Resin composition
The resin composition with thermosetting resin and heat-treated lignins addresses the challenge of achieving both heat and water resistance in molded articles, resulting in improved performance for industrial applications.
Patent Information
- Application Number
- JP2023052742
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Thermosetting resin molded articles often face a challenge in achieving both excellent heat resistance and water resistance, as these properties tend to contradict each other, making it difficult to improve both simultaneously.
A resin composition is formulated using a thermosetting resin and lignins, where the lignins have a dissolution rate of 50% by mass or less in N,N-dimethylformamide at 25°C, preferably containing heat-treated lignins such as carboxylic acid-modified or polyoxyethylene glycol-modified lignins, to enhance both heat and water resistance.
The resin composition results in molded articles with improved heat resistance and water resistance, suitable for various industrial applications.
Smart Images

Figure 2024141223000001 
Figure 2024141223000002 
Figure 2024141223000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a resin composition. [Background technology]
[0002] Conventionally, thermosetting resins are widely used in the manufacture of resin products (molded products). Examples of resin products include electrical parts, automobile parts, building materials, and daily necessities. Thermosetting resins are required to have various physical properties depending on the application. Examples of the physical properties required for resin products include mechanical strength, heat resistance, and electrical insulation.
[0003] In order to satisfy the physical properties required for a resin product, a thermosetting resin is used, for example, by mixing with various additives.
[0004] In recent years, from the viewpoint of environmental conservation, there has been a demand for using additives derived from plants. For example, lignins have been proposed as additives derived from plants. More specifically, for example, the following resin composition has been proposed. The resin composition contains a thermosetting resin and lignin modified with oxyethylene glycol (for example, see Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2021-123717 A Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, molded articles of thermosetting resins may be required to have particularly excellent heat resistance and water resistance depending on their applications. However, heat resistance and water resistance may be mutually exclusive, and it is difficult to improve both heat resistance and water resistance.
[0007] The present invention provides a resin composition capable of giving a molded article having excellent heat resistance and excellent water resistance. [Means for solving the problem]
[0008] The present invention [1] includes a resin composition containing a thermosetting resin and a lignin, in which the lignin has a solubility in N,N-dimethylformamide at 25°C of 50 mass% or less.
[0009] The present invention [2] includes the resin composition according to the above [1], in which the lignins contain lignin and / or modified lignin.
[0010] The present invention [3] includes the resin composition according to the above [2], in which the lignins contain heat-treated lignin and / or heat-treated modified lignin.
[0011] The present invention [4] includes the resin composition according to the above [3], in which the modified lignin contains a carboxylic acid-modified lignin and / or a polyoxyethylene glycol-modified lignin.
[0012] The present invention [5] comprises the resin composition according to any one of the above [1] to [4], wherein the lignins contain polyoxyethylene glycol-modified lignin that has been heat-treated under conditions of 140°C or higher and 220°C or lower for 2 hours or higher and 10 hours or lower.
[0013] The present invention [6] includes the resin composition according to any one of the above [1] to [5], in which the thermosetting resin contains a novolac-type phenolic resin.
[0014] The present invention [7] comprises the resin composition according to any one of the above [1] to [6], in which the amount of the lignins is 100 parts by mass or more per 100 parts by mass of the thermosetting resin. Effect of the Invention
[0015] The resin composition of the present invention contains a thermosetting resin and lignins. The solubility of the lignins in N,N-dimethylformamide is equal to or less than a predetermined value. Therefore, the resin composition can provide a molded product having excellent heat resistance and excellent water resistance. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] 1.Resin composition The resin composition of the present invention contains a thermosetting resin and a lignin.
[0017] (1) Thermosetting resin The thermosetting resin is not particularly limited, and may be any known thermosetting resin. For example, the thermosetting resin may be phenolic resin (such as novolac-type phenolic resin and resol-type phenolic resin), epoxy resin, melamine resin, urea resin, unsaturated polyester resin, urethane resin, and benzoguanamine resin. These may be used alone or in combination of two or more. From the viewpoint of achieving both heat resistance and water resistance, the thermosetting resin may preferably be phenolic resin, and more preferably be novolac-type phenolic resin.
