Carbon fiber reinforced molded body
By controlling fiber orientation and eliminating the pelletizing step in the extrusion molding process, the carbon fiber reinforced molded article achieves high mechanical strength and wide-frequency electromagnetic shielding using recycled fibers, addressing the limitations of existing technologies.
Patent Information
- Application Number
- JP2023052656
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing carbon fiber reinforced resin compositions using recycled fibers face challenges in achieving high mechanical properties and wide-frequency electromagnetic shielding performance, often requiring additional metal components that increase weight and environmental impact.
A carbon fiber reinforced molded article using recycled fibers is produced through extrusion molding, controlling fiber orientation to achieve an orientation coefficient of 0.35 or more, eliminating the pelletizing step, and combining with a thermoplastic resin to enhance mechanical strength and electromagnetic shielding across a wide frequency range.
The method results in a molded article with high bending strength and excellent electromagnetic shielding performance from 0.1 MHz to 110 GHz, maintaining environmental friendliness and reducing material costs.
Smart Images

Figure 2024141165000001 
Figure 2024141165000002 
Figure 2024141165000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a carbon fiber reinforced molding containing recycled carbon fibers and a thermoplastic resin. [Background technology]
[0002] Carbon fiber reinforced plastics (CFRP) are used in a wide range of fields, including automobiles, aircraft, and civil engineering temporary construction materials, due to their characteristics of light weight, excellent strength, and high durability. Carbon fiber reinforced resins are divided into thermosetting carbon fiber reinforced resins and thermoplastic carbon fiber reinforced resins (CFRTP: Carbon Fiber Reinforced Thermo Plastics), depending on the properties of the resin used for impregnation. Of these, thermoplastic carbon fiber reinforced resins are used especially as materials for automobiles, due to their advantages of short molding time and recyclability by heating.
[0003] Here, by using recycled carbon fiber (RCF) as carbon fiber (CF) instead of newly produced virgin carbon fiber (VCF), it is possible to reduce the environmental impact and material costs. However, when using recycled carbon fiber, although it is relatively easy to produce short fiber pellets, there is a problem that the fibers are subjected to shear forces and are significantly broken due to the two steps of pelletization and molding, making it difficult for the obtained molded body to exhibit excellent mechanical properties.
[0004] Furthermore, in recent years, electronic devices and communication means have become increasingly wireless, with electromagnetic waves of frequencies of, for example, 300 Hz to 10 MHz being generated from induction cookers and trains, 10 MHz to 300 MHz from radio broadcasts, 300 MHz to 3 GHz from microwave ovens, mobile phones, television broadcasts, and the like, and 2 GHz or higher being generated from in-vehicle products for electric vehicles such as electric vehicle batteries (particularly 18 GHz to 110 GHz, also known as millimeter waves, including 26 GHz to 29 GHz, which has attracted attention in recent years for 5G communications, etc.). For this reason, there is a demand for resin molded products and materials thereof with excellent electromagnetic wave shielding performance that can block electromagnetic waves generated from these sources.
[0005] As a material for improving mechanical properties and electromagnetic shielding performance, for example, Patent Document 1 describes an electromagnetic shielding resin composition consisting of a thermoplastic resin, a metal-coated carbon fiber, and a metal-coated graphite, while Patent Document 2 describes a fiber-reinforced polypropylene resin composition containing a polypropylene resin, a carbon fiber, and a modified polyolefin resin. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2005-298653 A [Patent Document 2] JP 2022-110895 A Summary of the Invention [Problem to be solved by the invention]
[0007] In Patent Document 1, the use of recycled carbon fibers is not considered in the first place. On the other hand, in Patent Document 2, recycled carbon fibers are used. However, in both Patent Documents 1 and 2, the resin composition is once pelletized as a raw material for the molded body, and as described above, there is a problem that the obtained molded body does not easily exhibit high mechanical properties. In addition, from the viewpoint of the manufacturing method, the number of steps increases by the pelletization step, and the process costs are also required.
[0008] Furthermore, although Patent Document 1 measures the shielding properties for electric field waves and magnetic field waves at a frequency of 500 MHz, and Patent Document 2 evaluates the electromagnetic wave shielding properties by reading the attenuation amount at 5 MHz, which corresponds to the radio wave band, it is unclear whether high electromagnetic wave shielding properties are exhibited in the wide frequency range of several MHz to several GHz generated from the above sources, and even in the millimeter wave band.
[0009] As described above, it is difficult to achieve both excellent electromagnetic wave shielding performance over a wide frequency range and high mechanical properties in a carbon fiber reinforced resin molding using recycled carbon fibers.
[0010] Incidentally, in order to improve the electromagnetic wave shielding performance, if metal components such as metal-coated carbon fiber or metal-coated graphite are included, as in Patent Document 1, the weight of the resin molding increases, making it difficult to reduce the weight. In addition, this not only makes it difficult to recycle, but also poses environmental issues.
