Ferrite particle, carrier core material for electrophotographic developer, carrier for electrophotographic developer, and electrophotographic developer
Ferrite particles with a controlled Sr or Ca composition gradient and resin coating address charge distribution issues in electrophotographic developers, ensuring stable image quality and reduced toner scattering.
Patent Information
- Application Number
- JP2023052502
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- 2043-03-29
AI Technical Summary
Existing electrophotographic developers face issues with charge amount distribution variability, leading to toner scattering and poor image density due to wear and peeling of resin coating layers, affecting long-term performance and image quality.
Ferrite particles with a controlled composition gradient of Sr or Ca based on particle size, combined with a resin coating layer, to achieve a sharp charge amount distribution and improved charge imparting ability.
The solution provides a high charge imparting ability with a sharp charge amount distribution, reducing toner scattering and maintaining good image quality over time, even under varying environmental conditions.
Smart Images

Figure 2024141060000001 
Figure 2024141060000002
Abstract
Description
[Technical field]
[0001] The present invention relates to ferrite particles, a carrier core material for an electrophotographic developer, a carrier for an electrophotographic developer, and an electrophotographic developer. [Background technology]
[0002] The electrophotographic development method is a method of developing an electrostatic latent image formed on a photoreceptor by attaching toner particles in a developer to the electrostatic latent image formed on the photoreceptor, and the developer used in this method is divided into a two-component developer consisting of toner particles and carrier particles, and a one-component developer using only toner particles. Among these developers, the magnetic brush method using a magnet roll is the mainstream development method using a two-component developer consisting of toner particles and carrier particles.
[0003] In two-component developers, the carrier particles are a carrier material that imparts a desired charge to the toner particles by being stirred together with the toner particles in a developing box filled with the developer, and then transports the charged toner particles to the surface of a photoreceptor to form a toner image on the photoreceptor. The carrier particles remaining on the developing roll that holds the magnet are returned from the developing roll to the developing box again, where they are mixed and stirred with new toner particles, and are used repeatedly for a certain period of time.
[0004] Unlike one-component developers, two-component developers have carrier particles that are mixed and stirred with toner particles, charge the toner particles, and transport them, allowing for good controllability when designing developers. Therefore, two-component developers are suitable for full-color developing devices that require high image quality, and high-speed printing devices that require reliability and durability in maintaining images.
[0005] Thus, during long-term use, the carrier particles must always triboelectrically charge the toner particles to the desired polarity and with a sufficient charge amount. However, when the distribution of the charge amount of the toner is wide, toner scattering caused by low-charged toner and image density defects caused by high-charged toner are likely to occur. That is, it is required that the carrier particles not only have the ability to charge the toner but also can control the charge amount distribution to be narrower.
[0006] In Patent Document 1, ferrite particles having excellent toner charge rise property and high charge stability are proposed by locally providing large convex portions on the surface of the ferrite particles serving as carrier particles. Specifically, Patent Document 1 discloses ferrite particles having a composition formula of M X Fe 3-X O4 (where M is at least one metal selected from the group consisting of Mg, Mn, Ca, Ti, Cu, Zn, Ni, 0 < X < 1), characterized in that the maximum height Rz of the particles is greater than 2.2 μm, and the average length RSm of the particles is greater than 19 μm and less than 26 μm.
[0007] In Patent Document 2, carriers having a sharp charge amount distribution are proposed by providing appropriate irregularities on the resin coating layer of the carrier coated with resin. Specifically, Patent Document 2 discloses an electrostatic charge image developing carrier having a coating film composed of at least a binder resin and fine particles, wherein the particle diameter (D) and the binder resin film thickness (h) satisfy 1 < [D / h] < 10, and the magnetization of the carrier at 1 kOe is in the range of 40 to 80 emu / g.
Prior Art Documents
Patent Documents
[0008]
Patent Document 1
Patent Document 2
Summary of the Invention
[0009] However, in the techniques described in Patent Documents 1 and 2, the charge distribution taking into account the particle size distribution of the carrier is not necessarily sufficiently examined, and the charge distribution is not sufficiently sharp. In particular, in a carrier having a resin coating layer on its surface, the resin coating layer may wear and peel off due to long-term use in a developing tank, exposing the carrier core material, and the charge imparting ability and charge distribution of the carrier core material become more influential, making it difficult to control the charge of the toner, and making it more likely to cause poor image density and toner scattering.
[0010] Therefore, an object of the present invention is to provide a carrier core material for an electrophotographic developer which has high charge-imparting ability and a sharp charge distribution, and therefore is less likely to cause poor image density or toner scattering, and which can provide good image quality even when used as a developer over a long period of time; a carrier for an electrophotographic developer formed by coating the surface of the carrier core material for an electrophotographic developer with a resin; and ferrite particles which become an electrophotographic developer using the carrier for an electrophotographic developer. [Means for solving the problem]
[0011] As a result of extensive research aimed at solving the above-mentioned problems, the inventors have discovered that when the proportion of Sr or Ca on the surface of a particle with a relatively small particle size and the proportion of Sr or Ca on the surface of a particle with a relatively large particle size satisfy certain conditions, ferrite particles can be obtained that provide a carrier core material for an electrophotographic developer with the desired charge-imparting ability and a sharp charge amount distribution.
[0012] That is, in the present invention, when the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 35 μm or less is X (atomic %) and the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 40 μm or more is Y (atomic %), the following formula: 1.10≦Y / X To provide ferrite particles which satisfy the above requirements.
