Composition, undercoat layer, electrode, and lithium ion secondary battery
A composition of conductive carbon material, olefin resin, and acrylic water-soluble polymer forms an undercoat layer to enhance lithium-ion battery safety and performance, particularly in high-temperature conditions.
Patent Information
- Application Number
- JP2023052346
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
AI Technical Summary
Lithium-ion secondary batteries face challenges in maintaining safety and performance, particularly in high-temperature environments, with increased DC resistance during charging and discharging, and after long-term storage.
A composition comprising a conductive carbon material, an olefin resin, and an acrylic water-soluble polymer is used to form an undercoat layer, which includes specific structural units and ratios to enhance safety and reduce DC resistance.
The composition effectively suppresses initial DC resistance and prevents increases in DC resistance in high-temperature environments, ensuring stable battery performance and safety.
Smart Images

Figure 00000042_0000 
Figure 00000042_0001 
Figure 00000042_0002
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a composition, an undercoat layer, an electrode, and a lithium ion secondary battery. [Background technology]
[0002] In recent years, lithium ion secondary batteries have been widely used as power sources for electronic devices, electric vehicles, and electricity storage. In particular, there has been a demand for batteries with high capacity, high output, and high energy density that can be installed in hybrid vehicles and the like. Such lithium ion secondary batteries have the advantage of having high energy density. On the other hand, sufficient safety measures are required because they use lithium metal and lithium ions.
[0003] Patent Document 1 discloses a positive electrode for a lithium ion secondary battery that improves the safety of the lithium ion secondary battery. The positive electrode disclosed in Patent Document 1 includes a positive electrode current collector and a positive electrode mixture layer. The positive electrode mixture layer is laminated on at least one side of the positive electrode current collector. The positive electrode mixture layer includes a positive electrode mixture layer and an undercoat layer. The undercoat layer is formed between the positive electrode current collector and the positive electrode mixture layer. The undercoat layer includes a conductive assistant, a binder, and thermally expandable microcapsules. The thermally expandable microcapsules have a maximum volume expansion temperature of 70°C to 180°C.
[0004] Patent Document 2 discloses a secondary battery having an intermediate layer containing a cured product of a curable resin having a specific functional group and a conductive material between a positive electrode current collector and a positive electrode mixture layer in order to suppress an increase in battery temperature when an internal short circuit occurs. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2019 / 189866 [Patent Document 2] International Publication No. 2018 / 198689 Summary of the Invention [Problem to be solved by the invention]
[0006] There is a demand for a lithium ion secondary battery that is excellent in safety and excellent in battery performance, in which the DC resistance at the initial stage of charging and discharging and the increase in DC resistance after long-term storage of the lithium ion secondary battery in a high-temperature environment are suppressed. The output of a lithium ion secondary battery in which the DC resistance at the initial stage of charging and discharging is suppressed is superior to the output of a lithium ion secondary battery in which the DC resistance at the initial stage of charging and discharging is not suppressed. The life of a lithium ion secondary battery in which the increase in DC resistance after long-term storage in a high-temperature environment is suppressed is superior to the life of a lithium ion secondary battery in which the increase in DC resistance after long-term storage in a high-temperature environment is not suppressed.
[0007] The problem to be solved by one embodiment of the present disclosure is to provide a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is safe, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage). The problem to be solved by another embodiment of the present disclosure is to provide an electrode and a lithium ion secondary battery that are highly safe, have low DC resistance during initial charging and discharging, and are suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage), and can stably provide excellent battery performance. [Means for solving the problem]
[0008] Specific means for solving the problems include the following aspects. <1> The conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) are included, the water-soluble acrylic polymer (C) has a structural unit derived from (meth)acrylamide and a structural unit derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group, the content of the structural unit derived from the (meth)acrylamide is 35% by mass to 95% by mass based on the total amount of the acrylic water-soluble polymer (C); A composition, wherein the content of the structural unit derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group is 5% by mass to 65% by mass based on the total amount of the water-soluble acrylic polymer (C). <2> The content of the conductive carbon material (A) is 1% by mass to 30% by mass based on the total amount of the composition, The content of the olefin resin (B) is 30% by mass to 90% by mass based on the total amount of the composition, The content of the acrylic water-soluble polymer (C) is 1% by mass to 20% by mass based on the total amount of the composition. <1> The composition described in <3> The olefin resin (B) contains an ethylene resin or a propylene resin. <1> or <2> The composition described in <4> The particle size of the olefin resin (B) is 0.1 μm to 9.0 μm, The softening point of the olefin resin (B) is 70° C. or higher. <1> ~ <3> 13. The composition according to any one of claims 1 to 12. <5> The water-soluble acrylic polymer (C) has a structural unit derived from (meth)acrylamide, a structural unit derived from a vinyl monomer having a carboxy group, and a structural unit derived from a vinyl monomer having a hydroxyl group. <1> ~ <4> 13. The composition according to any one of claims 1 to 12. <6> The acrylic water-soluble polymer (C) has a Tg of 150° C. or higher. <1> ~ <5> 13. The composition according to any one of claims 1 to 12. <7> Further, the composition contains an additive (D), The content of the additive (D) is 1% by mass to 50% by mass based on the total amount of the composition. <1> ~ <6> 13. The composition according to any one of claims 1 to 12. <8> The additive (D) includes carboxymethyl cellulose. <7> The composition described in <9> The additive (D) includes at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C to 180°C and an inorganic oxide filler. <7> or <8> The composition described in <10> The ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) measured by a laser light diffraction scattering method is 35 or less. <1> ~ <9> 13. The composition according to any one of claims 1 to 12. <11> The particle size distribution D99 measured by a laser light diffraction scattering method is 20 μm or less. <1> ~ <10> 13. The composition according to any one of claims 1 to 12. <12> The ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50) measured by a laser light diffraction scattering method is 20 or less. <1> ~ <11> 13. The composition according to any one of claims 1 to 12. <13> The above <1> ~ <12> An undercoat layer comprising the composition according to any one of claims 1 to 5. <14> A current collector and the <13> and a composite layer. <15> The current collector, the undercoat layer, and the composite layer are laminated in this order. <14> The electrode according to claim 1. <16> The above <14> or <15> A lithium ion secondary battery comprising the electrode according to claim 1. Effect of the Invention
[0009] According to the present disclosure, there is provided a composition (preferably an undercoat composition) and an undercoat layer suitable for forming an electrode that is safe, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage). In addition, according to other embodiments of the present disclosure, there are provided an electrode and a lithium ion secondary battery that are highly safe, have low DC resistance during initial charging and discharging, and are suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage), and can stably provide excellent battery performance. [Brief description of the drawings]
[0010] [Figure 1]FIG. 1 is a schematic cross-sectional view showing a laminated battery, which is an example of a lithium ion secondary battery according to the present disclosure. [Diagram 2] FIG. 2 is a schematic cross-sectional view of a positive electrode in a lithium-ion secondary battery according to an embodiment of the present disclosure. [Diagram 3] FIG. 2 is a schematic cross-sectional view of a negative electrode in a lithium-ion secondary battery according to an embodiment of the present disclosure. [Figure 4] FIG. 1 is a schematic side view showing an example of a three-roll mill. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The contents of the present disclosure will be described in detail below. The following description of the components may be based on a representative embodiment of the present disclosure, but the present disclosure is not limited to such an embodiment.
[0012] In the present disclosure, a numerical range indicated using "~" indicates a range including the numerical value described before "~" as the lower limit and the numerical value described before "~" as the upper limit. In the numerical ranges described in stages in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with the upper limit or lower limit of another numerical range described in stages. In addition, in the numerical ranges described in the present disclosure, the upper limit or lower limit described in a certain numerical range may be replaced with a value shown in the examples.
[0013] In the description of groups (atomic groups) in this specification, when there is no indication of whether they are substituted or unsubstituted, the term encompasses both unsubstituted groups (atomic groups) and substituted groups (atomic groups). For example, the term "alkyl group" encompasses not only alkyl groups without a substituent (unsubstituted alkyl groups) but also alkyl groups with a substituent (substituted alkyl groups).
[0014] In this specification, "(meth)acrylate" refers to both or either of acrylate and methacrylate, "(meth)acryl" refers to both or either of acryl and methacryl, and "(meth)acryloyl" refers to both or either of acryloyl and methacryloyl.
[0015] In this specification, the term "process" refers not only to an independent process, but also to a process that cannot be clearly distinguished from other processes, as long as the intended effect of the process is achieved. The present disclosure will be described in detail below.
[0016] (1) Composition The composition of the present disclosure contains a conductive carbon material (A), an olefin resin (B), and an acrylic water-soluble polymer (C). The acrylic water-soluble polymer (C) has a constituent unit derived from (meth)acrylamide and a constituent unit derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group. The content of the constituent unit derived from (meth)acrylamide is 35% by mass to 95% by mass based on the total amount of the acrylic water-soluble polymer (C). The content of the constituent unit derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group is 5% by mass to 65% by mass based on the total amount of the acrylic water-soluble polymer (C).
[0017] In the present disclosure, the term "conductive carbon material" refers to a carbon material having a volume resistivity at 20° C. of less than 40 Ω·cm, preferably less than 3 Ω·cm. In the present disclosure, the term "olefin-based resin" refers to a resin containing structural units derived from an olefin. Specifically, the term "olefin-based resin" includes a homopolymer of an olefin, a copolymer of two or more kinds of olefins, or a copolymer of an olefin and another monomer. In the present disclosure, the term "acrylic water-soluble polymer" refers to a polymer containing a structural unit derived from a monomer having a (meth)acryloyl group (hereinafter also referred to as "(meth)acrylic monomer"). The term "acrylic water-soluble polymer" includes a homopolymer of a (meth)acrylic monomer and a copolymer of two or more kinds of (meth)acrylic monomers. In the present disclosure, the term "water-soluble polymer" refers to a polymer that has a residual solid content of 0.1% or less when 1 g of the polymer is dissolved in 100 ml of water by stirring for 24 hours and then filtered through a 300 mesh wire screen. In the present disclosure, the terms "content" and "addition amount" are considered to be substantially the same.
[0018] Since the composition of the present disclosure has the above-mentioned configuration, it is possible to form an electrode that is excellent in safety, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance under high temperature conditions (especially after long-term storage). In other words, when the composition of the present disclosure is applied to a secondary battery having an electrode, it is possible to obtain a lithium ion secondary battery that has a good balance between safety and battery performance (i.e., output and life).
[0019] The reason why the present disclosure has an effect is not necessarily clear, but is presumed to be as follows. Among the resin components contained in the composition of the present disclosure, the water-dispersible olefin resin (B) has the function of melting in a lower temperature range. In other words, it is advantageous for the manifestation of the shutdown function during heat generation. The acrylic water-soluble polymer (C) contains (meth)acrylamide, which has excellent heat resistance. As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the heat resistance, electrolyte resistance, and ion permeability of the undercoat layer are improved in a well-balanced manner. Therefore, an electrode is obtained that is excellent in safety, and not only has a low DC resistance during initial charging and discharging, but also has a significantly suppressed increase in DC resistance under high-temperature environments (especially after long-term storage). As a result, when a lithium secondary battery is produced using the composition of the present disclosure, it becomes a lithium ion secondary battery with a good balance between safety and battery performance (i.e., output and life).
[0020] The composition of the present disclosure is preferably used for, for example, electrode components of lithium ion secondary batteries. In particular, the composition of the present disclosure is preferably used to form an undercoat layer included in an electrode of a lithium ion secondary battery having an electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector. In particular, the composition of the present disclosure is more preferably used to form an undercoat layer included in a positive electrode of a lithium ion secondary battery having a positive electrode in which an undercoat layer and a composite layer are laminated in this order on at least one main surface of a current collector.
[0021] In this disclosure, the term "current collector" refers to a sheet-like object for collecting electrons generated from an active material in a lithium-ion secondary battery and supplying the electrons to the active material. The term "main surfaces of a current collector" refers to a pair of opposing surfaces having the largest area among a plurality of pairs of opposing surfaces.
[0022] (1.1) Conductive carbon material (A) The composition of the present disclosure contains a conductive carbon material (A), which reduces the electrical resistance of the composition of the present disclosure.
[0023] Examples of the conductive carbon material (A) include graphite, carbon black, conductive carbon fiber, and fullerene. Examples of the graphite include artificial graphite and natural graphite (e.g., flake graphite, lump graphite, and amorphous graphite). Examples of the conductive carbon fiber (A) include carbon nanotubes, carbon nanofibers, and carbon fibers. The conductive carbon material (A) may be used alone or in combination of two or more.
[0024] The shape of the conductive carbon material (A) is not particularly limited, and may be particulate. When the conductive carbon material (A) is particulate, the particle size of the conductive carbon material (A) is not particularly limited. From the viewpoint of dispersing the conductive carbon material (A) between the particles contained in the undercoat layer and allowing it to function as a conductive assistant, the particle size of the conductive carbon material (A) is preferably 5 μm or less, more preferably 1 μm to 4 μm. In this case, the primary particle size of the particles of the conductive carbon material is preferably 0.5 μm or less, more preferably 0.1 μm to 0.4 μm. The particle size of the conductive carbon material (A) is a particle size (particle size distribution D50, median diameter) equivalent to a cumulative 50 volume % from the fine particle side in a volume-based particle size distribution measured by a particle size distribution measuring device based on a laser light diffraction scattering method.
[0025] The conductive carbon material (A) may be a commercially available product. Examples of commercially available carbon black products include "Super P" (manufactured by TIMCAL). Examples of commercially available flake graphite products include "KS-6" (manufactured by TIMREX).
[0026] The content of the conductive carbon material (A) is not particularly limited, and is preferably 1% by mass to 30% by mass with respect to the total amount of the composition. If the content of the conductive carbon material (A) is within the above range, the number of contact points between the conductive carbon materials (A) in the composition of the present disclosure is large, and the electrical resistance of the composition of the present disclosure at room temperature can be reduced by the percolation effect. Furthermore, when the temperature of the lithium ion secondary battery increases rapidly, the contact between the conductive carbon materials (A) is difficult to maintain, and the electrical resistance of the undercoat layer increases, so that the resulting lithium ion secondary battery can exhibit a shutdown function. In other words, the safety of the lithium ion secondary battery is excellent. The shutdown function includes preventing the progress of the battery reaction of the lithium ion secondary battery. The "battery reaction" refers to the insertion reaction and desorption reaction of lithium ions that occur between the positive electrode and the negative electrode. The higher the content of the conductive carbon material (A), the better the battery performance of the lithium ion secondary battery tends to be. From the viewpoint of ensuring the shutdown function, the content of the conductive carbon material (A) is preferably 28 mass% or less, more preferably 25 mass% or less, and even more preferably 20 mass% or less, based on the total amount of the composition. From the viewpoint of ensuring the battery performance, the content of the conductive carbon material (A) is preferably 3 mass% or more, more preferably 5 mass% or more, and even more preferably 10 mass% or more, based on the total amount of the composition.