[0011] The present invention has been made in consideration of these points, and aims to provide a molded body that is environmentally friendly by using recycled carbon fibers, and that has excellent electromagnetic shielding performance over a wide frequency range and high mechanical strength (particularly bending strength). [Means for solving the problem]
[0012] The present inventors have found that carbon fiber reinforced molded products using recycled carbon fibers, particularly carbon fiber reinforced extrusion molded products, exhibit mechanical properties that are equivalent to those using virgin carbon fibers, by controlling fiber orientation in the resin flow direction by extrusion molding. This manufacturing method can omit the pelletizing process. The present inventors have also found that by making the orientation coefficient of the molded product 0.35 or more, the mechanical properties (particularly bending strength) are improved, and excellent electromagnetic wave shielding performance is achieved as electrical properties in a wide frequency range (for example, about 0.1 MHz to 1000 MHz (1 GHz), 18 GHz to 110 GHz).
[0013] In order to achieve the above object, the carbon fiber reinforced molding of the present invention contains recycled carbon fiber and a thermoplastic resin, The orientation coefficient represented by the formula (1): orientation coefficient (η0) = (E - Em (1 - Vf)) / (Ef × Vf) (1) (where E is the elastic modulus of the composite material (GPa), Em is the elastic modulus of the resin (GPa), Vf is the fiber volume content, and Ef is the elastic modulus of the carbon fiber (GPa)) is 0.35 or more, - The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, -The electromagnetic shielding effect, measured in accordance with the KEC method, is 60 dB or more over the entire frequency range from 0.5 MHz to 10 MHz (0.5 MHz or more and 10 MHz or less).
[0014] The carbon fiber reinforced molding of the present invention contains recycled carbon fibers and a thermoplastic resin, The orientation coefficient represented by the above formula (1) is 0.35 or more, - The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, The electromagnetic shielding effect, measured in accordance with the KEC method, is 40 dB or more over the entire frequency range from 10 MHz to 100 MHz (10 MHz or more and 100 MHz or less).
[0015] The carbon fiber reinforced molding of the present invention contains recycled carbon fibers and a thermoplastic resin, The orientation coefficient represented by the above formula (1) is 0.35 or more, - The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, The electromagnetic shielding effect, measured in accordance with the KEC method, is 30 dB or more over the entire frequency range from 100 MHz to 1000 MHz (100 MHz or more and 1000 MHz or less). Effect of the Invention
[0016] According to the present invention, it is possible to provide a molded article which is environmentally friendly by using recycled carbon fibers, and which has excellent electromagnetic shielding performance over a wide frequency range and high mechanical strength (particularly bending strength). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below. Note that the present invention is not limited to the following embodiments, and can be appropriately modified and applied within the scope of the present invention.
[0018] <Carbon fiber reinforced molding> Carbon fiber reinforced molded products contain recycled carbon fibers and thermoplastic resins as raw materials. In other words, carbon fiber reinforced molded products can be called carbon fiber reinforced thermoplastic resins (CFRTP). Carbon fiber reinforced molded products use recycled carbon fibers, so the environmental impact and material costs are reduced compared to conventional molded products that use virgin carbon fibers. Examples of carbon fiber reinforced molded products include extrusion molded products, injection molded products, press molded products, and molded products that combine these.
[0019] (recycled carbon fiber) Recycled carbon fiber (RCF) refers to, for example, carbon fiber (CF) recovered from used carbon fiber reinforced resin (CFRP), and carbon fiber recovered from scraps of intermediate products (prepregs) of carbon fiber reinforced resin generated during the manufacturing process of carbon fiber reinforced resin. Recycled carbon fiber is generally a discontinuous fiber. Recycled carbon fiber may be a heated carbon fiber reinforced resin (heated CFRP product). In addition, recycled carbon fiber may contain (may use) a sizing agent, or may not contain (may not use) a sizing agent. Specific examples of recycled carbon fiber include those described in the examples below.
[0020] The content of recycled carbon fibers (hereinafter also referred to as "CF content") relative to the entire carbon fiber reinforced molding (total amount 100% by weight) is preferably 10% by weight or more, more preferably more than 10% by weight, and even more preferably 15% by weight or more, from the viewpoint of improving the mechanical strength of the molding. The upper limit of the content is not particularly limited, and is preferably 60% by weight or less, more preferably 50% by weight or less, even more preferably 40% by weight or less, even more preferably 35% by weight or less, and even more preferably 30% by weight or less.
[0021] (thermoplastic resin) Examples of the thermoplastic resin include polyester resins such as polycarbonate (PC) resin, phenoxy resin, and polybutylene terephthalate; nylon resin; olefin resins such as polyethylene and polypropylene; acid-modified olefin resins; polyphenylene sulfide resin; polysulfone resin; polyether ether ketone resin; polyimide resin; polystyrene resin; and ABS resin. Among the thermoplastic resins, polycarbonate resin, nylon resin, olefin resin, phenoxy resin, polybutylene terephthalate, and polyphenylene sulfide resin are preferred because they are superior in impact resistance, heat resistance, and recyclability and are low cost compared to thermosetting resins. The thermoplastic resin may be a recycled resin. Examples of the recycled resin include those derived from various containers such as bottles, disks, sheets, and the like.
[0022] (Other materials) The carbon fiber reinforced molding may contain other materials than the recycled carbon fiber and thermoplastic resin as raw materials, as long as the characteristics are not impaired. Examples of other materials include sizing agents, antistatic agents, flame retardants, compatibilizers, virgin carbon fibers, etc. Virgin carbon fibers refer to, for example, newly manufactured new carbon fibers that are generally sold as carbon fibers.
