Water-based treatment agent, method for producing rubber reinforcement member, rubber reinforcement member and rubber product
An aqueous treatment agent with resorcinol-formaldehyde condensate and ethylene-glycidyl methacrylate copolymer improves adhesion and bending resistance in rubber products by forming a flexible coating on reinforcing fibers for EPDM rubber.
Patent Information
- Application Number
- JP2023052428
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-28
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-28
AI Technical Summary
Conventional processing agents used to adhere reinforcing fibers to EPDM rubber result in hard coatings that compromise the flexibility and bending resistance of rubber products.
An aqueous treatment agent comprising resorcinol-formaldehyde condensate, rubber latex with ethylene-glycidyl methacrylate copolymer and chlorosulfonated polyethylene is applied to form a coating on reinforcing fibers, enhancing adhesion to EPDM rubber while maintaining flexibility.
The solution provides a rubber reinforcing member with improved bending resistance and adhesion to EPDM rubber, ensuring excellent adhesion between the matrix rubber and reinforcing member.
Smart Images

Figure 2024141011000005 
Figure 2024141011000006 
Figure 2024141011000007
Abstract
Description
[Technical field]
[0001] The present invention relates to an aqueous treatment agent for forming a rubber-reinforcing member, a method for producing a rubber-reinforcing member, a rubber-reinforcing member, and a rubber product. [Background technology]
[0002] In rubber products such as rubber belts or rubber tires, in order to improve their strength and durability, it is widely and commonly practiced to embed rubber reinforcing members such as rubber reinforcing cords and rubber reinforcing sheets in the matrix rubber constituting the rubber products. For example, in rubber reinforcing cords, glass fibers or chemical fibers are used as reinforcing fibers.
[0003] Ethylene propylene diene rubber (EPDM rubber) has excellent heat resistance, weather resistance, and ozone resistance. Therefore, it is widely used in rubber products such as transmission belts, conveyor belts, tires, rubber hoses, etc. EPDM rubber has been attracting attention in recent years from an environmental perspective due to its halogen-free structure.
[0004] When the matrix rubber of a rubber product is EPDM rubber, embedding reinforcing fibers directly in the EPDM rubber does not provide sufficient adhesion between the matrix rubber and the reinforcing fibers.
[0005] For example, Patent Document 1 discloses a resorcin-formaldehyde-latex-based treatment agent as a treatment agent for adhering a fiber material to a rubber composition containing EPDM. It is proposed to use a latex of an ethylene-glycidyl methacrylate copolymer as the latex component of the resorcin-formaldehyde-latex-based treatment agent. Patent Document 2 discloses a treatment agent containing a resorcin-formaldehyde condensate, a latex of an ethylene-glycidyl methacrylate copolymer, and a latex of a carboxyl-modified styrene-butadiene copolymer as a treatment agent for adhering a glass fiber cord to a rubber composition containing EPDM. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Patent No. 4286393 [Patent Document 2] Patent No. 4899495 Summary of the Invention [Problem to be solved by the invention]
[0007] The reinforcing member obtained by treating the reinforcing fiber with the above-mentioned conventional treating agent has excellent adhesion to EPDM rubber due to the coating formed on the surface of the reinforcing fiber. However, the reinforcing member obtained by treating the reinforcing fiber with the above-mentioned conventional treating agent becomes hard and loses flexibility due to the coating, resulting in a decrease in bending resistance.
[0008] Therefore, one of the objects of the present invention is to provide an aqueous treatment agent capable of forming a coating film capable of improving flex resistance while maintaining excellent adhesion to EPDM rubber. Another object of the present invention is to provide a rubber reinforcing member having improved flex resistance while maintaining excellent adhesion to EPDM rubber. Another object of the present invention is to provide a rubber product having excellent adhesion between the matrix rubber and the rubber reinforcing member and having flex resistance even when the matrix rubber contains EPDM rubber. [Means for solving the problem]
[0009] The present invention provides an aqueous treatment agent for producing a coating on a rubber-reinforcing member having a coating, comprising: The aqueous treatment agent is Resorcinol-formaldehyde condensate; Rubber latex and Including, The rubber latex contains, as rubber components, an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene.
[0010] From another aspect, the present invention provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: (a) supplying the aqueous treatment agent of the present invention to at least a part of a surface of a reinforcing substrate and drying the aqueous treatment agent to form a coating on the surface of the reinforcing substrate; The present invention provides a method for producing a rubber reinforcing member, comprising the steps of:
[0011] From another aspect, the present invention provides a rubber reinforcing member for reinforcing a rubber product, comprising: The rubber reinforcing member is A reinforcing base material; A coating provided so as to cover at least a portion of the surface of the reinforcing base material; Including, The coating contains a resorcinol-formaldehyde condensate and a rubber component, The rubber component includes an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene.
[0012] From another aspect, the present invention provides a method for producing a method for manufacturing a semiconductor device comprising the steps of: Matrix rubber; The rubber reinforcing member of the present invention, The present invention provides a rubber product comprising: Effect of the Invention
[0013] According to the present invention, it is possible to provide an aqueous treatment agent capable of forming a coating capable of improving flex resistance while ensuring excellent adhesion to EPDM rubber. Furthermore, according to the present invention, it is possible to provide a rubber reinforcing member having improved flex resistance while ensuring excellent adhesion to EPDM rubber. Furthermore, according to the present invention, it is possible to provide a rubber product having excellent adhesion between the matrix rubber and the rubber reinforcing member and having flex resistance even when the matrix rubber contains EPDM rubber. [Brief description of the drawings]
[0014] [Figure 1A] FIG. 1 is a partially exploded perspective view showing a schematic diagram of an example of a rubber product of the present invention. [Figure 1B] FIG. 2 is a cross-sectional view illustrating a schematic diagram of another example of the rubber product of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view showing a strand of an embodiment. [Diagram 3] FIG. 2 is a cross-sectional view showing a rubber reinforcing cord according to an embodiment of the present invention. [Figure 4] FIG. 2 is a diagram showing a schematic diagram of a bending test performed on the rubber reinforcing cords of the examples and the comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] A first aspect of the present invention is an aqueous treatment agent for producing a coating on a rubber reinforcing member having a coating, comprising: The aqueous treatment agent is Resorcinol-formaldehyde condensate; Rubber latex and Including, The rubber latex contains, as rubber components, an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene.
[0016] In the second aspect of the present invention, for example, in the aqueous treatment agent according to the first aspect, In the rubber component of the rubber latex, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 95% by mass or less, The content of chlorosulfonated polyethylene is 5% by mass or more and 85% by mass or less.
[0017] In the third aspect of the present invention, for example, in the aqueous treatment agent according to the second aspect, In the rubber component of the rubber latex, The content of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 70% by mass or less, The content of chlorosulfonated polyethylene is 30% by mass or more and 85% by mass or less.
[0018] In the fourth aspect of the present invention, for example, in the aqueous treatment agent according to the third aspect, In the rubber component of the rubber latex, The content of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 50% by mass or less, The content of chlorosulfonated polyethylene is 50% by mass or more and 85% by mass or less.
[0019] In the fifth aspect of the present invention, for example, in the aqueous treatment agent according to the fourth aspect, In the rubber component of the rubber latex, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 40% by mass or less, The content of the chlorosulfonated polyethylene is 60% by mass or more and 85% by mass or less.
