Laminate, packaging bag, and method for manufacturing laminate
Patent Information
- Application Number
- JP2023052929
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
【0026】 本開示によれば、外観及び強度物性に優れる積層体を提供することができる。また、本開示によれば、その積層体を含む包装袋を提供することができる。また、本開示によれば、その積層体を製造することができる。
Smart Images

Figure 2024141339000001_ABST
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a laminate, a packaging bag, and a method for manufacturing the laminate. [Background technology]
[0002] As part of efforts to address the environmental issues, packaging bags using plastic films (e.g., flexible bags) are becoming more and more popular as a replacement for bottles and cans. In many cases, flexible bags are made of a laminate of two or more films bonded together with an adhesive to improve their performance, such as strength, water resistance, moisture resistance, gas barrier properties including oxygen, and heat resistance.
[0003] When a packaging bag includes a printed layer, the printed layer is usually provided on the inner surface of a laminate that constitutes the packaging bag from the standpoint of preventing the ink from being scraped off due to wear and preventing ink transfer when multiple packaging bags are stacked, and a laminate with an outer layer / printed layer / adhesive layer / middle layer / adhesive layer / inner layer is commonly known (see, for example, Patent Document 1, etc.).
[0004] As the range of uses for flexible packaging bags expands, efforts are being made to improve the performance of adhesives used to bond films. For example, Patent Document 2 proposes a solvent-free adhesive composition that can form a boilable laminate. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Patent Publication No. 2004-238050 [Patent Document 2] Patent No. 7030271 Summary of the Invention [Problem to be solved by the invention]
[0006] Usually, when forming a printing layer, multiple colors of ink are printed on top of each other to create a pattern, but in this case, a step occurs between the areas where the ink overlaps a lot and the areas where the ink overlaps less. If such a step exists on the film surface that will be coated with the adhesive, the amount of adhesive used in general lamination will not be enough to fill the step, making it difficult to apply the adhesive evenly. This makes it easy for poor adhesion, air bubbles to get caught in the step, and appearance defects such as orange peel to occur.
[0007] In particular, solvent-free adhesives generally have high viscosities, so air bubbles contained in the adhesive during the laminate manufacturing process cannot escape from the system and tend to remain in the adhesive after bonding (curing reaction), i.e., in the adhesive layer. Such air bubbles not only deteriorate the appearance, but also cause a decrease in strength properties such as lamination strength and impact strength.
[0008] The present disclosure has been made to solve such problems, and has an object to provide a laminate having excellent appearance and strength. It is also an object to provide a packaging bag including the laminate. It is also an object to provide a manufacturing method for the laminate. [Means for solving the problem]
[0009] As a result of intensive research by the present inventors into the above problem, it was found that air bubbles contained in the adhesive tend to increase in size even after being sandwiched between films due to the flow of the adhesive, and as a result, the air bubbles are difficult to escape from the film. In addition, it was found that the adhesive is particularly prone to flow when stretched films are bonded together. From this knowledge, it was found that even if there is a step on the film surface due to a printed layer, the flow of the adhesive can be suppressed by bonding a stretched film and a non-stretched film, and as a result, the increase in the diameter of the air bubbles can be suppressed, and the air bubbles can be easily escaped from the film. The present disclosure has been made based on this knowledge. That is, the present disclosure provides the following [1] to
[13] .
[0010] [1] A laminate comprising: a first stretched film having a printed layer formed on one side thereof; a first adhesive layer arranged on the side of the first stretched film opposite the printed layer; a second adhesive layer arranged on the printed layer side of the first stretched film; a second stretched film arranged on the side of the first stretched film opposite the printed layer via the first adhesive layer; and a non-stretched film arranged on the printed layer side of the first stretched film via the second adhesive layer.
[0011] In this laminate, the second stretched film and the non-stretched film are arranged on both sides of the first stretched film on which the printed layer is formed, so that the occurrence of scraping of the printed layer, transfer of the printed layer, etc. can be suppressed. Here, a step is formed by the printed layer on the printed layer side of the first stretched film. However, since the non-stretched film is arranged on the printed layer side of the first stretched film via the second adhesive layer, when the first stretched film and the non-stretched film are bonded together in the production of the laminate, the flow of the second adhesive that becomes the second adhesive layer is suppressed, so that air bubbles contained in the adhesive are easily discharged from the step of the printed layer, and the step of the printed layer is easily filled with the adhesive. Therefore, it is possible to obtain an excellent strength property and appearance.
[0012] [2] The laminate according to [1], wherein the first adhesive layer and the second adhesive layer are cured products of a solventless adhesive.
[0013] [3] The laminate according to [1], wherein the first adhesive layer and the second adhesive layer are cured products of a solventless two-component curing polyurethane adhesive.
[0014] Solvent-free adhesives such as two-component curing polyurethane adhesives have a higher viscosity than solvent-based adhesives. However, even if the first adhesive layer and the second adhesive layer are cured products of solvent-free adhesives such as two-component curing polyurethane adhesives, by disposing a non-stretched film on the printed layer side of the first stretched film via the second adhesive layer, the flow of the adhesive that will become the second adhesive layer in the production of the laminate is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer, and the steps of the printed layer are easily filled with the adhesive. This makes it possible to obtain excellent strength properties and appearance.
[0015] [4] The laminate according to any one of [1] to [3], wherein at least one of the first stretched film and the second stretched film has gas barrier properties.