[0023] <Characteristics of carbon fiber reinforced moldings> (Orientation coefficient (η0)) In carbon fiber reinforced moldings, the orientation coefficient (η0) is an index that indicates the contribution of the fibers to the measurement axis relative to the plane of the molding. The orientation coefficient (η0) is a value between 0 and 1. If the orientation coefficient (η0) is too small, excellent bending strength will not be achieved, even if the amount of fiber is increased or the remaining fiber length is lengthened. On the other hand, if the orientation coefficient (η0) is too large, the elastic modulus of the composite material becomes too high, making it difficult to shape the material by heating.
[0024] The orientation coefficient (η0) is calculated, for example, by the formula (1) (hereinafter also referred to as "orientation coefficient (1)"). [Number 1] Orientation coefficient (η0) = (E - Em(1 - Vf)) / (Ef × Vf) (1).
[0025] In formula (1), "E" is the elastic modulus of the composite material (GPa), "Em" is the elastic modulus of the resin (GPa), "Vf" is the fiber volume content, and "Ef" is the elastic modulus of the carbon fiber (GPa). These elastic moduli refer to the "four-point bending modulus in the MD direction" described later.
[0026] The orientation coefficient (1) of the carbon fiber reinforced molding is 0.35 or more. By specifying the orientation coefficient (1) of the carbon fiber reinforced molding to be 0.35 or more, it is possible to achieve both excellent electromagnetic wave shielding performance in a wide frequency range of about 0.1 MHz to 1000 MHz and high mechanical strength (especially bending strength).
[0027] The orientation coefficient (1) is preferably 0.38 or more, more preferably 0.40 or more, and the upper limit thereof is preferably 0.55 or less.
[0028] (4-point bending strength in MD direction, 4-point bending modulus in MD direction) A carbon fiber reinforced molded product molded using a raw material containing recycled carbon fiber and a thermoplastic resin has a four-point bending strength in the resin flow direction (MD direction) by extrusion molding (T die casting) of 125 MPa or more, measured in accordance with JIS K 7074 (bending test method for carbon fiber reinforced plastics). Although the carbon fiber reinforced molded product uses recycled carbon fiber, it has physical properties equivalent to those of conventional molded products using virgin carbon fiber. The four-point bending strength and four-point bending modulus in the MD direction are measured, for example, by the method described in the examples below.
[0029] The four-point bending strength in the MD direction of the carbon fiber reinforced molding is 125 MPa or more, preferably 160 MPa or more, and more preferably 180 MPa or more.
[0030] The four-point bending elastic modulus in the MD direction of the carbon fiber reinforced molding is preferably 5.8 GPa or more, more preferably 8.0 GPa or more, and further preferably 10.0 GPa or more.
[0031] (Fiber volume fraction (Vf)) In the carbon fiber reinforced molding, the fiber volume fraction (Vf) measured according to the combustion method of JIS K 7075 (Testing method for fiber content and void content of carbon fiber reinforced plastics) is preferably 6% or more (CF content: 10% by weight or more) from the viewpoint of improving the mechanical strength of the molding. The upper limit is preferably 40% or less (CF content: 50% by weight or less), more preferably 23% or less (CF content: 30% by weight or less), from the viewpoint of suppressing poor dispersion of carbon fibers and reducing costs. The fiber volume fraction (Vf) is calculated, for example, by the method described in the examples below.
[0032] (Number average fiber length (Ln)) In the carbon fiber reinforced molding, the number average fiber length (Ln) of the remaining recycled carbon fibers is preferably 0.15 mm or more, more preferably 0.20 mm or more, from the viewpoint of improving the mechanical strength of the molding by leaving the remaining fiber length long. In addition, since the manufacturing method of the carbon fiber reinforced molding does not go through the pelletizing process, there is no further fiber breakage in the pelletizing process, and a carbon fiber reinforced molding having a longer remaining fiber length is obtained. The number average fiber length (Ln) of the recycled carbon fibers is calculated, for example, by the method described in the examples below.
[0033] (Degree of dispersion (Lw / Ln)) In the carbon fiber reinforced molding, the dispersion (Lw / Ln) of the remaining recycled carbon fibers is preferably 1.00 or more and 2.25 or less, more preferably 1.25 or more and 2.25 or less, from the viewpoint of improving the mechanical strength of the molding. A dispersion close to 1 means that the fiber length of the carbon fibers is uniform. On the other hand, a dispersion greater than 1 means that the carbon fibers have a mixture of long and short fiber lengths, and the fiber length variation is large. If the proportion of short carbon fibers increases and the fiber length distribution becomes wider, the mechanical strength of the molding is weakened, so the dispersion must be set within an appropriate range. The dispersion (Lw / Ln) is calculated, for example, by the method described in the examples below.
[0034] (Electromagnetic shielding performance in the frequency range of 0.1MHz to 1000MHz (1GHz)) In this specification, the electromagnetic shielding performance in the frequency band of 0.1 MHz to 1000 MHz (1 GHz) (hereinafter also referred to as the "first frequency band") refers to the electromagnetic shielding characteristic (electromagnetic shielding effectiveness (SE)) measured in accordance with the KEC method (a method for measuring electromagnetic shielding effectiveness developed by the KEC Kansai Electronics Industry Development Center, a general incorporated association).