[0020] In a sixth aspect of the present invention, for example, in the aqueous treatment agent according to any one of the first to fifth aspects, the content ratio of chlorosulfonated polyethylene in the rubber component of the rubber latex is equal to or greater than the content ratio of ethylene-glycidyl methacrylate copolymer, by mass ratio.
[0021] A seventh aspect of the present invention is (a) supplying an aqueous treatment agent according to any one of the first to sixth aspects to at least a part of a surface of a reinforcing substrate and drying the aqueous treatment agent to form a coating on the surface of the reinforcing substrate; A method for producing a rubber reinforcing member, comprising the steps of:
[0022] In an eighth aspect of the present invention, for example, in the production method according to the seventh aspect, The reinforcing substrate is a filament bundle, The manufacturing method includes: (b) bundling a plurality of filaments to form at least one said filament bundle; Further comprising: In the step (a), the aqueous treatment agent is supplied to at least a portion of the surface of the filament bundle, and then dried to produce a strand having the coating formed on the surface of the filament bundle.
[0023] In a ninth aspect of the present invention, for example, in the production method according to the seventh aspect, The reinforcing base material is a fiber sheet, In the step (a), the aqueous treatment agent is supplied to at least a part of the surface of the fiber sheet and then dried to form the coating on the fiber sheet.
[0024] A tenth aspect of the present invention is a rubber reinforcing member for reinforcing a rubber product, The rubber reinforcing member is A reinforcing base material; A coating provided so as to cover at least a portion of the surface of the reinforcing base material; Including, The coating contains a resorcinol-formaldehyde condensate and a rubber component, The rubber component includes an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene.
[0025] In an eleventh aspect of the present invention, for example, in the rubber reinforcing member according to the tenth aspect, In the rubber component of the coating, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 95% by mass or less, The content of chlorosulfonated polyethylene is 5% by mass or more and 85% by mass or less.
[0026] In the twelfth aspect of the present invention, for example, in the rubber reinforcing member according to the eleventh aspect, In the rubber component of the coating, The content of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 70% by mass or less, The content of chlorosulfonated polyethylene is 30% by mass or more and 85% by mass or less.
[0027] In the thirteenth aspect of the present invention, for example, in the rubber reinforcing member according to the twelfth aspect, In the rubber component of the coating, The content of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 50% by mass or less, The content of chlorosulfonated polyethylene is 50% by mass or more and 85% by mass or less.
[0028] In a fourteenth aspect of the present invention, for example, in the rubber reinforcing member according to the thirteenth aspect, In the rubber component of the coating, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 40% by mass or less, The content of the chlorosulfonated polyethylene is 60% by mass or more and 85% by mass or less.
[0029] In a fifteenth aspect of the present invention, for example, in the rubber reinforcing member according to any one of the tenth to fourteenth aspects, the content of chlorosulfonated polyethylene in the coating is equal to or greater than the content of ethylene-glycidyl methacrylate copolymer, by mass ratio.
[0030] In a sixteenth aspect of the present invention, for example, in the rubber-reinforcing member according to any one of the tenth to fifteenth aspects, the coating is provided on the outermost surface of the rubber-reinforcing member.
[0031] The rubber product according to the seventeenth aspect of the present invention is Matrix rubber; A rubber reinforcing member according to any one of the tenth to sixteenth aspects; Includes.
[0032] In an eighteenth aspect of the present invention, for example, in the rubber product according to the seventeenth aspect, the matrix rubber contains EPDM.
[0033] In a nineteenth aspect of the present invention, for example, in the rubber product according to the seventeenth or eighteenth aspect, the coating of the rubber reinforcing member and the matrix rubber are in contact with each other.
[0034] Hereinafter, an embodiment of the present invention will be described in detail.
[0035] (First embodiment) As a first embodiment, an embodiment of the aqueous treatment agent of the present invention will be described.
[0036] The aqueous treatment agent of the present embodiment is an aqueous treatment agent for forming a rubber-reinforcing member having a coating. That is, the aqueous treatment agent of the present embodiment is an aqueous treatment agent for producing a coating for a rubber-reinforcing member. The rubber-reinforcing member is, for example, a rubber-reinforcing cord, a rubber-reinforcing sheet, etc.
[0037] The aqueous treatment agent of this embodiment contains a resorcinol-formaldehyde condensate and a rubber latex. That is, the aqueous treatment agent of this embodiment contains a mixed liquid (RFL) of a resorcinol-formaldehyde condensate (RF) and a rubber latex (L). The rubber latex contains an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene (CSM) as a rubber component.
[0038] In the aqueous treatment agent of this embodiment, the rubber component of the rubber latex of the RFL contains an ethylene-glycidyl methacrylate copolymer and a CSM. By containing a combination of an ethylene-glycidyl methacrylate copolymer and a CSM as the rubber component, the aqueous treatment agent of this embodiment can produce a coating that can improve flex resistance while ensuring excellent adhesion to EPDM rubber on the surface of a reinforcing fiber (for example, a filament bundle or fiber sheet containing a plurality of filaments) used as a reinforcing substrate. The rubber latex in the aqueous treatment agent of this embodiment contains, for example, a rubber latex of an ethylene-glycidyl methacrylate copolymer and a rubber latex of a CSM.
[0039] In the aqueous treatment agent of this embodiment, the content of the ethylene-glycidyl methacrylate copolymer in the rubber component of the rubber latex is preferably 15% by mass or more and 95% by mass or less, and the content of the CSM is preferably 5% by mass or more and 85% by mass or less. By including the ethylene-glycidyl methacrylate copolymer and the CSM in such a ratio, the aqueous treatment agent of this embodiment can produce a coating film that is well balanced between adhesion and flex resistance.
[0040] In order to produce a coating film having an excellent balance between adhesion and flex resistance, in the aqueous treatment agent of this embodiment, it is more preferable that the rubber component of the rubber latex contains ethylene-glycidyl methacrylate copolymer in an amount of 15% by mass or more and 70% by mass or less and CSM in an amount of 30% by mass or more and 85% by mass or less.
[0041] In order to produce a coating film having an excellent balance between adhesion and flex resistance, in the aqueous treatment agent of this embodiment, it is more preferable that the rubber component of the rubber latex contains ethylene-glycidyl methacrylate copolymer in an amount of 15% by mass or more and 50% by mass or less and CSM in an amount of 50% by mass or more and 85% by mass or less.
[0042] In order to produce a coating film with an even better balance between adhesion and flex resistance, in the aqueous treatment agent of this embodiment, it is further preferable that the rubber component of the rubber latex contains ethylene-glycidyl methacrylate copolymer in an amount of 15% by mass or more and 40% by mass or less, and contains CSM in an amount of 60% by mass or more and 85% by mass or less.
[0043] In order to produce a coating film that has an excellent balance between adhesion and flex resistance, in the aqueous treatment agent of this embodiment, the content of CSM in the rubber component of the rubber latex, in terms of mass ratio, is preferably equal to or greater than the content of ethylene-glycidyl methacrylate copolymer, and more preferably greater than the content of ethylene-glycidyl methacrylate copolymer.
