Curable resin composition, molded body, cured object, film, composite material, cured composite material, laminate, metal foil with resin and varnish for circuit board material obtained therefrom
A curable resin composition with a modified vinyl aromatic polymer and thermoplastic resin addresses the dielectric and adhesive limitations of existing materials, offering improved signal transmission and heat resistance for high-frequency applications in electronic and aerospace industries.
Patent Information
- Application Number
- JP2023052999
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-03-29
- Publication Date
- 2024-10-10
AI Technical Summary
Existing resin compositions for printed wiring boards lack sufficient dielectric properties and adhesive properties, particularly in high-frequency applications, and are limited by high dielectric constants and dielectric loss tangents, which lead to signal transmission loss and delays.
A curable resin composition comprising a modified vinyl aromatic polymer blended with a thermoplastic resin and a curing catalyst, featuring specific structural units and functional groups to enhance dielectric and adhesive properties, including a polyfunctional vinyl aromatic compound and a halogen-containing vinyl compound to improve solvent solubility and crosslinking.
The composition exhibits excellent dielectric properties and adhesive properties, providing improved signal transmission and reduced delays in high-frequency applications, with enhanced heat resistance and moldability, suitable for electronic and aerospace industries.
Smart Images

Figure 2024141390000001 
Figure 2024141390000002 
Figure 2024141390000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a modified vinyl aromatic polymer, a curable resin composition, and a molded article, a cured product, a film, a composite material, a cured composite material, a laminate, a resin-coated metal foil, a varnish for circuit board materials, and the like obtained therefrom. [Background technology]
[0002] In recent years, there has been a remarkable trend toward miniaturization and high density in the packaging methods of electronic devices for communication, consumer, industrial, etc., and this has led to a demand for materials with better heat resistance, dimensional stability, and electrical properties. For example, copper-clad laminates made of thermosetting resins such as phenolic resin and epoxy resin have traditionally been used for printed wiring boards. As electronic devices become smaller and more functional, printed wiring boards are required to have substrate materials that are thin, lightweight, and capable of high-density wiring. Furthermore, in recent years, in order to process large amounts of data at high speed, signals are becoming increasingly high-frequency in computers and information device terminals. However, the higher the frequency, the greater the transmission loss of the electrical signal, and there is a strong demand for the development of printed wiring boards that can handle higher frequencies. The transmission loss in high-frequency circuits is greatly affected by dielectric loss, which is determined by the dielectric properties of the insulating layer (dielectric) around the wiring, and it is therefore necessary to have low dielectric constants and low dielectric dissipation factor (tan δ) for printed wiring board substrates (especially insulating resins). For example, in mobile communication-related devices, as signals become higher frequency, there is a strong demand for substrates with low dielectric dissipation factor to reduce transmission loss in the microwave band above 5 GHz.
[0003] Furthermore, electronic information devices such as computers are now equipped with high-speed microprocessors with operating frequencies exceeding 350 MHz, and delays in high-speed pulse signals on printed wiring boards have become a problem.Since the signal delay time on a printed wiring board increases in proportion to the square root of the relative dielectric constant εr of the insulator around the wiring, high-speed computers and other devices require printed wiring boards with a low dielectric constant.
[0004] In response to the above-mentioned technical trends in printed wiring boards, phenolic resins and epoxy resins, which have been widely used up until now, have a good balance of various performance properties such as heat resistance, dimensional stability, and adhesiveness, but have the disadvantage of having high dielectric constants and dielectric loss tangents in high frequency bands. Although cyanate ester resins have improved performance such as heat resistance and dielectric properties to some extent compared to conventional cured epoxy resins, they are insufficient in terms of the dielectric properties required for recent high-frequency printed wiring boards. Moreover, cyanate ester resins are usually solid or semi-solid at room temperature and have low solubility, and therefore have the disadvantage that a large amount of solvent is required to prepare a curable resin composition thereof. Bismaleimide resins, which have excellent retention of physical properties at high temperatures and high humidity and good electrical properties over a wide temperature range, are also widely used in the fields of advanced composite materials and electronics-related materials. However, bismaleimide resins also have insufficient dielectric properties as insulating resin materials used in high-frequency printed wiring board applications that require highly low dielectric properties. Furthermore, bismaleimide resins are brittle, have low chemical resistance in the presence of basic compounds, and are usually solid or semi-solid at room temperature, with low solubility.
[0005] As a new material for solving this problem, Patent Documents 1 to 3 disclose resin compositions containing polyphenylene ether resins containing vinylbenzyl groups at both ends. However, although these curable resins have an excellent balance between heat resistance and dielectric properties, the resulting cured products have a drawback in that they do not have a sufficient balance between dielectric properties and adhesiveness. Patent Documents 4 to 6 disclose a soluble polyfunctional vinyl aromatic copolymer synthesized from a divinyl aromatic compound and a curable resin composition containing the copolymer. Although the curable resin composition has better dielectric properties than the polyphenylene ether resin containing vinylbenzyl groups at both ends, the adhesiveness is insufficient. Patent Document 7 discloses a resin composition containing (A) a thermosetting resin having a molecular weight of 800 to 1500 and having a styrene group at its end, (B) a liquid epoxy resin, (C) a styrene-based thermoplastic elastomer, (D) a filler, and (E) a curing agent. However, the dielectric properties and adhesiveness of this resin composition are also insufficient for use as an adhesive material in fields where high-level properties are required. Patent Document 8 discloses a soluble polyfunctional vinyl aromatic copolymer obtained by copolymerizing a divinyl aromatic compound and a monovinyl aromatic compound, the copolymer having a chain-like hydrocarbon group or an aromatic hydrocarbon group via an ether bond or a thioether bond at a part of its terminal groups. However, this soluble polyfunctional vinyl aromatic copolymer also does not have a sufficient balance between dielectric properties and adhesiveness. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] JP 2016-191073 A [Patent Document 2] JP 2016-28885 A [Patent Document 3] JP 2015-86330 A [Patent Document 4] WO2018 / 181842 issue [Patent Document 5] WO2017 / 115813 [Patent Document 6] JP 2018-39995 A [Patent Document 7] JP 2016-147945 A [Patent Document 8] JP 2007-332273 A Summary of the Invention [Problem to be solved by the invention]
[0007] The present invention provides a curable resin composition that exhibits excellent dielectric properties and adhesive properties after curing and can be used as a dielectric material, an insulating material, or an adhesive material in the fields of the electric and electronics industry, the aerospace industry, etc. Another object of the present invention is to provide a film obtained from the curable resin composition, a cured product thereof, a curable composite material, a cured product thereof, a laminate, and a resin-coated copper foil, etc. [Means for solving the problem]
[0008] The present inventors have found that the above problems can be solved by a curable resin composition obtained by blending a modified vinyl aromatic polymer, which is a polymer mainly composed of a monovinyl aromatic compound, has a specific polyfunctional structural unit and a specific monofunctional structural unit in the polymer, and has a polymer terminal modified with a specific functional group, with a thermoplastic resin and a curing catalyst, and have completed the present invention.
[0009] That is, the present invention relates to (A) a modified vinyl aromatic polymer obtained by polymerizing a monovinyl aromatic compound (a) in the presence of a polyfunctional anionic polymerization initiator produced by reacting a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of an organic alkali metal compound (e), the active terminal of the polymer being modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h); 50 mol % or more of the total of structural units derived from the reaction involving the components (a), (b), (c), and (e) are one or more structural units selected from the group consisting of structural units (d1), (d2), and (d3) each independently containing a plurality of structural units (M1) derived from the monovinyl aromatic compound (a) represented by the following formulas (1), (2), and (3): less than 50 mol % in total of the structural units derived from the reaction involving the components (a), (b), (c), and (e) are one or more structural units selected from the group consisting of structural units (d4) and (d5) containing solely the structural unit (M1) derived from the monovinyl aromatic compound (a) represented by the following formulas (4) and (5): [ka] [ka] (R1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, R2 represents hydrogen or a hydrocarbon group having 1 to 3 carbon atoms, R3 represents a hydrocarbon group having 1 to 30 carbon atoms, and R4 represents hydrogen or a hydrocarbon group having 1 to 15 carbon atoms. M1 represents a structural unit derived from the monovinyl aromatic compound (a). m represents an integer of 1 to 3. In addition, l, n, o, p, s, t, u, v, and w represent the degree of polymerization of the structural unit derived from the monovinyl aromatic compound (a).) a modified vinyl aromatic polymer in which the active terminal of the polymer is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h), the average number of functional groups per molecule is 1.5 or more, the number average molecular weight Mn is 500 to 30,000, and the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is 1.0 to 10.0; A resin composition comprising (B) a thermoplastic resin and (C) a curing catalyst, The curable resin composition is characterized in that the blending ratios of the components (A), (B) and (C) satisfy the following formulae (1) to (3). (A) + (B) + (C) = 100 (wt%) (1) (A) = 5.0 to 95.0 (wt%) (2) (B)=94.9~0.1(wt%) (3) (C)=0.1-4.9(wt%) (4)
[0010] The present invention further relates to a molded article, a cured product, a film, a composite material, a laminate, a metal foil with a resin, or a varnish for a circuit board material, which is made of the above-mentioned curable resin composition. Effect of the Invention
[0011] The curable resin composition of the present invention is a material that exhibits excellent dielectric properties and adhesiveness after curing and has good moldability, and is therefore useful as a dielectric material, insulating material, heat-resistant material, structural material, etc. in fields such as the electrical and electronic industries and the aerospace and aircraft industries. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] The curable resin composition of the present invention contains (A) a modified vinyl aromatic polymer, (B) a thermoplastic resin, and (C) a curing catalyst in predetermined proportions as essential components.
[0013] In the curable resin composition of the present invention, the modified vinyl aromatic polymer (A) is a modified vinyl aromatic polymer in which the active end of a polymer obtained by polymerizing a monovinyl aromatic compound (a) in the presence of a polyfunctional anionic polymerization initiator produced by reacting a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of an organic alkali metal compound (e) is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h), and 50 mol % or more of the total of the structural units derived from the reactions involving the components (a), (b), (c), and (e) are structural units independently containing a plurality of structural units (M1) derived from the monovinyl aromatic compound (a), and less than 50 mol % of the total of the structural units derived from the reactions involving the components (a), (b), (c), and (e) are structural units containing only the structural unit (M1) derived from the monovinyl aromatic compound (a).
[0014] In the (A) modified vinyl aromatic polymer, 50 mol % or more of the total structural units derived from the reactions involving the components (a), (b), (c), and (e) are one or more structural units selected from the group consisting of polyfunctional structural units (d1), (d2), and (d3) each independently containing a plurality of structural units (M1) derived from the monovinyl aromatic compound (a) represented by the formulas (1), (2), and (3). [ka] Here, the structural unit (d1) containing a plurality of independent structural units (M1) derived from the monovinyl aromatic compound (a) represented by formula (1) is a structural unit produced by polymerizing the monovinyl aromatic compound (a) with a reaction product (multianion body) of a polyfunctional vinyl aromatic compound (b) and an organic alkali metal compound (e). The structural unit (d2) containing a plurality of independent structural units (M1) derived from the monovinyl aromatic compound (a) represented by formula (2) is a structural unit produced by polymerizing the monovinyl aromatic compound (a) with a reaction product (multianion) of an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms and an organic alkali metal compound. The structural unit (d3) containing multiple independent structural units (M1) derived from the monovinyl aromatic compound (a) represented by formula (3) is a structural unit generated by polymerizing the monovinyl aromatic compound (a) with the reaction product (monoanion) of the polyfunctional vinyl aromatic compound (b) and the organic alkali metal compound (e). At that time, the second vinyl group reacts with another living polymer to generate a branch.