[0035] Here, the excellent electromagnetic wave shielding performance in the first frequency band required for the carbon fiber reinforced molding means not only a shielding effect against electromagnetic waves of a certain frequency (one point), but also an electromagnetic wave shielding effect of at least 30 dB over a wide frequency range including electromagnetic waves of 300 Hz to 10 MHz generated from the above-mentioned IH cooking appliances, railways, etc., electromagnetic waves of 10 MHz to 300 MHz generated from radio broadcasts, etc., electromagnetic waves of 300 MHz to 3000 MHz (3 GHz) generated from microwave ovens, mobile phones, television broadcasts, etc., and electromagnetic waves of 2 GHz or higher generated from in-vehicle products for electric vehicles such as electric vehicle batteries. In other words, the carbon fiber reinforced molding has an electromagnetic wave shielding effect of at least 30 dB over the entire frequency range of 0.1 MHz to 1000 MHz (1 GHz).
[0036] The carbon fiber reinforced molding preferably has an electromagnetic shielding effect of at least 30 dB over the entire frequency range of 0.1 MHz to 0.5 MHz (0.1 MHz to 0.5 MHz, 100 kHz to 500 kHz), and more preferably has an electromagnetic shielding effect of at least 40 dB (99% shielding). In this specification, for example, "at least 30 dB over the entire frequency range of 0.1 MHz to 0.5 MHz" means that the minimum electromagnetic shielding effect measured within the frequency range of 0.1 MHz to 0.5 MHz is 30 dB or more. The average electromagnetic shielding effect measured within the frequency range of 0.1 MHz to 0.5 MHz is preferably 60 dB or more (99.9% shielding).
[0037] The carbon fiber reinforced molding has an electromagnetic wave shielding effect of at least 60 dB (99.9% shielding) over the entire frequency range of 0.5 MHz to 10 MHz, and preferably has an electromagnetic wave shielding effect of at least 70 dB. The carbon fiber reinforced molding preferably has a shielding effect of 60 dB or more (99.9% shielding) against 1 MHz electromagnetic waves.
[0038] The carbon fiber reinforced molding has an electromagnetic wave shielding effect of at least 40 dB (99% shielding) over the entire range of 10 MHz to 100 MHz. The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of 60 dB or more (99.9% shielding) against 10 MHz electromagnetic waves.
[0039] The carbon fiber reinforced molding has an electromagnetic wave shielding effect of at least 30 dB over the entire range of 100 MHz to 1000 MHz (1 GHz), and preferably has an electromagnetic wave shielding effect of at least 40 dB (99% shielding). The carbon fiber reinforced molding preferably has a shielding effect of 40 dB or more (99% shielding) against electromagnetic waves of 100 MHz. The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of 30 dB or more against electromagnetic waves of 300 MHz, 600 MHz, or 1000 MHz (1 GHz), and more preferably has an electromagnetic wave shielding effect of 40 dB or more (99% shielding).
[0040] (Electromagnetic shielding performance in the 18GHz to 110GHz frequency range) In this specification, the electromagnetic shielding performance in the frequency band of 18 GHz to 110 GHz (hereinafter also referred to as the "second frequency band") refers to the electromagnetic shielding characteristics (electromagnetic shielding effectiveness (SE)) measured in accordance with the free space method.
[0041] Here, the excellent electromagnetic shielding performance in the second frequency band required for the carbon fiber reinforced molding is, like the electromagnetic shielding performance in the first frequency band, not only a shielding effect against electromagnetic waves of a certain frequency (one point), but also an electromagnetic shielding effect over a wide frequency range including electromagnetic waves of 26 GHz to 29 GHz corresponding to the above-mentioned 5G communication, also called millimeter waves in the frequency band of 18 GHz to 110 GHz generated from in-vehicle products for electric vehicles such as electric vehicle batteries, of at least 40 dB or more (99% shielding). That is, it is preferable that the carbon fiber reinforced molding has an electromagnetic shielding effect of at least 40 dB or more over the entire frequency range of 18 GHz to 110 GHz.
[0042] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 50 dB over the entire range of 18 GHz to 26.5 GHz (18 GHz or more and 26.5 GHz or less).The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of 50 dB or more against 18 GHz electromagnetic waves.
[0043] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 60 dB (99.9% shielding) over the entire frequency range of 26 GHz to 29 GHz (26 GHz or more and 29 GHz or less), which corresponds to 5G communication. The average value of the electromagnetic wave shielding effect measured within the frequency range of 26 GHz to 29 GHz is preferably 70 dB or more.
[0044] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 60 dB (99.9% shielding) over the entire frequency range of 26.5 GHz to 40 GHz (26.5 GHz or more and 40 GHz or less).The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of 60 dB or more (99.9% shielding) against 30 GHz electromagnetic waves.
[0045] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 60 dB (99.9% shielding) over the entire frequency range of 40 GHz to 60 GHz (40 GHz or more and 60 GHz or less).
[0046] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 80 dB over the entire range of 60 GHz to 90 GHz (60 GHz or more and 90 GHz or less). The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of 80 dB or more against 60 GHz electromagnetic waves.
