Method for manufacturing polyvinyl chloride paste resin, plastisol composition, vinyl chloride sheet, and vinyl chloride foam

By adding polyoxyethylene styrenated phenyl ether during polymerization, plastisol viscosity is reduced, addressing handling challenges and improving thermal stability in polyvinyl chloride paste resin production.

JP2024140905AInactive Publication Date: 2024-10-10KANEKA CORP
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2023052270
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Conventional methods for reducing the viscosity of plastisol in polyvinyl chloride paste resin production are inadequate, leading to handling difficulties due to high viscosity.

Method used

Incorporating polyoxyethylene styrenated phenyl ether during polymerization at a conversion rate of 80% or less, specifically in the range of 20% to 60%, to reduce plastisol viscosity by suppressing the formation of low molecular weight polymers.

Benefits of technology

Significantly reduces plastisol viscosity, improves handling, and enhances thermal stability while maintaining cost-effectiveness.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140905000001
    Figure 2024140905000001
  • Figure 2024140905000002
    Figure 2024140905000002
Patent Text Reader

Abstract

To provide a polyvinyl chloride paste resin with which a lower viscosity of plastisol obtained can be achieved when manufacturing plastisol.SOLUTION: The problem can be solved by a manufacturing method of continuing polymerization by adding 0.05-1.5 pts.wt. of polyoxyethylene styrenated phenyl ether with respect to 100 pts.wt. of a monomer in a period of time during which a polymerization conversion rate is 80% or less in homopolymerization of vinyl chloride monomer, or copolymerization of vinyl chloride monomer and other ethylene-based unsaturated monomer.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing a polyvinyl chloride paste resin, a plastisol composition, a vinyl chloride sheet, and a vinyl chloride foam. [Background technology]

[0002] Polyvinyl chloride paste resins are mixed with appropriate amounts of compounding agents, such as plasticizers, stabilizers, fillers, foaming agents, and pigments, as needed, and then mixed and kneaded to form a fluid called plastisol, which is then processed into molded articles. However, plastisols containing these compounding agents generally have high viscosity, and after the plastisol is prepared in a mixer or the like, it tends to be difficult to handle, for example, it is difficult to remove from the mixer and transport.

[0003] For this reason, a commonly known method for reducing the viscosity of plastisol involves adding one or more anionic emulsifiers, such as alkali metal salts of higher alcohol sulfates or alkali metal salts of alkylbenzenesulfonic acids, or nonionic emulsifiers, such as polyoxyethylene alkyl ethers, sorbitan esters, or glycerin alkyl esters, to a polyvinyl chloride aqueous dispersion obtained after polymerization, followed by drying to obtain a polyvinyl chloride paste resin. Another technique for reducing the viscosity of plastisol has been disclosed, which involves adding a polyoxyethylene alkyl phenyl ether to the polymerization system after an anionic emulsifier has been added thereto, before the polymerization yield reaches 80% (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Publication No. 55-60504 Summary of the Invention [Problem to be solved by the invention]

[0005] Although the above-mentioned conventional techniques are excellent as techniques for reducing the viscosity of plastisol, there is still room for improvement in terms of further reducing the viscosity of plastisols.

[0006] An aspect of the present invention is to provide a polyvinyl chloride paste resin that can further reduce the viscosity of the resulting plastisol when it is produced. [Means for solving the problem]

[0007] As a result of intensive research to solve the above-mentioned problems, the present inventors have surprisingly found that when a predetermined amount of polyoxyethylene styrenated phenyl ether is added to a polymerization system while the polymerization conversion rate is not yet 80%, and the polymerization is continued, the viscosity of the resulting plastisol containing a polyvinyl chloride paste resin can be further reduced, and have thus completed the present invention.

[0008] That is, one embodiment of the present invention includes the following configuration.

[0009] [1] A method for producing a polyvinyl chloride paste resin, comprising a polymerization step of homopolymerizing a vinyl chloride monomer or copolymerizing a vinyl chloride monomer with another ethylenically unsaturated monomer, and a step of continuing the polymerization by adding 0.05 to 1.5 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of the monomer during a period when the polymerization conversion rate is 80% or less.

[0010] [2] The production method according to [1], wherein the amount of the polyoxyethylene styrenated phenyl ether added is 0.1 to 0.3 parts by weight per 100 parts by weight of the monomer.

[0011] [3] A plastisol composition comprising a polyvinyl chloride paste resin, a plasticizer, and a filler, produced by the production method according to [1] or [2].

[0012] [4] The plastisol composition according to [3], which contains calcium carbonate as the filler, and contains 100 parts by weight or more of the calcium carbonate per 100 parts by weight of the polyvinyl chloride paste resin.

[0013] [5] The plastisol composition according to [3] or [4], further comprising a chemical foaming agent.

[0014] [6] A vinyl chloride sheet made using the plastisol composition according to [3] or [4].

