed of, for example, an adhesive. Examples of the adhesive include an acrylic adhesive, a urethane adhesive, a silicone adhesive, and a rubber adhesive. The above-mentioned adhesive strength can be adjusted, for example, by the type, specific gravity, thickness, etc. of the adhesive layer. Among these, from the viewpoint of easily adjusting the adhesive strength to the above-mentioned range, an acrylic adhesive is preferable, and a two-liquid curing acrylic adhesive is more preferable. The adhesive may be, for example, any of an emulsion type, a solvent type, and a solventless type.
[0089] The adhesive layer may have an air release pattern on the surface opposite to the surface facing the decorative sheet, i.e., on the surface that contacts the adherend when the repair sheet is applied. The air release pattern is usually a groove, and the groove is preferably formed in a lattice shape. When the repair sheet is applied, air can escape along the groove, so that air can be prevented from being trapped between the adhesive layer of the repair sheet and the decorative material that is the adherend, that is, air bubbles can be prevented from being trapped. The width of the groove is preferably 0.5 mm or more and 20 mm or less, and the pitch of the groove is preferably 1 mm or more and 100 mm or less. The air release pattern can be formed, for example, by using a release layer having a pattern complementary to the pattern.
[0090] The thickness of the pressure-sensitive adhesive layer is preferably 1 μm or more, more preferably 5 μm or more, even more preferably 10 μm or more, and is preferably 100 μm or less, more preferably 80 μm or less, even more preferably 60 μm or less.
[0091] <Release layer> The repair sheet for the decorative material may have a release layer on the surface of the adhesive layer opposite to the surface facing the decorative sheet. Since the adhesive layer having adhesive properties is not exposed, such a repair sheet has excellent handleability before application.
[0092] As the release layer, for example, various forms called conventionally known release films, release films, separation films, release papers, separation papers, etc. can be appropriately used. For example, high-quality paper, coated paper, impregnated paper, plastic films, etc., with a release layer formed on one or both sides may be used. Examples of materials for forming the release layer include silicone resins, organic resin-modified silicone resins, fluororesins, aminoalkyd resins, melamine-based resins, acrylic resins, and polyesters. These resins may be, for example, emulsion-type, solvent-type, or solventless-type. When using a release film with a release layer, for example, a silicone release-type polyethylene terephthalate (PET) film, an untreated PET film, a polypropylene film, a silicone release-type paper, etc. can be used.
[0093] The thickness of the release layer is preferably 10 μm or more, more preferably 30 μm or more, and is preferably 200 μm or less, more preferably 150 μm or less.
[0094] [How to repair decorative materials] A method for repairing a decorative material using the repair sheet for a decorative material of the present disclosure will be described. In one embodiment, the repair method includes a step of attaching the repair sheet for a decorative material of the present disclosure to the decorative material to be repaired. In one embodiment, the repair method includes a first step of removing a part of the decorative material to be repaired to form an exposed surface, a second step of forming a primer layer on the exposed surface of the decorative material, and a third step of attaching the repair sheet for a decorative material of the present disclosure to the decorative material to be repaired so that the adhesive layer of the sheet contacts the primer layer.
[0095] The decorative material to be repaired is, for example, a component to be used outdoors. In one embodiment, the decorative material to be repaired comprises an exterior material and a decorative sheet provided on at least a portion of the surface of the exterior material. The decorative material may comprise an adhesive layer between the exterior material and the decorative sheet.
[0096] FIG. 3 shows a schematic cross-sectional view of one embodiment of a decorative material to be repaired. The decorative material 100 includes an exterior material 101, an adhesive layer 102, and a decorative sheet 103 in this order. That is, the exterior material 101, the adhesive layer 102, and the decorative sheet 103 are stacked in the thickness direction, which is the vertical direction on the paper surface of FIG. 3. The surface of the decorative sheet 103 is the observation surface. In FIG. 3, the details of the layer structure of the decorative sheet 103 are omitted. The decorative material 100 is obtained, for example, by laminating the surface of the exterior material 101 that needs to be decorated and the surface of the decorative sheet 103 facing the base layer side (not shown).