[0018] In other words, from the viewpoint of achieving both heat resistance and water resistance, the thermosetting resin preferably contains a phenol resin, more preferably contains a novolac type phenol resin, and further preferably consists of a novolac type phenol resin.
[0019] (2) Lignins Examples of lignins include lignin and modified lignin. That is, the lignins include lignin and / or modified lignin. Hereinafter, lignin refers to unmodified lignin. Modified lignin refers to a modified form of lignin.
[0020] Lignin (unmodified lignin) is a natural product and a polymeric phenolic compound. Lignin contains, for example, guaiacyl lignin (G type), syringyl lignin (S type), and / or p-hydroxyphenyl lignin (H type) as a basic skeleton. Lignin is, for example, naturally occurring lignin and is contained in plants in general. Modified lignin is a modified form of the above lignin (unmodified lignin). More specifically, examples of lignins (unmodified lignin and modified lignin) include soda lignin, sulfite lignin, kraft lignin, carboxylic acid modified lignin, and polyoxyethylene glycol modified lignin.
[0021] Soda lignin is obtained, for example, by digesting plant materials using the soda process. Sulfite lignin is obtained, for example, by digesting plant materials using the sulfite process. Kraft lignin is obtained, for example, by digesting plant materials using the Kraft process. Carboxylic acid modified lignin is obtained by digesting plant materials using carboxylic acid. Polyoxyethylene glycol modified lignin is obtained by digesting plant materials using polyoxyethylene glycol. These can be used alone or in combination of two or more. Plant materials are not particularly limited, and examples include coniferous plants, broadleaf plants, and grass plants. These can be used alone or in combination of two or more.
[0022] From the viewpoint of achieving both heat resistance and water resistance, the lignins are preferably carboxylic acid-modified lignin and polyoxyethylene glycol-modified lignin. That is, the lignins preferably contain carboxylic acid-modified lignin and / or PEG-modified lignin, and more preferably consist of carboxylic acid-modified lignin and / or PEG-modified lignin.
[0023] Carboxylic acid-modified lignin is modified lignin that is contained in black liquor, for example, when a plant material is cooked using a carboxylic acid (carboxylic acid cooking).
[0024] In the carboxylic acid digestion, the type and amount of the carboxylic acid are appropriately selected according to the required physical properties. More specifically, examples of the carboxylic acid include acetic acid, propionic acid, butyric acid, lauric acid, acrylic acid, methacrylic acid, linoleic acid, benzoic acid, 2-phenoxybenzoic acid, and 4-methylbenzoic acid. These can be used alone or in combination of two or more. As the carboxylic acid, acetic acid is preferably used.
[0025] The method of carboxylic acid digestion is not particularly limited. For example, a plant material is mixed with a carboxylic acid to obtain a mixture. If necessary, an inorganic acid is added to the mixture. Examples of inorganic acids include hydrochloric acid and sulfuric acid. Then, the mixture is heated to digest the plant material. This results in pulp and black liquor. In this case, the black liquor contains carboxylic acid-modified lignin. The carboxylic acid-modified lignin is recovered from the black liquor by a known method. The method of obtaining the carboxylic acid-modified lignin is not limited to the above. For example, lignins other than the carboxylic acid-modified lignin can be reacted with a carboxylic acid to obtain the carboxylic acid-modified lignin.
[0026] Polyoxyethylene glycol-modified lignin (PEG-modified lignin) is a modified lignin that is contained in black liquor, for example, when polyoxyethylene glycol (PEG) is used to cook plant material (PEG cooking).
[0027] In the PEG digestion, the type and amount of polyoxyethylene glycol (PEG) are appropriately selected according to the required physical properties. More specifically, from the viewpoint of achieving both heat resistance and water resistance, the number average molecular weight of polyoxyethylene glycol is, for example, 100 or more, preferably 200 or more, more preferably 300 or more, and even more preferably 400 or more, and, for example, 1000 or less, preferably 900 or less, more preferably 800 or less, even more preferably 600 or less, and particularly preferably 500 or less. The number average molecular weight can be determined as a polyoxyethylene glycol-equivalent molecular weight by a known gel permeation chromatography method.