[0013] In the ferrite particles according to the present invention, the ferrite particles are formed by the following formula: 0.30≦X≦0.80 0.36≦Y≦1.55 1.20≦Y / X≦2.00 It is preferable that the following is satisfied.
[0014] In the ferrite particles according to the present invention, it is preferable that the cumulative 50% particle diameter D50 in the volumetric particle size distribution is 30 μm or more and 50 μm or less, and the proportion of particles having a particle diameter of 40 μm or more in the number-based particle size distribution is 5% by number or more and 40% by number or less.
[0015] In the ferrite particles according to the present invention, it is preferable that the surface roughness Rz is 2.5 μm or more and 4.5 μm or less, and the standard deviation Rzσ of the surface roughness Rz is 0.2 μm or more and 1.0 μm or less.
[0016] The ferrite particles according to the present invention preferably contain 0.3 to 1.2% by weight of Sr or Ca, and more preferably contain 15 to 30% by weight of Mn and 45 to 65% by weight of Fe.
[0017] In the ferrite particles according to the present invention, the residual magnetization σr is 3.0 Am 2 It is preferable that the concentration is less than 1 / kg.
[0018] The present invention also provides a carrier core material for an electrophotographic developer, which contains the above-mentioned ferrite particles.
[0019] The present invention also provides a carrier for an electrophotographic developer, comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles.
[0020] The present invention also provides an electrophotographic developer comprising the above-mentioned carrier for electrophotographic developer and a toner. The electrophotographic developer according to the present invention is preferably used as a refill developer. Effect of the Invention
[0021] According to the present invention, it is possible to provide a carrier core material for an electrophotographic developer which has high charge-imparting ability and a sharp charge distribution, and therefore is less likely to cause poor image density or toner scattering, and which can provide good image quality even when used as a developer over a long period of time; a carrier for an electrophotographic developer formed by coating the surface of the carrier core material for an electrophotographic developer with a resin; and ferrite particles which become an electrophotographic developer using the carrier for an electrophotographic developer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Hereinafter, embodiments of the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer according to the present invention will be described. In this specification, the ferrite particles, the carrier core material for electrophotographic developer, the carrier for electrophotographic developer, and the electrophotographic developer each mean an aggregate of individual particles, that is, a powder, unless otherwise specified.
[0023] 1. Ferrite particles and carrier core material for electrophotographic developers First, the embodiment of the ferrite particles according to the present invention will be described. In the following, the ferrite particles according to the present invention will be described as being mainly used as a carrier core material for electrophotographic developer. However, the ferrite particles according to the present invention can be used for various applications such as magnetic ink, magnetic fluid, magnetic filler, filler for bonded magnet, and various functional fillers such as filler for electromagnetic wave shielding material, electronic component materials, etc., and the application of the ferrite particles is not limited to the carrier core material for electrophotographic developer.
[0024] (1) Components The ferrite particles according to the present invention are represented by MO·Fe2O3 (M: divalent metal element), and usually contain Fe as a main metal component, and are preferably composed of one or two components selected from Mn and Mg. These main metal components exist as a solid solution in a spinel structure. The ferrite particles according to the present invention preferably contain at least Fe and Mn as main metal components, and are preferably composed of Fe, Mn, and Mg as main metal components.
[0025] In the ferrite particles according to the present invention, the Fe content is preferably 45% by weight or more and 65% by weight or less. If the Fe content is within this range, it is easy to adjust the magnetization and resistance to the desired levels. The Fe content is more preferably 47% by weight or more, and even more preferably 48% by weight or more. Moreover, the Fe content is more preferably 60% by weight or less, and even more preferably 55% by weight or less.
[0026] In the ferrite particles according to the present invention, the Mn content is preferably 15% by weight or more and 30% by weight or less. If the Mn content is within this range, it is easy to adjust the magnetization and resistance to the desired levels. The Mn content is more preferably 16% by weight or more, and even more preferably 17% by weight or more. Moreover, the Mn content is more preferably 25% by weight or less, and even more preferably 22% by weight or less.
[0027] In the ferrite particles according to the present invention, the Mg content is preferably 0.5% by weight or more and 10% by weight or less. If the Mg content is within this range, it is easy to adjust the magnetization and resistance to the desired levels. The Mg content is more preferably 1.0% by weight or more, and even more preferably 1.5% by weight or more. Moreover, the Mg content is more preferably 5.0% by weight or less, and even more preferably 3.0% by weight or less.
[0028] It is also important that the ferrite particles according to the present invention contain Sr or Ca as a minor component. The content of Sr or Ca in the ferrite particles according to the present invention is preferably 0.3% by weight or more and 1.2% by weight or less. By making the content of Sr or Ca 0.3% by weight or more, the ability of the carrier for electrophotographic developer to impart charge to the toner is enhanced. By making the content of Sr or Ca 1.2% by weight or less, the carrier is less susceptible to the influence of environments such as high temperature and high humidity, and the environmental dependency of the charge amount is improved. The content of Sr or Ca is more preferably 0.4% by weight or more, and even more preferably 0.5% by weight or more. The content of Sr or Ca is more preferably 0.9% by weight or less, and even more preferably 0.8% by weight or less. The ferrite particles according to the present invention may contain either Sr or Ca, or may contain both Sr and Ca. When both Sr and Ca are contained, the above content is the total content of Sr and Ca.