[0044] In the aqueous treatment agent of this embodiment, the mass ratio of CSM to ethylene-glycidyl methacrylate copolymer (mass of CSM / mass of ethylene-glycidyl methacrylate copolymer) in the rubber component of the rubber latex is preferably 5 / 95 or more, more preferably 30 / 70 or more, and even more preferably 50 / 50 or more. In the aqueous treatment agent of this embodiment, the mass ratio of CSM to ethylene-glycidyl methacrylate copolymer (mass of CSM / mass of ethylene-glycidyl methacrylate copolymer) in the rubber component of the rubber latex is preferably 85 / 15 or less, and more preferably 70 / 30 or less.
[0045] In the aqueous treatment agent of this embodiment, the rubber component of the rubber latex may further contain another rubber component other than the ethylene-glycidyl methacrylate copolymer and the CSM. The other rubber component may be, for example, at least one selected from the group consisting of a styrene-butadiene copolymer, a dicarboxylated butadiene-styrene polymer, a styrene-butadiene-vinylpyridine terpolymer, a chloroprene rubber, a butadiene rubber, a nitrile rubber, a hydrogenated nitrile rubber, a carboxyl-modified nitrile rubber, and a carboxyl-modified hydrogenated nitrile rubber.
[0046] In order to prepare a coating having an excellent balance between adhesion and flex resistance, the rubber component of the rubber latex preferably has a total content of the ethylene-glycidyl methacrylate copolymer and the CSM of 70% by mass or more, more preferably 90% by mass or more. When the proportions of the ethylene-glycidyl methacrylate copolymer and the CSM in the rubber component of the rubber latex satisfy the above ranges, a coating having an excellent balance between adhesion and flex resistance can be prepared.
[0047] In order to prepare a coating film having a better balance between adhesion and flex resistance, the rubber component of the rubber latex may be substantially composed of an ethylene-glycidyl methacrylate copolymer and CSM. The rubber component of the rubber latex being substantially composed of an ethylene-glycidyl methacrylate copolymer and CSM means that the rubber component of the rubber latex does not contain any other components than the ethylene-glycidyl methacrylate copolymer and CSM, except for components that are inevitably mixed in. Specifically, the total content of the ethylene-glycidyl methacrylate copolymer and the CSM in the rubber component of the rubber latex is 95% by mass or more, preferably 98% by mass or more. The rubber component of the rubber latex may be composed only of an ethylene-glycidyl methacrylate copolymer and CSM.
[0048] In the aqueous treatment agent of this embodiment, the resorcin-formaldehyde condensate (RF) is not particularly limited. A resol type RF obtained by reacting resorcin and formaldehyde in the presence of an alkaline catalyst such as an alkali hydroxide and an amine, and a novolac type RF obtained by reacting resorcin and formaldehyde in the presence of an acid catalyst can be suitably used. A mixture of a resol type RF and a novolac type RF may be used. In particular, it is preferable to use an RF obtained by reacting resorcin (R) and formaldehyde (F) at a molar ratio R:F = 2:1 to 1:3. The content ratio of the RF component in the aqueous treatment agent is preferably 1 mass% or more, more preferably 5 mass% or more, in terms of solid content. The content ratio of the RF component in the solid content of the aqueous treatment agent is preferably 20 mass% or less, more preferably 15 mass% or less. When an aqueous treatment agent has an RF component content of 1% by mass or more and 20% by mass or less in terms of solid content, it is possible to produce a coating that has good adhesion to matrix rubber, particularly matrix rubber containing EPDM.
[0049] In the aqueous treatment agent of this embodiment, the mass ratio of the resorcinol-formaldehyde condensate to the rubber latex (mass of the resorcinol-formaldehyde condensate / mass of the rubber latex) in terms of solid content is preferably more than 0.05 and not more than 0.12, which allows the preparation of a coating film having better adhesion.
[0050] The aqueous treatment agent of the present embodiment may contain other components in addition to the resorcinol-formaldehyde condensate and the rubber latex, such as a crosslinking agent, a filler, a resin, a plasticizer, an antioxidant, a stabilizer, a metal oxide that is not a filler, and the like.
[0051] The components of the aqueous treatment agent of this embodiment (components other than the solvent) are dispersed or dissolved in the solvent. The solvent of the aqueous treatment agent of this embodiment is an aqueous solvent containing water at a ratio of 50% by mass or more. The content of water in the aqueous solvent may be 80% by mass or more, 90% by mass or more, or 100% by mass. As the aqueous solvent, water is preferably used because it is easy to handle, the concentration of the components is easy to control, and the environmental load is significantly reduced compared to organic solvents. The aqueous solvent may contain lower alcohols, etc. Examples of lower alcohols include alcohols with 4 or less carbon atoms or 3 or less carbon atoms (e.g., methanol, ethanol, and propanol). However, it is preferable that the aqueous solvent does not contain organic solvents other than lower alcohols.
[0052] Second embodiment As a second embodiment, an embodiment of a rubber reinforcing member and a rubber product of the present invention will be described.
[0053] The rubber reinforcing member of this embodiment includes a reinforcing substrate and a coating provided so as to cover at least a portion of the surface of the reinforcing substrate. The coating includes a resorcinol-formaldehyde condensate and a rubber component. The rubber component includes an ethylene-glycidyl methacrylate copolymer and a CSM.
[0054] The coating is provided so as to cover at least a part of the surface of the reinforcing base material. The coating may be provided directly on the surface of the reinforcing base material, or may cover the surface of the reinforcing base material via another layer.
[0055] As described above, the coating contains a resorcinol-formaldehyde condensate, and a rubber component containing an ethylene-glycidyl methacrylate copolymer and a CSM. By providing a coating having this configuration, the rubber reinforcing member of the present embodiment can improve bending resistance while ensuring excellent adhesion to EPDM rubber.
[0056] In the rubber reinforcing member of this embodiment, the rubber component of the coating preferably contains 15% by mass or more and 95% by mass or less of ethylene-glycidyl methacrylate copolymer and 5% by mass or more and 85% by mass or less of CSM. By providing a coating containing ethylene-glycidyl methacrylate copolymer and CSM in such a ratio, the rubber reinforcing member of this embodiment can have an excellent balance between adhesion and bending resistance.
[0057] In order to realize a rubber reinforcement component having an excellent balance between adhesion and flex resistance, it is more preferable that in the rubber component of the coating of this embodiment, the content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 70% by mass or less, and the content of CSM is 30% by mass or more and 85% by mass or less.
[0058] In order to realize a rubber reinforcement component having an excellent balance between adhesion and flex resistance, it is more preferable that in the rubber component of the coating of this embodiment, the content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 50% by mass or less, and the content of CSM is 50% by mass or more and 85% by mass or less.
[0059] In order to realize a rubber reinforcement component having an even better balance between adhesion and flex resistance, it is further preferable that in the rubber component of the coating of this embodiment, the content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 40% by mass or less, and the content of CSM is 60% by mass or more and 85% by mass or less.
[0060] In order to realize a rubber reinforcing member having an excellent balance between adhesion and flex resistance, in the rubber reinforcing member of this embodiment, the content of CSM in the coating, in mass ratio, is preferably equal to or greater than the content of ethylene-glycidyl methacrylate copolymer, and is more preferably greater than the content of ethylene-glycidyl methacrylate copolymer.