[0028] The method of PEG cooking is not particularly limited. For example, a plant material and PEG are mixed to obtain a mixture. If necessary, the above-mentioned inorganic acid is added to the mixture. Then, the mixture is heated to cook the plant material. This results in pulp and black liquor. In this case, PEG-modified lignin is contained in the black liquor. The PEG-modified lignin is recovered from the black liquor by a known method. The PEG-modified lignin is not particularly limited, but can be produced, for example, in accordance with the method described in JP 2017-197517 A.
[0029] From the viewpoint of achieving both heat resistance and water resistance, the lignins preferably contain modified lignin, and the modified lignin preferably contains carboxylic acid-modified lignin and / or polyoxyethylene glycol-modified lignin. That is, the lignins preferably contain carboxylic acid-modified lignin and / or polyoxyethylene glycol-modified lignin.
[0030] As the lignins, from the viewpoint of achieving both heat resistance and water resistance, a more preferred example is a PEG-modified lignin. That is, the lignins preferably contain a PEG-modified lignin, and more preferably consist of a PEG-modified lignin.
[0031] The lignins have a predetermined N,N-dimethylformamide solubility (DMF solubility). In other words, the solubility (solubility) of the lignins in N,N-dimethylformamide (DMF) is equal to or lower than a predetermined value. In other words, the resin composition contains the lignins having a predetermined N,N-dimethylformamide solubility (DMF solubility).
[0032] More specifically, from the viewpoint of achieving both heat resistance and water resistance, the solubility of lignins in N,N-dimethylformamide (DMF) (DMF solubility) at 25° C. is 50% by mass or less, preferably 45% by mass or less, more preferably 30% by mass or less, even more preferably 25% by mass or less, and particularly preferably 20% by mass or less. The solubility of lignins in N,N-dimethylformamide (DMF) (DMF solubility) at 25° C. is, for example, 0.1% by mass or more, preferably 1% by mass or more, more preferably 5% by mass or more, even more preferably 10% by mass or more, and particularly preferably 15% by mass or more.
[0033] When the solubility of the lignins in N,N-dimethylformamide (DMF) (DMF solubility) is within the above range, a molded article (described later) having excellent heat resistance and excellent water resistance can be obtained.
[0034] The dissolution rate (solubility) of lignins in N,N-dimethylformamide (DMF) is defined as the ratio of lignins that dissolve in N,N-dimethylformamide (DMF) when 1 g of lignins is mixed with 10 g of DMF at 25° C. More specifically, the dissolution rate of lignins in N,N-dimethylformamide (DMF) (DMF solubility) is measured in accordance with the examples described later.
[0035] The solubility in N,N-dimethylformamide (DMF) (DMF solubility) can be adjusted, for example, by heat treating the lignins.
[0036] For example, if the lignin and / or modified lignin is not heat-treated (heated) after digestion (recovery), the unheated (unheated) lignin and / or the unheated (unheated) modified lignin does not have the above-mentioned DMF solubility rate.
[0037] More specifically, when the lignin and / or modified lignin is not heat-treated (heated) after digestion (recovery), the DMF solubility of the unheated (unheated) lignin and / or the unheated (unheated) modified lignin exceeds, for example, 50% by mass, preferably 70% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, and particularly preferably 99% by mass or more. The DMF solubility is usually 100% by mass or less.
[0038] In contrast, when the lignin and / or modified lignin is heat-treated (heated) after digestion (recovery), the DMF solubility of the heat-treated (heated) lignin and / or the heat-treated (heated) modified lignin is adjusted to be within the above range.
[0039] Therefore, from the viewpoint of achieving both heat resistance and water resistance, the lignins preferably do not contain non-heat-treated lignins, but contain heat-treated lignins. That is, the lignins preferably do not contain non-heat-treated lignin and non-heat-treated modified lignin, but contain heat-treated lignin and / or heat-treated modified lignin. The lignins are more preferably composed of heat-treated lignin and / or heat-treated modified lignin.
[0040] Furthermore, from the viewpoint of achieving both heat resistance and water resistance, the lignins more preferably contain heat-treated PEG-modified lignin, and particularly preferably consist of heat-treated PEG-modified lignin.
[0041] In the following, lignins (lignin and / or modified lignin) that have not been heat-treated may be referred to as unheated lignins (unheated lignin and / or unheated modified lignin).
