Modified ethylene-vinyl alcohol-based resin composition, gas barrier material using same and method for producing same

A modified ethylene-vinyl alcohol resin composition with specific structural and compositional parameters addresses the challenges of high humidity gas barrier performance, biodegradability, and thermal stability, ensuring effective use in gas barrier materials.

JP2024140980APending Publication Date: 2024-10-10MITSUBISHI CHEM CORP

Patent Information

Application Number
JP2023052381
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2023-03-28
Publication Date
2024-10-10

AI Technical Summary

Technical Problem

Existing ethylene-vinyl alcohol (EVOH) resins face challenges in achieving high gas barrier properties under high humidity conditions, biodegradability, and thermal stability due to issues such as cloud point formation and difficulty in melt molding, which affect their performance and applicability in gas barrier materials.

Method used

A modified ethylene-vinyl alcohol resin composition with specific ethylene structural unit content, saponification degree, and degree of polymerization, incorporating a primary hydroxyl structural unit in the side chain and a conjugated polyene, is developed to address these issues, ensuring the resin composition satisfies certain formula relationships that enhance gas barrier properties and biodegradability.

Benefits of technology

The modified resin composition exhibits high gas barrier properties under high humidity, maintains thermal stability, and prevents appearance defects during application, making it suitable for use in gas barrier materials.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2024140980000008
    Figure 2024140980000008
  • Figure 2024140980000001
    Figure 2024140980000001
  • Figure 2024140980000002
    Figure 2024140980000002
Patent Text Reader

Abstract

To provide a modified ethylene-vinyl alcohol-based resin composition that exhibits good biodegradability and thermal stability, prevents poor appearance due to application of an aqueous solution to a substrate, even though the aqueous solution has a cloud point, or due to melt molding, and that can exhibit a high gas barrier property even under high humidity.SOLUTION: A resin composition comprises: a modified ethylene-vinyl alcohol-based resin having a primary hydroxyl structural unit in a side chain; and a conjugated polyene in an amount of 0.1 ppm to 500 ppm. The modified ethylene-vinyl alcohol-based resin has an ethylene structural unit content of 2.5 to 16.5 mol% and a saponification degree of more than 98.5 mol%. The modified ethylene-vinyl alcohol-based resin has a degree of polymerization (DPv) of 450 to 1350, as determined from the viscosity average molecular weight of a tetrahydrofuran solution of a modified ethylene-vinyl ester-based copolymer after reacetylation of the modified ethylene-vinyl alcohol-based resin. A relationship between the cloud point (Tcp) of a 4 mass% aqueous solution of the modified ethylene-vinyl alcohol-based resin and the degree of polymerization (DPv) satisfies the following formula (i). [Formula] -14×Tcp+1200≤DPv (i)SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a modified ethylene-vinyl alcohol resin composition, a gas barrier material having a layer made of the same, and a method for producing the same. [Background technology]

[0002] Attempts are being made to use gas barrier materials with a layer made of polyvinyl alcohol resin as food packaging materials that maintain transparency while also retaining aroma retention, solvent resistance, and oil resistance. It is believed that the gas barrier properties are expressed because the molecular mobility of the polymer chain is reduced due to hydrogen bonds between hydroxyl groups in the polyvinyl alcohol molecule.

[0003] When the polyvinyl alcohol-based resin is a homopolymer of polyvinyl alcohol, it has poor gas barrier properties, particularly under high humidity conditions. Therefore, attempts have been made to improve this by using an ethylene-vinyl alcohol-based resin (hereinafter, ethylene-vinyl alcohol-based resin may be referred to as an "EVOH-based resin").

[0004] Meanwhile, in recent years, there has been a demand for reducing the environmental burden, and from the perspective of further reducing the environmental burden (e.g., marine issues), there has been a demand for gas barrier resins with excellent biodegradability. However, EVOH-based resins with an ethylene structural unit content of 20 to 60 mol% have low biodegradability, and in order to achieve both biodegradability and gas barrier properties with EVOH-based resins, studies are underway on EVOH-based resins with an ethylene structural unit content of less than 20 mol%.

[0005] Methods for obtaining a gas barrier material using an EVOH-based resin include a melt molding method and a method in which an aqueous solution is applied to a substrate. When attempting to obtain a gas barrier material by melt molding of EVOH-based resins, if the degree of polymerization is too low, the molecular chains are not entangled enough to make the material perform well, but if the degree of polymerization is too high, the melt viscosity is too high, making it difficult to obtain a gas barrier material by melt molding.

[0006] On the other hand, when attempting to obtain a gas barrier material by applying an aqueous solution of an EVOH-based resin to a substrate, the degree of polymerization can be increased to increase the entanglement of polymer chains and thereby increase the strength of the material. However, in order to improve the gas barrier properties under high humidity conditions, it is necessary to increase the content of ethylene structural units, and such an aqueous solution may exhibit a cloud point.

[0007] The cloud point of an aqueous solution refers to the temperature at which, even if the aqueous solution is transparent or translucent at low temperatures, when it is heated, its solubility drops suddenly and it becomes opaque due to phase separation from water. This phenomenon is often seen in aqueous solutions of polyvinyl alcohol with low saponification degrees and nonionic surfactants with polyether chains such as polyoxyethylene, and is also seen in aqueous solutions of EVOH-based resins with high ethylene modification rates. The reason for the cloud point is that when these aqueous solutions are heated, it is energetically more favorable for the hydroxyl groups of polyvinyl alcohol to form hydrogen bonds within the polymer molecule than to form hydrogen bonds by interacting with the solvent water, so that the solubility in water drops suddenly and the solution becomes opaque.

[0008] As a method for obtaining a barrier material with improved gas barrier properties at high humidity by applying an aqueous solution of an EVOH-based resin to a substrate, for example, a barrier material using an aqueous solution of an EVOH-based resin having an ethylene modification rate of 2 to 19 mol%, a viscosity average degree of polymerization of 200 to 2000, and a saponification degree of 80 to 99.99 mol% has been proposed (Patent Document 1).

[0009] Patent Document 1 shows an example of obtaining an injection molded product or a blow molded product by melt molding, but does not show a method of obtaining a gas barrier material by melt molding, and the only method of obtaining a gas barrier material is to apply an aqueous solution to a substrate. In addition, in the examples of obtaining a gas barrier material, the melting points of the resins with a saponification degree of 98.0 mol% or more are all 196°C or more, so even if a gas barrier material is to be obtained by melt molding, melt molding is difficult, and improvements have been required. On the other hand, the only resins with a melting point of 190°C or less have a saponification degree of 95.5 mol%, and improvements in gas barrier properties under high humidity are required.

[0010] Regarding the cloud point of EVOH-based resins, Patent Document 2 discloses a ceramic molding binder using an EVOH-based resin having a cloud point of 90° C. or lower in a 0.1 to 10% aqueous solution concentration range, and reports that the cloud point of the aqueous solution decreases as the degree of saponification decreases, the degree of polymerization increases, and the ethylene content increases.

[0011] However, Patent Document 2 only reports a ceramic molding binder using an EVOH-based resin, and does not mention other applications. When applying an aqueous solution of EVOH resin to a substrate to obtain a gas barrier material, it goes without saying that a uniform coating is necessary to increase the barrier properties, but applying an aqueous solution with a cloud point has the drawback of causing phase separation during application and drying, or preventing the formation of a uniform coating surface, making it difficult to achieve high barrier properties. Therefore, up until now, EVOH resins with cloud points have been considered unsuitable for gas barrier materials.

[0012] Furthermore, even when an attempt was made to obtain a gas barrier material by applying an aqueous solution at a temperature below the cloud point, in the examples of Patent Document 2, EVOH-based resins with saponification degrees of 98.8 mol % and 98.5 mol % had low viscosity average polymerization degrees of 250 and 450, respectively, as determined by reacetylation in acetic anhydride and pyridine, and were therefore unsuitable for use as a gas barrier material.

[0013] Patent Document 3 discloses that a modified EVOH-based resin having an ethylene structural unit content of 1 mol % or more and less than 10 mol %, having 3 to 15 mol % of 1,3-propanediol structures in the main chain, and having a saponification degree of 99.0 to 99.3 mol % provides a gas barrier material having oxygen barrier properties even under high humidity conditions by applying an aqueous solution of the resin to a substrate, and also exhibits biodegradability, and pellets can be obtained by melt molding.

[0014] Patent Document 3 describes an example of a method for obtaining a gas barrier material, in which a 10% by mass aqueous solution of a modified EVOH-based resin is applied to a substrate and dried at 60°C with a hot air dryer, and describes that the sodium acetate content was determined by heating and dissolving the resin at 90°C for 2 hours or more. Therefore, it is considered that the cloud point of the example resin is at least above 90°C, but the relationship with the degree of polymerization is not determined.

[0015] Patent Document 4 proposes a modified EVOH-based resin that has 2.5 to 16.5 mol % of ethylene structural units and further has a specific amount of primary hydroxyl groups in the side chains as an EVOH-based resin that combines biodegradability and gas barrier properties.