[0027] (1.2) Olefin resin (B) The composition of the present disclosure contains an olefin-based resin (B). As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is further improved.
[0028] The material of the olefin resin (B) is not particularly limited. The softening point of the olefin resin (B) is preferably 150°C or less, more preferably 140°C or less, and even more preferably 135°C or less, from the viewpoint of more effectively exerting the shutdown function by melting the olefin resin (B) in a lower temperature range during a sudden temperature rise of the lithium ion secondary battery (hereinafter referred to as "effective exertion of the shutdown function"). The softening point of the olefin resin (B) is preferably 70°C or more, more preferably 90°C or more, even more preferably 110°C or more, and particularly preferably 120°C or more, from the viewpoint of maintaining the shape of the olefin resin (B) before and after the execution of the drying treatment performed in the manufacturing process of the positive electrode (hereinafter referred to as "shape maintenance of the olefin resin (B) during the positive electrode drying step"). The softening point of the olefin resin (B) is preferably 70°C or more, more preferably 90°C or more, even more preferably 110°C or more, and particularly preferably 120°C or more. The softening point of the olefin resin (B) is preferably 70°C to 150°C. The softening point of the olefin resin (B) is a value measured according to JIS K2207 (ring and ball method).
[0029] Examples of the olefin resin (B) include ethylene resins (e.g., polyethylene, ethylene-vinyl acetate copolymer (EVA), polyethylene oxide), propylene resins (e.g., polypropylene), polyvinyl chloride, polyvinylidene chloride, polyvinyl fluoride, polyvinylidene fluoride, polyamide, polystyrene, polyacrylonitrile, and polymethyl (meth)acrylate. Among these, the olefin resin (B) preferably contains an ethylene resin or a propylene resin from the viewpoint of achieving both effective shutdown function and shape retention of the olefin resin during the positive electrode drying step.
[0030] An "ethylene-based resin" is a resin whose main component is ethylene, and a "propylene-based resin" is a resin whose main component is propylene. Here, the "main component" means the component that is contained in the resin in the greatest amount. Examples of the ethylene-based resin include homopolymers or copolymers of ethylene. Among them, the ethylene-based resin is preferably a copolymer of ethylene and at least one kind of α-olefin. Examples of the propylene-based resin include homopolymers or copolymers of propylene.
[0031] The olefin resin (B) preferably contains a water-dispersible olefin resin, whereby when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is improved.
[0032] In the present disclosure, the term "water-dispersible olefin-based resin" refers to an olefin-based resin that is dispersible in water without the addition of at least one of a surfactant and an organic solvent.
[0033] Examples of the water-dispersible olefin resin material include polyethylene, polyethylene elastomers, polyolefin ionomers, and EVA.
[0034] The content of the water-dispersible olefin resin is not particularly limited, and is preferably 20% by mass or more, more preferably 50% by mass or more, and may be 100% by mass, based on the total amount of the olefin resin (B).
[0035] As the olefin-based resin (B), a commercially available product may be used. Commercially available products of the olefin resin (B) include the Chemipearl (registered trademark) series (polyolefin aqueous dispersions) manufactured by Mitsui Chemicals, Inc. Examples of finely divided aqueous dispersions of polyethylene or polypropylene include WP100, W100, W200, W300, W308, W310, W400, W401, W410, W4005, W500, WF640, W700, W800, W900, W950, P301W, and WH201.
[0036] The shape of the olefin resin (B) is not particularly limited, and may be particulate. When the olefin resin (B) is particulate, the particle size is not particularly limited. From the viewpoint of adjusting the particle size of the olefin resin so as to fall within the optimum film thickness range of the undercoat layer, the particle size of the olefin resin (B) is preferably 9.0 μm or less, more preferably 4.0 μm or less, and further preferably 2.0 μm or less, as an average primary particle size. From the viewpoint of the processability of the composition (e.g., slurry for the undercoat layer), the particle size of the olefin resin (B) is preferably 0.1 μm or more, more preferably 0.5 μm or more. The particle size of the olefin resin (B) is preferably 0.1 μm to 9.0 μm. The smaller the particle size of the olefin resin (B), the more likely the olefin resin (B) is to aggregate. The particle size of the olefin resin (B) is the average primary particle size measured by a Coal counter method.
[0037] The particle size of the olefin resin (B) is preferably 0.1 μm to 9.0 μm, and the softening point of the olefin resin (B) is preferably not less than 70° C. As a result, when the composition of the present disclosure is used as a raw material for the undercoat layer, the lithium ion secondary battery is less susceptible to thermal runaway, and the safety of the lithium ion secondary battery is further improved.
[0038] The olefin-based resin (B) may be used alone or in combination of two or more kinds. The content of the olefin resin (B) is preferably 30% by mass to 90% by mass based on the total amount of the composition. When the content of the olefin resin (B) is within the above range, the shutdown function can be satisfactorily ensured. The higher the content of the olefin resin (B), the better the safety of the lithium ion secondary battery becomes, whereas the battery performance of the lithium ion secondary battery tends to decrease. In other words, there is a trade-off between the safety of the lithium ion secondary battery and the battery performance of the lithium ion secondary battery. From this viewpoint, the content of the olefin resin (B) is preferably 80% by mass or less, more preferably 75% by mass or less, based on the total amount of the composition, from the viewpoint of reducing the resistance of the undercoat layer. In addition, the content of the olefin resin (B) is preferably 35% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 60% by mass or more, based on the total amount of the composition, from the viewpoint of effectively exerting the shutdown function.
[0039] (1.3) Acrylic water-soluble polymer (C) The composition of the present disclosure contains an acrylic water-soluble polymer (C).
[0040] The content of the acrylic water-soluble polymer (C) is not particularly limited, and is preferably 1% by mass or more, more preferably 2% by mass or more, and even more preferably 3% by mass or more, based on the total amount of the composition. The content of the acrylic water-soluble polymer (C) is not particularly limited, and is preferably 20% by mass or less, more preferably 15% by mass or less, and even more preferably 10% by mass or less, based on the total amount of the composition.
[0041] The acrylic water-soluble polymer (C) has a constitutional unit derived from (meth)acrylamide and a constitutional unit derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group (hereinafter also referred to as a "specific vinyl monomer"). The content of the constitutional unit derived from the (meth)acrylamide is 35% by mass to 95% by mass based on the total amount of the acrylic water-soluble polymer (C). The content of the constitutional unit derived from the specific vinyl monomer is 5% by mass to 65% by mass based on the total amount of the acrylic water-soluble polymer (C).
[0042] The glass transition temperature (Tg) of the acrylic water-soluble polymer (C) is not particularly limited, but is preferably at least 150° C. This provides the undercoat layer with better heat resistance. From the viewpoint of obtaining an undercoat layer having superior heat resistance, the glass transition temperature (Tg) of the acrylic water-soluble polymer (C) is more preferably 200° C. or higher, even more preferably 210° C. or higher, particularly preferably 220° C. or higher, even more preferably 230° C. or higher, and even more preferably 240° C. or higher. The glass transition temperature (Tg) of the water-soluble polymer is preferably 400° C. or lower, more preferably 300° C. or lower, and even more preferably 280° C. or lower. The glass transition temperature (Tg) was measured in the same manner as described in the Examples.
[0043] The content of the constitutional unit derived from (meth)acrylamide is 35% by mass or more, preferably 60% by mass or more, more preferably 70% by mass or more, and even more preferably 75% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the constitutional unit derived from (meth)acrylamide is preferably 95% by mass or less, preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0044] The content of the structural unit derived from the specific vinyl monomer is 5% by mass or more, preferably 10% by mass or more, more preferably 20% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the specific vinyl monomer is preferably 65% by mass or less, preferably 40% by mass or less, more preferably 30% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0045] The acrylic water-soluble polymer preferably has a constitutional unit derived from (meth)acrylamide, a constitutional unit derived from a vinyl monomer having a carboxy group (hereinafter also referred to as a "carboxyl group-containing vinyl monomer"), and a constitutional unit derived from a vinyl monomer having a hydroxyl group (hereinafter also referred to as a "hydroxyl group-containing vinyl monomer"), which provides excellent adhesion between the conductive carbon material (A) and the olefin resin (B) and enhances the binding strength due to the interaction between the acrylic polymers.
[0046] When the acrylic water-soluble polymer (C) has a constituent unit derived from a carboxy group-containing vinyl monomer and a constituent unit derived from a hydroxyl group-containing vinyl monomer, the content of the constituent unit derived from the carboxy group-containing vinyl monomer is preferably within the following range. The content of the structural unit derived from the carboxyl group-containing vinyl monomer is preferably 3% by mass or more, more preferably 5% by mass or more, and even more preferably 7% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the carboxyl group-containing vinyl monomer is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0047] When the acrylic water-soluble polymer (C) has a structural unit derived from a carboxyl group-containing vinyl monomer and a structural unit derived from a hydroxyl group-containing vinyl monomer, the content of the structural unit derived from the hydroxyl group-containing vinyl monomer is preferably within the following range. The content of the structural unit derived from the hydroxyl group-containing vinyl monomer is preferably 2% by mass or more, more preferably 5% by mass or more, and even more preferably 13% by mass or more, based on the total amount of the acrylic water-soluble polymer (C). From the viewpoint of obtaining an undercoat layer having excellent heat resistance, the content of the structural unit derived from the hydroxyl group-containing vinyl monomer is preferably 30% by mass or less, more preferably 20% by mass or less, and more preferably 15% by mass or less, based on the total amount of the acrylic water-soluble polymer (C).
[0048] (1.3.1) Raw material for acrylic water-soluble polymer (C) The acrylic water-soluble polymer (C) is a polymer obtained by polymerizing an acrylic water-soluble polymer raw material. The raw material of the acrylic water-soluble polymer (C) (hereinafter also referred to as "acrylic water-soluble polymer raw material") contains (meth)acrylamide and a specific vinyl monomer.
[0049] (1.3.1.1) (Meth)acrylamide The (meth)acrylamide may be methacrylamide and acrylamide, or may be methacrylamide, or may be acrylamide. From the viewpoint of improving heat resistance, the (meth)acrylamide is preferably methacrylamide.
[0050] The (meth)acrylamide content is preferably 35% by mass or more, more preferably 60% by mass or more, even more preferably 70% by mass or more, and particularly preferably 75% by mass or more, based on the total amount of the acrylic water-soluble polymer raw material. From the viewpoint of obtaining excellent heat resistance, the (meth)acrylamide content is preferably 95% by mass or less, preferably 90% by mass or less, and more preferably 80% by mass or less, based on the total amount of the water-soluble polymer raw material.
[0051] (1.3.1.2) Certain vinyl monomers The specific vinyl monomer is copolymerizable with (meth)acrylamide and has at least one of a carboxy group and a hydroxyl group.
[0052] The specific vinyl monomer is at least one selected from the group consisting of a carboxyl group-containing vinyl monomer and a hydroxyl group-containing vinyl monomer. From the viewpoint of improving the adhesion between the conductive carbon material (A) and the olefin resin (B) and the adhesion due to the interaction between the binders, the specific vinyl monomer is preferably a carboxyl group-containing vinyl monomer or a hydroxyl group-containing vinyl monomer.
[0053] The content of the specific vinyl monomer is preferably 5% by mass or more, more preferably 10% by mass or more, and more preferably 20% by mass or more, based on the total amount of the water-soluble polymer raw material. The content of the specific vinyl monomer is preferably 65% by mass or less, more preferably 40% by mass or less, and even more preferably 30% by mass or less, based on the total amount of the water-soluble polymer raw material.
[0054] (1.3.1.2.1) Carboxy group-containing vinyl monomers Examples of the carboxyl group-containing vinyl monomer include monocarboxylic acid, dicarboxylic acid, and salts thereof. Examples of the monocarboxylic acid include (meth)acrylic acid. Examples of the dicarboxylic acid include itaconic acid, maleic acid, fumaric acid, itaconic anhydride, maleic anhydride, and fumaric anhydride. These carboxyl group-containing vinyl monomers can be used alone or in combination of two or more. The carboxy group-containing vinyl monomer is preferably a monocarboxylic acid, more preferably (meth)acrylic acid, and even more preferably methacrylic acid.
[0055] The content of the carboxyl group-containing vinyl monomer is preferably 3% by mass or more, more preferably 5% by mass or more, and more preferably 7% by mass or more, based on the total amount of the acrylic water-soluble polymer raw material. The content of the carboxyl group-containing vinyl monomer is preferably 35% by mass or less, more preferably 30% by mass or less, and even more preferably 20% by mass or less, based on the total amount of the water-soluble polymer raw material. The content of the carboxyl group-containing vinyl monomer is preferably 20% by mass or more, more preferably 25% by mass or more, and more preferably 30% by mass or more, based on the total amount of the specific vinyl monomers. The content of the carboxyl group-containing vinyl monomer is preferably 95% by mass or less, more preferably 90% by mass or less, and even more preferably 85% by mass or less, based on the total amount of the specific vinyl monomers.
[0056] (1.3.1.2.2) Hydroxyl-containing vinyl monomers The hydroxyl-containing vinyl monomer includes a vinyl monomer having a hydroxyl group but no carboxyl group (hereinafter also referred to as "hydroxyl-containing vinyl monomer (c10)") and a vinyl monomer having a hydroxyl group and a carboxyl group (hereinafter also referred to as "hydroxyl-containing vinyl monomer (c20)").
[0057] Examples of the hydroxyl group-containing vinyl monomer (c10) include mono(meth)acrylates having a hydroxyl group (c11), di(meth)acrylates having a hydroxyl group (c12), and tri(meth)acrylates having a hydroxyl group (c13). Examples of the mono(meth)acrylate (c11) having a hydroxyl group include 2-hydroxyethyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 3-hydroxypropyl (meth)acrylate, 2-hydroxy-3-phenoxypropyl (meth)acrylate, 3-chloro-2-hydroxypropyl (meth)acrylate, butanediol mono(meth)acrylate, polyethylene glycol mono(meth)acrylate, 2-(6-hydrohexanoyloxy)ethyl acrylate, glycerin mono(meth)acrylate, trimethylolpropane mono(meth)acrylate, and pentaerythritol mono(meth)acrylate. Examples of the di(meth)acrylate (c12) having a hydroxyl group include glycerin di(meth)acrylate, trimethylolpropane di(meth)acrylate, and pentaerythritol di(meth)acrylate. An example of the tri(meth)acrylate (c13) having a hydroxyl group is pentaerythritol tri(meth)acrylate. These can be used alone or in combination of two or more types. The hydroxyl group-containing vinyl monomer (c10) is preferably a mono(meth)acrylate (c11) having a hydroxyl group, more preferably at least one of 2-hydroxyethyl(meth)acrylate and 2-hydroxypropyl(meth)acrylate, and even more preferably 2-hydroxyethyl methacrylate.
