Fiber-reinforced composite body and manufacturing method thereof

The fiber-reinforced composite with a controlled skin layer thickness addresses water infiltration issues, enhancing buoyancy and moldability for marine and water treatment applications.

JP2024140751APending Publication Date: 2024-10-10UBE NITTO KASEI CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2023052067
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Conventional fiber-reinforced composites face issues such as water infiltration leading to decreased buoyancy and settling, particularly in marine and water treatment applications.

Method used

A fiber-reinforced composite structure is developed with a core made of thermoplastic resin foam, an intermediate layer of impregnated reinforcing fibers, and a thermoplastic resin outer layer, featuring a controlled skin layer thickness of 3 μm to 30% of the core diameter, ensuring independent foaming and improved buoyancy.

Benefits of technology

The composite achieves enhanced quality with reduced apparent specific gravity, maintaining sufficient buoyancy and moldability, suitable for marine and water treatment materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140751000001_ABST
    Figure 2024140751000001_ABST
Patent Text Reader

Abstract

To provide a fiber-reinforced composite body with improved quality and a manufacturing method thereof.SOLUTION: Provided are a fiber-reinforced composite body and a manufacturing method thereof, and the fiber-reinforced composite body comprises at least: a middle core made of a thermoplastic resin; an intermediate layer made by integrally binding a reinforced fiber impregnated with a resin to an outer periphery of the middle core; and an outer layer covering the intermediate layer, and made of a thermoplastic resin. In the fiber-reinforced composite body, the middle core is composed of a resin foam a part or the whole of which has a closed cell foam, and a skin layer formed on a part or the whole of an outer peripheral surface of the middle core has a thickness of at least 3 μm, which is 30% or less of the diameter of the middle core.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a fiber-reinforced composite and a manufacturing method thereof, and more particularly to a fiber-reinforced composite having improved quality and a manufacturing method thereof. [Background technology]

[0002] Fiber-reinforced articles in which reinforcing fibers are bound with resin are strong and lightweight, and therefore are used as alternative materials to metal articles in a wide range of fields, such as automobile parts, electronic parts, agricultural and forestry materials, building materials, furniture, etc. For example, as one of the products using the technology related to the fiber-reinforced articles, pipes, rods, linear objects, etc., which use long-fiber bundles such as glass roving as reinforcing fibers and resin as a matrix, have been used for a long time in various industrial fields.

[0003] For example, Patent Document 1 discloses a reinforced plastic rod-shaped product having a three-layer structure in which the outer periphery of a core rod-shaped body made of a thermoplastic resin is covered with a thermosetting resin layer formed by integrally bonding reinforcing long fibers, and the outer periphery of the thermosetting resin layer is further covered with a thermoplastic resin layer, and at least one of the thermoplastic resins constituting the central rod-shaped body and the outer layer is formed from a thermoplastic resin that has chemical affinity with the thermoplastic resin that is the matrix component constituting the intermediate layer.

[0004] Also, for example, Patent Document 2 discloses a three-layer rod-shaped body that is characterized by being integrally molded with a core made of a polymer foam having a specific gravity of 1 or less, a reinforced plastic layer made of glass fiber and thermosetting resin provided on the outside of the core, and a coating layer made of synthetic resin provided on the outside of the reinforced plastic layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Jitszen No. 53-24376 [Patent Document 2] Japanese Utility Model Application Publication No. 60-184628 Summary of the Invention [Problem to be solved by the invention]

[0006] However, the conventional technology has problems such as water infiltration and filling the core when used in marine and water treatment fields, reducing buoyancy and causing sinking. Therefore, there is a need for further improvements to the conventional technology.

[0007] In view of the above circumstances, a main object of the present invention is to provide a fiber-reinforced composite material with improved quality and a method for producing the same. [Means for solving the problem]

[0008] As a result of intensive experimental investigation, the inventors of the present application discovered that by providing a skin layer on the core of a fiber-reinforced composite and further controlling the thickness of the skin layer within a specific range, a fiber-reinforced composite with improved quality and a method for producing the same can be obtained, and thus completed the present invention.

[0009] That is, the present invention provides a fiber-reinforced composite comprising at least a core made of a thermoplastic resin, an intermediate layer formed by integrally bonding reinforcing fibers impregnated with resin to the outer periphery of the core, and an outer layer made of a thermoplastic resin covering the intermediate layer, wherein the core is made of a resin foam that is partially or entirely independent, and the thickness of a skin layer formed on part or all of the outer periphery of the core is 3 μm or more and 30% or less of the diameter of the core. The core may have a closed cell ratio of 50% or more. The fiber-reinforced composite body according to the present invention may have an apparent specific gravity of less than 1.