[0015] In the (A) modified vinyl aromatic polymer, less than 50 mol % of the total of the structural units derived from the reactions involving the components (a), (b), (c), and (e) is one or more structural units selected from the group consisting of structural units (d4) and (d5) each containing solely the structural unit (M1) derived from the monovinyl aromatic compound (a) represented by formula (4) and formula (5). [ka] Here, the structural unit (d4) containing only the structural unit (M1) derived from the monovinyl aromatic compound (a) represented by formula (4) is a structural unit produced by polymerizing the monovinyl aromatic compound (a) with the reaction product (monoanion) of the polyfunctional vinyl aromatic compound (b) and the organic alkali metal compound (e). At that time, the second vinyl group remains unreacted. The structural unit (d5) containing only the structural unit (M1) derived from the monovinyl aromatic compound (a) represented by formula (5) is a structural unit produced by polymerizing the monovinyl aromatic compound (a) with the reaction product (monoanion) of an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms and an organic alkali metal compound, in which the second alkyl group remains unreacted.
[0016] The monovinyl aromatic compound (a), which is the main structural unit of the modified vinyl aromatic polymer (A), improves the solvent solubility, compatibility and processability of the polymer. Examples of monovinyl aromatic compounds include vinyl aromatic compounds such as styrene, vinylnaphthalene, vinylbiphenyl, and α-methylstyrene; nucleus alkyl-substituted vinyl aromatic compounds such as o-methylstyrene, m-methylstyrene, p-methylstyrene, o,p-dimethylstyrene, o-ethylvinylbenzene, m-ethylvinylbenzene, and p-ethylvinylbenzene; and cyclic vinyl aromatic compounds such as indene, acenaphthylene, benzothiophene, and coumarone, but are not limited thereto. These compounds also include each isomer and may be an isomer mixture. In order to prevent gelation of the polymer and improve solubility in a solvent, compatibility, and processability, styrene, ethylvinylbenzene, ethylvinylbiphenyl, ethylvinylnaphthalene, and indene are particularly preferred from the viewpoints of cost and availability. From the viewpoints of compatibility and cost, styrene, ethylvinylbenzene, and p-methylstyrene are more preferred.
[0017] The modified vinyl aromatic polymer (A) is a modified vinyl aromatic polymer in which the active terminal of the polymer produced by polymerization of a monovinyl aromatic compound (a) in the presence of a polyfunctional anionic polymerization initiator (z), which is produced from a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of an organic alkali metal compound (e), is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h), and the polymer has structural units derived from a reaction involving the components (a), (b), (c), and (e). Examples of the polyfunctional vinyl aromatic compound (b) preferably include, but are not limited to, diisopropenylbenzene, divinylbenzene, diisopropenylnaphthalene, divinylnaphthalene, diisopropenylbiphenyl, and divinylbiphenyl. These compounds include isomers such as m-isomer and p-isomer, and may be a mixture of these isomers. Examples of aromatic compounds (c) having 2 to 4 alkyl groups with 1 to 3 carbon atoms include, but are not limited to, xylene, trimethylbenzene, diethylbenzene, triethylbenzene, dipropylbenzene, tripropylbenzene, dimethylnaphthalene, trimethylnaphthalene, diethylnaphthalene, triethylnaphthalene, dipropylnaphthalene, tripropylnaphthalene, dimethylbiphenyl, trimethylbiphenyl, diethylbiphenyl, triethylbiphenyl, dipropylbiphenyl, and tripropylbiphenyl. These compounds also include isomers such as m-isomer and p-isomer, 1,2,4-position-3 substitution, and 1,3,5-position-3 substitution, and may be a mixture of these isomers. These components (b) and (c) can be used alone or in combination of two or more.
[0018] The modified vinyl aromatic polymer (A) has a terminal modified with a functional group having a vinyl group derived from the halogen-containing vinyl compound (h), and has an average functional group number of 1.5 or more per molecule. Therefore, the cured product exhibits good heat resistance. If the value obtained by dividing the number average molecular weight of the polymer by the functional group equivalent is 1.5 or more, it can be judged that 1.5 or more are functionalized. The amount of introduction by the modifying agent having a functional group is preferably 1.5 to 20, more preferably 2.0 to 10.0, and even more preferably 2.0 to 5.5, functional groups per molecule on average. It is particularly preferably 2.0 to 5.0.
[0019] The modified vinyl aromatic polymer (A) can be produced, for example, by the following method. The polyvinyl aromatic polymer can be produced by a method including the steps of: an initiation reaction step of reacting an organic alkali metal compound (e) with a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of at least one Lewis base selected from a tertiary monoamine, a tertiary diamine, and a chain ether or cyclic ether having two or more oxygen atoms in one molecule to produce a polyfunctional anionic polymerization initiator (z); a polymerization step of polymerizing a monovinyl aromatic compound (a) with the polyfunctional anionic polymerization initiator (z) produced to obtain a vinyl aromatic polymer; and a terminal modification step of reacting an halogen-containing vinyl compound (h) with an active terminal of the vinyl aromatic polymer to form a functional group.
[0020] The modified vinyl aromatic polymer of the present invention is a polymer made from components (a), (b), (c), (e) and (h). However, other monomers may be used and structural units derived from the other monomers may be introduced into the polymer within a range that does not impair the effects of components (a), (b), (c), (e) and (h).
[0021] Examples of other monomers include, but are not limited to, acrylonitrile, methyl (meth)acrylate, and ethyl (meth)acrylate. These can be used alone or in combination of two or more. The other monomers are preferably used in an amount of less than 30 mol% based on the total amount of all monomers constituting the polymer of the present invention. The amount is preferably 10 mol% or less, and more preferably 5 mol% or less.
[0022] In the method for producing a modified vinyl aromatic polymer of the present invention, in the initiation reaction step, an organic alkali metal compound (e) is reacted with a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms to produce a polyfunctional anionic polymerization initiator (z). It is preferable to react the polyfunctional vinyl aromatic compound (b) and / or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms with the organic alkali metal compound (e) in a molar ratio (b+c) / e of 0.2 or more and 0.9 or less.
[0023] In the modified vinyl aromatic polymer (A) of the present invention, the polymer having an active end produced by reacting the polyfunctional anionic polymerization initiator (z) prepared by reacting the organic alkali metal compound (e) as a polymerization initiator with the component (b) and / or the component (c) with the component (a) must have an initiator-derived multiple polymer unit structure degree (mol%) of 50 mol% or more, which indicates the proportion of structural units represented by formulas (1) to (3) each independently containing a polymer chain of the structural unit (M1) derived from the monovinyl aromatic compound (a) among the total structural units derived from the reactions involving the components (a), (b), (c), and (e) represented by formulas (1) to (5). The initiator-derived multiple polymer unit structure degree (mol%) is preferably 60 mol% or more, more preferably 70 mol% or more, and particularly preferably 80 mol% or more. On the other hand, the degree of initiator-derived single polymer unit structure (mol%), which indicates the proportion of structural units represented by formulas (4) and (5) each containing a polymer chain of the structural unit (M1) derived from the monovinyl aromatic compound (a) alone, among the total of structural units derived from the reactions involving the components (a), (b), (c), and (e) represented by formulas (1) to (5), must be less than 50 mol%, preferably less than 40 mol%, more preferably less than 30 mol%, and particularly preferably less than 20 mol%.
[0024] The degree of initiator-derived multiple polymer unit structure, which indicates the proportion of structures represented by formulas (1) to (3) each containing a plurality of independent polymer chains of the structural unit (M1) derived from the monovinyl aromatic compound (a) among the structural units derived from the reactions involving the components (a), (b), (c), and (e) represented by formulas (1) to (5), is a parameter that can be arbitrarily controlled and changed. However, if this ratio is less than 50 mol %, the branching reaction does not proceed sufficiently, so that the modification of the terminal functional group having the vinyl group derived from the halogen-containing vinyl compound (h) introduced per polymer molecule becomes insufficient, and the crosslinked structure does not increase sufficiently, which tends to reduce the effect of improving physical properties such as heat resistance.
[0025] In the process for producing the modified vinyl aromatic polymer (A), the organic alkali metal compound (e) used in the initiation reaction step in combination with the polyfunctional vinyl aromatic compound (b) and / or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms is not particularly limited, and examples thereof include organic alkali metal compounds containing alkali metals such as lithium, sodium, potassium, rubidium, and cesium. Of these, organic lithium compounds are preferred. Specific examples of these include alkyllithiums such as methyllithium, ethyllithium, n-propyllithium, i-propyllithium, n-butyllithium, sec-butyllithium, t-butyllithium, and 2-methyl-propyllithium, as well as phenyllithium, stilbenelithium, and naphthyllithium. Among these, in terms of superior reactivity with polyfunctional aromatic vinyl compounds, the organic alkali metal compound is more preferably n-butyllithium, sec-butyllithium, or tert-butyllithium, and even more preferably n-butyllithium and sec-butyllithium. The organic alkali metal compound (e) is reacted with the polyfunctional vinyl aromatic compound (b) to form a polyfunctional anionic polymerization initiator (z). When the monovinyl aromatic compound (a) is polymerized using this polyfunctional anionic polymerization initiator (z), a portion of the organic alkali metal compound (e) is incorporated into the resulting polymer. On the other hand, when the organic alkali metal compound (e) is reacted with an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms to form a polyfunctional anionic polymerization initiator (z), and the monovinyl aromatic compound (a) is polymerized using this polyfunctional anionic polymerization initiator (z), the organic alkali metal compound (e) is not incorporated into the resulting polymer.
[0026] The amount of organic alkali metal compound (e) used is preferably 0.2 to 0.9 (molar) relative to the total (molar) of the polyfunctional vinyl aromatic compound (b) and / or the aromatic compound (c) having 2 to 4 alkyl groups with 1 to 3 carbon atoms. More preferably, it is 0.3 to 0.7 times by mole. If the amount of organic alkali metal compound (e) used is less than 0.2 times by mole, the branching reaction does not proceed sufficiently, so that the amount of vinyl functional groups introduced to the terminal per polymer molecule decreases, and when the curable resin composition is prepared, the crosslinked structure does not increase sufficiently, and the effect of improving physical properties such as heat resistance tends to be small. On the other hand, if the organic alkali metal compound (e) is used in an amount exceeding 0.9 times by mole, the amount of the organic lithium compound (e) that does not react with the polyfunctional vinyl aromatic compound (b) and / or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms increases, and the amount of the modified vinyl aromatic polymer having a vinyl functional group introduced only at one end increases. As a result, when a curable resin composition is formed, the crosslinked structure does not increase sufficiently, and the effect of improving physical properties such as heat resistance tends to be reduced. It is preferable to use 3.0 to 300 mmol of the polyfunctional vinyl aromatic compound (b) and / or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms per mol of the monovinyl aromatic compound (a). More preferably, the amount of the polyfunctional anionic polymerization initiator (b) and (c) per mol of the polymerizable monomer (a) is 5.0 to 250 mmol, and even more preferably 10.0 to 200 mmol.