[0061] In the rubber reinforcing member of this embodiment, the mass ratio of CSM to ethylene-glycidyl methacrylate copolymer (mass of CSM / mass of ethylene-glycidyl methacrylate copolymer) in the rubber component of the coating is preferably 5 / 95 or more, more preferably 30 / 70 or more, and even more preferably 50 / 50 or more. In the rubber reinforcing member of this embodiment, the mass ratio of CSM to ethylene-glycidyl methacrylate copolymer (mass of CSM / mass of ethylene-glycidyl methacrylate copolymer) in the rubber component of the coating is preferably 85 / 15 or less, and more preferably 70 / 30 or less.
[0062] In the rubber reinforcing member of this embodiment, the rubber component of the coating may further contain another rubber component other than the ethylene-glycidyl methacrylate copolymer and the CSM. The other rubber component may be, for example, at least one selected from the group consisting of a styrene-butadiene copolymer, a dicarboxylated butadiene-styrene polymer, a styrene-butadiene-vinylpyridine terpolymer, a chloroprene rubber, a butadiene rubber, a nitrile rubber, a hydrogenated nitrile rubber, a carboxyl-modified nitrile rubber, and a carboxyl-modified hydrogenated nitrile rubber.
[0063] In order to realize a rubber-reinforcing member having an excellent balance between adhesion and flex resistance, in the rubber component of the coating of the rubber-reinforcing member of this embodiment, the total content of the ethylene-glycidyl methacrylate copolymer and the CSM is preferably 70 mass % or more, and more preferably 90 mass % or more. When the proportions of the ethylene-glycidyl methacrylate copolymer and the CSM in the rubber component of the coating satisfy the above ranges, a rubber-reinforcing member having an excellent balance between adhesion and flex resistance can be realized.
[0064] In order to realize a rubber reinforcing member having a better balance between adhesion and flex resistance, the rubber component of the coating may be substantially composed of an ethylene-glycidyl methacrylate copolymer and CSM in the rubber reinforcing member of this embodiment. The rubber component of the coating substantially composed of an ethylene-glycidyl methacrylate copolymer and CSM means that the rubber component of the coating does not contain any other components than the ethylene-glycidyl methacrylate copolymer and CSM, except for components that are inevitably mixed in. Specifically, the total content of the ethylene-glycidyl methacrylate copolymer and the CSM in the rubber component of the coating is 95% by mass or more, preferably 98% by mass or more. The rubber component of the coating may be composed of only an ethylene-glycidyl methacrylate copolymer and CSM.
[0065] In the rubber reinforcing member of this embodiment, the resorcin-formaldehyde condensate (RF) contained in the coating is not particularly limited. A resol type RF obtained by reacting resorcin and formaldehyde in the presence of an alkaline catalyst such as an alkali hydroxide and an amine, and a novolac type RF obtained by reacting resorcin and formaldehyde in the presence of an acid catalyst can be suitably used. A mixture of a resol type RF and a novolac type RF may be used. In particular, it is preferable to use an RF obtained by reacting resorcin (R) and formaldehyde (F) at a molar ratio R:F = 2:1 to 1:3. The content ratio of the RF component in the coating is preferably 1 mass% or more, more preferably 5 mass% or more. The content ratio of the RF component in the coating is preferably 20 mass% or less, more preferably 15 mass% or less. By providing a coating having an RF component content of 1% by mass or more and 20% by mass or less, a rubber reinforcing member that has good adhesion to matrix rubber, particularly matrix rubber containing EPDM, can be realized.
[0066] In the rubber reinforcing member of the present embodiment, the mass ratio of the resorcin-formaldehyde condensate to the rubber component in the coating (mass of resorcin-formaldehyde condensate / mass of rubber component) is preferably more than 0.05 and not more than 0.12, thereby realizing a rubber reinforcing member having better adhesiveness.
[0067] The coating in the rubber reinforcing member of the present embodiment may contain other components in addition to the resorcinol-formaldehyde condensate and the rubber latex, such as a crosslinking agent, a filler, a resin, a plasticizer, an antioxidant, a stabilizer, a metal oxide that is not a filler, and the like.
[0068] In the rubber reinforcing member of this embodiment, the coating may be provided on the outermost surface of the rubber reinforcing member. The coating has excellent adhesion to EPDM rubber. Therefore, even when the matrix rubber contains EPDM rubber, the rubber reinforcing member of this embodiment does not need to have another coating on the coating for the purpose of improving adhesion to the matrix rubber. Therefore, the rubber reinforcing member of this embodiment can achieve both sufficient adhesion to the matrix rubber and bending resistance while suppressing an increase in manufacturing costs. Note that the rubber reinforcing member of this embodiment may be provided with another coating in addition to the coating.
[0069] The mass of the coating provided at least on the surface of the reinforcing base material is not particularly limited and may be adjusted appropriately. For example, the coating is preferably provided so as to be within the range of 5% by mass or more and 35% by mass or less of the mass of the reinforcing base material. The mass of the coating may be 10% by mass or more of the mass of the reinforcing base material. The mass of the coating may be 25% by mass or less or 20% by mass or less of the mass of the reinforcing base material. The mass of the coating may be within the range of 10% by mass or more and 20% by mass or less of the mass of the reinforcing base material. If the mass of the coating is too large (the amount of the coating is too large), problems such as a decrease in the dimensional stability of the rubber reinforcing member in the rubber product and a decrease in the elastic modulus of the rubber reinforcing member may occur. On the other hand, if the mass of the coating is too small (the amount of the coating is too small), for example, in the case where the reinforcing member is a rubber reinforcing cord including strands, the strands may easily fray or the function of protecting the fibers by the coating may decrease, resulting in a decrease in the life of the rubber product.
[0070] The rubber-reinforcing member of the present embodiment is, for example, a rubber-reinforcing cord or a rubber-reinforcing sheet. Hereinafter, the rubber-reinforcing cord and the rubber-reinforcing sheet will be specifically described as the rubber-reinforcing member.
[0071] [Rubber reinforcement cord] The rubber reinforcing cord of this embodiment is a cord for reinforcing rubber products. This rubber reinforcing cord has at least one strand. This strand includes at least one filament bundle (reinforcing fiber) and a coating provided so as to cover at least a part of the surface of the filament bundle. In the rubber reinforcing cord, the filament bundle corresponds to the reinforcing substrate. The coating is the coating described above, that is, it includes a resorcinol-formaldehyde condensate and a rubber component including an ethylene-glycidyl methacrylate copolymer and a CSM.
[0072] In the rubber reinforcing cord of this embodiment, the filament bundle constituting the strand includes a plurality of filaments. The material of the filament is not particularly limited. For example, glass fiber filaments, polyvinyl alcohol fiber filaments typified by vinylon fiber, polyester fiber filaments, polyamide fiber filaments such as nylon and aramid fiber (aromatic polyamide), carbon fiber filaments, or polyparaphenylene benzobisoxazole (PBO) fiber filaments can be used as the filaments of the rubber reinforcing cord of this embodiment. Among these, it is preferable to use filaments of fibers excellent in dimensional stability, tensile strength, modulus, and flex fatigue resistance. For example, it is preferable to use at least one fiber filament selected from glass fiber filaments, aramid fiber filaments, polyparaphenylene benzobisoxazole fiber filaments, and carbon fiber filaments. In particular, it is preferable to use at least one fiber filament selected from glass fiber filaments, aramid fiber filaments, and carbon fiber filaments. The filament bundle may be composed of one type of filament, or may be composed of multiple types of filaments.