[0015] [7] A vinyl chloride foam obtained by using the plastisol composition according to [5]. [Effects of the Invention]

[0016] According to one aspect of the present invention, it is possible to provide a polyvinyl chloride paste resin that can realize a further reduction in viscosity of the resulting plastisol when it is produced. DETAILED DESCRIPTION OF THE INVENTION

[0017] One embodiment of the present invention will be described below, but the present invention is not limited thereto. The present invention is not limited to the respective configurations described below, and various modifications are possible within the scope of the claims. Furthermore, embodiments or examples obtained by combining the technical means disclosed in different embodiments or examples are also included in the technical scope of the present invention. All academic literature and patent documents described in this specification are incorporated herein by reference. Furthermore, unless otherwise specified in this specification, "A to B" representing a numerical range means "greater than or equal to A (including A and greater than A) and less than or equal to B (including B and less than B)."

[0018] Unless otherwise specified in this specification, the polymerization mode of the copolymer is not particularly limited, and the copolymer may be a random copolymer, a block copolymer, or a graft copolymer.

[0019] 1. Technical Concept of One Embodiment of the Present Invention In the course of investigations to solve the above-mentioned problems, the present inventors discovered that when a predetermined amount of polyoxyethylene styrenated phenyl ether was added to a polymerization system before the polymerization conversion rate reached 80%, and the polymerization was continued, the viscosity of the resulting plastisol containing a polyvinyl chloride paste resin could be further reduced significantly compared to the case where polyoxyethylene alkyl phenyl ether disclosed in Patent Document 1 was added.

[0020] Since polyoxyethylene styrenated phenyl ether has a lipophilic group and a hydrophilic group, it is thought that it cuts the surface interactions between particles of the polyvinyl chloride paste resin obtained by polymerization, and between the particles of the polyvinyl chloride paste resin and other components, thereby reducing the viscosity of the plastisol. Such an effect is also thought to be obtained by the polyoxyethylene alkyl phenyl ether added in the plastisol viscosity-reducing technology disclosed in Patent Document 1.

[0021] The reason why the addition of polyoxyethylene styrenated phenyl ether significantly reduces the viscosity of the plastisol compared to the addition of polyoxyethylene alkyl phenyl ether, a conventional technology, is unclear; however, it is believed that the presence of multiple phenyl groups in polyoxyethylene styrenated phenyl ether plays a role. One possible cause of the increased viscosity of the plastisol is the formation of low-molecular-weight polymers due to side reactions that occur before a polymerization conversion rate of 80%. That is, when polymerization progresses to a polymerization conversion rate of 70% to 80%, the amount of vinyl chloride monomer present in the polymerization system decreases. If radicals continue to be generated from the polymerization initiator under these conditions, the amount of radicals relative to the vinyl chloride monomer becomes excessive, resulting in the formation of low-molecular-weight polymers. The presence of multiple phenyl groups in polyoxyethylene styrenated phenyl ether is thought to effectively suppress the reaction of the generated radicals and reduce the generation of low-molecular-weight polymers. This reduction in low-molecular-weight polymers is therefore presumably responsible for the reduced viscosity.

[0022] 2. Method for producing polyvinyl chloride paste resin (2-1. Homopolymerization of vinyl chloride monomer or copolymerization of vinyl chloride monomer with other ethylenically unsaturated monomers) In a method for producing a polyvinyl chloride paste resin according to one embodiment of the present invention (hereinafter sometimes referred to as "the present production method"), the polyvinyl chloride paste resin is produced by homopolymerizing a vinyl chloride monomer or copolymerizing a vinyl chloride monomer with another ethylenically unsaturated monomer. That is, the present production method includes a polymerization step of homopolymerizing a vinyl chloride monomer or copolymerizing a vinyl chloride monomer with another ethylenically unsaturated monomer.

[0023] The polymerization method employed in the present production method is not particularly limited as long as it is a polymerization method using an emulsifier, but is preferably emulsion polymerization, fine suspension polymerization, seed emulsion polymerization, seed fine suspension polymerization, etc., and among these, seed emulsion polymerization is preferably used.

[0024] The other ethylenically unsaturated monomer is not particularly limited as long as it is an ethylenically unsaturated monomer copolymerizable with vinyl chloride monomer, and examples thereof include olefins such as ethylene, propylene, and butene; vinyl esters such as vinyl acetate, vinyl propionate, and vinyl stearate; vinyl ethers such as methyl vinyl ether, ethyl vinyl ether, octyl vinyl ether, and lauryl vinyl ether; vinylidenes such as vinylidene chloride; unsaturated carboxylic acids and their anhydrides such as acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, maleic anhydride, and itaconic anhydride; unsaturated carboxylic acid esters such as methyl acrylate, ethyl acrylate, monomethyl maleate, dimethyl maleate, and butylbenzyl maleate; aromatic vinyl compounds such as styrene, α-methylstyrene, and divinylbenzene; unsaturated nitriles such as acrylonitrile; and crosslinkable monomers such as diallyl phthalate. These other ethylenically unsaturated monomers may be used alone or in combination of two or more.

[0025] When copolymerizing vinyl chloride monomer with other ethylenically unsaturated monomers, the amount of vinyl chloride monomer used relative to the total amount of monomers is preferably 50 mol % or more, more preferably 70 mol % or more, even more preferably 80 mol % or more, and particularly preferably 90 mol % or more.

[0026] In the present production method, the polymerization temperature when the polymerization is carried out is not particularly limited, but is usually 40° C. to 70° C. The pressure when the polymerization is carried out is also not particularly limited, but is usually 0.50 MPa to 1.20 MPa.