[0027] The initiation reaction and polymerization reaction are desirably carried out in the presence of at least one Lewis base selected from a tertiary monoamine, a tertiary diamine, and a chain ether or cyclic ether having two or more oxygen atoms in one molecule, as a co-catalyst. Examples of tertiary monoamines include compounds such as trimethylamine, triethylamine, methyldiethylamine, 1,1-dimethoxytrimethylamine, 1,1-diethoxytrimethylamine, N,N-dimethylformamide diisopropyl acetal, N,N-dimethylformamide, and dicyclohexyl acetal; examples of tertiary diamines include compounds such as N,N,N',N'-tetramethyldiaminomethane, N,N,N',N'-tetramethylethylenediamine, N,N,N',N'-tetramethylpropanediamine, N,N,N',N'-tetramethyldiaminobutane, N,N,N',N'-tetramethyldiaminopentane, N,N,N',N'-tetramethylhexanediamine, dipiperidinomethane, and dipiperidinoethane. Examples of chain ethers or cyclic ethers having two or more oxygen atoms in one molecule include chain ethers such as ethylene glycol dimethyl ether (1,2-dimethoxyethane), diethylene glycol dimethyl ether, triethylene glycol dimethyl ether, and tetraethylene dimethyl ether; examples of cyclic ethers include compounds such as bis(2-oxolanyl)ethane, 2,2-bis(2-oxolanyl)propane, 1,1-bis(2-oxolanyl)ethane, 2,2-bis(2-oxolananyl)butane, 2,2-bis(5-methyl-2-oxolanyl)propane, and 2,2-bis(3,4,5-trimethyl-2-oxolanyl)propane, and these can be used alone or in combination of two or more. The amount of the Lewis base used is, for example, 0.02 to 6.0 mol relative to 1 mol of the organic alkali metal compound (e). It is preferably in the range of 0.1 to 4 mol. If it is less than 0.02 mol, the effect of the present invention is not exhibited, and if it is used in excess of 6 mol, it is not preferable because it becomes difficult to separate the Lewis base from the polymerization solvent in the solvent recovery step.
[0028] The polymerization of the monomer containing the monovinyl aromatic compound (a) is preferably carried out by solution polymerization in an inert solvent. The polymerization solvent is not particularly limited, and for example, a hydrocarbon-based solvent such as a saturated hydrocarbon or an aromatic hydrocarbon is used. Specifically, it includes aliphatic hydrocarbons such as butane, pentane, hexane, and heptane; alicyclic hydrocarbons such as cyclopentane, cyclohexane, methylcyclopentane, methylcyclohexane, dimethylcyclohexane, ethylcyclohexane, and decalin; aromatic hydrocarbons such as benzene, toluene, and xylene, and hydrocarbon-based solvents consisting of mixtures thereof. It is preferable that the monomer and the polymerization solvent, either alone or in the form of a mixture thereof, are treated with an organometallic compound in advance. By such treatment, impurities such as arenes and acetylenes contained in the monomer and the polymerization solvent can be removed, and a polymer having a high concentration of active ends can be obtained, resulting in a high modification rate.
[0029] The polymerization temperature is not particularly limited as long as it is a temperature at which living anionic polymerization proceeds, but from the viewpoint of productivity, it is preferably from -20°C to 150°C, and from the viewpoint of ensuring a sufficient amount of reaction with active terminals in the terminal modification step after completion of polymerization, it is preferably from -20°C to 120°C, more preferably from 0°C to 100°C.
[0030] The polymerization reaction can be carried out in any of a batch system and a continuous system. In a continuous system, one or more connected reactors can be used. The reactor can be a tank type with an agitator, a tube type, or the like. In the case of a batch system, the molecular weight distribution of the polymer obtained is generally narrow, and Mw / Mn tends to be about 1.0 or more and less than 3.0. In the case of a continuous system, the molecular weight distribution is generally wide, and Mw / Mn tends to be about 1.5 or more and less than 10.
[0031] In the method for producing the modified vinyl aromatic polymer (A), a vinyl aromatic polymer having an active end is obtained by an initiation reaction and a polymerization reaction, and then a halogen-containing vinyl compound (h) serving as a modifier is reacted with the active end to introduce a functional group into the active end of the polymer.
[0032] Examples of the halogen-containing vinyl compound (h) include halogen-containing vinyl aromatic compounds such as chloromethylstyrene (CMS), p-chloromethylstyrene, m-chloromethylstyrene, o-chlorostyrene, p-chlorostyrene, m-chlorostyrene, o-chlorostyrene, p-chloro-α-methylstyrene, m-chloro-α-methylstyrene, p-bromomethylstyrene, and p-bromostyrene; vinyl-2-chloromethyl ether, vinyl-2-chloroethyl ether, vinyl-3-chlorobutyl ether, isopropenyl chloromethyl ether, isopropenyl-2-chloroethyl ether, vinyl-2-bromomethyl ether, and vinyl-2-chloroethyl ether. -bromoethyl ether and other halogen-containing vinyl ether compounds, vinyl chloroacetate, vinyl bromoacetate, vinyl 3-chloropropionate, vinyl 3-chloroisobutyrate, vinyl 4-chlorobutyrate, vinyl 6-chlorocaproate, vinyl 3-bromopropionate, p-chlorophenylvinyl acetate and other halogen-containing vinyl acetate compounds, methyl methacrylate chloride, butyl methacrylate chloride, ethyl methacrylate chloride, methyl acrylate chloride, methyl methacrylate bromide, butyl methacrylate bromide and other halogen-containing (meth)acrylic ester compounds, which can be used alone or in combination of two or more. Among the above halogen-containing vinyl compounds, from the viewpoint of electrical properties, halogen-containing vinyl aromatic compounds are most preferably used.
[0033] The amount of the halogen-containing vinyl compound (h) is not particularly limited, but in the initiation reaction step, the equivalent of the halogen-containing vinyl compound (modifier) is preferably in the range of 0.3 to 6 times the equivalent of the carbanion, which is the active terminal (active species) of the polymer derived by reacting the polyfunctional anionic polymerization initiator (z) obtained by reacting the organic alkali metal compound (e) with the polyfunctional vinyl aromatic compound (b) and / or (c) components with the monovinyl aromatic compound (a). If the amount added is 0.3 times or more, the desired modification rate can be obtained in the polymer. A more preferable lower limit is 0.5 times, even more preferably 0.7 times, and particularly preferably 0.9 times. On the other hand, a more preferable upper limit is 3.0 times, even more preferably 2.0 times, and particularly preferably 1.5 times. If it is less than 0.3 times, an undesired side reaction occurs in which the polymer chain becomes a polymer twice or more the initial polymer, and the desired polymer cannot be obtained. Although it may be used in an amount exceeding 6 times, since there is no change in the compound introduced into the polymer, it is usually used in the range of 0.5 moles to 1.5 moles.
[0034] When reacting the halogen-containing vinyl compound (h) as a modifying agent with the active terminal of the polymer, the reaction temperature and reaction time are, for example, −20° C. to 120° C., and the reaction is performed for 30 seconds or more. In the case where the polymerization process is a batch process, the terminal modification process may be carried out in the reactor used in the polymerization process, or may be carried out in the next reactor. In the case where the polymerization process is a continuous process, the terminal modification process is carried out in the next reactor. The terminal modification process is preferably carried out immediately following the polymerization process, and the modifying agent is preferably mixed and the reaction carried out within 5 minutes. The reactor for the modification reaction is preferably one that can perform sufficient stirring. Specifically, a static mixer type reactor, a stirrer-equipped tank type reactor, etc. can be mentioned.
[0035] The modified vinyl aromatic polymer (A) obtained by such a production method has an active end modified with a halogen-containing vinyl compound (h) and may be molded and cured by itself, but may also be used for functional group modification and synthesis of high molecular weight multi-branched components of other polymerizable resins. In the modified vinyl aromatic polymer (A), a multi-branched component is generated, which is a structural unit containing a plurality of independent polymer chains of the structural unit (M1) derived from the polymerization of the monovinyl aromatic compound (a) in the presence of a multifunctional anionic polymerization initiator (z) generated by reacting an organic alkali metal compound (e) with a multifunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms. The ratio of the multi-branched component is defined as the initiator-derived multi-polymer unit structure degree, and is expressed as a molar fraction relative to the sum of the structural units derived from the reaction involving the components (a), (b), (c), and (e). The initiator-derived multi-polymer unit structure degree is preferably 0.50 or more. By making the initiator-derived multi-polymer unit structure degree 0.50 or more, the amount of the modifier introduced can be increased. It is more preferably 0.70 or more, even more preferably 0.80 or more, and particularly preferably 0.90 or more.
[0036] The average number of functional groups per molecule in the modified vinyl aromatic polymer (A) (the amount of vinyl groups introduced per molecule) can be calculated from the vinyl equivalent (g / eq) and number average molecular weight Mn of the modified vinyl aromatic polymer by the following formula (1). Average number of functional groups per molecule (amount of vinyl groups introduced per molecule) = [(number average molecular weight Mn) / (vinyl equivalent)] (1) The vinyl equivalent of a modified vinyl aromatic polymer means the mass of a resin containing one equivalent of a vinyl group. The vinyl equivalent is calculated by the following formula: 13 C-NMR and 1 From the H-NMR measurement results, the amount of vinyl group introduced at the terminal can be calculated.
[0037] The average number of functional groups per molecule in the modified vinyl aromatic polymer (A) (amount of vinyl groups introduced per molecule) is preferably 1.5 to 20. More preferably, it is 1.7 to 10, and even more preferably, it is 2 to 5. If the average number of functional groups per molecule exceeds 20, the viscosity increases rapidly during molding, so that molding defects such as poor appearance and voids tend to occur, and molding processability tends to deteriorate. If the average number of functional groups per molecule is less than 1.5, the crosslinking structure cannot be sufficiently formed during curing, so that the heat resistance tends to be insufficient.
[0038] The modified vinyl aromatic polymer (A) contains 65.0 to 99.5 mol % of structural units derived from the monovinyl aromatic compound (a). In terms of molar fraction, it is 0.65 to 0.995. The lower limit is preferably 0.70, more preferably 0.75. On the other hand, the upper limit is preferably 0.994, more preferably 0.993. The optimum range is 0.70 to 0.99.
[0039] The molar fraction of the structural unit derived from the monovinyl aromatic compound (a) is calculated by the following formula (2) when it consists of a structural unit derived from the monovinyl aromatic compound (a) and a structural unit derived from the polyfunctional vinyl aromatic compound (b) or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms. (a) / [(a)+(b)+(c)] (2) In formula (2), (a) is the molar fraction of structural units derived from the monovinyl aromatic compound (a), (b) is the molar fraction of structural units derived from the polyfunctional vinyl aromatic compound (b), and (c) is the molar fraction of structural units derived from the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms. Even when structural units other than those derived from (a), (b) and (c) are contained, the preferred molar fraction of the structural units derived from (a) is generally within the above range.