[0010] The present invention also provides a method for producing a fiber-reinforced composite comprising at least a core made of a thermoplastic resin, an intermediate layer formed by integrally bonding reinforcing fibers impregnated with resin to the outer periphery of the core, and an outer layer made of a thermoplastic resin covering the intermediate layer, wherein the core is made of a resin foam that is partially or entirely independent, and the thickness of a skin layer formed on part or all of the outer periphery of the core is 3 μm or more and 30% or less of the diameter of the core, and the method for producing a fiber-reinforced composite includes at least the steps of forming the skin layer and adjusting the thickness of the formed skin layer. Effect of the Invention

[0011] According to the present invention, it is possible to provide a fiber-reinforced composite body and a manufacturing method thereof with improved quality. Note that the effects described here are not necessarily limited to those described herein, and may be any of the effects described in this specification. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a reference end view showing one embodiment of a fiber-reinforced composite body 1 according to the present invention. [Diagram 2] FIG. 2 is a schematic conceptual diagram showing one embodiment of the production line 2. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the drawings. The embodiment described below is merely one example of a typical embodiment of the present invention, and the scope of the present invention should not be construed as being narrow.

[0014] 1. Fiber-reinforced composite 1 1 is a reference end view showing one embodiment of a fiber-reinforced composite 1 according to the present invention. The fiber-reinforced composite 1 according to the present invention (hereinafter also simply referred to as "composite 1 according to the present invention") includes at least a core 11, an intermediate layer 12, and an outer layer 13. Furthermore, it is possible to provide a plurality of intermediate layers 12 and outer layers 13 as necessary.

[0015] Furthermore, in the fiber-reinforced composite 1 of the present invention, the core 11 is made of a resin foam having independent bubbles in part or in whole, and the thickness of the skin layer 111 formed on part or all of the outer peripheral surface of the core 11 is 3 μm or more and 30% or less of the diameter of the core.

[0016] The composite 1 according to the present invention has improved quality as compared with the conventional technology, as shown in the examples described later, and is therefore expected to be used as an alternative material to metal articles in a wide range of fields, such as automobile parts, electronic parts, agricultural and forestry materials, building materials, furniture, marine materials, water treatment materials, etc. It is also expected to be used as a filament material for 3D printers, molded products using the material, etc.

[0017] The apparent specific gravity of the composite 1 according to the present invention is preferably less than 1, more preferably less than 0.9, and even more preferably less than 0.8. When the apparent specific gravity of the composite 1 according to the present invention is less than 1, the lightweight nature of the composite 1 according to the present invention can be ensured. When used for applications such as marine materials and water treatment materials, sufficient buoyancy can be obtained. The apparent specific gravity can be, for example, 0.15 or more, 0.2 or more, or 0.3 or more.

[0018] The shape of the composite 1 according to the present invention may be, for example, a substantially cylindrical shape or a substantially polygonal tubular shape. "Substantially cylindrical" specifically refers to a shape whose cross section is a circle or a flat shape such as an ellipse. "Substantially polygonal tubular" specifically refers to a shape whose cross section is a polygon such as a triangle or a rectangle. Each part will be described in detail below.

[0019] (1) Core 11 In the present invention, the core 11 is made of a thermoplastic resin and is a resin foam in which part or all of the thermoplastic resin is an independent bubble. In this specification, the term "independent bubble" refers to a state in which each bubble is independent and not connected to other bubbles.

[0020] In the present invention, the independent cell ratio in the resin foam is preferably 50% or more, more preferably 55% or more, and even more preferably 60% or more. With an independent cell ratio of 50% or more, it is expected that the resin foam will recover from stress applied during molding, and the composite 1 according to the present invention can have a compressive stress. Furthermore, it is possible to prevent a decrease in buoyancy when used in the marine field, water treatment field, and the like. The independent cell ratio in the resin foam may be 100% or less, or may be 95% or less from the viewpoint of ease of production. The independent cell ratio in the resin foam can be measured, for example, by the method shown in the examples described later.

[0021] The specific gravity of the core 11 is preferably 0.7 or less, more preferably 0.65 or less, and even more preferably 0.6 or less. By making the specific gravity of the core 11 0.7 or less, the lightweight nature of the composite 1 according to the present invention can be ensured. When used for marine materials, water treatment materials, and the like, sufficient buoyancy can be obtained. In addition, the apparent specific gravity can be, for example, 0.01 or more, or 0.015 or more.