[0073] The number of filaments contained in the filament bundle is not particularly limited. The filament bundle may contain, for example, 200 to 24,000 filaments.
[0074] The surface of the filament contained in the filament bundle may be pretreated to increase the adhesive strength. A preferred example of the pretreatment agent is a compound containing at least one functional group selected from the group consisting of an epoxy group and an amino group. Examples of the pretreatment agent include aminosilane, epoxysilane, novolac type epoxy resin, bisphenol A type epoxy resin, bisphenol F type epoxy resin, brominated epoxy resin, bisphenol AD type epoxy resin, glycidylamine type epoxy resin, etc. Specific examples include the Denacol series of Nagase ChemteX Corporation, the Epiclon series of DIC Corporation, and the Epicoat series of Mitsubishi Chemical Corporation. In addition, polyurethane resins and isocyanate compounds can also be used as the pretreatment agent. For example, a treatment agent containing at least one selected from the group consisting of an epoxy resin, a urethane resin, and an isocyanate compound may be used as the pretreatment agent. By pretreating with such a treatment agent, a resin layer containing at least one selected from the group consisting of an epoxy resin, a urethane resin, and an isocyanate compound is further provided between the filament bundle and the coating. By pretreating the surface, it is possible to increase the adhesion between the matrix rubber and the rubber reinforcing cord, even when using fiber filaments that are difficult to bond, such as polyparaphenylene terephthalamide fiber filaments. Note that the coating (pretreatment agent film) made of a pretreatment agent formed on the filament surface by pretreatment of the filaments is different from the coating that covers at least a part of the surface of the filament bundle as specified in this embodiment, and is not included in the coating specified in this embodiment.
[0075] The number of filament bundles included in the rubber reinforcing cord is not limited, and may be one or more. The filament bundle may be a bundle of multiple filament bundles. In this case, each of the multiple filament bundles may be twisted or not twisted. Furthermore, the multiple filament bundles may be twisted together or not twisted. The number of twists of the filament bundle is not particularly limited. The number of twists (hereinafter sometimes referred to as first twists) added to one filament bundle may be in the range of, for example, 1 to 6 times / 25 mm. Furthermore, the number of twists (hereinafter sometimes referred to as second twists) added to multiple filament bundles may be in the range of, for example, 1 to 8 times / 25 mm. The first twist and the second twist may be in the same direction, i.e., a rung twist, or a moro twist, in which the first twist and the second twist are in the opposite directions. The twist direction is not limited, and may be in the S direction or the Z direction.
[0076] The coating is provided so as to cover at least a part of the surface of the filament bundle. The coating may be provided directly on the surface of the filament bundle, or may cover the surface of the filament bundle via another layer.
[0077] The rubber-reinforcing cord of this embodiment may or may not be provided with a further coating other than the coating. As described above, the "further coating" does not include the pretreatment agent film. Therefore, even if the rubber-reinforcing cord has this coating provided on the surface of a filament bundle including filaments on which the pretreatment agent film is provided, it can be considered as a "rubber-reinforcing cord not provided with a further coating other than the coating."
[0078] The number of twists of the rubber reinforcing cord of this embodiment is not particularly limited. The number of twists (hereinafter sometimes referred to as first twists) added to one strand may be in the range of, for example, 1 to 6 times / 25 mm. Furthermore, the number of twists (hereinafter sometimes referred to as second twists) added to a plurality of strands may be in the range of, for example, 1 to 8 times / 25 mm. It may be a rung twist in which the first twist direction and the second twist direction are the same, or a moro twist in which the first twist direction and the second twist direction are opposite. There is no limitation on the twist direction, and it may be the S direction or the Z direction.
[0079] [Rubber reinforcing sheet] The rubber reinforcing sheet of this embodiment is a sheet for reinforcing rubber products. This rubber reinforcing sheet includes a fiber sheet as a reinforcing substrate and a coating formed on the fiber sheet. In the rubber reinforcing sheet, the fiber sheet corresponds to the reinforcing substrate. The coating is the coating described above, that is, it includes a resorcinol-formaldehyde condensate, an ethylene-glycidyl methacrylate copolymer, and a rubber component including CSM.
[0080] The coating of the rubber-reinforcing sheet of this embodiment is similar to the coating of the rubber-reinforcing cord of this embodiment described above, and therefore a detailed description of the coating of the rubber-reinforcing sheet is omitted here.
[0081] The fiber sheet, which is a reinforcing base material, is a sheet composed of reinforcing fibers. The reinforcing fibers are not particularly limited as long as they increase the shape stability and strength of the reinforcing fiber sheet. For example, glass fibers, polyvinyl alcohol fibers such as vinylon fibers, polyester fibers, nylon, polyamide fibers such as aramid (aromatic polyamide), carbon fibers, or polyparaphenylene benzoxazole fibers can be used. A preferred example of the fiber sheet is one in which nylon fibers are woven into a sheet. These fibers may be used alone or in combination. The fiber sheet is not limited in shape as long as it is in the form of a sheet, and may be a woven fabric or a nonwoven fabric.
[0082] In the rubber-reinforcing sheet of this embodiment, the detailed description of the configuration other than the coating, such as the shape of the rubber-reinforcing sheet and specific examples of the fiber sheet, may be the same as that disclosed in, for example, JP-A-2006-144932. Therefore, detailed description of the configuration other than the coating, such as the fiber sheet, is omitted here.
[0083] [Method of manufacturing rubber reinforcing members] An example of a method for producing the rubber reinforcing member of this embodiment (hereinafter, referred to as the production method of this embodiment) is described below. The matters described for the aqueous treatment agent of the first embodiment and the rubber reinforcing member, rubber reinforcing cord, and rubber reinforcing sheet of this embodiment can be applied to the production method below, so duplicated explanations may be omitted. In addition, the matters described for the production method of this embodiment below can be applied to the aqueous treatment agent of the first embodiment and the rubber reinforcing member, rubber reinforcing cord, and rubber reinforcing sheet of this embodiment.
[0084] The manufacturing method of this embodiment is as follows: (a) supplying a treatment agent to at least a portion of a surface of a reinforcing substrate and drying the treatment agent to form a coating on the surface of the reinforcing substrate; The treatment agent is the aqueous treatment agent of the first embodiment.
[0085] In the manufacturing method of the present embodiment, when a filament bundle is used as the reinforcing base material, a rubber reinforcing cord can be manufactured by the manufacturing method of the present embodiment. For example, when the reinforcing fiber is a filament bundle in the manufacturing method of the present embodiment, the manufacturing method of the present embodiment can be, for example, (b) bundling a plurality of filaments to form at least one said filament bundle; In the above (a), an aqueous treatment agent is supplied to at least a portion of the surface of the filament bundle, and then dried to produce a strand having a coating formed on the surface of the filament bundle.
[0086] When a rubber-reinforcing cord is manufactured by the manufacturing method of this embodiment, the manufacturing method of this embodiment includes bundling a plurality of filaments to prepare at least one filament bundle, and supplying a treatment agent to at least a part of the surface of the filament bundle and drying the bundle to prepare a strand having a coating formed on the surface of the filament bundle. The treatment agent is the aqueous treatment agent of the first embodiment.
