Hollow structure board and method for manufacturing the same
The hollow structural plate, featuring thermoplastic resin foam with a controlled skin layer, addresses the stability and surface issues of conventional foamed resin plates, offering lightweight, cushioned, and aesthetically pleasing solutions with improved strength and printability.
Patent Information
- Application Number
- JP2023052059
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Conventional hollow plates made of foamed thermoplastic resin face issues with poor strength stability and surface condition, limiting their practical applications.
A hollow structural plate design comprising a pair of plate-like bodies made of thermoplastic resin foam, with a skin layer on the outermost surface and a rib partitioning the space between them, where the skin layer has no foaming and is between 3 μm and 50% of the plate's thickness, ensuring a lightweight and stable structure.
The solution provides a lightweight plate with excellent cushioning properties, stable strength, and a smooth surface, enhancing designability, printability, and cleaning performance, while maintaining structural integrity.
Smart Images

Figure 00000000_0000_ABST
Abstract
Description
[Technical field]
[0001] The present invention relates to a hollow structure board and a manufacturing method thereof, and more particularly to a hollow structure board that is lightweight and has excellent shock-absorbing properties while also exhibiting excellent strength stability and surface condition, and a manufacturing method thereof. [Background technology]
[0002] Hollow resin boards are lightweight boards used for partitions and dividers, but to provide them with shock-absorbing properties, it is necessary to either attach a shock-absorbing material to them or to set the weight per unit area (i.e., basis weight) low when the thickness of the hollow resin board is constant. However, attaching a shock-absorbing material leads to increased costs and weight, and even if the basis weight is reduced, there is a manufacturing limit to the lower limit of the basis weight, and when trying to make each structural part of the hollow board thinner in order to improve its light weight and shock-absorbing properties, problems arise such as the structure of the hollow board itself becoming unmaintainable.
[0003] In response to this, for example, Patent Document 1 discloses a foamed thermoplastic resin hollow plate, which is characterized in that the thermoplastic resin is foamed in a thermoplastic resin hollow plate having multiple ribs interposed between a pair of thin thermoplastic resin plates arranged in parallel in order to reduce the weight of the hollow plate. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-29257 Summary of the Invention [Problem to be solved by the invention]
[0005] However, while conventional hollow panels made of foamed thermoplastic resins are lightweight and have excellent cushioning properties, they have problems such as poor strength stability and surface condition, and there is a need for further technological development.
[0006] In view of the above circumstances, the present invention has as its main object to provide a hollow structure board that is lightweight and has excellent shock-absorbing properties while also exhibiting excellent strength stability and surface condition, and a method for manufacturing the same. [Means for solving the problem]
[0007] The present invention first provides a hollow structure plate comprising at least a pair of plate-like bodies arranged approximately parallel to each other and a rib dividing the space between the pair of plate-like bodies, the pair of plate-like bodies being made of a thermoplastic resin foam, and the outermost layer of the plate-like bodies having a skin layer with no foaming visible on the surface that is 3 μm or more in thickness and 50% or less of the thickness of the plate-like bodies. The thermoplastic resin foam may have an apparent expansion ratio including the skin layer of 1.1 or more and 5.0 or less. The thermoplastic resin foam may be composed of 50% or more closed cells. The volume of the closed cell is 0.00005 mm 3 More than 0.25mm 3 It may be the following.
[0008] The present invention also provides a method for producing a hollow structure plate comprising at least a pair of plate-like bodies arranged approximately parallel to each other and a rib dividing the space between the pair of plate-like bodies, the pair of plate-like bodies being made of a thermoplastic resin foam, and the outermost layer of the plate-like bodies having a skin layer with no visible foaming on the surface that is 3 μm or more in thickness and 50% or less of the thickness of the plate-like bodies, the method comprising at least a step of preparing the skin layer. Effect of the Invention
[0009] In view of the above circumstances, the present invention provides a hollow structure board that is lightweight and has excellent shock-absorbing properties while also exhibiting excellent strength stability and surface condition, and a method for manufacturing the same. Note that the effects described here are not necessarily limited to those described herein, and may be any of the effects described in this specification. [Brief description of the drawings]
[0010] [Figure 1] 1 is a perspective view showing a schematic view of a first embodiment of a hollow structure plate 1 according to the present invention. [Diagram 2] 2 is a schematic end view taken along line XX of the first embodiment shown in FIG. 1. [Diagram 3] FIG. 2 is a perspective view showing a schematic diagram of a second embodiment of a hollow structure plate 1 according to the present invention. [Figure 4] 4 is a schematic end view of the second embodiment taken along line YY shown in FIG. 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. The embodiment described below is merely one example of a typical embodiment of the present invention, and the scope of the present invention should not be construed as being narrow.