[0022] In the present invention, the expansion ratio of the resin foam is preferably 1.3 or more, and more preferably 1.5 or more. When the expansion ratio is 1.3 or more, a fiber-reinforced composite 1 having excellent light weight can be provided. Furthermore, the expansion ratio of the resin foam is preferably 100 or less, more preferably 75 or less, and even more preferably 50 or less. When the expansion ratio is 100 or less, moldability can be improved. The expansion ratio of the resin foam can be calculated, for example, by dividing the weight of the obtained resin foam by the volume determined by the water throwing method to determine the density.

[0023] In the present invention, in the resin foam, the average cell diameter in the cross-sectional direction of the cell cells 112 forming the closed cells is preferably 10 μm or more, more preferably 50 μm or more. By having an average cell diameter of 10 μm or more, a fiber-reinforced composite 1 having superior light weight can be provided. In addition, the average cell diameter in the cross-sectional direction of the cell cells 112 is preferably 500 μm or less, more preferably 450 μm or less. By having an average cell diameter of 500 μm or less, moldability can be improved. The average cell diameter of the cell cells 112 can be measured, for example, in accordance with ASTM D3576-3577. The average cell diameter in the length direction can be set appropriately.

[0024] In the present invention, the closed cell ratio in the resin foam is preferably 50% or more, and more preferably 55% or more. When the closed cell ratio is 50% or more, a fiber-reinforced composite 1 having superior light weight can be provided. Furthermore, the closed cell ratio in the resin foam is preferably 100% or less, and more preferably 90% or less. When the closed cell ratio is 100% or less, moldability can be improved. The closed cell ratio in the resin foam can be measured, for example, in accordance with ASTM D 2856.

[0025] <Resin foam> In this specification, the term "resin foam" refers to a foamed thermoplastic resin composition containing at least a thermoplastic resin and a foaming agent. In the present invention, a part or the whole of the core 11 is formed of a resin foam, but it is preferable that the central portion is made of a thermoplastic resin and the periphery is covered with a resin foam.

[0026] Examples of thermoplastic resins include polyester-based resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PENp), and liquid crystal polyester (LCP); polyimide-based resins; polyolefin-based resins such as polypropylene (PP), polyethylene (PE), and polyisobutylene (PB); styrene-based resins such as polystyrene (PS), acrylonitrile-styrene resin (AS), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-acrylic-styrene resin (AAS), and acrylonitrile-ethylene propylene rubber-styrene (AES); polyphenylene ether-based resins; polyamide-based resins; polycarbonate-based resins; polyarylate-based resins; polyphenylsulfone-based resins; polysulfone-based resins; polyethersulfone-based resins, etc. Two or more of these may be used in combination.

[0027] In the present invention, among these, styrene-based resins are preferred as the thermoplastic resin, and among styrene-based resins, polystyrene and acrylonitrile-butadiene-styrene resins are preferred because these thermoplastic resins have excellent adhesion to the intermediate layer 12 described below.

[0028] Examples of the foaming agent include physical foaming agents and chemical foaming agents, and from the viewpoint of productivity, the chemical foaming agents are preferred. Examples of chemical foaming agents include organic chemical foaming agents and inorganic chemical foaming agents. Examples of organic chemical foaming agents include azodicarbonamide, hydrazodicarbonamide, azodicarboxylate barium salt, dinitrosopentaethylenetetramine, nitrosoguanidine, 4,4'-oxybis(benzenesulfonic acid hydrazide), trihydrazine symmetric triazine, barium azodicarboxylate, azobisisobutyronitrile, and toluenesulfonyl hydrazide. Examples of inorganic chemical foaming agents include sodium hydrogen carbonate, sodium carbonate, zinc carbonate, ammonium hydrogen carbonate, ammonium carbonate, and ammonium nitrite. Examples of physical foaming agents include air, oxygen, nitrogen, carbon dioxide, ethane, propane, n-butane, isobutane, n-pentane, isopentane, n-hexane, isohexane, cyclohexane, heptane, ethylene, propylene, water, petroleum ether, methyl chloride, ethyl chloride, monochlorotrifluoromethane, dichlorodifluoromethane, and dichlorotetrafluoroethane. These foaming agents can be appropriately selected taking into consideration the type of thermoplastic resin used, the desired expansion ratio, etc., and in the present invention, two or more of these may be used in combination.

[0029] The content of the foaming agent is not particularly limited, but can be appropriately set in consideration of the type of foaming agent and thermoplastic resin used, the desired expansion ratio, etc. For example, the content is preferably 0.01 parts by mass or more and 10 parts by mass or less, and more preferably 0.05 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the thermoplastic resin.