[0027] (2-2. Addition of polyoxyethylene styrenated phenyl ether) This production method includes a step of adding 0.05 to 1.5 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of the monomer during the polymerization step of homopolymerizing vinyl chloride monomer or copolymerizing vinyl chloride monomer with another ethylenically unsaturated monomer while the polymerization conversion rate is 80% or less, thereby continuing the polymerization. This allows for even lower viscosity of the resulting plastisol when it is produced.

[0028] Furthermore, by adding polyethylene styrenated phenyl ether during polymerization, the amount of one or more anionic or nonionic emulsifiers added to the polyvinyl chloride aqueous dispersion obtained after polymerization to reduce the viscosity of the plastisol can be reduced, thereby improving heat resistance and reducing costs. Furthermore, compared to the conventional technology of adding polyoxyethylene alkyl phenyl ether during polymerization, adding a small amount of polyethylene styrenated phenyl ether can further reduce the viscosity of the plastisol, allowing for a reduction in the amount added, thereby improving heat resistance, suppressing bleeding, and reducing costs. In addition, the viscosity-reducing effect can be achieved even when the plastisol contains compounding agents such as calcium carbonate.

[0029] The polyoxyethylene styrenated phenyl ether may, for example, be a compound represented by the following formula (1):

[0030] [ka]

[0031] In the formula (1), n ​​is 4 to 120, more preferably 9 to 22, and even more preferably 12 to 14.

[0032] The polyoxyethylene styrenated phenyl ether may be polyoxyethylene monostyrenated phenyl ether, polyoxyethylene distyrenated phenyl ether, polyoxyethylene tristyrenated phenyl ether, or a mixture of two or more of these, which are represented by formula (1). The polyoxyethylene styrenated phenyl ether may also be one or more selected from polyoxyethylene monostyrenated phenyl ether, polyoxyethylene distyrenated phenyl ether, and polyoxyethylene tristyrenated phenyl ether, each of which may be a mixture of a plurality of compounds having different numbers of n.

[0033] In the present production method, polyoxyethylene styrenated phenyl ether may be added during a period when the polymerization conversion rate is 80% or less, but more preferably, polyoxyethylene styrenated phenyl ether is added during a period when the polymerization conversion rate is 20% to 80%, and even more preferably, during a period when the polymerization conversion rate is 40% to 60%.

[0034] Adding polyoxyethylene styrenated phenyl ether during the period when the polymerization conversion rate is 20% or more has the advantage that the viscosity of the resulting plastisol can be further reduced when the plastisol is produced.

[0035] The polyoxyethylene styrenated phenyl ether may be added all at once, may be added in several divided portions, or may be added continuously.

[0036] Here, the percentage of polymerization conversion at that point can be calculated, for example, by removing the reaction mixture present in the polymerization vessel at that point, removing the remaining monomer by vaporization, measuring the solids concentration of the resulting polyvinyl chloride aqueous dispersion, and dividing this by the theoretical solids concentration assuming that all of the added monomers have polymerized.The solids concentration of the polyvinyl chloride aqueous dispersion can be calculated using the following formula based on weight data obtained by the following operations.

[0037] A certain amount of polyvinyl chloride aqueous dispersion is poured into an aluminum container whose weight (w1) has been measured in advance, and after measuring the weight (w2), the container is dried for 1 hour in a dryer at 120°C. The weight (w3) of the aluminum container containing the dried solid content is measured. Solids concentration of polyvinyl chloride aqueous dispersion (%) = (w3-w1) / (w2-w1) x 100 In this production method, polymerization is continued by adding 0.05 to 1.5 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of monomer during a period when the polymerization conversion rate is 80% or less. Adding 0.05 parts by weight or more of polyoxyethylene styrenated phenyl ether per 100 parts by weight of monomer further reduces the viscosity of the resulting plastisol when it is produced. Furthermore, adding more than 1.5 parts by weight of polyoxyethylene styrenated phenyl ether does not result in further reduction in the viscosity of the plastisol. Therefore, from the viewpoints of improving heat resistance and reducing costs, it is preferable to add 1.5 parts by weight or less of polyoxyethylene styrenated phenyl ether during a period when the polymerization conversion rate is 80% or less. The amount of polyoxyethylene styrenated phenyl ether added during the period when the polymerization conversion rate is 80% or less may be within the above-mentioned range, but is more preferably 0.1 to 1.0 part by weight, and even more preferably 0.1 to 0.3 parts by weight.

[0038] (2-3. Emulsifiers other than polyoxyethylene styrenated phenyl ether) In a production method according to one embodiment of the present invention, the anionic emulsifier may be added before and / or after the initiation of polymerization. Here, "before the initiation of polymerization" refers to a time before the initiation of polymerization, "after the initiation of polymerization" refers to a time from the initiation of polymerization to the end of polymerization, and "at the initiation of polymerization" refers to the time when the addition of the polymerization initiator to the system begins. Furthermore, "at the end of polymerization" refers to the time when the pressure inside the polymerizer becomes 0.3 MPa or less and the addition of the polymerization initiator to the system is completed.