[0040] The modified vinyl aromatic polymer (A) contains 0.5 to 35.0 mol % in total of structural units derived from the polyfunctional vinyl aromatic compound (b) or the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms. In terms of molar fraction, it is 0.005 to 0.35. The lower limit is preferably 0.006, more preferably 0.007. On the other hand, the upper limit is preferably 0.35, more preferably 0.30. It is most preferably 0.01 to 0.25. The molar fraction of structural units derived from the polyfunctional vinyl aromatic compound (b) and the aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms is calculated by the following formula (3) when the structural units consist only of structural units derived from (a), (b) and (c). [(b)+(c)] / [(a)+(b)+(c)] (3) Here, (a), (b) and (c) are synonymous with formula (2).
[0041] The modified vinyl aromatic polymer (A) may contain other structural units in addition to the above structural units.
[0042] The modified vinyl aromatic polymer (A) has a number average molecular weight Mn (measured by gel permeation chromatography in terms of standard polystyrene) of 500 to 30,000. The lower limit is preferably 600, more preferably 700, even more preferably 800, and particularly preferably 900. On the other hand, the upper limit is preferably 25,000, more preferably 20,000, even more preferably 15,000, and particularly preferably 10,000. If Mn is less than 500, the production cost increases and it tends to be difficult to carry out industrially. On the other hand, if it exceeds 30,000, the crosslink density decreases, the heat resistance is likely to decrease, and the compatibility with other resins tends to decrease. The molecular weight distribution (Mw / Mn) is preferably in the range of 1.0 to 10.0. The upper limit is preferably 5.0 or less, more preferably 3.0 or less, even more preferably 2.5 or less, and particularly preferably 2.0 or less. If Mw / Mn exceeds 10.0, gel tends to occur.
[0043] The modified vinyl aromatic polymer (A) is soluble in a solvent selected from toluene, xylene, tetrahydrofuran, dichloroethane, and chloroform, and is preferably soluble in any of these solvents. It is preferable that the polymer dissolves in an amount of 50 g or more in 100 g of the solvent. More preferably, the polymer dissolves in an amount of 80 g or more.
[0044] The curable resin composition of the present invention contains, as essential components, the above-mentioned modified vinyl aromatic polymer (A), as well as a thermoplastic resin (B) and a curing catalyst (C).
[0045] The content of the modified vinyl aromatic polymer (A) relative to the total of the components (A), (B), and (C) must satisfy the following formula (4). (A) / (A+B+C)=5.0~95.0(wt%) (4) The amount of the component (A) is preferably 14.8 to 93.0 (wt%). If the amount of the component (A) is less than 5.0 wt%, the improvement in the heat resistance and chemical resistance of the curable composition due to the addition of the modified vinyl aromatic polymer (A) is insufficient, whereas if it exceeds 95.0 wt%, the mechanical properties are unfavorably reduced.
[0046] The thermoplastic resin (B) is a component that improves the mechanical properties of the curable resin composition of the present invention.Examples of the thermoplastic resin (B) include polystyrene, polyphenylene ether resin, polyetherimide resin, polyethersulfone resin, PPS resin, polycyclopentadiene resin, polycycloolefin resin, etc.; polyolefins such as polyethylene, polypropylene, polybutene, ethylene-propylene copolymer, poly(4-methyl-pentene) and derivatives thereof; polyamides such as nylon 4, nylon 6, nylon 6·6, nylon 6·10, nylon 12 and derivatives thereof; polyesters such as polyethylene terephthalate, polybutylene terephthalate, polyethylene naphthalate, polyethylene terephthalate-polyethylene glycol block copolymer and derivatives thereof; polyphenylene ether, modified polyphenylene ether, polycarbonate, polyacetal, polysulfone, polyvinyl chloride and copolymers thereof, polyvinylidene chloride and copolymers thereof, polymethyl methacrylates, acrylic (or methacrylic) acid ester copolymers, polystyrenes, acrylonitrile-styrene copolymers, acrylonitrile-styrene-butadiene copolymers, etc. Examples of the liquid crystal polymers include polystyrenes and copolymers thereof, polyvinyl acetates, polyvinyl formals, polyvinyl acetals, polyvinyl butyrals, ethylene-vinyl acetate copolymers and hydrolysates thereof, polyvinyl alcohols, polyvinyl ethers such as polymethoxyethylene and polyethoxyethylene, polyacrylamides, polyphosphazenes, polyethersulfones, polyetherketones, polyetherimides, polyphenylene sulfides, polyamideimides, thermoplastic polyimides, and aromatic polyesters, side-chain liquid crystal polymers containing a liquid crystal component in the side chain, known thermoplastic elastomers such as styrene-ethylene-propylene copolymers, styrene-ethylene-butylene copolymers, styrene-butadiene copolymers, styrene-isoprene copolymers, hydrogenated styrene-butadiene copolymers, and hydrogenated styrene-isoprene copolymers, and rubbers such as polybutadiene and polyisoprene, and thermoplastic block copolymers into which at least one functional group selected from an epoxy group, a carboxylic acid group, and a maleic anhydride group has been introduced.
[0047] Among these thermoplastic resins, it is preferable to use a block copolymer having a polymer segment with a glass transition temperature of 20°C or less in order to improve the toughness effect. It is more preferable to use a block copolymer having a polymer segment with a glass transition temperature of 0°C or less. The block copolymer having a polymer segment with a glass transition temperature of 20°C or less mentioned here is preferably a rubber such as a styrene-conjugated diene block copolymer, or a rubber such as a hydrogenated styrene-conjugated diene block copolymer. From the viewpoint of the thermal oxidative deterioration resistance of the curable resin composition of the present invention, hydrogenated rubbers such as a hydrogenated styrene-conjugated diene block copolymer are most preferable. The structure of the hydrogenated block copolymer is obtained by hydrogenating a block copolymer consisting of a polymer block A mainly composed of at least one vinyl aromatic compound and a polymer block B mainly composed of at least one conjugated diene compound, for example: A.B. A.B.A. BABA [AB-]4-Si [BAB-]4-Si The hydrogenated block copolymer is a vinyl aromatic compound-conjugated diene compound block copolymer having the above structure. The hydrogenated block copolymer contains 5 to 85 wt%, preferably 10 to 70 wt%, and more preferably 15 to 40 wt% of the vinyl aromatic compound.
[0048] Further, referring to the block structure, the polymer block A mainly composed of a vinyl aromatic compound has a structure of a polymer block consisting of only a vinyl aromatic compound or a copolymer block of a vinyl aromatic compound containing more than 50% by weight, preferably 70% by weight or more of a vinyl aromatic compound and a hydrogenated conjugated diene compound, and further, the polymer block B mainly composed of a hydrogenated conjugated diene compound has a structure of a polymer block consisting of only a hydrogenated conjugated diene compound or a copolymer block of a hydrogenated conjugated diene compound containing more than 50% by weight, preferably 70% by weight or more of a hydrogenated conjugated diene compound and a vinyl aromatic compound.
[0049] Furthermore, the polymer block A mainly composed of these vinyl aromatic compounds and the polymer block B mainly composed of the hydrogenated conjugated diene compound may have a distribution of the hydrogenated conjugated diene compound or the vinyl aromatic compound in the molecular chain in each polymer block that is random, tapered (wherein the monomer component increases or decreases along the molecular chain), partially block-like, or any combination thereof. When there are two or more polymer blocks mainly composed of the vinyl aromatic compound and two or more polymer blocks mainly composed of the hydrogenated conjugated diene compound, the polymer blocks may have the same structure or different structures.
[0050] The vinyl aromatic compound constituting the hydrogenated block copolymer may be one or more selected from, for example, styrene, α-methylstyrene, p-methylstyrene, vinyltoluene, p-tertiary butylstyrene, etc., and styrene is preferred. The conjugated diene compound before hydrogenation constituting the hydrogenated conjugated diene compound may be one or more selected from, for example, butadiene, isoprene, 1,3-pentadiene, 1,3-dimethyl-1,3-butadiene, etc., and butadiene, isoprene, and combinations thereof are preferred. Butadiene is most preferred from the viewpoint of compatibility with the (A) component and the (B) component of the present invention.
[0051] The number average molecular weight of the hydrogenated block copolymer having the above structure to be used in the present invention is not particularly limited, but the number average molecular weight can be in the range of 5,000 to 1,000,000, preferably 10,000 to 500,000, and more preferably 30,000 to 300,000. The molecular structure of the hydrogenated block copolymer may be linear, branched, radial, or any combination thereof. The amount of thermoplastic resin (B) blended (wt %) relative to the total amount of components (A), (B), and (C) must satisfy the following mathematical formula (5). (B) / (A+B+C)=94.9~0.1(wt%) (5) The blending amount of the (B) component is preferably 85 to 5 (wt%). If the blending amount of the (B) component is less than 0.1 wt%, the improvement in the mechanical properties of the curable composition due to the addition of the thermoplastic resin (B) is insufficient, whereas if it exceeds 94.9 wt%, the heat resistance and chemical resistance are reduced, which is undesirable.
[0052] The curable resin composition of the present invention may further contain a curable reactive resin (D) as required. The curable reactive resin may be a thermosetting resin or a resin or compound that copolymerizes with the modified vinyl aromatic polymer of the present invention to give a cured resin. Examples of the curable reactive resin include vinyl ester resin, polyvinylbenzyl resin, unsaturated polyester resin, curable vinyl resin, curable polyphenylene ether resin, maleimide resin, epoxy resin, polycyanate resin, phenol resin, and one or more vinyl compounds having one or more polymerizable unsaturated hydrocarbon groups in the molecule. The amount of the curable reactive resin (D) to be blended relative to the total amount of the components (A), (B), (C) and (D) preferably satisfies the following formula (6). (D) / (A+B+C+D)=2.0~60.0(wt%) (6) The amount of component (D) is preferably 5.0 to 50.0 (wt%). If the amount of component (D) is less than 2.0 wt%, the improvement in heat resistance of the curable composition due to the addition of the curable reactive resin (D) is insufficient, whereas if it exceeds 60.0 wt%, the mechanical properties are unfavorably reduced.