[0042] Furthermore, heat-treated lignins (lignin and / or modified lignin) may be referred to as heated lignins (heated lignin and / or heat-modified lignin).
[0043] The heat treatment method is not particularly limited. A known heat treatment device is used for the heat treatment. Examples of the heat treatment device include a blower dryer and a heating furnace, and preferably a blower dryer.
[0044] The heat treatment conditions are appropriately set according to the type of lignins so that the DMF solubility of the lignins is adjusted to the above range. For example, when the lignins contain PEG-modified lignin, the heat treatment temperature is, for example, 100°C or higher, preferably 120°C or higher, more preferably 140°C or higher. When the lignins contain PEG-modified lignin, the heat treatment temperature is, for example, 250°C or lower, preferably 240°C or lower, more preferably 220°C or lower, even more preferably 200°C or lower, and particularly preferably 180°C or lower. When the lignins contain PEG-modified lignin, the heat treatment time is, for example, 0.1 hours or more, preferably 0.5 hours or more, more preferably 1 hour or more, even more preferably 1.5 hours or more, and particularly preferably 2 hours or more. Furthermore, when the lignins contain PEG-modified lignin, the heat treatment time is, for example, 24 hours or less, preferably 18 hours or less, more preferably 12 hours or less, even more preferably 10 hours or less, and particularly preferably 8 hours or less.
[0045] When the lignins contain PEG-modified lignin and the heat treatment temperature and heat treatment time are within the above ranges, the DMF solubility of the lignins can be adjusted to the above ranges. Therefore, a molded product (described later) having excellent heat resistance and excellent water resistance can be obtained. In other words, from the viewpoint of achieving both heat resistance and water resistance, the lignins more preferably contain PEG-modified lignin heat-treated under the above heat treatment conditions. The lignins particularly preferably consist of PEG-modified lignin heat-treated under the above heat treatment conditions.
[0046] (3) Additives The resin composition may contain additives. The additives are not particularly limited, and known additives may be used. Examples of additives include curing agents, fillers, release agents, colorants, plasticizers, and stabilizers. These may be used alone or in combination of two or more. The additives preferably include curing agents, fillers, and release agents.
[0047] The curing agent is selected depending on, for example, the type of thermosetting resin. For example, when a phenolic resin is used as the thermosetting resin, a phenolic resin curing agent is preferably used as the curing agent. The phenolic resin curing agent is not particularly limited, but examples thereof include hexamethylenetetramine, methylolmelamine, and methylolurea. These can be used alone or in combination of two or more kinds. The phenolic resin curing agent is preferably hexamethylenetetramine.
[0048] Examples of the filler include wood flour, pulp, and glass fiber. These can be used alone or in combination of two or more. Preferred examples of the filler include wood flour and glass fiber. From the viewpoint of heat resistance, more preferred examples are wood flour. From the viewpoint of water resistance, more preferred examples are glass fiber.
[0049] The release agent may be, for example, a metal soap. Examples of the metal soap include calcium stearate, magnesium stearate, and zinc stearate. These may be used alone or in combination of two or more. A preferred example of the metal soap is zinc stearate.
[0050] (4) Method for producing resin composition The resin composition is produced, for example, as a mixture of a thermosetting resin and a lignin. The resin composition is preferably produced as a mixture of a thermosetting resin, a lignin, and an additive.
[0051] More specifically, in the production of the resin composition, a thermosetting resin and lignins having the above-mentioned DMF solubility are first prepared. The lignins having the above-mentioned DMF solubility are obtained, for example, by heat-treating unheated lignins as described above.
[0052] Next, in this method, the thermosetting resin and the lignins are kneaded (mixed). Furthermore, additives are added to the thermosetting resin and the lignins as necessary.
[0053] The mass ratio of the thermosetting resin to the lignins is appropriately set according to the desired physical properties. For example, the amount of the lignins is, for example, 10 parts by mass or more, preferably 50 parts by mass or more, more preferably 100 parts by mass or more, relative to 100 parts by mass of the thermosetting resin. Also, the amount of the lignins is, for example, 1000 parts by mass or less, preferably 500 parts by mass or less, more preferably 300 parts by mass or less, relative to 100 parts by mass of the thermosetting resin.