[0029] (2) Ratio of Sr or Ca according to particle size Here, the ability to impart charge to the toner is determined by frictional charging between the electrophotographic developer carrier and the toner, and is therefore greatly affected by the particle size and specific surface area of the electrophotographic developer carrier (ferrite particles). In general, there is a strong correlation between the particle size and specific surface area of the particles, and the larger the particle size, the smaller the specific surface area. Therefore, electrophotographic developer carriers with larger particle sizes have a relatively weaker ability to impart charge than electrophotographic developer carriers with smaller particle sizes. In other words, it is considered that the particle size distribution causes variation in the ability of the electrophotographic developer carrier to impart charge to the toner, resulting in a wide distribution of charge in the toner.
[0030] On the other hand, if the particle size distribution of the carrier for electrophotographic developer is made too sharp, the amount of toner that enters the gaps between the particles increases relatively, which reduces the frequency of contact with the toner, and this can lead to a decrease in the charge amount and a widening of the charge amount distribution, as well as a significant decrease in production yield.
[0031] Therefore, in the present invention, when Sr or Ca, which is known to increase the ability to impart charge to toner, is added to the ferrite particles, a gradient in composition (particularly the ratio of Sr or Ca) according to the particle size of the ferrite particles is provided, thereby reducing the variation in the ability to impart charge due to the particle size and making the charge distribution sharp. In other words, it is important to set the ratio of Sr or Ca on the surface of a particle with a relatively large particle size higher than the ratio of Sr or Ca on the surface of a particle with a relatively small particle size.
[0032] More specifically, in the present invention, when the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 35 μm or less is X (atomic %) and the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 40 μm or more is Y (atomic %), the following formula is satisfied: 1.10≦Y / X It is important to satisfy the following. If Y / X is less than 1.10, the charge imparting ability to the toner varies widely and the charge distribution becomes broad, which makes it easier for toner scattering and insufficient image density to occur. Y / X is preferably 1.20 or more, and more preferably 1.25 or more. However, if Y / X is too large, the charge imparting ability to the toner is more likely to vary, so Y / X is preferably 2.50 or less, more preferably 2.00 or less, and even more preferably 1.75 or less.
[0033] The proportion X (atomic %) of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 35 μm or less is calculated by the following formula: 0.30≦X≦0.80 It is preferable that the above is satisfied. By making X 0.30 or more, sufficient charge-imparting ability can be obtained. Furthermore, by making X 0.80 or less, the toner is less susceptible to environmental influences such as high temperature and high humidity, and the environmental dependency of the charge amount is improved. It is more preferable that X is 0.35 or more, and even more preferable that X is 0.40 or more. Furthermore, it is more preferable that X is 0.70 or less, and even more preferable that X is 0.65 or less.
[0034] The ratio Y (atomic %) of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 40 μm or more is calculated by the following formula: 0.36≦Y≦1.55 It is preferable that the above is satisfied. By making Y 0.36 or more, sufficient charge-imparting ability can be obtained. Furthermore, by making Y 1.55 or less, the toner is less susceptible to environmental influences such as high temperature and high humidity, and the environmental dependency of the charge amount is improved. It is more preferable that Y is 0.45 or more, and even more preferable that Y is 0.60 or more. Furthermore, it is more preferable that Y is 1.15 or less, and even more preferable that Y is 0.95 or less.
[0035] The proportion of Sr or Ca in element mapping of the particle surface can be measured by energy dispersive X-ray analysis (EDX analysis). In EDX analysis, the content of elements at a depth of about several μm in the ferrite particle can be measured. A specific measurement method will be described in the examples below.
[0036] (3) Particle size distribution In the ferrite particles according to the present invention, the volume cumulative 50% particle diameter D50 in the volume-based particle size distribution is preferably 30 μm or more and 50 μm or less. By making D50 30 μm or more, adhesion of the carrier for electrophotographic developer is less likely to occur, and by making D50 50 μm or less, the particle diameter becomes appropriate for the toner, improving the charging ability. D50 is more preferably 33 μm or more. Also, D50 is more preferably 45 μm or less, and even more preferably 42 μm or less.
[0037] In the ferrite particles according to the present invention, the ratio D of particles having a particle diameter of 62 μm or more in the particle size distribution based on volume +62 is preferably 12% by volume or less, and more preferably 10% by volume or less. +62 By making the ratio D of particles having a particle diameter of 22 μm or less in the volumetric particle size distribution to 12% or less, a sharp distribution with few large particles is obtained, so that the toner transport ability is improved and image quality is improved.-22 is preferably 3% by volume or less, and more preferably 1.5% by volume or less. -22 By setting the amount of the toner particles to 3% by volume or less, a sharp distribution with a small number of small particles is achieved, making it difficult for carrier adhesion to occur.
[0038] In addition, in the ferrite particles according to the present invention, the ratio P of particles having a particle diameter of 40 μm or more in the particle size distribution based on the number +40 is preferably 5% by number or more and 40% by number or less. +40 If the amount of the toner particles is within this range, the interparticle voids are appropriately filled without reducing the yield, and the charge imparting property of the toner can be easily adjusted to a desired value. +40 More preferably, the percentage is 8% by number or more. +40 It is more preferable that the number of particles is 20% or less.
[0039] (4) Surface quality In the ferrite particles according to the present invention, the surface roughness Rz is preferably 2.5 μm or more and 4.5 μm or less. By making Rz 2.5 μm or more, the charge imparting ability tends to be increased due to the moderately present unevenness. By making Rz 4.5 μm or less, the decrease in fluidity due to excessive unevenness is suppressed, and the charge imparting ability of the toner is improved by increasing the frequency of contact with the toner. Rz is more preferably 2.8 μm or more. Also, Rz is more preferably 4.0 μm or less.