[0030] In addition, the resin foam may contain other optional components such as a cell regulator, a stabilizer, an ultraviolet absorber, a colorant, an antioxidant, a crystallization promoter, a lubricant, a crosslinking agent, a surfactant, a shrinkage inhibitor, a flame retardant, and an anti-deterioration agent, but the present invention is not limited to these.

[0031] <Skin Layer 111> As described above, the present invention is characterized in that the thickness of skin layer 111 in core 11 is 3 μm or more and 30% or less of the diameter of the core. In this specification, the term "skin layer" refers to a region formed on a part or all of the outer circumferential surface of core 11, in which no air bubbles are generated.

[0032] If the skin layer 111 is absent or extremely thin, the core 11 may melt depending on the type of impregnating resin used to form the intermediate layer 12. Even if the independent foaming rate of the core 11 is high, the impregnating resin may penetrate into the core 11 and connect the bubbles. Furthermore, if the skin layer 111 is absent, the dimensional accuracy of the core 11 during molding is poor, and as a result, the conformity of the intermediate layer 12 and the outer layer 13 is poor, and the quality of the fiber-reinforced composite 1 is low. Furthermore, if the skin layer 111 is absent, the dimensional accuracy is low during the integral molding of the core 11, intermediate layer 12, and outer layer 13, and the stress of squeezing (compression) due to the reinforcing fibers impregnated in the resin, the amount of heat generated during curing, etc. become non-uniform, resulting in molding defects. In this specification, the term "impregnating resin" refers to a resin that impregnates reinforcing fibers.

[0033] The inventors of the present application also found that even if a skin layer 111 is present, if the thickness is less than 3 μm, the bubbles will be connected due to the erosion of the foamed region of the core 11 by the impregnated resin, making it difficult to form independent bubbles and resulting in poor moldability, while if the thickness exceeds 30% of the diameter of the core, the rate of bubbles in the core 11 will be low, resulting in poor moldability, and further, when used for applications such as marine materials and water treatment materials, there will be problems such as insufficient buoyancy. That is, in the composite 1 according to the present invention, a skin layer 111 is provided on the core 11, and further, the thickness of the skin layer 111 is controlled within the above-mentioned specific range, thereby succeeding in dramatically improving the quality.

[0034] In addition, in the present invention, the thickness of the skin layer 111 in the core 11 is 3 μm or more and 30% or less of the diameter of the core, but it is preferable that the thickness of the skin layer 111 is 5 μm or more and 25% or less of the diameter of the core.

[0035] (2) Middle Class 12 In the present invention, the intermediate layer 12 is a layer formed by integrally bonding reinforcing fibers impregnated with a resin to the outer periphery of the central core 11. In the embodiment shown in Fig. 1, the intermediate layer 12 is a single layer, but the present invention is not limited thereto, and multiple intermediate layers 12 may be provided as necessary.

[0036] Examples of the resin include thermoplastic resin and thermosetting resin. Reinforced fibers impregnated with thermoplastic resin are generally called fiber reinforced thermoplastic resin (FRTP). Reinforced fibers impregnated with thermosetting resin are generally called fiber reinforced plastic (FRP). In the present invention, any of these can be used as the material for forming the intermediate layer 12.

[0037] <Thermoplastic Resin Used in the Intermediate Layer 12> Examples of thermoplastic resins used as the matrix resin in the intermediate layer 12 include polyolefin resins such as polypropylene (PP), polyethylene (PE), and polyisobutylene (PB); polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PENp), and liquid crystal polyester (LCP); styrene resins such as polystyrene (PS), acrylonitrile-styrene resin (AS), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-acrylic-styrene resin (AAS), and acrylonitrile-ethylene propylene rubber-styrene (AES); urethane resins, etc. Other examples include polyvinyl alcohol (PVA), polyoxymethylene (POM), polyamide (PA), polycarbonate (PC), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyphenylene sulfide (PPS), polyphenylene ether (PPE), modified PPE, polyimide (PI), polyamideimide (PAI), polyetherimide (PEI), polysulfone (PSU), modified PSU, polyethersulfone (PES), polyketone (PK), polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyarylate (PAR), polyethernitrile (PEN), etc. In the present invention, two or more of these may be used in combination.

[0038] <Thermosetting Resin Used in the Intermediate Layer 12> Examples of the thermosetting resin used as the matrix resin in the intermediate layer 12 include unsaturated polyester resins (e.g., terephthalic acid resins, isophthalic acid resins, etc.), vinyl ester resins (e.g., epoxy acrylate resins, etc.), epoxy resins, thermosetting polyamide resins, phenolic resins, etc. In the present invention, two or more of these may be used in combination.