[0097] The exterior material is a molded body used outdoors, for example, a molded body exposed to direct sunlight every day. The shape of the exterior material is not particularly limited, and examples thereof include plate materials such as flat plates and curved plates, three-dimensional shaped articles, sheets, and films. Examples of the exterior material include resin members, wood members, and inorganic members.
[0098] Examples of resin members include sheets, plates, and three-dimensional articles made of polyolefin, vinyl chloride resin, styrene resin, (meth)acrylic resin, polyester, polycarbonate, polyamide, polyimide, cellulose resin, phenol resin, rubber, etc.
[0099] Examples of the wooden members include boards or three-dimensional articles made of wood fiberboards such as wood veneers, wood plywood, particle boards, medium density fiberboards (MDF), and laminated lumber. In one embodiment, the decorative material is a decorative board in which the exterior material is a wooden member.
[0100] Examples of inorganic members include metal members and other inorganic members. Examples of metal members include sheets, plates, or three-dimensional articles made of iron, aluminum, copper, tin, titanium, alloys containing at least one of these metals (e.g., carbon steel, stainless steel, duralumin, brass, and bronze), etc. Examples of other inorganic members include plates or three-dimensional articles made of glass, ceramics such as porcelain, non-cement ceramic materials such as gypsum, lightweight aerated concrete (ALC) plates, etc.
[0101] Examples of exterior materials include exterior materials for building structures, exterior materials for vehicles, ships and aircraft, and exterior materials for industrial machines. Examples of exterior materials (building materials) for building structures include exterior walls, roofs, eaves ceilings, floors, fences, pillars, gateposts, various doors such as entrance doors and gates, window materials, handrails, balcony partitions, roofing materials for terraces or carports, fences, framework parts for roof decks or wood decks, soundproof walls or windbreak walls for agricultural houses, general roads and highways, etc. Examples of exterior materials for vehicles include window materials such as side windows, rear windows, roof windows, front windows and quarter windows; headlight covers, turn signal lamp lenses, reflectors; and pillars. Examples of vehicles include light vehicles such as automobiles, railway vehicles, construction machines, and golf carts.
[0102] The thickness of the exterior material may be appropriately selected depending on the application and material, and in one embodiment, may be 0.1 mm or more, 0.3 mm or more, 0.5 mm or more, 10 mm or less, 5 mm or less, or 3 mm or less.
[0103] The exterior material 101 is a part that forms the framework of the decorative material 100 that is the object of repair. In one embodiment, the decorative sheet 103 included in the decorative material 100 to be repaired is a highly weather-resistant decorative sheet that can withstand outdoor use, similar to the decorative sheet included in the repair sheet of the present disclosure described above. The decorative sheet 103 may include the layers described for the decorative sheet described above. The decorative sheet 103 includes a base layer and a design layer, and may further include a transparent resin layer and / or a surface protective layer, and may further include at least one layer selected from a transparent adhesive layer, a primer layer, and a back primer layer. The details of these layers are as described above, and will not be described here. The adhesive layer 102 is a layer for attaching the decorative sheet 103 to the exterior material 101. Details of the adhesive layer 102 are the same as those of the adhesive layer described above, and therefore will not be described here.
[0104] <1st process> In the first step, a part of the decorative material to be repaired is removed to form an exposed surface. In the first step, for example, a part of the decorative sheet included in the decorative material to be repaired is removed from the observation surface to the middle of the thickness direction. The depth to which the decorative sheet is removed is preferably, for example, a depth at which the surface protective layer and most of the transparent resin layer are removed. In other words, it is preferable to remove a part of the decorative sheet to a depth greater than the depth at which the surface protective layer disappears. The surface protective layer and transparent resin layer of a decorative sheet used outdoors generally contain a weatherproofing agent as an additive. Since the decorative sheet has deteriorated with age to the extent that repair is required, the additives such as the weatherproofing agent may bleed out from the surface protective layer and transparent resin layer. The bled-out additives may affect the adhesion of the repair sheet. By removing the surface protective layer and most of the transparent resin layer, the effect can be reduced.