[0016] When attempting to obtain a gas barrier material by coating the solution of the modified EVOH-based resin in Patent Document 4, only an aqueous solution with low light transmittance is obtained, or a mixed solvent of water and alcohol must be used. Thus, there has been a demand for a modified EVOH-based resin that can improve the properties of the aqueous solution, or an EVOH-based resin that can be stably melt-molded. [Prior art documents] [Patent documents]

[0017] [Patent Document 1] JP 2000-309607 A [Patent Document 2] JP 2000-272970 A [Patent Document 3] International Publication No. 2022 / 97718 [Patent Document 4] International Publication No. 2021 / 235507 Summary of the Invention [Problem to be solved by the invention]

[0018] Therefore, the present invention has been made in consideration of the above circumstances, and an object of the present invention is to provide a modified ethylene-vinyl alcohol resin composition which exhibits good biodegradability and thermal stability, prevents poor appearance caused by application of the aqueous solution to a substrate or melt molding, even though the aqueous solution has a cloud point, and exhibits high gas barrier properties even under high humidity. [Means for solving the problem]

[0019] However, the present inventors have conducted extensive research in light of the above circumstances, and as a result have discovered a resin composition comprising a modified ethylene-vinyl alcohol resin having a primary hydroxyl group structural unit in a side chain and 0.1 ppm or more and 500 ppm or less of a conjugated polyene, the modified ethylene-vinyl alcohol resin having an ethylene structural unit content of 2.5 to 16.5 mol % and a saponification degree of more than 98.5 mol %, and the modified ethylene-vinyl alcohol resin has a viscosity average molecular weight calculated from a tetrahydrofuran solution of a modified ethylene-vinyl ester copolymer after reacetylation. The present inventors have found that by using a modified ethylene-vinyl alcohol-based resin composition having a degree of polymerization (DPv) of 450 or more and 1,350 or less, and in which the relationship between the cloud point (Tcp) of a 4 mass% aqueous solution of the modified ethylene-vinyl alcohol-based resin and the degree of polymerization (DPv) satisfies the following formula (i), a modified ethylene-vinyl alcohol-based resin composition can be obtained that exhibits good biodegradability and thermal stability, prevents poor appearance due to application of the aqueous solution to a substrate or melt molding, despite the cloud point of the aqueous solution, and exhibits high gas barrier properties even under high humidity, thereby completing the present invention. [Formula] -14×Tcp+1200≦DPv…(i)

[0020] That is, the present invention has the following aspects. [1] A resin composition comprising a modified ethylene-vinyl alcohol resin having a primary hydroxyl group structural unit in a side chain and a conjugated polyene in an amount of 0.1 ppm or more and 500 ppm or less, The modified ethylene-vinyl alcohol resin has an ethylene structural unit content of 2.5 to 16.5 mol% and a saponification degree of more than 98.5 mol%, the degree of polymerization (DPv) calculated from the viscosity average molecular weight of a tetrahydrofuran solution of the modified ethylene-vinyl ester copolymer after reacetylation of the modified ethylene-vinyl alcohol resin is 450 or more and 1350 or less; A modified ethylene-vinyl alcohol resin composition, wherein the relationship between the cloud point (Tcp) of a 4 mass % aqueous solution of the resin composition and the degree of polymerization (DPv) satisfies the following formula (i): [Formula] -14×Tcp+1200≦DPv…(i) [2] The modified ethylene-vinyl alcohol resin composition according to [1], wherein the modified ethylene-vinyl alcohol resin satisfies the following formula (ii) between the melting point (Tm) and the cloud point (Tcp): [Formula] 0.4×Tcp+155≦Tm≦0.2×Tcp+179…(ii) [3] The modified ethylene-vinyl alcohol resin composition according to [1] or [2], wherein the cloud point (Tcp) is 15° C. or higher. [4] The modified ethylene-vinyl alcohol resin composition according to [2] or [3], wherein the melting point (Tm) is 190° C. or lower. [5] A gas barrier material having a layer made of the modified ethylene-vinyl alcohol resin composition according to any one of [1] to [4]. [6] A method for producing a gas barrier material, comprising applying an aqueous solution of the modified ethylene-vinyl alcohol resin composition according to any one of [1] to [4] to a substrate at a temperature at which the substrate does not exhibit a cloud point. Effect of the Invention

[0021] The modified ethylene-vinyl alcohol resin composition of the present invention exhibits good biodegradability and thermal stability, and is also able to prevent poor appearance due to application of the aqueous solution to a substrate or melt molding, even though the aqueous solution has a cloud point, and exhibits high gas barrier properties even under high humidity conditions. [Brief description of the drawings]

[0022] [Figure 1]FIG. 1 is a graph showing the relationship between the temperature and light transmittance used to determine the cloud point in Examples 2, 5, and 6. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] The present invention will be described below based on examples of the mode for carrying out the present invention. However, the present invention is not limited to the embodiment described below.

[0024] In the present invention, when expressed as "X to Y" (X and Y are any numbers), unless otherwise specified, it includes the meaning of "X or more and Y or less", as well as "preferably larger than X" or "preferably smaller than Y". Furthermore, when it is expressed as "X or more" (X is any number) or "Y or less" (Y is any number), it also includes the meaning that "it is preferably greater than X" or "it is preferably less than Y". Furthermore, "x and / or y (x and y are optional configurations)" means at least one of x and y, and means the following three cases: x only, y only, and x and y.

[0025] In the present invention, the term "film" includes the meanings of "tape" and "sheet". In the present invention, the term "main component" refers to the component that is most abundant in the target substance, and is usually preferably 50 mass% or more of the target substance, more preferably 60 mass% or more, even more preferably 70 mass% or more, particularly preferably 80 mass% or more, especially preferably 90 mass% or more, and even more preferably 99 mass% or more, and may be 100 mass%.

[0026] A modified ethylene-vinyl alcohol resin composition according to one embodiment of the present invention (hereinafter, sometimes referred to as "the modified EVOH resin composition") is a resin composition containing a modified ethylene-vinyl alcohol resin having a primary hydroxyl group structural unit in a side chain and a conjugated polyene in an amount of 0.1 ppm or more and 500 ppm or less, The modified ethylene-vinyl alcohol resin has an ethylene structural unit content of 2.5 to 16.5 mol% and a saponification degree of more than 98.5 mol%, the degree of polymerization (viscosity average degree of polymerization: DPv) calculated from the viscosity average molecular weight of a tetrahydrofuran solution of the modified ethylene-vinyl ester copolymer after reacetylation of the modified ethylene-vinyl alcohol resin is 450 or more and 1350 or less; The relationship between the cloud point (Tcp) of a 4 mass % aqueous solution of the modified ethylene-vinyl alcohol resin and its DPv satisfies formula (i). [Formula] -14×Tcp+1200≦DPv…(i)

[0027] This modified EVOH-based resin composition contains a modified ethylene-vinyl alcohol-based resin (hereinafter, sometimes referred to as "EVOH-based resin") as a main component, and each component contained in this modified EVOH-based resin composition will be described below.

[0028] [Modified EVOH resin] An EVOH-based resin is a thermoplastic resin obtained by saponifying an ethylene-vinyl ester-based copolymer, which is a copolymer of ethylene and a vinyl ester-based monomer, and is mainly composed of ethylene structural units and vinyl alcohol structural units, and usually contains a small amount of vinyl ester structural units that remain unsaponified.

[0029] The modified EVOH-based resin contained in the present modified EVOH-based resin composition is an EVOH-based resin having a primary hydroxyl group structural unit in the side chain, specifically, an EVOH-based resin having a structural unit of the following general formula (1).

[0030] [ka] (In the formula, R 1 ~R 3 each independently represents a hydrogen atom or an organic group, and X represents a single bond or a bonding chain.

[0031] R 1 ~R3 is not particularly limited as long as it is a hydrogen atom or an organic group. Examples of the organic group include hydrocarbon groups such as alkyl groups, alkenyl groups, alkynyl groups, phenyl groups, and naphthyl groups (these hydrocarbon groups may have hydroxyl groups, fluorine, chlorine, bromine, and the like as substituents).

[0032] The bonding chain (X) bonding the polymer main chain and the primary hydroxyl group structure is not particularly limited, and examples thereof include hydrocarbons such as alkylene, alkenylene, alkynylene, phenylene, and naphthylene (these hydrocarbons may have a hydroxyl group, fluorine, chlorine, bromine, etc. as a substituent), hydrocarbons bonded to the polymer main chain by an ether bond such as oxyalkylene, oxyalkenylene, oxyalkynylene, oxyphenylene, and oxynaphthylene (these hydrocarbons may have a hydroxyl group, fluorine, chlorine, bromine, etc. as a substituent), -CO-, -CO(CH2)mCO-, -CO(CH2)mCOR 4 -, -NR 5 -,-CONR 5 - etc. (R 4 ,R 5 are independently any substituent, preferably a hydrogen atom or an alkyl group, and m is a natural number.

[0033] The modified EVOH resin can be obtained, for example, by copolymerizing a monomer having a primary hydroxyl group on the side chain and / or a monomer in which the primary hydroxyl group on the side chain is protected with an ester or the like with ethylene and a vinyl ester monomer, followed by saponification.

[0034] The method for producing the modified EVOH resin will be described below. First, ethylene, a vinyl ester monomer, and a monomer having a primary hydroxyl group on the side chain and / or a monomer in which the primary hydroxyl group on the side chain is protected with an ester or the like are copolymerized.

[0035] Examples of the vinyl ester monomer include vinyl formate, vinyl acetate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl benzoate, vinyl versatate, and vinyl trifluoroacetate. These may be used alone or in combination of two or more. Among them, vinyl acetate is preferred from the economical viewpoint.

[0036] Examples of the monomer having a primary hydroxyl group in the side chain include monohydroxyalkyl group-containing monomers such as allyl alcohol, 3-buten-1-ol, 4-penten-1-ol, 5-hexen-1-ol, 6-hepten-1-ol, and methallyl alcohol; and dihydroxyalkyl group-containing monomers such as 2-methylene-1,3-propanediol, 3,4-diol-1-butene, 4,5-diol-1-pentene, 4,5-diol-3-methyl-1-pentene, 5,6-diol-1-hexene, and glycerin monoallyl ether. These may be used alone or in combination of two or more.

[0037] In addition, examples of the monomer in which the primary hydroxyl group of the side chain is protected with an ester or the like (hereinafter, sometimes referred to as "monomer in which the hydroxyl group is protected with an ester or the like") include, for example, acetate esters of the monomers having the above-mentioned primary hydroxyl group of the side chain. Specific examples include monoacetoxyalkyl group-containing monomers such as allyl acetate, 3-butenyl acetate, 4-pentenyl acetate, 5-hexenyl acetate, 6-heptenyl acetate, and methallyl acetate; diacetoxyalkyl group-containing monomers such as 2-methylene-1,3-propanediol diacetate, 3,4-diacetoxy-1-butene, 4,5-diacetoxy-1-pentene, 4,5-diacetoxy-3-methyl-1-pentene, 5,6-diacetoxy-1-hexene, and 3-allyloxy-1,2-propanediol diacetate. These may be used alone or in combination of two or more kinds.

[0038] A monomer having a primary hydroxyl group in a side chain and a monomer in which the hydroxyl group is protected with an ester or the like can be used in combination and copolymerized with ethylene and vinyl ester monomers. Among them, from the viewpoint of productivity, a monomer in which the hydroxyl group is protected with an ester or the like is preferred, a diacetoxyalkyl group-containing monomer is more preferred, 3,4-diacetoxy-1-butene and 2-methylene-1,3-propanediol diacetate are more preferred, and 3,4-diacetoxy-1-butene is particularly preferred.