[0039] In the present invention, among these, thermosetting resins are particularly preferred as the material for forming the mid layer 12, and among thermosetting resins, unsaturated polyester resins and vinyl ester resins are preferred because thermosetting resins are preferred from the viewpoints of molding stability, ease of molding, and cost reduction.

[0040] <Reinforced fiber> The reinforcing fibers are preferably, for example, a base material having the form of a continuous long fiber bundle or a fiber braid (for example, a woven fabric, a knitted fabric, a braid, etc.), because the use of these ensures continuous impregnation and continuous formation of the outer layer 13, resulting in excellent productivity.

[0041] Examples of reinforcing fibers that can be used include organic fibers such as olefin fibers, aramid fibers, and liquid crystal polyester (LCP) fibers, glass fibers, inorganic fibers such as carbon fibers, ceramic fibers such as Tyranno fibers, metal fibers such as boron fibers, copper fibers, and stainless steel fibers, and amorphous fibers. In the present invention, mixed fabrics of these fibers can also be used.

[0042] In the present invention, among these, glass fiber and carbon fiber are particularly preferred as reinforcing fibers, because these fibers are compatible with the impregnating resin, and glass fiber is more preferred from the viewpoint of cost reduction.

[0043] As the glass fiber, for example, long fibers such as glass fiber monofilament, glass fiber strand, glass fiber roving, glass fiber yarn, etc., can be used. Among these, glass fiber roving and glass fiber yarn are particularly preferred as the glass fiber in the present invention. Also, glass fiber braids such as glass fiber woven fabrics, glass fiber braids, and glass fiber knitted fabrics can be used.

[0044] The glass fiber may be surface-treated with a surface treatment agent such as an epoxy silane coupling agent or an acrylic silane coupling agent. Examples of the glass composition of the glass fiber include E glass, S glass, and C glass. In the present invention, E glass is particularly preferred as the glass composition. The cross section of the glass fiber monofilament may be substantially circular or may be substantially flat, such as an ellipse.

[0045] There are three types of carbon fibers: "pitch-based" fibers made from coal tar pitch or petroleum pitch, "PAN-based" fibers made from polyacrylonitrile, and "rayon-based" fibers made from cellulose fibers. Any of these carbon fibers may be used in the present invention.

[0046] The diameter of the reinforcing fiber is not particularly limited, but is preferably 3 μm to 40 μm, more preferably 10 μm to 23 μm. If it is less than 3 μm, the number of reinforcing fibers used will increase, which will deteriorate the workability and increase the number of personnel required for preparation during molding, resulting in increased costs. If it exceeds 40 μm, it will lead to a decrease in impregnation and poor impregnation efficiency.

[0047] The number of reinforcing fibers used is not particularly limited, but the ratio of fibers in the intermediate layer 12 (Vf: fiber content) is preferably 20% to 80%, and more preferably 30% to 70%. If Vf is less than 20%, the intermediate layer 12 cannot maintain a predetermined shape, and the physical properties of the fiber-reinforced composite 1 are deteriorated. If Vf exceeds 80%, the frictional resistance between the reinforcing fibers and the drawing increases, and the compressive stress applied to the center core 11 during drawing increases, resulting in poor molding stability and molding efficiency.

[0048] The reinforcing fibers may be prepared by weaving, braiding, knitting, or the like to a desired length by a known method, or may be wound into a long length and used. The reinforcing fibers may be heated as necessary to increase the impregnation of the resin into the reinforcing fibers or to remove moisture from the reinforcing fibers.

[0049] The volume content of the reinforcing fibers (bundles) is preferably 20% to 80%, and more preferably 40% to 60%, of the entire intermediate layer 12. If the volume content is lower than 20%, the reinforcing effect of the reinforcing fibers is reduced. Conversely, if the volume content exceeds 80%, the amount of resin is small, which adversely affects the bending strength.

[0050] (3) Outer layer 13 The outer layer 13 is a layer made of a thermoplastic resin and covers the intermediate layer 12. In the embodiment shown in Fig. 1, the outer layer 13 is a single layer, but the present invention is not limited to this, and multiple outer layers 13 may be provided as necessary.