[0105] Methods for removing part of the decorative material include, for example, a method using sandpaper (e.g., sandpaper, abrasive paper), specifically, a method of removing the surface of the decorative sheet by manually moving sandpaper back and forth against the surface of the decorative sheet, and a method of removing the surface of the decorative sheet using an electric sander (electric file) with sandpaper attached, and these may be combined.
[0106] <Second process> In the second step, a primer layer is formed on the exposed surface of the decorative material from which a portion has been removed in the first step. In the second step, for example, a primer layer is formed on the exposed surface of the decorative sheet from which a portion has been removed in the first step. By forming the primer layer, the adhesion of the repair sheet to the decorative material is improved in the next third step.
[0107] Materials for forming the primer layer include, for example, urethane resin, acrylic resin, acrylic polyol resin, cellulose resin, polyester, vinyl chloride-vinyl acetate copolymer, vinyl chloride-vinyl acetate-(meth)acrylic copolymer, chlorinated polyethylene, and chlorinated polypropylene. Methods for forming the primer layer include, for example, a method of applying a liquid primer material to the exposed surface. Examples of the application method include a method in which an operator at the construction site applies the liquid primer material by hand using a brush or a bar coater (coating bar).
[0108] <3rd process> In the third step, the decorative material repair sheet of the present disclosure is attached to the decorative material to be repaired so that the adhesive layer of the sheet is in contact with the primer layer. The decorative material repair sheet may have a release layer on the surface of the adhesive layer before application, i.e., before the third step. During application, the release layer is peeled off and removed from the adhesive layer to expose the adhesive layer. The peeling operation of the release layer is performed, for example, by hand or using a peeling device on site.
[0109] The adhesive layer of the repair sheet is placed opposite the primer layer provided on the decorative material, the repair sheet is pressed against the decorative material, and the repair sheet is attached to the decorative material while releasing air. When the adhesive layer has an air release pattern, it is possible to prevent air from being trapped between the adhesive layer of the repair sheet and the primer layer provided on the decorative material. It is preferable that 24 hours or more have passed since the completion of application until the adhesive strength of the repair sheet to the decorative material stabilizes at a predetermined adhesive strength.
[0110] Examples of tools that can be used to press the repair sheet against the decorative material include a spatula, squeegee, smoothing brush, and roller. Alternatively, the repair sheet may be pressed against the decorative material by hand without using a tool.
[0111] According to the repair method of the present disclosure, at least a portion of the deteriorated decorative sheet of the decorative material to be repaired can be easily replaced with a new decorative sheet related to the repair sheet, and the appearance of the decorative material can be easily renewed to a state with almost no fading or deterioration.
[0112] Fig. 4 shows a schematic cross-sectional view of one embodiment of a repaired decorative material. The repaired decorative material comprises, in this order, a decorative material 100, a primer layer 110, and a repair sheet 1. Specifically, the repaired decorative material comprises, in this order, an exterior material 101, an adhesive layer 102, a decorative sheet 103' from which a portion has been removed, a primer layer 110, an adhesive layer 3, and a decorative sheet 2. In Fig. 4, details of the layer structures of the decorative sheet 2 and the decorative sheet 103' are omitted.