[0039] Furthermore, a copolymerizable ethylenically unsaturated monomer may be copolymerized as a copolymerization component within a range that does not impair the effects of the present invention (for example, 10% by mass or less of the copolymerization components). Examples of such ethylenically unsaturated monomers include olefins such as propylene, 1-butene, and isobutene; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, and (anhydrous) itaconic acid, or their salts; and unsaturated acids having 1 to 10 carbon atoms. Examples of the vinyl ethers include mono- or di-alkyl esters of C1 to C18; acrylamide, N-alkyl methacrylamide having 1 to 18 carbon atoms, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salt; acrylamides such as acrylamidopropyldimethylamine or its acid salts or its quaternary salts; methacrylamide, N-alkyl methacrylamide having 1 to 18 carbon atoms, N,N-dimethylmethacrylamide, 2-methacrylamidopropanesulfonic acid or its salts; N-vinyl amides such as N-vinylpyrrolidone, N-vinylformamide, and N-vinylacetamide; vinyl cyanides such as acrylonitrile and methacrylonitrile; vinyl ethers such as alkyl vinyl ethers, hydroxyalkyl vinyl ethers, and alkoxyalkyl vinyl ethers having 1 to 18 carbon atoms; vinyl halides such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; and vinyl silanes. These may be used alone or in combination of two or more.

[0040] In these copolymerization reactions, known methods can be used, such as bulk polymerization, solution polymerization, suspension polymerization, dispersion polymerization, emulsion polymerization, etc. Among them, solution polymerization is preferably used because it is easy to control the copolymerization.

[0041] When such copolymerization is carried out by solution polymerization, examples of the solvent used include lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, 1-propanol, 2-propanol, butanol, and ketones, such as acetone and 2-butanone. These may be used alone or in combination of two or more. Among them, methanol is preferably used because of the ease of controlling the polymerization reaction. In addition, 2-propanol is preferably used when synthesizing a copolymer with a low degree of polymerization.

[0042] The amount of the solvent used can be appropriately selected in consideration of the polymerization degree of the desired modified EVOH resin and the chain transfer constant of the solvent. When the solvent is methanol or 2-propanol, S (solvent) / M (monomer) is preferably 0.01 to 10 (mass ratio), more preferably 0.05 to 7 (mass ratio).

[0043] As a method for feeding the copolymerization components in solution polymerization, any method can be adopted, such as initial lump-sum feeding, divided feeding, or continuous feeding such as the Hanna method taking into consideration the reactivity ratio of the monomers.

[0044] A polymerization initiator is used in the copolymerization. Examples of such polymerization initiators include azo initiators such as 2,2'-azobisisobutyronitrile, 2,2'-azobis(2,4-dimethylvaleronitrile), and 2,2'-azobis(4-methoxy-2,4-dimethylvaleronitrile), and peroxide initiators such as acetyl peroxide, benzoyl peroxide, lauryl peroxide, t-butyl peroxy neodecanoate, 1,1,3,3-tetramethylbutyl peroxy neodecanoate, diisopropyl peroxy dicarbonate, and di-2-ethylhexyl peroxy dicarbonate. These may be used alone or in combination of two or more.

[0045] The amount of the polymerization initiator to be used varies depending on the polymerization degree of the target EVOH-based resin and the type of polymerization initiator, and cannot be generally determined, but is selected according to the polymerization rate. For example, when 2,2'-azobisisobutyronitrile or t-butylperoxyneodecanoate is used, the amount is usually 10 to 2000 ppm, preferably 50 to 1000 ppm, based on the vinyl ester-based monomer.

[0046] The polymerization temperature for the copolymerization is preferably selected from the range of 40° C. to the boiling point depending on the solvent used and the ethylene pressure.

[0047] In addition, the copolymerization may be carried out in the presence of a chain transfer agent within a range that does not impair the effects of the present invention. Examples of the chain transfer agent include aldehydes such as acetaldehyde, propionaldehyde, and crotonaldehyde; and mercaptans such as 2-hydroxyethanethiol. These may be used alone or in combination of two or more. The amount of the chain transfer agent added during copolymerization is determined according to the chain transfer constant of the chain transfer agent and the polymerization degree of the desired modified EVOH resin, but generally, 0.1 to 10 parts by mass is preferred for 100 parts by mass of the vinyl ester monomer.

[0048] The degree of polymerization of the ethylene-vinyl ester copolymer can be controlled by the polymerization method in the polymerization process, the monomer concentration in solution polymerization (the above-mentioned S (solvent) / M (monomer) ratio), the ratio of the vinyl ester monomer to other monomers, particularly the ratio of the vinyl ester monomer to a monomer having a primary hydroxyl group in the side chain or a monomer whose hydroxyl group is protected with an ester or the like, the amount of polymerization initiator used, the amount of chain transfer agent used, and the polymerization rate. In general, the higher the monomer concentration, the smaller the amount of other monomers in the ratio of the vinyl ester monomer to other monomers, the smaller the amount of polymerization initiator used, the smaller the amount of chain transfer agent used, and the smaller the polymerization rate, the higher the polymerization degree tends to be.

[0049] After copolymerization of the copolymerization components, it is also preferable to add a conjugated polyene such as sorbic acid as a polymerization inhibitor in order to reliably terminate the reaction. This conjugated polyene dissolves in the cleaning fluid when the modified EVOH resin described below is washed, so the content decreases as the washing proceeds. However, the amount of conjugated polyene present in the modified EVOH resin can be controlled by controlling the washing method. The preferred structure of the conjugated polyene, the amount to be added, and the mechanism of action will be described later.

[0050] The ethylene-vinyl ester copolymer thus obtained can be saponified to obtain an EVOH resin. In addition, it is preferable to reduce the content of unreacted vinyl ester monomer remaining in the solution by heating or the like before saponification in terms of suppressing coloration of the resulting modified EVOH resin composition. The saponification method can be a known method, and for example, is performed by adding a saponification catalyst to the ethylene-vinyl ester copolymer obtained above in a state of being dissolved in alcohol or water-containing alcohol.

[0051] Examples of the alcohol include lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, and propanol. These may be used alone or in combination of two or more. Among these, methanol is preferred. The concentration of the ethylene-vinyl ester copolymer in the alcohol is appropriately selected depending on the viscosity, and is usually 5 to 60% by mass.

[0052] Examples of the saponification catalyst include alkali catalysts such as hydroxides and alcoholates of alkali metals, such as sodium hydroxide, potassium hydroxide, sodium methylate, sodium ethylate, potassium methylate, and potassium ethylate; and acid catalysts such as sulfuric acid, hydrochloric acid, nitric acid, and metasulfonic acid. Preferred are hydroxides and alcoholates of sodium, such as sodium hydroxide and sodium methylate.

[0053] The temperature for saponification is not limited, but is preferably in the range of 20 to 140°C. As the saponification proceeds, particulate matter is generated, which indicates that the reaction has proceeded. If a gel-like product precipitates at this time, the product may be pulverized. The particulate matter thus generated is washed and dried to obtain a modified EVOH-based resin. When a monomer in which a hydroxyl group is protected by an ester or the like is copolymerized, the ester or the like of the protected monomer is simultaneously deprotected by the saponification reaction and converted into a primary hydroxyl group in the side chain.

[0054] For example, when 3,4-diacetoxy-1-butene is used as a copolymerization component, the modified EVOH-based resin obtained by deprotection through saponification has a primary hydroxyl group represented by the following general formula (2) in the side chain.

[0055] [ka]

[0056] Furthermore, when 2-methylene-1,3-propanediol diacetate is used as a copolymerization component, the modified EVOH-based resin obtained by deprotection through saponification has a primary hydroxyl group represented by the following general formula (3) in the side chain.

[0057] [ka]

[0058] In order to increase the degree of saponification of the modified EVOH-based resin, it is also preferable to carry out a secondary saponification in which by-products (vinyl acetate as the vinyl ester-based monomer, or methyl acetate when methanol is used as the solvent during saponification) are removed from the particulate matter once produced by washing or the like, and then the product is dispersed again in alcohol or the like, and an alkali catalyst or the like is added to cause further reaction.

[0059] In the modified EVOH-based resin, the protecting groups may not be completely deprotected in the saponification reaction, leaving a small amount of ester groups remaining, and the protecting groups on the side chains may also not be completely deprotected, leaving a small amount of ester groups remaining.

[0060] After the saponification reaction is completed, the alkali catalyst or acid catalyst is neutralized as necessary, and the resulting product is subjected to solid-liquid separation, washed, and dried to obtain an EVOH-based resin.

[0061] <Physical properties of modified EVOH resin> The content of ethylene structural units in the modified EVOH resin is from 2.5 to 16.5 mol %, preferably from 5 to 16 mol %, and more preferably from 7 to 15 mol %. If the content of ethylene structural units is too low, there will be a large number of hydroxyl groups in the resin, and under high humidity conditions there will be more room for moisture to interact with the hydroxyl groups, making it difficult to exhibit gas barrier properties. In addition, when attempting to perform melt molding, the melting point of the modified EVOH-based resin will be high and it will tend to be easily decomposed. Moreover, if the content of ethylene structural units is too high, the gas barrier properties at low humidity tend to decrease, and biodegradability tends to decrease, and there is also a drawback that it becomes difficult to design a resin that has a preferable cloud point. The content of the ethylene structural unit in the modified EVOH resin can be controlled by adjusting the ethylene pressure during copolymerization.

[0062] The content of primary hydroxyl group structural units in the side chains of the modified EVOH-based resin (hereinafter sometimes referred to as "side chain primary hydroxyl group structural units") is usually 2.5 mol% or more, preferably 2.5 to 10 mol%, particularly preferably 3 to 6 mol%, and even more preferably 3 to 4.5 mol%. The content of the side chain primary hydroxyl group structural unit can be controlled by the amount of a monomer having a primary hydroxyl group in the side chain or a monomer in which the hydroxyl group is protected with an ester or the like, which is used as a copolymerization monomer.