[0051] <Thermoplastic Resin Used in Outer Layer 13> Examples of thermoplastic resins used in the outer layer 13 include polyolefin resins such as polypropylene (PP), polyethylene (PE), and polyisobutylene (PB); polyester resins such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polytrimethylene terephthalate (PTT), polyethylene naphthalate (PENp), and liquid crystal polyester (LCP); styrene resins such as polystyrene (PS), acrylonitrile-styrene resin (AS), acrylonitrile-butadiene-styrene resin (ABS), acrylonitrile-acrylic-styrene resin (AAS), and acrylonitrile-ethylene propylene rubber-styrene (AES); urethane resins, etc. Other examples include polyvinyl alcohol (PVA), polyoxymethylene (POM), polyamide (PA), polycarbonate (PC), polymethyl methacrylate (PMMA), polyvinyl chloride (PVC), polyphenylene sulfide (PPS), polyphenylene ether (PPE), modified PPE, polyimide (PI), polyamideimide (PAI), polyetherimide (PEI), polysulfone (PSU), modified PSU, polyethersulfone (PES), polyketone (PK), polyetherketone (PEK), polyetheretherketone (PEEK), polyetherketoneketone (PEKK), polyarylate (PAR), polyethernitrile (PEN), etc. In the present invention, two or more of these may be used in combination.

[0052] Among these, in the present invention, polyethylene and acrylonitrile-butadiene-styrene resin are particularly preferred as the thermoplastic resin from the viewpoints of cost reduction, moldability, and physical properties.

[0053] 2. Manufacturing method of fiber-reinforced composite 1 2 is a schematic conceptual diagram showing one embodiment of the production line 2. The production method according to the present invention is a method for producing the above-mentioned fiber-reinforced composite 1, which includes at least the steps of forming the skin layer 111 and adjusting the thickness of the formed skin layer 111. Other steps may also be performed as necessary. The production method according to the present invention will now be described in detail with reference to FIG.

[0054] (1) A process for making the reinforcing fibers recoverable The required number of long fiber-like reinforcing fibers 23 are inserted into predetermined guide holes in a collective guide, and passed through a production line 2 consisting of an impregnation operation guide in an impregnation tank 24, a squeeze 26 for vertically aligning the fibers in a predetermined arrangement around the outer periphery of the core 11, and a melt extruder 27 for the outer layer 13, etc., to prepare the reinforcing fibers (bundles) 23 for collection.

[0055] (2) Injecting the resin composition When the impregnating resin is a thermosetting resin, a liquid curable resin composition containing a thermosetting resin and a thermosetting agent is poured into the impregnation tank 24. On the other hand, when the impregnating resin is a thermoplastic resin, a thermoplastic resin that has been molten by applying heat, or a thermoplastic resin that has been liquefied by adding a solvent is poured into the impregnation tank 24.

[0056] (3) A step of forming the core 11 (including a step of forming a skin layer 111 and adjusting the thickness of the formed skin layer 111). To form the core 11, a thermoplastic resin composition containing a thermoplastic resin, a foaming agent, and, if necessary, other optional components is continuously extruded from a melt extruder 21 for the core 11 into a cylindrical shape of specified dimensions, which is continuously withdrawn and cooled in a cooling tank 22 for the core 11, thereby forming the core 11 consisting of a resin foam partly or entirely of which are independent bubbles.

[0057] At this time, a temperature gradient in a generally L-shape is applied from the inlet side to the outlet side of the melt extruder 21 for the core 11. This forms a skin layer 111, and the thickness of the skin layer 111 can be adjusted by adjusting the degree of the temperature gradient. As the temperature gradient, for example, the temperature can be increased from the melting temperature to the foaming agent decomposition temperature, and the temperature can be decreased from the foaming agent decomposition temperature to the melting temperature.

[0058] Specifically, the temperature is preferably set to 40°C≦maximum temperature−minimum temperature≦90°C. That is, for example, when the inlet and outlet of the melt extruder are set to 190°C (minimum temperature), the maximum temperature is set in the range of 230°C to 280°C. By setting the temperature at 40°C or higher, the gas can be prevented from escaping and efficient foaming can be achieved, and it is possible to prevent the skin layer 111 from being formed thinner than the intended thickness of the skin layer 111. By setting the temperature at 90°C or lower, it is possible to prevent the skin layer 111 from becoming thicker and to avoid a situation in which the friction with the die becomes too large to extrude the layer. Furthermore, the gas generated during the melt-kneading of the thermoplastic resin and the foaming agent in the cylinder does not escape from the inlet and outlet of the melt extruder 21 for the core 11, so that the cell cells 112 can be efficiently formed and foamed at a desired independent foaming rate.

[0059] (4) forming an uncured tubular article While taking up the prepared reinforcing fibers 23, an impregnation operation guide is lowered into the impregnation tank 24, and the reinforcing fibers 23 are impregnated with the thermoplastic resin composition or thermosetting resin composition. This is then vertically attached to the outer periphery of the core 11 running through the center of the hole of the constriction 26, and the excess resin composition is gradually squeezed out by the constriction 26. The reinforcing fibers 23 are vertically attached to the core 11, and an uncured tubular object provided with an uncured intermediate layer 12 is formed.