[0113] The present disclosure relates to, for example, the following [1] to [7]. [1] A repair sheet for decorative materials, the repair sheet comprising a decorative sheet and an adhesive layer, the decorative sheet comprising a thermoplastic resin sheet as a base layer, a design layer, and a transparent resin layer, in that order, the adhesive layer being provided on the side of the base layer opposite the side facing the design layer, the repair sheet having an upper yield point load of 25 N / 10 mm or more and 80 N / 10 mm or less, as measured in accordance with the test method of JIS K6732:1996, and an adhesive strength of 40 N / 25 mm or less 24 hours after application to a SUS-BA plate, as measured in accordance with Method 1 of the test method of JIS Z0237:2022, at a peel angle of 180° and a peel speed of 300 mm / min. [2] A repair sheet for decorative materials as described in [1] above, in which the adhesive strength of the repair sheet to a SUS-BA plate is 25 N / 25 mm or more. [3] A repair sheet for a decorative material as described in [1] or [2] above, wherein the repair sheet further comprises a release layer on the side of the adhesive layer opposite to the side facing the decorative sheet. [4] A repair sheet for a decorative material described in any one of [1] to [3], wherein the pressure-sensitive adhesive layer has an air vent pattern on the side of the pressure-sensitive adhesive layer opposite to the side facing the decorative sheet. [5] The repair sheet for a decorative material according to any one of [1] to [4] above, wherein the decorative sheet further comprises a surface protective layer. [6] The repair sheet for a decorative material described in [5] above, further comprising a primer layer between the transparent resin layer and the surface protective layer. [7] A method for repairing a decorative material, comprising: a first step of removing a portion of the decorative material to be repaired to form an exposed surface; a second step of forming a primer layer on the exposed surface of the decorative material; and a third step of attaching a decorative material repair sheet described in any one of [1] to [6] above to the decorative material so that the adhesive layer of the sheet is in contact with the primer layer. EXAMPLES
[0114] Hereinafter, the repair sheet for decorative materials of the present disclosure will be described in more detail based on examples, but the repair sheet for decorative materials of the present disclosure is not limited in any way by the examples.
[0115] [Example 1] A 60 μm thick colored polypropylene sheet (hereinafter also referred to as "PP") was prepared as a thermoplastic resin sheet. A 2 μm thick back primer layer was formed on one side of the thermoplastic resin sheet using a polyester / polyurethane mixed resin. A 2 μm thick wood grain design layer was formed on the other side of the thermoplastic resin sheet by gravure printing. A 2 μm thick transparent adhesive layer was formed on the design layer using a urethane resin adhesive. A transparent polypropylene resin was laminated on the transparent adhesive layer by extrusion lamination to form a 80 μm thick transparent resin layer (hereinafter also referred to as "PP-A"). After corona discharge treatment was performed on the surface of the transparent resin layer, a 2 μm thick primer layer was formed by coating a two-component curing urethane resin. After applying a urethane acrylate-based electron beam curable resin (EB resin) to the surface of the primer layer, the electron beam curable resin was cured by irradiating it with an electron beam using an electron beam irradiation device under conditions of an acceleration voltage of 175 KeV and 5 Mrad to form a surface protective layer with a thickness of 5 μm. A two-component curing acrylic adhesive (NT-138, Nikkei Shinka Co., Ltd., hereinafter also referred to as "Adhesive A") was applied to the back primer layer, and then dried to form an adhesive layer with a thickness of 30 μm. In this way, a repair sheet for the decorative material of Example 1 (hereinafter also referred to as "adhesive sheet") was obtained. The layer structure of the pressure-sensitive adhesive sheet is as follows: pressure-sensitive adhesive layer (30 μm) / back primer layer (2 μm) / thermoplastic resin sheet (60 μm) / design layer (2 μm) / transparent adhesive layer (2 μm) / transparent resin layer (80 μm) / primer layer (2 μm) / surface protective layer (5 μm).
[0116] [Example 2] The adhesive layer was made of an emulsion adhesive (WQ-1000, manufactured by Nippon Paint Holdings Co., Ltd., foam density 0.4 g / cm 3 , coating amount 30g / m 2An adhesive sheet was obtained in the same manner as in Example 1, except that an adhesive sheet B was used instead of the adhesive sheet B.