[0058] The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 2% by mass or more, more preferably 5% by mass or more, more preferably 13% by mass or more, based on the total amount of the acrylic water-soluble polymer raw material. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 30% by mass or less, more preferably 20% by mass or less, and even more preferably 15% by mass or less, based on the total amount of the water-soluble polymer raw material. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 5% by mass or more, more preferably 10% by mass or more, more preferably 15% by mass or more, based on the total amount of the specific vinyl monomers. The content of the hydroxyl group-containing vinyl monomer (c10) is preferably 80% by mass or less, more preferably 75% by mass or less, and even more preferably 70% by mass or less, based on the total amount of the specific vinyl monomers.
[0059] Examples of the hydroxyl group-containing vinyl monomer (c20) include ricinoleic acid, lesquerolic acid, 15-hydroxylinoleic acid, auricolic acid, hydroxypalmitoleic acid, caffeic acid, etc. These can be used alone or in combination of two or more kinds.
[0060] (1.3.1.3) Water-soluble copolymerizable monomers The acrylic water-soluble polymer raw material may contain a copolymerizable monomer that is copolymerizable with (meth)acrylamide and / or a specific vinyl monomer (hereinafter also referred to as a "water-soluble copolymerizable monomer").
[0061] Examples of the water-soluble copolymerizable monomer include (meth)acrylic acid alkyl esters (e.g., methyl (meth)acrylate, ethyl (meth)acrylate, etc.), functional group-containing vinyl monomers (e.g., 2-aminoethyl (meth)acrylate, glycidyl (meth)acrylate, etc., (meth)acrylonitrile, allylsulfonic acid, 2-methacryloyloxyethyl acid phosphate, etc.), vinyl esters (e.g., vinyl acetate, vinyl propionate, etc.), aromatic vinyl monomers (e.g., Examples of the vinyl monomer include styrene, α-methylstyrene, etc.), N-substituted unsaturated carboxylic acid amides (for example, N-methylol (meth)acrylamide, etc.), heterocyclic vinyl compounds (for example, vinylpyrrolidone, etc.), vinylidene halide compounds (for example, vinylidene chloride, vinylidene fluoride, etc.), α-olefins (for example, ethylene, propylene, etc.), dienes (for example, butadiene, etc.), and crosslinkable vinyl monomers (for example, methylene bis (meth) acrylamide, divinylbenzene, etc.).
[0062] The content of the water-soluble copolymerizable monomer is within a range in which the water solubility of the water-soluble polymer is maintained, and is, for example, 37% by mass or less, preferably 15% by mass or less, and 0% by mass or more, particularly preferably 0% by mass, relative to the total amount of the water-soluble polymer raw material.
[0063] (1.3.1.4) Polymerization method for water-soluble polymer raw material The water-soluble polymer can be obtained by polymerizing the water-soluble polymer raw material by a known method. More specifically, for example, the water-soluble polymer raw material and a polymerization initiator are mixed in water, the water-soluble polymer raw material is polymerized, and then, if necessary, aged. The polymerization initiator is not particularly limited and may be any known polymerization initiator. The polymerization temperature may be 30° C. to 95° C. The polymerization time may be 0.5 hours to 20 hours. The maturation time may be 0.5 hours to 6 hours.
[0064] (1.4) Additives (D) The composition of the present disclosure may contain an additive (D) as necessary. Depending on the type of additive (D), various functions can be imparted to the composition of the present disclosure.
[0065] In the present disclosure, the term "additive" refers to components other than the conductive carbon material (A), the olefin-based resin (B), and the water-soluble acrylic polymer (C).
[0066] Examples of additives (D) include thickening stabilizers, thermally expandable microcapsules having a maximum volume expansion temperature of 70°C to 180°C (hereinafter simply referred to as "thermally expandable microcapsules"), inorganic oxide fillers, curable resin fillers, scaly fillers, binder resins, synthetic rubbers, non-solid contents, etc.
[0067] The term "thermally expandable microcapsule" refers to a particle having an outer shell made of a thermoplastic resin and a volatile expanding agent, which is a core component, encapsulated in the outer shell. In detail, the thermally expandable microcapsule is preferably one that, in contact with an electrolyte solution described below, softens and foams to cause a volume expansion when exposed to a temperature (e.g., 70°C to 160°C) immediately before the onset of thermal runaway due to abnormal heat generation in a lithium ion secondary battery. The "maximum volume expansion temperature" refers to the temperature at which the expanded volume of the thermally expandable microcapsule becomes maximum when the volatile expanding agent contained in the thermally expandable microcapsule gasifies and the thermally expandable microcapsule expands in volume. The temperature at which the volatile expanding agent contained in the thermally expandable microcapsule gasifies and the thermally expandable microcapsule starts to expand in volume is called the "volume expansion start temperature."
[0068] When additive (D) is contained, the content of additive (D) is preferably 1 mass % to 50 mass % relative to the total amount of the composition. When the content of additive (D) is within the above range, the shutdown function due to the properties of additive (D) can be more effectively exhibited. The content of the additive (D) has a small effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and from the viewpoints of effectively exerting the shutdown function and maintaining the battery performance, the content of the additive (D) is preferably 40 mass% or less, more preferably 30 mass% or less, based on the total amount of the composition. Also, from the viewpoints of effectively exerting the shutdown function, the content of the additive (D) is preferably 5 mass% or more, more preferably 10 mass% or more, based on the total amount of the composition.
[0069] (1.4.1) Thickening agents The composition of the present disclosure may contain a thickening stabilizer. The composition of the present disclosure may not contain a thickening stabilizer. When the composition of the present disclosure contains a thickening stabilizer and is used as a raw material for the undercoat layer, it becomes possible to stably disperse particles when preparing a slurry for the undercoat layer.
[0070] Examples of thickening stabilizers include carboxymethylcellulose (CMC), polyvinyl alcohol (PVA), methylcellulose (MC), hydroxypropylcellulose (HPC), polyethylene glycol (PEG), polyethylene oxide (PEO), polyvinylpyrrolidone (PVP), polyacrylic acid (PAA), polycarboxylate ammonium salts, sugars exemplified by glycosides such as lecithin and saponin, and polysaccharides such as xanthan gum, polyether polyols such as sucrose polyether polyol, polyoxypropylene sorbitol ether, trimethylolpropane polyether polyol, and pentaerythritol polyether polyol, oxidized starch, starch phosphate, casein, and various modified starches.
[0071] The content of the thickening stabilizer is preferably 1 to 50% by mass relative to the total amount of the composition. From the viewpoint of effectively exerting the shutdown function and maintaining the battery performance, the content of the thickening stabilizer is preferably 15% by mass or less, more preferably 10% by mass or less, relative to the total amount of the composition. From the viewpoint of more effectively dispersing the fine particles in the undercoat slurry, the content of the thickening stabilizer is preferably 1% by mass or more, more preferably 2% by mass or more, relative to the total amount of the composition.
[0072] Commercially available CMC products include "1130", "1140", "1240", "1250", "1260", "1330", "2200", and "DL100L" manufactured by Daicel Miraize Co., Ltd.
[0073] (1.4.2) Thermally expandable microcapsules The composition of the present disclosure may contain thermally expandable microcapsules. The composition of the present disclosure may not contain thermally expandable microcapsules. When the composition of the present disclosure contains thermally expandable microcapsules and is used as a raw material for an undercoat layer, the thermally expandable microcapsules undergo volumetric expansion due to abnormal heat generation in the lithium ion secondary battery, efficiently increasing the DC resistance of the electrode and improving the safety of the lithium ion secondary battery.
[0074] The volume expansion starting temperature of the thermally expandable microcapsules is preferably 120°C to 130°C. The maximum volume expansion temperature of the thermally expandable microcapsules is preferably 145°C to 155°C.
[0075] The thermoplastic resin constituting the outer shell preferably contains a (co)polymer containing vinylidene chloride and a (co)polymer containing (meth)acrylonitrile. This allows the thermoplastic resin constituting the outer shell to have excellent electrolyte resistance, thermoplasticity, and excellent gas barrier properties. In particular, from the viewpoint of electrolyte resistance, the thermoplastic resin constituting the outer shell is preferably a (co)polymer containing (meth)acrylonitrile as the main component (51 mass% or more). The raw material of the thermoplastic resin constituting the outer shell may contain a crosslinkable monomer in addition to a polymerizable monomer in order to improve the foaming properties and heat resistance of the resulting thermally expandable microcapsule.
[0076] The boiling point of the volatile expanding agent is preferably selected so that the maximum volume expansion temperature of the thermally expandable microcapsules is higher than the softening point of the olefin resin (B). The boiling point is preferably selected so that the volume expansion start temperature of the thermally expandable microcapsules is equal to the softening point of the olefin resin (B). This allows the DC resistance of the electrode to increase efficiently when the temperature of the undercoat layer rises above the softening point of the olefin resin (B) due to heat generation in the lithium ion secondary battery. As a result, the safety of the lithium ion secondary battery is further improved. Examples of the volatile expanding agent include low molecular weight hydrocarbons having a boiling point of 100°C or less, non-flammable or flame-retardant compounds, etc. As the low molecular weight hydrocarbons having a boiling point of 100°C or less, low molecular weight hydrocarbons are preferably used. Examples of the low molecular weight hydrocarbons include propane, propylene, n-butane, isobutane, butene, isobutene, isopentane, neopentane, n-pentane, n-hexane, isohexane, heptane, and petroleum ether. Examples of the non-flammable or flame-retardant compounds include halogenated hydrocarbons (e.g., methyl chloride, methylene chloride, fluorotrichloromethane, difluorodichloromethane, chlorotrifluoromethane, etc.), and chlorofluorocarbons. The volatile expanding agent may be used alone or in combination of two or more.
[0077] The particle size of the thermally expandable microcapsules is not particularly limited, and is preferably from 1 μm to 40 μm, more preferably from 3 μm to 30 μm, and further preferably from 5 μm to 25 μm.
[0078] The particle size of the thermally expandable microcapsules is the particle size (particle size distribution D50, median diameter) equivalent to 50% cumulative volume from the fine particle side in the volume-based particle size distribution measured using a particle size distribution measuring device based on the laser light diffraction scattering method.
[0079] The content of the thermally expandable microcapsules is preferably 0% by mass to 50% by mass relative to the total amount of the composition. The content of the thermally expandable microcapsules has a small effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and is preferably 50% by mass or less, more preferably 40% by mass or less, relative to the total amount of the composition, from the viewpoint of maintaining the shutdown function and battery performance. The content of the thermally expandable microcapsules is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition, from the viewpoint of enhancing the shutdown function due to the thermal expansion of the thermally expandable microcapsules during abnormal heat generation.
[0080] As the thermally expandable microcapsules, commercially available products may be used. Commercially available thermally expandable microcapsules include the "Matsumoto Microsphere (registered trademark)" series manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd., the "EXPANCEL (registered trademark)" series manufactured by Akzo Nobel, and the "ADVANCELL (registered trademark)" series manufactured by Sekisui Chemical Co., Ltd.
[0081] (1.4.3) Inorganic oxide fillers The composition of the present disclosure may contain an inorganic oxide filler. The composition of the present disclosure may not contain an inorganic oxide filler. When the composition of the present disclosure contains an inorganic oxide filler, the inorganic oxide filler functions as a filler. Increasing the content of the inorganic oxide filler contributes to improving the heat resistance of the positive electrode, while minimizing the content of the inorganic oxide filler forms an undercoat layer that adheres closely to the positive electrode mixture layer, and the undercoat layer melts in the event of an internal short circuit, contributing to improving safety. Furthermore, by selecting the type and physical properties of the inorganic oxide filler, it is also possible to decompose the electrolyte and generate gas when the battery is overcharged.
[0082] Examples of inorganic oxide fillers include aluminum oxide (α-Al2O3, γ-Al2O3), aluminum hydroxide (Al(OH)3), boehmite (AlOOH)), magnesia (magnesium oxide: MgO), magnesium hydroxide (Mg(OH)2), zirconia (ZrO2), titania (TiO2), silica (SiO2), silicon dioxide (SiO2), silicon carbide (SiC), aluminum nitride (AlN), boron nitride (BN), mica, and graphite oxide (e.g., expanded graphite). The inorganic oxide filler may be used alone or in combination of two or more. Among them, it is preferable that the inorganic oxide filler contains aluminum oxide.
[0083] The shape of the inorganic oxide filler is not particularly limited, and examples thereof include a spherical shape, a needle shape, an ellipsoid shape, a plate shape, a scale shape, etc. The particle size of the inorganic oxide filler is not particularly limited, and is preferably 0.01 μm to 5 μm. The particle size of the inorganic oxide filler is the particle size (particle size distribution D50, median diameter) that corresponds to 50% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method.
[0084] The content of the inorganic oxide filler is preferably 0% by mass to 50% by mass relative to the total amount of the composition. The content of the inorganic oxide filler has little effect on the content ratio of the conductive carbon material (A) and the olefin resin (B), and from the viewpoint of maintaining the shutdown function and battery performance, the content is preferably 40% by mass or less, more preferably 30% by mass or less, relative to the total amount of the composition. In addition, the content of the inorganic oxide filler is preferably 5% by mass or more, more preferably 10% by mass or more, relative to the total amount of the composition, from the viewpoint of suppressing the fluidity of the olefin resin (B) dissolved in the undercoat layer at high temperatures and maintaining the shutdown function for a long period of time.
[0085] (1.4.4) Binder resin The composition of the present disclosure may contain a binder resin as another component. When the composition of the present disclosure is used as a raw material for an undercoat layer, the binder resin can improve the physical properties of the undercoat layer (e.g., electrolyte permeability and peel strength) and can also improve the battery performance of a lithium ion secondary battery.
[0086] Examples of the binder resin include polyvinylidene fluoride (PVDF), polytetrafluoroethylene (PTFE), PVDF copolymer, hydroxypropylmethylcellulose, polyvinyl alcohol, and diacetylcellulose. The PVDF copolymer is a copolymer of vinylidene fluoride and other monomers, and examples of the PVDF copolymer include PVDF-HFP (hexafluoropropylene) and PVDF-PEO (polyoxyethylene). Among them, the binder resin preferably contains PVDF from the viewpoint of reducing the resistance of the undercoat layer.
[0087] As the binder resin, a commercially available product may be used. Commercially available PVDF products include the Kureha (registered trademark) KF Polymer series manufactured by Kureha Corporation, such as "W#1100", "W#1300", "W#1700", "W#7200", and "W#7300".