[0047] The carbon fiber reinforced molding preferably has an electromagnetic wave shielding effect of at least 70 dB over the entire range of 90 GHz to 110 GHz (90 GHz or more and 110 GHz or less). The carbon fiber reinforced molding preferably has a shielding effect of 80 dB or more against electromagnetic waves at 90 GHz. The carbon fiber reinforced molding preferably has a shielding effect of 70 dB or more against electromagnetic waves at 110 GHz.
[0048] <Production of carbon fiber reinforced moldings> In the following, an extrusion molded body will be taken as an example of the manufacture of a carbon fiber reinforced molded body. The carbon fiber reinforced molded body is manufactured, for example, by a T-die extrusion method. In this manufacturing method, pellets containing recycled carbon fibers in a thermoplastic resin are not used as a raw material, and a pelletizing process in which recycled carbon fibers are introduced into a molten thermoplastic resin and kneaded to prepare pellets in advance is not performed. Specifically, a carbon fiber reinforced molded body is manufactured by introducing recycled carbon fibers into a molten thermoplastic resin, kneading the mixture, and extruding the mixture as is. That is, the manufacturing method of a carbon fiber reinforced molded body includes a kneading process in which recycled carbon fibers and a thermoplastic resin are kneaded, and an extrusion molding process in which the kneaded molten mixture is extruded to form a desired shape, and the kneading process and the extrusion molding process are performed in-line.
[0049] Here, in-line extrusion molding means that a series of processes from feeding the thermoplastic resin and recycled carbon fiber to extrusion molding is carried out on one production line. In other words, this manufacturing method does not require a process such as pelletizing the thermoplastic resin and recycled carbon fiber on a separate line before extrusion molding. By manufacturing in-line without going through a pelletizing process, the obtained carbon fiber reinforced molded body has excellent mechanical strength equivalent to that of conventional molded bodies using virgin carbon fiber.
[0050] More specifically, recycled carbon fibers are fed into the molten thermoplastic resin whose viscosity has been reduced in the kneading process using a side feeder, and the resin is melt-kneaded in a single-axis (single-axis) extruder, and in-line processing (processing performed simultaneously on the extrusion molding line) is performed simultaneously with extrusion molding in the extrusion molding process. At this time, the orientation of the recycled carbon fibers in the flow direction (MD direction) of the extrusion molding resin is controlled by extrusion molding (T-die casting), so that the carbon fiber reinforced molded body exhibits excellent mechanical properties. In this manufacturing method, in a series of processes, the temperature of the extruder described later is adjusted within a predetermined range to sufficiently reduce the viscosity of the thermoplastic resin, so that the shear force applied to the recycled carbon fibers is suppressed. In addition, by omitting the pelletizing process, the shear force applied to the recycled carbon fibers is suppressed, and the breakage of the recycled carbon fibers is suppressed, so that the recycled carbon fibers tend to remain with their fiber length long. The fact that the recycled carbon fibers remain in the molded body in a long fiber length state is one of the factors that cause the carbon fiber reinforced molded body to exhibit excellent mechanical properties.
[0051] (Kneading process) The method for producing a carbon fiber reinforced molded body by the T-die extrusion method will be described in more detail. First, the cylinder temperature and die temperature of the single screw extruder are set to a temperature 50°C to 150°C higher than the glass transition point of the thermoplastic resin. The above temperature of the single screw extruder is, for example, about 220°C to 300°C. The thermoplastic resin is fed into the extruder with the temperature controlled within the above range, melted, and the resin viscosity is reduced.
[0052] Next, the recycled carbon fiber is fed into the extruder and kneaded. A side feeder is used to feed the recycled carbon fiber. Specifically, the recycled carbon fiber is fed from the side feeder into the area where the thermoplastic resin is sufficiently melted.
[0053] The side-fed recycled carbon fiber and the mixed thermoplastic resin are melt-kneaded at a screw rotation speed of, for example, about 30 rpm or more and 78 rpm or less.
[0054] (Extrusion molding process) Finally, by in-line extrusion molding from a T-die, a flat carbon fiber reinforced molding (CFRTP plate) having a thickness of, for example, about 1 mm to 10 mm can be obtained. The lower limit of the thickness is not particularly limited, and may be 2 mm or more. The shape of the carbon fiber reinforced molding is not limited to a flat plate shape, and it can be molded into various shapes.
[0055] The extruder is preferably a single-screw (single-screw) extruder from the viewpoint of controlling the orientation of the recycled carbon fibers in the flow direction (MD) of the resin, but a twin-screw extruder may also be used. EXAMPLES
[0056] The present invention will be described below based on examples. Note that the present invention is not limited to these examples, and these examples can be modified or changed based on the spirit of the present invention, and they are not excluded from the scope of the present invention.