[0012] 1.Hollow structural board 1 Fig. 1 is a perspective view showing a first embodiment of a hollow structure plate 1 according to the present invention, and Fig. 3 is a perspective view showing a second embodiment of a hollow structure plate 1 according to the present invention. The hollow structure plate 1 according to the present invention comprises at least a pair of plate-like bodies 11 and a rib 12 that divides the space between the pair of plate-like bodies 11. Note that the thickness of the skin layer 111 shown in Figs. 1 to 4 is for convenience, and the present invention is not limited to this thickness.
[0013] In this specification, the term "plate-like" refers to a substantially plate-like shape, and may be partially curved or have an uneven surface. In this specification, the term "rib" refers to a structure that divides the space between the plate-like bodies 11 into two or more, and the shape of the rib is not particularly limited. In addition, in Figs. 1 and 3, the angle between the plate-like bodies 11 and the rib 12 is approximately 90°, but the present invention is not limited to this. Furthermore, the plate-like bodies 11 and the rib 12 may be integrally molded, and in this case, the upper end and / or the lower end of the rib 12 may be rounded.
[0014] In addition, in the present invention, the pair of plate-like bodies 11 are made of a thermoplastic resin foam, and the outermost layer of the plate-like body 11 has a skin layer 111 on the surface where no foam is observed, which is 3 μm or more and 50% or less of the thickness of the plate-like body.
[0015] In the present invention, it is preferable that the rib 12 that separates the space between the pair of plate-like bodies 11 is also made of a thermoplastic resin foam. Moreover, the rib 12 may not have a skin layer 111 as shown in Fig. 1, or may have a skin layer 111 as shown in Fig. 3. That is, the present invention may include any of the embodiments.
[0016] The hollow structure plate 1 according to the present invention is lightweight and has excellent cushioning properties, while also having excellent strength stability. In addition, since the surface condition is good, the appearance is beautiful and has excellent design, and since there are no problems such as ink retention or severe bleeding, the printability is also good. Furthermore, since it has excellent effects such as preventing adhesion and accumulation of dirt, dust, etc., it is also excellent in cleanability. In addition, it also has effects such as heat insulation and sound absorption that can be expected from thermoplastic resin foam. Therefore, it is expected to be used in a wide range of fields, such as partition boards, partitions (partitions), heat insulation materials, packaging materials, cushioning materials, returnable boxes, sound absorbing materials, building materials, interior materials for vehicles, etc.
[0017] In the present invention, although not shown, both ends of the hollow structure plate 1 can be processed into a desired shape by heat treatment including thermocompression bonding, or can be sealed (sealed).
[0018] <Thermoplastic resin foam> In this specification, the term "thermoplastic resin foam" refers to a foamed thermoplastic resin composition containing at least a thermoplastic resin and a foaming agent. In the present invention, the pair of plate-like bodies 11 and preferably the rib 12 are formed of a thermoplastic resin foam.
[0019] Examples of thermoplastic resins include polyester-based resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PENp), and liquid crystal polyester (LCP); polyimide-based resins; polyolefin-based resins such as polypropylene (PP), polyethylene (PE), and polyisobutylene (PB); styrene-based resins such as polystyrene (PS), acrylonitrile-styrene resin (AS), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-acrylic-styrene resin (AAS), and acrylonitrile-ethylene propylene rubber-styrene (AES); polyphenylene ether-based resins; polyamide-based resins; polycarbonate-based resins; polyarylate-based resins; polyphenylsulfone-based resins; polysulfone-based resins; and polyethersulfone-based resins. In the present invention, two or more of these may be used in combination, or commercially available products may be used.