[0054] The kneading method is not particularly limited. For example, a known kneader can be used. Examples of the kneader include a single screw extruder, a multi-screw extruder, a roll kneader, a kneader, a Henschel mixer, and a Banbury mixer.
[0055] The kneading conditions are not particularly limited. For example, the kneading temperature is, for example, 80°C or higher, preferably 90°C or higher, and more preferably 100°C or higher. The kneading temperature is, for example, 180°C or lower, preferably 170°C or lower, and more preferably 160°C or lower. The kneading time is, for example, 3 minutes or higher, preferably 5 minutes or higher. The kneading time is, for example, 30 minutes or lower, and preferably 20 minutes or lower.
[0056] This results in a resin composition containing a thermosetting resin and lignins.
[0057] The resin composition may further contain the above-mentioned additives as necessary. The content of the additives is appropriately set depending on the purpose and application.
[0058] For example, when a curing agent is used as an additive, the amount of the curing agent is, for example, 1 part by mass or more, preferably 2 parts by mass or more, relative to 100 parts by mass of the thermosetting resin. Also, the amount of the curing agent is, for example, 100 parts by mass or less, preferably 50 parts by mass or less, relative to 100 parts by mass of the thermosetting resin.
[0059] Furthermore, for example, when a filler is used as an additive, the amount of the filler is, for example, 10 parts by mass or more, preferably 20 parts by mass or more, relative to 100 parts by mass of the thermosetting resin. Also, the amount of the filler is, for example, 300 parts by mass or less, preferably 200 parts by mass or less, relative to 100 parts by mass of the thermosetting resin.
[0060] In addition, for example, when a release agent is used as an additive, the amount of the release agent is, for example, 0.01 parts by mass or more, preferably 0.1 parts by mass or more, relative to 100 parts by mass of the thermosetting resin, and the amount of the release agent is, for example, 50 parts by mass or less, preferably 20 parts by mass or less, relative to 100 parts by mass of the thermosetting resin.
[0061] The timing of adding the additive is not particularly limited. The additive may be added to, for example, the thermosetting resin and / or the lignin in advance. The additive may also be mixed at the same time as, for example, the thermosetting resin and the lignin when they are mixed. The additive may also be added to the mixture of the thermosetting resin and the lignin after mixing the thermosetting resin and the lignin.
[0062] This results in a resin composition containing the thermosetting resin, the lignins, and the additives.
[0063] (5) Effects The resin composition contains a thermosetting resin and lignins. The solubility of the lignins in N,N-dimethylformamide is equal to or less than a predetermined value. Therefore, the resin composition can be used to obtain a molded product having excellent heat resistance and excellent water resistance.
[0064] Therefore, the above-mentioned resin composition is suitably used in the production of molded articles.
[0065] 2. Molded products (1) Manufacturing of molded products In producing a molded product, the resin composition is molded by a known molding method for molding a thermosetting resin, more specifically, transfer molding and compression molding.
[0066] The molding conditions are not particularly limited and are appropriately set according to the purpose and application. More specifically, the molding temperature is, for example, 120°C or higher, preferably 150°C or higher. The molding temperature is, for example, 250°C or lower, preferably 200°C or lower. The molding time is, for example, 1 minute or longer, preferably 5 minutes or longer. The molding time is, for example, 30 minutes or shorter, preferably 15 minutes or shorter.
[0067] In this way, a molded article is produced. The molded article is cured, if necessary.
[0068] The curing conditions are not particularly limited and are appropriately set according to the purpose and use. More specifically, the curing temperature is, for example, 120 °C or higher, preferably 150 °C or higher. Also, the curing temperature is, for example, 250 °C or lower, preferably 200 °C or lower. The curing time is, for example, 30 minutes or longer, preferably 60 minutes or longer. Also, the curing time is, for example, 300 minutes or shorter, preferably 150 minutes or shorter.
[0069] (2) Function and effect The above-mentioned molded article is obtained by molding the above-mentioned resin composition. The above-mentioned resin composition contains a thermosetting resin and lignins. And the dissolution rate of lignins in N,N-dimethylformamide is below a predetermined value. Therefore, the above-mentioned molded article has excellent heat resistance and excellent water resistance.