[0057] <Manufacture of carbon fiber reinforced molded body (kneaded extrusion plate)> The polycarbonate (PC) resin shown in each table was put into a single-screw extruder with the cylinder temperature and die temperature set to 220 to 300 ° C. as a thermoplastic resin and melted. Then, the recycled carbon fiber (RCF, fiber length: 3 mm to 6 mm) shown in each table was fed from a side feeder at the content shown in each table (see "CF content" in the table) to the site where the polycarbonate resin was melted. Then, the mixture was melt-kneaded at a screw rotation speed of 30 to 78 rpm shown in each table and extruded from a T-die to obtain a flat carbon fiber reinforced molding (CFRTP plate) with a thickness of about 2 mm. If necessary, the CFRTP plate was subjected to a heat press treatment (see "press" in the table) at a temperature of 200 ° C. and a pressure of 5 MPa for 10 minutes in order to reduce voids in the obtained CFRTP plate. Through the above process, a CFRTP plate for evaluation with a thickness of 1.6 mm to 2.4 mm (based on JIS K 7074) was obtained. Comparative Example 4 is an extrusion molded article using polycarbonate resin pellets containing virgin carbon fiber (VCF). Comparative Example 5 is an extrusion molded article using polycarbonate resin pellets containing recycled carbon fiber (RCF). Comparative Example 6 is an injection molded article using polycarbonate resin pellets containing virgin carbon fiber (VCF). Comparative Example 7 is an extrusion molded article of polycarbonate resin (without carbon fiber).
[0058] <Evaluation of carbon fiber reinforced molded body (kneaded extruded plate)> <Calculation of fiber volume fraction (Vf)> The fiber volume fraction (Vf) of each CFRTP sheet for evaluation was calculated according to the combustion method of JIS K 7075. Specifically, the mass of each CFRTP sheet for evaluation, which is a measurement sample, was measured using an electric furnace and an electronic balance, and then the sample was heated from room temperature at a temperature increase rate of 20°C / min in a crucible under a nitrogen atmosphere, and when the temperature reached 550°C, the sample was incinerated for 10 minutes to incinerate the resin in the sample. Since carbon fiber does not decompose when heated under a nitrogen atmosphere, the weight at 550°C was taken as the carbon fiber weight, and the value multiplied by the specific gravity was taken as the carbon fiber volume. In addition, the weight of the incinerated resin was taken as the resin weight, and the value multiplied by the specific gravity of the resin was taken as the resin volume. Then, the fiber volume fraction (Vf) [%] was calculated using formula (3) in JIS K 7075. The results are shown in each table.
[0059] Calculation of weight average fiber length (Lw) and number average fiber length (Ln) The weight average fiber length (Lw) and number average fiber length (Ln) were obtained by the following method. First, each evaluation CFRTP plate was dissolved in a solvent that dissolves polycarbonate (PC) resin, and then filtered to obtain a recycled carbon fiber (RCF) residue. The residue was observed under an optical microscope at 50 to 100 times magnification, and the lengths of 1,000 randomly selected fibers were measured. The measured values (mm) (two decimal places are significant figures) were used to calculate the length based on the following formula. [Number 2] Weight average fiber length (Lw) = Σ(Wi × Li) / ΣWi =Σ(πri 2 ×Li×ρ×ni×Li) / Σ(πri 2 ×Li×ρ×ni) (When ri and ρ are constant, the above formula is simplified to the following formula.) ≒Σ(Li 2 ×ni) / Σ(Li×ni) (2). [Number 3] Number average fiber length (Ln) = Σ(Li × ni) / Σni (3). [About each symbol in the formula] · Li: Fiber length of fibrous filler. ·ni: number of fibrous fillers with fiber length Li. · Wi: Weight of fibrous filler. · ri: fiber diameter of fibrous filler. ·ρ : density of fibrous filler.
[0060] <Calculation of dispersibility (Lw / Ln)> The degree of dispersion (Lw / Ln) was calculated based on the following formula using the weight average fiber length (Lw) and number average fiber length (Ln) calculated above. [Number 4] Dispersity (Lw / Ln) = weight average fiber length (Lw) / number average fiber length (Ln) (4).
[0061] <Calculation of orientation coefficient (η0)> The orientation coefficient (η0) was calculated based on the bending modulus of each evaluation CFRTP plate and the above-mentioned formula (1). In formula (1), "E" (elastic modulus of composite material) is the "bending modulus (MD)" of each example in the table, "Em" (elastic modulus of resin) is the "bending modulus (MD)" (2.3 [GPa]) of Comparative Example 7 in the table, "Vf" is the "fiber volume content (Vf)" of each example in the table, and "Ef" (elastic modulus of carbon fiber) is the tensile modulus of a representative carbon fiber, which is 230 [GPa]. The orientation coefficient (η0) of Example 6 refers to the calculated value when "Em" (elastic modulus of resin) is "2.6 GPa".
[0062] <Measurement of bending strength in MD direction and bending modulus in MD direction> A four-point bending test was performed according to JIS K 7074 to measure the bending strength and bending modulus in the MD direction of each evaluation CFRTP plate. Specifically, a sample was cut out from each evaluation CFRTP plate so as to have a width of 15 mm and a length of 100 mm. Next, using a tensile tester (manufactured by Shimadzu Corporation, product name: Autograph 5000) equipped with a four-point bending jig, a four-point bending measurement of the above sample was performed under the conditions of a crosshead speed of 5 mm / min, a support span of 81 mm, an indenter span of 27 mm, a support diameter of 4 mm, and an indenter diameter of 10 mm, and the four-point bending strength [MPa] and the four-point bending modulus [GPa] were measured in the MD direction. In addition, a three-point bending test was performed in accordance with JIS K 7171 for Comparative Example 7, which is an extrusion molded product of a thermoplastic resin not containing carbon fiber. Specifically, a test piece was cut out from the evaluation PC (polycarbonate) plate of Comparative Example 7 to have a length of 80 mm, a width of 10 mm, and a thickness of 4 mm. Next, using the above-mentioned tensile tester equipped with a three-point bending jig, a three-point bending measurement of the above-mentioned test piece was performed under the conditions of a crosshead speed of 2 mm / min, a support span of 64 mm, a support diameter of 5 mm, and an indenter diameter of 5 mm, and the three-point bending strength [MPa] and three-point bending modulus [GPa] were measured in the MD direction. The results are shown in each table.