[0060] (5) Melt-coating the outer layer 13 The uncured tubular product is passed through a crosshead of a melt extruder 27 for the outer layer 13, extrusion-coated into a circular shape with a thermoplastic resin that forms the outer layer 13, and then cooled in a cooling tank 28 for the outer layer 13, thereby melt-coating the product.

[0061] (6) Step of obtaining fiber-reinforced composite 1 When a thermosetting resin is used as the impregnating resin, the uncured tubular article coated with a thermoplastic resin is introduced into a curing tank 29 to thermally cure the uncured thermosetting resin composition inside, and then cooled in a cooling tank 30 for the fiber-reinforced composite 1 to obtain a fiber-reinforced composite 1 in which the layers are closely and integrally formed. When a thermoplastic resin is used as the impregnating resin, the curing tank 29 is not necessary, and the fiber-reinforced composite 1 in which the layers are closely and integrally formed can be obtained by cooling in a cooling tank 30 for the fiber-reinforced composite 1.

[0062] The obtained fiber-reinforced composite 1 may be taken up by a take-up machine 31 or the like, as necessary. The taken-up fiber-reinforced composite 1 may be cut to a predetermined length by a cutter 32 or the like. EXAMPLES

[0063] The present invention will now be described in further detail with reference to examples. The embodiment described below is merely a representative example of the present invention, and the scope of the present invention should not be construed as being narrow.

[0064] <Manufacturing of fiber-reinforced composites> The raw materials used in the production are listed below. Thermoplastic resin of the core: ABS resin (Toyolac (registered trademark) 600-309N, manufactured by Toray Industries, Inc.) Reinforced fiber in the middle layer: Glass fiber (Nitto Boseki Co., Ltd., (2200tex) RS220RL-510AH) Impregnating resin: Unsaturated polyester resin (manufactured by Japan U-PICA Corporation, U-PICA (registered trademark) 3464) Thermoplastic resin of outer layer: ABS resin (Toyolac (registered trademark) 600-309N, manufactured by Toray Industries, Inc.) Foaming agent: Chemical foaming agent (Panslen HB27A, manufactured by Eiwa Chemical Industry Co., Ltd.)

[0065] The fiber-reinforced composites according to Examples 1 to 6 have the same structure as the embodiment shown in Fig. 1, and were produced by a method similar to the production method according to the present invention described above. The fiber-reinforced composites according to Comparative Examples 1 and 2 have the same structure as the embodiment shown in Fig. 1, but the thickness of the skin layer is outside the range of the present invention, and were produced by a method similar to the production method according to the present invention described above, except that the thickness of the skin layer was adjusted outside the range of the present invention in the production method according to the present invention described above.

[0066] <Evaluation> Each of the produced fiber-reinforced composites was evaluated for skin layer thickness, independent cell ratio, roundness, and whether or not it floats on water.

[0067] Skin thickness Measurements were taken from the cross section (direction perpendicular to the longitudinal direction) using a microscope (Keyence, VHX-5000). At any given location, a virtual circle representing the outer diameter of the core and a virtual circle at the interface of the skin layer were drawn at a magnification of 30, and the average value was calculated from the difference at any five points.

[0068] [Independent foaming rate] First, the open cell ratio was calculated by the following method. Three samples with a length of 2 cm in the longitudinal direction were randomly cut from each core, and their weights (weight before immersion) were measured. Next, the samples were immersed in water and left for 3 minutes under a vacuum of 0.09 MPa or less, and then removed. After that, the moisture on the surface and cross section was thoroughly wiped off, and the weights of the samples (weight after immersion) were measured. The open cell ratio (%) was then calculated from the following formula (1). F1={(Mm) / [m×(f-1) ] / S0}×100...(1) F1: Open cell rate (%) M: Weight after soaking (g) m: Weight before soaking (g) f: Foaming ratio S0: Specific gravity of the solid component of the core

[0069] Next, based on the obtained open cell ratio, the closed cell ratio (%) was calculated according to the following formula (2). F2 = 100 - F1 (2) F2: Closed bubble rate (%) F1: Open cell rate (%)

[0070] [Circularity] Measurements were taken from the cross section (direction perpendicular to the longitudinal direction) using a microscope (Keyence, VHX-5000). Specifically, measurements were taken five times at three different points on the cross section at a position 10 mm from the end of the fiber-reinforced composite. Three points on the measured circle (three points selected by dividing 360 degrees into thirds) were then approximated as a perfect circle, and the diameter was calculated. The circularity was calculated from the difference between the maximum and minimum diameters of the five points obtained, and the circularity was calculated by dividing the circularity by the diameter of the fiber-reinforced composite.