[0053] The curable resin composition of the present invention is cured by crosslinking the vinyl groups of the modified vinyl aromatic polymer by heating or other means, and a curing catalyst (C) is blended as an essential component for the purpose of lowering the reaction temperature and promoting the crosslinking reaction of the unsaturated groups. Examples of curing catalysts that generate radicals or cationic active species capable of initiating the polymerization of vinyl groups by heat or light are shown below. Examples of the thermal radical polymerization initiator include benzoyl peroxide, cumene hydroperoxide, 2,5-dimethylhexane-2,5-dihydroperoxide, 2,5-dimethyl-2,5-di(t-butylperoxy)hexyne-3, di-t-butyl peroxide, t-butylcumyl peroxide, α,α'-bis(t-butylperoxy-m-isopropyl)benzene, 2,5-dimethyl-2,5-di(t-butylperoxy)hexane, dicumyl peroxide, di-t-butylperoxyisophthalate, and t-butylperoxybenzene. peroxides such as benzoate, 2,2-bis(t-butylperoxy)butane, 2,2-bis(t-butylperoxy)octane, 2,5-dimethyl-2,5-di(benzoylperoxy)hexane, di(trimethylsilyl)peroxide, trimethylsilyltriphenylsilylperoxide, 2-phenylazo-4-methoxy-2,4-dimethylvaleronitrile, 1-[(1-cyano-1-methylethyl)azo]formamide, 1,1'-azobis(cyclohexane-1-carbonitrile), 2,2'-azobis(2-methylbutyronitrile), 2, 2'-Azobisisobutyronitrile, 2,2'-Azobis(2,4-dimethylvaleronitrile), 2,2'-Azobis(2,4-dimethyl-4-methoxyvaleronitrile), 2,2'-Azobis(2-methylpropionamidine) dihydrochloride, 2,2'-Azobis(2-methyl-N-phenylpropionamidine) dihydrochloride, 2,2'-Azobis[N-(4-chlorophenyl)-2-methylpropionamidine] dihydrochloride, 2,2'-Azobis[N-(4-hydrophenyl)-2-methylpropionamidine] dihydrochloride , 2,2'-azobis[2-methyl-N-(phenylmethyl)propionamidine]dihydrochloride, 2,2'-azobis[2-methyl-N-(2-propenyl)propionamidine]dihydrochloride, 2,2'-azobis[N-(2-hydroxyethyl)-2-methylpropionamidine]dihydrochloride, 2,2'-azobis[2-(5-methyl-2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(4,5,6,7-tetrahydro-1H-1,3-diazepin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis[2-(5-hydroxy-3,4,5,6-tetrahydropyrimidin-2-yl)propane]dihydrochloride, 2,2'-azobis{2-[1-(2-hydroxyethyl)-2-imidazolin-2-yl]propane}dihydrochloride, 2,2'-azobis[2-(2-imidazolin-2-yl)propane], 2,2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)-2-hydroxyethyl]propionamide}, 2 , 2'-azobis{2-methyl-N-[1,1-bis(hydroxymethyl)ethyl]propionamide}, 2,2'-azobis[2-methyl-N-(2-hydroxyethyl)propionamide], 2,2'-azobis(2-methylpropionamide), 2,2'-azobis(2,4,4-trimethylpentane), 2,2'-azobis(2-methylpropane), dimethyl-2,2-azobis(2-methylpropionate), 4,4'-azobis(4-cyanopentanoic acid), 2,2'-azobis[2-(hydroxymethyl)propionitrile], 2,2'-azobis(tert-butane), and other azo compounds, 2,3-dimethyl-2,3-diphenylbutane, etc., are included. On the other hand, the photoradical polymerization initiator is not particularly limited, and examples thereof include 2,2-diethoxyacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 1-hydroxycyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-[4-(2-hydroxyethoxy)phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)benzyl]phenyl}-2-methylpropan-1-one, 2-methyl-1-(4- alkylphenone compounds such as 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, benzophenone compounds such as 4,4'-bis(dimethylamino)benzophenone, and 2-carboxybenzophenone, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin benzoin compounds such as benzoin isobutyl ether, thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, and other thioxanthone compounds, 2-(4-methoxyphenyl)-4,6-bis(trichloromethyl)-sec-triazine, 2-(4-methoxynaphthyl)-4,6-bis(trichloromethyl)-sec-triazine, 2-(4-ethoxynaphthyl)-4,6-bis(trichloromethyl)-sec-triazine, 2-(4-ethoxyphenyl)-4,6-bis(trichloromethyl)-sec-triazine, halomethylated triazine compounds such as 2-trichloromethyl-5-[β-(2'-benzofuryl)vinyl]-1,3,4-oxadiazole, 2-trichloromethyl-5-[β-(2'-(6"-benzofuryl)vinyl)]-1,3,4-oxadiazole, and 2-trichloromethyl-5-furyl-1,3,4-oxadiazole; halomethylated oxadiazole compounds such as 2,2'-bis(2-chlorophenyl)-4,4',5,5'-tetraphenyl-1,Biimidazole compounds such as 2'-biimidazole, 2,2'-bis(2,4-dichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, and 2,2'-bis(2,4,6-trichlorophenyl)-4,4',5,5'-tetraphenyl-1,2'-biimidazole, 1-[4-(phenylthio)-,2-(O-benzoyloxime)]-1,2-octanedione, 1-[9-ethyl-6-(2-methylbenzoyl) Examples of the compounds include oxime ester compounds such as bis(η5-2,4-cyclopentadiene-1-yl)-bis(2,6-difluoro-3-(1H-pyrrol-1-yl)-phenyl)titanium, titanocene compounds such as p-dimethylaminobenzoic acid and p-diethylaminobenzoic acid, and acridine compounds such as 9-phenylacridine. The photocationic polymerization initiator generates a strong acid such as tetrafluoroboric acid or hexafluorophosphoric acid upon UV irradiation or heating, and this strong acid protonates an oxygen atom of a cationic polymerizable compound described below to form a cationic active species, thereby initiating a polymerization reaction. Any known compound can be used without any particular limitation. Examples of the photocationic polymerization initiator include aromatic sulfonium salts (C1), aromatic iodonium salts (C2), aromatic diazonium salts, aromatic ammonium salts, thioxanthonium salts, and (2,4-cyclopentadiene-1-yl)[(1-methylethyl)benzene]-iron salts, each of which has a cationic moiety of aromatic sulfonium, aromatic iodonium, aromatic diazonium, aromatic ammonium, thioxanthonium, (2,4-cyclopentadiene-1-yl)[(1-methylethyl)benzene]-iron cation, or thianthrhenium, and an anionic moiety of BF4-, PF6-, SbF6-, or [BX4]- (wherein X represents a functional group in which two or more hydrogen atoms of a phenyl group are substituted with fluorine atoms or trifluoromethyl groups). These photocationic polymerization initiators may be used alone or in combination of two or more kinds in any ratio as necessary.Examples of the aromatic sulfonium salt (C1) include bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluorophosphate, bis[4-(diphenylsulfonio)phenyl]sulfide bishexafluoroantimonate, bis[4-(diphenylsulfonio)phenyl]sulfide bistetrafluoroborate, bis[4-(diphenylsulfonio)phenyl]sulfide tetrakis(pentafluorophenyl)borate, diphenyl-4-(phenylthio)phenylsulfonium hexafluorophosphate, diphenyl-4-(phenylthio)phenylsulfonium hexafluoroantimonate, diphenyl-4-(phenylthio)phenylsulfonium tetrafluoroborate, and diphenyl-4-(phenylthio)phenylsulfonium. Tetrakis(pentafluorophenyl)borate, triphenylsulfonium hexafluorophosphate, triphenylsulfonium hexafluoroantimonate, triphenylsulfonium tetrafluoroborate, triphenylsulfonium tetrakis(pentafluorophenyl)borate, bis[4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl]sulfide bishexafluorophosphate, bis[4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl]sulfide bishexafluoroantimonate, bis[4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl]sulfide bistetrafluoroborate, bis[4-(di(4-(2-hydroxyethoxy))phenylsulfonio)phenyl]sulfide tetrakis(pentafluorophenyl)borate, and the like can be used.Examples of the aromatic iodonium salt (C2) include diphenyliodonium hexafluorophosphate, diphenyliodonium hexafluoroantimonate, diphenyliodonium tetrafluoroborate, diphenyliodonium tetrakis(pentafluorophenyl)borate, bis(dodecylphenyl)iodonium hexafluorophosphate, bis(dodecylphenyl)iodonium hexafluoroantimonate, bis(dodecylphenyl)iodonium tetrafluoroborate, bis(dodecylphenyl)iodonium tetrakis(pentafluorophenyl)borate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluorophosphate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium hexafluoroantimonate, 4-methylphenyl-4-(1-methylethyl)phenyliodonium tetrafluoroborate, and 4-methylphenyl-4-(1-methylethyl)phenyliodonium. Tetrakis(pentafluorophenyl)borate, etc. can be used. In addition, examples of aromatic diazonium salts that can be used include phenyldiazonium hexafluorophosphate, phenyldiazonium hexafluoroantimonate, phenyldiazonium tetrafluoroborate, and phenyldiazonium tetrakis(pentafluorophenyl)borate. In addition, examples of aromatic ammonium salts that can be used include 1-benzyl-2-cyanopyridinium hexafluorophosphate, 1-benzyl-2-cyanopyridinium hexafluoroantimonate, 1-benzyl-2-cyanopyridinium tetrafluoroborate, 1-benzyl-2-cyanopyridinium tetrakis(pentafluorophenyl)borate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluorophosphate, 1-(naphthylmethyl)-2-cyanopyridinium hexafluoroantimonate, 1-(naphthylmethyl)-2-cyanopyridinium tetrafluoroborate, and 1-(naphthylmethyl)-2-cyanopyridinium tetrakis(pentafluorophenyl)borate.As the thioxanthonium salt, S-biphenyl 2-isopropyl thioxanthonium hexafluorophosphate and the like can be used. As the (2,4-cyclopentadiene-1-yl) [(1-methylethyl) benzene]-iron salt, (2,4-cyclopentadiene-1-yl) [(1-methylethyl) benzene]-iron (II) hexafluorophosphate, (2,4-cyclopentadiene-1-yl) [(1-methylethyl) benzene]-iron (II) hexafluoroantimonate, 2,4-cyclopentadiene-1-yl) [(1-methylethyl) benzene]-iron (II) tetrafluoroborate, 2,4-cyclopentadiene-1-yl) [(1-methylethyl) benzene]-iron (II) tetrakis (pentafluorophenyl) borate and the like can be used. These can be used alone or in combination of two or more kinds. The amount of the curing catalyst (C) to be blended relative to the total amount of the components (A), (B) and (C) must satisfy the following formula (7). (C) / (A+B+C)=0.1-4.9(wt%) (7) The amount of component (C) is preferably 0.2 to 2.0 (wt%). If the amount of component (C) is less than 0.1 wt%, the degree of improvement in moldability and heat resistance of the curable composition due to the addition of the curing catalyst (C) is insufficient, whereas if it exceeds 4.9 wt%, the mechanical properties are unfavorably reduced.
[0054] The resin composition of the present invention may contain a flame retardant. As the flame retardant, a wide variety of known flame retardants may be used, such as halogen-based flame retardants, phosphate-based flame retardants, phosphazene-based flame retardants, and phosphinate-based flame retardants. A filler can be blended in the curable resin composition of the present invention. The filler can be added for the purpose of improving the heat resistance of the cured product, and is not particularly limited. For example, metal oxides such as silica, metal hydroxides such as mica, talc, etc. can be mentioned. The content of the filler is, for example, 10 to 200 parts by mass with respect to 100 parts by mass of the total of the composition. The curable resin composition of the present invention may also contain other additives, such as antifoaming agents such as silicone-based antifoaming agents and acrylic acid ester-based antifoaming agents, heat stabilizers, antistatic agents, ultraviolet absorbers, dyes or pigments, lubricants, dispersants, etc., as necessary.
[0055] The curable resin composition of the present invention can be prepared into a varnish to be used as a resin varnish for the purpose of impregnating a substrate (fibrous substrate) for forming a prepreg when producing a prepreg, or for the purpose of using the composition as a circuit board material for a printed wiring board, a printed circuit board, a flexible printed wiring board, a build-up wiring board, etc. The resin varnish is prepared by dissolving the resin composition in an organic solvent. The organic solvent is not particularly limited as long as it dissolves the curable resin composition and does not inhibit the curing reaction, and any known organic solvent can be used. For example, ketones such as acetone, methyl ethyl ketone, and methyl isobutyl ketone, esters such as ethyl acetate, propyl acetate, and butyl acetate, polar solvents such as dimethylacetamide and dimethylformamide, and aromatic hydrocarbon solvents such as toluene and xylene can be used alone or in combination of two or more. When preparing the resin varnish, the amount of the organic solvent used is, for example, 10 to 1000 parts by weight based on 100 parts by weight of the curable resin composition of the present invention.