[0063] The measured bending strength [MPa] in the MD direction and bending modulus [GPa] in the MD direction were evaluated based on the following evaluation criteria. Note that "△" or higher indicates usable (acceptable) strength or modulus. "○" indicates sufficient strength or modulus. "◎" indicates excellent strength or modulus equivalent to that of an injection molded body of polycarbonate resin pellets containing virgin carbon fiber (VCF). The results are shown in each table. (Evaluation criteria for bending strength in MD direction [MPa]) ◎: 180MPa or more. ○: 160MPa or more but less than 180MPa. △: 125MPa or more but less than 160MPa. ×: Less than 125MPa. (Evaluation criteria for bending modulus in MD direction [GPa]) ◎: 10.0 GPa or higher. ○: 8.0 GPa or more but less than 10.0 GPa. △: 5.8GPa or more but less than 8.0GPa. ×: Less than 5.8 GPa.
[0064] <Evaluation of electromagnetic wave shielding performance in the first frequency band> The electromagnetic shielding effect in the first frequency band was quantitatively evaluated as the electromagnetic shielding performance (dB) of each evaluation CFRTP sheet by the KEC method using the electromagnetic shielding property measurement system (https: / / www.kptc.jp / kiki / 194 / ) developed by the KEC Kansai Electronics Industry Promotion Center, a general incorporated association. The results are shown in Tables 1 and 2. -Electromagnetic wave measurement frequency range: 0.1MHz (100kHz) to 1000MHz (1GHz). -Electromagnetic wave measurement frequency pitch: 0.01MHz. Measurement sample: W×D×H=140mm×140mm×2mm. · Atmosphere temperature: 25℃, relative humidity: 30~50%.
[0065] <Evaluation of electromagnetic wave shielding performance in the second frequency band> The electromagnetic shielding effect in the second frequency band was quantitatively evaluated by the free space method as the electromagnetic wave shielding performance (dB) of each evaluation CFRTP sheet. The results are shown in Tables 3 and 4. -Electromagnetic wave measurement frequency range: 18GHz~110GHz. -Electromagnetic wave measurement frequency pitch: 0.01GHz. Measurement equipment: Anritsu Corporation wideband vector network analyzer: ME7838A. Fixture for free space method: Keycom Co., Ltd., DPS24-01. Measurement sample: W×D×H=140mm×140mm×2mm.
[0066] The measured electromagnetic shielding performance was evaluated based on the following evaluation criteria. "△" or better indicates minimum shielding performance (pass). "○" indicates good shielding performance. "◎" indicates high shielding performance (shielding rate: 99.9%). The results are shown in each table. ◎: 60dB or more. ○: 40dB or more but less than 60dB. △: 30dB or more but less than 40dB. ×: Less than 30dB.
[0067] [Table 1]
[0068] [Table 2]
[0069] [Table 3]
[0070] [Table 4]
[0071] The various materials used in the production of the carbon fiber reinforced moldings are shown below. <Polycarbonate resin (PC resin, thermoplastic resin)> ·PC301-30: Manufactured by Sumika Polycarbonate Co., Ltd. PC1600: Polycarbonate plate manufactured by Takiron C.I. Co., Ltd., density: 1.2g / cm 3 , Tensile yield stress: 63MPa, Nominal tensile strain at break: 90%, Tensile modulus: 2250MPa, Flexural strength: 91MPa, Flexural modulus: 2300MPa, Volume resistivity: ≧1.0×10 13 Ω·m. <Polyamide resin (PA resin, thermoplastic resin)> PA6_CM1007: Toray Industries, Amilan, Grade: CM1007, Density: 1.13g / cm 3 , Water absorption: 1.8% (24 hours, 23°C), Tensile strength: 80MPa (23°C), Nominal tensile break strain: 30%, Tensile yield strain: 2.0%, Flexural strength: 110MPa, Volume resistivity: 1.0×10 12 ~10 13 Ω·m. <Recycled Carbon Fiber (RCF)> CF-N C6: Manufactured by Nippon Polymer Industries Co., Ltd., fiber length: 6mm, sizing material: none. CFRP heated product: Manufactured by Carbon Fiber Recycle Industry Co., Ltd., fiber length: 3mm, sizing material: none. <Virgin carbon fiber (VCF)-containing polycarbonate resin> · PC-C-20: Pyrofil (registered trademark) pellets (CFRTP pellets) manufactured by Mitsubishi Chemical Corporation. DSP-201: CFRTP pellets manufactured by Teijin Limited. <Recycled carbon fiber (RCF)-containing polycarbonate resin> DJK-XB-C6: CFRTP pellets made from PCX-10325B (polycarbonate resin manufactured by Sumika Polycarbonate Co., Ltd.) and the above CF-N C6. <Recycled carbon fiber (RCF) nonwoven fabric> - Hayate (registered trademark), manufactured by Yuho Co., Ltd., is a blend of carbon fiber (recycled carbon fiber) and thermoplastic fiber (equivalent to PA6_CM1007), which minimizes damage to the carbon fiber during the carding process and leaves the remaining fiber length long. It is an intermediate material for thermoplastic carbon fiber reinforced plastics, resin ratio: 50% by weight, basis weight: 250g / m 2 , Remaining fiber length: 70mm.