[0039] Examples of the anionic emulsifier include, but are not limited to, salts of fatty acids, alkyl sulfates, alkylbenzenesulfonic acids, alkyl sulfosuccinic acids, α-olefinsulfonic acids, alkyl ether phosphates, and the like. Examples of the salts include potassium salts, sodium salts, and ammonium salts. These may be used alone or in combination of two or more. More specific examples of the anionic emulsifier include sodium lauryl sulfonate (sodium lauryl sulfate), sodium dodecylbenzenesulfonate, sodium isooctylbenzenesulfonate, sodium dilauryl sulfosuccinate, sodium myristate, sodium laurate, potassium myristate, and potassium laurate.

[0040] The amount of the anionic emulsifier used is not particularly limited, but is preferably 0.2 to 2.0 parts by weight, more preferably 0.3 to 0.8 parts by weight, and even more preferably 0.4 to 0.6 parts by weight, relative to 100 parts by weight of the monomer in all polymerization steps. If the amount of the anionic emulsifier used is within the above range, the polyvinyl chloride-based aqueous dispersion obtained by polymerization is stabilized, which is preferable.

[0041] The timing of use of the anionic emulsifier is not particularly limited, and it may be added before the initiation of polymerization, after the initiation of polymerization, or both before and after the initiation of polymerization. Adding the anionic emulsifier both before and after the initiation of polymerization is preferred because it stabilizes the polymerization reaction and ensures consistent latex quality. When the anionic emulsifier is added both before and after the initiation of polymerization, the amount of the anionic emulsifier added before the initiation of polymerization is preferably 0.01 to 0.2 parts by weight, more preferably 0.02 to 0.1 parts by weight, and even more preferably 0.04 to 0.08 parts by weight, based on 100 parts by weight of the monomer. Furthermore, when the anionic emulsifier is added both before and after the initiation of polymerization, the amount of the anionic emulsifier added after the initiation of polymerization is preferably 0.05 to 1.0 parts by weight, more preferably 0.1 to 0.5 parts by weight, and even more preferably 0.2 to 0.4 parts by weight, per 100 parts by weight of the monomer. Setting the amounts of the anionic emulsifier added before and after the initiation of polymerization within the above ranges advantageously achieves a balance between stability during polymerization and low viscosity when the sol is formed. When the anionic emulsifier is added after the initiation of polymerization, it may be added continuously, all at once, or in portions. When the anionic emulsifier is added after the initiation of polymerization, the timing of its addition is not particularly limited, but it can be added between the time when the polymerization conversion rate reaches 2% to 10% and the time when the polymerization conversion rate reaches 50% to 70%. This is preferable because it allows for uniform addition within the system.

[0042] Furthermore, in a production method according to one embodiment of the present invention, it is more preferable to add polyoxyethylene styrenated phenyl ether during a period when the polymerization conversion rate is 80% or less after initiation of polymerization in the presence of the anionic emulsifier. Adding polyoxyethylene styrenated phenyl ether during a period when the polymerization conversion rate is 80% or less after initiation of polymerization in the presence of the anionic emulsifier has the advantage of improving polymerization stability and reducing scale. In another embodiment, it is also preferable to add the anionic emulsifier both before and after the initiation of polymerization, and then add polyoxyethylene styrenated phenyl ether during a period when the polymerization conversion rate is 80% or less. In this case, it is advantageous to be able to suppress side reactions in the latter half of the polymerization.

[0043] In this production method, polyoxyethylene styrenated phenyl ether may be added in the aforementioned amount during the period when the polymerization conversion rate is 80% or less, but other nonionic emulsifiers may also be added as long as they do not adversely affect the effects of the present invention. Examples of such other nonionic emulsifiers include sorbitan esters, polyoxyethylene alkyl ethers, and polyoxyethylene alkyl esters. These may be used alone or in combination of two or more.

[0044] The amount of the nonionic emulsifier used is not particularly limited, but is preferably 0.01 to 0.5 parts by weight, more preferably 0.1 to 0.3 parts by weight, relative to 100 parts by weight of the monomer in all polymerization steps. If the amount of the nonionic emulsifier used is within the above range, a balance can be achieved between the viscosity-reducing effect of the plastisol and the deterioration of the thermal stability of the vinyl chloride sheet, which is preferable.

[0045] The timing of use of the nonionic emulsifier is not particularly limited, and it may be added before the start of polymerization, after the start of polymerization, or both before and after the start of polymerization.

[0046] The anionic emulsifier and nonionic emulsifier can also be added to the polyvinyl chloride aqueous dispersion obtained after polymerization, as long as they do not adversely affect the effects of the present invention.

[0047] (2-4. Polymerization initiator) Examples of polymerization initiators used in this production method include hydrogen peroxide, organic peroxides, azo initiators, and peroxodisulfates (also referred to as "persulfates"). Examples of the organic peroxides include t-butyl hydroperoxide, cumene hydroperoxide, t-butylperoxyisopropyl carbonate, paramenthane hydroperoxide, 1,1,3,3-tetramethylbutyl hydroperoxide, benzoyl peroxide, and lauroyl peroxide. Examples of the azo initiators include 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile). Examples of the peroxodisulfates include ammonium persulfate, potassium persulfate, and sodium persulfate. These polymerization initiators may be used alone or in combination of two or more.