[0088] The binder resin may be used alone or in combination of two or more kinds. The content of the binder resin is preferably 1% by mass to 20% by mass with respect to the total amount of the composition. The shutdown function depends on the balance between the content of the binder resin and the total content of the olefin resin (B) and the acrylic water-soluble polymer (C). When the content ratio of the binder resin to the total amount of the composition is high, the content ratio of the olefin resin (B) and the acrylic water-soluble polymer (C) to the total amount of the composition is low, and therefore the shutdown function may be reduced. When the content of the binder resin is within the above range, it is possible to achieve both the processability of the composition (for example, the slurry for the undercoat layer) and the assurance of the shutdown function. The content of the binder resin is preferably 15% by mass or less, more preferably 10% by mass or less, based on the total amount of the composition, from the viewpoint of ensuring the shutdown function in relation to the content of the olefin resin (B) and the acrylic water-soluble polymer (C). Also, the content of the binder resin is preferably 2% by mass or more, more preferably 3% by mass or more, based on the total amount of the composition, from the viewpoint of the processability of the composition (e.g., slurry for undercoat layer).
[0089] (1.4.5) Synthetic rubber The composition of the present disclosure may contain a synthetic rubber as another component. When the composition of the present disclosure is used as a raw material for an undercoat layer, the adhesion between the undercoat layer and the current collector is improved, and the battery resistance can be further reduced.
[0090] Examples of synthetic rubbers include styrene butadiene rubber (SBR), acrylonitrile-butadiene rubber, acrylonitrile-butadiene-styrene rubber, hydrogenated styrene butadiene rubber (HSBR), butylene rubber, polybutadiene, and polyisoprene rubber. Among them, from the viewpoint of low resistance of the undercoat layer, it is preferable that the synthetic rubber is appropriately mixed with a water-dispersible binder such as an emulsion of SBR, and it is more preferable that the synthetic rubber contains SBR. The synthetic rubber may be used alone or in combination of two or more kinds.
[0091] The shape of the synthetic rubber is not particularly limited, and it may be in the form of particles.
[0092] As the synthetic rubber, commercially available products may be used. Examples of commercially available synthetic rubber products include "TRD2001" (aqueous dispersion of styrene butadiene rubber particles) manufactured by JSR Corporation.
[0093] (1.4.6) Non-solids The composition of the present disclosure may contain non-solid contents. Examples of the non-solid contents include various blending components derived from the slurry for the undercoat layer (e.g., surfactants, dispersants, wetting agents, defoamers, etc.), water, etc.
[0094] The composition of the present disclosure further contains an additive (D), and the content of the additive (D) is 1 mass% to 50 mass% based on the total amount of the composition, and the additive (D) preferably contains carboxymethyl cellulose, which can stabilize the dispersion of the fine particles in the undercoat slurry.
[0095] The composition of the present disclosure further contains an additive (D), and the content of the additive (D) is 1 mass % to 50 mass % based on the total amount of the composition, and the additive (D) preferably contains at least one of a thermally expandable microcapsule and an inorganic oxide filler having a maximum volume expansion temperature of 70° C. to 180° C. This makes it easier for the olefin resin (B) to exhibit the shutdown function.
[0096] The composition of the present disclosure further contains an additive (D), the content of the additive (D) is 1 mass% to 50 mass% based on the total amount of the composition, and the additive (D) preferably contains aluminum oxide, which makes it easier for the olefin resin (B) to exhibit the shutdown function.
[0097] (1.5) Physical properties of the composition Various physical properties of the composition of the present disclosure will be described.
[0098] In the composition of the present disclosure, from the viewpoint of forming an electrode which is excellent in safety, has low DC resistance during initial charging and discharging, and is suppressed from increasing in DC resistance in a high-temperature environment, the ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) measured by a laser light diffraction scattering method is preferably 35 or less.
[0099] "Particle size distribution D99 measured by laser light diffraction scattering method" refers to the particle size corresponding to the cumulative 99% by volume from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on the laser light diffraction scattering method. The method for measuring D99 is the same as that described in the Examples. "Particle size distribution D10 measured by laser light diffraction scattering method" refers to the particle size corresponding to 10% by volume cumulative from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D10 is the same as that described in the Examples.
[0100] The ratio (D99 / D10) of 35 or less indicates that the number of aggregates of the components in the composition is small (in other words, the number of components dispersed in the composition is large). That is, the lower the ratio (D99 / D10), the fewer the number of aggregates of the components in the composition. The conductive carbon material (A) in the composition is uniformly dispersed, and a uniform conductive path is easily formed in the undercoat layer. This makes it possible to suppress the initial DC resistance of the battery charge / discharge and the increase in DC resistance after long-term storage in a high-temperature environment. Furthermore, the olefin resin (B) and the acrylic water-soluble polymer (C) in the composition are uniformly dispersed, making it easier to efficiently exert the shutdown function. As a result, the composition of the present disclosure is excellent in safety, and makes it possible to form an electrode in which the DC resistance at the initial stage of charge / discharge is kept low and the increase in DC resistance in a high-temperature environment is significantly suppressed. Therefore, a lithium-ion secondary battery with excellent battery performance is obtained.
[0101] From the viewpoint of improving the safety and battery performance of the lithium ion secondary battery, the ratio (D99 / D10) is more preferably from 3.0 to 30.0, further preferably from 3.0 to 22.0, and particularly preferably from 3.0 to 15.0.
[0102] Methods for adjusting the ratio (D99 / D10) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a film mix, ultrasonic waves, and a high-pressure homogenizer.
[0103] In the composition of the present disclosure, the particle size distribution D99 measured by a laser light diffraction scattering method is preferably 20 μm or less. The smaller the aggregates of the fine particles, the better the dispersibility of the materials contained in the composition. When D99 is 20 μm or less, it is easier to improve the safety and battery performance of the lithium ion secondary battery compared to when D99 exceeds 20 μm. From the viewpoint of improving the safety and battery performance of the lithium ion secondary battery, D99 of the composition is more preferably 2.0 μm to 20.0 μm, further preferably 2.0 μm to 15.0 μm, and particularly preferably 2.0 μm to 10.0 μm.
[0104] Methods for adjusting the D99 of the composition to within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a Disper, a Filmix, ultrasonic waves, and a high-pressure homogenizer.
[0105] The composition of the present disclosure has a particle size distribution D10 measured by a laser light diffraction scattering method of preferably 0.1 μm to 1.5 μm, more preferably 0.1 μm to 1.0 μm, and even more preferably 0.1 μm to 0.7 μm. When D10 is within the above range, the dispersibility of the materials contained in the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are more easily improved than when D10 is not within the above range.
[0106] Methods for adjusting D10 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0107] In the composition of the present disclosure, the ratio (D99 / D50) of the particle size distribution D99 to the particle size distribution D50 (also simply referred to as "D50") measured by a laser light diffraction scattering method is preferably 20 or less. The ratio (D99 / D50) being 20 or less indicates that the size of the aggregates is suppressed relative to the median diameter of the fine particles in the composition. The ratio (D99 / D50) being 20 or less provides excellent dispersibility of the composition. This makes it easier to improve the safety and battery performance of the lithium ion secondary battery compared to when the ratio (D99 / D50) is more than 20. From the viewpoint of improving the safety and battery performance of the lithium ion secondary battery, the ratio (D99 / D50) is more preferably 2.0 to 16.0, even more preferably 2.0 to 10.0, and particularly preferably 2.0 to 6.0.
[0108] "Particle size distribution D50 measured by laser light diffraction scattering method" refers to the particle size corresponding to cumulative 50 volume % from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D50 is the same as that described in the Examples.
[0109] Methods for adjusting the ratio (D99 / D50) within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, an ultrasonic wave, and a high-pressure homogenizer.
[0110] The particle size distribution D50 of the composition of the present disclosure measured by a laser light diffraction scattering method is not particularly limited, and is preferably 0.5 μm to 5.0 μm, more preferably 0.5 μm to 3.0 μm, and further preferably 0.5 μm to 2.0 μm. If D50 is within the above range, the dispersibility of the composition is excellent, and the safety and battery performance of the lithium ion secondary battery are likely to be improved.
[0111] Methods for adjusting D50 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0112] The composition of the present disclosure has a particle size distribution D90 (also simply referred to as "D90") measured by a laser light diffraction scattering method of preferably 1.0 μm to 10.0 μm, more preferably 1.0 μm to 7.0 μm, and even more preferably 1.0 μm to 4.0 μm. When D90 is within the above range, the composition has excellent dispersibility, and the safety and battery performance of the lithium ion secondary battery are easily improved. "Particle size distribution D90 measured by laser light diffraction scattering method" refers to the particle size corresponding to cumulative 90 volume % from the fine particle side in the volume-based particle size distribution measured by a particle size distribution measuring device based on laser light diffraction scattering method. The method for measuring D90 is the same as the method described in the Examples.
[0113] Methods for adjusting D90 within the above range include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a filmix, ultrasonic waves, and a high-pressure homogenizer.
[0114] (1.6) Preferred composition Regarding the content ratios of the above-mentioned conductive carbon material (A), olefin resin (B) and acrylic water-soluble polymer (C), from the viewpoint of effectively exerting the shutdown function and maintaining the battery performance, it is preferable that the content of the conductive carbon material (A) is 1 mass % to 30 mass % relative to the total amount of the composition, the content of the olefin resin (B) is 30 mass % to 90 mass % relative to the total amount of the composition, and the content of the acrylic water-soluble polymer (C) is 1 mass % to 20 mass % relative to the total amount of the composition.
[0115] (1.6.1) Preferred composition (i) In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirement (a1), which allows the conductive carbon material (A) and the olefin resin (B) to have excellent adhesion to each other and maintain the electrolyte performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1) and (a2), which improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), and (a3), which improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), and (a4), which allows the energy density of the lithium secondary battery to be maintained and improves the balance between the effective exertion of the shutdown function and the maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), (a4), and (a5), which provide an electrode with excellent resistance to high-temperature treatment, maintain the energy density of the lithium secondary battery, and improve the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (a1), (a2), (a3), (a4), (a5), and (a6), which, when applied to a lithium secondary battery equipped with an electrode, can provide a lithium ion secondary battery with a better balance between safety and battery performance (i.e., output and life).
[0116] (1.6.1.1) Requirements (a1) ~ Requirements (a6) Requirement (a1): The content of the structural unit derived from (meth)acrylamide is 60% by mass to 85% by mass based on the total amount of the acrylic water-soluble polymer (C). Requirement (a2): The content of the conductive carbon material (A) is 10% by mass to 20% by mass with respect to the total amount of the composition. Requirement (a3): The content of the olefin resin (B) is 60% by mass to 80% by mass based on the total amount of the composition. Requirement (a4): The particle size of the olefin resin (B) is 1 μm to 3 μm. Requirement (a5): The softening point of the olefin resin (B) must be 120°C or higher. Requirement (a6): The composition of the present disclosure further contains an additive (D), and the additive (D) contains CMC.
[0117] (1.6.2) Preferred composition (ii) In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirement (b1), which allows the conductive carbon material (A) and the olefin resin (B) to have excellent adhesion to each other and maintain the electrolyte performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1) and (b2), which improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), and (b3), which improves the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), and (b4), which allows the energy density of the lithium secondary battery to be maintained and improves the balance between the effective exertion of the shutdown function and the maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), (b4), and (b5), which provide an electrode with excellent resistance to high-temperature treatment, maintain the energy density of the lithium secondary battery, and improve the balance between effective exertion of the shutdown function and maintenance of battery performance. In addition to the above-mentioned configuration, the composition of the present disclosure preferably satisfies the following requirements (b1), (b2), (b3), (b4), (b5), and (b6), which, when applied to a lithium secondary battery equipped with an electrode, can provide a lithium ion secondary battery with a particularly excellent balance between safety and battery performance (i.e., output and life).
[0118] (1.6.2.1) Requirements (b1) ~ Requirements (b6) Requirement (b1): The content of the structural unit derived from (meth)acrylamide is 60% by mass to 85% by mass based on the total amount of the acrylic water-soluble polymer (C). Requirement (b2): The content of the conductive carbon material (A) is 10% by mass to 20% by mass with respect to the total amount of the composition. Requirement (b3): The content of the olefin resin (B) is 70% by mass to 80% by mass based on the total amount of the composition. Requirement (b4): The particle size of the olefin resin (B) is 1 μm to 2 μm. Requirement (b5): The softening point of the olefin resin (B) must be 120°C or higher. Requirement (b6): The composition of the present disclosure further contains an additive (D), and the additive (D) contains CMC.
[0119] (1.7) Method for producing the composition The method for producing the composition of the present disclosure preferably includes mixing the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) to prepare a mixture (hereinafter also referred to as the "mixing step"), and dispersing the mixture using a dispersing roll (hereinafter also referred to as the "dispersing step"). The mixing step and the dispersing step can be performed in this order, and when performed in this order, another step (for example, a step of kneading the mixture) may be included between the mixing step and the dispersing step.
[0120] (1.7.1) Mixing process In the mixing step, the conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) are mixed to prepare a mixture. The mixing method is not particularly limited and may be any known method. The amounts of the conductive carbon material (A), the olefin resin (B), and the water-soluble acrylic polymer (C) are the same as the ranges already described for the contents of the conductive carbon material (A), the olefin resin (B), and the water-soluble acrylic polymer (C) in the composition of the present disclosure.
[0121] (1.7.2) Dispersion process In the dispersion step, the mixture is dispersed using a dispersion roll. This results in a composition in which the raw materials are more dispersed than in the mixture before the dispersion step. As a result, when the electrode thus prepared is provided in a secondary battery, the obtained composition can not only reduce the DC resistance during initial charging and discharging, but also effectively suppress an increase in DC resistance in a high-temperature environment, compared to a case in which the dispersion step is not performed. The treatment of dispersing the mixture using a dispersing roll is also called a “dispersion treatment.” The mixture may be kneaded in advance before the dispersion treatment.
[0122] The dispersion method is not particularly limited, and examples thereof include a method using a kneading device. Examples of the kneading device include a kneader, a two-roll mill, a three-roll mill, a planetary mixer, a ball mill, a horizontal sand mill, a vertical sand mill, an annular bead mill, an attritor, a high shear mixer, a disperser, a film mix, an ultrasonic wave, and a high-pressure homogenizer. Among them, the kneading device is preferably a three-roll mill from the viewpoint of dispersing the fine particles more uniformly in the mixture. When a kneading device is used, the method of dispersing the mixture includes batch dispersion, pass dispersion, and circulation dispersion. The method of dispersing the mixture may be a combination of two or more methods. "Batch dispersion" refers to a method of dispersing the mixture using only a kneading device without using piping or the like. "Pass dispersion" refers to a method of dispersing the mixture by passing the mixture through the kneading device using a kneading system. The kneading system includes a kneading device, a first tank that supplies the mixture to the kneading device through piping, and a second tank that receives the mixture after the kneading process. "Circulation dispersion" refers to a method of dispersing the mixture by returning the mixture after the kneading process in the second tank to the first tank and circulating it.