[0020] Other examples include olefin-based elastomers, styrene-based elastomers, etc. Examples of olefin-based elastomers include ethylene-α-olefin copolymer elastomers such as ethylene-propylene copolymer elastomers (EPR), ethylene-butene copolymer elastomers (EBR), ethylene-hexene copolymer elastomers (EHR), and ethylene-octene copolymer elastomers (EOR); and ethylene-α-olefin-diene terpolymer elastomers such as ethylene-propylene-ethylidenenorbornene copolymer, ethylene-propylene-butadiene copolymer, and ethylene-propylene-isoprene copolymer. Examples of styrene-based elastomers include styrene-butadiene-styrene triblock copolymer elastomer (SBS), styrene-isoprene-styrene triblock copolymer elastomer (SIS), styrene-ethylene-butylene copolymer elastomer (SEB), styrene-ethylene-propylene copolymer elastomer (SEP), styrene-ethylene-butylene-styrene copolymer elastomer (SEBS), styrene-ethylene-butylene-ethylene copolymer elastomer (SEBC), and hydrogenated styrene-butadiene elastomer (HSBR). Examples of the elastomer include styrene-based elastomers such as styrene-ethylene propylene-styrene copolymer elastomer (SEPS), styrene-ethylene ethylene propylene-styrene copolymer elastomer (SEEPS), styrene-butadiene butylene-styrene copolymer elastomer (SBBS), partially hydrogenated styrene-isoprene-styrene copolymer elastomer, partially hydrogenated styrene-isoprene butadiene-styrene copolymer elastomer, and hydrogenated polymer-based elastomers such as ethylene-ethylene butylene-ethylene copolymer elastomer (CEBC). In the present invention, two or more of these may be used in combination, or commercially available products may be used.
[0021] In the present invention, among these, it is preferable to use a resin having a melt flow rate (MFR, in the case of polypropylene, measured at 230°C and 2.16 kgf) of 0.5 g / 10 min or more and 5.0 g / 10 min or less as indicated in JISK7210:2014 (ISO1133:2011) as the thermoplastic resin. If the MFR is less than 0.5 g / min, foaming becomes difficult. If the MFR is more than 5.0 g / 10 min, it becomes difficult to maintain the structure of the hollow structure plate 1 during molding. Specific examples of resins having an MFR of 0.5 g / 10 min to 5.0 g / 10 min include polypropylene, polyethylene, polystyrene, polycarbonate, polyethylene terephthalate, and acrylonitrile-butadiene-styrene resins, and the like are not particularly limited in the present invention, but among these, polypropylene and polystyrene are particularly preferable.
[0022] Examples of the foaming agent include physical foaming agents, chemical foaming agents, etc. In the present technology, although there is no particular limitation, from the viewpoint of productivity, chemical foaming agents are preferred. Examples of chemical foaming agents include organic chemical foaming agents and inorganic chemical foaming agents. Examples of organic chemical foaming agents include azodicarbonamide, hydrazodicarbonamide, azodicarboxylate barium salt, dinitrosopentaethylenetetramine, nitrosoguanidine, 4,4'-oxybis(benzenesulfonic acid hydrazide), trihydrazine symmetric triazine, barium azodicarboxylate, azobisisobutyronitrile, and toluenesulfonyl hydrazide. Examples of inorganic chemical foaming agents include sodium hydrogen carbonate, sodium carbonate, zinc carbonate, ammonium hydrogen carbonate, ammonium carbonate, and ammonium nitrite. Examples of physical foaming agents include air, oxygen, nitrogen, carbon dioxide, ethane, propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, isohexane, cyclohexane, heptane, ethylene, propylene, water, petroleum ether, methyl chloride, ethyl chloride, monochlorotrifluoromethane, dichlorodifluoromethane, and dichlorotetrafluoroethane. These foaming agents can be appropriately selected taking into consideration the type of thermoplastic resin used, the desired expansion ratio, etc., and two or more of these may be used in combination.
[0023] The content of the foaming agent is not particularly limited, but can be appropriately set in consideration of the type of foaming agent used, the desired expansion ratio, etc. For example, the content is preferably 0.01 parts by mass or more and 10 parts by mass or less, and more preferably 0.05 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin.
[0024] The thermoplastic resin foam may further contain, as other optional components, a cell regulator, a stabilizer, an ultraviolet absorber, a colorant, an antioxidant, a crystallization promoter, a lubricant, a crosslinking agent, a surfactant, a shrinkage inhibitor, a flame retardant, an anti-deterioration agent, etc., but the present invention is not limited to these.