[0056] The cured product obtained by curing the curable resin composition of the present invention can be used as a molded product, a laminate, a casting, an adhesive, a coating, or a film. The cured product of the varnish for circuit boards is a laminate, and the method for obtaining this cured product can be to impregnate a substrate such as glass fiber, carbon fiber, polyester fiber, polyamide fiber, alumina fiber, or paper with the varnish for circuit boards, heat and dry the substrate to obtain a prepreg, which can be laminated alone or with a metal foil such as copper foil, and then hot press molded.
[0057] The curable resin composition of the present invention can also be used together with a substrate as a curable composite material. As the substrate, known materials are used, and examples thereof include various glass cloths such as roving cloth, cloth, chopped mat, and surfacing mat, asbestos cloth, metal fiber cloth, and other synthetic or natural inorganic fiber cloths, woven or nonwoven fabrics obtained from liquid crystal fibers such as fully aromatic polyamide fibers, fully aromatic polyester fibers, and polybenzozal fibers, woven or nonwoven fabrics obtained from synthetic fibers such as polyvinyl alcohol fibers, polyester fibers, and acrylic fibers, natural fiber cloths such as cotton cloth, linen cloth, and felt, carbon fiber cloth, and natural cellulose-based cloths such as kraft paper, cotton paper, and paper-glass mixed fiber paper, and other cloths and papers, which can be used alone or in combination of two or more kinds. The blending ratio of the substrate in the curable composite material is, for example, in the range of 5 to 90% by weight. If necessary, a coupling agent, such as a silane coupling agent, a titanate coupling agent, an aluminum-based coupling agent, or a zircoaluminate coupling agent, may be used to improve the interfacial adhesion between the resin and the substrate. The curable composite material can be obtained, for example, by dissolving the curable resin composition in an organic solvent, impregnating the substrate with the composition, and then drying the composition. The curable composite material can be cured by a method such as heating to obtain a cured composite material. The curable resin composition or the curable composite material can be cured, for example, at a temperature of 80 to 300°C and a pressure of 0.1 to 1000 kg / cm. 2 This can be done within the range.
[0058] The laminate of the present invention is composed of a cured composite material layer and a metal foil layer, and an adhesive may be used as necessary. Examples of the metal foil include copper foil and aluminum foil, and the thickness thereof is, for example, in the range of 1 to 200 μm. The curable resin composition of the present invention can also be molded into a film having a thickness of, for example, 1 to 200 μm. EXAMPLES
[0059] The present invention will now be described with reference to examples, but is not limited thereto. In each example, all parts are by weight. The methods for measuring and evaluating each physical property are as follows.
[0060] 1) Polymer molecular weight and molecular weight distribution The molecular weight and molecular weight distribution of the polymer were measured using GPC (Tosoh Corporation, HLC-8220GPC) and a Tosoh Corporation, TSKgel MultiporeH column. XL -M: 2 pieces, TSKgel G1000H XL The column used was one TSKguardcolumn MP(XL) as a guard column, tetrahydrofuran (THF) as a solvent, a flow rate of 1.0 ml / min, a column temperature of 38°C, and a calibration curve based on monodisperse polystyrene.
[0061] 2) Polymer structure Using a JEOL JNM-LA600 nuclear magnetic resonance spectrometer, 13 C-NMR and 1 The NMR analysis was performed using 1H NMR spectroscopy in chloroform-d1 as the solvent and the resonance line of tetramethylsilane as the internal standard.
[0062] 3) Analysis of end groups The calculation of the end group is as follows: 13 C-NMR and 1 The amount of vinyl groups introduced at the terminals was calculated from the H-NMR measurement results, and the number of vinyl terminal groups contained in one molecule of the modified vinyl aromatic polymer was calculated from the amount of vinyl groups introduced at the terminals and the number average molecular weight obtained by the above GPC measurement.
[0063] 4) Thermogravimetry (TGA) The weight loss at 350℃ (TGA) was measured according to JIS K7120. 350 ) was sought.
[0064] Synthesis Example 1 Synthesis of modified vinyl aromatic polymer (A) 300 ml (233.7 g) of cyclohexane and 8.71 ml (60.0 mmol) of triethylamine (cocatalyst) were charged, and 3.84 g (60.0 mmol) of sec-butyllithium (pure content) was added at 30°C. [ka] After adding 46.2 ml of n-hexane solution containing [ka] A solution of 60 ml (46.7 g) of cyclohexane was added over 3 hours. Stirring was continued at 30°C for 1 hour, and the first stage initiation reaction was completed. It is believed that this initiation reaction produces the following polyfunctional anionic polymerization initiator (z1). [ka] Next, 50.0 g (0.48 mol) of styrene (structural formula below) [ka] was added over 60 min to initiate the second stage polymerization. The temperature of the reaction solution rose due to the heat of polymerization, reaching a maximum temperature of 65°C. After the polymerization reaction was completed, a small sample of the polymerization solution was taken and analyzed by gas chromatography (GC). No unreacted monomer was observed, and it was confirmed that the polymerization conversion rate was nearly 100%. GPC analysis showed that the Mn of the polymer at the end of the second stage polymerization was 3500, Mw was 4010, and Mw / Mn was 1.14. Next, 9.16 g (60.0 mmol) of chloromethylstyrene (structural formula below, manufactured by AGC Seimi Chemical, CMS-14) was added as a modifier. [ka] The modified vinyl aromatic polymer-containing polymer solution obtained in the second stage polymerization was added to a three-neck flask containing 200 ml (155.8 g) of cyclohexane over a period of 15 minutes to carry out the third stage modification reaction. After the modification reaction was completed, filtration was carried out. The obtained polymerization solution was poured into a large amount of methanol, and the reprecipitated modified vinyl aromatic polymer was filtered and then dried in a vacuum dryer at 30°C to obtain 63.24 g (yield: 97.0 wt%) of modified vinyl aromatic polymer (A) calculated as solid content.
[0065] The analytical results of the modified vinyl aromatic polymer (A) are shown in Table 1. When the recovered modified vinyl aromatic polymer (A) was dissolved in cyclohexane, no formation of gel or microgel was observed. The resulting modified vinyl aromatic polymer (A) had an Mn of 4540, an Mw of 6210, and an Mw / Mn ratio of 1.37. 13 C-NMR and 1 By H-NMR analysis, it was confirmed that the modified vinyl aromatic polymer (A) contains 9.52 mol % (5.26 wt %) of structural units derived from sec-butyllithium, 4.76 mol % (7.28 wt %) of structural units derived from diisopropenylbenzene, 76.19 mol % (76.68 wt %) of structural units derived from styrene, and 9.52 mol % (10.55 wt %) of structural units derived from chloromethylstyrene, and that 4.10 units of the modifier were introduced per molecule of the modified vinyl aromatic polymer (A). A polyfunctional anionic polymerization initiator (z1) was produced by an initiation reaction between sec-butyllithium (e) and diisopropenylbenzene (b), and then styrene (a) was polymerized. The polymer was then modified at its active end with chloromethylstyrene. In the structural units derived from the reaction involving styrene (a), diisopropenylbenzene (b), and sec-butyllithium (e), the proportion of structural units containing multiple independent structural units (M1) derived from styrene (a) (initiator-derived multiple polymer unit structure degree) was 94.7 mol%. Thermogravimetric analysis (TGA) showed that the weight loss at 350°C (TGA 350 ) was 0.67 wt%.
[0066] Comparative synthesis example 1 3.0 mol (390.6 g) of divinylbenzene, 1.8 mol (229.4 g) of ethylvinylbenzene, 10.2 mol (1066.3 g) of styrene, and 15.0 mol (1532.0 g) of n-propyl acetate were charged into a 5.0 L reactor, and 600 mmol of a diethyl ether complex of boron trifluoride was added at 70 ° C. and reacted for 4 hours. After the polymerization solution was stopped with an aqueous sodium bicarbonate solution, the oil layer was washed three times with pure water, and the polymer was recovered by degassing under reduced pressure at 60 ° C. The obtained polymer was weighed, and it was confirmed that 896.7 g of vinyl aromatic polymer (B) was obtained.
[0067] The resulting vinyl aromatic polymer (B) had an Mn of 2,980, an Mw of 41,300, and an Mw / Mn of 13.9. 13 C-NMR and 1 Based on the results of H-NMR analysis, GC analysis, and the number average molecular weight converted into standard polystyrene, the constitutional units of polymer (B) were calculated as follows. Structural units derived from divinylbenzene (a): 30.4 mol% (33.1 wt%) Structural units derived from ethylvinylbenzene (c): 12.2 mol% (14.2 wt%) Structural units derived from styrene (b): 57.4 mol% (52.7 wt%) Structural units having residual vinyl groups derived from divinylbenzene (a): 23.9 mol% (25.9 wt%) Content of pendant vinyl group-containing DVB units per molecule of vinyl aromatic polymer (B): 5.93 (units / molecule) The polymerization reaction of Comparative Synthesis Example 1 does not use sec-butyl lithium (e) unlike Synthesis Example 1, and does not generate a polyfunctional anionic polymerization initiator, so it is a cationic polymerization of divinylbenzene (b), ethylvinylbenzene (a) and styrene (a), and is not a living polymerization, so that structural units derived from the polyfunctional anionic polymerization initiator could not be detected in the polymer. However, 9.9 mol % (10.8 wt %) of the structural units derived from divinylbenzene (a) in the polymer were branched structures, so the apparent degree of multiple polymer unit structure not derived from the initiator was 32.6 mol %. As a result of TGA measurement, the weight loss at 350°C was 1.83 wt%. The vinyl aromatic polymer (B) was soluble in toluene, xylene, THF, dichloroethane, dichloromethane, and chloroform (100 g or more of the vinyl aromatic polymer (B) was dissolved in 100 g of each solvent), and no gel formation was observed.
[0068] Synthesis Example 2 Synthesis of modified vinyl aromatic polymer (C) 300 ml (233.7 g) of cyclohexane and 4.90 ml (60.0 mmol) of the cocatalyst tetrahydrofuran were charged, and 3.84 g (60.0 mmol) of sec-butyllithium was added at 30°C. [ka] After adding 46.2 ml of n-hexane solution containing [ka] A solution of 60 ml (46.7 g) of cyclohexane was added over 3 hours. Stirring was continued at 30° C. for 1 hour, and the first stage initiation reaction was completed. Therefore, as in Synthesis Example 1, this initiation reaction is considered to produce the above-mentioned polyfunctional anionic polymerization initiator (z1). Next, 25.0 g (0.24 mol) of styrene (structural formula below) [ka] was added over 60 min to initiate the second stage polymerization. The temperature of the reaction solution rose due to the heat of polymerization, reaching a maximum temperature of 65°C. After the polymerization reaction was completed, a small sample of the polymerization solution was taken and analyzed by gas chromatography (GC). No unreacted monomer was observed, and it was confirmed that the polymerization conversion rate was nearly 100%. GPC analysis showed that the Mn of the polymer at the end of the second stage polymerization was 1760, Mw was 2020, and Mw / Mn was 1.15. Next, 9.16 g (60.0 mmol) of chloromethylstyrene (structural formula below, manufactured by AGC Seimi Chemical, CMS-14) was added as a modifier. [ka] The modified vinyl aromatic polymer-containing polymer solution obtained in the second stage polymerization was added to a three-neck flask containing 200 ml (155.8 g) of cyclohexane over a period of 15 minutes to carry out the third stage modification reaction. After the modification reaction was completed, filtration was carried out. The obtained polymerization solution was poured into a large amount of methanol, and the reprecipitated modified vinyl aromatic polymer was filtered and then dried in a vacuum dryer at 30°C to obtain 39.40 g (yield: 98.0 wt%) of modified vinyl aromatic polymer (C) in terms of solid content.