[0040] In addition, in the ferrite particles according to the present invention, it is preferable that the standard deviation Rzσ of the surface roughness Rz is 0.2 μm or more and 1.0 μm or less. By making Rzσ 0.2 μm or more, it becomes easy to manufacture by a method including sintering by solid-phase reaction. By making Rzσ 1.0 μm or less, when used with a resin coating, exposure of the core material due to variations in the resin coating is unlikely to occur, and carrier adhesion due to charge injection is unlikely to occur. It is more preferable that Rzσ is 0.3 μm or more. It is also more preferable that Rzσ is 0.8 μm or less.
[0041] (5) Magnetization In the ferrite particles according to the present invention, the residual magnetization σr is 3.0 Am 2 / kg. σr is preferably less than 3.0 Am 2 If the toner has a toner particle diameter of less than 2.5 Am / kg, the toner particles are less likely to aggregate due to residual magnetization, and the toner particles are less likely to have a lower chargeability and less likely to have uneven charge distribution. 2 / kg or less. Also, σr is usually 0.5Am 2 / kg or more.
[0042] (6) Manufacturing method The method for producing the ferrite particles according to the present invention is not particularly limited, but it is preferable to produce them by the following method.
[0043] First, the raw materials for producing the ferrite particles according to the present invention are appropriately weighed, and then pulverized and mixed for 0.5 hours or more (preferably 1 to 20 hours) using a ball mill or a vibration mill to obtain a pulverized product. The raw materials are not particularly limited, but are preferably selected so as to have a composition containing the above-mentioned elements. As the raw material for Fe, it is preferable to use Fe2O3. As the raw material for Mn, it is preferable to use one or more compounds selected from Mn3O4 and MnO2. As the raw material for Mg, it is preferable to use one or more compounds selected from Mg(OH)2, MgO, and MgCO3. As the raw material for Sr, it is preferable to use SrCO3. As the raw material for Ca, it is preferable to use CaCO3.
[0044] In the ferrite particles according to the present invention, it is necessary to provide a gradient in composition (particularly the ratio of Sr or Ca) according to the particle size, and this gradient can be adjusted by a method of mixing and firing granulated materials with different compositions and particle sizes. Specifically, a method is exemplified in which two types of blended raw materials having a desired composition ratio are prepared, and in the granulation stage, the particle size of the granulated materials is adjusted by changing the granulation conditions (e.g., atomizer rotation speed, etc.), thereby preparing two types of granulated materials with different particle sizes, and mixing and firing the sintered products so that the D50 of the sintered products becomes the desired particle size.
[0045] The composition gradient according to the particle size can also be adjusted by changing the particle size of the Sr or Ca raw material used. Specifically, there are a method of preparing raw materials with different particle sizes, and a method of pulverizing only the Sr or Ca raw material with a bead mill, etc. The finer the particle size of the raw material, the more likely it is that a solid-phase reaction will occur and precipitate on the particle surface. For example, in the granulation stage, the raw material of the metal that is the main component, such as Fe, Mn, or Mg, is pulverized to a desired particle size, and then the Sr or Ca raw material is added and mixed, thereby making it possible to prepare a slurry in which only Sr or Ca in the raw material has a different particle size.
[0046] Although it is possible to easily precipitate Sr or Ca on the particle surface by increasing the firing temperature, it is difficult to create a gradient in the particle size distribution. In addition, the method of mixing fired materials with different firing temperatures may result in mixing two types of particles with different surface properties or shapes, which may result in the charge distribution not being sharp.
[0047] The pulverized material thus obtained is pelletized using a pressure molding machine or the like, and then pre-fired at a temperature of 700 to 1100°C in the atmosphere. Instead of using a pressure molding machine, water may be added to the pulverized material to form a slurry, which may then be granulated using a spray dryer. After pre-fired, the material is further pulverized using a ball mill or a vibration mill, and then water and, if necessary, a dispersant or binder are added to adjust the viscosity, and the material is granulated and granulated using a spray dryer. When pulverizing after pre-fired, water may be added and pulverized using a wet ball mill or a wet vibration mill.
[0048] The grinding machine such as a ball mill or a vibration mill is not particularly limited, but in order to effectively and uniformly disperse the raw material, it is preferable to use fine beads having a particle size of 1 mm or less as the media used. The degree of grinding can be controlled by adjusting the diameter, composition, and grinding time of the beads used. In order to uniformly disperse the raw material, it is preferable to grind the material so that the volume average particle size (D50) of the ground product is 5 μm or less, more preferably 3.0 μm or less, and even more preferably 2.5 μm or less.
[0049] Next, in order to obtain ferrite powder with a uniform particle size, it is preferable to classify the granulated material before firing to remove fine particles contained in the granulated material. The classification of the granulated material can be performed using a known air classification, a sieve, or the like.
[0050] The classified granules are then fired. The granules are preferably fired after being fired primarily in a firing furnace such as a rotary kiln, which passes the granules (material to be fired) through a hot section while flowing. By performing primary firing in a firing furnace such as a rotary kiln, which passes the granules through a hot section while flowing, organic substances such as binders used during granulation can be removed from the granules in a relatively short time and uniformly, compared to performing primary firing while the granules are placed stationary in a bowl or the like. At the same time, part of the ferrite reaction can be promoted during primary firing, and the occurrence of variations in surface Rz during the subsequent main firing can be suppressed.