[0025] In the present invention, the apparent expansion ratio of the thermoplastic resin foam including the skin layer 111 described below is preferably 1.1 or more and 5.0 or less. By setting the apparent expansion ratio to 1.1 or more, it is possible to reduce the weight of the same apparent structure. Also, by setting the apparent expansion ratio to 5.0 or less, it is possible to prevent the breakage of the closed cell.
[0026] The expansion ratio of the thermoplastic resin foam including the skin layer 111 described later can be determined, for example, by determining the density of the thermoplastic resin, and dividing the density of the thermoplastic resin by the apparent density of the foam obtained to obtain the expansion ratio. The apparent density can be determined, for example, by dividing the weight of the hollow structure plate 1 obtained by multiplying the total cross-sectional area of the skin layer 111, the plate-like body 11, and the rib 12 by the length.
[0027] In the present invention, the thermoplastic resin foam is preferably composed of 50% or more of closed cells (i.e., the closed cell ratio is preferably 50% or more), more preferably 60% or more of closed cells, even more preferably 70% or more of closed cells, even more preferably 80% or more of closed cells, and particularly preferably 90% or more of closed cells. By being composed of 50% or more of closed cells, it is possible to reduce the weight and improve the buoyancy and heat insulation. The closed cell ratio in the thermoplastic resin foam may be 100% or less, or may be 99% or less from the viewpoint of ease of production.
[0028] The closed cell ratio in a thermoplastic resin foam can be determined, for example, by a method described in JIS K7138:2006 "Rigid foamed plastics - Determination of open cell ratio and closed cell ratio" or the like.
[0029] In the present invention, the volume of the closed cell is 0.00005 mm 3 More than 0.25mm 3 It is preferable that the value is less than 0.0001 mm. 3 More than 0.13mm 3 It is more preferable that the volume of the closed cell is 0.00005 mm or less. 3 By setting the volume of the closed cell at 0.25 mm or more, the foaming agent can be efficiently used, and a lightweight hollow structure board 1 can be provided. 3 By satisfying the following conditions, local deterioration of physical properties can be suppressed, and a hollow structure board 1 with stable strength can be provided.
[0030] In the present invention, the aspect ratio of the closed cell is preferably 1.1 or more, where the direction in which the ribs 12 are formed is the vertical side and the direction perpendicular to the vertical side and in which the ribs 12 are not formed is the horizontal side. By making the aspect ratio 1.1 or more, in combination with the molecular orientation of the resin component, it is possible to obtain ease of tearing in the direction of the ribs 12.
[0031] <Skin Layer 111> In this specification, the term "skin layer" refers to a portion on the surface where no bubbles are observed, i.e., a dense surface portion on the surface where no broken bubbles are observed and which is in a smooth, film-like state.
[0032] In the present invention, by making the skin layer 111 3 μm or more, it is possible to improve the design, printability, and cleanability (prevention of adhesion of dirt, dust, etc.). In addition, by making the skin layer 111 50% or less of the thickness of the plate-like body 11, it is possible to reduce the weight in terms of apparent volume.
[0033] The surface roughness (Ra; arithmetic mean height (μm)) of the skin layer 111 in the present invention is preferably Ra10 μm or less, and more preferably Ra5 μm or less. By making the surface roughness of the skin layer 111 Ra10 μm or less, it is possible to improve the design, printability, and cleanability (prevention of adhesion of dirt, dust, etc.).
[0034] 2. Manufacturing method of hollow structure plate 1 The manufacturing method according to the present invention is a method for manufacturing the hollow structure board 1 described above, which includes at least a step of producing the skin layer 111. If necessary, other steps such as an extrusion foam molding step may be performed. Each step will be described in detail below.
[0035] (1)Extrusion foam molding process In this step, extrusion foam molding is performed using a conventionally known method. As an example, a foamable resin composition obtained by mixing a thermoplastic resin, a foaming agent, and other optional components is fed into an extruder equipped with a screw or the like. The extruder may be used alone or in combination with a tandem extruder.
[0036] Next, the foamable resin composition is heated and kneaded by the screw of the extruder under heating, while an extrusion force is applied in the direction of the tip of the screw. The kneading conditions here vary depending on the types of thermoplastic resin, foaming agent, etc. used, but the heating conditions are, for example, 200°C to 300°C, and are preferably set to a temperature equal to or higher than the melting temperature of the thermoplastic resin or the decomposition temperature of the foaming agent or foaming component. In addition, the screw rotation speed and extrusion speed can be appropriately selected, although they vary depending on the type of screw (for example, screw diameter, etc.).