[0069] The analytical results of the modified vinyl aromatic polymer (C) are shown in Table 1. When the recovered modified vinyl aromatic polymer (C) was dissolved in cyclohexane, no formation of gel or microgel was observed. The resulting modified vinyl aromatic polymer (C) had an Mn of 2260, an Mw of 3140, and an Mw / Mn of 1.39. 13 C-NMR and 1 By H-NMR analysis, it was confirmed that the modified vinyl aromatic polymer (C) contained 15.38 mol % (8.53 wt %) of structural units derived from sec-butyllithium, 7.69 mol % (11.81 wt %) of structural units derived from diisopropenylbenzene, 61.54 mol % (62.18 wt %) of structural units derived from styrene, and 15.38 mol % (17.49 wt %) of structural units derived from chloromethylstyrene, and that 3.75 units of the modifier were introduced per molecule of the modified vinyl aromatic polymer (C). A polyfunctional anionic polymerization initiator (z1) was produced by an initiation reaction between sec-butyllithium (e) and diisopropenylbenzene (b), and then styrene (a) was polymerized. The active end of the polymer was then modified with chloromethylstyrene. In the structural units derived from the reaction involving styrene (a), diisopropenylbenzene (b), and sec-butyllithium (e), the proportion of structural units containing multiple independent structural units (M1) derived from styrene (a) (initiator-derived multiple polymer unit structure degree) was 89.6 mol%. Thermogravimetric analysis (TGA) showed that the weight loss at 350°C (TGA 350 ) was 0.81 wt%.
[0070] The analytical results of the modified vinyl aromatic polymers of Synthesis Examples 1 and 2 and Comparative Synthesis Example 1 are shown in Table 1. [Table 1]
[0071] Synthesis Example 3 Synthesis of modified vinyl aromatic polymer (D) (modification with silane compound) 270 ml (210.3 g) of cyclohexane and 5 g of a cyclohexane solution containing 1.73 ml (9.0 mmol) of 2,2-di(2-tetrahydrofuryl)propane were charged, and 50 g of a cyclohexane solution containing 2.88 g (45.0 mmol) of n-butyllithium was added at 50°C. Then, 4.71 g of DVB-630 (structural formula below) from which impurities had been removed (divinylbenzene (mixture of m- and p-forms) component: 22.5 mmol, ethylvinylbenzene (mixture of m- and p-forms) component: 13.7 mmol), [ka] Styrene (structural formula below) 28.01g (269mmol) [ka] The polymerization was started by adding the polymerisation heat. The temperature of the reaction solution rose due to the heat of polymerization, and reached a maximum of 81°C. After the polymerization reaction was completed, 12.53 g (45.0 mmol) of 3-glycidoxypropyltriethoxysilane (GPTES: structural formula below) was added to the reactor as a modifier. [ka] After the polymerization reaction was completed, 10.63 g (90.0 mmol) of succinic acid was added, and the mixture was stirred and filtered. The resulting polymerization solution was concentrated by devolatilization to obtain 44.43 g (yield: 98.2 wt %) of a functional group-modified vinyl aromatic polymer D in terms of solid content.
[0072] The resulting functional group-modified vinyl aromatic polymer (D) had an Mn of 2410, an Mw of 4240, and an Mw / Mn of 1.76. 13 C-NMR and 1By H-NMR analysis, functional group modified vinyl aromatic copolymer D contained 6.43 mol% (6.47 wt%) of structural units derived from divinylbenzene, 3.92 mol% (3.94 wt%) of structural units derived from ethylvinylbenzene, 76.8 mol% (61.9 wt%) of structural units derived from styrene, and 12.9 mol% (27.7 wt%) of structural units derived from 3-glycidoxypropyltriethoxysilane. The crosslinked structural units derived from divinyl aromatic compounds were 6.30 mol% (6.34 wt%), so the crosslinking degree (crosslinked structural units derived from divinyl aromatic compounds / structural units derived from divinyl aromatic compounds), which represents the ratio of crosslinked structural units to structural units derived from divinyl aromatic compounds, was 0.98. In addition, the structural unit derived from divinylbenzene having a residual vinyl group contained in the functional group modified vinyl aromatic copolymer D was 0.13 mol% (0.13wt%), so the molar fraction of the vinyl group-containing structural unit derived from divinylbenzene to the sum of the structural units derived from divinyl aromatic compounds and the structural units derived from monovinyl aromatic compounds was 0.0015. The amount of GPTES modifier introduced was an average of 2.4 functional groups per molecule. In addition, 50 mol% or more of these functional groups were alkoxysilyl groups, and the remainder were hydroxyl groups, etc. The TGA measurement results showed that the weight loss at 350°C was 0.98wt%. A sample prepared by dissolving 0.5g of functional group modified vinyl aromatic copolymer D in 100g of toluene was placed in a quartz cell, and the haze (turbidity) was measured using an integrating sphere light transmittance measuring device with toluene as the reference sample. The haze value was 0.03.
[0073] Examples 1 to 6, Comparative Examples 1 and 2 Resin compositions were prepared using the polymers A to D obtained in Synthesis Examples 1 to 3 and Comparative Synthesis Example 1. That is, in the blending ratios (parts by weight) shown in Tables 2 to 3, each of the polymers A to D, the curable reactive resin SA9000, the curable reactive resin OPE-2St, the thermoplastic resin K-1, and the heat stabilizer S-1 were blended together with the solvent toluene, stirred to dissolve, and then curing catalysts (reaction initiators) P-1 and P-2 were added to prepare a resin composition solution.
[0074] Here, the components used are as follows: Thermoplastic resin K-1: Hydrogenated styrene-butadiene block copolymer (Kraton Polymer Japan Co., Ltd., product name: KRATON A1536HU) Curable reactive resin SA9000: Polyphenylene oligomer with methacryloyl groups at both ends, in which the terminal hydroxyl groups of polyphenylene ether have been modified with methacryloyl groups (Mw=1900, number of terminal functional groups: 2 / molecule, manufactured by SABIC Innovative Plastics, Inc.) Curable reactive resin OPE-2St-1: Polyphenylene oligomer with vinyl groups at both ends (Mn=1160, manufactured by Mitsubishi Gas Chemical Co., Ltd., reaction product of 2,2',3,3',5,5'-hexamethylbiphenyl-4,4'-diol·2,6-dimethylphenol polycondensate and chloromethylstyrene) Heat stabilizer S-1: Pentaerythritol tetrakis[3-(3,5-di-tert-butyl-4-hydroxyphenyl)propionate] (manufactured by ADEKA Corporation, product name: Adeka STAB AO-60) Curing catalyst P-1: 2,2'-azobis(2,4,4-trimethylpentane) (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., product name: VR-110) Curing catalyst P-2: α,α'-di(t-butylperoxy)diisopropylbenzene (manufactured by NOF Corporation, trade name: Perbutyl P)
[0075] The prepared thermosetting resin composition solution was cast onto a stand with a polyethylene terephthalate resin (PET) sheet attached to obtain a film. The obtained film had a thickness of about 50 to 60 μm, was not sticky, and had excellent film-forming properties. This film was dried in an air oven at 80°C for 10 minutes, and then thermally cured at 180°C for 1 hour in a vacuum press molding machine to obtain a cured film of about 50 μm. The properties of the resulting cured film were measured and evaluated, and the results are shown in Tables 3 to 6.
[0076] 1) Solution viscosity The viscosity of the varnish solution of the resin composition was measured at a measurement temperature of 25°C using an E-type viscometer.
[0077] 2) Tensile strength and tensile elongation at break Tensile strength and elongation were measured using a tensile testing device. Elongation was measured from a tensile test chart.
[0078] 3) Glass transition temperature The test pieces used for the glass transition temperature test were prepared by vacuum press molding a 50 μm thick cured film using a vacuum press molding machine, and test pieces with a width of 3.0 mm, a thickness of 50 μm, and a length of 40 mm were prepared. These test pieces were set in a DMA (dynamic viscoelasticity measurement device) measuring device and measured by scanning from 30°C to 320°C at a heating rate of 3°C / min under a nitrogen stream, and Tg was determined from the peak top of the tan δ curve.
[0079] 4) Dielectric constant and dielectric tangent In accordance with the JIS C2565 standard, the dielectric constant and dielectric loss tangent at 18 GHz were measured using a cavity resonator dielectric constant measuring device manufactured by AET Corporation, using flat test pieces of the cured product that had been dried and then stored for 24 hours in a room at a temperature of 23°C and a humidity of 50%. In addition, the cured product plate test pieces were left to stand for 500 hours at a temperature of 85° C. and a relative humidity of 85%, after which the dielectric constant and dielectric loss tangent were measured, and the dielectric constant and dielectric loss tangent after a moist heat resistance test were also measured. Furthermore, in order to confirm the heat resistance reliability of the material, the cured flat test piece was left in an air atmosphere at a temperature of 135°C for 150 hours, and then the dielectric constant and dielectric loss tangent were measured. The dielectric constant and dielectric loss tangent after the heat resistance reliability test were measured.
[0080] 5) Copper foil peel strength The resin composition varnish was cast on a 18μm thick copper foil (product name F2-WS copper foil, Rz 2.0μm, Ra 0.3μm) to prepare a resin-coated copper foil, which was then dried in an air oven at 80℃ for 10 minutes, placed on an FR-4 substrate with the copper foil etched out, and molded and cured by a vacuum press molding machine to obtain a laminate for evaluation. The curing conditions were a temperature rise of 3℃ / min, a pressure of 3MPa, and a retention time of 60 minutes at 200℃ to obtain a cured laminate as a copper-clad laminate for evaluation. A test piece 20 mm wide and 100 mm long was cut out from the cured laminate obtained in this way, and a 10 mm wide parallel cut was made on the copper foil surface, after which the copper foil was continuously peeled off at a speed of 50 mm / min in a direction 90° to the surface, and the stress at that time was measured with a tensile tester, and the minimum stress value was recorded as the copper foil peel strength (based on JIS C6481). The copper foil peel strength test after the moist heat resistance test was performed by leaving the above test pieces at a temperature of 85° C. and a relative humidity of 85% for 500 hours, and then measuring the peel strength in the same manner as above.