[0051] When the primary firing is performed using the above-mentioned type of firing furnace, the temperature is preferably, for example, 750°C or higher and 1050°C or lower. By performing the primary firing in this temperature range, it becomes easier to efficiently remove organic matter and perform the ferrite reaction while suppressing abnormal grain growth and suppressing the occurrence of variations in surface roughness Rz as described above. Furthermore, in order to efficiently remove organic matter and perform the ferrite reaction, it is more preferable to perform the primary firing at a temperature of 800°C or higher, and even more preferable to perform the primary firing at a temperature of 850°C or higher. Furthermore, in order to suppress abnormal grain growth, it is more preferable to perform the primary firing at a temperature of 1000°C or lower, and even more preferable to perform the primary firing at a temperature of 980°C or lower.
[0052] The main firing is preferably performed in an inert atmosphere or a weakly oxidizing atmosphere by holding at a temperature of 1050°C to 1300°C for 4 hours to 24 hours, more preferably 1100°C to 1250°C. Note that, an inert atmosphere or a weakly oxidizing atmosphere refers to an atmosphere of a mixed gas of nitrogen and oxygen with an oxygen concentration of 0.1 volume% (1000ppm) to 5 volume% (50000ppm), more preferably 0.1 volume% (1000ppm) to 3.5 volume% (35000ppm), and even more preferably 0.1 volume% (1000ppm) to 2.5 volume% (25000ppm). By performing the main firing in the above temperature and oxygen concentration ranges, the ferrite reaction proceeds, and the desired saturation magnetization and residual magnetization can be obtained.
[0053] The fired product is then crushed and classified to obtain ferrite particles. As a classification method, the particle size is adjusted to a desired particle size using existing air classification, mesh filtration, sedimentation, etc. In the case of dry recovery, recovery can also be performed using a cyclone, etc. When adjusting the particle size, two or more of the above-mentioned classification methods may be selected and performed, or the conditions may be changed to remove coarse particles and fine particles using one classification method. Thereafter, if necessary, the surface of the ferrite particles is subjected to a surface oxidation treatment by low-temperature heating, for example, heat treatment at 300°C to 700°C, to adjust the surface resistance of the ferrite particles.
[0054] 2. Carrier for electrophotographic developer Next, the electrophotographic developer carrier according to the present invention will be described. The electrophotographic developer carrier according to the present invention is characterized by comprising the above-mentioned ferrite particles and a resin coating layer provided on the surface of the ferrite particles. That is, the above-mentioned ferrite particles are characterized by being used as a core material of the electrophotographic developer carrier. The ferrite particles are as described above, so here, the resin coating layer will be mainly described.
[0055] (1) Coating resin The type of resin (coating resin) constituting the resin coating layer is not particularly limited. For example, fluororesin, acrylic resin, epoxy resin, polyamide resin, polyamideimide resin, polyester resin, unsaturated polyester resin, urea resin, melamine resin, alkyd resin, phenol resin, fluoroacrylic resin, acrylic-styrene resin, silicone resin, etc. can be used. In addition, modified silicone resins obtained by modifying silicone resins with acrylic resins, polyester resins, epoxy resins, polyamide resins, polyamideimide resins, alkyd resins, urethane resins, fluororesins, etc. may also be used.
[0056] In addition, from the viewpoint of suppressing the resin peeling due to mechanical stress received during stirring and mixing with the toner, the coating resin is preferably a thermosetting resin. Suitable thermosetting resins for the coating resin include epoxy resins, phenolic resins, silicone resins, unsaturated polyester resins, urea resins, melamine resins, alkyd resins, and resins containing these. However, as described above, the type of coating resin is not particularly limited, and an appropriate one can be selected depending on the type of toner to be combined and the usage environment.
[0057] The resin coating layer may be formed using one type of resin, or may be formed using two or more types of resin. When using two or more types of resin, one resin coating layer may be formed by mixing two or more types of resin, or multiple resin coating layers may be formed. For example, it is also preferable to provide a first resin coating layer having good adhesion to the ferrite particles on the surface of the ferrite particles, and provide a second resin coating layer on the surface of the first resin coating layer to impart the carrier with the desired charging performance.
[0058] (2) Resin coating amount The amount of resin (amount of resin coating) covering the surface of the ferrite particles is preferably 0.1% by weight or more and 10% by weight or less with respect to the ferrite particles used as a carrier core material for electrophotographic developer. By making the amount of resin coating 0.1% by weight or more, the surface of the ferrite particles can be sufficiently coated with resin, and the desired charge-imparting ability can be obtained. In addition, by making the amount of resin coating 10% by weight or less, aggregation of carrier particles during production is unlikely to occur, so that a decrease in productivity such as a decrease in yield and fluctuations in developer properties such as developer fluidity in an actual machine or charge-imparting ability to a toner can be suppressed.
[0059] (3) Additives The resin coating layer may contain additives such as a conductive agent and a charge control agent for the purpose of controlling the electric resistance, charge amount, and charge speed of the carrier.
[0060] Examples of the conductive agent include conductive carbon, oxides such as titanium oxide and tin oxide, and various organic conductive agents. However, since the electrical resistance of the conductive agent is low, if the amount of the conductive agent added is too large, charge leakage is likely to occur. Therefore, the content of the conductive agent is preferably 0.25% by weight or more and 20.0% by weight or less, more preferably 0.5% by weight or more and 15.0% by weight or less, and even more preferably 1.0% by weight or more and 10.0% by weight or less, based on the solid content of the coating resin.