[0016] [5] The laminate according to any one of [1] to [4], wherein at least one of the first stretched film and the second stretched film has an inorganic vapor deposition layer.
[0017] When the film has a gas barrier property or an inorganic vapor deposition layer, air bubbles are unlikely to pass through the film. However, even if at least one of the first stretched film and the second stretched film has a gas barrier property or an inorganic vapor deposition layer, the unstretched film is bonded to the printed layer side of the first stretched film via the second adhesive layer, so that the flow of the adhesive that becomes the second adhesive layer in the production of the laminate is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer, and the steps of the printed layer are easily filled with the adhesive. Therefore, it is possible to obtain an excellent strength property and appearance.
[0018] [6] The laminate according to any one of [1] to [5], wherein at least one of the first stretched film and the second stretched film contains at least one of nylon, polypropylene, and polyethylene terephthalate.
[0019] [7] A packaging bag produced by forming a packaging film including the laminate described in any one of [1] to [6].
[0020] [8] The packaging bag described in [7], which is for boiling or retorting.
[0021] [9] A method for manufacturing a laminate, comprising: a stretched film laminating process for placing a second stretched film, via a first adhesive, on the side opposite the printed layer of a first stretched film having a printed layer formed on one side thereof; and a non-stretched film laminating process for placing a non-stretched film, via the second adhesive, on the printed layer side of the first stretched film.
[0022] In this method for producing a laminate, a second stretched film and a non-stretched film are disposed on both sides of a first stretched film on which a printed layer is formed, so that scraping of the printed layer, transfer of the printed layer, etc. can be suppressed. Here, a step is formed by the printed layer on the printed layer side of the first stretched film. However, since a non-stretched film is disposed on the printed layer side of the first stretched film via a second adhesive, the flow of the second adhesive is suppressed, so that air bubbles contained in the adhesive are easily discharged from the step of the printed layer, and the step of the printed layer is easily filled with the adhesive. As a result, a laminate with excellent strength properties and appearance can be obtained.
[0023]
[10] The method for producing a laminate according to [9], wherein the stretched film laminating step is carried out after the non-stretched film laminating step. In this production method, by carrying out the stretched film laminating step after the non-stretched film laminating step, a laminate having a more excellent appearance can be obtained.
[0024]
[11] The method for producing a laminate according to [9] or
[10] , in which a solvent-free adhesive is used as the first adhesive and the second adhesive. A solvent-free adhesive has a higher viscosity than a solvent-based adhesive. However, even if a solvent-free adhesive is used as the first adhesive and the second adhesive, by disposing a non-stretched film on the printed layer side of the first stretched film via the second adhesive, the flow of the second adhesive is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer, and the steps of the printed layer are easily filled with the adhesive. Therefore, a laminate having excellent strength properties and appearance can be obtained.
[0025]
[12] The method for producing a laminate according to any one of [9] to
[11] , wherein at least one of the first stretched film and the second stretched film has gas barrier properties. A film having gas barrier properties does not allow air bubbles to pass through. However, even if at least one of the first stretched film and the second stretched film has gas barrier properties, by disposing a non-stretched film on the printed layer side of the first stretched film via a second adhesive, the flow of the second adhesive is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer, and the steps of the printed layer are easily filled with the adhesive. Therefore, a laminate having excellent strength properties and appearance can be obtained. Effect of the Invention
[0026] According to the present disclosure, it is possible to provide a laminate having excellent appearance and strength. According to the present disclosure, it is also possible to provide a packaging bag including the laminate. According to the present disclosure, it is also possible to manufacture the laminate. [Brief description of the drawings]
[0027] [Figure 1] FIG. 1 is a schematic cross-sectional view showing one embodiment of a laminate according to the present disclosure. [Diagram 2] FIG. 2 is an enlarged schematic cross-sectional view of a first stretched film in the laminate shown in FIG. [Diagram 3] FIG. 3 is a schematic cross-sectional view showing a method for producing a laminate. [Figure 4] FIG. 4 is a schematic cross-sectional view showing a method for producing a laminate. [Diagram 5] FIG. 5 is a schematic cross-sectional view showing a method for producing a laminate. [Figure 6] FIG. 6 is a schematic cross-sectional view showing the laminates of Examples 1 to 5. [Figure 7] FIG. 7 is a schematic cross-sectional view showing the laminates of Comparative Examples 1 to 4. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0028] In this specification, a numerical range indicated using "~" indicates a range including the numerical values described before and after "~" as the minimum and maximum values, respectively. In addition, unless specifically stated otherwise, the units of the numerical values described before and after "~" are the same. In the numerical ranges described in stages in this specification, the upper limit or lower limit of a certain numerical range may be replaced with the upper limit or lower limit of a numerical range of another stage. In addition, in the numerical ranges described in this specification, the upper limit or lower limit of the numerical range may be replaced with a value shown in the examples. In addition, the upper limit and lower limit values described individually can be combined arbitrarily.
[0029] Hereinafter, embodiments of the present disclosure will be described in detail with reference to the drawings where necessary. However, the present disclosure is not limited to the following embodiments.
[0030] <Laminate> Fig. 1 is a schematic cross-sectional view showing one embodiment of a laminate of the present disclosure. The laminate 1 shown in Fig. 1 is a laminate obtained by laminating a first stretched film 2, a second stretched film 3, and a non-stretched film 4. The laminate 1 includes a first adhesive layer 5 that bonds the first stretched film 2 and the second stretched film 3, and a second adhesive layer 6 that bonds the first stretched film 2 and the non-stretched film 4. In the laminate 1, the non-stretched film 4, the second adhesive layer 6, the first stretched film 2, the first adhesive layer 5, and the second stretched film 3 are laminated in this order. The thickness of the laminate 1 is, for example, 30 to 100 µm.