[0087] By the above method, a coating is formed on at least a part of the surface of the reinforcing substrate. The method of supplying the aqueous treatment agent to at least a part of the surface of the reinforcing substrate is not limited, and for example, the aqueous treatment agent may be applied to the surface of the reinforcing substrate, or the reinforcing substrate may be immersed in the aqueous treatment agent.
[0088] The drying conditions, that is, the conditions of the heat treatment for removing the solvent of the aqueous treatment agent, are not particularly limited. For example, drying may be performed in an atmosphere of 80° C. to 280° C. for 0.1 to 2 minutes.
[0089] The aqueous treatment agent is preferably supplied to at least a part of the surface of the reinforcing substrate so that the mass of the coating is 5% by mass or more and 35% by mass or less with respect to the mass of the reinforcing substrate. The aqueous treatment agent may be supplied to at least a part of the surface of the reinforcing substrate so that the mass of the coating is 10% by mass or more with respect to the mass of the reinforcing substrate. The aqueous treatment agent may be supplied to at least a part of the surface of the reinforcing substrate so that the mass of the coating is 25% by mass or less, or 20% by mass or less with respect to the mass of the reinforcing substrate. The aqueous treatment agent may be supplied to at least a part of the surface of the reinforcing substrate so that the mass of the coating is 10% by mass or more and 20% by mass or less with respect to the mass of the reinforcing substrate.
[0090] When a rubber reinforcing cord is manufactured by the manufacturing method of this embodiment, that is, when a filament bundle is used as a reinforcing base material, the filament bundle on which the coating is formed may be twisted in one direction. The twisting direction may be the S direction or the Z direction. The number of filaments contained in the filament bundle and the number of twists of the filament bundle have been described above, so explanations are omitted. In this manner, the rubber reinforcing cord of this embodiment can be manufactured. Note that a plurality of filament bundles on which the coating is formed may be formed, and the plurality of filament bundles may be bundled and then subjected to a final twist. The direction of the final twist may be the same as or different from the twist direction of the filament bundle (the direction of the primary twist). Also, a plurality of filament bundles on which the coating is formed may be formed, and the filament bundles may not be twisted individually, but the bundle of the plurality of filament bundles may be twisted.
[0091] The filament bundle may be twisted before forming the coating, with the type, number and twist number of the filaments being as described above.
[0092] A plurality of strands manufactured as described above may be prepared and twisted together. That is, the manufacturing method of the present embodiment may further include twisting together the plurality of strands.
[0093] In a preferred example of the manufacturing method of this embodiment, a filament bundle is coated with or impregnated with an aqueous treatment agent, and then the bundle is twisted in one direction to form a rubber reinforcing cord.
[0094] When a rubber reinforcing sheet is manufactured by the manufacturing method of this embodiment, i.e., when a fiber sheet is used as the reinforcing base material, one example of a method for manufacturing a rubber reinforcing member of this embodiment is to form a coating on the fiber sheet by supplying the reinforcing base material to a fiber sheet in the above (a) and drying the aqueous treatment agent to at least a portion of the surface of the fiber sheet.
[0095] The method for supplying the aqueous treatment agent to the fiber sheet is not particularly limited, and for example, the fiber sheet can be immersed in a bath containing the aqueous treatment agent, and after it is pulled out, the coating can be formed by removing the solvent through a drying oven. Furthermore, the method for producing a rubber-reinforcement sheet of this embodiment can be applied to the method for producing a rubber-reinforcement sheet disclosed in, for example, JP-A-2006-144932, except for the description of the components of the aqueous treatment agent.
[0096] [Rubber products] The rubber product of this embodiment includes a matrix rubber and the above-mentioned rubber reinforcing member of this embodiment. In other words, the rubber product of this embodiment is a rubber product reinforced with at least one reinforcing member selected from the group consisting of the rubber reinforcing cord of this embodiment and the rubber reinforcing sheet of this embodiment. The rubber product is not particularly limited. Examples of the rubber product of this embodiment include automobile and bicycle tires and transmission belts. Examples of the transmission belt include meshing transmission belts and friction transmission belts. Examples of the meshing transmission belt include toothed belts such as automotive timing belts. Examples of the friction transmission belt include flat belts, round belts, V-belts, V-ribbed belts, etc. That is, the rubber product of this embodiment may be a toothed belt, flat belt, round belt, V-belt, or V-ribbed belt. The rubber product of this embodiment may be a hose for household use, industrial use, automotive use, agricultural use, etc.
[0097] The rubber product of this embodiment may be formed, for example, by embedding the rubber reinforcing cord of this embodiment in a rubber composition (matrix rubber). That is, an example of the rubber product of this embodiment includes, for example, a matrix rubber and a rubber reinforcing cord embedded in the matrix rubber. The method of embedding the rubber reinforcing cord in the matrix rubber is not particularly limited, and a known method may be applied. For example, the rubber reinforcing cord of this embodiment is embedded in the rubber product of this embodiment (for example, a rubber belt). Therefore, the rubber product of this embodiment has excellent adhesion in which the matrix rubber and the rubber reinforcing cord are firmly bonded to each other, and can achieve high mechanical strength. The rubber product of this embodiment is particularly suitable for applications such as a timing belt for a vehicle engine and a belt for driving an accessory for a vehicle.
[0098] The rubber product of this embodiment may have a configuration in which the rubber reinforcing sheet of this embodiment is embedded inside the rubber main body portion (a component formed of matrix rubber) of the rubber product, or may have a configuration in which it is arranged so as to cover the surface of the rubber main body portion.
[0099] The matrix rubber in the rubber product of this embodiment includes, for example, EPDM. The rubber reinforcing member constituting the rubber product of this embodiment has excellent adhesion to matrix rubber including EPDM. In addition, EPDM is excellent in heat resistance, weather resistance, ozone resistance, etc. Therefore, according to this configuration, a rubber product having high strength and excellent flex resistance, and excellent heat resistance, weather resistance, ozone resistance, etc. can be realized.
[0100] The matrix rubber in the rubber product of the present embodiment may contain another rubber component other than EPDM. For example, it may contain chloroprene rubber, CSM rubber, hydrogenated nitrile rubber, carboxyl-modified nitrile rubber, carboxyl-modified hydrogenated nitrile rubber, natural rubber, styrene-butadiene rubber (i.e., styrene-butadiene copolymer), etc. The hydrogenated nitrile rubber may be hydrogenated nitrile rubber in which a zinc acrylate derivative (e.g., zinc methacrylate) is dispersed.
[0101] In the rubber product of the present embodiment, the coating of the rubber reinforcing member and the matrix rubber may be in contact with each other.
[0102] As an example of a rubber product, a toothed belt is shown in Fig. 1A. The toothed belt 10 shown in Fig. 1A includes a belt body 11 and a plurality of rubber reinforcing cords 12. The belt body 11 includes a belt portion 13 and a plurality of tooth portions 14 protruding from the belt portion 13 at regular intervals. The rubber reinforcing cord 12 is embedded inside the belt portion 13 so as to be parallel to the longitudinal direction of the belt portion 13. The rubber reinforcing cord 12 is the rubber reinforcing cord of this embodiment.