[0061] Examples of the charge control agent include various charge control agents and silane coupling agents that are generally used for toners. The types of these charge control agents and coupling agents are not particularly limited, but charge control agents such as nigrosine dyes, quaternary ammonium salts, organometallic complexes, and metal-containing monoazo dyes, aminosilane coupling agents, and fluorine-based silane coupling agents can be preferably used. The content of the charge control agent is preferably 0.25% by weight or more and 20.0% by weight or less, more preferably 0.5% by weight or more and 15.0% by weight or less, and even more preferably 1.0% by weight or more and 10.0% by weight or less, based on the solid content of the coating resin.
[0062] 3. Electrophotographic Developer Next, an embodiment of the electrophotographic developer according to the present invention will be described The electrophotographic developer contains the above-mentioned carrier for electrophotographic developer and toner.
[0063] (1) Toner As the toner constituting the electrophotographic developer, for example, either a polymerized toner produced by a polymerization method or a pulverized toner produced by a pulverization method can be preferably used. These toners may contain various additives, and any toner may be used as long as it can be used as an electrophotographic developer in combination with the above carrier.
[0064] The toner volume average particle diameter (cumulative 50% particle diameter D50) is preferably 2 μm to 15 μm, more preferably 3 μm to 10 μm. When the toner volume average particle diameter (cumulative 50% particle diameter D50) is within the above range, an electrophotographic developer that enables high-quality electrophotographic printing can be obtained.
[0065] Regarding the mixture ratio of the carrier and the toner, the toner concentration is preferably 3% by weight or more and 15% by weight or less. An electrophotographic developer containing the toner at the above concentration can easily obtain a desired image density and can better suppress fogging and toner scattering. On the other hand, when the electrophotographic developer is used as a refill developer, the toner is preferably 2 parts by weight or more and 50 parts by weight or less per part by weight of the carrier.
[0066] (2) Application to electrophotographic devices The electrophotographic developer according to the present invention can be suitably used in various electrophotographic developing devices that apply a magnetic brush development method in which a carrier is attracted and attached to a magnetic drum or the like by magnetic force to form a brush-like toner, and a visible image is formed by attaching the toner to an electrostatic latent image formed on a photoconductor or the like while applying a bias electric field. The electrophotographic developer according to the present invention can be used not only in electrophotographic developing devices that use a DC bias electric field when applying a bias electric field, but also in electrophotographic developing devices that use an AC bias electric field in which an AC bias electric field is superimposed on a DC bias electric field. EXAMPLES
[0067] <Example 1> The MnO raw material, MgO raw material, and Fe2O3 raw material as main component raw materials were weighed out so that the molar ratio of MnO:MgO:Fe2O3 was 39.0:10.0:51.0. The SrO raw material was weighed out so that the molar ratio of main component raw material:SrO was 100:0.8. Note that trimanganese tetroxide was used as the Mn raw material, magnesium oxide was used as the MgO raw material, ferric oxide was used as the Fe2O3 raw material, and strontium carbonate was used as the SrO raw material.
[0068] The weighed raw materials were then pulverized for 5 hours in a dry media mill (vibration mill, 1 / 8 inch diameter stainless steel beads), and the resulting pulverized material was made into pellets of approximately 1 mm square using a roller compactor. The resulting pellets were passed through a vibrating sieve with 3 mm openings to remove coarse powder, and then through a vibrating sieve with 0.5 mm openings to remove fine powder. The pellets were then placed in a continuous electric furnace and heated at 900°C for 3 hours for pre-firing. The pellets were then pulverized for 6 hours using a dry media mill (vibration mill, 1 / 8 inch diameter stainless steel beads) until the average particle size (D50) was approximately 5 μm.
[0069] Water was added to the obtained pulverized material, and the material was pulverized for 6 hours using a wet media mill (horizontal bead mill, zirconia beads with a diameter of 1 mm). The particle size of the obtained slurry (the primary particle size of the pulverized material) was measured using a laser diffraction particle size distribution analyzer (LA-950, manufactured by Horiba, Ltd.), and the average particle size (D50) was about 2.3 μm. Furthermore, an appropriate amount of dispersant was added to the obtained slurry, and 0.5 wt% of PVA (polyvinyl alcohol) was added as a binder relative to the solid content (the amount of the pre-calcined material in the slurry), and the mixture was then granulated and dried using a spray dryer. The particle size of the obtained granulated material was adjusted to obtain granulated material A with an average particle size (D50) of about 42 μm.
[0070] Granulated material B having an average particle size (D50) of about 55 μm was obtained in the same manner as granulated material A, except that the MnO raw material, MgO raw material, and Fe2O3 raw material were weighed out as main component raw materials so that the molar ratio of MnO:MgO:Fe2O3 was 39.0:10.0:51.0, and the SrO raw material was weighed out so that the molar ratio of main component raw material:SrO was 100:1.2. The particle size of the granulated material was adjusted by adjusting the atomizer rotation speed during granulation with a spray dryer, and the particle size was also adjusted.
[0071] The granulated material obtained by mixing the granulated material A and the granulated material B in a ratio of 2:1 was heated in an air atmosphere at 950°C for 2 hours using a rotary electric furnace to perform primary firing. After that, the granulated material was fired in a tunnel electric furnace at a firing temperature (holding temperature) of 1200°C and an oxygen concentration of 0.3% by volume for 3 hours. At this time, the heating rate was 200°C / hour and the cooling rate was 150°C / hour. The fired material obtained was crushed by a hammer crusher, and further classified by a gyro shifter (vibrating sieve) and a turbo classifier (air flow classifier) to adjust the particle size, and low magnetic products were separated by magnetic separation to obtain ferrite particles.