[0123] The three-roll mill will be described with reference to Fig. 4. In Fig. 4, the reference character D1 indicates the rotation direction of the first roll 91 (hereinafter also referred to as the "feed roll 91"). The reference character D2 indicates the rotation direction of the second roll 92 (hereinafter also referred to as the "intermediate roll 92"). The reference character D3 indicates the rotation direction of the third roll 93 (hereinafter also referred to as the "finishing roll 93").
[0124] As shown in Fig. 4, the three-roll mill 90 includes a feed roll 91, an intermediate roll 92, a finishing roll 93, and a blade 94. The feed roll 91 and the intermediate roll 92 are disposed with a first distance L1 (see Fig. 4) between them. The intermediate roll 92 and the finishing roll 93 are disposed with a second distance L2 (see Fig. 4) between them. The blade 94 is disposed so as to come into contact with the surface of the finishing roll 93.
[0125] In the three-roll mill 90, as shown in Fig. 4, the mixture 1110 is stored in the upper space formed by the feed roll 91 and the intermediate roll 92. The mixture 1110 attached to the surface of the feed roll 91 is transferred to the surface of the intermediate roll 92. The mixture 1110 attached to the surface of the intermediate roll 92 is transferred to the surface of the finishing roll 93. The mixture 1110 attached to the surface of the finishing roll 93 is scraped off by the blade 94.
[0126] Each of the feed roll 91, the intermediate roll 92, and the finishing roll 93 may be a roll used in a known three-roll mill. The feed roll 91, the intermediate roll 92, and the finishing roll 93 each have approximately the same diameter. The blade 94 may be, for example, a doctor blade.
[0127] The rotation speeds of the feed roll 91, the intermediate roll 92, and the finishing roll 93 are not particularly limited, and may be in the order of speed from the feed roll 91, the intermediate roll 92, to the finishing roll 93. The rotation speed of the feed roll 91 is not particularly limited, but is preferably 5 rpm (revolutions per minute) to 84 rpm, and more preferably 16 rpm to 56 rpm. The rotation speed of the intermediate roll 92 is not particularly limited, but is preferably 16 rpm to 240 rpm, and more preferably 50 rpm to 160 rpm. The rotation speed of the finishing roll 93 is not particularly limited, but is preferably 50 rpm to 600 rpm, and more preferably 150 rpm to 400 rpm. The ratio of the rotation speed of the intermediate roll 92 to the rotation speed of the charge roll 91 (rotation speed of the intermediate roll 92 / rotation speed of the charge roll 91) is preferably 2.0 to 4.0, more preferably 2.5 to 3.5, from the viewpoint of uniformly dispersing the fine particles in the mixture. The ratio of the rotation speed of the finishing roll 93 to the rotation speed of the charge roll 91 (rotation speed of the finishing roll 93 / rotation speed of the charge roll 91) is preferably 5.0 to 12.0, more preferably 6.5 to 10.0, from the viewpoint of uniformly dispersing the fine particles in the mixture.
[0128] The first interval L1 is not particularly limited, and from the viewpoint of uniformly dispersing the fine particles in the mixture, it is preferably 0 mm to 0.05 mm, and more preferably 0 mm to 0.02 mm. The second distance L2 is not particularly limited, and is preferably 0 mm to 0.05 mm, and more preferably 0 mm to 0.02 mm, from the viewpoint of uniformly dispersing the fine particles in the mixture.
[0129] The number of dispersion treatments (hereinafter also referred to as the "number of treatments") may be one or more. In particular, the number of treatments is preferably three. When the number of treatments is three, the conductive carbon material (A) and the olefin resin (B) in the mixture are more likely to be uniformly dispersed than when the number of treatments is two or less or four or more. As a result, a composition is obtained that can be used to form a lithium ion secondary battery in which the DC resistance at the beginning of charging and discharging and the increase in the DC resistance under a high-temperature environment (especially after long-term storage) are more effectively suppressed.
[0130] (2) Undercoat The undercoat layer of the present disclosure contains the composition of the present disclosure described above. The composition of the present disclosure is as described above, so a description thereof will be omitted here.
[0131] The thickness of the undercoat layer is not particularly limited. The thickness of the undercoat layer is preferably 50 μm or less, more preferably 20 μm or less, from the viewpoint of suppressing the DC resistance of the lithium ion secondary battery in normal operation. The thickness of the undercoat layer is preferably 0.1 μm or more, more preferably 0.2 μm or more, from the viewpoint of increasing the DC resistance when the lithium ion secondary battery is abnormally heated and more reliably expressing the shutdown function.
[0132] The position where the undercoat layer is formed is preferably at least a part of at least one of the main surfaces of the positive electrode current collector, and may be appropriately selected depending on the coating pattern of the positive electrode mixture layer (for example, intermittent coating, stripe coating, etc.).
[0133] (3) Electrode The electrode of the present disclosure includes a current collector, the undercoat layer of the present disclosure described above, and a composite layer. The term "electrode" refers to at least one of the positive electrode and the negative electrode of a lithium ion secondary battery.
[0134] Since the electrode of the present disclosure has the above-mentioned configuration, it is possible to fabricate a lithium ion secondary battery that is excellent in safety and in which an increase in DC resistance is suppressed during the initial charge / discharge period and in high-temperature environments (especially after long-term storage).
[0135] In the electrode of the present disclosure, it is preferable that the electrode has a current collector, an undercoat layer, and a composite layer laminated in this order. As a result, the electrode of the present disclosure increases the electrical resistance between the current collector and the composite layer when the temperature of the lithium ion secondary battery rises suddenly. This suppresses overheating of the lithium ion secondary battery. Therefore, the electrode of the present disclosure can improve the safety of the lithium ion secondary battery. Furthermore, the electrode of the present disclosure can suppress an increase in the DC resistance of the lithium ion secondary battery even if the lithium ion secondary battery is stored for a long period of time in a high-temperature environment.
[0136] The electrode of the present disclosure may be a positive electrode or a negative electrode. Among them, the electrode of the present disclosure is preferably a positive electrode. When the electrode of the present disclosure is a positive electrode, the electric resistance of the positive electrode increases, so that the resulting lithium ion secondary battery can exhibit a good shutdown function.
[0137] (3.1) Positive electrode The positive electrode of the present disclosure may include a current collector (hereinafter also referred to as a "positive electrode current collector"), an undercoat layer, and a mixture layer (hereinafter also referred to as a "positive electrode mixture layer").
[0138] Positive electrodes of the present disclosure include a first positive electrode configuration, a second positive electrode configuration, a third positive electrode configuration, and a fourth positive electrode configuration. The first positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on both main surfaces of a current collector. The second positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode mixture layer are laminated in this order on one main surface of a current collector, and a positive electrode mixture layer is laminated on the other main surface of the current collector. The fourth positive electrode configuration indicates a configuration in which an undercoat layer and a positive electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the positive electrode composite layer is laminated on the other main surface of the current collector.
[0139] (3.1.1) Positive electrode current collector Examples of the material of the positive electrode current collector include aluminum, nickel, stainless steel (SUS), copper, etc. "Aluminum" includes pure aluminum and aluminum alloys.
[0140] (3.1.2) Undercoat layer The details of the undercoat layer and the composition forming it have been described above, and therefore a detailed description thereof will be omitted here.
[0141] (3.1.3) Positive electrode composite layer The positive electrode mixture layer contains a positive electrode active material and a binder.
[0142] (3.1.3.1) Positive electrode active material The positive electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions, and can be appropriately adjusted depending on the application of the lithium ion secondary battery.
[0143] Examples of the positive electrode active material include a first oxide and a second oxide. The first oxide contains lithium (Li) and nickel (Ni) as constituent metal elements. The second oxide contains Li, Ni, and at least one metal element other than Li and Ni as constituent metal elements. Examples of metal elements other than Li and Ni include transition metal elements and typical metal elements. The second oxide preferably contains the metal elements other than Li and Ni in an amount equivalent to or less than Ni in terms of atomic number. The metal elements other than Li and Ni may be, for example, at least one selected from the group consisting of Co, Mn, Al, Cr, Fe, V, Mg, Ca, Na, Ti, Zr, Nb, Mo, W, Cu, Zn, Ga, In, Sn, La, and Ce. The positive electrode active material may be used alone or in combination of two or more.
[0144] The positive electrode active material preferably contains a lithium-containing composite oxide (hereinafter, sometimes referred to as "NCM") represented by the following formula (X). The lithium-containing composite oxide (X) has the advantages of high energy density per unit volume and excellent thermal stability.
[0145] LiNi a Co b Mn c O2… Formula (X)
[0146] In formula (X), a, b and c each independently represent more than 0 and less than 1, and the sum of a, b and c is 0.99 to 1.00.
[0147] A specific example of NCM is LiNi 0.33 Co 0.33 Mn 0.33 O2, LiNi 0.5 Co 0.3 Mn 0.2 O2, LiNi 0.5 Co 0.2 Mn 0.3 O2, LiNi 0.6 Co 0.2 Mn 0.2 O2, LiNi 0.8 Co 0.1 Mn 0.1 Examples include O2.
[0148] The positive electrode active material may contain a lithium-containing composite oxide (hereinafter sometimes referred to as "NCA") represented by the following formula (Y).
[0149] Li t Ni 1-x-y Co x Al y O2… Formula (Y)
[0150] In formula (Y), t is 0.95 to 1.15, x is 0 to 0.3, y is 0.01 to 0.2, and the sum of x and y is less than 0.5.
[0151] A specific example of NCA is LiNi 0.8 Co 0.15Al 0.05 Examples include O2.
[0152] The content of the positive electrode active material is preferably 10 mass % or more, more preferably 30 mass % or more, still more preferably 50 mass % or more, and particularly preferably 70 mass % or more, based on the total amount of the positive electrode mixture layer. The content of the positive electrode active material is preferably 99.9 mass % or less, and more preferably 99 mass % or less, based on the total amount of the positive electrode mixture layer.
[0153] (3.1.3.2) Binder Examples of the binder include polyvinyl acetate, polymethyl methacrylate, nitrocellulose, fluororesin, and rubber particles. Examples of fluororesins include polytetrafluoroethylene (PTFE), polyvinylidene fluoride (PVDF), tetrafluoroethylene-hexafluoropropylene copolymer (FEP), vinylidene fluoride-hexafluoropropylene copolymer, and the like. Examples of the rubber particles include styrene-butadiene rubber particles and acrylonitrile rubber particles. Among these, from the viewpoint of improving the oxidation resistance of the positive electrode mixture layer, it is preferable that the binder contains a fluororesin. The binder may be used alone or in combination of two or more kinds. The content of the binder is preferably 0.1% by mass to 4% by mass based on the total amount of the positive electrode mixture layer from the viewpoint of achieving both the physical properties of the positive electrode mixture layer (eg, electrolyte permeability, peel strength, etc.) and the battery performance.
[0154] (3.1.3.3) Conductive additives The positive electrode mixture layer may further contain a conductive assistant. As the conductive assistant, a known conductive assistant can be used. As the known conductive assistant, a conductive carbon material is preferable. As the conductive carbon material, graphite, carbon black, conductive carbon fiber, fullerene, etc. can be mentioned. As the conductive carbon fiber, carbon nanotube, carbon nanofiber, carbon fiber, etc. can be mentioned. As the graphite, for example, artificial graphite, natural graphite, etc. can be mentioned. As the natural graphite, for example, flake graphite, lump graphite, and earthy graphite can be mentioned. The conductive assistant may be used alone or in combination of two or more kinds. The material of the conductive assistant may be a commercially available product.
[0155] (3.1.3.4) Other ingredients The positive electrode mixture layer may contain other components such as a thickener, a surfactant, a dispersant, a wetting agent, and a defoamer.
[0156] (3.2) Negative electrode The negative electrode of the present disclosure includes a current collector (hereinafter also referred to as a "negative electrode current collector") and a mixture layer (hereinafter also referred to as a "negative electrode mixture layer"), and may also include an undercoat layer.
[0157] Negative electrodes of the present disclosure may include a first negative electrode configuration, a second negative electrode configuration, a third negative electrode configuration, and a fourth negative electrode configuration. The first negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on both main surfaces of a current collector. The second negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on one main surface of a current collector, and an undercoat layer is laminated on the other main surface of the current collector. The third negative electrode configuration shows a configuration in which an undercoat layer and a negative electrode mixture layer are laminated in this order on one main surface of a current collector, and a negative electrode mixture layer is laminated on the other main surface of the current collector. The fourth negative electrode configuration indicates a configuration in which an undercoat layer and a negative electrode composite layer are laminated in this order on one main surface of a current collector, and neither the undercoat layer nor the negative electrode composite layer is laminated on the other main surface of the current collector.
[0158] (3.2.1) Negative electrode current collector Examples of the material for the negative electrode current collector include copper, aluminum, nickel, stainless steel (SUS), and nickel-plated steel.
[0159] (3.2.2) Undercoat layer The undercoat layer is the same as that exemplified as the undercoat layer of the positive electrode.
[0160] (3.2.3) Negative electrode composite layer The negative electrode mixture layer contains a negative electrode active material and a binder.
[0161] (3.2.3.1) Negative electrode active material The negative electrode active material is not particularly limited as long as it is a material capable of absorbing and releasing lithium ions. The negative electrode active material is preferably at least one selected from the group consisting of, for example, metallic lithium, lithium-containing alloys, metals or alloys capable of alloying with lithium, oxides capable of doping and dedoping lithium ions, transition metal nitrides capable of doping and dedoping lithium ions, and carbon materials capable of doping and dedoping lithium ions. Among these, the negative electrode active material is preferably a carbon material capable of doping and dedoping lithium ions (hereinafter referred to as "carbon material").
[0162] Examples of carbon materials include carbon black, activated carbon, graphite materials, and amorphous carbon materials. These carbon materials may be used alone or in combination of two or more. The form of the carbon material is not particularly limited, and may be, for example, fibrous, spherical, or flaky. The particle size of the carbon material is not particularly limited, and is preferably 5 μm to 50 μm, and more preferably 20 μm to 30 μm. Examples of amorphous carbon materials include hard carbon, coke, mesocarbon microbeads (MCMB) calcined at 1500° C. or less, and mesophase pitch carbon fiber (MCF). Examples of the graphite material include natural graphite and artificial graphite. Examples of the artificial graphite include graphitized MCMB and graphitized MCF. The graphite material may contain boron. The graphite material may be coated with a metal or amorphous carbon. Examples of the metal material that coats the graphite material include gold, platinum, silver, copper, and tin. The graphite material may be a mixture of amorphous carbon and graphite.