[0063] The side chain primary hydroxyl structural unit has an effect of lowering the melting point of the modified EVOH resin as the content of the structural unit increases. Also, in the range where the water solubility of the modified EVOH resin is poor due to the ethylene structural unit and the hydroxyl groups of the vinyl alcohol structural units tend to interact with each other in an aqueous solution of the modified EVOH resin, the side chain primary hydroxyl structural unit is a particularly effective structural unit for ensuring interaction with the solvent water even when the molecular motion in the aqueous solution is intense at high temperatures, and therefore the cloud point can be controlled.

[0064] If the content of side chain primary hydroxyl structural units is too low, the effect of lowering the melting point of the modified EVOH-based resin is small, and the resin tends to be easily decomposed during melt molding. In addition, the cloud point becomes too low when an aqueous solution is prepared, making it necessary to lower the coating temperature for the substrate, which is an unfavorable tendency. Furthermore, if the content of side chain primary hydroxyl structural units is too high, the affinity with water will be high, making it difficult to ensure gas barrier properties under high humidity conditions, and it will be necessary to use a large amount of monomers having primary hydroxyl groups in the side chains and / or monomers in which the primary hydroxyl groups in the side chains are protected with esters, etc., during production, which will tend to increase production costs.

[0065] The saponification degree of the modified EVOH-based resin is more than 98.5 mol%, preferably 98.7 mol% or more and less than 99.9 mol%, preferably 99.0 mol% or more and less than 99.8 mol%. If the saponification degree is too low, the barrier function, especially under high humidity, tends to be reduced, and the aroma retention, solvent resistance, and oil resistance tend to be reduced. If the saponification degree is too high, strict conditions must be used during production, and the price tends to be high.

[0066] The content of the modified EVOH resin in the present modified EVOH resin composition is usually 80% by mass or more, preferably 90% by mass or more, and more preferably 95% by mass or more.

[0067] The degree of polymerization of the modified EVOH resin, as determined from the viscosity average molecular weight of a tetrahydrofuran solution of a modified ethylene-vinyl ester copolymer after reacetylation of the resin (viscosity average degree of polymerization: DPv), is from 450 to 1350, preferably from 500 to 1250, and more preferably from 600 to 1200. The degree of polymerization (DPv) is determined by the method described in the Examples.

[0068] If the DPv is too low, the entanglement between the resin molecules decreases, and the gas barrier material tends to become brittle, which is undesirable. Furthermore, if the DPv is too high, the degree of polymerization will be high, so that when the aqueous solution is applied to a substrate, the viscosity will be too high and streaks will tend to form, and during melt molding, the viscosity will be too high and a load will tend to be placed on the molding machine, both of which are undesirable.

[0069] [Conjugated polyenes] The modified EVOH-based resin composition contains a conjugated polyene together with a modified EVOH-based resin. The conjugated polyene may be a conjugated diene having a structure in which two carbon-carbon double bonds and one carbon-carbon single bond are alternately linked, a conjugated triene having a structure in which three carbon-carbon double bonds and two carbon-carbon single bonds are alternately linked, or a conjugated polyene having a structure in which a greater number of carbon-carbon double bonds and carbon-carbon single bonds are alternately linked.

[0070] However, when the number of conjugated carbon-carbon double bonds is 8 or more, the molded product tends to be colored by the color of the conjugated polyene itself, so the number of conjugated carbon-carbon double bonds is preferably 7 or less. In addition, the above-mentioned conjugated double bonds consisting of two or more carbon-carbon double bonds may be present in a single molecule without being conjugated with each other. For example, compounds such as tung oil that have three conjugated trienes in the same molecule are also included in the conjugated polyenes.

[0071] Specific examples of conjugated polyenes include isoprene, 2,3-dimethyl-1,3-butadiene, 2,3-diethyl-1,3-butadiene, 2-t-butyl-1,3-butadiene, 1,3-pentadiene, 2,3-dimethyl-1,3-pentadiene, 2,4-dimethyl-1,3-pentadiene, 3,4-dimethyl-1,3-pentadiene, 3-ethyl-1,3-pentadiene, 2-methyl-1,3-pentadiene, 3-methyl-1,3-pentadiene, 4-methyl-1,3-pentadiene, 1,3-hexadiene, 2,4-hexadiene, 2,5-dimethyl-2,4-hexadiene, 1,3-octadiene, 1,3-cyclopentadiene, 1,3-cyclohexadiene, 1-phenyl-1,3-butadiene, 1,4-diphenyl-1,3-butadiene, 1-methoxy-1,3-butadiene, 2-methoxy-1,3-butadiene, 1-ethoxy-1,3-butadiene, 2-ethoxy-1,3-butadiene conjugated dienes having a conjugated structure with two carbon-carbon double bonds, such as oxy-1,3-butadiene, 2-nitro-1,3-butadiene, chloroprene, 1-chloro-1,3-butadiene, 1-bromo-1,3-butadiene, 2-bromo-1,3-butadiene, fulvene, tropone, ocimene, phellandrene, myrcene, farnesene, cembrene, sorbic acid, sorbic acid esters, sorbic acid salts, and abietic acid; conjugated trienes having a conjugated structure with three carbon-carbon double bonds, such as 1,3,5-hexatriene, 2,4,6-octatriene-1-carboxylic acid, eleostearic acid, tung oil, and cholecalciferol; and conjugated polyenes having a conjugated structure with four or more carbon-carbon double bonds, such as cyclooctatetraene, 2,4,6,8-decatetraene-1-carboxylic acid, retinol, and retinoic acid. In addition, for those having multiple stereoisomers such as 1,3-pentadiene, myrcene, and farnesene, any of them may be used. Such conjugated polyenes may be used alone or in combination of two or more kinds.

[0072] Among these, the conjugated polyene is preferably at least one selected from the group consisting of sorbic acid, sorbic acid esters, and sorbic acid salts, and is particularly preferably sorbic acid. These conjugated polyenes can be used as polymerization inhibitors added when terminating copolymerization reaction in the production of EVOH-based resins. When these conjugated polyenes are used as polymerization inhibitors, polymerization can be terminated reliably, and they tend to be easy to handle. In addition, when these conjugated polyenes are added later in a predetermined amount to the modified EVOH-based resin composition, they tend to be easy to handle.

[0073] The content of the conjugated polyene is 0.1 to 500 ppm, preferably 0.2 to 400 ppm, more preferably 0.2 to 20 ppm, even more preferably 0.2 to 10 ppm, and particularly preferably 0.2 to 5 ppm, relative to the modified EVOH-based resin composition. If the content of the conjugated polyene is too low, the thermal stability of the modified EVOH-based resin composition tends to deteriorate, and for example, when a gas barrier material is obtained by melt molding as described below, gels and lumps tend to be easily generated during long-term operation. Also, if the content of the conjugated polyene is too high, the gas barrier property and biodegradability tend to decrease.

[0074] Conjugated polyenes are also thought to contribute to the appropriate cloud point. Although the mechanism of action is not clear, it is thought that the conjugated double bonds in the conjugated polyenes interact with the ethylene units of the modified EVOH resins, moderately inhibiting the intermolecular interactions of the hydrophobic groups of the resins, which in turn makes it easier for intermolecular interactions to occur between the hydroxyl groups, and the molecular motion becomes more intense, making the resins more likely to aggregate. In addition, when sorbic acid is used as the conjugated polyene, there is an advantage that it can contribute to preventing putrefaction of the aqueous solution.

[0075] [Other ingredients] The present modified EVOH-based resin composition may contain other components in addition to the modified EVOH-based resin and conjugated polyene within a range that does not impair the effects of the present invention (for example, 10% by mass or less of the present modified EVOH-based resin composition). Examples of the other components include thermoplastic resins other than the modified EVOH-based resin, plasticizers, lubricants, stabilizers, surfactants, colorants, ultraviolet absorbers, antistatic agents, drying agents, crosslinking agents, metal salts, fillers, various fibers, etc. These may be used alone or in combination of two or more.

[0076] [Method of manufacturing the modified EVOH-based resin composition] The present modified EVOH-based resin composition is produced by mixing the modified EVOH-based resin, the conjugated polyene, and, if necessary, other components. Examples of the production method include known methods such as a dry blending method, a melt mixing method, a solution mixing method, and an impregnation method, and these can be combined in any desired manner. As described above, the conjugated polyene may be contained in the modified EVOH-based resin by using it as a polymerization inhibitor during the production of the modified EVOH-based resin.

[0077] <Modified EVOH Resin Composition> The modified EVOH-based resin composition thus obtained has a relationship between the cloud point (Tcp) of a 4 mass% aqueous solution and the degree of polymerization (viscosity average degree of polymerization: DPv) calculated from the viscosity average molecular weight of a tetrahydrofuran solution of a modified ethylene-vinyl ester-based copolymer after reacetylation of the modified EVOH-based resin, which satisfies the following formula (i): [Formula] -14×Tcp+1200≦DPv…(i)

[0078] Here, the cloud point (Tcp) refers to the temperature at which the transmittance of a 4% by mass aqueous solution at 430 nm becomes 50% or less when the solution is heated from a temperature at which the transmittance is 80% or more at less than 20°C to 90°C at a heating rate of 1°C / min, in accordance with the method for determining the transparency of an aqueous solution in JIS K-6726.

[0079] We consider the significance of using the viscosity-average degree of polymerization (DPv) as an index. The gas barrier properties are closely related to the mobility of molecular chains in the amorphous part, and it is believed that the mobility of molecular chains is largely due to the maintenance of hydrogen bonds and entanglement within the resin molecules. Molecular weight is a preferred index that reflects the entanglement of such resin molecules. Here, the index reflecting the molecular weight of a resin includes the number average molecular weight, viscosity average molecular weight, and weight average molecular weight determined by size exclusion chromatography, and the principles and methods of determining them are specified in JIS K7252-2. Among these, it is preferable to use the viscosity average molecular weight, which reflects the entanglement state of resin molecules, as an index rather than the number average molecular weight, which reflects the properties of each individual resin strand.

[0080] This section describes a method for determining the viscosity average molecular weight by size exclusion chromatography. Specifically, the modified ethylene-vinyl ester resin obtained by reacetylating the modified EVOH resin is subjected to size exclusion chromatography of the tetrahydrofuran solution, and the viscosity average molecular weight is determined according to JIS K7252-2. The K and α in the Mark-Houwink-Sakurada formula required to determine the viscosity average molecular weight are K=3.5×10, which is given as the value of polyvinyl acetate in tetrahydrofuran in Annex B of the same standard. 2 cm 3 / g, a value calculated using α=0.63 can be used. Reacetylation can be carried out by the method shown in the Examples.