[0031] (First oriented film) Fig. 2 is a schematic cross-sectional view showing an enlarged view of the first stretched film in the laminate shown in Fig. 1. As shown in Figs. 1 and 2, the first stretched film 2 has a base film 21 which is a stretched film, and a printed layer 22 formed on the base film 21. That is, the first stretched film 2 can be said to be a film with the printed layer 22. There may be an area on the base film 21 where the printed layer 22 is not formed. That is, the printed layer 22 may be provided on at least a part of the base film 21.
[0032] The base film 21 may be any film on which the printed layer 22 can be formed, and may be, for example, a resin film such as a biaxially stretched resin film. The resin film is usually transparent so that a pattern can be displayed by the printed layer 22. Examples of the resin film include a biaxially stretched film of at least one of polyesters such as polyethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, polyamides such as nylon, polypropylene, polystyrene, polyimide, polyvinyl alcohol, polyvinyl chloride, and ethylene-vinyl alcohol copolymers, and a composite film in which two or more of these films are laminated. The base film 21 may include a barrier layer such as an aluminum foil, a metal deposition layer, or a transparent deposition layer of an inorganic oxide (deposition layer of an inorganic oxide). That is, the first stretched film 2 may be a barrier film including the printed layer 22. Depending on the application, the base film 21 may also include other functional layers such as a concealment layer.
[0033] The thickness of the base film 21 is, for example, 10 to 60 μm.
[0034] The printed layer 22 is a layer formed of one or more color inks. Note that the color inks used as materials for printing and the color inks contained in the printed layer may have different compositions due to the influence of the layer formation process, such as drying and curing, but for convenience, these will be collectively referred to as color inks in this specification.
[0035] The color ink contains, for example, a pigment and a binder resin. As the color ink, general gravure ink, flexographic ink, offset ink, and ink for digital printing can be used. When the color ink is an oil-based gravure ink, the binder resin can be a mixture of a urethane resin and a vinyl chloride-vinyl acetate copolymer resin. The color ink may contain various additives other than the pigment and the binder resin, and a solvent (for example, a volatile organic solvent). As the color ink, for example, vegetable oil ink, biomass ink, and the like can also be used.
[0036] (Second Stretched Film) The second stretched film 3 is disposed on the side of the first stretched film 2 opposite the printed layer 22 via a first adhesive layer 5. In other words, the second stretched film 3 is attached to the side of the first stretched film 2 opposite the printed layer 22 by the first adhesive layer 5.
[0037] The second stretched film 3 may be a known impact-resistant film used for packaging bags. Examples of the impact-resistant film include a biaxially oriented nylon film, a biaxially oriented polypropylene film, and a biaxially oriented polyethylene terephthalate film.
[0038] The thickness of the second stretched film 3 is, for example, 15 to 30 μm.
[0039] (Non-oriented film) The non-stretched film 4 is disposed on the printed layer 22 side of the first stretched film 2 via the second adhesive layer 6. That is, the non-stretched film 4 is attached to the surface of the first stretched film 2 on the printed layer 22 side by the second adhesive layer 6. Examples of the non-stretched film 4 include a non-stretched polypropylene film and a non-stretched polyethylene film.
[0040] The thickness of the unstretched film 4 is, for example, 15 to 60 μm. (First adhesive layer and second adhesive layer)
[0041] The first adhesive layer 5 and the second adhesive layer 6 are cured products of coating films obtained by adhesives such as inorganic solvent-based adhesives. The first adhesive layer 5 can be formed, for example, by applying an adhesive to at least one surface of the second stretched film 3, bonding the second stretched film 3 to the surface of the first stretched film 2 opposite the printed layer 22, and then curing the adhesive. The second adhesive layer 6 can be formed, for example, by applying an adhesive to at least one surface of the non-stretched film 4, bonding the non-stretched film 4 to the surface of the first stretched film 2 facing the printed layer 22, and then curing the adhesive.
[0042] Examples of solvent-free adhesives include two-component curing polyurethane adhesives in which a base material such as polyester polyol, polyether polyol, or acrylic polyol is treated with an aromatic or aliphatic isocyanate compound having two or more functional groups as a curing agent. In such adhesives, the components react with each other by heating or the like (for example, the hydroxyl group of the base material reacts with the isocyanate group of the curing agent) to harden the adhesive layer, forming an adhesive layer. That is, the adhesive layer is a (reaction) cured product of the two-component curing polyurethane adhesive, which is a solvent-free adhesive. The fact that the adhesive layer is formed using a solvent-free adhesive rather than a solvent-based adhesive can be analyzed, for example, by Fourier transform infrared spectroscopy.
[0043] The first adhesive layer 5 has a thickness of, for example, 0.3 to 5.0 μm. The second adhesive layer 6 has a thickness of, for example, 0.3 to 5.0 μm. In the first stretched film 2, when there is a region on the base film 21 where the printed layer 22 is not formed, the second adhesive layer 6 has a thickness from the base film 21 to the non-stretched film 4. In the first stretched film 2, when there is no region on the base film 21 where the printed layer 22 is not formed, the second adhesive layer 6 has a thickness from the lowest position of the printed layer 22 to the non-stretched film 4. In either case, the thickness of the first adhesive layer 5 and the thickness of the second adhesive layer 6 can be approximately the same.