[0072] <Examples 2 to 9 and Comparative Examples 1 to 3> Ferrite particles were obtained in the same manner as in Example 1, except that the blending amounts of the raw materials used in the production of granulated material A and granulated material B and the average particle sizes (D50) of granulated material A and granulated material B were changed as shown in Table 1. In Example 8, calcium carbonate was used as the CaO raw material instead of the SrO raw material.
[0073] [Table 1]
[0074] The following points were evaluated for the ferrite particles obtained in Examples 1 to 9 and Comparative Examples 1 to 3. The results are shown in Table 2.
[0075] <Elemental analysis> The content of metal components in the ferrite particles was measured by chemical analysis (ICP). Specifically, 0.2 g of ferrite particles was weighed, and 60 ml of pure water, 20 ml of 1N hydrochloric acid, and 20 ml of 1N nitric acid were added to the weighed ferrite particles, and the mixture was heated to prepare an aqueous solution in which the ferrite particles were completely dissolved. The resulting aqueous solution was placed in an ICP analyzer (ICPS-1000IV, manufactured by Shimadzu Corporation) to measure the content of the metal components Fe, Mn, Mg, Sr, and Ca.
[0076] <Particle size distribution> The particle size distribution of the ferrite particles was measured by a laser diffraction scattering method. Specifically, 10 g of ferrite particles and 80 ml of water were first placed in a 100 ml beaker, and 2 to 3 drops of a dispersant (sodium hexametaphosphate) were added. Next, an ultrasonic homogenizer (UH-150 type, manufactured by SMT) was used to set the output level to 4, disperse for 20 seconds, and then the bubbles formed on the surface of the beaker were removed to prepare a measurement sample. Then, a Microtrac particle size analyzer (Model MT3300II, manufactured by Nikkiso) was used to measure the particle size distribution of the ferrite particles in the measurement sample under the condition of a refractive index of 2.42, and the cumulative 50% particle diameter D50 (μm) in the particle size distribution based on volume, and the proportion of particles with a particle diameter of 22 μm or less D -22 (Volume%) and the ratio of particles with a particle diameter of 62 μm or more D +62 The percentage of particles with a particle diameter of 40 μm or more in the particle size distribution based on the number of particles, P +40 The percentage (number %) was calculated.
[0077] <Magnetization> The residual magnetization of the ferrite particles was measured using a vibrating sample magnetometer (VSM-C7-10A, manufactured by Toei Kogyo Co., Ltd.). Specifically, the ferrite particles were first packed into a cell with an inner diameter of 5 mm and a height of 2 mm, and then set in the above-mentioned apparatus. A magnetic field was then applied and swept up to 1K·1000 / 4π·A / m (=1kOe). The applied magnetic field was then reduced, and a hysteresis curve was created on a recording paper. The residual magnetization was measured from the data of this curve.
[0078] <Superficiality> To evaluate the surface properties of the ferrite particles, the surface roughness Rz (μm) and the standard deviation Rzσ (μm) of the surface roughness Rz were measured. Specifically, a hybrid laser microscope (mc2000, manufactured by Lasertec) was used to obtain the three-dimensional shape of the surface of the ferrite particles to be measured (measurement target particles). As a pretreatment, double-sided tape was attached to a slide glass, and ferrite particles were sprinkled on the adhesive surface to fix the ferrite particles on the slide glass. In addition, a xenon lamp was used as the light source, the magnification of the objective lens was set to 100 times, and the measurement target particles were selected, and the three-dimensional shape of the surface was obtained by the automatic photography function of the software LMeye7 attached to the device.
[0079] Twenty-one 15.0 μm line segments were drawn at 0.75 μm intervals on the three-dimensional image of the measurement target particle obtained as described above, and the measurement profile curve on each line segment was extracted. Correction was performed on each of the obtained measurement profile curves using a profile curve filter to extract a roughness curve. Then, as the cutoff value of the profile curve filter, λs, which separates the roughness component from a shorter wavelength component, and λc, which separates the roughness component from the waviness component, were used, and the respective cutoff values were set to λs = 0.0025 mm and λc = 0.0800 mm, and the surface roughness Rz (μm) was calculated from the obtained roughness curve. In this way, the average value of the surface roughness Rz (μm) obtained based on the 21 line segments was taken as the Rz (μm) of each measurement target particle. In the same procedure, the average value of the surface roughness Rz values of the 30 measurement target particles was taken as the surface roughness Rz (μm) of each ferrite particle, and its standard deviation Rzσ (μm) was also calculated.
[0080] <edx> The proportion (atomic %) of Sr or Ca on the particle surface was measured by energy dispersive X-ray analysis (EDX analysis). Incidentally, EDX analysis can measure the content of elements at a depth of about several μm in ferrite particles. Specifically, first, images of ferrite particles were taken using a scanning electron microscope (SEM, SU8020, Hitachi High-Technogies) under conditions of an acceleration voltage of 20 kV, a WD of 15 mm, and a magnification of 150 times. Next, the obtained images were imported into an energy dispersive X-ray analyzer (EMax X-Max50, Horiba, Ltd.), and particles with no particle overlap and a particle diameter of 35 μm or less were selected by region selection. Incidentally, the selection was limited to particles with a ratio of the minimum Feret diameter to the maximum Feret diameter of 1.0 to 1.2, and particles in which two or more particles were aggregated were also selected within this range. Then, mapping collection was performed for constituent elements such as Fe, Mn, Mg, Sr, and Ca, and the percentage of Sr or Ca (atomic %) was calculated from the obtained X-ray spectrum peaks. The average value of the percentages of Sr or Ca (atomic %) measured in this way for 100 particles was taken as the percentage X (atomic %) of Sr or Ca in the elemental mapping of the particle surface of a particle with a particle diameter of 35 μm or less. The same operation was performed for particles with a particle diameter of 40 μm or more, and the percentage Y (atomic %) of Sr or Ca in the elemental mapping of the particle surface of a particle diameter of 40 μm or more was calculated.