[0048] The polymerization initiator used in this production method can be used in combination with a reducing agent such as sodium sulfite, sodium thiosulfate, sodium hydroxymethanesulfinate, ascorbic acid, sodium ascorbate, Rongalite, Bruggolite (registered trademark) FF-6, or thiourea dioxide, as needed. From an environmental perspective, Bruggolite (registered trademark) FF-6 and thiourea dioxide, which do not generate formaldehyde, are particularly preferred reducing agents. These reducing agents can be used alone or in combination of two or more.

[0049] The amount of the polymerization initiator used is preferably 0.01 to 5 parts by weight, more preferably 0.02 to 3 parts by weight, relative to 100 parts by weight of the monomer. When the amount of the polymerization initiator used is 0.01 part by weight or more, polymerization proceeds smoothly. When the amount is 5 parts by weight or less, heat generation can be suitably controlled.

[0050] (2-5. Other additives) In the present production method, other additives such as dispersants other than emulsifiers, catalysts, and other polymerization aids may be used.

[0051] Examples of dispersants other than the emulsifiers include higher alcohols such as lauryl alcohol, myristyl alcohol, cetyl alcohol, and stearyl alcohol; higher fatty acids such as lauric acid, myristic acid, palmitic acid, and stearic acid; and the like. These dispersants may be used alone or in combination of two or more.

[0052] The catalyst can be, for example, a transition metal complex produced by using a transition metal salt and a chelating agent in combination. Examples of the transition metal salt include ferrous sulfate, ferrous chloride, copper sulfate, and copper chloride. Examples of the chelating agent include disodium ethylenediaminetetraacetate (EDTA·2Na), tartaric acid, and ammonia. When ferrous sulfate is used as the transition metal salt and EDTA·2Na is used as the chelating agent, Fe-EDTA is produced and functions as a catalyst.

[0053] Examples of the other polymerization aids include aromatic hydrocarbons, polyvinyl alcohol, gelatin, particle size adjusters (sodium sulfate, sodium bicarbonate, etc.), chain transfer agents, antioxidants, etc. These polymerization aids can be used alone or in combination of two or more.

[0054] (2-6. Drying process) After homopolymerization of vinyl chloride monomer or copolymerization of vinyl chloride monomer with other ethylenically unsaturated monomer, the resulting polyvinyl chloride aqueous dispersion (hereinafter sometimes referred to as "latex" in this specification) is dried by spray drying, fluidized bed drying, etc., to obtain a polyvinyl chloride paste resin. Therefore, this production method may include a polymerization step of homopolymerizing vinyl chloride monomer or copolymerizing vinyl chloride monomer with other ethylenically unsaturated monomer, and a drying step of drying the latex obtained in the polymerization step.

[0055] In one embodiment of the present invention, the obtained polyvinyl chloride paste resin may be a resin obtained by drying a single latex obtained by the polymerization step, a resin obtained by blending two or more types of latex and drying the blend, or a resin obtained by mixing multiple polyvinyl chloride paste resins that have been dried separately.

[0056] (2-7. Polyvinyl chloride paste resin) The average degree of polymerization of the polyvinyl chloride paste resin obtained in one embodiment of the present invention is not particularly limited, but is preferably in the range of 400 to 2500, and more preferably in the range of 600 to 2000. Here, the average degree of polymerization can be measured in accordance with JIS K6721.

[0057] The particle size of the polyvinyl chloride paste resin obtained in one embodiment of the present invention is not particularly limited, but preferably has a wide distribution in the range of 0.1 μm to 15 μm when plastisolized. When particles of 0.5 μm to less than 4 μm are designated as component X and particles of 4 μm to 15 μm are designated as component Y, the volume ratio of component X to component Y is preferably in the range of X / Y = 10 / 90 to 60 / 40. If necessary, the polyvinyl chloride paste resin may be mixed with a polyvinyl chloride paste resin obtained by drying a latex separately prepared by emulsion polymerization or fine suspension polymerization, which has a peak at less than 0.5 μm, or by mixing and drying the polyvinyl chloride paste resin in the latex state. The particle size distribution of the latex can be measured using a centrifugal particle size analyzer (CPS) manufactured by CPS.

[0058] 3. Plastisol Composition (3-1. Plastisol Composition) A plastisol composition according to one embodiment of the present invention (hereinafter sometimes referred to as "the plastisol composition") contains a polyvinyl chloride paste resin produced by the above-described production method, a plasticizer, and a filler.

[0059] The plasticizer is not particularly limited, but examples thereof include diisononyl phthalate, dioctyl phthalate, etc. The content of the plasticizer is not limited thereto, but is preferably 50 to 200 parts by weight, more preferably 50 to 100 parts by weight, relative to 100 parts by weight of the polyvinyl chloride paste resin. If the content of the plasticizer is within the above range, it is possible to prepare a plastisol, and bleeding of the plasticizer from the molded body is reduced, which is preferable.