[0163] (3.2.3.2) Binder Examples of the binder contained in the negative electrode mixture layer include the same binders as those exemplified as the binder contained in the positive electrode mixture layer. The binder contained in the negative electrode mixture layer may be the same as or different from the binder contained in the positive electrode mixture layer. The content of the binder contained in the negative electrode mixture layer is not particularly limited, and may be the same as the exemplified content of the binder contained in the positive electrode mixture layer.
[0164] (3.2.3.3) Conductive additives The negative electrode mixture layer preferably contains a conductive assistant. Examples of the conductive assistant include the same conductive assistants as those exemplified as the conductive assistants that can be contained in the positive electrode mixture layer.
[0165] (3.2.3.4) Other ingredients In addition to the above components, the negative electrode mixture layer may contain other components, such as a thickener, a surfactant, a dispersant, a wetting agent, and a defoamer.
[0166] The electrode of the present disclosure preferably has a current collector, an undercoat layer, and a composite layer laminated in this order.
[0167] (4) Lithium-ion secondary battery The lithium ion secondary battery of the present disclosure includes the above-described electrode of the present disclosure. A lithium ion secondary battery generally includes an exterior body, electrodes (positive and negative electrodes), a separator, and an electrolyte. The exterior body accommodates the electrodes (positive and negative electrodes), the separator, and the non-aqueous electrolyte.
[0168] Hereinafter, an example will be described in which the positive electrode and the negative electrode are the electrodes of the present disclosure.
[0169] (4.1) Exterior body Examples of the exterior body include an exterior body including a laminate film, an exterior body consisting of a battery can and a battery can lid, etc. The shape of the exterior body is not particularly limited and is appropriately selected depending on the application of the lithium ion secondary battery, etc.
[0170] (4.2) Electrode The battery includes a positive electrode and a negative electrode as electrodes. The positive electrode is capable of absorbing and releasing lithium ions. The negative electrode is capable of absorbing and releasing lithium ions. In the lithium ion secondary battery of the present disclosure, at least one of the positive electrode and the negative electrode is the electrode of the present disclosure. When one of the positive electrode and the negative electrode of the lithium ion secondary battery of the present disclosure is the electrode of the present disclosure, the other of the positive electrode and the negative electrode may be a known electrode used in lithium ion secondary batteries.
[0171] (4.3) Separator The separator separates the positive electrode and the negative electrode. For example, a porous resin plate can be used as the separator. The material of the porous resin plate can be resin or nonwoven fabric containing the resin. Examples of the resin include polyethylene (PE), polypropylene (PP), polymethylpentene (PMP), polyester, cellulose, polyamide, and the like. Among them, the separator is preferably a porous resin sheet having a single layer or multilayer structure. The material of the porous resin sheet is mainly composed of one or more kinds of polyolefin resin. The thickness of the separator is preferably 5 μm to 30 μm. The separator is preferably disposed between the positive electrode and the negative electrode.
[0172] (4.4) Non-aqueous electrolyte The non-aqueous electrolyte contains an electrolyte and a non-aqueous solvent. (4.4.1) Electrolyte The electrolyte preferably contains at least one of a fluorine-containing lithium salt (hereinafter also referred to as a "fluorine-containing lithium salt") and a fluorine-free lithium salt.
[0173] Examples of the fluorine-containing lithium salt include inorganic acid anion salts and organic acid anion salts. Examples of inorganic acid anion salts include lithium hexafluorophosphate (LiPF6), lithium tetrafluoroborate (LiBF4), lithium hexafluoroarsenate (LiAsF6), and lithium hexafluorotantalate (LiTaF6). Examples of organic acid anion salts include lithium trifluoromethanesulfonate (LiCF3SO3). Among them, LiPF6 is particularly preferred as a fluorine-containing lithium salt. Examples of fluorine-free lithium salts include lithium perchlorate (LiClO4), lithium tetrachloroaluminate (LiAlCl4), and lithium decachlorodecaborate (Li2B 10 Cl 10 ) are mentioned.
[0174] When the electrolyte contains a fluorine-containing lithium salt, the content of the fluorine-containing lithium salt is preferably 50 mass % to 100 mass %, more preferably 60 mass % to 100 mass %, and further preferably 80 mass % to 100 mass %, based on the total amount of the electrolyte. When the fluorine-containing lithium salt contains lithium hexafluorophosphate (LiPF6), the content of lithium hexafluorophosphate (LiPF6) is preferably 50 mass% to 100 mass%, more preferably 60 mass% to 100 mass%, and even more preferably 80 mass% to 100 mass%, based on the total amount of the electrolyte.
[0175] When the non-aqueous electrolyte contains an electrolyte, the concentration of the electrolyte in the non-aqueous electrolyte is preferably 0.1 mol / L to 3 mol / L, and more preferably 0.5 mol / L to 2 mol / L. When the non-aqueous electrolyte contains lithium hexafluorophosphate (LiPF6), the concentration of lithium hexafluorophosphate (LiPF6) in the non-aqueous electrolyte is preferably 0.1 mol / L to 3 mol / L, and more preferably 0.5 mol / L to 2 mol / L.
[0176] (4.4.2) Nonaqueous solvents The non-aqueous electrolyte generally contains a non-aqueous solvent. Examples of non-aqueous solvents include cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, fluorine-containing chain carbonates, aliphatic carboxylic acid esters, fluorine-containing aliphatic carboxylic acid esters, γ-lactones, fluorine-containing γ-lactones, cyclic ethers, fluorine-containing cyclic ethers, chain ethers, fluorine-containing chain ethers, nitriles, amides, lactams, nitromethane, nitroethane, sulfolane, trimethyl phosphate, dimethyl sulfoxide, and dimethyl sulfoxide phosphate. The non-aqueous solvents may be used alone or in combination of two or more.
[0177] Examples of cyclic carbonates include ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of fluorine-containing cyclic carbonates include fluoroethylene carbonate (FEC), difluoroethylene carbonate (DFEC), and trifluoropropylene carbonate. Examples of chain carbonates include dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), and dipropyl carbonate (DPC). An example of the fluorine-containing chain carbonates is methyl 2,2,2-trifluoroethyl carbonate. Examples of the aliphatic carboxylate esters include methyl formate, methyl acetate, methyl propionate, methyl butyrate, methyl isobutyrate, methyl trimethylbutyrate, ethyl formate, ethyl acetate, ethyl propionate, ethyl butyrate, ethyl isobutyrate, and ethyl trimethylbutyrate. Examples of the fluorine-containing aliphatic carboxylates include methyl difluoroacetate, methyl 3,3,3-trifluoropropionate, ethyl difluoroacetate, and 2,2,2-trifluoroethyl acetate. Examples of γ-lactones include γ-butyrolactone and γ-valerolactone. Examples of cyclic ethers include tetrahydrofuran, 2-methyltetrahydrofuran, tetrahydropyran, 1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, and 1,4-dioxane. Examples of chain ethers include 1,2-ethoxyethane (DEE), ethoxymethoxyethane (EME), diethyl ether, 1,2-dimethoxyethane, and 1,2-dibutoxyethane. Examples of fluorine-containing chain ethers include HCF2CF2CH2OCF2CF2H, CF3CF2CH2OCF2CF2H, HCF2CF2CH2OCF2CFHCF3, CF3CF2CH2OCF2CFHCF3, and C6F 13 OCH3, C6F 13 OC2H5, C8F 17 OCH3, C8F 17 Examples include OC2H5, CF3CFHCF2CH(CH3)OCF2CFHCF3, HCF2CF2OCH(C2H5)2, HCF2CF2OC4H9, HCF2CF2OCH2CH(C2H5)2, and HCF2CF2OCH2CH(CH3)2. Examples of nitriles include acetonitrile, glutaronitrile, adiponitrile, methoxyacetonitrile, and 3-methoxypropionitrile. An example of the amides is N,N-dimethylformamide. Examples of lactams include N-methylpyrrolidinone, N-methyloxazolidinone, and N,N'-dimethylimidazolidinone.
[0178] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates. In this case, the total proportion of the cyclic carbonates, fluorine-containing cyclic carbonates, chain carbonates, and fluorine-containing chain carbonates is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the non-aqueous solvent.
[0179] The non-aqueous solvent preferably contains at least one selected from the group consisting of cyclic carbonates and chain carbonates. In this case, the total proportion of the cyclic carbonates and chain carbonates in the non-aqueous solvent is preferably 50% by mass to 100% by mass, more preferably 60% by mass to 100% by mass, and even more preferably 80% by mass to 100% by mass, based on the total amount of the non-aqueous solvent.
[0180] The content of the nonaqueous solvent is preferably 99% by mass or less, more preferably 97% by mass or less, and even more preferably 90% by mass or less, based on the total amount of the nonaqueous electrolyte. The content of the nonaqueous solvent is preferably 60% by mass or more, and even more preferably 70% by mass or more, based on the total amount of the nonaqueous electrolyte.
[0181] The intrinsic viscosity of the nonaqueous solvent is preferably 10.0 mPa·s or less at 25° C., from the viewpoint of further improving the dissociation property of the electrolyte and the mobility of ions.
[0182] (4.4.3) Electrolyte Additives The non-aqueous solvent may contain an electrolyte additive. This makes it possible to make it difficult for side reactions that are not the original battery reaction to proceed during the charge / discharge cycle of the lithium ion secondary battery. The battery reaction is a reaction in which lithium ions enter and leave (intercalate) the positive electrode and the negative electrode. The side reactions include a reductive decomposition reaction of the non-aqueous electrolyte by the negative electrode, an oxidative decomposition reaction of the non-aqueous electrolyte by the positive electrode, and elution of metal elements in the positive electrode active material. The electrolyte additive is not particularly limited, and any known additive can be used. For example, the additives described in JP-A-2019-153443 can be used.
[0183] (5) An example of a lithium-ion secondary battery An example of a lithium ion secondary battery according to an embodiment of the present disclosure will be specifically described with reference to Fig. 1 and Fig. 2. Fig. 1 is a schematic cross-sectional view of a lithium ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 2 is a schematic cross-sectional view of a positive electrode 11 in the lithium ion secondary battery 1 according to an embodiment of the present disclosure. Fig. 3 is a schematic cross-sectional view of a negative electrode 12 in the lithium ion secondary battery 1 according to an embodiment of the present disclosure.
[0184] The lithium ion secondary battery 1 according to the embodiment of the present disclosure is a laminated type. As shown in FIG. 1, the lithium ion secondary battery 1 includes a battery element 10, a positive electrode lead 21, a negative electrode lead 22, and an exterior body 30. The battery element 10 is enclosed inside the exterior body 30. The exterior body 30 is formed of a laminate film. The positive electrode lead 21 and the negative electrode lead 22 are attached to the battery element 10. The positive electrode lead 21 and the negative electrode lead 22 are led out in opposite directions from the inside to the outside of the exterior body 30.
[0185] As shown in FIG. 1, the battery element 10 is formed by laminating a positive electrode 11, a separator 13, and a negative electrode 12. 2, the positive electrode 11 is formed by forming a positive electrode composite layer 11B on both main surfaces of a positive electrode collector 11A with an undercoat layer. The positive electrode collector 11A with an undercoat layer is formed by forming an undercoat layer 111 on both main surfaces of a positive electrode collector 110. 3, negative electrode 12 is formed by forming negative electrode composite layer 12B on both main surfaces of undercoat layer-attached negative electrode current collector 12A. Undercoat layer-attached negative electrode current collector 12A is formed by forming undercoat layer 121 on both main surfaces of negative electrode current collector 120. As shown in FIG. 1, a positive electrode composite layer 11B formed on one main surface of a positive electrode collector 11A with an undercoat layer of a positive electrode 11 and a negative electrode composite layer 12B formed on one main surface of a negative electrode collector 12A with an undercoat layer of a negative electrode 12 adjacent to the positive electrode 11 are opposed to each other via a separator 13.
[0186] A non-aqueous electrolyte is injected into the interior of the exterior body 30. The non-aqueous electrolyte permeates the positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B. In the lithium-ion secondary battery 1, one unit cell layer 14 is formed by the adjacent positive electrode mixture layer 11B, the separator 13, and the negative electrode mixture layer 12B.
[0187] In this embodiment, the lithium ion secondary battery 1 is a laminated type, but the present disclosure is not limited thereto, and the lithium ion secondary battery 1 may be, for example, a wound type. The wound type is formed by stacking a positive electrode, a separator, a negative electrode, and a separator in this order and winding them into a layered shape. The wound type includes a cylindrical type and a rectangular type. 1, the directions in which the positive electrode lead 21 and the negative electrode lead 22 protrude from the inside of the exterior body 30 to the outside are opposite directions relative to the exterior body 30, but the present disclosure is not limited thereto. For example, the directions in which the positive electrode lead and the negative electrode lead protrude from the inside of the exterior body 30 to the outside may be the same direction relative to the exterior body 30. EXAMPLES
[0188] Hereinafter, the embodiments of the present disclosure will be described in detail with reference to examples. Note that the present disclosure is not limited to the description of these examples.
[0189] [1] Preparation The products used in the examples and comparative examples are as follows. The physical properties of each product are the catalog values.
[0190] [1.1] Conductive carbon material (A) Super-P: "Super-P" manufactured by TIMCAL (conductive carbon black, solid content: 100% by mass) KS-6: TIMREX's "KS-6" (flake graphite, solid content: 100% by mass)
[0191] [1.2] Olefin resin (B) W300: "Chemipearl (registered trademark) W300" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size (average primary particle size measured by the Cole counter method; the same applies below): 3.0 μm, softening point (ring and ball method): 132°C) W700: "Chemipearl (registered trademark) W700" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 132°C) W900: "Chemipearl (registered trademark) W900" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 132°C) W950: "Chemipearl (registered trademark) W950" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polyethylene, solid content concentration: 40% by mass, particle size: 0.6 μm, softening point (ring and ball method): 113°C) WP100: "Chemipearl (registered trademark) WP100" manufactured by Mitsui Chemicals, Inc. (water dispersion of low molecular weight polypropylene, solid content concentration: 40% by mass, particle size: 1.0 μm, softening point (ring and ball method): 148°C)
[0192] [1.3] Acrylic water-soluble polymer (C) As the acrylic water-soluble polymer (C), acrylic water-soluble polymer (C-1) to acrylic water-soluble polymer (C-5') were prepared as follows.