[0081] Regarding the relationship between the molecular weight and the degree of polymerization, in the case of a copolymer in which a plurality of monomer units are copolymerized as in the present invention, the average molecular weight per repeating unit is calculated from the content of each monomer unit of the copolymer, and the molecular weight calculated by size exclusion chromatography is divided by the average molecular weight, so that the degree of polymerization can be calculated. An example of the conversion method is shown in the Examples.

[0082] In the above-mentioned reacetylation, it is believed that only the acetylation reaction of hydroxyl groups occurs, and the degree of polymerization of the modified EVOH-based resin is believed to remain unchanged before and after reacetylation. Therefore, it is believed that the viscosity average degree of polymerization of the modified ethylene-vinyl ester-based resin determined in this manner directly indicates the viscosity average degree of polymerization of the modified EVOH-based resin.

[0083] Here, when the viscosity average degree of polymerization is determined by a method of measuring the relative viscosity of an aqueous solution with water at 30.0° C. as specified in JIS K6726, there is a drawback in that the degree of polymerization cannot be determined for a modified EVOH-based resin having a cloud point of less than 30° C. However, by using the viscosity average molecular weight of an ethylene-vinyl ester copolymer as an indicator as in the present invention, there is an advantage that when a comparison with the viscosity average degree of polymerization measured for an aqueous solution of an EVOH-based resin as specified in JIS K6726 is required, the standard is consistent, making the comparison easy even when the aqueous solution has a cloud point of less than 30° C.

[0084] As mentioned above, it has been reported that the cloud point of an aqueous solution decreases with a lower saponification degree, a higher polymerization degree, and a higher ethylene content. It is also known that the cloud point of an aqueous polyvinyl alcohol solution depends on the aqueous solution concentration and the salt concentration of sodium acetate, etc.

[0085] In order to exhibit gas barrier properties, particularly gas barrier properties under high humidity conditions, it is preferable for the degree of saponification, degree of polymerization, and content of ethylene structural units to be within specific ranges. When the relationship between the cloud point and viscosity average degree of polymerization of a modified EVOH-based resin exhibiting favorable gas barrier properties was investigated, it was found that a range satisfying formula (i) is preferable.

[0086] The fact that the cloud point of an aqueous solution decreases as the degree of polymerization of a resin increases is related to the fact that the entanglement of resin molecules in an aqueous solution increases with increasing degree of polymerization, the resin molecules become less mobile with increasing degree of polymerization, and the contribution of the resin ends decreases with increasing degree of polymerization, and is thought to be related to the tendency that when molecular motion in an aqueous solution becomes more active with increasing temperature, hydrogen bonds are more likely to be formed within the resin molecules, and the water molecules of the solvent lose the opportunity to interact with the hydroxyl groups of the resin. The method of controlling the degree of polymerization has already been described.

[0087] In order to improve the gas barrier properties under high humidity conditions, it is considered preferable that the interaction between the hydroxyl groups of the modified EVOH-based resin is strong even in the presence of water molecules, which are present in large amounts depending on the humidity; in other words, it is considered preferable that the resin exhibits a cloud point in an appropriate range.

[0088] A resin whose aqueous solution shows a cloud point is a resin whose aqueous solution shows a point where the hydrogen bonds between intramolecular hydroxyl groups become stronger than the interaction with the water molecules in the aqueous solution. Therefore, by using a resin whose aqueous solution shows a cloud point as a gas barrier material, it is considered that under high humidity conditions, the hydrogen bonds between intramolecular hydroxyl groups become stronger, suppressing the influence of water caused by humidity, and high gas barrier properties can be exhibited. If the gas barrier layer does not have a uniform appearance, it is inferior in commercial value and is difficult to exhibit gas barrier properties, so it is necessary to form the gas barrier layer on the substrate under conditions that do not show a cloud point. The method for this purpose may be melt molding or applying an aqueous solution at a temperature below the cloud point and drying it. The present modified EVOH-based resin composition is a material that uses a resin that shows such a cloud point to provide a gas barrier material with high barrier properties even under high humidity conditions.

[0089] The cloud point (Tcp) of a 4 mass % aqueous solution of the modified EVOH-based resin (or resin composition) is preferably 15° C. or higher, more preferably 25° C. or higher, and even more preferably 30° C. or higher. When forming a gas barrier material by applying an aqueous solution to a substrate, in order to obtain a gas barrier material with good appearance, it is preferable that the aqueous solution is homogeneous at the time of application. Therefore, for example, in the range of Tcp<15°C, the temperature at the time of application must be less than 15°C, and such a restriction tends to be undesirable. In addition, water-insoluble modified EVOH-based resins are said to be favorable for exhibiting gas barrier properties due to the strong interaction between hydroxyl groups, but are not favorable because they have low biodegradability due to the difficulty in allowing bacteria to access them, which is necessary for them to exhibit biodegradability.

[0090] Furthermore, Tcp<70° C. is more preferable. By setting the range within this range, when used as a gas barrier material, even under conditions of high humidity and the presence of a large amount of water molecules in the external environment, hydrogen bonds between the modified EVOH-based resins are firmly maintained, and gas barrier properties are easily exhibited.

[0091] If the formula (i) is not satisfied, that is, if the range is "DPv<-14 × Tcp+1200," the degree of polymerization will be too low, resulting in too many resin ends, or the entanglement of the molecules will be too little, resulting in increased interaction with water due to humidity, which is undesirable for exhibiting gas barrier properties under high humidity conditions, or the balance of the introduction amounts of ethylene structural units and side chain primary hydroxyl structural units will be poor, resulting in poor interaction with water and a poor appearance of the gas barrier material, which are undesirable.

[0092] As described above, in order to obtain a modified EVOH resin having such a DPv, and in turn to obtain an ethylene-vinyl ester copolymer having such a DPv, the polymerization method in the polymerization process, the monomer concentration in solution polymerization, the amount of polymerization initiator used, and the amount of chain transfer agent used are controlled.

[0093] Furthermore, it is preferable that Tcp satisfies the following formula (ii) in relation to the melting point (Tm) of the modified EVOH resin. [Formula] 0.4×Tcp+155≦Tm≦0.2×Tcp+179…(ii)

[0094] As described above, the melting point of the EVOH-based resin can be controlled by the ethylene structural unit content and the saponification degree. Furthermore, the melting point can be controlled by the content of the side-chain primary hydroxyl group structural unit, and is also slightly affected by the degree of polymerization.

[0095] In the range of "Tm < 0.4×Tcp + 155", it is not preferable because there is a tendency that the gas barrier property under high humidity cannot be exhibited, or sufficient cooling is required to obtain a gas barrier material during melt molding, which takes time. On the other hand, in the range of "0.2×Tcp + 179 < Tm", it is not preferable because the melting point is too high during melt molding, and the modified EVOH-based resin tends to decompose.

[0096] Furthermore, as the upper limit of the melting point (Tm) of the modified EVOH-based resin, Tm ≤ 190°C is preferable. If the melting point is too high, when trying to obtain a gas barrier material by melt molding, the modified EVOH-based resin tends to decompose, which is not preferable. Also, if the introduction amount of the ethylene structural unit is too small, there is a tendency to be inferior in gas barrier property under high humidity, or when trying to produce a gas barrier material by coating an aqueous solution because the introduction amount of the side-chain primary hydroxyl group structural unit is too small, the cloud point becomes too low and the coating conditions tend to be restricted.

[0097] The biodegradability of this modified EVOH-based resin composition is preferably 30% or more, more preferably 35% or more, and particularly preferably 40% or more. The above biodegradability is determined by the method described in the examples with reference to the method described in JIS K6950.

[0098] By forming this modified EVOH-based resin composition into a film, it can be suitably used as a gas barrier material such as a stretched film or a food packaging material. In particular, since this modified EVOH-based resin composition exhibits a cloud point, even under high humidity, the hydrogen bonds between the modified EVOH-based resins are less likely to be affected by water molecules derived from humidity, and thus it has the characteristic of easily exhibiting a high barrier property.

[0099] [Method for producing a gas barrier material] The method for forming the present modified EVOH-based resin composition into a gas barrier material is not particularly limited, but preferred examples include (i) a method in which an aqueous solution of the present modified EVOH-based resin composition is applied to a base resin film and dried to form a layer of the modified EVOH-based resin composition to form a gas barrier material, and (ii) a method in which the present modified EVOH-based resin composition is melt-molded to form a gas barrier material.

[0100] In the above method (i), when preparing an aqueous solution of the modified EVOH-based resin composition, a solvent other than water that has affinity with water may be used in combination. Examples of such a solvent include lower alcohols having 1 to 5 carbon atoms, such as methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, and 2-butanol. In order to comply with recent regulations on the emission of volatile organic compounds (VOCs), it is also preferable to use only water. When only water is used, it is preferable to apply the water at a temperature below the cloud point (Tcp).

[0101] The solid content concentration in the aqueous solution of the modified EVOH-based resin composition is usually 0.5 to 30% by mass, and preferably 4 to 20% by mass. Examples of the method for applying the aqueous solution of the modified EVOH-based resin composition include known methods such as bar coating, roll coating, die coating, gravure coating, comma coating, screen printing, etc. Among these, the bar coater is preferred.

[0102] In addition, the temperature at which the aqueous solution of the modified EVOH-based resin composition is applied to the substrate is preferably a temperature at which the cloud point (Tcp) is not observed, in order to prevent defects in appearance.

[0103] After coating, water is removed at the coating temperature until fluidity is lost, and then the coating is dried, for example, by heat treatment at 60 to 105°C for 0.5 to 10 minutes to obtain a gas barrier material made of a modified EVOH-based resin.

[0104] Furthermore, examples of the melt molding method in the above method (ii) include extrusion molding, injection molding, inflation molding, press molding, blow molding, etc. In this case, the conditions for producing the gas barrier material can be selected regardless of the cloud point of the aqueous solution.