[0044] Compared to solvent-based adhesives, solvent-free adhesives reduce the environmental impact of the manufacturing process by not using solvents, and can be applied thinly. However, they have poor wettability and are prone to air bubbles remaining between the films when bonding multiple films together, especially if there are steps on the film surface that will be coated with the adhesive.
[0045] In particular, when the first stretched film 2 and / or the second stretched film 3 has an inorganic vapor deposition layer formed thereon for the purpose of improving barrier properties, the air or gas in the bubbles has difficulty permeating the inorganic vapor deposition layer, making it more difficult for the bubbles to pass through the film and be released.
[0046] The present inventors have found that air bubbles contained in the adhesive tend to increase in size even after being sandwiched between films due to the flow of the adhesive, and as a result, the air bubbles are difficult to remove from the film. They have also found that the adhesive is particularly prone to flow when stretched films are bonded together. Based on this knowledge, they have found that even if there is a step on the film surface due to a printed layer, the flow of the adhesive can be suppressed by bonding a stretched film and a non-stretched film together, and as a result, the increase in the diameter of the air bubbles can be suppressed, and the air bubbles can be easily removed from the film. The present disclosure is based on this knowledge.
[0047] In addition, in conventional laminate manufacturing methods and configurations, when an adhesive layer is formed using a solvent-free adhesive, poor appearance and poor adhesion may occur due to steps on the surface of the film. However, in this embodiment, even when an adhesive layer is formed using a solvent-free adhesive, a good appearance and excellent adhesive strength can be obtained.
[0048] The laminate 1 described above can be suitably used, for example, to form a packaging bag (e.g., a soft bag) for packaging contents. Specifically, a packaging bag can be manufactured by laminating two non-stretched films together and processing them into a bag. Examples of contents include liquids such as liquid seasonings, toiletries, soups, and liquid detergents, solids such as stews, and solid-liquid mixtures of liquids and solids such as curry.
[0049] <Method of manufacturing laminate> The method for producing a laminate according to the present disclosure includes a stretched film laminating step of disposing a second stretched film via a first adhesive on the side opposite to the printed layer of a first stretched film having a printed layer formed on one side thereof, and a non-stretched film laminating step of disposing a non-stretched film via a second adhesive on the printed layer side of the first stretched film. The non-stretched film laminating step is performed, for example, before the stretched film laminating step.
[0050] Hereinafter, an example of a method for producing a laminate will be described with reference to FIGS.
[0051] 3 to 5 are schematic cross-sectional views showing a method for producing a laminate. The method for producing a laminate shown in Fig. 3 to 5 includes a step (i) of forming a printed layer 22 including a colored ink layer on a base film 21 to obtain a first stretched film 2, a step (ii) of arranging a non-stretched film 4 on the printed layer 22 side of the first stretched film 2 via a second adhesive 61, and a step (iii) of arranging a second stretched film 3 on the side opposite to the printed layer 22 of the first stretched film 2 via a first adhesive 51.
[0052] (Step (i)) In step (i), a printed layer 22 including a color ink layer is formed on a base film 21 to produce a first stretched film 2 (see FIG. 3). The amount and type of color ink used may be set according to the type of image to be expressed. Drying conditions for the color ink are not particularly limited, and may be set according to the amount of solvent contained in the color ink.
[0053] (Step (ii)) In step (ii), the unstretched film 4, which is an unstretched polyethylene or unstretched polypropylene film, is placed on the printed layer 22 of the first stretched film 2 via a solvent-free second adhesive 61. Specifically, first, the second adhesive 61 is placed (coated) on the unstretched film 4 (see FIG. 3). Next, the surface of the first stretched film 2 on the side of the printed layer 22 is placed on the second adhesive 61 (see FIGS. 3 and 4).
[0054] (Step (iii)) In step (iii), the second stretched film 3 is placed on the surface of the first stretched film 2 opposite the printed layer 22 via a first adhesive 51. Specifically, first, the first adhesive 51 is placed (coated) on the second stretched film 3 (see FIG. 4). Next, the surface of the first stretched film 2 opposite the printed layer 22 is placed on the first adhesive 51 (see FIGS. 4 and 5).
[0055] <Packaging bag> A packaging bag (not shown) according to an embodiment of the present disclosure is a packaging bag (e.g., a soft bag) made by producing a packaging film (not shown) including the laminate 1 of the above embodiment. Examples of the packaging bag include a flat pouch-shaped packaging bag and a self-supporting packaging bag (standing pouch). Such a packaging bag may be for boiling or retorting.
[0056] The flat pouch-shaped packaging bag may be, for example, one sheet of packaging film folded in half so that the non-stretched films 4 face each other and then heat-sealed on three sides to form a bag shape, or two sheets of packaging film stacked together so that the non-stretched films 4 face each other and then heat-sealed on all four sides to form a bag shape.
[0057] In this manner, in the laminate 1 according to the present embodiment, the second stretched film 3 and the non-stretched film 4 are disposed on both sides of the first stretched film 2 on which the printed layer 22 is formed, so that the occurrence of scraping of the printed layer 22, transfer of the printed layer 22, etc. can be suppressed. Here, a step is formed by the printed layer 22 on the printed layer 22 side of the first stretched film 2. However, since the non-stretched film 4 is disposed on the printed layer 22 side of the first stretched film 2 via the second adhesive layer 6, when the first stretched film 2 and the non-stretched film 4 are bonded together in the manufacture of the laminate 1, the flow of the second adhesive 61 that becomes the second adhesive layer 6 is suppressed, so that air bubbles contained in the adhesive are easily discharged from the step of the printed layer 22, and the step of the printed layer 22 is easily filled with the adhesive. Therefore, it is possible to obtain an excellent strength property and appearance.