[0071] To evaluate moldability, the circularity was calculated from the following formula (3) and evaluated as follows. Circularity = circularity ÷ diameter of fiber-reinforced composite × 100 (3) 〇: Circularity is 90% or more ×: Circularity is less than 90%

[0072] [Does it float on water?] The fiber-reinforced composite was placed in a 30 cm deep water tank (water temperature: 18°C) with the outer layer side in contact with the bottom, and after 3 minutes it was placed in water and visually confirmed whether it floated.

[0073] The evaluation of whether or not the sample floated on water was carried out as follows. 〇: The fiber-reinforced composite comes into contact with the water surface at least partially within 30 seconds △: Fiber-reinforced composite comes into contact with the water surface at least partially for more than 30 seconds within 3 minutes ×: No part of the fiber-reinforced composite comes into contact with the water surface within 3 minutes

[0074] <Evaluation> The evaluation results are shown in Tables 1 and 2 below.

[0075] [Table 1]

[0076] [Table 2]

[0077] <Consideration> The fiber-reinforced composites of Examples 1 to 6 had improved quality compared to the fiber-reinforced composites of Comparative Example 1 and Comparative Example 2. Specifically, it was found that the fiber-reinforced composites of Examples 1 to 6 had excellent designability due to good roundness, and could be used without problems in applications such as marine materials and water treatment materials due to their floating properties. Therefore, it was found that a fiber-reinforced composite with improved quality can be provided by providing a fiber-reinforced composite having at least a core made of a thermoplastic resin, an intermediate layer formed by integrally bonding reinforcing fibers impregnated with a resin to the outer periphery of the core, and an outer layer made of a thermoplastic resin that covers the intermediate layer, the core being made of a resin foam that is partially or entirely independent foam, and the thickness of the skin layer formed on a part or all of the outer periphery of the core being 3 μm or more and 30% or less of the diameter of the core. [Industrial Applicability]

[0078] According to the present invention, it is possible to provide a fiber-reinforced composite and a manufacturing method thereof with improved quality. Therefore, the fiber-reinforced composite 1 according to the present invention is expected to be used more than ever before in a wide range of fields, such as automobile parts, electronic parts, agricultural and forestry materials, building materials, furniture, marine materials, and water treatment materials, as a material to replace metal articles. It is also expected to be used as a filament material for 3D printers, a molded body using the material, and the like. [Explanation of symbols]

[0079] 1: Fiber-reinforced composite 11: Core 111: Skin layer 112: Bubble cell 12: Middle class 13: Outer layer 2: Production line 21: Melt extruder for core 11 22: Cooling tank for core 11 23: Reinforced fiber 24: Impregnation tank 25: Resin-impregnated reinforcement fiber 26: Aperture 27: Melt extruder for outer layer 13 28: Cooling tank for outer layer 13 29:Curing tank 30: Cooling tank for fiber-reinforced composite 1 31: Pick-up machine 32: Cutting machine

Claims

1. A core made of a thermoplastic resin; An intermediate layer formed by integrally bonding reinforcing fibers impregnated with resin to the outer periphery of the core; an outer layer covering the intermediate layer and made of a thermoplastic resin; At least The core is made of a resin foam that is partially or entirely closed-celled, A fiber-reinforced composite, wherein a skin layer formed on all or part of the outer peripheral surface of the core has a thickness of 3 μm or more and 30% or less of the diameter of the core.

2. 2. The fiber-reinforced composite according to claim 1, wherein the core has a closed cell ratio of 50% or more.

3. 3. The fiber-reinforced composite according to claim 1 or 2, having an apparent specific gravity of less than 1.

4. A method for producing a fiber-reinforced composite comprising at least a core made of a thermoplastic resin, an intermediate layer formed by integrally bonding reinforcing fibers impregnated with a resin to an outer periphery of the core, and an outer layer made of a thermoplastic resin and covering the intermediate layer, the core being made of a resin foam partly or entirely formed as an independent bubble, and a skin layer formed on a part or entirely of an outer periphery of the core having a thickness of 3 μm or more and 30% or less of a diameter of the core, forming the skin layer and adjusting the thickness of the formed skin layer; A method for producing a fiber-reinforced composite, comprising at least the steps of:

Citation Information

Patent Citations

  • A three-layer structure composed of a reinforced plastic stick

    JP1978024376U

  • A three-layer structure of bar

    JP1985184628U