[0105] In this way, a gas barrier material having a layer made of the present modified EVOH-based resin composition is obtained. The gas barrier material may be a single-layer gas barrier material or a multi-layer gas barrier material, but a multi-layer structure is preferable. The multi-layer barrier material preferably has at least one layer made of the present modified EVOH-based resin composition. The multi-layer gas barrier material may be laminated with a layer made of the present modified EVOH-based resin composition, or may be laminated with another base resin.

[0106] Examples of the base resin include polyethylene resins such as linear low-density polyethylene, low-density polyethylene, very low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-propylene (block and random) copolymers, and ethylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; polypropylene resins such as polypropylene and propylene-α-olefin (α-olefin having 4 to 20 carbon atoms) copolymers; (unmodified) polyolefin resins such as polybutene, polypentene, and polycyclic olefin resins (polymers having a cyclic olefin structure in at least one of the main chain and side chain); and modified olefin resins such as unsaturated carboxylic acid-modified polyolefin resins obtained by graft-modifying these polyolefins with unsaturated carboxylic acid or its ester, polyolefin resins in the broad sense, ionomers, ethylene-vinyl acetate copolymers, and ethylene-acrylic acid copolymers. Examples of the base resin include ethylene-acrylic acid ester copolymers, polyester resins, polyamide resins (including copolymerized polyamides), polyvinyl chloride, polyvinylidene chloride, acrylic resins, polystyrene, vinyl ester resins, polyester elastomers, polyurethane elastomers, polystyrene elastomers, halogenated polyolefins such as chlorinated polyethylene and chlorinated polypropylene, and aromatic or aliphatic polyketones. These may be used alone or in combination of two or more. Furthermore, these base resins may be subjected to a surface treatment such as a corona treatment.

[0107] The thickness of the layer made of the present modified EVOH-based resin composition is usually 1 to 200 μm, preferably 1 to 100 μm, more preferably 1 to 50 μm. When the gas barrier material has a multi-layer structure, the thickness is the total thickness of all layers made of the present modified EVOH-based resin composition contained in the gas barrier material.

[0108] The oxygen permeability of the layer made of the modified EVOH-based resin composition was 3(cc·3μm / m 2 ·day·atm) or less, and more preferably 2.9 (cc·3μm / m 2·day·atm) or less, and more preferably 2.5 (cc·3μm / m 2 ·day·atm) or less, and particularly preferably 2 (cc·3μm / m 2 ·day·atm). The lower limit is usually 0 (cc·3μm / m 2 The oxygen permeability can be determined by an oxygen permeability measuring device. EXAMPLES

[0109] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples as long as it does not depart from the gist of the invention. In the examples, "parts" and "%" are based on mass.

[0110] The calculation of the content of each structural unit in the EVOH resin or EVOH resin composition, and the measurement methods of the melting point, cloud point, viscosity average degree of polymerization, conjugated polyene content, thermal stability test, and biodegradability are shown below.

[0111] [Calculation of content of each monomer unit and degree of saponification] (In the case of a copolymer having a 1,2-butanediol structure as a side chain primary hydroxyl group structural unit) ·1H-NMR measurement: Approximately 50 mg of EVOH-based resin was weighed into a vial, 1 mL of deuterated dimethyl sulfoxide was added, and the resin was dissolved by heating and stirring. After visually confirming that the resin had dissolved, about 10 drops of deuterated trifluoroacetic acid were added using a Pasteur pipette to prepare a measurement solution. This was measured at 50°C using a Bruker Ascend 400 nuclear magnetic resonance analyzer. The integral values ​​of δ0.9-1.9 ppm, δ1.9-2.0 ppm, and δ3.15-4.15 ppm were defined as a, b, and c, respectively. ·13C-NMR measurement: Approximately 200 mg of EVOH-based resin was weighed into a vial, 1 mL of deuterated dimethyl sulfoxide was added, and the resin was dissolved by heating and stirring at 80° C. After visually confirming dissolution, the resin was measured at 90° C. using a Bruker Ascend 400 nuclear magnetic resonance spectrometer. The integral value of δ 64.0 to 75.0 ppm divided by the integral value of δ 63.2 to 64.0 ppm was defined as d. If the ethylene structural unit, vinyl alcohol structural unit, 1,2-butanediol structural unit, and structural unit derived from unsaponified acetyl group of the EVOH-based resin are E, V, D, and A, respectively, then of the above four variables a to d, Since d=(V+A) / D+1, A=b / 3 V = {[c × (d-1)] - b} / (d + 2) D=(V+A) / (d-1) ·E=[a-(2×V)-(3×D)-(2×A)] / 4 This was then converted into a percentage to determine the content of each structural unit.

[0112] (In the case of a copolymer having a 1,3-propanediol structure as a side chain primary hydroxyl group structural unit) First, 1H-NMR was measured for the ethylene-vinyl ester-1,3-propanediol diacetate copolymer before saponification after copolymerization to determine the ratio of ethylene, vinyl ester, and 1,3-propanediol diacetate, and these ratios were used as the ratio of ethylene, vinyl alcohol, and 1,3-propanediol after the saponification reaction. The saponification degree was calculated assuming that the acetyl groups of the vinyl ester and 1,3-propanediol diacetate were saponified at the same molar ratio. That is, after the copolymerization was completed, a small amount of the methanol solution of the ethylene-vinyl ester-1,3-propanediol diacetate copolymer was sampled, and the ethylene-vinyl ester-1,3-propanediol diacetate copolymer was precipitated in ion-exchanged water. The precipitate was dried at 60°C under reduced pressure to obtain a dried ethylene-vinyl ester-1,3-propanediol diacetate copolymer. Approximately 50 mg of this dried product was weighed into a vial, 1 mL of deuterated dimethyl sulfoxide was added, and the mixture was dissolved by heating and stirring. This was measured at 50°C using a Bruker Ascend 400 nuclear magnetic resonance apparatus. The integral values ​​of δ 0.6-1.0 ppm, δ 1.0-1.85 ppm, δ 3.7-4.1 ppm, and δ 4.4-5.3 ppm were defined as x, y, z, and w, respectively. When the contents of the ethylene, vinyl ester, and 1,3-propanediol diacetate structural units were defined as a, b, and c (mol%), respectively, the values ​​were calculated as follows. ·a=(2x+2y-z-4w) / (2x+2y+z+4w)×100 b=8w / (2x+2y+z+4w)×100 c=2z / (2x+2y+z+4w)×100 The degree of saponification was determined by measuring 1H-NMR of the EVOH resin after saponification. That is, about 50 mg of the EVOH resin was weighed into a vial, 1 mL of deuterated dimethyl sulfoxide was added, and the resin was dissolved by heating and stirring. After visually confirming the dissolution, about 10 drops of deuterated trifluoroacetic acid were added using a Pasteur pipette to prepare a measurement solution. This was measured at 80°C using a Bruker Ascend 400 nuclear magnetic resonance apparatus. It was determined from the integral ratio of the methyl protons of the residual vinyl acetate units at δ 1.85 to 2.1 ppm and the methine protons of the vinyl alcohol units at δ 3.15 to 4.15 ppm.

[0113] [Melting point] The melting peak temperature was determined as the melting point using a differential scanning calorimeter (TA Instrument's "Q2000") according to the method of measuring the melting temperature after a certain heat treatment as specified in JIS K7121. Specifically, the sample was heated from -50°C to 250°C at a rate of 10°C / min, melted, cooled to -50°C at a rate of 10°C / min, and then heated again from -50°C to 250°C at a rate of 10°C / min. The temperature at the apex of the melting peak during the second heating was determined as the melting point.

[0114] [Cloud point] The cloud point was measured as follows. That is, the EVOH-based resin (or resin composition) was mixed with water so as to obtain a 4% by mass aqueous solution, which was then heated to 95°C and then cooled to 10°C. At this time, if insoluble matter was observed or turbidity was observed, it was judged to be "insoluble in water" and the subsequent light transmittance measurement was not carried out. The obtained aqueous solutions in which no insoluble matter or turbidity was observed were measured for light transmittance at 430 nm and an optical path length of 10 mm using a JASCO V-750 spectrophotometer and the attached temperature change measurement program, while heating at a temperature increase rate of 1° C. / min from the lower of a temperature at which the transmittance was 80% or more or 20° C., and were measured from when the light transmittance reached 1% or less until the temperature was further increased by 15° C. or more. The temperature at which the light transmittance reached 50% in this measurement was taken as the cloud point. When the light transmittance was more than 50% even after heating up to 90° C., it was considered that no cloud point was observed, and the cloud point was judged to be “absent” (see Table 2). Measuring the light transmittance at 430 nm of a 4 mass % aqueous solution corresponds to the method for measuring the transparency of an aqueous polyvinyl alcohol solution in JIS K6726.

[0115] [Viscosity average degree of polymerization] The EVOH resin was reacetylated with acetic anhydride and pyridine to obtain an EVOH resin. The tetrahydrofuran solution of the EVOH resin was subjected to size exclusion chromatography and treated in accordance with JIS K7252-2 to obtain the value. Specifically, first, the EVOH-based resin was reacetylated by the following procedure. 0.5g of EVOH-based resin was dispersed in a mixed solvent of 4.0g of glacial acetic acid, 4.0g of acetic anhydride, and 0.5g of pyridine, and dissolved at 130°C. The mixture was then reacted at 130°C for 3 hours with occasional stirring. After the reaction was completed, the mixture was cooled and transferred onto a polytetrafluoroethylene sheet and air-dried at room temperature (23°C) for 2 days to form a film. The film was placed in a vacuum dryer at 60°C, and the volatile components were removed while occasionally turning the film over, to obtain a reacetylated product. The reacetylated product is then subjected to size exclusion chromatography. The reacetylated product obtained as described above, i.e., a 0.5% solution of ethylene-vinyl ester copolymer in tetrahydrofuran (THF) was injected into a high-performance liquid chromatograph (Waters ACQUITY APC system) using four columns in series: one ACQUITY APC XT450, one ACQUITY APC XT200, and two ACQUITY APC XT45. The elution time and the signal intensity at that time were recorded using a differential refractive index detector. The molecular weight was calibrated with standard polystyrene. In addition, the K and α in the Mark-Houwink-Sakurada equation for calculating the viscosity average molecular weight are K=3.5×10, which is shown as the value of polyvinyl acetate in tetrahydrofuran in JIS K7252-2, Appendix B. 2 cm 3 / g, α = 0.63 was used. The viscosity average molecular weight Mv thus obtained was converted into the viscosity average degree of polymerization DPv by the following formula. [Formula] DPv = Mv × 100 / [(28 × a) + (44 × b) + (X × c)] a, b, and c were determined by the above-mentioned NMR. They are the contents (percentages) of the ethylene structural unit, the vinyl alcohol structural unit, and the side chain primary hydroxyl structural unit, respectively. X is the molecular weight of the side chain primary hydroxyl structural unit, and is 88 in the case of the structural unit of the general formula (2) or (3).