[0081] <Electrostatic properties> To evaluate the electrostatic charge of ferrite particles (carrier core material), the amount of charge Q under normal temperature and humidity (N / N) conditions was measured. N / N and its standard deviation Q N / N The charge amount measurement device used was a device consisting of a cylindrical aluminum tube (sleeve), a magnet roll placed inside the sleeve, and a cylindrical electrode placed to surround the outside of the sleeve. The sleeve has a diameter of 31 mm and a length of 76 mm. The magnet roll has a structure in which a total of eight magnets (magnetic flux density 0.1 T) are arranged so that their N poles and S poles alternate. The cylindrical sleeve and the cylindrical electrode are set so that the gap between them is 5.0 mm.
[0082] The charge amount and charge amount distribution in a normal temperature and humidity (N / N) environment were measured as follows. First, ferrite particles (carrier core material) and a commercially available negative polarity toner (cyan toner, for Fuji Xerox DocuPrint C3530) used in full-color printers were weighed so that the toner concentration was 7.5% by weight and the total weight was 50 g. The weighed ferrite particles and toner were exposed to a normal temperature and humidity environment of a temperature of 20° C. and a relative humidity of 55% for 12 hours or more. Thereafter, the ferrite particles and toner were placed in a 50 ml glass bottle and stirred at a rotation speed of 120 rpm for 30 minutes to prepare a developer.
[0083] 0.5 g of the obtained developer was uniformly attached onto the sleeve of the charge amount measuring device. Next, while the sleeve was fixed, the inner magnet roll was rotated at a rotation speed of 100 rpm, and in this state, a DC voltage of 2000 V was applied between the outer electrode and the sleeve for 60 seconds. The toner in the developer was transferred to the outer electrode by the voltage application. At this time, an electrometer (insulation resistance meter model 6517A, made by KEITHLEY) was connected to the cylindrical electrode, and the charge amount of the transferred toner was measured. After 60 seconds, the applied voltage was turned off, the rotation of the magnet roll was stopped, the outer electrode was removed, and the toner that had transferred to the electrode was collected and its weight was measured. Then, from the measured charge amount and weight of the toner, the charge amount Q was calculated. N / N (μC / g) was calculated.
[0084] The charge distribution of the developer obtained above was measured using a charge amount / particle size distribution measuring device (E-SPART Analyzer EST-G, manufactured by Hosokawa Micron). The measurement was performed by holding the developer with an electromagnet and spraying nitrogen gas at an appropriate pressure to separate only the toner from the developer, which was then introduced into the measuring section of the measuring device. Analysis was performed on 3,000 toner particles, and the standard deviation Q of the charge amount per particle size was obtained. N / N σ (μC / g) was calculated.
[0085] [Table 2]
[0086] From the above results, it is apparent that the ferrite particles obtained in Examples 1 to 9 have a high charge imparting ability and a sharp charge amount distribution.< / edx>
Claims
1. When the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 35 μm or less is X (atomic %), and the ratio of Sr or Ca in elemental mapping of the surface of a particle having a particle diameter of 40 μm or more is Y (atomic %), the following formula: 1.10≦Y / X Fulfill Ferrite particles.
2. The following formula: 0.30≦X≦0.80 0.36≦Y≦1.55 1.20≦Y / X≦2.00 Fulfill The ferrite particles of claim 1.
3. A cumulative 50% particle diameter D50 in a volume-based particle size distribution is 30 μm or more and 50 μm or less, The proportion of particles with a particle diameter of 40 μm or more in the particle size distribution based on the number standard P +40 is 5% by number or more and 40% by number or less The ferrite particles of claim 1.
4. The surface roughness Rz is 2.5 μm or more and 4.5 μm or less, The standard deviation Rzσ of the surface roughness Rz is 0.2 μm or more and 1.0 μm or less. The ferrite particles according to claim 1 .
5. Contains 0.3% to 1.2% by weight of Sr or Ca The ferrite particles according to claim 1 .
6. Contains 15% by weight or more and 30% by weight or less of Mn and 45% by weight or more and 65% by weight or less of Fe The ferrite particles according to claim 5.
7. Residual magnetization σr is 3.0 Am 2 / kg The ferrite particles according to claim 1 .
8. The ferrite particles according to any one of claims 1 to 7 are included. Carrier core material for electrophotographic developers.
9. The present invention comprises a ferrite particle according to any one of claims 1 to 7 and a resin coating layer provided on the surface of the ferrite particle. Carrier for electrophotographic developer.
10. A toner carrier for electrophotographic developer according to claim 9. Electrophotographic developers.
11. Used as a refill developer The electrophotographic developer of claim 10.
Citation Information
Patent Citations
Ferrite powder, carrier core for electro-photography developing agent, carrier for electro-photography developing agent, and electro-photography developing agent
CN110928152A
Ferrite carrier core material for electrophotographic developer, ferrite carrier and production method of the same, and electrophotographic developer using the ferrite carrier
JP2012181398A
Ferrite particle, and carrier for electrophotographic development and electrophotographic developer using the same
JP2015151287A
Ferrite particle, and carrier for electrophotographic development and electrophotographic developer using the same
JP2015157727A
Ferrite particle having outer shell structure
JP2016138014A