[0103] FIG. 1B shows a toothed belt as another example of a rubber product. The toothed belt 20 shown in FIG. 1B includes a belt body 21 and a rubber reinforcing sheet 22. The belt body 21 includes a belt portion 23 and a plurality of tooth portions 24 protruding from the belt portion 23 at regular intervals. The rubber reinforcing sheet 22 is arranged so as to cover the surface of the belt body 21 on the side on which the tooth portions 24 are formed. As shown in FIG. 1B, for example, a rubber reinforcing cord 25 may be embedded inside the belt portion 23. The rubber reinforcing sheet 22 is the rubber reinforcing sheet of this embodiment. The rubber reinforcing cord 25 is the rubber reinforcing cord of this embodiment. As a rubber reinforcing member in the toothed belt 20, only the rubber reinforcing sheet 22 may be provided. EXAMPLES
[0104] Hereinafter, the embodiments of the present invention will be described more specifically with reference to examples and comparative examples.
[0105] [Manufacture of rubber reinforcing cords] A glass fiber (filament bundle) was prepared by bundling 200 glass filaments (E glass composition, average diameter 9 μm). Three of these glass fibers were aligned, and an aqueous treatment agent having components as shown in Tables 1 to 3 below was applied to them. After that, the fibers were dried for 1 minute in a drying oven set at 150° C. Thus, a strand was formed.
[0106] The formed strand had a cross section as shown in FIG. 2. That is, a coating 32 was provided so as to cover the surface of three bundles of glass fibers 31 made of a large number of glass filaments, and a strand 30 was formed. The three glass fibers 31 were bonded to each other by the coating 32. The strand thus obtained was pre-twisted at a rate of 2 times / 25 mm. Then, 11 of the pre-twisted strands were aligned and top-twisted at a rate of 2 times / 25 mm. In this way, a rubber reinforcing cord 40 having a cross section as shown in FIG. 3 was obtained. The ratio of the coating to the obtained cord was 20% by mass. The mass of the coating relative to the mass of the filament bundle was a value obtained by a method of ignition loss by heating at 650±20°C. In this way, the reinforcing cords of Examples 1 to 7 and Comparative Examples 1 to 9 were obtained.
[0107] [Adhesion evaluation (adhesion strength with matrix rubber and fracture morphology)] Two rubber pieces (width 25 mm × length 50 mm × thickness 5 mm) having the composition shown in Table 4 were prepared. Next, a plurality of rubber reinforcing cords were arranged so that there were no gaps between the rubber reinforcing cords, and sandwiched between the two rubber pieces, so that the rubber reinforcing cords were parallel to the longitudinal direction of the rubber pieces. In this embodiment and the comparative example, about 30 rubber reinforcing cords were arranged in parallel on a rubber piece having a width of 25 mm. The rubber reinforcing cord sandwiched between the two rubber pieces was heated at 165°C for 30 minutes to bond the rubber piece and the rubber reinforcing cord. The adhesiveness between the rubber reinforcing cord and the matrix rubber (i.e., the rubber piece) of the test piece obtained in this way was evaluated by a 180-degree peel test. Specifically, a tensile tester was used, one of the rubber pieces of the test piece was held by one chuck of the tensile tester, and the other chuck was held by the other rubber piece of the test piece and the multiple rubber reinforcing cords arranged in parallel, and the test piece was pulled in the longitudinal direction so that the peeling direction was 180 degrees to the adhesive surface. The pulling speed was set to 50 mm / min. The measured peel strength between the matrix rubber and the rubber reinforcing cord of each Example and Comparative Example was taken as the adhesive strength. The peel strength was taken as the average value calculated from the maximum and minimum values of the peel force (the maximum and minimum values were added and divided by 2).
[0108] The failure mode of the test specimens was evaluated on a 6-point scale, with "5" being "complete rubber failure," where the failure occurred while the rubber reinforcing cord and the matrix rubber remained bonded, leaving the matrix rubber completely on the rubber reinforcing cord, and "0" being "interface delamination," where delamination occurred at the interface between the matrix rubber and the rubber reinforcing cord. "4" was a condition in which rubber remained on 75% of the surface area of the rubber reinforcing cord, "3" was a condition in which rubber remained on 50% of the surface area of the rubber reinforcing cord, and "2" was a condition in which rubber remained on 25% of the surface area of the rubber reinforcing cord.
[0109] Here, the ratio of the area of the matrix rubber remaining in the surface area of the rubber reinforcing cord was obtained using a photographic printed image of the surface of the rubber reinforcing cord. Specifically, a photograph was first taken so that the entire peeled interface of the test piece was included, and the entire test piece was cut out from the printed image of the photograph, and the weight W of the printed image of the entire cut-out test piece was measured. Next, the rubber portion was cut out from the printed image of the entire test piece, and the total weight w of the cut-out rubber portion was measured. From the obtained values of weights W and w, the proportion of the remaining rubber ((w / W) x 100%) was calculated.
[0110] The results of the adhesiveness evaluation of the rubber-reinforcing cords of each Example and Comparative Example are shown in Tables 1 to 3. In Table 1, Example 2 is compared with Comparative Examples 1 and 3 to 6 for the purpose of making it easier to understand the effects of the aqueous treatment agent and rubber-reinforcing cord of the present invention. Table 2 shows Examples 1 to 7, and Table 3 shows Comparative Examples 1 to 9.
[0111] [Flexibility evaluation] Two rubber pieces (width 10 mm × length 500 mm × thickness 3 mm) made of the composition shown in Table 4 were prepared. Next, one rubber reinforcing cord was placed in the center of the rubber pieces so that the rubber reinforcing cord was parallel to the longitudinal direction of the rubber pieces, and the rubber pieces were sandwiched between the two rubber pieces. The rubber reinforcing cord sandwiched between the two rubber pieces was heated at 165°C for 30 minutes to bond the rubber pieces and the rubber reinforcing cord. The test piece thus obtained was used as a test piece for evaluating bending resistance.
[0112] A bending test was conducted on each test piece by bending it 50,000 times. The bending test was conducted using a bending tester 50 shown in FIG. 4. The tensile strength of each test piece was measured before and after the bending test. Here, the tensile strength was measured using a commonly used tensile tester and a commonly used cord grip, and the breaking strength (unit: N / cord) obtained at that time was used.
[0113] The bending tester 50 was equipped with one flat pulley 51 with a diameter of 10 mm, a motor (not shown), and four guide pulleys 52. First, the prepared test piece 53 was hung on the five pulleys. Then, a weight was attached to one end 53a of the test piece 53, and a load of 20 N was applied to the test piece 53. In this state, the other end 53b of the test piece 53 was reciprocated 50,000 times in the direction of the arrow shown in FIG. 4, so that the test piece 53 was repeatedly bent at the flat pulley 51. The bending test was carried out at room temperature. After the bending test of the test piece 53 was carried out in this manner, the tensile strength of the test piece 53 after the bending test was measured.
[0114] The tensile strength of the test piece after the bending test was determined as a percentage of the tensile strength of the test piece before the bending test, i.e., strength retention (%). The higher the strength retention value, the better the bending resistance. The evaluation results of the bending resistance of the rubber reinforcing cords of each Example and Comparative Example are shown in Tables 1 to 3.