[0116] [Conjugated polyene content] When the conjugated polyene was sorbic acid, the content was determined as follows. The resin composition was freeze-pulverized, and 200 mg was weighed out. 3.5 mL of methanol was added to disperse the resin composition, and then 1.5 mL of water was added. A mixed solvent of methanol / water = 7 / 3 was added to make the total volume 10 mL, and the mixture was dissolved by irradiating with ultrasonic waves for 60 minutes to prepare a sample. The amount of sorbic acid in this sample was quantified by liquid chromatography. The lower limit of quantification in this method is 0.1 ppm, and if the amount is below the lower limit of quantification, it is expressed as "less than 0.1 ppm."

[0117] [Thermal stability test] 1 g of the resin composition was placed in an Erlenmeyer flask, 100 mL of the solvent shown in Table 3 was poured in, and the mixture was stirred at 95°C for 1 hour, and then cooled to a temperature below the cloud point (Tcp). After that, it was visually confirmed that the solution was a homogeneous solution. Next, 1 g of the resin composition was placed in an aluminum dish and allowed to stand in an inert oven filled with nitrogen at 230°C for 30 minutes to melt. The molten resin composition was cooled to room temperature (23°C) and solidified, then crushed, and 100 mL of the solvent shown in Table 3 was poured into it, stirred at 95°C for 1 hour, and then cooled to a temperature below the cloud point (Tcp). This was visually confirmed, and the thermal stability was evaluated according to the following criteria. (Evaluation Criteria) ◯ (very good): There was no undissolved matter and the solution was homogeneous. × (poor): Undissolved matter was found.

[0118] [Biodegradability] The biodegradability was evaluated according to the method described in JIS K6950 under the following conditions. Equipment: BOD TESTER 200F (manufactured by Taitec) Inoculum source: Return sludge from sewage treatment plants treating domestic sewage Standard test culture medium: 100mL ·Inoculum concentration: 90mg / L ·Temperature: 25±1℃ Duration: 28 days The degree of biodegradation was calculated from the biochemical oxygen consumption and the theoretical oxygen demand.

[0119] <Example 1> [Synthesis of modified ethylene-vinyl ester copolymers] In a temperature-controllable autoclave, 460 parts of vinyl acetate, 44 parts of 3,4-diacetoxy-1-butene as a monomer with a primary hydroxyl group in the side chain protected with an ester or the like, and 179 parts of methanol were charged, and the system was once replaced with nitrogen gas, then replaced with ethylene, and the temperature was raised to 67°C while stirring. After the temperature was raised, ethylene was forced in so that its partial pressure was 1.25 MPa, and a solution in which 0.103 parts of t-butyl peroxy neodecanoate was dissolved in 5.2 parts of methanol (2% solution) was added over 4 hours while continuing stirring, to carry out a polymerization reaction. After the addition was completed, stirring was continued for another 3 hours at 67°C to continue the polymerization reaction. Thereafter, a solution of 0.096 parts of sorbic acid (0.021 parts per 100 parts of vinyl acetate monomer charged) dissolved in 100 parts of methanol was added as a polymerization termination reaction, and the mixture was cooled to room temperature (23°C). To further reduce the amount of unreacted monomer, the mixture was heated to 75°C to remove volatiles and then methanol was added repeatedly to obtain a methanol solution of ethylene-vinyl acetate-3,4-diacetoxybutene copolymer.

[0120] [Synthesis of modified EVOH-based resin composition] Next, primary saponification was carried out. The above solution was diluted with methanol to adjust the concentration to 30%, and stirred in a kneader. While maintaining the solution temperature at 45°C, an 8.7% methanol solution of sodium hydroxide was added in an amount such that the sodium hydroxide was 9 mmol equivalent to the vinyl acetate unit of the copolymer, and stirring was continued. After about 15 minutes, the saponification product precipitated with an increase in viscosity, and finally became a slurry containing particulate matter. After 1 hour, an 8.7% methanol solution of sodium hydroxide was added in an amount such that the sodium hydroxide was 11 mmol equivalent to the vinyl acetate unit of the copolymer, and primary saponification was continued for another 1 hour. In order to further advance the saponification, secondary saponification was carried out. The resulting slurry was once filtered, and then dispersed again in methanol in an amount 5 times the amount of the saponified product. While stirring with a kneader, an 8.7% methanol solution of sodium hydroxide was added in an amount such that the sodium hydroxide was 50 mmol equivalent to the first vinyl acetate unit in the copolymer, and reacted at 50°C for 3 hours. After the reaction, the mixture was neutralized with acetic acid, and the slurry was again filtered to obtain a wet cake. The wet cake was washed three times with methanol in an amount 5 times the mass of the wet cake, filtered, and then dried in a hot air dryer at 100°C for 8 hours to obtain a modified EVOH-based resin composition. The resulting modified EVOH-based resin had a 1,2-butanediol structure as a side chain primary hydroxyl group structural unit.

[0121] The content of ethylene structural units, the content of 1,2-butanediol structural units and the degree of saponification of the obtained modified EVOH-based resin by NMR measurement were 10.6 mol %, 4.0 mol % and 99.7 mol %, respectively. The content of sorbic acid as conjugated polyene in this modified EVOH resin was 0.4 ppm.The melting point and cloud point were 182°C and 40°C, respectively. Furthermore, in the thermal stability test, when water was used as the solvent, a homogeneous solution of water could be obtained. Also, even when the resin composition was melted once, a homogeneous solution of water was obtained, and the thermal stability was good. The biodegradability was 46%. The modified EVOH resin was then acetylated again to obtain a modified ethylene-vinyl ester resin with a viscosity average molecular weight (Mv) of 5.87 × 10 4 From this viscosity average molecular weight, the content of ethylene structural units previously calculated, and the content of 1,2-butanediol structural units, the viscosity average degree of polymerization (DPv) of the modified ethylene-vinyl ester resin was calculated to be 705. This DPv is considered to be the same value as the DPv of the modified EVOH resin before reacetylation. The production conditions and the like of Example 1 are shown in Table 1 below, and the physical properties and the like are shown in Tables 2 and 3 below.

[0122] [Table 1]

[0123] <Examples 2 to 4> Polymerization was performed by changing the amount of vinyl acetate charged, the type and amount of monomer having a primary hydroxyl group in the side chain protected with an ester, the amount of methanol, the partial pressure of ethylene, and the amount of t-butylperoxyneodecanoate in Example 1 as shown in Table 1. The addition time of t-butylperoxyneodecanoate, the duration of polymerization after the addition of t-butylperoxyneodecanoate was completed, the polymerization termination reaction step, the step of reducing unreacted monomers, and the primary saponification were performed in the same manner as in Example 1, and then a modified EVOH-based resin composition was obtained in the same manner as in Example 1, except that the presence or absence of secondary saponification, the amount of alkali used in the secondary saponification, and the washing method of the wet cake after saponification were changed as shown in Table 1. In Example 3, only the primary saponification was carried out, and the secondary saponification was not carried out.

[0124] <Comparative Examples 1 and 2> Polymerization was carried out by changing the amount of vinyl acetate charged, the type and amount of monomer having a primary hydroxyl group in the side chain protected with an ester, the amount of methanol, the partial pressure of ethylene, and the amount of t-butylperoxyneodecanoate in Example 1 as shown in Table 1. The addition time of t-butylperoxyneodecanoate, the duration of polymerization after the addition of t-butylperoxyneodecanoate was completed, the polymerization termination reaction step, and the step of reducing unreacted monomers were carried out in the same manner as in Example 1, and then the primary saponification step was changed as follows. The solution after the process of reducing the unreacted monomer was diluted with methanol to adjust the concentration to 10%, and while stirring in a flask equipped with a stirrer and a cooling tube, a 3.5% methanol solution of sodium hydroxide was added in an amount such that the sodium hydroxide was 10 mmol equivalent to the vinyl acetate unit of the copolymer while maintaining the solution temperature at 45°C, to carry out primary saponification. After about 30 minutes, the saponified product precipitated, eventually becoming a slurry containing particulate matter.

[0125] In Comparative Example 2, secondary saponification was carried out to further promote saponification. The resulting slurry was once filtered and then dispersed again in methanol in an amount 20 times the amount of the saponified product, and while stirring in a flask equipped with a stirrer and a cooling tube, a 3.5% methanol solution of sodium hydroxide was added in an amount such that the amount of sodium hydroxide was 50 mmol equivalent to the initial vinyl acetate unit in the copolymer, and the reaction was carried out at 50° C. for 3 hours. In Comparative Example 1, secondary saponification was not carried out. This was neutralized with acetic acid, and the slurry was filtered to obtain a wet cake. The wet cake was washed three times with five times its mass of methanol and filtered, and then dried in a hot air dryer at 100°C for 8 hours to obtain a modified EVOH-based resin composition.

[0126] <Examples 5 and 6, Comparative Examples 3 to 8> The amount of vinyl acetate charged, the type and amount of the monomer having a primary hydroxyl group in the side chain protected with an ester, and the amount of methanol in Example 1 were changed as shown in Table 1, and the replacement of nitrogen gas and ethylene in the system and the heating to 67°C were performed in the same manner as in Example 1. After the temperature was raised, the ethylene partial pressure was changed as shown in Table 1 and injected, and while continuing stirring, a solution in which 0.082 parts of 2,2'-azobisisobutyronitrile was dissolved in 10 parts of methanol was added, and the polymerization reaction was carried out by maintaining the internal temperature at 67°C for 4 hours while stirring. Thereafter, as a polymerization reaction termination step, a solution in which 0.096 parts of sorbic acid was dissolved in 100 parts of methanol was added, and the mixture was cooled to room temperature (23°C). In order to further reduce the amount of unreacted monomer, removal of volatile matters under reduced pressure and addition of methanol were repeated. Next, the above solution was diluted with methanol to adjust the concentration to 10%, and while stirring in a flask equipped with a stirrer and a cooling tube, a 3.5% methanol solution of sodium hydroxide was added in an amount such that the sodium hydroxide was 10 mmol equivalent relative to the vinyl acetate unit of the copolymer while maintaining the solution temperature at 45° C., to carry out primary saponification. After about 30 minutes, the saponified product precipitated, eventually becoming a slurry containing particulate matter.