[0037] The melt-kneaded foamable resin composition is then extruded into a low-pressure region through a die having a predetermined shape, and the foaming agent or the decomposed components of the foaming agent are vaporized to foam the foamable resin composition, while molding it into a predetermined shape. The temperature of the die varies depending on the types of thermoplastic resin, foaming agent, etc. used, but is preferably equal to or lower than the temperature set during heat kneading. If the die temperature is higher than the temperature during heat kneading, foaming on the surface of the molded product becomes noticeable, impairing the appearance, destroying independent cells to form interconnected holes, and making molding itself difficult.
[0038] (2) Step of preparing skin layer 111 In this step, the skin layer 111 is produced. The skin layer 111 can be formed by lowering the temperature gradient of the die and setting it lower than the previous flow channel temperature. More specifically, for example, the skin layer 111 is produced by using air cooling or a cooling sizing former while melt extrusion foaming from a die opening set at a temperature lower than the cylinder temperature. That is, the step of producing the skin layer 111 is carried out simultaneously when the foamable resin composition is molded into a predetermined shape in the extrusion foam molding step. The extruded molded body is cooled by a primary cooling (air cooling) mechanism such as cooling air and a cooling roll, and passes through a secondary cooling mechanism to obtain the hollow structure plate 1 according to the present invention.
[0039] In the manufacturing method according to the present invention, the ratio of the skin layer 111 at the outermost layer of the plate-like body 11 to the thickness of the plate-like body 11 and the thickness of the skin layer 111 can be controlled by adjusting the structure and temperature of the die and the temperature and speed of the primary cooling (air cooling) in this process. In addition, the apparent expansion ratio including the skin layer 111, the closed expansion ratio, and the volume of the closed cells of the thermoplastic resin foam can be controlled by adjusting the amount of foaming agent and the like added and the cooling speed from the molten state (secondary cooling: cooling sizing former temperature, take-up speed).
[0040] (3) Other processes In the manufacturing method according to the present invention, as other steps, the obtained hollow structure plate 1 may be collected by a collecting machine or cut to a desired size by a cutting machine, if necessary. In addition, a step may be performed in which both ends of the hollow structure plate 1 are processed into a desired shape by heat treatment including thermocompression or sealed. This can improve the shape retention during use. EXAMPLES
[0041] The present invention will now be described in further detail with reference to examples. The embodiment described below is merely a representative example of the present invention, and the scope of the present invention should not be construed as being narrow.
[0042] <Manufacturing of hollow structural panels> In Examples 1 to 7, in the manufacturing method of the hollow structure board 1 described above, a skin layer was formed on the outermost layer of the hollow structure board, and the hollow structure board of the embodiment shown in Figs. 1 and 2 was manufactured.
[0043] In Comparative Examples 1 to 3, a hollow structure plate having a pair of plate-like bodies and a rib structure partitioning the space between the pair of plate-like bodies was formed from a thermoplastic resin, not a thermoplastic resin foam. As a manufacturing method, the hollow structure plate was produced by conventional extrusion molding.
[0044] For Comparative Example 4, a hollow structure plate was produced in the same manner as in the above-mentioned manufacturing method of hollow structure plate 1, except that a skin layer was not formed. For Comparative Example 5, a hollow structure plate was produced in the same manner as in the above-mentioned manufacturing method of hollow structure plate 1, except that a thickness of the skin layer was set to 1 μm. Furthermore, for Comparative Example 6, a hollow structure plate was produced in the same manner as in the above-mentioned manufacturing method of hollow structure plate 1, except that a ratio of the skin layer at the outermost layer to the thickness of the plate-like body was set to 66.7%.
[0045] <Evaluation> The hollow structure plates thus produced were evaluated for their strength stability, cushioning properties, and surface condition (printability and cleanability).
[0046] [Strength stability] To test for strength stability, a hollow structural board measuring 100 mm wide (in the direction where the ribs are formed) x 1000 mm long (in the direction where the ribs are not formed) was bent into a U-shape by applying force from both ends, the position at which it broke was measured, and the percentage that was ±200 mm from the centre was calculated.