[0070] Therefore, the above-mentioned molded article is widely used in various industrial fields where both heat resistance and water resistance are required. Such industrial fields include, for example, the field of electrical parts, the field of automotive parts, the field of building materials, and the field of daily necessities.
Examples
[0071] Next, the present invention will be described based on examples and comparative examples, but the present invention is not limited by the following examples. Note that "parts" and "%" are based on mass unless otherwise specified. Also, the specific numerical values such as the blending ratio (content ratio), physical property values, parameters, etc. used in the following description can be replaced with the upper limit values (numerical values defined as "below" and "less than") or lower limit values (numerical values defined as "above" and "exceeding") of the corresponding blending ratio (content ratio), physical property values, parameters, etc. described in the above "Mode for Carrying Out the Invention".
[0072] 1. PEG-modified lignin Production Example 1 (unheated PEG200-modified lignin) <Production of PEG-modified lignin> Lignin modified with polyethylene glycol having a number average molecular weight of 200 (hereinafter referred to as PEG200-modified lignin) was produced by the following method.
[0073] That is, 230 parts by mass of commercially available polyethylene glycol having a number average molecular weight of 200 (hereinafter referred to as PEG200) and 0.69 parts by mass of sulfuric acid as an acid catalyst (0.3 parts by mass with respect to 100 parts by mass of PEG200) were placed in a reaction vessel and stirred. Next, 46 parts by mass of absolutely dry Japanese cedar wood powder was put into the reaction vessel, the temperature was raised to 140 °C under normal pressure, and the mixture was reacted for 90 minutes with stirring. Next, the reaction vessel was cooled, and after confirming that the temperature had dropped to 40 °C or lower, 280 parts by mass of sodium hydroxide (0.2 mol / L) was added and stirred for 30 minutes. Next, the obtained solid component (pulp) was removed by a filter press, and the solution component was recovered. Next, sulfuric acid was added to the obtained solution component to adjust the pH to 2.0. Thereby, a suspension of PEG200-modified lignin was obtained. Thereafter, PEG200-modified lignin was recovered by centrifugation. Thereby, unheated PEG200-modified lignin was obtained.
[0074] <Measurement of DMF dissolution rate> The DMF dissolution rate of PEG200-modified lignin at 25 °C was measured by the following method.
[0075] First, 1 g of PEG-modified lignin was sampled to obtain a sample. That is, the mass of the sample was set to 1 g. The moisture content of the sample at 105 °C was measured with a moisture meter (HS153, manufactured by Mettler Toledo).
[0076] Next, at 25 °C, 1 g of the sample was mixed with 10 g of N,N-dimethylformamide (DMF), and these were stirred for 10 minutes. Next, the mixture of PEG-modified lignin and DMF was filtered under reduced pressure. In the filtration under reduced pressure, GA-100 glass fiber filter paper manufactured by Advantec was used. Next, 2 g of dimethylformamide was added to the filter paper to wash the filtration residue. Next, the filter paper and the filtration residue were dried.
[0077] Thereafter, the mass of the filtration residue was measured at 25° C. Then, the DMF solubility of the sample (PEG200-modified lignin) was calculated using the following formula. The results are shown in Table 1.
[0078]
number
[0079] Production Example 2 (Unheated PEG400-modified lignin) An unheated PEG400-modified lignin was obtained in the same manner as in Production Example 1, except that polyethylene glycol having a number average molecular weight of 400 (hereinafter, PEG400) was used instead of polyethylene glycol having a number average molecular weight of 200.
[0080] The DMF solubility of the PEG400-modified lignin at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 1.
[0081] Production Example 3 (Unheated PEG600-modified lignin) An unheated PEG600-modified lignin was obtained in the same manner as in Production Example 1, except that polyethylene glycol having a number average molecular weight of 600 (hereinafter, referred to as PEG600-) was used instead of polyethylene glycol having a number average molecular weight of 200.
[0082] The DMF solubility of the PEG600-modified lignin at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 1.
[0083] 2. Heat-modified lignin Production Example 4 (Heated PEG200 Modified Lignin) The unheated PEG200-modified lignin obtained in Production Example 1 was heat-treated at 180° C. for 4 hours using a blower dryer. This resulted in a heat-treated (180° C.×4 hours) PEG200-modified lignin (heated PEG200 lignin).