[0117] [Example 3] An adhesive sheet was obtained in the same manner as in Example 1, except that the adhesive layer was changed to G25 (F38 / F75) (manufactured by Nichiei Shinka Co., Ltd., substrateless double-sided adhesive sheet, acrylic adhesive, hereinafter also referred to as "Adhesive C").
[0118] [Example 4] An adhesive sheet was obtained in the same manner as in Example 1, except that the adhesive layer was changed to Mold Fit 50 (manufactured by Nichiei Shinka Co., Ltd., substrate-less double-sided adhesive sheet, acrylic adhesive, hereinafter also referred to as "Adhesive D").
[0119] [Comparative Example 1] A 60 μm thick colored polypropylene sheet was prepared as a thermoplastic resin sheet. A 2 μm thick back primer layer was formed on one side of the thermoplastic resin sheet using a polyester / polyurethane mixed resin. A 2 μm thick wood grain design layer was formed on the other side of the thermoplastic resin sheet by gravure printing. A 30 μm thick adhesive layer was formed on the back primer layer using adhesive B to obtain a pressure sensitive adhesive sheet of Comparative Example 1.
[0120] [Comparative Example 2] An adhesive sheet was obtained in the same manner as in Comparative Example 1, except that the adhesive layer was changed to Adhesive C.
[0121] [Comparative Example 3] An adhesive sheet was obtained in the same manner as in Comparative Example 1, except that the adhesive layer was changed to Adhesive D.
[0122] [Example 5] A 60 μm thick colored polypropylene sheet was prepared as a thermoplastic resin sheet. A 2 μm thick back primer layer was formed on one side of the thermoplastic resin sheet using a polyester / polyurethane mixed resin. A 2 μm thick wood grain design layer was formed on the other side of the thermoplastic resin sheet by gravure printing. A 2 μm thick transparent adhesive layer was formed on the design layer using a urethane resin adhesive. A 100 μm thick transparent resin layer (hereinafter also referred to as "PP-B") was formed by laminating a transparent polypropylene resin on the transparent adhesive layer by extrusion lamination. After corona discharge treatment was performed on the surface of the transparent resin layer, a 2 μm thick primer layer was formed by coating a two-component curing urethane resin. A urethane acrylate electron beam curable resin (EB resin) was coated on the surface of the primer layer, and then an electron beam irradiation device was used to irradiate electron beams under conditions of an acceleration voltage of 175 KeV and 5 Mrad to cure the electron beam curable resin, thereby forming a 5 μm thick surface protection layer. On the back surface primer layer, a 30 μm-thick adhesive layer was formed using adhesive B. In this manner, a pressure-sensitive adhesive sheet of Example 5 was obtained.
[0123] [Example 6] An adhesive sheet was obtained in the same manner as in Example 5, except that the adhesive layer was changed to Adhesive C.
[0124] [Comparative Example 4] An adhesive sheet was obtained in the same manner as in Example 5, except that the adhesive layer was changed to Adhesive D.
[0125] [Example 7] A 60 μm thick colored polypropylene sheet was prepared as a thermoplastic resin sheet. A 2 μm thick back primer layer was formed on one side of the thermoplastic resin sheet using a polyester / polyurethane mixed resin. A 2 μm thick wood grain design layer was formed on the other side of the thermoplastic resin sheet by gravure printing. A 2 μm thick transparent adhesive layer was formed on the design layer using a urethane resin adhesive. Polyvinyl chloride was laminated on the transparent adhesive layer by extrusion lamination to form a 80 μm thick transparent resin layer (hereinafter also referred to as "PVC"). After corona discharge treatment was performed on the surface of the transparent resin layer, a 2 μm thick primer layer was formed by coating a two-component curing urethane resin. A urethane acrylate-based electron beam curable resin (EB resin) was coated on the surface of the primer layer, and then an electron beam was irradiated at an acceleration voltage of 175 KeV and 5 Mrad using an electron beam irradiation device to cure the electron beam curable resin, forming a 5 μm thick surface protection layer. On the back surface primer layer, a 30 μm-thick adhesive layer was formed using adhesive B. In this manner, an adhesive sheet of Example 7 was obtained.