[0060] The filler is not particularly limited, but examples thereof include calcium carbonate. The content of the filler is not limited thereto, but is preferably 0 to 200 parts by weight, more preferably 50 to 100 parts by weight, per 100 parts by weight of the polyvinyl chloride paste resin. A filler content within the aforementioned range is preferable because it allows the preparation of a plastisol and allows the use of a filler within a range that maintains the strength of the molded body. Blending calcium carbonate as the filler is preferable because it offers advantages such as low cost and flame retardancy. However, plastisol compositions containing large amounts of calcium carbonate tend to be difficult to handle, particularly due to their high viscosity, making it difficult to remove or transfer the plastisol from a mixer after preparation. The use of a polyvinyl chloride paste resin produced by the aforementioned production method has the advantage of reducing the viscosity of plastisol compositions containing, for example, 100 parts by weight or more, or even 200 parts by weight or more, of calcium carbonate per 100 parts by weight of the polyvinyl chloride paste resin. The upper limit of the calcium carbonate content is preferably 100 parts by weight or less, more preferably 200 parts by weight or less, based on 100 parts by weight of the polyvinyl chloride paste resin.

[0061] The plastisol composition may further contain a chemical foaming agent in addition to the polyvinyl chloride paste resin, plasticizer, and filler produced by the aforementioned production method. By including a chemical foaming agent, a foam can be produced by heat molding. The chemical foaming agent is not particularly limited, but examples include ADCA (azodicarbonamide), OBSH (4,4'-oxybis(benzenesulfonylhydrazide)), and sodium bicarbonate (sodium bicarbonate). The content of the chemical foaming agent is not limited thereto, but is preferably 0.5 to 10 parts by weight, more preferably 1 to 3 parts by weight, per 100 parts by weight of the polyvinyl chloride paste resin. A content of the chemical foaming agent within the aforementioned range is preferred because it allows the production of foams with uniform cell shape.

[0062] Furthermore, the plastisol composition according to one embodiment of the present invention may further contain, as necessary, a stabilizer, a diluent, a pigment, a surface treatment agent, a thixotropic agent, an antioxidant, an ultraviolet absorber, a flame retardant, an antistatic agent, a lubricant, an adhesion promoter, and the like, in addition to the polyvinyl chloride paste resin produced by the above-described production method, a plasticizer, a filler, and, if necessary, a chemical foaming agent.

[0063] (3-2. Method for producing plastisol composition) The plastisol composition can be obtained by mixing and kneading the polyvinyl chloride paste resin produced by the above-described production method with a plasticizer, a filler, and, if necessary, a chemical foaming agent, as well as stabilizers, diluents, pigments, surface treatment agents, thixotropic agents, antioxidants, UV absorbers, flame retardants, antistatic agents, lubricants, adhesion promoters, etc., as necessary. The plastisol composition according to one embodiment of the present invention preferably does not contain a diluent and / or solvent, or, if it contains a diluent and / or solvent, preferably contains 10 parts by weight or less of these per 100 parts by weight of the polyvinyl chloride paste resin. If the diluent and solvent contained in the composition are 10 parts by weight or less, defects such as voids are less likely to occur in the molded product after heat molding.

[0064] [4. PVC sheets, PVC foam] The present invention also includes a vinyl chloride sheet and a vinyl chloride foam obtained by molding the plastisol composition according to one embodiment of the present invention.

[0065] Examples of the vinyl chloride sheet include carpet backing, canvas, leather, etc. Examples of a method for producing the vinyl chloride sheet include a step of coating a plastisol composition containing the present polyvinyl chloride paste resin, a plasticizer, and a filler onto a substrate such as non-flammable paper, woven fabric, or non-woven fabric through a coating blade (hereinafter referred to as a coater) whose gap with the substrate surface is adjusted to a predetermined thickness, and a step of heating the coated product to gel it, thereby obtaining a vinyl chloride sheet.

[0066] Examples of vinyl chloride foams include wallpaper, flooring, and leather. An example of a vinyl chloride foam manufacturing method will be described below, using wallpaper as an example. However, the vinyl chloride foam and its manufacturing method are not limited thereto. Wallpaper, as defined in JIS A6921, refers to a material primarily used as an interior finish on the walls and ceilings of buildings. One example of a wallpaper manufacturing method is a paste processing method, specifically, a method comprising the steps of: coating a plastisol composition containing a polyvinyl chloride paste resin, a plasticizer, a filler, and a chemical foaming agent onto a substrate such as flame-retardant paper through a coater with a predetermined thickness to allow a gap between the substrate surface and the coating; heating the coating to gel, thereby obtaining a thin coating called a "raw roll." This raw roll can then be printed as needed, and, if necessary, further heated to foam. The thickness of the raw roll is not particularly limited, but is preferably within the range of 50 μm to 200 μm. The conditions for heating the coated material to gel are not particularly limited, but are preferably set to a surface temperature of 130°C to 180°C for 5 to 50 seconds. The conditions for heating the raw material to foam are also not particularly limited, but are preferably set to a surface temperature of 180°C to 350°C for 5 to 50 seconds. The heating furnace used for these heating processes is not particularly limited, but typically, a hot air circulating furnace or a far-infrared furnace is preferably used. Furthermore, if necessary, to enhance the design of the final product, a foam inhibitor such as trimellitic anhydride or benzotriazole, which suppresses decomposition of the chemical foaming agent during the printing process on the raw material, can be printed in a desired pattern, or a textured pattern can be applied to the surface of the final product by pressing a roll with the desired textured pattern against the surface immediately after foaming. [Example]

[0067] EXAMPLES The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to these examples.