[0072] (Discussion of the Examples) Although the carbon fiber reinforced molded products in each Example use recycled carbon fiber (RCF), which is a discontinuous fiber, they achieved physical properties (MD 4-point bending strength of 125 MPa or more (MD 4-point bending modulus of 5.8 GPa or more) equivalent to those of Comparative Example 4 (CFRTP pellet extrusion molded product) and Comparative Example 6 (CFRTP pellet injection molded product), which use virgin carbon fiber (VCF). This is probably because the manufacturing method of the carbon fiber reinforced molding in each example does not have a pelletizing process, so the shear force applied to the recycled carbon fiber is suppressed, and as a result, fiber breakage is suppressed. Another factor is that the recycled carbon fiber remains in the molding with its long fiber length without being pelletized. Furthermore, the carbon fiber reinforced moldings of each Example not only had higher mechanical strength than Comparative Examples 1 to 3, but also achieved electromagnetic wave shielding performance of 30 dB or more over the entire wide frequency range of 0.1 MHz to 1000 MHz (1 GHz). Furthermore, compared with Comparative Examples 1 to 3, the carbon fiber reinforced moldings of each Example not only had higher mechanical strength, but also achieved electromagnetic wave shielding performance of 40 dB or more (99% shielding) over the entire wide frequency range of 18 GHz to 110 GHz, and in particular, at least 60 dB or more (99.9% shielding) over the entire frequency range of 26 GHz to 29 GHz, which corresponds to 5G communications. The excellent mechanical and electrical properties are believed to be due to the orientation coefficient (1) of 0.35 or more. [Industrial Applicability]
[0073] As described above, the present invention is suitable for a carbon fiber reinforced molding containing recycled carbon fibers and a thermoplastic resin.
Claims
1. A carbon fiber reinforced molding containing recycled carbon fibers and a thermoplastic resin, Equation (1): Orientation coefficient (η 0 )=(E-Em(1-Vf)) / (Ef x Vf) (1) (wherein E is the elastic modulus of the composite material (GPa), Em is the elastic modulus of the resin (GPa), Vf is the fiber volume content, and Ef is the elastic modulus of the carbon fiber (GPa)) is 0.35 or more, The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, A carbon fiber reinforced molding having an electromagnetic wave shielding effect of 60 dB or more over the entire frequency range from 0.5 MHz to 10 MHz, as measured in accordance with the KEC method.
2. A carbon fiber reinforced molding containing recycled carbon fibers and a thermoplastic resin, Equation (1): Orientation coefficient (η 0 )=(E-Em(1-Vf)) / (Ef x Vf) (1) (wherein E is the elastic modulus of the composite material (GPa), Em is the elastic modulus of the resin (GPa), Vf is the fiber volume content, and Ef is the elastic modulus of the carbon fiber (GPa)) is 0.35 or more, The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, A carbon fiber reinforced molding having an electromagnetic wave shielding effect of 40 dB or more over the entire range of 10 MHz to 100 MHz, as measured in accordance with the KEC method.
3. A carbon fiber reinforced molding containing recycled carbon fibers and a thermoplastic resin, Equation (1): Orientation coefficient (η 0 )=(E-Em(1-Vf)) / (Ef x Vf) (1) (wherein E is the elastic modulus of the composite material (GPa), Em is the elastic modulus of the resin (GPa), Vf is the fiber volume content, and Ef is the elastic modulus of the carbon fiber (GPa)) is 0.35 or more, The four-point bending strength in the MD direction measured in accordance with JIS K 7074 is 125 MPa or more, A carbon fiber reinforced molding having an electromagnetic wave shielding effect of 30 dB or more over the entire frequency range of 100 MHz to 1000 MHz, as measured in accordance with the KEC method.
4. 4. The carbon fiber reinforced molding according to claim 1, wherein the electromagnetic wave shielding effect measured in accordance with the KEC method is 30 dB or more over the entire range of 0.1 MHz to 0.5 MHz.
5. 4. The carbon fiber reinforced molding according to claim 1, wherein the recycled carbon fiber content is 5% by weight or more.
6. The carbon fiber reinforced molding according to any one of claims 1 to 3, characterized in that the four-point bending modulus in the MD direction measured in accordance with JIS K 7074 is 5.8 GPa or more.
7. The carbon fiber reinforced molding according to any one of claims 1 to 3, characterized in that the number average fiber length of the recycled carbon fibers is 0.15 mm or more.
Citation Information
Patent Citations
Carbon fiber / polycarbonate resin composite pellet and method for producing the same
JP2018188496A
Discontinuous fiber composite material and its manufacturing method
JP2018523599A
Resin composition, method for producing resin composition, and molded body
JP2019163354A
Recycled-carbon-fiber bundle composition and production method therefor
WO2022249680A1
Resin composition for electromagnetic wave-shielding, and molded item
JP2005298653A