[0058] In addition, solvent-free adhesives such as two-component curing polyurethane adhesives have a higher viscosity than solvent-based adhesives. However, even if the first adhesive layer 5 and the second adhesive layer 6 are cured products of solvent-free adhesives such as two-component curing polyurethane adhesives, the non-stretched film 4 is disposed on the printed layer 22 side of the first stretched film 2 via the second adhesive layer 6, so that the flow of the second adhesive 61 that becomes the second adhesive layer 6 in the production of the laminate 1 is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer 22, and the steps of the printed layer 22 are easily filled with the adhesive. This makes it possible to obtain excellent strength properties and appearance.
[0059] In addition, if the film has gas barrier properties or an inorganic deposition layer, air bubbles are unlikely to pass through the film. However, even if at least one of the first stretched film 2 and the second stretched film 3 has gas barrier properties or an inorganic deposition layer, the unstretched film 4 is bonded to the printed layer 22 side of the first stretched film 2 via the second adhesive layer 6, so that the flow of the second adhesive 61 that becomes the second adhesive layer 6 in the production of the laminate 1 is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer 22, and the steps of the printed layer 22 are easily filled with the adhesive. Therefore, the laminate can have excellent strength properties and appearance.
[0060] In the method for producing a laminate according to the present embodiment, the second stretched film 3 and the non-stretched film 4 are disposed on both sides of the first stretched film 2 on which the printed layer 22 is formed, so that scraping of the printed layer 22, transfer of the printed layer 22, and the like can be suppressed. Here, a step is formed by the printed layer 22 on the printed layer 22 side of the first stretched film 2. However, since the non-stretched film 4 is disposed on the printed layer 22 side of the first stretched film 2 via the second adhesive 61, the flow of the second adhesive 61 is suppressed, so that air bubbles contained in the adhesive are easily discharged from the step of the printed layer 22, and the step of the printed layer 22 is easily filled with the adhesive. Therefore, a laminate 1 having excellent strength properties and appearance can be obtained.
[0061] Furthermore, in this method for producing a laminate, a laminate having a more excellent appearance can be obtained by carrying out the non-stretched film laminating step before the stretched film laminating step.
[0062] Furthermore, solvent-free adhesives have a higher viscosity than solvent-based adhesives. However, even if solvent-free adhesives are used as the first adhesive 51 and the second adhesive 61, by disposing the non-stretched film 4 on the printed layer 22 side of the first stretched film 2 via the second adhesive 61, the flow of the second adhesive 61 is suppressed, and air bubbles contained in the adhesive are easily discharged from the steps of the printed layer 22, and the steps of the printed layer 22 are easily filled with the adhesive. Therefore, it is possible to obtain a laminate 1 having excellent strength properties and appearance.
[0063] Furthermore, a film having gas barrier properties does not allow air bubbles to pass through. However, even if at least one of the first stretched film 2 and the second stretched film 3 has gas barrier properties, by disposing the non-stretched film 4 on the printed layer 22 side of the first stretched film 2 via the second adhesive 61, the flow of the second adhesive 61 is suppressed, so that air bubbles contained in the adhesive are easily discharged from the steps of the printed layer 22, and the steps of the printed layer 22 are easily filled with the adhesive. Therefore, a laminate 1 having excellent strength properties and appearance can be obtained.
[0064] Although an embodiment of the laminate, packaging bag, and laminate manufacturing method of the present disclosure has been described above, the laminate, packaging bag, and laminate manufacturing method of the present disclosure are not limited to the above embodiment.
[0065] For example, in the above embodiment, an example of a method for manufacturing a laminate was shown, but the non-stretched film laminating step may be performed after the stretched film laminating step. In addition, in the non-stretched film laminating step, the second adhesive may be placed on the first stretched film so that the surface of the first stretched film facing the printed layer side and the second adhesive face each other, and then the non-stretched film may be placed on the second adhesive. In addition, in the stretched film laminating step, the first adhesive may be placed on the second stretched film, and then the first stretched film may be placed on the first adhesive so that the first adhesive faces the surface of the first stretched film opposite the printed layer. EXAMPLES
[0066] The present disclosure will be described in more detail with reference to the following examples, but the present disclosure is not limited to these examples.
[0067] <Examples 1 to 5> Fig. 6 is a schematic cross-sectional view showing the laminates of Examples 1 to 5. As shown in Fig. 6, in Examples 1 to 5, the laminates of Examples 1 to 5 were produced in the order shown in Table 1 using a printed ONY film in which a printed layer was formed on an ONY film "ONMB-RT" (manufactured by Unitika Ltd.), which is a stretched film, a non-stretched polypropylene film "ZK207" (manufactured by Toray Advanced Film Co., Ltd.), which is a non-stretched film, and a transparent vapor deposition barrier film "GL-ARH" (manufactured by Toppan Printing Co., Ltd.), which is a stretched film. In Fig. 6 and Table 1, the ONY film is shown as "ONY", the printed layer as "ink", the non-stretched polypropylene film as "CPP", the adhesive as "adh", the adhesive layer which is a cured product of the adhesive as "ADH", and the transparent vapor deposition barrier film as "PET".