[0193] [1.3.1] Acrylic water-soluble polymer (C-1) A separable flask equipped with a stirrer and reflux cooling was charged with 240.0 parts by mass of distilled water, and the mixture was replaced with nitrogen gas and then heated to 70°C. Then, 0.6 parts by mass of ammonium persulfate was added, and the following water-soluble monomer raw material was added continuously over 3 hours, and the mixture was maintained for another 3 hours, and the pH was adjusted to 9.0 with aqueous ammonia to complete the polymerization. An appropriate amount of water was added to obtain an aqueous solution of an acrylic water-soluble polymer (C-1). The solid content of the aqueous solution of the acrylic water-soluble polymer (C-1) was 15.0%.
[0194] <Water-soluble monomer raw material> Methacrylamide 40.0 parts by mass Methacrylic acid 50.0 parts by mass 2-Hydroxyethyl methacrylate 10.0 parts by mass 25% ammonia water 50.0 parts by mass Distilled water 240.0 parts by weight
[0195] [1.3.1.2] Glass transition temperature (Tg) The glass transition temperature (Tg) of the water-soluble acrylic polymer (C-1) contained in the obtained aqueous solution was calculated by the following FOX equation (1). Formula (1): 1 / Tg=W1 / Tg1+W2 / Tg2+ +Wn / Tgn In equation (1), Tg is the glass transition temperature of the copolymer (unit: K), Tgi (i = 1, 2, ... n) is the glass transition temperature (unit: K) when monomer i forms a homopolymer, and Wi (i = 1, 2, ... n) is the mass fraction of monomer i in all monomers.
[0196] [1.3.2] Acrylic water-soluble polymers (C-2) to (C-5') Aqueous solutions of the acrylic water-soluble polymer (C-2) to the acrylic water-soluble polymer (C-5') were produced in the same manner as in Example 1, except that the formulation was changed according to the description in Table 1. The glass transition temperatures of the acrylic water-soluble polymer (C-2) to the acrylic water-soluble polymer (C-5') were determined in the same manner as in Example 1.
[0197] [Table 1]
[0198] In Table 1, "240 / 240" indicates that 240 parts by mass of distilled water was initially charged into the flask, and then 240 parts by mass of distilled water was used when dissolving the monomer.
[0199] [1.3.3] Comparative resin for acrylic water-soluble polymer (C) As comparative resins for the acrylic water-soluble polymer (C), the following resins were prepared. Polyacrylic acid: "Polyacrylic acid" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (polyacrylic acid aqueous solution, solids concentration: approximately 25% by mass) Polyacrylamide: "Polyacrylamide" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (polyacrylamide aqueous solution, solids concentration: approximately 10% by mass)
[0200] [1.4] Additives (D) CMC: "2200" manufactured by Daicel Miraize Co., Ltd. (sodium carboxymethylcellulose, solid content: 100% by mass) PVDF: Kureha Corporation's "W#7200" (vinylidene fluoride resin, solid content: 100% by mass) SBR: JSR Corporation's "TRD2001" (aqueous dispersion of styrene butadiene rubber particles, solid content: 50% by mass) MC: Matsumoto Microsphere (registered trademark) FN-100SS manufactured by Matsumoto Yushi Pharmaceutical Co., Ltd. (microcapsule, solid content concentration: 100% by mass, maximum volume expansion temperature: 180°C) Al2O3: "Aluminum oxide" manufactured by Fujifilm Wako Pure Chemical Industries, Ltd. (average particle size: 2 μm, solid content: 100% by mass)
[0201] Specific numerical values of the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "not more than" or "less than") or lower limit values (numerical values defined as "not less than" or "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Form for carrying out the invention." In addition, unless otherwise specified in the following description, "parts" and "%" are based on mass.
[0202] [2] Preparation of positive electrode current collector with undercoat layer [2.1] Preparation of slurry for undercoat layer Example 1 The slurry for the undercoat layer was prepared using a 5 L planetary dispenser. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used for dispersing the slurry for the undercoat layer. 58 parts by mass of "Super-P" (A) was pre-mixed for 5 minutes (preparation step A). 229.0 parts by mass of "CMC aqueous solution" (D) was added to the "Super-P" (A) powder and mixed for an additional 20 minutes to obtain a first mixture (Preparation step B). The "CMC aqueous solution" (D) was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.6% by mass relative to the total amount of the "CMC aqueous solution" (D). The first mixed solution was added with 527.8 parts by mass of "CMC aqueous solution" (D) and mixed for 20 minutes. This addition operation was repeated three times to obtain a second mixed solution (preparation step C). The total amount of "CMC aqueous solution" (D) added to the first mixed solution was 1583.4 parts by mass. To the second mixed liquid, 95.4 parts by mass of “acrylic water-soluble polymer (C-1)” (C) and 471.3 parts by mass of “W700” (B) were added, kneaded for 20 minutes, and vacuum degassed for 30 minutes to obtain a third mixed liquid (preparation step D). The third mixed solution was dispersed twice using a three-roll mill shown in Fig. 4 under the conditions of a roll gap of 10 μm and a roll rotation speed of 300 rpm (gear ratio 1:3:9) (preparation step E). That is, the rotation speed of the charge roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first gap L1 was 10 μm, and the second gap L2 was 10 μm. In this way, a slurry (composition) for the undercoat layer having a solid content concentration of 12.4 mass% was prepared (preparation step E).
[0203] (Examples 2 to 8, Comparative Examples 1 to 5) Except for changing the materials and amounts added in each of the preparation steps A to D as shown in Table 2, the same procedure as in Example 1 was carried out to prepare a slurry (composition) for an undercoat layer.
[0204] [Table 2]
[0205] In Table 2, "WSP" refers to an acrylic water-soluble polymer, "PA" refers to polyacrylic acid, and "PAA" refers to polyacrylamide.
[0206] Example 9 The slurry for the undercoat layer was prepared using a 5 L planetary dispenser. A three-roll mill (BR-300HCVIII, manufactured by Imex Co., Ltd.) was used for dispersing the slurry for the undercoat layer. 58 parts by mass of "Super-P" (A) and 87.0 parts by mass of "Al2O3" (D) were mixed for 10 minutes to obtain a mixture (preparation step A). The mixture was added with 550.0 parts by mass of "CMC aqueous solution" (D) and further mixed for 20 minutes to obtain a first mixed liquid (Preparation step B). "CMC aqueous solution" (D) was prepared by adding "CMC" (D) to distilled water so that the content of "CMC" (D) was 1.0% by mass relative to the total amount of "CMC aqueous solution" (D). The first mixed solution was added with 300.0 parts by mass of "CMC aqueous solution" (D) and mixed for 20 minutes. This addition operation was repeated three times to obtain a second mixed solution (preparation step C). The total amount of "CMC aqueous solution" (D) added to the first mixed solution was 900.0 parts by mass. To the second mixed solution, 95.4 parts by mass of “acrylic water-soluble polymer (C-3)” (C) and 290.0 parts by mass of “W700” (B) were added, kneaded for 20 minutes, and vacuum degassed for 30 minutes to obtain a third mixed solution (preparation step D). The third mixed solution was dispersed twice using a three-roll mill shown in Fig. 4 under the conditions of a roll gap of 10 μm and a roll rotation speed of 300 rpm (gear ratio 1:3:9) (Preparation step E). That is, the rotation speed of the charge roll 91 was 33.3 rpm, the rotation speed of the intermediate roll 92 was 100 rpm, the rotation speed of the finishing roll 93 was 300 rpm, the first gap L1 was 10 μm, and the second gap L2 was 10 μm. In this way, a slurry (composition) for the undercoat layer having a solid content concentration of 14.9 mass% was prepared (Preparation step E).
[0207] Example 10 Except for changing the additive materials in the preparation step A as shown in Table 3, the same procedure as in Example 9 was carried out to prepare slurries (compositions) for the undercoat layer.
[0208] [Table 3]
[0209] In Table 3, "WSP" refers to an acrylic water-soluble polymer.
[0210] [2.2] Coating and drying of undercoat layer The undercoat layer slurry was applied using a die coater. The coating thickness after drying is 3 μm (coating weight is about 0.2 mg / cm 2The slurry for the undercoat layer was applied to one main surface of an aluminum foil (thickness 20 μm, width 200 mm, positive electrode current collector) and dried so that the thickness of the coating after drying was 3 μm. Next, the slurry for the undercoat layer was similarly applied to the other main surface (uncoated surface) of the aluminum foil and dried so that the coating thickness after drying was 3 μm. In this way, an aluminum foil roll (positive electrode current collector with an undercoat layer) was obtained in which the undercoat layer was coated on both sides.
[0211] [3] Positive electrode preparation [3.1] Preparation of positive electrode mixture slurry A 5 L planetary dispenser was used to prepare the positive electrode mixture slurry. "NCM523" (Umicore, composition formula: LiNi 0.5 Co 0.2 Mn 0.3 O2), 30 parts by mass of "Super-P" (conductive carbon manufactured by TIMCAL) as a conductive additive, and 30 parts by mass of "KS-6" (flake graphite manufactured by TIMREX) as a conductive additive were mixed for 10 minutes to obtain a mixture for the positive electrode. 50 parts by mass of "NMP" was added to the mixture for the positive electrode, and mixed for 20 minutes to obtain a first mixture for the positive electrode. To the first positive electrode mixed solution, 350 parts by mass of "PVDF solution" was added and kneaded for 30 minutes, then 260 parts by mass of "PVDF solution" was added and kneaded for 15 minutes, and then 220 parts by mass of "PVDF solution" was added and kneaded for 15 minutes to obtain a second positive electrode mixed solution. The "PVDF solution" was prepared by adding "PVDF" to "NMP" so that the "PVDF" content was 8 mass% of the total amount of "PVDF solution". To adjust the viscosity, 80 parts by mass of "NMP" was added to the second positive electrode mixture, which was mixed for 30 minutes and then vacuum degassed for 30 minutes. In this way, a positive electrode mixture slurry with a solid content concentration of 65 mass % was prepared.
[0212] [3.2] Coating and drying The positive electrode mixture slurry was applied using a die coater. The mass of the positive electrode mixture layer (coating film after drying) is 19.0 mg / cm2 The positive electrode mixture slurry was applied onto one main surface (i.e., the undercoat layer) of a positive electrode current collector with an undercoat layer (aluminum foil thickness: 20 μm, thickness of one undercoat layer: 3 μm, width: 200 mm) and dried so that the mass of the positive electrode mixture layer (coated film after drying) became 19.0 mg / cm 2 The positive electrode mixture slurry was similarly applied onto the other main surface (that is, the undercoat layer) of the positive electrode current collector with the undercoat layer so that the positive electrode mixture slurry became equal to or larger than the undercoat layer, and then dried. The positive electrode roll thus obtained (the total amount of coating on both sides is 38.0 mg / cm 2 ) was dried in a vacuum drying oven at 130°C for 12 hours.
[0213] [3.3] Press A 35-ton press was used to press the positive electrode roll. The gap between the upper and lower rolls was adjusted to press the positive electrode to a density of 2.9±0.05 g / cm. 3 The mixture was pressed using a 35 ton press so that the thickness became
[0214] [3.4] Slit The positive electrode roll was slit so as to obtain the area of the positive electrode composite layer (front surface: 56 mm × 334 mm, back surface: 56 mm × 408 mm) and an area for tab welding margins, thereby obtaining a positive electrode in which an undercoat layer was laminated on the aluminum foil.
[0215] [4] Negative electrode production [4.1] Preparation of negative electrode mixture slurry A 5 L planetary dispenser was used to prepare the negative electrode mixture slurry. 1050 parts by mass of "natural graphite" as the negative electrode active material and "Super-P" (conductive carbon, BET specific surface area 62 m) as the conductive additive 2 The mixture was mixed for 10 minutes to obtain a negative electrode mixture. To the mixture for the negative electrode, 450 parts by mass of the "CMC aqueous solution" was added, and the mixture was further mixed for 20 minutes to obtain a first mixture for the negative electrode. To the first negative electrode mixed solution, 150 parts by mass of the "CMC aqueous solution" was added and mixed for an additional 30 minutes, then 293.5 parts by mass of the "CMC aqueous solution" was added and mixed for an additional 30 minutes, and 450 parts by mass of water as a solvent was added and mixed for 15 minutes to obtain a second negative electrode mixed solution. To the second negative electrode mixture, 45 parts by mass of "SBR aqueous solution" (manufactured by JSR Corporation, solid content concentration: 50% by mass) was added, and the mixture was kneaded for 15 minutes and then vacuum degassed for 10 minutes. In this way, a negative electrode mixture slurry with a solid content concentration of 45 mass % was prepared.
[0216] [4.2] Coating and drying The negative electrode mixture slurry was applied using a die coater. The mass of the negative electrode mixture layer (coating film after drying) is 11.0 mg / cm 2 The negative electrode mixture slurry was applied to one main surface of a copper foil (thickness 10 μm, negative electrode current collector) and dried so that the mass of the negative electrode mixture layer (coated film after drying) was 11.0 mg / cm. 2 The negative electrode composite slurry was applied to the other main surface of the copper foil and dried so that the negative electrode composite slurry was applied to the other main surface of the copper foil. 2 ) was dried in a vacuum drying oven at 120°C for 12 hours.
[0217] [4.3] Press A small press was used to press the negative electrode roll. The gap between the upper and lower rolls was adjusted to press the negative electrode roll to a density of 1.45±0.05g / cm. 3 The mixture was pressed using a small press so that the thickness became
[0218] [4.4] Slit The negative electrode roll was slit so as to obtain the area of the negative electrode mixture layer (front surface: 58 mm×372 mm, back surface: 58 mm×431 mm) and an area for a tab welding margin, thereby obtaining a negative electrode.
[0219] [5] Fabrication of a wound battery (design capacity 1Ah) [5.1] Winding The separator used was a polyethylene porous film (60.5 mm×450 mm) with a porosity of 45% by volume and a thickness of 25 μm. The negative electrode, separator, positive electrode with an undercoat layer, and separator obtained above were stacked and wound, and then press-molded. Next, an aluminum tab was bonded to the margin of the positive electrode with the undercoat layer by an ultrasonic bonding machine, and a nickel tab was bonded to the margin of the negative electrode by an ultrasonic bonding machine. This was sandwiched between laminate films, and three sides were heat-sealed. This resulted in an exterior body having an opening (hereinafter referred to as the "first exterior body").
[0220] [5.2] Injection of non-aqueous electrolyte Ethylene carbonate (EC), methyl ethyl carbonate (EMC), and dimethyl carbonate (DMC) were mixed in a volume ratio of EC:EMC:DMC=3:3:4 to obtain a mixed solvent. LiPF6 was dissolved in the mixed solvent to a concentration of 1.0 mol / L to prepare a non-aqueous electrolyte. Before injecting the non-aqueous electrolyte, the first exterior body was dried under reduced pressure at 70°C for 12 hours in a vacuum dryer. After injecting 4.7±0.1 g of electrolyte into the first exterior body, the opening of the first exterior body was heat sealed while drawing a vacuum. This produced a lithium ion secondary battery precursor.