[0081] 6) Formability An uncured film of the curable resin composition was laminated on a copper-clad laminate that had been subjected to a blackening treatment, and vacuum lamination was performed using a vacuum laminator at a temperature of 110°C and a press pressure of 0.1 MPa, and the adhesion state between the blackened copper foil and the film was evaluated. The evaluation was performed with a rating of "○" for a good adhesion state between the blackened copper foil and the film, and with a rating of "×" for an adhesion state in which the blackened copper foil and the film could be easily peeled off.
[0082] [Table 2]
[0083] [Table 3]
[0084] According to Tables 2 to 3, the curable resin compositions of Examples 1 to 6 have improved compatibility with thermoplastic resins and therefore improved adhesion to copper foil, compared to the comparative examples. Furthermore, they are materials that have excellent dielectric properties after a moist heat resistance test and a heat resistance reliability test, and also have good moldability.
[0085] Synthesis Example 4 Synthesis of modified vinyl aromatic polymer (E) 250 ml (194.8 g) of cyclohexane and 2.94 ml (36.0 mmol) of the cocatalyst tetrahydrofuran were charged, and 3.84 g (60.0 mmol) of sec-butyllithium was added at 50°C. [ka] After adding 46.2 ml of a cyclohexane / n-hexane solution containing [ka] A solution of 60 ml (46.7 g) of cyclohexane was added over 1 hour. Stirring was continued at 50°C for 15 hours, and the first stage initiation reaction was completed. It is believed that this initiation reaction produces the following polyfunctional anionic polymerization initiator (z2). [ka] Next, the temperature of the reactor was lowered to 30°C, and 50.0 g (0.48 mol) of styrene (structural formula below) was added. [ka] was added over 60 min to initiate the second stage polymerization. The temperature of the reaction solution rose due to the heat of polymerization, reaching a maximum temperature of 58°C. After the polymerization reaction was completed, a small sample of the polymerization solution was taken and analyzed by gas chromatography (GC). No unreacted monomer was observed, and it was confirmed that the polymerization conversion rate was nearly 100%. GPC analysis showed that the Mn of the polymer at the end of the second stage polymerization was 1860, Mw was 2530, and Mw / Mn was 1.36. Next, 9.16 g (60.0 mmol) of chloromethylstyrene (structural formula below, manufactured by AGC Seimi Chemical, CMS-14) was added as a modifier. [ka] The modified vinyl aromatic polymer-containing polymer solution obtained in the second stage polymerization was added to a three-neck flask containing 200 ml (155.8 g) of cyclohexane over a period of 30 minutes to carry out the third stage modification reaction. After the modification reaction was completed, filtration was carried out. The obtained polymerization solution was poured into a large amount of methanol, and the reprecipitated modified vinyl aromatic polymer was filtered and then dried in a vacuum dryer at 30°C to obtain 57.80 g (yield: 96.0 wt%) of modified vinyl aromatic polymer (E) calculated as solid content.
[0086] The analytical results of the modified vinyl aromatic polymer (E) are shown in Table 4. When the recovered modified vinyl aromatic polymer (E) was dissolved in cyclohexane, no formation of gel or microgel was observed. The resulting modified vinyl aromatic polymer (E) had an Mn of 2550, an Mw of 6210, and an Mw / Mn ratio of 1.68. 13 C-NMR and 1 By H-NMR analysis, it was confirmed that the modified vinyl aromatic polymer (E) contained 5.26 mol % (5.29 wt %) of structural units derived from m-xylene, 84.21 mol % (83.03 wt %) of structural units derived from styrene, and 10.53 mol % (11.68 wt %) of structural units derived from chloromethylstyrene, and that 2.34 units of the modifier were introduced per molecule of the modified vinyl aromatic polymer (E). A polyfunctional anionic polymerization initiator (z2) was produced by an initiation reaction between sec-butyllithium (e) and xylene (c), and then styrene (a) was polymerized. The active end of the polymer was then modified with chloromethylstyrene. In the structural units derived from the reaction involving styrene (a), xylene (c), and sec-butyllithium (e), the proportion of structural units containing multiple independent structural units (M1) derived from styrene (a) (initiator-derived multiple polymer unit structure degree) was 85.7 mol%. Thermogravimetric analysis (TGA) showed that the weight loss at 350°C (TGA 350 ) was 0.67 wt%.
[0087] [Table 4]
[0088] Examples 7 and 8 Using the polymer E obtained in Synthesis Example 4, a resin composition solution was prepared in the blending ratio (parts by weight) shown in Table 5. [Table 5]
[0089] According to Table 5, the curable resin compositions of Examples 7 and 8 also exhibit excellent dielectric properties and adhesive properties after curing. [Industrial Applicability]
[0090] The curable resin composition of the present invention is useful as a dielectric material, insulating material, heat-resistant material, structural material, adhesive, sealant, paint, coating agent, sealant, printing ink, dispersant, etc. in fields such as the electric / electronic industry, the space / aircraft industry, and the building / construction industry. Furthermore, it can be processed into a film, sheet, or prepreg and used in plastic optical parts, touch panels, flat displays, film liquid crystal elements, and various optical elements such as optical waveguides and optical lenses.
Claims
1. (A) in the presence of a polyfunctional anionic polymerization initiator produced by reacting a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of an organic alkali metal compound (e), a modified vinyl aromatic polymer in which the active terminal of a polymer obtained by polymerizing a monovinyl aromatic compound (a) is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h); 50 mol % or more of the total of structural units derived from reactions involving the components (a), (b), (c), and (e) are one or more structural units selected from the group consisting of structural units (d1), (d2), and (d3), each of which independently contains a plurality of structural units (M1) derived from a monovinyl aromatic compound (a) represented by the following formulas (1), (2), and (3): less than 50 mol % in total of the structural units derived from the reaction involving the components (a), (b), (c), and (e) are one or more structural units selected from the group consisting of structural units (d4) and (d5) each containing solely a structural unit (M1) derived from the monovinyl aromatic compound (a) represented by the following formulas (4) and (5): 【Chemistry 1】 【Chemistry 2】 (R1 represents an aromatic hydrocarbon group having 6 to 30 carbon atoms, R2 represents hydrogen or a hydrocarbon group having 1 to 3 carbon atoms, R3 represents a hydrocarbon group having 1 to 30 carbon atoms, and R4 represents hydrogen or a hydrocarbon group having 1 to 15 carbon atoms. M1 represents a structural unit derived from a monovinyl aromatic compound (a). m represents an integer of 1 to 3. In addition, l, n, o, p, s, t, u, v, and w represent the degree of polymerization of the structural unit derived from the monovinyl aromatic compound (a).) a modified vinyl aromatic polymer in which the active terminal of the polymer is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h), the average number of functional groups per molecule is 1.5 or more, the number average molecular weight Mn is 500 to 30,000, and the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn is 1.0 to 10.0; A resin composition comprising (B) a thermoplastic resin and (C) a curing catalyst, A curable resin composition, characterized in that the blending ratios of the respective components (A), (B) and (C) satisfy the following formulas (1) to (3). (A)+(B)+(C)=100(wt%) (1) (A) = 5.0 to 95.0 (wt%) (2) (B) = 94.9 to 0.1 (wt%) (3) (C) = 0.1 to 4.9 (wt%) (4)
2. 2. The curable resin composition according to claim 1, wherein the modified vinyl aromatic polymer (A) has a number average molecular weight Mn of 500 to 10,000.
3. 2. The curable resin composition according to claim 1, wherein the ratio Mw / Mn of the weight average molecular weight Mw to the number average molecular weight Mn of the modified vinyl aromatic polymer (A) is 1.0 to 3.
0.
4. The resin composition according to claim 1, further comprising (D) a thermosetting resin.
5. 2. The curable resin composition according to claim 1, wherein the functional group-modified vinyl aromatic copolymer (A) further contains a structural unit derived from a conjugated diene compound.
6. The curable resin composition according to claim 1, wherein the component (B) is one or more thermoplastic resins selected from the group consisting of a thermoplastic homopolymer or copolymer of a monomer containing 50 to 100 mol% of one or more monomers selected from the group consisting of butadiene, isoprene, styrene, ethylstyrene, divinylbenzene, N-vinylphenylmaleimide, acrylic acid esters, and acrylonitrile, a polyphenylene ether which may have a substituent, a polyolefin having a ring structure, a polysiloxane, a polyester, a polysulfone, a polyethersulfone, a polyamide, a polyimide, a polyamideimide, and a polyetherimide.
7. 2. The curable resin composition according to claim 1, wherein the component (C) is one or more curing catalysts selected from the group consisting of radical initiators and cationic polymerization initiators.
8. 5. The curable resin composition according to claim 4, wherein the component (D) is a thermosetting resin containing one or more functional groups selected from the group consisting of an epoxy group, a cyanate group, a vinyl group, an ethynyl group, an isocyanate group, and a hydroxyl group.
9. The curable resin composition according to claim 1 , further comprising (E) a flame retardant and / or (F) a filler.
10. A molded article obtained by molding the curable resin composition according to any one of claims 1 to 9.
11. A cured product obtained by curing the curable resin composition according to any one of claims 1 to 9.
12. A film comprising the curable resin composition according to any one of claims 1 to 9.
13. A composite material comprising the curable resin composition according to any one of claims 1 to 9 and a substrate, the composite material comprising the substrate in an amount of 5 to 90% by weight.
14. A cured composite material obtained by curing the composite material according to claim 13.
15. A laminate comprising a layer of the cured composite material of claim 14 and a metal foil layer.
16. A resin-coated metal foil having a film of the curable resin composition according to any one of claims 1 to 9 on one side of the metal foil.
17. A varnish for circuit board materials, obtained by dissolving the curable resin composition according to any one of claims 1 to 9 in an organic solvent.
18. In the presence of a polyfunctional anionic polymerization initiator produced by reacting a polyfunctional vinyl aromatic compound (b) and / or an aromatic compound (c) having 2 to 4 alkyl groups having 1 to 3 carbon atoms in the presence of an organic alkali metal compound (e), A method for producing a modified vinyl aromatic polymer, in which an active terminal of a polymer obtained by polymerizing a monovinyl aromatic compound (a) is modified with a functional group having a vinyl group derived from a halogen-containing vinyl compound (h), comprising the steps of: 50 mol % or more of the total of the structural units derived from the reactions involving the components (a), (b), (c), and (e) are structural units each independently containing a plurality of structural units (M1) derived from the monovinyl aromatic compound (a); less than 50 mol % in total of the structural units derived from the reactions involving the components (a), (b), (c), and (e) are structural units containing only the structural unit (M1) derived from the monovinyl aromatic compound (a); The method for producing a modified vinyl aromatic polymer further comprises modifying the active terminal of the polymer with a vinyl functional group derived from a halogen-containing vinyl compound (h) to obtain a modified vinyl aromatic polymer having an average number of functional groups per molecule of 1.5 or more, a number average molecular weight (Mn) of 500 to 30,000, and a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of 1.0 to 10.0.
Citation Information
Patent Citations
Soluble polyfunctional vinyl aromatic copolymer and its manufacturing method
JP2007332273A
Resin composition, prepreg, metal-clad laminate, and printed wiring board
JP2015086330A
Metal-clad laminate and method for producing the same, metal foil with resin and printed wiring board
JP2016028885A
Resin composition, insulation film and semiconductor device
JP2016147945A
Prepreg and laminate sheet
JP2016191073A