[0126] [Example 8] An adhesive sheet was obtained in the same manner as in Example 7, except that the adhesive layer was changed to Adhesive C.
[0127] [Comparative Example 5] An adhesive sheet was obtained in the same manner as in Example 7, except that the adhesive layer was changed to Adhesive D.
[0128] [Comparative Example 6] A polyester film having a thickness of 125 μm (Lumirror #125-S10, manufactured by Toray Industries, Inc., hereinafter also referred to as "PET") was prepared as a thermoplastic resin sheet. A design layer having a wood grain pattern was formed by gravure printing so as to have a thickness of 2 μm on one side of the thermoplastic resin sheet. A pressure-sensitive adhesive layer having a thickness of 30 μm was formed on the other side of the thermoplastic resin sheet using Adhesive B to obtain a pressure-sensitive adhesive sheet of Comparative Example 6.
[0129] [Comparative Example 7] An adhesive sheet was obtained in the same manner as in Comparative Example 6, except that the adhesive layer was changed to Adhesive C.
[0130] [Comparative Example 8] An adhesive sheet was obtained in the same manner as in Comparative Example 6, except that the adhesive layer was changed to Adhesive D.
[0131] [Evaluation of adhesive sheets] <Upper yield point load> The adhesive sheet was punched out into a dumbbell-shaped test piece with the shape and dimensions shown in "Figure 3" of JIS K6732:1996 to prepare a dumbbell-shaped test piece. The test piece was prepared so that the long axis direction of the dumbbell-shaped test piece was aligned with the machine direction (MD) of the adhesive sheet. In accordance with "9.3 Tensile test" of JIS K6732:1996, the test piece was pulled using a tensile compression tester (Orientec Co., Ltd., Tensilon universal material testing machine, RTC-1250A) at a temperature of 23°C and a tensile speed of 200 mm / min, a load-elongation curve was created, and the upper yield point load was obtained.
[0132] <Adhesive strength> The adhesive strength of the adhesive sheet was measured as follows. A test piece of the adhesive sheet 25 mm wide and 100 mm long was pressed against the adherend (SUS-BA plate) with a 2 kg roller going back and forth once so that the exposed adhesive layer was in contact with the adherend, and then left to stand for 24 hours under an environment of 23°C temperature and 50% RH. After standing, the adhesive strength to the SUS-BA plate was measured by peeling the test piece in the length direction under the conditions of 25 mm wide, 180° peel angle, and 300 mm / min peel speed using a tensile tester (Orientec Co., Ltd., Tensilon universal material testing machine, RTC-1250A) in accordance with JIS Z0237:2022 (Adhesive tape and adhesive sheet test method) test method, method 1 (temperature 23°C, humidity 50% RH, tape and sheet peeled at 180° against stainless steel test plate). The SUS plate used was SUS304, surface finished BA, and had a thickness of 1.5 mm, a width of 100 mm, and a length of 150 mm.
[0133] <Repositionability> Exterior square timber (LIXIL Corporation, 8TYD55RA, □70mm) was treated with a primer (3M, DP-900N3) to prepare an adherend. The prepared pressure-sensitive adhesive sheet was attached to the adherend with fingers, and then peeled off with fingers. The presence or absence of defects was evaluated based on human sensibility according to the following criteria. A: The adhesive sheet can be peeled off without any stress. B: When peeling off the adhesive sheet, the adhesive sheet stretches, reducing the design, or The adhesive sheet adheres firmly to the adherend and cannot be peeled off.
[0134] <Lifting and peeling> An exterior square timber (LIXIL Corporation, 8TYD55RA, □70mm) was treated with a primer (3M, DP-900N3) to prepare an adherend. The prepared pressure-sensitive adhesive sheet was attached to the adherend using a squeegee so that one side of the adherend was covered with the pressure-sensitive adhesive sheet and the linear length of the covered area from the corner of the adjacent side was 5mm, and the adherend was then stored at room temperature for one week. After storage, the pressure-sensitive adhesive sheet was checked for lifting or peeling. A: There is no lifting or peeling anywhere on the adhesive sheet. B: Lifting or peeling is observed at the corners or over the entire pressure sensitive adhesive sheet from the substrate.