[0221] [5.3] Activation process The lithium ion secondary battery precursor was kept at room temperature (25°C) for 24 hours. Next, the lithium ion secondary battery precursor was charged at a constant current of 0.05C (0.05C-CC) for 4 hours, and then rested for 12 hours. Then, it was charged at a constant current and constant voltage of 0.1C to 4.2V (0.1C-CCCV), rested for 30 minutes, and then discharged at a constant current of 0.1C to 2.8V (0.1C-CC). Furthermore, a charge-discharge cycle (charging to 4.2V at 0.1C-CCCV and discharging to 2.8V at 0.1C-CC) was repeated five times. Then, the lithium ion secondary battery precursor was stored at 25°C for five days in a fully charged state of 4.2V (SOC100%). In this way, wound-type batteries (lithium ion secondary batteries) of Examples 1 to 19, Comparative Examples 1 to 10, and Reference Example were obtained.
[0222] [6] Evaluation method The following particle size distribution measurements were performed on the slurries for undercoat layers prepared in Examples 1 to 10 and Comparative Examples 1 to 5. The following safety (heating), safety (nail penetration), initial DCIR, and DCIR after high-temperature storage were evaluated on the wound-type batteries of Examples 1 to 10, Comparative Examples 1 to 5, and the Reference Example. The evaluation results are shown in Table 5.
[0223] [6.1] Particle size distribution 1.0 g of the slurry for the undercoat layer (hereinafter also referred to as "sample") of Examples 1 to 10 and Comparative Examples 1 to 5 and 50 ml of water were placed in a 100 ml beaker, and the lumps of the sample were crushed with a spatula and mixed lightly with a dropper. Next, the sample was dispersed in water using a tabletop ultrasonic cleaner (Honda Electronics Co., Ltd., W-113 model). At this time, the tabletop ultrasonic cleaner was set to an output of 100 W and 28 kHz, and dispersion was performed for 60 seconds. Thereafter, bubbles formed on the surface of the aqueous solution in the beaker were removed, and the volume-based particle size distribution of the sample was measured by a laser light diffraction scattering method using a particle size distribution measuring device (Microtrac-Bell Co., Ltd., Microtrac MT3300EXII). From this measurement, D10, D50, D90 and D99 in the volume particle size distribution were obtained. The measurement results of D10, D50, D90 and D99 are shown in Table 5.
[0224] [6.2] Safety (heating) A wound battery (design capacity 1 Ah) was charged at 0.1 C at a constant current and constant voltage (0.1 C-CCCV) up to 4.2 V in a temperature environment of 25°C, and safety (heating) was evaluated. The measurement cell was placed in a thermostatic bath heated to 50°C, and the AC resistance was measured at 1 kHz (amplitude 10 mV) while the temperature of the thermostatic bath was raised at 5°C / min. The cell temperature was recorded as the temperature obtained by a temperature measurement terminal installed on the top surface of the cell. The AC resistance was measured using a ModuLab XM ECS electrochemical measurement system manufactured by Solartron.
[0225] From the measured resistance values, the resistance rise start temperature and the resistance change ratio were calculated. The resistance rise start temperature was calculated as the temperature at which the resistance value reached 1.5 times the resistance value at 50°C, which was set to 1. The resistance change ratio was calculated as the relative ratio of the resistance value at 150°C to the resistance value at 50°C, which was set to 1.
[0226] Using the measurement results of the resistance rise starting temperature and the resistance change ratio, the safety (heating) was evaluated according to the following criteria. Acceptable evaluations of safety (heating) are "A" and "B".
[0227] A: The resistance rise starting temperature is 90°C or less, and the resistance change rate is 20 times or more. B: The resistance rise starting temperature is more than 90° C., and the resistance change ratio is 20 times or more. Or, the resistance rise starting temperature is 90° C. or less, and the resistance change ratio is less than 20 times. C: The resistance rise starting temperature is more than 90°C, and the resistance change rate is less than 20 times.
[0228] [6.3] Forced internal short circuit test (nail penetration test) A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1C-CCCV) at 0.1C up to 4.2V in a temperature environment of 25°C, and a nail penetration test was performed (nail diameter 3mm, nail penetration speed 1.0mm / sec). A nail with a diameter of 3 mm was inserted into the center of the wound battery (cell) at a speed of 1.0 mm / sec to short-circuit the positive and negative electrodes inside the battery container. The short-circuit behavior of the battery was then observed. The nail penetration test was carried out on the same level of batteries multiple times (3 to 6 times) and the total number of test batteries was evaluated according to the following criteria. Acceptable evaluations for the nail penetration test are "A" and "B".
[0229] A: The percentage of batteries whose internal temperature exceeded 300°C was less than 10% of the total number of tested batteries. B: The percentage of batteries whose internal temperature exceeded 300°C was more than 10% and less than 60% of the total number of test batteries. C: The percentage of batteries whose internal temperature exceeded 300°C was 60% or more of the total number of test batteries.
[0230] [6.4] Initial DCIR Assessment [6.4.1] Initial DCIR measurement A wound battery (design capacity 1 Ah) was charged at a constant current and constant voltage (0.1C-CCCV) up to 4.2 V in a temperature environment of 25°C, and the initial DCIR was measured. The battery was discharged at a constant current of 0.1C for 10 seconds (0.1C-CC-10s) and then charged at a constant current of 0.1C for 10 seconds (0.1C-CC-10s). Next, the battery was discharged at a constant current of 0.2 C for 10 seconds (0.2C-CC-10s), and then charged at a constant current of 0.2 C for 10 seconds (0.2C-CC-10s). Next, the battery was discharged at a constant current of 0.5 C for 10 seconds (0.5C-CC-10s), and then charged at a constant current of 0.5 C for 10 seconds (0.5C-CC-10s). Next, the battery was discharged at a constant current of 1.0 C for 10 seconds (1.0 C-CC-10 s), and then charged at a constant current of 1.0 C for 10 seconds (1.0 C-CC-10 s). Next, the battery was discharged at a constant current of 2.0 C for 10 seconds (2.0C-CC-10s), and then charged at a constant current of 2.0 C for 10 seconds (2.0-CC-10s). The first DC resistance (DCIR) was calculated based on each voltage drop (=voltage before discharge started--voltage 10 seconds after discharge started) due to "CC10s discharge" at each discharge rate of 0.1C to 2.0C and each current value (i.e., each current value corresponding to discharge rates of 0.1C to 2.0C).
[0231] [6.4.2] Evaluation method Based on the above measured values, a first relative value was calculated with the measured value of the first direct current resistance (DCIR) of the reference example (without an undercoat layer) set at 100, and the initial DCIR was evaluated according to the following criteria. The first relative values of the first DC resistance are shown in Table 5. Acceptable ratings for the initial DCIR rating are "A" and "B".
[0232] A: The first relative value is 100 or less. B: The first relative value is greater than 100 and is 105 or less. C: The first relative value exceeds 105.
[0233] [6.5] DCIR evaluation after high temperature storage [6.5.1] DCIR measurement after high temperature storage The wound battery (design capacity 1 Ah) was charged at 0.1 C to 4.2 V at a constant current and constant voltage (0.1 C-CCCV) in a temperature environment of 25° C., and then left in a charged state for 28 days in an atmosphere of 60° C. Thus, a battery after high-temperature storage was obtained. A DCIR evaluation process similar to the above-mentioned initial DCIR evaluation process was performed to determine the second DCIR.
[0234] [6.5.2] Evaluation method Based on the above measured values, a second relative value was calculated with the measured value of the second direct current resistance (DCIR) of the reference example (without undercoat layer) set at 100, and the DCIR after high temperature storage was evaluated according to the following criteria. The second relative value of the second DC resistance is shown in Table 5. Acceptable ratings for the DCIR rating after high temperature storage are "A" and "B".
[0235] A: The second relative value is 105 or less. B: The second relative value is greater than 105 and is 110 or less. C: The second relative value exceeds 110.
[0236] [Table 4]
[0237] [Table 5]
[0238] In Tables 4 and 5, "MA" refers to a constituent unit derived from methacrylamide. "COOH" refers to a constituent unit derived from a vinyl monomer having a carboxy group. "OH" refers to a constituent unit derived from a vinyl monomer having a hydroxyl group. "Start temperature" refers to the temperature at which resistance rise begins. "Change ratio" refers to the resistance change ratio. "Initial" refers to the initial DCIR evaluation. "After high temperature storage" refers to the DCIR evaluation after high temperature storage. "PA" refers to polyacrylic acid. "PAA" refers to polyacrylamide.
[0239] The acrylic water-soluble polymers (C) of Comparative Examples 1 to 5 did not satisfy the following: the content of the constitutional unit derived from (meth)acrylamide is 35% (30% to 95% by mass) relative to the total amount of the acrylic water-soluble polymer (C), and the content of the constitutional unit derived from vinyl monomer is 5% to 65% (70% by mass) relative to the total amount of the acrylic water-soluble polymer (C). Therefore, in Comparative Example 1, the evaluation result of the DCIR evaluation after high-temperature storage was "C". In Comparative Examples 2 and 4, the evaluation results of the initial DCIR evaluation and the DCIR evaluation after high-temperature storage were "C". In Comparative Example 3, the evaluation results of the safety (heating), safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "C". In Comparative Example 5, the evaluation results of the safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "C". As a result, it was found that the compositions of Comparative Examples 1 to 5 are not suitable for forming electrodes that are safe, have low DC resistance during initial charging and discharging, and are suppressed from increasing in DC resistance under high temperature environments (especially after long-term storage).
[0240] The compositions of Examples 1 to 10 contained a conductive carbon material (A), an olefin resin (B), and an acrylic water-soluble polymer (C). The acrylic water-soluble polymer (C) satisfied the following: the content of the structural unit derived from (meth)acrylamide was 35% (30% to 95% by mass) relative to the total amount of the acrylic water-soluble polymer (C), and the content of the structural unit derived from a vinyl monomer was 5% to 65% (70% by mass) relative to the total amount of the acrylic water-soluble polymer (C). Therefore, in Examples 1 to 10, the evaluation results of safety (heating), safety (nail penetration), initial DCIR evaluation, and DCIR evaluation after high-temperature storage were "A" or "C". As a result, it was found that the compositions of Examples 1 to 10 are suitable for forming electrodes that are safe, have low DC resistance during initial charging and discharging, and suppress an increase in DC resistance in high-temperature environments (especially after long-term storage). [Explanation of symbols]
[0241] 1. Lithium-ion secondary battery 10 Battery element 11 Positive electrode 11A Positive electrode current collector with undercoat layer 11B Positive electrode composite layer 12 Negative electrode 12A Negative electrode current collector with undercoat layer 12B Negative electrode composite layer 13 Separator 14 Cell Layer 21 Positive lead 22 Negative lead 30 Exterior body 110 Positive electrode current collector 111,121 Undercoat layer 120 Negative electrode current collector
Claims
1. The conductive carbon material (A), the olefin resin (B), and the acrylic water-soluble polymer (C) are contained, the water-soluble acrylic polymer (C) has a structural unit derived from (meth)acrylamide and a structural unit derived from a vinyl monomer having at least one of a carboxy group and a hydroxyl group, the content of the (meth)acrylamide-derived structural unit is 35% by mass to 95% by mass based on the total amount of the acrylic water-soluble polymer (C); The content of the structural unit derived from the vinyl monomer having at least one of a carboxy group and a hydroxyl group is 5% by mass to 65% by mass based on the total amount of the water-soluble acrylic polymer (C).
2. The content of the conductive carbon material (A) is 1% by mass to 30% by mass based on the total amount of the composition; The content of the olefin resin (B) is 30% by mass to 90% by mass based on the total amount of the composition, The composition according to claim 1, wherein the content of the acrylic water-soluble polymer (C) is 1% by mass to 20% by mass based on the total amount of the composition.
3. The composition of claim 1 , wherein the olefin-based resin (B) comprises an ethylene-based resin or a propylene-based resin.
4. The particle size of the olefin-based resin (B) is 0.1 μm to 9.0 μm, The composition according to claim 1, wherein the olefin resin (B) has a softening point of 70°C or higher.
5. The composition according to claim 1, wherein the water-soluble acrylic polymer (C) has a structural unit derived from (meth)acrylamide, a structural unit derived from a vinyl monomer having a carboxy group, and a structural unit derived from a vinyl monomer having a hydroxyl group.
6. The composition according to claim 1 , wherein the water-soluble acrylic polymer (C) has a Tg of 150° C. or higher.
7. Further, it contains an additive (D), The composition according to claim 1, wherein the content of the additive (D) is 1 mass% to 50 mass% based on the total amount of the composition.
8. 8. The composition of claim 7, wherein the additive (D) comprises carboxymethyl cellulose.
9. The composition according to claim 7, wherein the additive (D) comprises at least one of a thermally expandable microcapsule having a maximum volume expansion temperature of 70°C to 180°C and an inorganic oxide filler.
10. 2. The composition according to claim 1, wherein the ratio of particle size distribution D99 to particle size distribution D10 (D99 / D10) is 35 or less, as measured by a laser light diffraction scattering method.
11. The composition according to claim 1, having a particle size distribution D99 measured by a laser light diffraction scattering method of 20 μm or less.
12. 2. The composition according to claim 1, wherein the ratio of particle size distribution D99 to particle size distribution D50 (D99 / D50) is 20 or less, as measured by a laser light diffraction scattering method.
13. An undercoat layer comprising the composition according to any one of claims 1 to 12.
14. An electrode comprising a current collector, the undercoat layer of claim 13, and a composite layer.
15. The electrode according to claim 14 , wherein the current collector, the undercoat layer, and the composite layer are laminated in this order.
16. A lithium ion secondary battery comprising the electrode according to claim 14.
Citation Information
Patent Citations
Electrochemical cell acrylic water dispersion and aqueous paste and manufacturing method of electrode and battery consisting of the same
JP2012151108A
Binder for carbon coat foil coating solution, carbon coat foil coating solution, carbon coat foil, electrode for lithium ion secondary battery, and lithium ion secondary battery
JP2013229187A
Aqueous solution of thermally crosslinkable binder for lithium ion battery, electrode slurry for lithium ion battery and manufacturing method thereof, electrode for lithium ion battery, and lithium ion battery
JP2020024896A
PTC functional composition, PTC functional composition layer, coated current collector for non-aqueous electrolyte secondary battery, electrode for non-aqueous electrolyte secondary battery, and non-aqueous electrolyte secondary battery
JP2023147402A
Electrically conductive composition, under layer-attached current collector for electric storage devices, electrode for electric storage devices, and electric storage device
WO2016158480A1