[0115] [Table 1]
[0116] [Table 2]
[0117] [Table 3]
[0118] [Table 4]
[0119] As shown in Table 1, the rubber reinforcing cord of Example 1, in which a coating was formed using the aqueous treatment agent of the present invention, that is, the aqueous treatment agent containing a resorcinol-formaldehyde condensate and a rubber latex containing an ethylene-glycidyl methacrylate copolymer and CSM as rubber components, had excellent adhesion to EPDM rubber and also excellent flex resistance. In contrast, the rubber reinforcing cord of Comparative Example 1, in which the rubber component was only an ethylene-glycidyl methacrylate copolymer, was able to have excellent adhesion to EPDM rubber but had poor flex resistance. In addition, the rubber reinforcing cords of Comparative Examples 3 to 6, in which an aqueous treatment agent containing an ethylene-glycidyl methacrylate copolymer and a rubber component other than CSM was used, had improved flex resistance but poor adhesion despite containing an ethylene-glycidyl methacrylate copolymer. A comparison between Example 1 and Comparative Examples 3 to 6 shows that a coating with an excellent balance between adhesion and flex resistance can be produced by combining an ethylene-glycidyl methacrylate copolymer with CSM.
[0120] From the results shown in Table 2, the rubber-reinforcing cords of Examples 1 to 5, in which the content of ethylene-glycidyl methacrylate copolymer was 15% by mass or more and 95% by mass or less and the content of CSM was 5% by mass or more and 85% by mass or less, had excellent adhesion to EPDM rubber while also having better flex resistance. That is, it is found that the rubber-reinforcing cords of Examples 1 to 5 can form a coating with an excellent balance between adhesion and flex resistance.
[0121] From the results shown in Table 3, the rubber-reinforcing cord of Comparative Example 2, which contained only CSM as the rubber component, had improved flex resistance but poor adhesion to the matrix rubber. Also, the rubber-reinforcing cords of Comparative Examples 7 to 9, which used an aqueous treatment agent containing CSM and a rubber component other than ethylene-glycidyl methacrylate copolymer, had very good flex resistance but very poor adhesion. [Industrial Applicability]
[0122] The present invention can be used in a rubber reinforcing member for reinforcing a rubber product. [Explanation of symbols]
[0123] 10, 20 Toothed belt 11, 21 Belt body 12, 25 Rubber reinforcement cord 13, 23 Belt section 14, 24 teeth 22 Rubber Reinforcement Sheet 30 Strands 31 Glass fiber 32 Coating 40 Rubber Reinforcement Cord 50 Bending test machine 51 Flat pulley 52 Guide pulley 53 Test Pieces
Claims
1. An aqueous treatment agent for producing a coating on a rubber-reinforcing member having a coating, comprising: The aqueous treatment agent is resorcinol-formaldehyde condensate; Rubber latex and Including, The rubber latex contains, as a rubber component, an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene. Water-based treatment agent.
2. In the rubber component of the rubber latex, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 95% by mass or less, The content of chlorosulfonated polyethylene is 5% by mass or more and 85% by mass or less. The aqueous treatment agent according to claim 1.
3. In the rubber component of the rubber latex, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 70% by mass or less, The content of chlorosulfonated polyethylene is 30% by mass or more and 85% by mass or less; The aqueous treatment agent according to claim 2.
4. In the rubber component of the rubber latex, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 50% by mass or less, The content of chlorosulfonated polyethylene is 50% by mass or more and 85% by mass or less. The aqueous treatment agent according to claim 3.
5. In the rubber component of the rubber latex, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 40% by mass or less, The content of chlorosulfonated polyethylene is 60% by mass or more and 85% by mass or less. The aqueous treatment agent according to claim 4.
6. In the rubber component of the rubber latex, the content ratio of chlorosulfonated polyethylene is equal to or greater than the content ratio of ethylene-glycidyl methacrylate copolymer, by mass ratio. The aqueous treatment agent according to claim 1.
7. (a) supplying the aqueous treatment agent according to any one of claims 1 to 6 to at least a part of a surface of a reinforcing substrate and drying the aqueous treatment agent to form a coating on the surface of the reinforcing substrate; A method for producing a rubber reinforcing member, comprising the steps of:
8. The reinforcing substrate is a filament bundle, The manufacturing method includes: (b) bundling a plurality of filaments to form at least one said filament bundle; Further comprising: In the step (a), the aqueous treatment agent is supplied to at least a part of the surface of the filament bundle, and then dried to produce a strand having the coating formed on the surface of the filament bundle. The method for producing the rubber reinforcing member according to claim 7.
9. The reinforcing base material is a fiber sheet, In the step (a), the aqueous treatment agent is supplied to at least a part of the surface of the fiber sheet, and then dried to form the coating on the fiber sheet. The method for producing the rubber reinforcing member according to claim 7.
10. A rubber reinforcing member for reinforcing a rubber product, The rubber reinforcing member is A reinforcing base material; A coating provided so as to cover at least a portion of the surface of the reinforcing base material; Including, The coating contains a resorcinol-formaldehyde condensate and a rubber component, The rubber component contains an ethylene-glycidyl methacrylate copolymer and a chlorosulfonated polyethylene. Rubber reinforcing material.
11. In the rubber component of the coating, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 95% by mass or less, The content of chlorosulfonated polyethylene is 5% by mass or more and 85% by mass or less. The rubber reinforcing member according to claim 10.
12. In the rubber component of the coating, The content of ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 70% by mass or less, The content of chlorosulfonated polyethylene is 30% by mass or more and 85% by mass or less; The rubber reinforcing member according to claim 11.
13. In the rubber component of the coating, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 50% by mass or less, The content of chlorosulfonated polyethylene is 50% by mass or more and 85% by mass or less. The rubber reinforcing member according to claim 12.
14. In the rubber component of the coating, The content ratio of the ethylene-glycidyl methacrylate copolymer is 15% by mass or more and 40% by mass or less, The content of chlorosulfonated polyethylene is 60% by mass or more and 85% by mass or less. The rubber reinforcing member according to claim 13.
15. In the coating, the content of chlorosulfonated polyethylene is equal to or greater than the content of ethylene-glycidyl methacrylate copolymer, by mass ratio. The rubber reinforcing member according to claim 10.
16. The coating is provided on the outermost surface of the rubber reinforcing member. The rubber reinforcing member according to claim 10.
17. Matrix rubber; A rubber reinforcing member according to any one of claims 10 to 16, Rubber products including.
18. The matrix rubber includes ethylene propylene diene rubber. The rubber product according to claim 17.
19. The coating of the rubber reinforcing member and the matrix rubber are in contact with each other. The rubber product according to claim 17.
Citation Information
Patent Citations
Fiber-reinforced rubber composite
JP1987131035A
Cooling device for engine
JP1993086968A
Treating process for bonding rubber composition and textile material
JP2001040105A
Coating liquid for glass fiber and rubber-reinforcing glass fiber using the same
JP2007197553A
Coating liquid for coating fiber and rubber-reinforcing fiber using the same
JP2008002050A
Cited By
Treatment agent, rubber-reinforcing member obtained using same, rubber product, and method for producing rubber-reinforcing member
WO2026230447A1