[0068] [Production Example: Production of polyvinyl chloride seed latex] The following substances were placed in a 300 L pressure vessel equipped with a stirrer and a temperature-control jacket. Ion-exchanged water: 150 kg Sodium lauryl sulfate (anionic emulsifier): 12g Kishida Chemical Company, Rongalit (sodium formaldehyde sulfoxylate, reducing agent): 128g FeSO4 7H2O (transition metal salt): 2.5g EDTA (chelating agent): 4.1g The pressure inside the pressure vessel was reduced using a vacuum pump until the pressure inside reached -0.09 MPa or less. After that, 136 kg of vinyl chloride monomer was fed into the pressure vessel, and the temperature inside the pressure vessel was raised to 50°C with stirring using a temperature-control jacket.

[0069] After the temperature inside the pressure vessel became constant, a 0.3% aqueous solution of t-butyl hydroperoxide (a water-soluble organic peroxide) was continuously fed into the pressure vessel so that the total amount of t-butyl hydroperoxide was 0.015 parts by weight per 100 parts by weight of the monomer, until the pressure inside the polymerization reactor decreased to 0.3 MPa.

[0070] During the period from when the polymerization conversion rate reached 2% to 10% to when it reached 50% to 70%, a 5% aqueous solution of sodium lauryl sulfate was continuously fed into the pressure vessel at a constant speed from a pipe separate from that for t-butyl hydroperoxide so that the total amount of sodium lauryl sulfate was 0.4 parts by weight per 100 parts by weight of monomer.

[0071] After the pressure in the pressure vessel had dropped to 0.3 MPa or less, the feeding of t-butyl hydroperoxide was stopped, and the unreacted monomer was recovered to obtain a polyvinyl chloride seed latex.

[0072] Example 1 The following substances were placed in a 300 L pressure vessel equipped with a stirrer and a temperature-control jacket. Ion-exchanged water: 150 kg Polyvinyl chloride seed latex obtained in the manufacturing example: 4.2 kg (solids) Sodium lauryl sulfate (anionic emulsifier): 100g Kishida Chemical Company, Rongalit (sodium formaldehyde sulfoxylate, reducing agent): 68g FeSO4 7H2O (transition metal salt): 0.34g EDTA (chelating agent): 0.57g The pressure in the pressure vessel was reduced using a vacuum pump until the pressure inside reached -0.09 MPa or less. Then, 150 kg of vinyl chloride monomer was fed into the pressure vessel, and the temperature inside the pressure vessel was raised with stirring using a temperature-control jacket until the temperature inside the pressure vessel reached 58°C. After the temperature inside the pressure vessel became constant, a 0.3% aqueous solution of hydrogen peroxide was continuously fed into the pressure vessel so that the total amount of hydrogen peroxide was 0.01 parts by weight per 100 parts by weight of monomer, until the pressure inside the polymerization reactor had dropped to 0.3 MPa.

[0073] During the period from when the polymerization conversion rate reached 2% to 10% to when it reached 50% to 70%, a 5% aqueous solution of sodium lauryl sulfate was continuously fed into the pressure vessel at a constant rate from a pipe separate from the hydrogen peroxide pipe so that the total amount of sodium lauryl sulfate was 0.4 parts by weight per 100 parts by weight of the monomer.

[0074] From the time when the polymerization addition rate reached approximately 40% to the time when the polymerization addition rate reached approximately 60%, a 30% aqueous solution of polyethylene styrenated phenyl ether (manufactured by Daiichi Kogyo Seiyaku Co., Ltd., Noigen (registered trademark) EA-137) was continuously fed into the pressure vessel at a constant rate so that the total amount of polyethylene styrenated phenyl ether was 0.3 parts by weight per 100 parts by weight of monomer.

[0075] After the pressure in the pressure vessel had dropped to 0.3 MPa or less, the supply of hydrogen peroxide was stopped, and the unreacted monomer was recovered to obtain a polyvinyl chloride latex.

[0076] The polyvinyl chloride latex obtained by the above procedure was dried with a spray dryer and then pulverized to obtain a polyvinyl chloride paste resin.

[0077] Example 2 A polyvinyl chloride paste resin was obtained in the same manner as in Example 1, except that the amount of polyethylene styrenated phenyl ether added between the time when the polymerization addition rate reached approximately 40% and the time when the polymerization addition rate reached approximately 60% was changed so that the total amount of polyethylene styrenated phenyl ether was 0.1 parts by weight per 100 parts by weight of monomer.

[0078] Comparative Example 1 A polyvinyl chloride paste resin was obtained in the same manner as in Example 1, except that polyethylene styrenated phenyl ether was not added.

[0079] Comparative Example 2 A polyvinyl chloride paste resin was obtained in the same manner as in Example 1, except that polyoxyethylene alkyl phenyl ether (Noigen (registered trademark) EA-130T, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was used instead of polyethylene styrenated phenyl ether, and a 30% aqueous solution of polyoxyethylene alkyl phenyl ether was continuously fed into the pressure vessel at a constant speed from the time when the polymerization addition rate reached approximately 40% to the time when the polymerization addition rate reached approximately 60% so that the total amount of polyoxyethylene alkyl phenyl ether was 0.3 parts by weight per 100 parts by weight of monomer.