[0127] In Examples 5 and 6 and Comparative Examples 4 to 6 and 8, in order to further advance the saponification, secondary saponification was carried out by filtering the produced slurry once and then dispersing it again in methanol in an amount 20 times the amount of the saponified product. While stirring in a flask equipped with a stirrer and a cooling tube, a 3.5% methanol solution of sodium hydroxide was added in an amount such that the amount of sodium hydroxide was 50 mmol equivalent to the first vinyl acetate unit in the copolymer, and the reaction was carried out at 50°C for 3 hours. In Comparative Examples 3 and 7, secondary saponification was not carried out. After the saponification reaction, the mixture was neutralized with acetic acid, and the slurry was filtered again to obtain a wet cake. The wet cake was washed three times with methanol having a mass five times that of the wet cake, and then filtered to obtain particles. In Examples 5 and 6 and Comparative Examples 3 to 7, the particles after filtration were dried in a hot air dryer at 100° C. for 8 hours to obtain modified EVOH-based resin compositions. In Comparative Example 8, the particles after filtration were further subjected to Soxhlet extraction with methanol for one day, and then dried in a hot air dryer at 100° C. for 8 hours to obtain a modified EVOH-based resin composition.

[0128] The content of ethylene structural units, the content of side chain primary hydroxyl structural units, the degree of saponification, the conjugated polyene compound and its content, the melting point, the cloud point, the viscosity average degree of polymerization of the reacetylated modified ethylene-vinyl ester resin determined in accordance with JIS K7252-2, the solvent used in the thermal stability test and its solubility, and the biodegradability of the obtained modified EVOH-based resin compositions or EVOH-based resin compositions of Examples 2 to 6 and Comparative Examples 1 to 8 were determined in the same manner as in Example 1. The results are shown in Tables 2 and 3 below. FIG. 1 shows the relationship between the temperature used to determine the cloud point and the light transmittance in Examples 2, 5, and 6.

[0129] [Table 2]

[0130] [Table 3]

[0131] From the results of Table 3 above, in the thermal stability test, when the resin composition was not melted, a homogeneous solution was obtained for all the Examples and Comparative Examples. Also, when the resin composition was melted once, a homogeneous solution was obtained for all the Examples 1 to 6 and Comparative Examples 1 to 7, and the thermal stability was good. However, in Comparative Example 8, a homogeneous solution could not be obtained, and the thermal stability was poor.

[0132] The obtained resin compositions of Examples 1 to 6 and Comparative Examples 1 to 8 were used to carry out the following evaluations.

[0133] [Pellet production] The modified EVOH resin compositions of Examples 1 to 4 were extruded under the following conditions to prepare pellets. (Pelletizing conditions) Extruder: Shibaura Machine Co., Ltd., twin-screw kneading extruder TEM-18DS Screw: 2-axis, 20mmΦ, L / D=48 Cylinder temperature setting: 170~220℃ Header temperature setting: 210℃ Cooling method of extruded resin: air cooling belt ·Discharge amount: 4kg / hr

[0134] [Melt-extrusion monolayer film production and appearance evaluation criteria] The pellets obtained in Example 1 were extruded under the following conditions to obtain a melt-extruded monolayer film, which was used as a gas barrier material as it is. (Film production conditions) Extruder: Brabender Plastograph EC-plus Screw: Single shaft, 20mmΦ, full flight Cylinder temperature setting: 170~220℃ Cooling roll temperature setting: 80℃ Film thickness: 20μm (Appearance criteria) The appearance of the gas barrier material was judged visually, with those without streaks and with a smooth appearance being rated "good" and those with streaks and a rough appearance being rated "poor."

[0135] [Melt-extrusion multilayer film production and appearance evaluation criteria] The obtained pellets of Examples 2, 3 and 4 were extruded under the following conditions to obtain a melt-extruded multilayer film having a multilayer structure of LLDPE / LLDPE / gas barrier layer (layer made of modified EVOH-based resin composition) / LLDPE / LLDPE, which was used as a gas barrier material as it is. (Film production conditions) Extruder: Plastics Engineering Research Institute, 3-type 5-layer inflation film machine Screw: Single shaft, 20mmΦ, full flight Cylinder temperature setting: 180~210℃ Film thickness: 90μm (LLDPE 40μm / gas barrier layer 10μm / LLDPE 40μm) LLDPE: Novatec LL UF240, manufactured by Mitsubishi Chemical Corporation (Appearance criteria) The appearance of the gas barrier material was judged visually, with those without streaks and with a smooth appearance being rated "good" and those with streaks and a rough appearance being rated "poor."

[0136] [Film production by solution casting and appearance criteria] Aqueous solutions of the resin compositions of Examples 5 and 6 and Comparative Examples 1 to 5, 7, and 8 were applied to a PET film substrate (38 μm thick) with a bar coater at a temperature below the cloud point (Tcp), and the water was subsequently evaporated below the cloud point to obtain a roughly dried gas barrier material. This roughly dried gas barrier material was dried at 80° C. for 5 minutes to obtain a gas barrier material having a 3 μm layer made of the resin composition. Since the resin composition of Comparative Example 6 was not soluble in water, a gas barrier material was not produced. (Appearance criteria) The appearance of the gas barrier material was visually judged, and those without streaks and with a smooth appearance were rated as "good", and those with runny, streaky or rough appearance were rated as "poor".

[0137] [Oxygen permeability] The oxygen permeability of the obtained gas barrier material at 23°C and 65% RH was measured using an oxygen permeability measuring device ("OXTRAN2 / 20" manufactured by MOCON). This measurement value was converted to a value for a thickness of 3 μm of the resin composition, and used as a value indicating the gas barrier property. In Examples 1, 2, 5, and 6 and Comparative Examples 2 to 5, 7, and 8, the same measurements were also made at a humidity of 0% RH. Table 4 shows the appearance of the gas barrier material and the measurement results of oxygen permeability.

[0138] [Table 4]

[0139] In the case of a resin composition having a degree of saponification lower than the range of the present invention, such as Comparative Example 1, the oxygen permeability at 65 RH% was 3.0 cc / m 2 ·day·atm (at 3μm conversion), which was undesirable. As in Comparative Examples 2 and 4, resins in which the relationship between the cloud point and the degree of polymerization does not satisfy formula (i) fail to produce gas barrier materials with good appearance (Comparative Example 2), and the oxygen permeability at 65 RH% is 3.0 cc / m 2 ·day·atm (when converted into 3 μm) and the biodegradability was low (Comparative Example 4), which was undesirable. A resin composition having too high a degree of polymerization, such as that in Comparative Example 3, was not preferable because it was not possible to obtain a gas barrier material with a good appearance. In the case of Comparative Example 5, where no clouding point was observed, the oxygen transmission rate at 65 RH% was 3.0 cc / m 2 ·day·atm (at 3μm conversion), which was undesirable. As in Comparative Example 6, the water-insoluble material was undesirable because of its low biodegradability. When the degree of polymerization was too low, as in Comparative Example 7, the appearance was poor (the melting point was high and the biodegradability was low because there was no modification with primary hydroxyl groups on the side chains), which was undesirable. When the content of the conjugated polyene was too low, as in Comparative Example 8, the thermal stability was unfavorable, as shown in Table 3. [Industrial Applicability]

[0140] The modified EVOH-based resin composition of the present invention exhibits good biodegradability and thermal stability, and prevents poor appearance due to application of the aqueous solution to a substrate or melt molding, even though the aqueous solution has a cloud point. It also exhibits high gas barrier properties even under high humidity. Therefore, the composition can be suitably used in fields where a reduction in environmental load is required, particularly as a gas barrier material for food packaging and the like.

Claims

1. A resin composition comprising a modified ethylene-vinyl alcohol resin having a primary hydroxyl group structural unit in a side chain and a conjugated polyene in an amount of 0.1 ppm or more and 500 ppm or less, The modified ethylene-vinyl alcohol resin has an ethylene structural unit content of 2.5 to 16.5 mol% and a saponification degree of more than 98.5 mol%, the degree of polymerization (DPv) of the modified ethylene-vinyl alcohol resin calculated from the viscosity average molecular weight of a tetrahydrofuran solution of the modified ethylene-vinyl ester copolymer after reacetylation is 450 or more and 1350 or less; The relationship between the cloud point (Tcp) of a 4 mass% aqueous solution of the resin composition and the degree of polymerization (DPv) satisfies the following formula (i): [Formula] −14 × Tcp + 1200 ≦ DPv ... (i)

2. The modified ethylene-vinyl alcohol resin composition according to claim 1, wherein the following formula (ii) is satisfied between the melting point (Tm) and the cloud point (Tcp) of the modified ethylene-vinyl alcohol resin. [Formula] 0.4×Tcp+155≦Tm≦0.2×Tcp+179…(ii)

3. The modified ethylene-vinyl alcohol resin composition according to claim 1 or 2, wherein the cloud point (Tcp) is 15° C. or higher.

4. The modified ethylene-vinyl alcohol resin composition according to claim 2, wherein the melting point (Tm) is 190° C. or lower.

5. A gas barrier material having a layer made of the modified ethylene-vinyl alcohol resin composition according to claim 1 or 2.

6. A method for producing a gas barrier material, comprising applying an aqueous solution of the modified ethylene-vinyl alcohol resin composition according to claim 1 or 2 to a substrate at a temperature not exhibiting a cloud point.

Citation Information

Patent Citations

  • Binder for molding ceramics

    JP2000272970A

  • Modified vinyl alcohol-based polymer

    JP2015034262A

  • Ethylene-vinyl ester copolymer saponification product and hose or storage container for high-pressure gas

    JP2016069481A

  • Dispersion stabilizer for suspension polymerization, and manufacturing method for vinyl resin

    WO2015019614A1

  • Resin composition and molded article using same, and multilayer structure