[0068] [Table 1]
[0069] Example 1 As shown in Table 1, in Example 1, in the first step, a printed layer (ink) was formed on an ONY film (ONY) to obtain a printed ONY film (ONY / ink). The printed layer (ink) was formed by gravure printing colored inks on the ONY film (ONY). As the colored inks, "Rio Alpha White", "Rio Alpha Yellow" and "Rio Alpha Indigo" manufactured by Toyo Ink Co., Ltd. were used.
[0070] In Example 1, as the second step following the first step, a non-oriented polypropylene film (CPP) was laminated onto the surface of the printed layer (ink) of the printed ONY film (ONY / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the non-oriented polypropylene film (CPP), and then the solvent-free adhesive (adh) was placed opposite the surface of the printed layer (ink) of the printed ONY film (ONY / ink), and the non-oriented polypropylene film (CPP) was bonded to the surface of the printed layer (ink) of the printed ONY film (ONY / ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0071] In Example 1, as the third step following the second step, a transparent vapor deposition barrier film (PET) was laminated to the side of the printed ONY film (ONY / ink) opposite the printed layer (ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied to the side of the printed ONY film (ONY / ink) opposite the printed layer (ink), and then the side of the printed ONY film (ONY / ink) opposite the printed layer (ink) was bonded to the transparent vapor deposition barrier film (PET). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0072] Thereafter, the solvent-free adhesive (adh) was cured to obtain a laminate of Example 1, which was formed by laminating in this order an unstretched polypropylene film (CPP), an adhesive layer (ADH) formed by the curing of the solvent-free adhesive (adh), a printed ONY film (ONY / ink), an adhesive layer (ADH) formed by the curing of the solvent-free adhesive (adh), and a transparent vapor deposition barrier film (PET).
[0073] Example 2 In Example 2, in the first step, a printed ONY film (ONY / ink) was obtained in the same manner as in Example 1.
[0074] In Example 2, as the second step following the first step, a non-oriented polypropylene film (CPP) was laminated onto the printed layer (ink) side of the printed ONY film (ONY / ink) in the same manner as in Example 1.
[0075] In Example 2, as the third step following the second step, a transparent vapor deposition barrier film (PET) was laminated onto the side of the printed ONY film (ONY / ink) opposite the printed layer (ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied to the transparent vapor deposition barrier film (PET), and then a transparent vapor deposition barrier film (PET) was attached to the side of the printed ONY film (ONY / ink) opposite the printed layer (ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0076] Thereafter, the solvent-free adhesive (ADH) was cured to obtain a laminate similar to that in Example 1.
[0077] Example 3 In Example 3, in the first step, a printed ONY film (ONY / ink) was obtained in the same manner as in Example 1.
[0078] In Example 3, as the second step following the first step, a non-oriented polypropylene film (CPP) was laminated onto the surface of the printed layer (ink) of the printed ONY film (ONY / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the surface of the printed layer (ink) of the printed ONY film (ONY / ink), and then the surface of the printed layer (ink) of the printed ONY film (ONY / ink) was bonded to the non-oriented polypropylene film (CPP). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0079] In Example 3, as the third step following the second step, a transparent vapor deposition barrier film (PET) was laminated to the side of the printed ONY film (ONY / ink) opposite the printed layer (ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied to the side of the printed ONY film (ONY / ink) opposite the printed layer (ink), and then the side of the printed ONY film (ONY / ink) opposite the printed layer (ink) was bonded to the transparent vapor deposition barrier film (PET). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The solvent-free adhesive (ADH) was then cured to obtain a laminate similar to that of Example 1.
[0080] Example 4 In Example 4, in the first step, a printed ONY film (ONY / ink) was obtained in the same manner as in Example 1.
[0081] In Example 4, as the second step following the first step, a transparent vapor deposition barrier film (PET) was laminated onto the surface of the printed ONY film (ONY / ink) opposite the printed layer (ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the transparent vapor deposition barrier film (PET), and then a transparent vapor deposition barrier film (PET) was attached to the surface of the printed ONY film (ONY / ink) opposite the printed layer (ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0082] In Example 4, as the third step following the second step, a non-oriented polypropylene film (CPP) was laminated onto the surface of the printed layer (ink) of the printed ONY film (ONY / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the non-oriented polypropylene film (CPP), and then the solvent-free adhesive (adh) was placed opposite the surface of the printed layer (ink) of the printed ONY film (ONY / ink), and the non-oriented polypropylene film (CPP) was attached to the surface of the printed layer (ink) of the printed ONY film (ONY / ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0083] Thereafter, the solvent-free adhesive (ADH) was cured to obtain a laminate similar to that in Example 1.
[0084] Example 5 In Example 5, as a first step, a printed ONY film (ONY / ink) was obtained in the same manner as in Example 1. In Example 5, as a second step following the first step, a transparent vapor deposition barrier film (PET) was laminated on the surface opposite to the printed layer (ink) of the printed ONY film (ONY / ink) in the same manner as in Example 4.
[0085] In Example 5, as the third step following the second step, a non-oriented polypropylene film (CPP) was laminated onto the surface of the printed layer (ink) of the printed ONY film (ONY / ink). In this lamination process, the solvent-free adhesive (adh) and the surface of the printed layer (ink) of the printed ONY film (ONY / ink) were coated with the solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh), and then the solvent-free adhesive (adh) and the surface of the printed layer (ink) of the printed ONY film (ONY / ink) were placed opposite each other, and the surface of the printed layer (ink) of the printed ONY film (ONY / ink) was bonded to the non-oriented polypropylene film (CPP). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0086] Thereafter, the solvent-free adhesive (ADH) was cured to obtain a laminate similar to that in Example 1.