[0080] Comparative Example 3 A polyvinyl chloride paste resin was obtained in the same manner as in Example 1, except that polyoxyethylene tridecyl ether (Noigen (registered trademark) TDS-80, manufactured by Daiichi Kogyo Seiyaku Co., Ltd.) was used instead of polyethylene styrenated phenyl ether, and a 30% aqueous solution of polyoxyethylene tridecyl ether was continuously fed into the pressure vessel at a constant speed from the time when the polymerization addition rate reached approximately 40% to the time when the polymerization addition rate reached approximately 60% so that the total amount of polyoxyethylene tridecyl ether was 0.3 parts by weight per 100 parts by weight of monomer.

[0081] Comparative Example 4 A polyvinyl chloride paste resin was obtained in the same manner as in Example 1, except that the polyethylene styrenated phenyl ether was added after the completion of the polymerization (after the pressure inside the polymerization reactor had dropped to 0.3 MPa) instead of during the polymerization.

[0082] [Evaluation of polyvinyl chloride paste resin] 100 g of the obtained polyvinyl chloride paste resin, 80 g of diisononyl phthalate (plasticizer), 100 g of calcium carbonate BF300 (manufactured by Bihoku Funka Kogyo Co., Ltd.), and 3 g of Adekastab AC-285 (stabilizer, manufactured by AKEKA Co., Ltd.) were placed in a stainless steel cup. The mixture was kneaded in a dissolver (manufactured by Primix Corporation, LAVOLTION) first at 350 rpm for 1 minute, then at 1000 rpm for 2 minutes, and then again at 1000 rpm for 1 minute to prepare a plastisol composition.

[0083] The prepared plastisol compositions were stored at 25°C, and the viscosity was measured using a BM viscometer one hour, one day, and one week after the start of storage. The evaluation results are shown in Table 1. In Table 1, "EA-137" represents polyethylene styrenated phenyl ether, "EA-130T" represents polyoxyethylene alkyl phenyl ether, and "TDS-80" represents polyoxyethylene tridecyl ether.

[0084] [Table 1]

[0085] 〔summary〕 Examples 1 and 2 and Comparative Examples 1 and 3 showed that by continuing the polymerization while adding 0.3 parts by weight or 0.1 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of monomer during the period when the polymerization conversion rate was 80% or less, the viscosity of the resulting plastisol composition containing a polyvinyl chloride paste resin was significantly reduced compared to the cases where no polyoxyethylene styrenated phenyl ether was added / where polyoxyethylene tridecyl ether was added.

[0086] Example 1 and Comparative Example 2 demonstrated that by continuing polymerization by adding 0.3 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of monomer during a period when the polymerization conversion rate was 80% or less, the viscosity of the resulting plastisol composition containing a polyvinyl chloride paste resin was significantly reduced, even compared to when the same amount of polyoxyethylene alkyl phenyl ether was added during the same period. Furthermore, Example 2 and Comparative Example 2 demonstrated that even when the amount of polyoxyethylene styrenated phenyl ether added was reduced by one-third, the viscosity of the plastisol composition was still lower than when the polyoxyethylene alkyl phenyl ether was added during the same period. Furthermore, the plastisol composition containing a polyvinyl chloride paste resin obtained in Example 2 showed less discoloration over time than the plastisol composition containing a polyvinyl chloride paste resin obtained in Comparative Example 2. This is believed to be due to the improved thermal stability of the plastisol composition due to the reduced amount of polyoxyethylene styrenated phenyl ether added.

[0087] Comparative Example 4 showed that even if 0.3 parts by weight of polyoxyethylene styrenated phenyl ether was added to 100 parts by weight of the monomer after polymerization, the viscosity-reducing effect of the resulting plastisol composition containing the polyvinyl chloride paste resin was low. [Industrial Applicability]

[0088] According to one embodiment of the present invention, it is possible to provide a polyvinyl chloride paste resin that can realize even lower viscosity of the resulting plastisol when it is produced. Therefore, the polyvinyl chloride paste resin and plastisol composition according to one embodiment of the present invention are very useful as raw materials / materials for various vinyl chloride sheets and vinyl chloride foams, and can be used in a wide range of industrial fields.

Claims

1. The method includes a polymerization step of homopolymerizing vinyl chloride monomer or copolymerizing vinyl chloride monomer with another ethylenically unsaturated monomer, The method for producing a polyvinyl chloride paste resin includes a step of continuing polymerization by adding 0.05 to 1.5 parts by weight of polyoxyethylene styrenated phenyl ether per 100 parts by weight of monomer during a period in which the polymerization conversion rate is 80% or less in the polymerization step.

2. The method according to claim 1, wherein the amount of the polyoxyethylene styrenated phenyl ether added is 0.1 to 0.3 parts by weight based on 100 parts by weight of the monomer.

3. A plastisol composition comprising a polyvinyl chloride paste resin produced by the method of claim 1, a plasticizer, and a filler.

4. 4. The plastisol composition according to claim 3, comprising calcium carbonate as the filler, and containing 100 parts by weight or more of said calcium carbonate per 100 parts by weight of the polyvinyl chloride paste resin.

5. The plastisol composition of claim 3 further comprising a chemical blowing agent.

6. A vinyl chloride sheet obtained by using the plastisol composition according to claim 3.

7. A vinyl chloride foam obtained by using the plastisol composition according to claim 5.

Citation Information

Patent Citations

  • Preparation of vinyl chloride resin for paste

    JP1980060504A