[0084] The DMF solubility of the heat-treated PEG200-modified lignin (heated PEG200 lignin) at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 2.
[0085] Production Example 5 (Heated PEG400 Modified Lignin) The unheated PEG400-modified lignin obtained in Production Example 2 was heat-treated at 180° C. for 4 hours. This resulted in a heat-treated (180° C.×4 hours) PEG400-modified lignin (heated PEG400 lignin).
[0086] The DMF solubility of the heat-treated PEG400-modified lignin (heated PEG400 lignin) at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 2.
[0087] Production Example 6 (Heated PEG600 modified lignin) The unheated PEG600-modified lignin obtained in Production Example 6 was heat-treated at 180° C. for 4 hours. This resulted in a heat-treated (180° C.×4 hours) PEG600-modified lignin (heated PEG600 lignin).
[0088] The DMF solubility of the heat-treated PEG600-modified lignin (heated PEG600 lignin) at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 2.
[0089] Production Examples 7 to 10 (Heated PEG400 Modified Lignin) A heat-treated PEG400-modified lignin (heated PEG400 lignin) was obtained in the same manner as in Production Example 5, except that the heat treatment temperature and heat treatment time were changed as shown in Table 3.
[0090] The DMF solubility of the heat-treated PEG400-modified lignin (heated PEG400 lignin) at 25° C. was calculated in the same manner as in Production Example 1. The results are shown in Table 3.
[0091] 3.Resin composition Examples 1 to 10 and Comparative Examples 1 to 6 According to the formulations shown in Tables 1 to 3, novolac-type phenolic resin (manufactured by Asahi Organic Chemicals Co., Ltd.), lignins of Production Examples 1 to 10, wood flour (manufactured by Asahi Organic Chemicals Co., Ltd.) as a filler, hexamethylenetetramine (Hexamine, manufactured by Lignite Corporation) as a curing agent, and zinc stearate (manufactured by Wako Pure Chemical Industries, Ltd.) as a release agent were sequentially blended and kneaded with two heated rolls at 100°C for 5 minutes to obtain a resin composition.
[0092] 4. Evaluation The resin compositions obtained in each of the Examples and Comparative Examples were transfer molded at 170° C. for 15 minutes to obtain molded articles. The molded articles were then heat-cured at 180° C. for 2 hours. The molded articles were then evaluated by the following methods.
[0093] (1) Glass transition temperature (heat resistance) The solid dynamic viscoelasticity was measured using Rheogel-E4000 (manufactured by UBM) (frequency 1 Hz, heating rate 2°C / min). The peak temperature of the obtained tan δ curve was determined as the glass transition temperature (Tg).
[0094] (2) Water absorption rate (water resistance) The initial mass (dry mass) of the molded article was measured. The molded article was then immersed in boiling water for 2 hours. Thereafter, the mass (absorbed water mass) and the increase in mass of the molded article were measured. The water absorption rate of the molded article was calculated using the following formula.
[0095] Water absorption rate (mass%) = 100 x (mass increase after immersion in boiling water / dry mass)
[0096] [Table 1]
[0097] [Table 2]
[0098] [Table 3]
Claims
1. Contains a thermosetting resin and lignins, The resin composition, wherein the solubility of the lignins in N,N-dimethylformamide at 25°C is 50% by mass or less.
2. The resin composition according to claim 1 , wherein the lignins contain lignin and / or modified lignin.
3. The resin composition according to claim 2 , wherein the lignins contain heat-treated lignin and / or heat-treated modified lignin.
4. The resin composition according to claim 3 , wherein the modified lignin contains a carboxylic acid-modified lignin and / or a polyoxyethylene glycol-modified lignin.
5. The resin composition according to claim 1 , wherein the lignins contain polyoxyethylene glycol-modified lignin that has been heat-treated under conditions of 140° C. or higher and 220° C. or lower for 2 hours or higher and 10 hours or lower.
6. The resin composition according to claim 1 , wherein the thermosetting resin contains a novolac-type phenolic resin.
7. The resin composition according to claim 1 , wherein the amount of the lignins is 100 parts by mass or more relative to 100 parts by mass of the thermosetting resin.
Citation Information
Patent Citations
Resin composition
JP2021123717A