[0087] <Comparative Examples 1 to 4> Fig. 7 is a schematic cross-sectional view showing the laminates of Comparative Examples 1 to 4. As shown in Fig. 7, in Comparative Examples 1 to 4, the laminates of Comparative Examples 1 to 4 were produced in the order shown in Table 2 using a printed transparent vapor deposition barrier film in which a printing layer was formed on a transparent vapor deposition barrier film "GL-ARH" (manufactured by Toppan Printing Co., Ltd.), which is a stretched film, a non-stretched polypropylene film "ZK207" (manufactured by Toray Advanced Film Co., Ltd.), which is a non-stretched film, and an ONY film "ONMB-RT" (manufactured by Unitika Ltd.), which is a stretched film. In Fig. 7 and Table 2, the ONY film is shown as "ONY", the printing layer as "ink", the non-stretched polypropylene film as "CPP", the adhesive as "adh", the adhesive layer which is a cured product of the adhesive as "ADH", and the transparent vapor deposition barrier film as "PET".
[0088] [Table 2]
[0089] Comparative Example 1 As shown in Table 2, in Comparative Example 1, in the first step, a printed layer (adh) was formed on a transparent vapor deposition barrier film (PET) to obtain a printed transparent vapor deposition barrier film (PET / ink). The printed layer (ink) was formed by gravure printing colored inks on the transparent vapor deposition barrier film (PET). As colored inks, "Rio Alpha White", "Rio Alpha Yellow" and "Rio Alpha Blue" manufactured by Toyo Ink Co., Ltd. were used.
[0090] In Comparative Example 1, as the second step following the first step, an ONY film (ONY) was laminated onto the surface of the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the surface of the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink), and then the solvent-free adhesive (adh) and the ONY film (ONY) were placed opposite each other, and the surface of the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink) was bonded to the ONY film (ONY). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0091] In Comparative Example 1, as the third step following the second step, a non-oriented polypropylene film (CPP) was laminated on the surface opposite the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the non-oriented polypropylene film (CPP), and then the non-oriented polypropylene film (CPP) was bonded to the surface opposite the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0092] Thereafter, the solvent-free adhesive (adh) was cured to obtain a laminate of Comparative Example 1, which was formed by laminating, in this order, an unstretched polypropylene film (CPP), an adhesive layer (ADH) formed by the cured solvent-free adhesive (adh), an ONY film (ONY), an adhesive layer (ADH) formed by the cured solvent-free adhesive (adh), and a printed transparent vapor deposition barrier film (PET / ink).
[0093] Comparative Example 2 In Comparative Example 2, in the first step, a printed transparent vapor-deposited barrier film (PET / ink) was obtained in the same manner as in Comparative Example 1.
[0094] In Comparative Example 2, as the second step following the first step, an ONY film (ONY) was laminated onto the surface of the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the ONY film (ONY), and then the solvent-free adhesive (adh) and the ONY film (ONY) were placed opposite each other, and the ONY film (ONY) was bonded to the surface of the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0095] In Comparative Example 3, as the third step following the second step, a non-oriented polypropylene film (CPP) was laminated to the side opposite the printed layer (ink) of the printed transparent vapor-deposited barrier film (PET / ink) in the same manner as in Comparative Example 2.
[0096] Thereafter, the solvent-free adhesive (ADH) was cured to obtain the same laminate as in Comparative Example 1.
[0097] Comparative Example 3 In Comparative Example 3, in the first step, a printed transparent vapor-deposited barrier film (PET / ink) was obtained in the same manner as in Comparative Example 1.
[0098] In Comparative Example 3, as the second step following the first step, a non-oriented polypropylene film (CPP) was laminated onto the ONY film (ONY). In this lamination process, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the non-oriented polypropylene film (CPP), and then the non-oriented polypropylene film (CPP) was attached to the ONY film (ONY). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0099] In Comparative Example 3, as the third step following the second step, an ONY film (ONY) was laminated onto the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink). In this lamination, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink), and then the solvent-free adhesive (adh) and the ONY film (ONY) were placed opposite each other, and the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink) was bonded to the ONY film (ONY). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0100] Thereafter, the solvent-free adhesive (ADH) was cured to obtain the same laminate as in Comparative Example 1.
[0101] Comparative Example 4 In Comparative Example 4, in the first step, a printed transparent vapor-deposited barrier film (PET / ink) was obtained in the same manner as in Comparative Example 1.
[0102] In Comparative Example 4, as a second step following the first step, a non-oriented polypropylene film (CPP) was laminated onto an ONY film (ONY) in the same manner as in Comparative Example 3.
[0103] In Comparative Example 4, as the third step following the second step, an ONY film (ONY) was laminated onto the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink). In this lamination, a solvent-free adhesive "TSN-4864A / TSN-4864B3" (manufactured by Toyo-Morton Co., Ltd.) (adh) was applied onto the ONY film (ONY), and then the solvent-free adhesive (adh) was placed opposite the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink), and the ONY film (ONY) was bonded to the printed layer (ink) side of the printed transparent vapor-deposited barrier film (PET / ink). The solvent-free adhesive (adh) was applied in an amount of 2 g / m 2 The coating was performed using a roll coater so that the coating solution was as follows:
[0104] Thereafter, the solvent-free adhesive (ADH) was cured to obtain the same laminate as in Comparative Example 1.