[0047] The evaluation method was to compare the obtained ratios with the following evaluations. Over 80%: ◎ Between 50% and 80%: Yes Less than 50%: ×
[0048] [Buffering properties] Regarding the cushioning properties, the surface hardness was measured using an A-type hardness tester (Durometer Type A, manufactured by Shimadzu Corporation) at the midpoint between adjacent ribs on the liner surface in a plan view.
[0049] The evaluation method was to compare the obtained A hardness with the following evaluation. That is, the evaluation was performed by subtracting the A-hardness measurement value of the corresponding product from the A-hardness measurement value of the resin alone (non-foamed) with the same structure and basis weight. The corresponding product is shown in Tables 1 and 2 below as a "comparison of cushioning properties." More than 5°:◎ More than 0° and less than 5°:○ Below 0°: ×
[0050] [Surface condition (printability and cleanability)] Regarding the surface condition (printability and cleanability), the surface roughness was measured using a measuring instrument (Surface Measuring Instrument SV-600, manufactured by Mitutoyo Corporation). The measurement point was the midpoint between adjacent ribs on the liner surface in a plan view. The lower the surface roughness, the less the ink will remain and the better the effect of preventing the adhesion and accumulation of dirt, dust, etc.
[0051] The surface roughness was evaluated according to the following criteria. Ra5μm or less:◎ More than Ra5μm and less than Ra10μm:〇 Ra over 10μm: ×
[0052] <Evaluation> The evaluation results are shown in Tables 1 and 2 below.
[0053] [Table 1]
[0054] [Table 2]
[0055] <Consideration> The hollow structure boards of Examples 1 to 7 were lighter and more stable in strength, and also had better stability in strength and surface condition than the hollow structure boards of Comparative Examples 1 to 6. On the other hand, none of the hollow structure boards of Comparative Examples 1 to 6 were excellent in all of these items. Therefore, it was found that a hollow structure board that is lighter and more stable in strength can be provided by providing at least a pair of plate-like bodies arranged approximately parallel to each other and a rib that divides the space between the pair of plate-like bodies, the pair of plate-like bodies being made of a thermoplastic resin foam, and the outermost layer of the plate-like bodies having a skin layer with no foaming on the surface being 3 μm or more and 50% or less of the thickness of the plate-like bodies. [Industrial Applicability]
[0056] According to the present invention, it is possible to provide a hollow structure board and a manufacturing method thereof that are lightweight, have excellent strength stability, and have excellent strength stability and surface condition. The hollow structure board 1 according to the present invention is lightweight, has excellent strength stability, has a beautiful appearance and excellent design, and has no problems such as ink retention, so it has good printability. It is also excellent in cleaning properties because it is excellent in preventing adhesion and accumulation of dirt, dust, etc. In addition, it also has effects such as heat insulation and sound absorption that can be expected from thermoplastic resin foam. Therefore, it is expected to be used in a wide range of fields such as partition boards, partitions (partitions), heat insulation materials, packaging materials, cushioning materials, returnable boxes, sound absorbing materials, building materials, interior materials for vehicles, etc. [Explanation of symbols]
[0057] 1:Hollow structure plate 11: Plate-shaped body 12: Rib 111: Skin layer
Claims
1. A pair of plate-like bodies arranged approximately parallel to each other; A rib that divides a space between the pair of plate-like bodies; At least The pair of plate-like bodies are made of a thermoplastic resin foam, The outermost layer of the plate-like body is a skin layer with no bubbles visible on the surface, the skin layer being 3 μm or more and 50% or less of the thickness of the plate-like body.
2. The hollow structure board according to claim 1 , wherein the apparent expansion ratio of the thermoplastic resin foam including the skin layer is 1.1 or more and 5.0 or less.
3. The hollow structure board according to claim 1 or 2, wherein the thermoplastic resin foam is composed of 50% or more closed cells.
4. The volume of the closed cell is 0.00005 mm 3 0.25mm or more 3 4. The hollow structural plate according to claim 3, wherein:
5. A method for manufacturing a hollow structure plate comprising at least a pair of plate-like bodies arranged approximately parallel to each other and a rib dividing the space between the pair of plate-like bodies, the pair of plate-like bodies being made of a thermoplastic resin foam, and the outermost layer of the plate-like bodies having a skin layer with no visible foaming on the surface that is 3 μm or more and 50% or less of the thickness of the plate-like bodies, the method comprising at least a step of preparing the skin layer.
Citation Information
Patent Citations