[0135] <Design> Exterior square timber (LIXIL Corporation, 8TYD55RA, □70mm) was treated with a primer (3M, DP-900N3) to prepare the adherend. The adhesive sheet was attached to the corners of the adherend while pulling the adhesive sheet so that no air bubbles or slack remained. The adhesive sheet was evaluated based on human sensibility according to the following criteria to see whether there was any deterioration in design due to stretching, etc. A: There is no noticeable decrease in design. B: The adhesive sheet stretches during application, causing a perceived decrease in design.
[0136] <Shape conformity> Exterior square timber (LIXIL Corporation, 8TYD55RA, □70mm) was treated with a primer (3M, DP-900N3) to prepare the adherend. The adhesive sheet was attached to the corners of the adherend while pulling the adhesive sheet so that no air bubbles or slack remained. The adhesive sheet was evaluated based on human sensibility according to the following criteria to see whether there were any problems, mainly with its ability to conform to the corner shape when attached. A: There are no problems with conforming to the shape of corners and workability is good. B: It is impossible to make the sheet conform to the corner shape without any gaps, It is very difficult.
[0137] [Table 1] [Explanation of symbols]
[0138] 1. Repair sheet for decorative materials 2. Decorative sheet 3. Adhesive layer 10...Base material layer 20. Design layer 26...Transparent adhesive layer 30...Transparent resin layer 40 Primer layer 50...Surface protective layer 60···Back primer layer 100···Cosmetic materials 101...Exterior materials 102 Adhesive layer 103...Decorative sheet 110 Primer layer
Claims
1. A repair sheet for decorative materials, The repair sheet includes a decorative sheet and a pressure-sensitive adhesive layer, the decorative sheet includes a thermoplastic resin sheet as a base layer, a design layer, and a transparent resin layer in this order, and the pressure-sensitive adhesive layer is provided on a surface of the base layer opposite to a surface facing the design layer, The repair sheet has an upper yield point load of 25 N / 10 mm or more and 80 N / 10 mm or less, as measured in accordance with the test method of JIS K6732:1996; The repair sheet has an adhesive strength of 40 N / 25 mm or less 24 hours after application to a SUS-BA plate, measured at a peel angle of 180° and a peel speed of 300 mm / min in accordance with JIS Z0237:2022 test method 1. Repair sheet for decorative materials.
2. 2. The repair sheet for decorative materials according to claim 1, wherein the adhesive strength of the repair sheet to a SUS-BA plate is 25 N / 25 mm or more.
3. 2. The repair sheet for a decorative material according to claim 1, further comprising a release layer on a surface of the pressure-sensitive adhesive layer opposite to the surface facing the decorative sheet.
4. 2. The repair sheet for a decorative material according to claim 1, wherein the pressure-sensitive adhesive layer has an air vent pattern on a surface of the pressure-sensitive adhesive layer opposite to a surface facing the decorative sheet.
5. The decorative material repair sheet according to claim 1 , wherein the decorative sheet further comprises a surface protective layer.
6. The repair sheet for decorative materials according to claim 5 , further comprising a primer layer between the transparent resin layer and the surface protective layer.
7. A first step of removing a portion of a decorative material to be repaired to form an exposed surface; A second step of forming a primer layer on the exposed surface of the decorative material; A third step of attaching the decorative material repair sheet according to any one of claims 1 to 6 to the decorative material such that the adhesive layer of the sheet is in contact with the primer layer; The decorative material repair method comprises the steps of:
Citation Information
Patent Citations
Decorative material adaptable to reforming and its use method
JP2000094566A
Reform corresponding decorative material and reforming method
JP2002127291A