[0105] <Evaluation> The laminates produced in Examples 1 to 5 and Comparative Examples 1 to 4 were aged in an environment of 40° C. and then evaluated for the following evaluation items. The results are shown in Table 3.
[0106] (exterior) Observations were made over a 1m distance in the flow direction and evaluated using the following criteria. A: No air bubbles with a diameter of 0.5 mm or more exist B: Bubbles with a diameter of 0.5 mm or more and less than 1 mm are present C: Bubbles with a diameter of 1 mm or more are present
[0107] (Lamination strength (adhesive strength)) Samples were cut into strips measuring 15 mm in the width direction and 50 mm in the machine direction, and the laminate strength (adhesive strength) of the obtained samples was measured at a peel speed of 300 mm / min and a peel angle of 90 degrees, and evaluated using the following index. In Examples 1 to 5, the laminate strength between a non-oriented polypropylene film (CPP) and an ONY film (ONY) was evaluated, and in Comparative Examples 1 to 4, the laminate strength between a transparent vapor-deposited barrier film (PET) and an ONY film (ONY) was evaluated. The results are shown in Table 3. A: 2N / 15mm or more B: 1N / 15mm or more, less than 2N / 15mm C: Less than 1N / 15mm
[0108] The laminate was folded in half so that the non-oriented polypropylene film (CPP) side was on the inside, and the two sides were heat-sealed to form a bag. The size of the bag was 297 mm x 420 mm. After 800 g of pure water was poured into the bag, the remaining side was heat-sealed in the same manner while preventing air from entering, to prepare a sample. The sample was retorted for 40 minutes at a pressure of 0.25 MPa and 135°C using a hot water storage type high-temperature and high-pressure cooking sterilizer, then removed and cooled, and the contents were discharged, after which the sample was cut into a strip shape of 15 mm in the width direction and 50 mm in the flow direction, and the laminate strength (adhesive strength) of the obtained sample was measured under conditions of a peel speed of 300 mm / min and a peel angle of 90 degrees, and evaluated according to the following index. In Examples 1 to 5, the laminate strength between the non-oriented polypropylene film (CPP) and the ONY film (ONY) was evaluated, and in Comparative Examples 1 to 4, the laminate strength between the transparent vapor deposition barrier film (PET) and the ONY film (ONY) was evaluated. The results are shown in Table 3. A: 2N / 15mm or more B: 1N / 15mm or more, less than 2N / 15mm C: Less than 1N / 15mm
[0109] [Table 3]
[0110] As shown in Table 3, the laminates of Examples 1 to 5 did not have any areas that were rated "C" in either the appearance or laminate strength evaluation items, and were confirmed to be laminates having good appearance and excellent adhesive strength.
[0111] Furthermore, the laminates of Examples 1 to 3 and the laminates of Examples 4 and 5 had regions in which the appearance was evaluated as "B", but the laminates of Examples 1 to 3 did not have regions in which the appearance was evaluated as "B", and it was confirmed that the laminates had good appearances. [Explanation of symbols]
[0112] Reference Signs List 1: laminate, 2: first stretched film, 3: second stretched film, 4: unstretched film, 5: first adhesive layer, 6: second adhesive layer, 21: base film, 22: printed layer, 51: first adhesive, 61: second adhesive.
Claims
1. A first stretched film having a print layer formed on one surface thereof; A first adhesive layer disposed on the opposite side of the first stretched film from the printed layer; A second adhesive layer disposed on the printing layer side of the first stretched film; a second stretched film disposed on the opposite side of the first stretched film from the printing layer via the first adhesive layer; a non-stretched film disposed on the printing layer side of the first stretched film via the second adhesive layer, Laminate.
2. The first adhesive layer and the second adhesive layer are cured products of a solvent-free adhesive. The laminate according to claim 1 .
3. The first adhesive layer and the second adhesive layer are cured products of a solvent-free two-component curing polyurethane adhesive. The laminate according to claim 1 .
4. At least one of the first stretched film and the second stretched film has gas barrier properties. The laminate according to claim 1 .
5. At least one of the first stretched film and the second stretched film has an inorganic vapor deposition layer. The laminate according to claim 1 .
6. At least one of the first stretched film and the second stretched film contains at least one of nylon, polypropylene, and polyethylene terephthalate. The laminate according to claim 1 .
7. A packaging bag produced by producing a packaging film comprising the laminate according to any one of claims 1 to 6.
8. The packaging bag according to claim 7, which is for boiling or retorting.
9. a stretched film lamination step of disposing a second stretched film via a first adhesive on an opposite side of the first stretched film having a printed layer formed on one side thereof, the opposite side of the printed layer; A non-stretched film laminating process of placing a non-stretched film on the printing layer side of the first stretched film via a second adhesive. A method for manufacturing a laminate.
10. The stretched film lamination step is performed after the non-stretched film lamination step. A method for producing the laminate according to claim 9.
11. A solvent-free adhesive is used as the first adhesive and the second adhesive. A method for producing the laminate according to claim 9.
12. At least one of the first stretched film and the second stretched film has gas barrier properties. A method for producing the laminate according to claim 9.
Citation Information
Patent Citations
JP238050A
adhesive composition
JP7030271B2